High-capacity cathodes for all-solid-state thin-film batteries
The LRCO cathode material addresses the low energy density and high-temperature annealing limitations of TFBs by providing high capacity and flexibility without annealing, enhancing energy storage performance and substrate compatibility.
Patent Information
- Application Number
- JP2024522436
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-14
- Filing Date
- 2022-10-12
- Publication Date
- 2024-10-18
AI Technical Summary
Current thin film batteries (TFBs) are limited by low energy density and require high-temperature annealing, which increases processing time and cost while limiting substrate compatibility.
Development of a cathode material composed of lithium, ruthenium, and cobalt oxides (LRCO) that can be fabricated without thermal annealing, allowing for higher energy density and compatibility with a variety of substrates, including flexible thermoplastics.
The LRCO cathode material achieves nearly twice the charge storage capacity of previous cathodes, operates reversibly without annealing, and can be fabricated on flexible substrates, reducing production costs and expanding application possibilities.
Smart Images

Figure 2024538118000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE Embodiments described herein relate generally to energy storage devices and methods of forming energy storage devices. More particularly, the energy storage device is a solid-state lithium thin-film battery. [Background technology]
[0002] Solid-state lithium thin-film batteries are utilized to enable enhanced energy storage performance, improved cycle life, enhanced safety, and high specific energy. Current approaches to fabricate thin-film batteries (TFBs) utilize a series of reduced pressure deposition operations to deposit the cell components onto a macroscopically thick substrate. Examples of these techniques include thermal evaporation, sputtering, chemical vapor deposition, pulsed laser deposition, and related techniques. TFBs are utilized for applications in smart sensors, microcomputers, biomedical health care devices, small robots, etc.
[0003] TFBs are currently limited in overall energy density. Therefore, thin-film cathode materials with higher specific energy are needed. The specific energy of the thin-film cathode determines most of the overall energy density of the cell. On the cathode side, many polycrystalline inorganic cathode compounds have been developed, but they have limited specific energy or poor charging reversibility. Furthermore, polycrystalline thin-film cathodes typically require high-temperature annealing to achieve the preferred crystalline phase and optimal energy storage performance. High-temperature annealing adds significant processing time and additional cost while limiting the material compatibility of the substrate.
[0004] Therefore, what is needed is a cathode material that has high specific capacity and reduced processing requirements. Summary of the Invention
[0005] The present inventors have developed a novel cathode material that can be used in a variety of lithium thin film battery applications. The novel cathode material is based on lithium, ruthenium, cobalt and their oxides, and provides energy density equal to or greater than current cathode materials. In addition, the novel cathode material can be prepared without a thermal annealing step. Due to the lack of high temperature conditions required for thermal annealing, the cathode material disclosed herein can be assembled on a wide variety of substrates, including flexible thermoplastic materials with low melting temperatures.
[0006] The present disclosure is generally directed to an energy storage device and a method of forming an energy storage device. In one embodiment, an energy storage device is described. The energy storage device includes a cathode, an anode, and an electrolyte. The cathode includes lithium, ruthenium, cobalt, and oxygen. The anode is disposed adjacent to the cathode. The electrolyte is disposed between the cathode and the anode.
[0007] In another embodiment, an energy storage device is described that includes a support substrate, a platinum coating disposed on a portion of the support substrate, a cathode disposed on the platinum coating, an anode disposed adjacent to the cathode, and an electrolyte disposed between the cathode and the anode. The cathode includes lithium, ruthenium, cobalt, and oxygen. The anode includes lithium. In some embodiments, the cathode is a metal of the formula Li 2+x Ru 1-x Co x O 3 In some embodiments, the cathode material has lithium, ruthenium, cobalt, and oxygen in amounts based on the formula Li 2+x Ru 1-x Co x O 3In some embodiments, the cathode is of the formula (1-x)Li 2 RuO 3 +xLiCoO 2 +yLi 2 In some embodiments, the cathode material has lithium, ruthenium, cobalt, and oxygen in amounts based on the formula (1-x)Li 2 RuO 3 +xLiCoO 2 +yLi 2 O), y is 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0 In some embodiments, the formula (1-x)Li is 0.36, 0.37, 0.38, 0.39, 0.40, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, and 0.60. 2 RuO 3 +xLiCoO 2 +yLi 2O), x is 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0 any one of, less than, greater than, between, or within any range thereof.
[0008] In yet another embodiment, a method of forming an energy storage device is described. The method includes depositing a cathode coating on a support substrate in a processing region of a processing chamber, depositing an electrolyte on the cathode layer, and depositing an anode on the electrolyte. The deposited cathode layer includes lithium, ruthenium, cobalt, and oxygen.
[0009] In yet another embodiment, an energy storage device is described. The energy storage device includes a cathode including lithium, oxygen, and two or more metals. The two or more metals are selected from the group of ruthenium, cobalt, tin, iridium, and manganese. The energy storage device further includes an anode disposed adjacent to the cathode, and an electrolyte disposed between the cathode and the anode.
[0010] In yet another embodiment, a method of forming an energy storage device is described. The method includes depositing a cathode coating on a support substrate in a processing region of a processing chamber, depositing an electrolyte on the cathode coating, and depositing an anode on the electrolyte. The cathode coating includes lithium, oxygen, and at least two of ruthenium, cobalt, tin, iridium, and manganese.
[0011] So that the method of the features of the present disclosure described above can be understood in detail, a more particular description of the present disclosure briefly summarized above may be made by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings illustrate only typical embodiments of the present disclosure and therefore should not be construed as limiting the scope of the disclosure, as the present disclosure may admit of other equally effective embodiments. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic cross-sectional view of a thin film battery according to embodiments described herein. [Diagram 2] 1 is a schematic cross-sectional view of a processing chamber for depositing one or more coatings according to embodiments described herein. [Diagram 3] 2A-2C illustrate a method of forming the thin-film battery of FIG. 1 according to embodiments described herein. [Figure 4A-4B] 1 is a graph showing X-ray diffraction patterns of cathodes synthesized at different temperatures. [Figure 5A-5B] FIG. 2 shows a scanning electron microscope image of cathode material powder. [Figures 6A-6C] 1 is a graph showing charge / discharge curves of lithium-ion half-cells assembled with LRCO cathode material after synthesis of the LRCO cathode material at various calcination temperatures. [Figure 7A-7C] 1 is a graph showing the cycling stability curves of lithium-ion half-cells assembled with LRCO cathode materials after synthesis of the LRCO cathode materials at various calcination temperatures. [Figure 8A-8B] 1 is a graph showing X-ray diffraction patterns of cathodes synthesized with varying cobalt content. [Figure 9A-9B] 1 is a graph showing the charge / discharge curves of lithium-ion half-cells assembled with the LRCO cathode material after synthesis of the LRCO cathode material with varying cobalt content. [Figure 10A-10B]1 is a graph showing the cycling stability curves of lithium-ion half-cells assembled with the LRCO cathode material after synthesis of the LRCO cathode material with varying cobalt content. [Figures 11A-11D] 1 is a graph showing X-ray photoelectron spectroscopy measurements of coatings deposited from sputtering targets formed from LRCO material. [Fig. 12A-12F] FIG. 1 shows plan-view scanning electron micrographs of thin films deposited from sputtering targets formed from LRCO material after various annealing operations. [Figure 13] FIG. 1 shows the X-ray diffraction patterns of cathodes annealed at various annealing temperatures. [Figure 14A-14D] FIG. 1 shows a scanning electron micrograph of a thin film deposited from a sputtering target formed from LRCO material and annealed. [Figure 15] 1 is a graph showing charge / discharge curves of a lithium-ion half-cell assembled with a LRCO cathode material after cycling using a first charging pattern. [Figure 16] 1 is a graph showing the cycling stability curves of a lithium-ion half-cell assembled with a LRCO cathode material after cycling using a first charging pattern. [Figures 17A-17C] 1 is a graph showing the charge / discharge voltage profiles of a LRCO thin film battery at 0.3 C from 2.0 V to 3.8, 3.9, and 4.0 V for the 1st, 50th, and 100th cycles, respectively. [Figures 18A-18C] 1 is a graph showing the discharge capacity / coulombic efficiency of a LRCO thin film battery from 2.0 V to 3.8, 3.9 and 4.0 V, respectively, over a given number of cycles. [Figure 19] Figure 13 is a graph of the rate performance of a LRCO / LCO thin film cell with a 300 nm thick cathode at 3, 10, 15, 27, 33 μA / cm2, then back to 3 μA / cm2. Cycling performance: 2.0-3.9 V (LRCO) and 3.0-4.2 V (LCO) vs. Li / Li+ at 25 °C. [Figure 20A-20B] 1 is a graph showing charge / discharge curves of a lithium thin film cell assembled with a LRCO cathode material after annealing the first cathode material at various temperatures. [Figure 21A-21B] 1 is a graph showing cycling stability curves of a lithium thin film cell assembled with a LRCO cathode material after annealing the first cathode material at various temperatures. [Figure 22] 1A to 1C are schematic diagrams illustrating a method for manufacturing a thin-film battery. [Figure 23A-23B] FIG. 1 shows schematics and plan-view scanning electron microscope (SEM) images of LRCO thin films on Si wafers comparing deposited film morphology with respect to sputtering target-substrate distance. [Fig. 24A-24B] FIG. 1 shows plan and cross-sectional SEM images of as-deposited LRCO thin films on Si wafers with thermal oxide at a sputtering distance of 5 cm. [Diagram 25] 1 is a graph showing XRD patterns comparing a LRCO sputtering target, an as-deposited LRCO thin film, and a thermally oxidized Si wafer substrate. [Figure 26] 1 shows a cross-sectional SEM image of an as-deposited LRCO thin film on a Si wafer (deposition distance was 10 cm). [Figure 27] FIG. 13 shows the EDS spectrum and corresponding elemental composition of as-deposited LRCO thin films on Si wafers with thermal oxide at a sputtering distance of 10 cm. [Figure 28] FIG. 1 shows a 3D schematic structure of a LRCO thin-film battery. [Figures 29A-29D] FIG. 13 shows cross-sectional SEM images of a completed thin-film cell with a 300 nm thick LRCO cathode along with the corresponding P, Ru and Si elemental EDS maps, respectively. [Diagram 30] FIG. 1 shows digital images of two completed thin-film batteries on a quartz slide. [Diagram 31]FIG. 13 is a graph showing the differential capacity versus voltage of a 300 nm thick as-deposited LRCO thin film cell for the charging step from 2.0 to 4.0 V in the second cycle at 10 μA / cm2 (0.3 C). [Fig. 32A-32B] FIG. 13 is a graph showing the cycling performance of a LRCO thin film battery with a 300 nm thick as-deposited cathode from 2.0 to 3.9 V at 10 μA / cm2 (0.3 C) over 300 cycles, and a graph showing a cycling performance comparison among three LRCO thin film batteries cycled from 2.0 to 4.0 V at 10 μA / cm2 (0.3 C). [Fig. 33A-33B] FIG. 13 is a cyclic voltammogram graph of an LCO thin film cell with a 300 nm thick as-deposited cathode from 3.0 to 4.2 V at a scan rate of 0.1 mV / s, and a differential capacity versus voltage graph of an as-deposited LCO thin film cell during the charging step of the second cycle from 3.0 to 4.2 V at 10 μA / cm2. [Diagram 34] FIG. 13 is a cyclic voltammogram graph of a LRCO / LCO thin film cell with a 300 nm thick as-deposited cathode at a scan rate of 0.1 mV / s and a voltage range of 2.0 to 3.9 V vs. Li / Li+. [Diagram 35] FIG. 2 is a cycling performance graph of an LCO thin film battery with a 300 nm thick as-deposited cathode cycled from 3.0 to 4.2 V at 10 μA / cm2. [Diagram 36] 1 is a graph comparing typical inorganic thin film cathode candidates, including the specific capacity for the cathode, capacity retention after a certain number of cycles, and annealing temperature (RT = room temperature). [Figure 37] 1 is a graph showing the open circuit voltage of a Kapton® based LRCO thin film battery during the first 5 minutes under bending and the remaining 5 minutes at rest (flat). [Fig. 38A-38B]FIG. 13 is a graph showing the cycling performance of a LRCO thin film battery with a 300 nm thick as-deposited cathode on a PET substrate that was bent for 120 cycles, and on a Kapton substrate that remained flat for 60 cycles and then bent for the remaining 60 cycles. [Figure 39A-39B] FIG. 13 shows images of a flexible LRCO TFB on a PET substrate with operating LED before and after bending, respectively. [Diagram 40] 1 is a graph comparing typical inorganic thin film cathode candidates on flexible substrates, including the specific capacity for the cathodes, capacity retention after 100 cycles, and annealing temperature. The capacity retention of LiMnO4 (700° C.), LiNi0.5Mn1.5O4 (RT), and Li4Ti5O12 (230° C.) is reported at the 80th, 20th, and 90th cycles, respectively. [Diagram 41] 1 is a table comparing the properties of various thin film cathode materials. [Diagram 42] 1 is a table comparing various thin film cathodes on flexible substrates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Embodiments of the present disclosure are directed to high capacity thin film cathodes for solid-state lithium thin film batteries. In some embodiments, the solid-state lithium thin film batteries are fabricated with sub-millimeter dimensions, e.g., on the order of 100 μm×100 μm. In some embodiments, the solid-state lithium thin film batteries are several micrometers to tens of micrometers thick, e.g., about 5 μm to about 30 μm thick, e.g., about 5 μm to about 20 μm thick, e.g., about 5 μm to about 15 μm thick. The cathode composition comprises LiRu 2 O 3 and LiCoO 2 It is synthesized as a solid solution of LiCoO and contains lithium, ruthenium, cobalt and oxygen. The thin film cathode is fabricated on a substrate by radio frequency magnetron sputtering technique, and the as-deposited thin film cathode is LiCoO 2The cathode has roughly twice the discharge capacity of current thin film cathodes such as those described above. The cathode also works well in the as-deposited, unannealed state and has been shown to be reversible.
[0014] The cathode composition is approximately (1-x)Li 2 RuO 3 +xLiCoO 2 +yLi 2 In embodiments where y is the same as x, the formula becomes Li 2+x Ru 1-x Co x O 3 As described herein, y can vary from about 0.05 to about 0.6, such as from about 0.1 to about 0.4. For example, in certain embodiments, y is substantially equal to 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, etc. X can similarly vary from about 0.05 to about 0.5, such as from about 0.1 to about 0.3. For example, in certain embodiments, x is substantially equal to 0.1, 0.2, 0.3, 0.4, 0.5, etc. Materials containing lithium, ruthenium, cobalt, and oxygen as described herein may also be referred to as LRCO materials, and films formed from LRCO materials may also be referred to as LRCO thin films. The atomic ratio of each of the elements in the LRCO material may vary as described herein, but in some embodiments, the LRCO material includes each of lithium, ruthenium, cobalt, and oxygen.
[0015] In some embodiments, materials other than LRCO materials are utilized and the cathode is formed from an anion redox active material. The anion redox active material includes LRCO materials and other materials described herein. The anion redox active material may be an anion redox active perlithiated transition metal oxide. The anion redox active material may be a mixture of at least one lithium metal oxide and a lithiated ruthenium oxide (Li 2 RuO 3 ) and lithiated iridium oxide (Li 2 IrO 3) or a combination thereof. Lithium metal oxides include lithium oxides of iron (Fe), cobalt (Co), nickel (Ni), manganese (Mn), tin (Sn), titanium (Ti), palladium (Pd), silver (Ag), zinc (Zn), gallium (Ga), indium (In), and vanadium (V). In some embodiments, the lithium metal oxides include one or a combination of iron (Fe), cobalt (Co), nickel (Ni), manganese (Mn), tin (Sn), titanium (Ti), and vanadium (V). Lithium metal oxides include one or a combination of lithium iron oxide, lithium cobalt oxide, lithium nickel oxide (LNO), lithium manganese oxide (LMO), lithium tin oxide, lithium titanium oxide (LTO), and lithium vanadium oxide. Thus, lithium metal oxides include LiFeO 2 , LiCoO 2 , LiNiO 2 , LiMnO 2 , LiMn 2 O 4 , Li 2 MnO 3 , LiSnO, Li 2 TiO 3 and LiV 3 O 8 One or a combination of the following may be mentioned.
[0016] In some embodiments where cobalt is replaced with tin, LiRu 2 O 3 and LiCoO 2 The solid solution with LiRu 2 O 3 and LiSnO 2 In some embodiments where cobalt is replaced with iridium, LiRu 2 O 3 and LiCoO 2 The solid solution with LiRu 2 O 3 and LiIrO 3Similarly, an alternative transition metal, such as manganese (Mn), may be substituted with ruthenium (Ru) in the composition. In some embodiments where manganese is substituted with ruthenium, LiRu 2 O 3 and LiCoO 2 The solid solution with LiMn 2 O 4 and LiCoO 2 and a solid solution containing LiMnO 2 and LiCoO 2 In some embodiments, LiRu is replaced by a solid solution comprising: 2 O 3 and LiMn 2 O 4 and LiCoO 2 , LiSnO 2 and Li 2 IrO 3 Other combinations of perlithiated transition metal oxides are contemplated but not expressly disclosed herein. Substitution of the compounds within the composition is made possible, at least in part, by the ability of the oxygen atoms within the compounds to participate in redox reactions. At least Li 2 RuO 3 and Li 2 IrO 3 has improved electrical conductivity compared to other lithium metal oxides. 2 RuO 3 and Li 2 IrO 3 At least one of the compounds is utilized. The improved electrical conductivity improves the performance of the thin film battery. At least one of the anion redox active materials is a LRCO material as described herein.
[0017] In some embodiments, the cathode material is deposited on a rigid substrate. In further embodiments, the cathode material is deposited on a flexible substrate. As used herein, "flexible" is defined as being capable of at least one of bending, stretching, and / or compressing without cracking, breaking, cracking, and the like. In some embodiments, the flexible substrate can be made of or include a metal. Non-limiting examples of flexible metal substrates are platinum foil and aluminum foil. In some embodiments, the flexible substrate is a thermoplastic substrate.Thermoplastic substrates include amorphous thermoplastics, semi-crystalline thermoplastics, crystalline thermoplastics, and elastomeric materials, including, but not limited to, polyimides, poly(aryl ether ketones) (PAEK), poly(butylene terephthalate) (PBT), poly(butyrate), poly(ether ether ketone) (PEEK), poly(etherimide) (PEI), poly(2-hydroxyethyl methacrylate) (pHEMA), poly(isocyanurate) (PIR), poly(methyl methacrylate) (PMMA), poly(oxymethylene) (POM); poly(phenylsulfone) (PPSF), poly(styrene) (PS), poly(trimethylene terephthalate) (PTT), poly(urea) (PU); poly(amide)-based thermoplastics, such as aliphatic poly(amides), poly(phthalamide) (PPA), and aramids (aromatic poly(amides) ...trimethylene terephthalate) (PTT), poly(urea) (PU); poly(amide)-based thermoplastics, such as aliphatic poly(amides), poly(phthalamide) (PPA), and aramids (aromatic poly(amides)); poly(phenylsulfone) (PPSF), poly(styrene) (PS), poly(phenylsulfone) (PPSF), poly(styrene) (PS), poly(phenylsulfone) (PPSF), poly(phenylsulfone) (PPSF), poly(phenylsulfone) (PPSF), poly(phenylsulfone) (PPSF), poly(phenylsulfone) (PPSF), poly(phenylsulfone) (PPSF), poly( poly(carbonate)-based thermoplastics; poly(ester)-based thermoplastics such as poly(ethylene) naphthalate (PEN) and poly(ethylene terephthalate) (PET); poly(olefin)-based thermoplastics such as poly(ethylene) (PE), poly(propylene) (PP), poly(propylene carbonate) (PPC), poly(methylpentene) (PMP) and poly(butene-1) (PB-1); poly(stannane)-based thermoplastics; poly(sulfone)-based thermoplastics; poly(vinyl)-based thermoplastics such as poly(vinyl chloride) (PVC), poly(vinylidene fluoride) (PVDF), poly(vinyl fluoride) (PVF), poly(vinyl nitrate) (PVN) and poly-(4-vinylphenol) (PVP); and cellulosic thermoplastics such as cellulose ester thermoplastics and cellulose ether thermoplastics.
[0018] In some embodiments, the electrolyte comprises lithium phosphate oxynitride (LiPON). In further embodiments, the electrolyte comprises LiAlSiO 4 , lithium lanthanum titanate (LLTO), lithium sulfuric oxynitride phosphate (LiPSON), lithium borate oxynitride (LiBON), LiPON, and combinations thereof.
[0019] As described herein, the LRCO cathode is deposited in a thin film format. The thin film format and LRCO cathode described herein are theorized to provide nearly double the charge storage capacity over previous cathode materials. As described herein, LRCO thin film batteries were prepared by RF magnetron sputtering and then incorporated into thin film batteries. LRCO thin films can be formed using LRCO-containing sputtering targets. LRCO-containing sputtering targets may be sputtered onto a substrate using RF magnetron sputtering techniques, where RF power is applied to a magnetron assembly of a process chamber and the LRCO material is sputtered from the sputtering target onto a substrate disposed within the process chamber.
[0020] The experimental methods utilized to form the exemplary LRCO cathodes and thin film batteries are further described herein. The resulting LRCO cathodes and thin film batteries were then tested as described herein.
[0021] 1 is a schematic cross-sectional view of a thin-film battery 100 according to an embodiment described herein. The thin-film battery 100 includes a substrate 102, a current collector 104, a cathode 106, an electrolyte 108, and an anode 110. The substrate 102 may be used to support the current collector 104, the cathode 106, the electrolyte 108, and the anode 110. In some embodiments, the cathode 106 is disposed between the current collector 104 and the electrolyte 108. In some embodiments, the electrolyte 108 is disposed between the cathode 106 and the anode 110. As described herein, the cathode 106 is a LRCO electrode and contains each of lithium, ruthenium, cobalt, and oxygen.
[0022] The substrate 102 may be an inorganic material, an organic material, or a combination thereof. Inorganic materials include silicon, aluminum oxide (AL), and the like. 2 O 3), quartz, and some polymers. In other embodiments, the methods described herein allow for the use of organic materials for the substrate 102, such as one or more polymers. As described herein, the methods used to form the cathode 106 allow for the use of lower cost flexible substrates, such as polymer substrates. As described herein, the substrate 102 is a supporting substrate and is generally used to support other elements of the thin film battery 100. The other elements of the thin film battery 100 are formed on the substrate, which may later be diced or cut into the form of multiple thin film batteries 100.
[0023] The current collector 104 is formed on the substrate 102. The current collector 104 can be a thin film current collector disposed on the substrate 102. The current collector 104 can be formed of an electronically conductive material. In some embodiments, the current collector 104 is formed of gold, silver, platinum, aluminum, a carbon-based current collector, or a combination thereof. Other electronically conductive materials are contemplated but are not listed herein for brevity. In some embodiments, the current collector 104 is a platinum metal current collector. The current collector 104 can have a current collector thickness T1 of greater than about 50 nm, such as greater than about 200 nm, such as between about 200 nm and about 1000 nm, such as between about 200 nm and about 500 nm. In some embodiments, the current collector thickness T1 is between about 50 nm and about 200 nm.
[0024] The cathode 106 is formed on the current collector 104 such that the current collector 104 provides a low electronic resistance connection to the cathode 106. The cathode 106 described herein is a LRCO electrode. LRCO electrodes contain either lithium, ruthenium, cobalt, and oxygen. The general composition of the LRCO electrode layer is of the formula (1-x)Li 2 RuO 3 +xLiCoO 2 +yLi 2O). Y varies between about 0.05 and 0.6, such as about 0.1 to about 0.4, such as about 0.2 to about 0.3. X varies between about 0.05 and 0.5, such as about 0.1 to about 0.3, such as about 0.2 to about 0.3. As described herein, x and y may be equal to 0.1, 0.2 or 0.3. As described above, the LRCO composition may include Li 2 RuO 3 and LiCoO 2 Li 2 RuO 3 vs. LiCoO 2 The ratio of may be varied to vary the cobalt concentration in the composition. In embodiments where x is greater than about 0.3, lower discharge capacities have been shown to be typical. In embodiments where x and y are assumed to be the same, the formula is Li 2+x Ru 1-x Co x O 3 Formula Li 2+x Ru 1-x Co x O 3 The atomic ratios provided by are approximate and the composition ratios may be slightly altered to fall within the atomic ratios described herein.
[0025] In some embodiments, the cathode is formed on the current collector 104, but the current collector 104 is a free-standing current collector. A free-standing current collector is not disposed on a substrate, such as the substrate 102. In this embodiment, the current collector 104 may be a thin foil, such as an electrically conductive foil. In some embodiments, the cathode is formed on the current collector 104, and the current collector 104 is later removed from the substrate 102 so that the substrate 102 can be removed.
[0026] As described herein, the atomic ratio of lithium to ruthenium in the cathode 106 can be from about 6:1 to about 2:1, such as from about 5:1 to about 2.2:1, such as from about 4:1 to about 2.5:1. In some embodiments, the atomic ratio of lithium to cobalt is controlled to be from about 23:1 to about 4:1, such as from about 21:1 to about 5:1, such as from about 15:1 to about 6:1, such as from about 12:1 to about 6:1. The ratio of cobalt has been shown to directly affect the electrochemical performance of the thin-film battery 100, with cobalt concentrations of about x=0.1 to about x=0.3 having improved electrochemical performance. In some embodiments, cobalt concentrations of about x=0.2 to about x=0.3 have improved electrochemical performance compared to cobalt concentrations of x=0.1. The atomic ratio of ruthenium to cobalt can be from about 10:1 to about 1:1, such as from about 8:1 to about 2:1, for example, from about 7:1 to about 2:1.
[0027] The cathode 106 further has a cathode thickness T2. The cathode thickness T2 is large enough to cover the current collector 104 while forming a thin-film cathode for the thin-film battery 100. As described herein, the cathode 106 can have a cathode thickness T2 of greater than about 50 nm, such as from about 50 nm to about 40,000 nm, such as from about 50 nm to about 4,000 nm, such as from about 50 nm to about 750 nm, such as from about 100 nm to about 500 nm, such as from about 100 nm to about 350 nm, such as about 250 nm or about 300 nm. The cathode compositions described herein allow a thin-film cathode to be formed relatively uniformly throughout the cathode. As described herein, the cathode has greater uniformity when deposited as an amorphous layer using physical vapor deposition (PVD) and before annealing.
[0028] In the embodiments described herein, the cathode 106 in the thin-film battery 100 can be either an annealed or unannealed film. If the cathode 106 is deposited using a PVD operation, no binder is utilized and the cathode 106 can be entirely amorphous and non-crystalline. In the embodiments herein, the grain size is less than 300 nm to reduce the possibility of short circuits in the thin-film battery 100. The reduced grain size further provides higher coulombic efficiency and reduced capacity fade. In some embodiments, the grain size is less than 250 nm, e.g., less than 200 nm, e.g., less than 150 nm, e.g., 100 nm. Increasing the grain size would increase the thickness of the electrolyte 108 to reduce the possibility of short circuits, thus limiting the coulombic efficiency, cost, and size of the thin-film battery 100.
[0029] The cathode 106 has a surface roughness (Ra) of less than about 1000 nm, e.g., less than about 700 nm, e.g., less than about 500 nm, e.g., about 300 nm. Reducing the surface roughness can improve the formation of electrolyte thereon, reducing the potential for shorting the thin-film battery 100. Surface roughness is directly correlated to grain size and decreases as grain size decreases.
[0030] The electrolyte 108 is formed over the cathode 106 and the substrate 102, with the electrolyte 108 covering the entire surface of the cathode 106. The electrolyte 108 is a solid-state electrolyte and may be deposited on the substrate 102 in the same manner as the cathode 106, for example, by solution casting or CVD or PVD techniques. As described herein, the electrolyte 108 may be a solid lithium ion conductor. A solid lithium ion conductor is utilized to conduct lithium ions between the cathode 106 and the anode 110. The electrolyte 108 may be as described herein and is a lithium phosphate oxynitride (LiPON) material. LiPON material is a Li x PO y N zwhere x-2y+3z-5 for various combinations of y and z. One exemplary atomic ratio is Li 3.3 PO 3.9 N 0.17 Additional examples of possible electrolytes can be found in any one of the following: BATES, JB(1992).Electrical properties of amorphous lithium electrolyte thin films.Solid State Ionics, 53-56, 647-654. https: / / doi.org / 10.1016 / 0167-2738(92)90442-r, Bates, JB, Dudney, NJ, Gruzalski, GR, Zuhr, RA, Choudhury, A., Luck, CF, & Robertson, JD (1993). Fabrication and characterization of amorphous lithium electrolyte thin films and rechargeable thin-film batteries.Journal of Power Sources,43(1-3),103-110.https: / / doi.org / 10.1016 / 0378-7753(93)80106-y, and Yu, X., Bates, JB, Jellison, GE, Hart, FX(1997).A stable thin-film lithium electrolyte:Lithium phosphorus oxynitride.Journal of The Electrochemical Society,144(2),524-532.https: / / doi.org / 10.1149 / 1.1837443.
[0031] The electrolyte thickness T3 is the thickness of the electrolyte 108 formed on the cathode 106. The electrolyte thickness T3 may be the distance separating the cathode 106 and the anode 110. The electrolyte thickness may be from about 0.05 μm to about 3 μm, for example, from about 0.5 μm to about 2 μm, for example, from about 1 μm to about 1.5 μm.
[0032] The anode 110 is disposed on the electrolyte 108. The anode 110 may be deposited using a slurry coating or PVD method. Other deposition methods, such as chemical vapor deposition (CVD) or atomic layer deposition (ALD), may also be utilized. The anode 110, such as a lithium metal foil, may be prefabricated. The anode 110 may be graphite, lithium metal, silicon alloy, titanium oxide, or other metallic materials. Other metallic materials may include germanium, indium, aluminum, tin, magnesium, zinc, silver, or gold. In some embodiments, the anode 110 is Li 4 Ti 5 O 12 , TiO 2 or SnO 2 In the embodiments described herein, the anode 110 is a lithium metal anode. In one example, the anode 110 is a lithium metal thin film. The anode 110 has an anode thickness T4. The anode thickness T4 can be about 0.05 μm to about 10 μm, such as about 1 μm to about 10 μm, such as about 1 μm to about 5 μm, such as about 1 μm to about 3 μm, such as about 2 μm.
[0033] In some embodiments, the anode 110 is replaced by a thin metal film. The thin metal film can be formed of a metal or an alloy. In some embodiments, the thin metal film is one or a combination of nickel or copper. The thin metal film is in turn deposited on the electrolyte 108. When a thin metal film is used, lithium metal is plated onto the metal film during charging of the thin film battery 100 and peels off from the thin metal film during discharging of the thin film battery 100. In some embodiments, the electrolyte 108 includes a lithium ion conductor and lithium metal is plated and peels off from the thin metal film during charging and discharging. In this embodiment, the thin metal film acts as a current collector and the thin film battery 100 is an anode-less thin film battery.
[0034] The total thickness T of the thin-film battery 100 excluding the substrate 102 0is less than about 150 μm, such as less than about 100 μm, such as less than about 50 μm, such as less than about 30 μm, such as less than about 25 μm, such as less than 20 μm, such as less than 10 μm. 0 The small size allows the thin film battery 100 to be utilized in a multitude of applications, such as medical devices, microcomputers, small robotics, etc. Additional layers and materials may also be used within the thin film battery 100.
[0035] In some embodiments, the substrate 102 may be omitted, and the current collector 104 is utilized as the base of the thin-film battery 100. In these embodiments, the current collector 104 may form the entire bottom surface of the thin-film battery 100.
[0036] In yet other embodiments, the structure of the thin-film battery 100 may be inverted such that the anode 110 is disposed on a current collector on the substrate 102, the electrolyte 108 is disposed on the anode 110 and the substrate 102, and the cathode 106 is formed on the electrolyte 108. In this embodiment, the anode 110 and cathode 106 of FIG. 1 may be switched, and the cathode current collector may be disposed on top of the cathode 106.
[0037] In some embodiments, multiple thin-film batteries 100 are stacked on top of each other, so that each individual thin-film battery 100 forms a cell, and two or more cells are stacked on top of each other. In these embodiments, a second current collector and / or a second cathode is disposed on the anode 100, the metal thin film and / or the electrolyte 108. A second electrolyte is formed on the second cathode / second current collector, and a second anode is formed on the second electrolyte. A third and / or a fourth battery cell may be disposed on top of the second cell. Stacking of the thin-film batteries 100 is possible by the absence of an annealing operation, and by keeping the thin-film batteries 100 below about 700° C., e.g., below about 500° C., e.g., below about 300° C. The low-temperature maintenance formation method allows stacking because the material of the electrolyte 108 is not damaged or destroyed, as it would be if it were at a high temperature, e.g., above about 300° C.
[0038] In some embodiments, the thin-film battery 100 includes a cathode 106 that includes an anion redox active material. The anion redox active material includes at least one of a lithium metal oxide and a lithiated ruthenium oxide (Li 2 RuO 3 ) and lithiated iridium oxide (Li 2 IrO 3 ) or a combination thereof. Lithium metal oxides include lithium oxides of iron (Fe), cobalt (Co), nickel (Ni), manganese (Mn), tin (Sn), titanium (Ti), palladium (Pd), silver (Ag), zinc (Zn), gallium (Ga), indium (In), aluminum (Al) and vanadium (V). In some embodiments, the lithium metal oxides include one or a combination of iron (Fe), cobalt (Co), nickel (Ni), manganese (Mn), tin (Sn), titanium (Ti) aluminum (Al) and vanadium (V). Lithium metal oxides include one or a combination of lithium iron oxide, lithium cobalt oxide, lithium nickel oxide (LNO), lithium manganese oxide (LMO), lithium tin oxide, lithium titanium oxide (LTO), lithium nickel manganese oxide (NMC), lithium nickel cobalt aluminum oxide (NCA) and lithium vanadium oxide. Therefore, the lithium metal oxide is LiFeO 2 , LiCoO 2 , LiNiO 2 , LiMnO 2 , LiMn 2 O 4 , Li 2 MnO 3 , LiSnO, Li 2 TiO 3 , LiNi 1-x-y Mn x Co y O 2 , LiNi 0.8 Co 0.15 Al 0.05 O 2 and LiV 3 O 8One or a combination of the following may be mentioned.
[0039] The thin-film battery 100 further includes an anode 110 disposed adjacent to the cathode 106, and an electrolyte 108 disposed between the cathode 106 and the anode 110. The anode 110, electrolyte 108, current collector, and substrate 102 are similar to those previously described. The method of forming the thin-film battery 100 may be the same for various combinations of two or more metals. In one embodiment, the method of forming the thin-film battery 100 includes depositing the cathode 106 on the supporting substrate 102, depositing the electrolyte 108 on the cathode 106, and depositing the anode 110 on the electrolyte 108 in a processing region of a processing chamber. The cathode 106 includes lithium, oxygen, and at least two of ruthenium, cobalt, tin, iridium, and manganese.
[0040] 2 is a schematic cross-sectional view of a processing chamber 200 for depositing one or more films according to embodiments described herein. The processing chamber includes a chamber body 202, a substrate support assembly 204 disposed within the chamber body 202, a sputtering assembly 206 disposed above the chamber body 202, a gas supply 210, an exhaust pump 214, and a controller 230. The processing chamber 200 described herein is used to form one or more thin films on a substrate 250. The thin films may be similar to the films shown in FIG. 1 and in the thin film battery 100.
[0041] The chamber body 202 includes a processing region 208 disposed therein. The processing region 208 may be isolated from the atmosphere surrounding the chamber body 202 such that the processing region 208 is at an isolated reduced pressure. The chamber body 202 may include a number of openings positioned to allow other components to be inserted into the chamber body 202 and the processing region 208 therethrough.
[0042] The substrate support assembly 204 is disposed within the processing region 208 and includes a support pedestal 224 and an actuator 226 coupled to the support pedestal 224. The support pedestal 224 is configured to support a substrate 250 and includes a substrate support surface 205. The support pedestal 224 may be configured with one or more heaters, one or more cooling channels, and one or more backside gas lines (not shown) disposed therein. The actuator 226 is configured to move the support pedestal 224 such that the actuator 226 can move the support pedestal 224 vertically or rotate the substrate about an axis of the support pedestal 224. In the embodiments described herein, the support pedestal 224 is configured to be raised and lowered to move adjacent the sputtering target 218 during processing of the substrate.
[0043] The sputtering assembly 206 is disposed on the substrate support assembly 204. The sputtering assembly 206 is configured to sputter one or more materials onto the substrate 150. The sputtering assembly 206 includes a sputtering target 218, a magnetron assembly 220, and a power supply 222. The power supply 222 is configured to provide power to the magnetron assembly 220. The power supply 222 may further bias the sputtering assembly 206 by biasing the sputtering target 218. The power supply 222 may be an AC power supply or an RF power supply. The magnetron assembly 220 includes a plurality of magnets disposed therein and is configured to move within a volume of the magnetron assembly 220. At least one surface of the sputtering target 218 is exposed to the processing region 208, and a surface of the sputtering target 218 facing the substrate 250 is disposed within the processing region 208. In other embodiments, the positions of the sputtering assembly 206 and the substrate support assembly 204 are reversed, with the sputtering assembly 206 positioned below the substrate support assembly 204 and the substrate 102 .
[0044] The gas source 210 is in fluid communication with the processing region 208 and is configured to supply one or more process gases to the processing region 208 through one or more openings 212 disposed in the chamber body 202. The gas source 210 can be configured to flow a single gas, a gas mixture, or multiple gases to the processing region 208. In some embodiments, the gas source 210 includes multiple gas sources. In the embodiments described herein, the gas source 210 is configured to supply one or more inert gases, such as helium, neon, or argon. The gas source 210 may also be configured to supply a process gas, such as nitrogen or oxygen, to the processing region 208.
[0045] An exhaust pump 214 is also in fluid communication with the processing region 208 and is configured to remove one or more process gases from the processing region 208. The exhaust pump 214 removes the process gases through one or more exhaust openings 216 disposed through the chamber body 202. The exhaust pump 214 may apply a reduced pressure to the processing region 208. In the embodiments described herein, the gas supply 210 and exhaust pump 214 may purge the processing region 208 between processing operations or when moving a substrate, such as substrate 250, into or out of the processing region 208.
[0046] The controller 230 is configured to control the processing of the substrate 250 in the processing chamber 200. The controller 230 described herein can be configured to control the actuator 226, the sputtering assembly 206, the gas supply 210, and the exhaust pump 214. The controller 230 can be one controller or multiple individual controllers. The controller 230 is a general-purpose computer used to control one or more components found in the processing chamber 200. The system controller 230 is generally designed to facilitate the control and automation of one or more of the processing sequences disclosed herein, and typically includes a central processing unit (CPU) 232, a memory 234, and supporting circuits (or I / O) 236. Software instructions and data can be encoded and stored in the memory 234 (e.g., a non-transitory computer readable medium) for instructing the CPU 232. A program (or computer instructions) readable by a processing unit in the system controller determines which tasks are executable in the processing chamber 200. For example, the non-transitory computer readable medium includes a program configured to perform one or more of the methods described herein when executed by the CPU 232. Preferably, the program includes code for performing tasks related to monitoring, executing and controlling the movement, support and / or alignment of the substrate, and performing various process recipe tasks and process recipe steps of various process modules.
[0047] FIG. 3 illustrates a method 300 for forming the thin-film battery 100 of FIG. 1. The method 300 can form a thin-film battery with reduced thickness and increased capacity. The method 300 can be performed in one or more processing chambers similar to the processing chamber 200 of FIG. 2. The method 300 includes an operation 302 of depositing a cathode coating, e.g., cathode 106, on a substrate, e.g., substrate 102. In the embodiments described herein, a current collector, e.g., current collector 104, is already disposed on the substrate. The current collectors described herein can be formed from any one of gold, silver, platinum, carbon nanotubes, other conductive materials, or combinations thereof.
[0048] The formation of the cathode coating may be performed using a suitable deposition technique. As described herein, the cathode coating may be deposited either using a slurry coating or using a CVD or PVD operation. Forming the cathode coating on a substrate using a PVD operation has been shown to result in a more uniform deposition with smaller grain size. When the cathode coating is deposited using a PVD operation, the cathode coating may be an amorphous coating. The PVD operation includes sputtering a LRCO material onto a substrate from a sputtering target, such as sputtering target 218. The sputtering target is formed from a LRCO material, such as the LRCO-1, LRCO-2, or LRCO-3 material described herein. The LRCO material forming the sputtering target includes each of lithium, ruthenium, cobalt, and oxygen.
[0049] During deposition of the LRCO material, the process chamber was filled with approximately 1×10 -8 Torr ~ approx. 1×10 -5 Torr, e.g., about 1×10 -7 Torr ~ approx. 1×10 -6 Torr, e.g., about 5×10 -7 The process chamber is evacuated to a base pressure of about 1 mTorr. After evacuating to the base pressure, the process chamber is brought to a working pressure. The working pressure is from about 1 mTorr to about 5 Torr, such as from 10 mTorr to about 1 Torr, such as about 15 mTorr. The working pressure is the pressure at which the cathode coating is formed using PVD techniques.
[0050] Power is applied to a magnetron assembly, such as magnetron assembly 206 in FIG. 2. The power density applied to the sputtering assembly is about 1 W / cm. 2 ~ approx. 8 W / cm 2 , for example, about 1.2 W / cm 2 ~Approx. 7.5W / cm 2 , for example, about 2 W / cm 2 ~about 6W / cm 2 , e.g. 2.5 W / cm 2 ~about 5W / cm2 , for example, about 3 W / cm 2 ~about 4W / cm 2 It is.
[0051] The substrate is positioned at a sputtering distance from the surface of a sputtering target, e.g., sputtering target 218. The sputtering distance is the distance between the surface of the sputtering target facing the substrate and the top surface of the substrate. The sputtering distance during a PVD process is from about 3 cm to about 25 cm, e.g., from about 5 cm to about 20 cm, e.g., from about 5 cm to about 15 cm, e.g., from about 5 cm to about 10 cm. In exemplary embodiments described herein, the sputtering distance is one of 5 cm or 10 cm.
[0052] During the PVD process, one or more process gases may be flowed into the process region. The process gases include one or more inert gases and one or more process gases. The one or more inert gases may be one of helium, neon, or argon. As described herein, the inert gas is argon. The inert gas flows at a flow rate between about 1 sccm and about 20 sccm, such as between about 2 sccm and about 10 sccm, such as between about 3 sccm and about 5 sccm. A second gas, e.g., a process gas, may also be supplied to the process region during the PVD process. The second gas may be nitrogen (N 2 ), oxygen (O 2 ), or a combination thereof. In exemplary embodiments described herein, the second gas is oxygen and is flowed into the processing region at a flow rate between about 0.5 sccm and about 5 sccm, such as between about 1 sccm and about 3 sccm, such as about 1 sccm.
[0053] During deposition of the cathode layer on the substrate, the temperature in the processing area is less than about 100° C. The reduction in temperature allows the use of additional substrate materials other than aluminum oxide, silicon or quartz substrates. In some embodiments, a polymer-containing substrate may be utilized. The polymer-containing substrate may be an organic or inorganic substrate.
[0054] The above process conditions for PVD deposition of a LRCO cathode are exemplary and may be adjusted to compensate for different chamber configurations, deposition rates and substrate sizes.
[0055] After the cathode is deposited on the substrate, the cathode may be optionally annealed during operation 304. The optional annealing of the cathode is performed for a duration of at least about 1 hour, such as from about 1 hour to about 20 hours, such as from about 1 hour to about 10 hours, such as from about 1 hour to about 6 hours, such as about 1 hour. The annealing temperature is from about 100° C. to about 800° C., such as from about 100° C. to about 700° C., such as from about 400° C. to about 650° C. The length and temperature of the cathode during operation 304 directly correlate to the grain size generated in the cathode. In embodiments described herein, the grain size after the optional annealing is less than 250 nm, such as less than 200 nm, such as less than 150 nm, such as 100 nm. In embodiments without annealing, the cathode remains amorphous.
[0056] In either embodiment with or without optional annealing operation 304, an electrolyte is formed on the cathode layer during operation 306. The formation of the electrolyte may be performed using similar deposition conditions as the deposition of the cathode layer. In some embodiments, the electrolyte is also formed using a PVD process. In other embodiments, the electrolyte is deposited using a CVD process or an ALD process. Other methods may also be utilized to form the electrolyte. The electrolyte is a solid lithium ion conductor. In some embodiments, the electrolyte is formed from a LiPON material. The electrolyte may be sputtered onto the substrate using a LiPON sputtering target, resulting in the cathode being covered by the electrolyte.
[0057] After covering the cathode layer with the electrolyte, during operation 308, an anode is formed on the electrolyte. The anode may be similar to the anode 110 of FIG. 1. The anode is formed using a similar method to that used to deposit the cathode and electrolyte. The anode may be deposited using one of a PVD method, a CVD method, an ALD method, etc. The anode, for example, a lithium metal foil, may be prefabricated. The anode is formed of one or a combination of graphite, lithium metal, or another metal material. In the embodiment described herein, the anode is a lithium metal anode. The anode is deposited in a different process chamber than the cathode or electrolyte, and each of the anode, electrolyte, and cathode is formed in a separate process chamber.
[0058] In some embodiments, the substrate 102 is omitted or replaced. In embodiments in which the substrate 102 is omitted, the current collector 104 has a greater thickness, and the cathode 104, electrolyte 108, and anode 110 are formed on the current collector 104 without the substrate 102 disposed below the current collector 104.
[0059] In some embodiments, the structure of the thin-film battery 100 is inverted, with the anode current collector disposed on the substrate 100. The anode 110 may then be deposited on the anode current collector, followed by the electrolyte 108 formed on the anode 110. Once the electrolyte 108 is formed, the cathode 106 may then be formed on the electrolyte 108. In this embodiment, the current collector 104 may be disposed on the cathode 106 and away from the substrate 100. In this embodiment, operation 308 occurs before any of operations 302, 304, or 306. Operation 308 is modified to deposit the anode on the substrate. After the anode is deposited, the electrolyte is deposited during operation 306. The cathode may then be subsequently deposited on the electrolyte and annealed during operations 302 and 304.
[0060] experiment The following non-limiting examples are provided to further illustrate the embodiments described herein, however, the examples are not intended to be all inclusive or to limit the scope of the embodiments described herein. EXAMPLES
[0061] Example 1 The materials and methods described above were experimentally tested as follows. First, LRCO powder was synthesized. The LRCO material was prepared using a solid state method. 2 CO 3 (Alfa Aesar, 99.9% purity, 10% by weight excess), RuO 2 (Alfa Aesar, 99.9% purity) and CoCO 3 The (Alfa Aesar, 99.9% purity) precursor was weighed according to the desired stoichiometry, mixed with anhydrous acetone (Fisher Chemical) and ground in a planetary ball mill (DECO, PBM-V-0.4L). Excess Li 2 CO 3 was included to compensate for possible Li losses during high temperature annealing and / or during the sputtering process in later steps. The milled / mixed powders were heated to temperatures between 900 and 1100 °C at 2 °C / min in a muffle furnace (air atmosphere) and then soaked at the final temperature for 12 h before cooling. The effect of the final annealing temperature on the structural and electrochemical properties was investigated.
[0062] The LRCO target is formed from the LRCO powder. The LRCO powder is Li 2.2 Ru 0.8 Co 0.2 O 3 The general chemical composition of the 2-inch sputtering target for thin film deposition is Li 2.2 Ru 0.8 Co 0.2 O 3The LRCO powder was prepared by high temperature sintering of the powder. First, any agglomerates in the LRCO powder were manually broken down using a mortar and pestle. The fine powder was then mixed with a solution of 5 wt% polyethylene oxide in N,N-dimethylformamide (DMF) binder solution, and the mixture was then heated to 70°C to remove the DMF solvent. The LRCO and poly(ethylene oxide) (PEO) binder mixture was cold pressed into a 2-inch diameter die at 11 metric tons for 5 minutes. The pellets were then placed in clean alumina pans and sintered in a room air muffle furnace. The following heating profile was used to sinter the target: The temperature was ramped to 300°C at 5°C / min. The temperature was then subsequently ramped to 550°C at 1°C / min with a dwell time of 0.5 hours at 550°C. It is theorized that the binder burnout occurs during the 550°C. The temperature was then subsequently ramped to 900°C at 20°C / min and dwelled at 900°C for approximately 5 hours. After the dwell at 900°C, the furnace was cooled at 2°C / min. After the sintered target was sufficiently cooled, it was attached to a copper backing plate (OHFC) using silver-filled vacuum grade epoxy (Dynaloy, KL-325K). The target was cured under vacuum at 70°C before being placed in the sputtering chamber.
[0063] Once the target was placed in the chamber, the thin films were deposited on the substrate in the sputtering chamber. RF magnetron sputtering was used in a reduced pressure deposition chamber to produce the LRCO thin films. Typically, non-optimized process parameters for RF magnetron sputtering include 5×10 -7 The deposition chamber was cooled to 300° C. for 1 hour with a base pressure of 1000 sq. mTorr, a working pressure of 15 mTorr, a power of 70 W, a substrate-to-target distance of 5–10 cm, an argon gas flow rate of 3 sccm into the deposition chamber, and an oxygen (O) flow rate of 1 sccm into the deposition chamber. 2) gas flow rates were included. Optical grade fused silica slides (AdValue Technology, FQ-S-001, 1 inch (length) x 1 inch (width) x 0.04 inch (thickness)) were used as substrates for all thin films deposited by the targets. LRCO thin films on quartz slides are typically 300 nm thick and are characterized by scanning electron microscopy (SEM).
[0064] Ultra high purity N 2 2 inch Li in atmosphere 3 PO 4 A thin film (nominal 1 μm) of lithium phosphate oxynitride (LiPON) was deposited directly on top of the cathode layer by radio frequency (RF) magnetron sputtering of a powder target (99.95%, Kurt J. Lesker). A custom-built sputtering chamber was used to deposit approximately 1 × 10 -7 The deposition was performed with a 500 keV gas pump at 1000 keV and pumped to 1000 keV Torr. The main deposition parameters were a forward wave power of 80 W, a nitrogen gas flow rate of 5 sccm, an operating nitrogen pressure of 20 mTorr, and a target-substrate distance of 5 cm. -6 Approximately 2 μm thick Li metal was thermally evaporated as the anode material in a vacuum chamber with a base pressure of 10 Torr. A quartz crystal monitor (QCM) was used to monitor the Li deposition rate in-situ.
[0065] For the cathodic annealing process, the as-deposited LRCO(Li 2.2 Ru 0.8 Co 0.2 O 3 A 300 nm thick film of 1000 nm ... 2 The mixture was transferred to a tube furnace for annealing under ambient atmosphere. As described herein, LRCO has the molecular formula Li 2+x Ru 1-x Co x O 3has a molar ratio of x=0.2. However, the concentration of cobalt in the material can vary. When x=0.1, LRCO is referred to as LRCO-1. When x=0.2, LRCO is referred to as LRCO-2. When x=0.3, LRCO is referred to as LRCO-3. Unless otherwise specified herein, x=2, and the LRCO material has a similar composition to LRCO-2. The furnace temperature is first increased to the set point at a ramp rate of 2° C. / min, then held for the desired time, and finally allowed to cool naturally to room temperature.
[0066] Materials characterization To determine the structure of LRCO powders and thin films, X-ray powder diffraction (XRD) was performed using a Rigaku Synergy-S diffraction system with a CuKα microfocus X-ray source. The XRD powder patterns were refined by MDI Jade 9 software. Inductively coupled plasma mass spectrometry (ICP-MS) (Perkin Elmer NexION 2000) was used to characterize the elemental composition (Li, Ru, and Co) of LRCO and to determine the exact stoichiometry of the LRCO powder. For postmortem analysis, the cells were carefully disassembled in an Ar-filled glove box. All samples were dried under vacuum, placed in hermetically sealed plastic bottles, and then transferred to the various analytical systems. Scanning electron microscopy (SEM) and energy dispersive X-ray spectroscopy (EDS) were performed on a ZEISS Crossbeam 340 FIB-SEM system using an accelerating voltage of 7.5 kV. To analyze the cross-sections of the samples, the sample substrates were manually broken.
[0067] Electrochemical characterization For the liquid coin cells, a slurry was prepared by adding a binder solution containing 10 wt% polyvinylidene fluoride (PVDF) in N-methyl-2-pyrrolidone (NMP) solvent to a LRCO powder mixture containing 80 wt% active material and 10 wt% Super P conductive carbon. The slurry was cast onto an aluminum foil current collector and dried overnight at 100 °C under vacuum before assembling the cell. Metal Li foil (1.9 mm × 0.75 mm, 99.9%, Alfa Aesar) was scraped, rolled, and cut into disks with a diameter of 1.43 cm and placed on a slightly larger diameter microporous glass fiber separator that served as a spacer to define the separation of the electrodes. The electrolyte used was 100 μl of 1.0 M LiPF6 (Gotion) in 1:1:1 EC:EMC:DMC. The coin cells were cycled from 2.0 V to 4.5 V using a battery cycler (BT-2043, Arbin Instruments). The first two cycles were set at a 0.02 C rate as the formation period. The cell temperature was controlled at 25 °C. The electrode area was defined by the geometric area of the cathode side. Potentiostatic electrochemical impedance (PEIS) measurements were performed over a frequency range of 3 MHz to 0.1 Hz at room temperature with 10 mV AC amplitude.
[0068] The thin-film batteries were cycled using a battery cycler (BT-2043, Arbin Instruments) in an Ar-filled glove box from 2.0 V to various charging potentials. The electrode area was defined by the geometric area of the cathode side. Potentiostatic electrochemical impedance (PEIS) measurements were performed at room temperature with 10 mV AC amplitude over a frequency range of 3 MHz to 0.1 Hz.
[0069] result To determine the optimal annealing temperature for the synthesis of LRCO powder, Li 2.2 Ru 0.8 Co 0.2 O 3The effect of annealing temperature (900°C, 1000°C, and 1100°C) on the microstructure of the monoclinic Li SiO 2 was investigated. Figures 4A-4B show the X-ray diffraction patterns of the cathodes synthesized at three different temperatures. Figure 4B shows a selected area of Figure 4A. 2 RuO 3 The structure (herein referred to as LRO) is given in PDF# 01-072-4645 and is hexagonal LiCoO 2 The structure (referred to herein as LCO) is assigned to PDF# 01-073-0964 (diffraction data is publicly available at the International Center for Diffraction Data database, icdd.com). LRCO is expected to crystallize into constituent LRO and LCO phases with space groups C2 / c and R3m symmetries, respectively. All LRCO powders are assigned to monoclinic LRO with space group C2 / c, where each LiO 6 The octahedral gap is filled with six RuO 6 surrounded by octahedra and therefore hexagonal LiRu in the transition metal layer 6Adjacent units are possible. A small stacking order of the transition metal layers along the monoclinic c-axis of LRO could be observed at angles ranging from 20 to 25°, especially at 900 and 1000 °C. The cationic order of the transition metal layers can be further examined by the intensity ratio of the characteristic peaks associated with the (002) and (020) planes. A higher (002) / (020) ratio indicates a higher cationic order, which results in a larger stacking order of the transition metal layers. As shown in Figure 4B, LRCO annealed at 1000 °C has the highest (002) / (020) ratio, indicating the highest stacking order of the transition metal layers and enhanced structural perfection. The (002), (010), (202) and (222) planes are separated into two peaks. One reason that the (002), (010), (202) and (222) planes have two peaks is that when the diffraction peak intensity exceeds the linear range of the sensor, the main peak will be visibly split. Alternatively, the two peaks can correspond to an increase in the degree of order due to high temperature, which causes the doped metallic material to be more uniformly distributed within the lattice, followed by a reduction in symmetry due to an over ordered structure.
[0070] With increasing annealing temperature, no new diffraction peaks are observed and all observed reflections can be assigned to the LRO PDF card, suggesting phase purity. At low Co content (x=0.2), it is difficult to observe diffraction peaks from the LCO phase. However, samples at higher sintering temperatures (1100°C) tend to be less crystalline, with weaker peak intensities and less distinct characteristic peaks.
[0071] Figures 5A-B are scanning electron microscope images of LRCO cathode material powder. As can be seen in the images in Figures 5A-B, for the sample heated at 1100°C, a disordered morphology prevails, with the particles sintered together. Compared to the powders heated at 900°C and 1100°C, the samples below 1000°C show sharper peaks, representing a higher degree of crystallinity. Therefore, we tentatively conclude that 1000°C is the optimal annealing temperature for the solid solution reaction.
[0072] To correlate the LRCO structures obtained at the three annealing temperatures with electrochemical performance, lithium-ion battery cathodes were prepared by incorporating the LRCO powder into a typical electrode slurry and casting the slurry onto an Al current collector. The LRCO cathode was incorporated into a coin cell along with a Li metal anode and a standard liquid electrolyte. The battery cell was operated at approximately 0.1 C (30 mAg -1 At a current density of Li + The cathode slurries were cycled galvanostatically from 2.0 V to 4.5 V vs. Li / Li. The cathode slurries were not optimized for long-term cycling studies. Thus, the electrochemical characterization provides a comparative study to understand the effect of annealing temperature on the electrochemical properties (e.g., initial charge capacity, lithiation potential, and charging reversibility). The corresponding voltage profiles and integrated capacity are provided in Figures 6A-6C and 7A-7C. Figures 6A-6C are graphs showing charge-discharge curves of lithium-ion cells assembled with the LRCO cathode material after synthesizing the LRCO cathode material at various calcination temperatures. Figures 7A-7C are graphs showing cycle stability curves of lithium-ion cells assembled with the LRCO cathode material after synthesizing the LRCO cathode material at various calcination temperatures. As shown in Figures 6A-6C, when initially charged to 4.5 V, Li was charged at various charge plateaus. 2.2 Ru 0.8 Co 0.2 O 3Lithium delithiation from the cathode occurs. The LRCO-2 cathode calcined at 1100° C. exhibits two clear charging plateaus. The first plateau is located at about 3.6 V and corresponds to the Ru 4+ / Ru 5+ The second plateau is located at about 3.8 V, which corresponds to the oxidation of Co 3+ / Co 4+ The vertical tail above 4.2 V corresponds to lithium desorption from the cathode side with loss of oxygen and anion redox reactions, i.e., the formation of peroxo / superoxol-like species ( This is due to the following: TIFF2024538118000002.tif6170).
[0073] After firing the cathode at 900°C, the LRCO-2 half coin cell was cycled to an initial discharge capacity of 255mAhg. -1 The initial coulombic efficiency was 70.5% and the capacity retention at the 70th cycle was 53.6%. After firing the cathode at a temperature of 1000 °C, the LRCO-2 half coin cell was cycled with an initial discharge capacity of 238 mAhg. -1 The initial coulombic efficiency was 94.3% and the capacity retention at the 70th cycle was 73.3%. After firing the cathode at a temperature of 1100 °C, the LRCO-2 half coin cell was cycled with an initial discharge capacity of 211 mAhg. -1 The initial coulombic efficiency was 83.9% and the capacity retention at the 70th cycle was 70.3%.
[0074] At a firing temperature of 900°C, the cycle stability shown in Figure 7A was observed. The initial discharge capacity was 255mAhg. -1 The initial coulombic efficiency is 70.5%, which shows the highest initial discharge capacity compared to the other two firing temperatures. The specific capacity gradually decreases during cycling, reaching 136 mAhg after 70 cycles. -1As shown in FIG. 7B, when the calcination temperature was increased to 1000° C., the LRCO-2 cathode showed an improved first discharge capacity (238 mAhg -1 ), an initial coulombic efficiency of 94.3%, and the highest capacity retention after 70 cycles (73.3%). At 1100 °C, this variant delivered 211 mAhg -1 The sample calcined at 1000 °C also exhibits the highest crystallinity and transition metal cation ordering (LiM 2 ), which improves the transport of Li-ions. Based on the comparison of the XRD powder patterns and electrochemical performance at the three calcination temperatures, 1000° C. is tentatively believed to be the preferred calcination temperature for the LRCO-2 cathode.
[0075] To determine the optimal Co substitution in LRCO, Li 2+x Ru 1-x Co x O 3 A series of compounds were prepared with x = 0.1, 0.2 and 0.3 in CoCO3 by solid state synthesis of LRCO powder. 3 The composition was varied through the ratio of 0.1 to 0.25. The composition of the synthesized powder was confirmed using ICP-MS.
[0076] Similar microstructural and electrochemical characterizations were carried out to determine the optimal Co substitution amount in LRCO. 2+x Ru 1-x Co x O 3The microstructure of the series of powders (x=0.1, 0.2 and 0.3) was characterized by XRD (shown in Figures 8A and 8B). LRCO-1, LRCO-2 and LRCO-3 crystallize into the LRO monoclinic structure. It should be noted that LRCO does not crystallize into the LCO-type rhombohedral structure until the Co content is above 0.4. Figures 8A-B show the X-ray diffraction patterns of cathodes synthesized with varying cobalt content.
[0077] As shown in Figures 8A and 8B, when Co substitution is increased, no new diffraction peaks can be observed and all current peaks can be indexed with the LRO PDF card, suggesting phase purity. As the Co content increases, sharper peaks are observed, indicating higher crystallinity. Substitution of Ru by Co leads to a change in the crystal structure, confirmed through a decrease in the superlattice peak intensity (20°-30°). When x=0.3, the peak intensity drops to a negligible level. The presence of small superlattice peaks can be used to represent the in-plane cation ordering of Li and Ru / Co in the transition metal layer.
[0078] As shown in FIG. 8B, the samples with increased cobalt content (x=0.2 and 0.3) had a higher (002) / (020) ratio than the sample with lower cobalt content (x=0.1). This indicates a greater stacking order of the transition metal layers and enhanced structural perfection. This is consistent with our electrochemical performance expectations, where cobalt at x=0.2 and x=0.3 has a similar but higher capacity retention after 70 cycles as cobalt at x=0.1 (FIGS. 7A-7C and 10A-10B). When the Co content reached x=0.3, only the (010) plane disappeared. This is attributed to the decrease in the Ru ratio. The intensity of most other crystal planes was enhanced for x=0.3. Therefore, the Co ratios at x=0.2 and x=0.3 are beneficial compared to x=0.1.
[0079] To evaluate the effect of cobalt substitution on electrochemical performance, LRCO-1 and LRCO-3 were incorporated into lithium-ion half cells and cycled galvanostatically using the previous cycling protocol. Figures 9A-B and 10A-B show that LRCO-1 and LRCO-3, respectively, produced 238 mAhg -1 and 210mAhg -1 It has been revealed that the device outputs an initial discharge capacity of 1000mV.
[0080] 9A-9B show charge / discharge curves for lithium-ion cells assembled with the LRCO cathode material after synthesis of the LRCO cathode material with varying cobalt content. Figure 9A shows the charge / discharge curve for the LRCO cathode material with a cobalt content of x=0.1. Figure 9B shows the charge / discharge curve for the LRCO cathode material with a cobalt content of x=0.3.
[0081] 10A-10B show the cycling stability curves of lithium-ion cells assembled with the LRCO cathode material after synthesis with varying cobalt content. Figure 10A shows the cycling stability curves for the LRCO cathode material with a cobalt content of x=0.1. Figure 10B shows the cycling stability curves for the LRCO cathode material with a cobalt content of x=0.3.
[0082] As seen in Figures 10A and 10B, when the Co substitution was increased to x = 0.3, the capacity retention decreased from 72.8% (obtained at x = 0.1) to 64.9%, suggesting that the lower cobalt concentration provides better electrochemical performance by providing reversible anion redox chemistry, cation ordering within the superlattice structure, and facile charge transfer processes.
[0083] LRCO-2(Li 2.2 Ru 0.8 Co 0.2 O 3) Cathode powder synthesis was performed based on the desired sintering temperature and cobalt content, followed by preparation of sputtering targets. The LRCO-2 composition was consolidated into a 2-inch diameter sputtering target (LRCO sputtering target) by high temperature sintering. Thin film cathodes were prepared by RF sputtering of the LRCO sputtering target. The resulting cathodes were dense lithium insertion compounds (e.g., lithium metal oxides) fabricated in a "thin" supported film format and functioned as anodes in solid-state electrochemical cells. These electrochemical cells include a supporting substrate, a thin film cathode, a solid lithium ion conductor (i.e., solid electrolyte), and an anode (e.g., lithium metal).
[0084] 11A-11B are graphs showing X-ray photoelectron spectroscopy (XPS) measurements of films deposited from sputtering targets formed from LRCO material. XPS analysis was performed to investigate the oxidation state of transition metals in as-deposited LRCO thin films (thin films prior to any annealing). FIG. 11A shows a global elemental survey of the LRCO film on the substrate. FIG. 11B shows the Co 2p region of the survey of FIG. 11A. The Co 2p spectrum is shown separately in FIG. 11B at approximately 780.9 eV (Co 2p 3 / 2 ) and about 796.3 eV (Co 2p 1 / 2 ) binding energy, which is in good agreement with LCO and can be attributed to the presence of Co in the +3 charge state. FIG. 11B shows a high-resolution scan of the O 1s region of the survey of FIG. 11A. FIG. 11D shows a high-resolution scan of the Ru 3p region of the survey of FIG. 11A. 486.7 eV (3p 1 / 2 ) and 464.0 eV (3p 3 / 2 ), the two Ru 3p core peaks appearing in FIG. 12D indicate that the oxidation state of Ru is 4+.
[0085] To further explore the difference in morphology of LRCO thin films deposited from the LRCO-2 target at a target-sample distance of 5 cm as a function of annealing temperature, top-down and cross-sectional SEM images are compared in Figures 12A-12F. Figure 12A shows the morphology of the as-deposited, unannealed LRCO thin film. Figure 12B shows the morphology of the LRCO thin film after annealing at 300°C for 1 hour. Figure 12C shows the morphology of the LRCO thin film after annealing at 400°C for 1 hour. Figure 12D shows the morphology of the LRCO thin film after annealing at 500°C for 1 hour. Figure 12E shows the morphology of the LRCO thin film after annealing at 600°C for 1 hour. Figure 12F shows the morphology of the LRCO thin film after annealing at 700°C for 1 hour.
[0086] At annealing temperatures of 300°C and 400°C (FIGS. 12B and 12C), a few crystal grains appeared on the surface, but the majority of the remainder were spherical particles similar to the as-deposited film (FIG. 12A). Starting at 500-600°C (FIGS. 12D and 12E), these remaining columnar surfaces began to crystallize. At 700°C (FIG. 12F), the entire film surface was fully crystallized, and the particles exhibited a polyhedral morphology with an average size of about 50 nm to about 100 nm.
[0087] To make a comparison between different annealing temperatures, the XRD patterns of the thin films are presented in Figure 13. Since the substrates are gold-coated thermal silicon oxide wafers, the gold and silicon oxide (SiO 2) diffraction peaks (as determined from the matching PDF card database) also appeared in the diffractograms. As the temperature increased, most of the diffraction peaks intensified as a result of the enhanced crystallinity, which can be demonstrated by SEM in Figures 12A-12F. As the annealing temperature increased, the (312) and (006) Bragg peaks became more dissociated at about 60° to about 65°. It is worth noting that some unknown peaks (labeled by "?") could not be assigned to LRO, LCO, gold or silicon oxide phases. These peaks may be due to impurity phases, e.g., Co, due to the high temperature annealing. 3 O 4 or RuO 2 Another possibility is that lithium reacts with gold at high temperatures, resulting in the presence of impurities. Furthermore, the morphologies described herein correspond to films deposited at a sputtering distance of 5 cm, whereas a sputtering distance of 10 cm may produce a different morphology.
[0088] SEMs of annealed LRCO-2 thin films (at 450° C. for 3 hours) are shown in FIG. 14A-D. FIG. 14A and FIG. 14B are top-view SEMs of annealed LRCO-2 thin films. FIG. 14C and FIG. 14D are cross-sectional SEMs of annealed LRCO-2 thin films. Many nanoscale particles appear after annealing, whose average size can range from about 50 nm to about 650 nm (FIG. 14C), and the possibility of short circuit increases greatly when depositing LiPON layer as electrolyte. Surprisingly, the total thickness of LRCO-2 thin films is reduced from about 300 nm to about 200 nm, as shown in FIG. 14D. Some highly crystallized regions are even thinner, e.g., about 120 nm (FIG. 14C). The non-uniform grain size distribution is unfavorable and will result in non-uniform Li-ion transport during cycling, resulting in low coulombic efficiency and rapid capacity fade. One possible explanation is that deposition over such large distances leads to a large chemical composition difference between the target and the deposited film due to the loss of low atomic mass lithium during the sputtering process, which leads to lithium deficiency in the film and the formation of impurity phases, such as RuO, during the subsequent annealing step. 2 Or Co 3 O 4 may occur.
[0089] The LRCO thin films discussed herein are fully functional reversible cathodes with significant capacity in the as-deposited, non-annealed state. Therefore, the electrochemical characterization and energy storage performance testing discussed herein focuses primarily on amorphous thin films of LRCO. There are also practical motivations for the use of as-deposited / non-annealed thin films. The use of as-deposited thin films eliminates the annealing step, greatly broadening substrate compatibility while reducing production costs. For the electrochemical characterization described herein, a 250 nm thick thin film cathode was deposited by sputtering a LRCO-2 target onto a platinum current collector supported on a quartz substrate. One micrometer of LiPON and nominally 2 micrometers of Li were sequentially deposited on the LRCO coating. 20 μA / cm2 The thin film cells were cycled between 2.0 V and 4.5 V at a rate of 20 μA / cm 2 and the current density was calculated using the cathode area. 2 Cycling between 2.0 V and 4.5 V at a rate of 105 μAh / cm is described herein as the first charging pattern. 2 A stable capacity of 67.5 μAh / cm2 was reversibly evaluated over 20 charge / discharge cycles. 2 LiCoO provides a capacitance of 100-150μm 2 This is a significant improvement over the cathode. Furthermore, the LCO film is thermally annealed at temperatures exceeding several hundred degrees Celsius to fully crystallize the LCO microstructure for optimal energy storage performance.
[0090] The voltage profile and cycling capacity of as-deposited LRCO-2 are provided in FIG. 15 and FIG. 16, respectively. FIG. 15 is a graph showing charge-discharge curves of a lithium-ion cell assembled with the LRCO cathode material after cycling using a first charging pattern. The charge-discharge curves in FIG. 15 are provided for the 1st, 10th, and 20th cycles. FIG. 16 is a graph showing the cycling stability curves of a lithium-ion cell assembled with the LRCO cathode material over 20 cycles using a first charging pattern. As shown in FIG. 16, the average coulombic efficiency over 20 cycles is 97.6% (excluding the 1st cycle), and the discharge capacity is 105.5 μAh / cm 2 The temperature was maintained at about 25° C. during the test.
[0091] The coulombic efficiency of the cell, sometimes referred to as reversibility, can be further improved by charging the LRCO at a lower current density to a lower potential. Figures 17 and 18 show the charge / discharge voltage profile and cycling performance as a function of charging potential. On the first charge to 3.8 V, the LRCO was 57.5 μAh / cm 2When discharged from 3.8 V to 2.0 V at a current density of 10 μA / cm2, the thin-film battery has a capacity of 101.3 μAh / cm2. 2 The first charge capacity of the LRCO thin film is 1.0-1.5 μm (FIG. 17A). The low first charge capacity is likely due to the large sputtering target-substrate distance (10 cm) resulting in the loss of the lightest Li atoms during sputtering, resulting in a Li-deficient LRCO thin film composition. After lithiation in the first discharge, the charge capacity recovers and matches the discharge capacity. Suppressed first charge capacity is observed for all charge potentials (FIGS. 17B and 17C). Over 175 cycles at a charge voltage of 3.8 V, the average coulombic efficiency was 99.5% with 86.8% capacity retention (FIG. 18A). Increasing the charge potential to 3.9 V results in more Li ions intercalating and deintercalating, resulting in a capacity of 104.2 μAh / cm. 2 The initial discharge capacity of 100 μAh / cm is obtained (FIG. 18B). The capacity retention further increases to 91.8% over 175 cycles (94.4% at the 100th cycle) with a higher average coulombic efficiency of 99.8% (FIG. 18B). With a charge cutoff voltage of 4.0 V, the discharge capacity is 111.7 μAh / cm 2 18B and 18C).
[0092] The LRCO thin film cathode also demonstrates exceptional rate performance, as shown in Figure 19. Figure 19 shows the rate performance of a LRCO thin film cell using an as-deposited cathode of 300 nm thickness. The current density was increased from 3 to 10, 15, 27 and 33 μA / cm. 2 to 3 μA / cm 2 The reversibility was further evaluated by measuring the discharge capacity stepwise while returning the battery to 1C (33 μA / cm). Each rate included 5 cycles in the voltage range of 2.0 to 3.9 V (LRCO) and 3.0 to 4.2 V (LCO). 2 ) current rate, 88.8 μAh / cm LRCO 2-μm specific capacity of 108.5μAh / cm at 0.1C 2 -μm, which represents a capacity utilization of 81.8%. As expected, the discharge capacity is strongly dependent on the current density, but after the rate test at 0.1C (3 μA / cm 2 ) is a further indication of the stability of the LRCO cathode. Meanwhile, the as-deposited LCO provides roughly one-third of the specific capacitance of the as-deposited LRCO thin film (3 μA / cm 2 37.1 vs 108.4 μAh / cm 2 Furthermore, the current density was reduced to 33 μA / cm 2 When the temperature rises to 100°C, the discharge capacity of LCO is only 8.6 μAh / cm 2 which represents a relatively low capacity utilization of 25.6% (compared to over 80% for LRCO). Given the excellent specific capacity and rate capability, LRCO is an excellent candidate, offering easy lithiation and delithiation, low resistance, and high volumetric capacity. 2 RuO 3 The issues associated with the cathode, such as oxygen gassing and voltage decay, can be addressed by using LiCoO in a thin film format. 2 This can be addressed by mixing with and limiting the charging potential.
[0093] The ability to obtain significant capacity in as-deposited LRCO allows the formation of thin film batteries without thermal annealing. Thermal annealing adds significant processing cost and time to the preparation of LCO thin film cathodes. Typically, LCO films are annealed at temperatures above 500° C. Thermal annealing also requires that the substrate is thermally stable. Typical substrates are inorganic materials, such as aluminum oxide (Al 2 O 3 ) or quartz. Although this initial demonstration of LRCO thin films used quartz substrates, the methods disclosed herein also include annealing-free thin film preparation on flexible, low melting temperature substrates, such as polymeric substrates.
[0094] In some embodiments, thermal annealing is used to crystallize the as-deposited LRCO, thereby increasing the specific energy, Li + The diffusivity and lithiation (lithiation) potential are expected to increase. In some embodiments, the LRCO thin films were annealed at 450° C. and 650° C. for 3 hours. The annealed LRCO thin films demonstrate reversible and stable charge capacity, as shown in FIGS. 20A-B and 21A-B.
[0095] 20A-20B show the charge-discharge curves of a lithium-ion cell assembled with the LRCO cathode material after annealing the LRCO cathode material at various temperatures. In FIG. 20A-20B, the LRCO thin film was charged at 3 μA / cm 2 In Li / Li + Between 2.0 V and 3.8 V for 3 μA / cm 2 In Li / Li + The LRCO thin film cathode was annealed at 450° C. for 3 hours in FIG. 20A. The LRCO thin film cathode was annealed at 650° C. for 3 hours in FIG. 20B. The temperature was maintained at 25° C. during cycling of the LRCO cathode thin film battery.
[0096] 21A-21B show the cycling stability curves of lithium-ion cells assembled with the LRCO cathode material after annealing the LRCO cathode material at various temperatures. In FIG. 21A, the LRCO thin film cathode was annealed at 450° C. for 3 hours. In FIG. 21B, the LRCO thin film cathode was annealed at 650° C. for 3 hours. The LRCO thin film battery was charged to 3.8 V for the first 10 cycles and to 4.0 V for the next 5 cycles. The discharge potential remained fixed at 2.0 V while varying the upper charge limit. The temperature was maintained at 25° C. during cycling of the LRCO cathode thin film battery.
[0097] As shown in Figures 20A-B and 21A-B, the annealed thin films have lower capacity than the as-deposited non-annealed films described previously. The lower capacity is attributed to the shift of the lithiation potential to higher potentials in the crystalline state. For both annealing temperatures (450°C and 650°C), increasing the charging potential to 4.0 V significantly increases the specific capacity / specific energy. As discussed in Figures 14A-D, after annealing, non-uniform crystalline grains grew. The non-uniform crystalline grains after annealing vary in size from about 50 nm to about 600 nm, which hinders effective Li-ion transport and reduces the coulombic efficiency. Large grains may undergo large volume changes during cycling, which may subsequently cause the structure to collapse and short circuit. The large grain size may be the reason why the annealed cathodes show lower coulombic efficiency, increased capacity fade, and eventually short circuit.
[0098] Example 2 (1-x)Li 2 RuO 3 +xLiCoO 2 +yLi 2 Lithium ruthenium cobalt oxide (LRCO) cathode material with the chemical formula of 0, where Y is between about 0.05 and 0.6, and X is between about 0.05 and 0.5, was used to prepare low temperature energy dense cathode thin films. The LRCO thin films were prepared by RF magnetron sputtering and shown to be smooth, uniform and electrochemically active without further thermal annealing, and thin film batteries on flexible thermoplastic substrates could be successfully fabricated and operated. 39 μAh cm -2 μm -1 Compared to lithium cobalt oxide (LCO) coatings, which have a specific capacity of 110 μAh cm at 0.3 C rate, LRCO has a specific capacity of 110 μAh cm at 0.3 C rate. -2 μm -1 and over 92% capacity retention over 150 cycles. This discharge capacity is close to the optimized theoretical capacity (67 μAh cm) of annealed polycrystalline LCO. -2 μm -1 ) even exceeds
[0099] LRCO was prepared by conventional solid-phase synthesis. 2 CO 3 (Alfa Aesar, 99.9% purity, 35% excess by weight), RuO 2 (Alfa Aesar, 99.9% purity) and CoCO 3 (Alfa Aesar, 99.9% purity) precursor was mixed with the desired stoichiometry ((1-x)Li 2 RuO 3 -xLiCoO 2 -yLi 2 The mixture was weighed according to the formula (I) and mixed with anhydrous acetone (Alfa Aesar) and ground in a planetary ball mill (DECO, PBM-V-0.4L). 2 CO 3 was included to compensate for Li loss during high temperature annealing and / or subsequent sputtering. The powder mixture was heated in a muffle furnace (air atmosphere) at a rate of 2°C / min to a temperature of 1000°C, held for 12 hours, and then cooled under ambient conditions.
[0100] A 2-inch sputtering target for thin film deposition was prepared by high temperature sintering of the synthetic LRCO powder. First, the LRCO powder chunks were crushed using a mortar and pestle. The fine powder was then mixed with a solution of 5 wt% polyethylene oxide (PEO) in N,N-dimethylformamide (DMF) binder solution, and the mixture was then heated to 70°C to remove the DMF solvent. The LRCO and PEO binder mixture was cold pressed into a 2-inch (5.08 cm) diameter die at 48 MPa for 5 minutes. The pellet was then removed from the die, placed in a clean alumina pan, and sintered in a muffle furnace at 900°C for 5 hours. After the sintered target was cooled sufficiently, it was attached to a copper backing plate (OHFC) using silver-filled vacuum grade epoxy (Dynaloy, KL-325K). The target was cured at 70°C under vacuum before being placed in the sputtering chamber.
[0101] LRCO and LCO thin films were fabricated by RF magnetron sputtering in a custom-built reduced pressure deposition chamber. An LCO sputtering target (99.9% purity) with a size of (2.00 in. (5.08 cm) diameter x 0.125 in. (0.3175 cm) thickness) was purchased from Kurt J. Lesker. The process parameters for RF magnetron sputtering are provided in Table 1. Optical grade fused quartz slides (AdValue Technology, FQ-S-001, 2.54 x 2.54 x 0.1 cm) were used as substrates for all thin film cell assemblies. Prior to the deposition of the thin film cathode, 100 nm thick Pt was deposited as a cathode current collector by direct current (DC) sputtering (Denton Vacuum DESK-II DC Sputtering System). 0.6 cm 2 Thin film cathodes with areas of 0.1 nm to 0.5 nm were typically deposited to a thickness of 300 nm and confirmed by scanning electron microscopy (SEM). TIFF2024538118000003.tif86170
[0102] Ultra high purity N 2 2 inch (5.08 cm) Li in atmosphere 3 PO 4 Thin films (1 μm and 5 cm thick) of lithium phosphate oxynitride (LiPON) were deposited by radio frequency (RF) magnetron sputtering of a powder target (99.95%, Kurt J. Lesker). 2 ) was deposited directly on top of the cathode layer. Prior to deposition, the custom-built sputtering chamber was pumped to approximately 5×10 -7 The deposition was performed with a 2 μm thick Li metal as the anode and current collector, and the deposition pressure was pumped to 1000 MPa (1.0 MPa) at 100 MPa (1.0 MPa). The deposition pressure was 100 MPa (1.0 MPa) at 100 MPa (1.0 MPa) and the deposition pressure was 100 MPa (1.0 MPa). The deposition pressure was 100 MPa (1.0 MPa) at ... -7 Thermal evaporation was performed in a custom-built vacuum chamber with a base pressure of 1000 Torr. The Li deposition rate was monitored in-situ using a quartz crystal monitor (QCM). A schematic diagram of the thin-film battery fabrication process is shown in Figure 28.
[0103] Materials characterization Inductively coupled plasma mass spectrometry (ICP-MS) was performed using a Perkin Elmer NexION 200 to identify the chemical composition of the LRCO target. Powder X-ray diffraction (XRD) and thin film XRD were performed using a Rigaku Synergy-S diffraction system and a Bruker D8 Advance system, respectively, with a CuKα microfocus X-ray source to determine the structure of the LRCO powder and thin films. XRD patterns were refined by MDI Jade 9 software. X-ray photoelectron spectroscopy (XRS) was performed using a Krato Axis Ultra DLD XPS system with a monochromated Al Kα source at 15 kV and 10 mA. Survey scans were performed with a pass energy of 160 eV from 1200 to 5 eV in 1 eV increments. For calibration, the aliphatic C 1s peak was assigned to 284.6 eV. Ten high-resolution scans were used with a pass energy of 20 eV for O 1s, Ru 3d, and Co 2p. Detailed peak deconvolution was analyzed by CasaXPS software. For postmortem analysis, the cells were carefully disassembled in an Ar-filled glove box. All samples were placed in hermetically sealed plastic bottles and then transferred to the various analytical systems. Scanning electron microscopy (SEM) and energy dispersive X-ray spectroscopy (EDS) were performed on a ZEISS Crossbeam 340 FIB-SEM system using an accelerating voltage of 7.5 kV. To analyze the cross-sections of the samples, the sample substrates were manually broken.
[0104] Electrochemical characterization The thin-film battery was cycled using a battery cycler (BT-2043, Arbin Instruments) under various charging potentials in an Ar-filled glove box. The electrode area was defined by the geometric area of the cathode side. Cyclic voltammetry was performed reversibly from 2.0 V to 3.9 V at a scan rate of 0.1 mV / s. 3, 10, 15, 27, 33, and back to 3 μA / cm. 2In Li / Li + A rate capability test (five cycles as one ramp period) was used at 25° C. with 2.0 to 3.9 V (LRCO) and 3.0 to 4.2 V (LCO) vs.
[0105] Structural and morphological characterization For structural and morphological characterization, LRCO thin films were first prepared on flat model Si wafer substrates. To prevent possible interdiffusion of Li into Si during sputtering, the Si wafer was coated with a 300 nm thick thermal oxide layer. Figures 23A and 23B provide a conceptual illustration of the LRCO film morphology based on the corresponding SEM characterization. The film morphology strongly depends on the sputtering target-substrate distance. A typical distance of 5 cm was first used to sputter LRCO thin films, and the morphology shown in Figure 23A was obtained. Surprisingly, LRCO was deposited as columns separated by voids, which may increase the possibility of short circuits in the completed thin-film battery due to incomplete coverage by the thin-film electrolyte. Moreover, the columnar morphology increases the contact area and non-uniformity of the contact surface between the electrolyte and the cathode, leading to non-uniform Li-ion transport through the cathode. Increasing the sample distance during deposition from 5 cm to 10 cm results in an isotropic, smooth, featureless film as shown in FIG. 23B; the columnar morphology disappears (FIGS. 24A-B). At longer sputtering deposition distances, the kinetic energy of the sputtered atoms is reduced through atom-atom collisions, resulting in moderate surface temperatures and preventing crystallization during deposition. Although the deposition rate was reduced from 20 nm / min (at a distance of 5 cm) to 5 nm / min (at 10 cm), a featureless cathode surface is beneficial, allowing for a more uniform Li-ion flux transport (FIG. 26).
[0106] Turning now to Figures 24A-24B, scanning electron micrographs of two fields of a thin film deposited from a sputtering target formed from LRCO material are depicted. The first field of view, Figure 24A, is a plan view of a thin film deposited using a LRCO-2 sputtering target at a sputtering target-to-substrate distance of 5 cm. The second field of view, Figure 24B, is a cross-sectional view of a thin film deposited from a LRCO-2 sputtering target at a sputtering target-to-substrate distance of 5 cm. As mentioned above, an unexpected finding is that the morphology of the deposited thin film depends on the distance between the substrate and the target during sputtering. As shown in Figures 24A-24B, at a sputtering distance of 5 cm, the thin film develops with a columnar / particulate morphology, resulting in significant film roughness. However, at 10 cm, the film is uniform, smooth, and has no obvious surface topography. Functional cathode thin films can be prepared at both distances. For the thin film cell electrochemical data contained herein, a sputtering distance of 10 cm was used.
[0107] The LRCO target is ((1-x)Li 2 RuO 3 -xLiCoO 2 -yLi 2 0.79Li), where x is the content of Co in the target and y is the ratio of excess Li in the target. 2 RuO 3 -0.18LiCoO 2 -0.66Li 2The chemical composition of the LRCO target, O, was confirmed by ICP-MS (see Table 2). For the liquid coin cells, a slurry was prepared by adding a binder solution containing 10 wt. % PVDF in N-methyl-2-pyrrolidone (NMP) solvent to the LRCO powder mixture containing 80 wt. % active material and 10 wt. % Super P carbon. The slurry was cast onto an Al foil current collector and dried overnight at 100 °C under vacuum before assembling the cell. Metallic Li foil (1.9 mm × 0.75 mm, 99.9%, Alfa Aesar) was ground, rolled, and cut into disks with a diameter of 1.43 cm and placed on a slightly larger diameter microporous separator (fiberglass) that served as a spacer to define the separation of the electrodes. The electrolyte used was 100 μl of 1.0 M LiPF in 1:1:1 EC:EMC:DMC. 6 (Gotion). The coin cells were cycled from 2.0 V to 4.5 V using a battery cycler (BT-2043, Arbin Instruments). The first two cycles were set at 0.02 C rate as the formation period. The cell temperature was controlled at 25 °C. Excess Li was added to the target to compensate for Li loss during high temperature firing of the sputtering target and long distance sputtering deposition. Since lithium is the lightest metallic element, it is expected that the increase in substrate-target distance will reduce the lithium to transition metal ratio and decrease the sputter yield in the final coating composition. The Ru:Co atomic ratio of 4:1 was confirmed by EDS (provided in Figure 27), showing a match between the target and the sputtered sample. Therefore, (0.8Li 2 RuO 3 -0.2LiCoO 2 -xLi 2 The general composition of ZnO was assigned to all the LRCO thin film cathodes prepared in this study. TIFF2024538118000004.tif48170
[0108] To study the crystallinity and microstructure of the LRCO thin films, XRD was performed on smooth featureless films (deposited at a distance of 10 cm). The XRD patterns of the precursor LRCO powder for the sputtering target, the LRCO thin film and the substrate (thermal oxide on Si wafer) are provided in Figure 25. The XRD spectrum of the LRCO target shows monoclinic Li 2 RuO 3 Structure (PDF# 01-072-4645) and hexagonal LiCoO 2 The structure was assigned (PDF# 01-073-0964, diffraction data publicly available at the International Center for Diffraction Data database, icdd.com). Space group Li with TIFF2024538118000005.tif5170 2 RuO 3 and space group LiCoO with TIFF2024538118000006.tif5170 2 The synthetic LRCO target was formed from a solid solution of hexagonal α-NaFeO 2 type structure, in which six RuO 6 LiO with one interstitial octahedron 6 This encloses the octahedron, thereby forming LiRu in the TM layer. 6 The crystal planes (020) and (111), which are considered to be superlattice peaks, are monoclinic Li 2 RuO 3 For the LRCO thin film, three diffraction peaks (stars) are due to the SiO 2The peaks in the LRCO film are assigned to the layer, and all the remaining peaks can be assigned to the corresponding LRCO characteristic reflections. Broad amorphous diffraction peaks are not prominent in the diffractogram, and three LRCO crystal planes, including (113), (202), and (312), can be assigned to the target. Although SEM suggests that the film is amorphous, the sharp (113) reflection found in the LRCO film indicates that the as-deposited thin film is at least partially crystalline (no post-deposition annealing was performed). This crystallinity likely arises from heat accumulated on the substrate during the sputtering process. This thermal energy promotes the rearrangement of absorbed Li, Ru, Co, and O atoms. Compared to the fully crystalline LRCO sputtering target, the broad full width at half maximum of the (202) and (312) planes suggests the presence of nanocrystalline LRCO phase in the film, demonstrating that the as-prepared LRCO thin film is a mixed composition of amorphous and nanocrystalline structures.
[0109] Electrochemical characterization of as-deposited LRCO in TFB By sequentially depositing Pt, LRCO, LiPON and Li metal coatings on a quartz substrate, a LRCO TFB was successfully fabricated, as shown by the 3D schematic in FIG. 28 and the SEM micrographs in FIG. 29A-D. A digital photograph of the thin-film cell is provided in FIG. 30. A thermally evaporated Li metal anode, approximately 2 micrometers thick, was the last layer deposited on the TFB and was not coated with a protective layer. Inevitable air exposure during sample transfer results in the Li surface being oxidized and non-conductive, resulting in a charged center of the Li layer observed in the SEM photographs. Under this Li metal layer, the SEM and corresponding phosphorus mapping clearly show a dense and intact LiPON layer with a thickness of 1 μm. The EDS mapping of ruthenium (FIG. 29A-D), in combination with the SEM micrographs, demonstrated a featureless layer of 300 nm thick LRCO thin-film cathode. Since the LRCO coating is the thinnest, the EDS mapping intensity of Ru was not as strong as that of P or Si, but the coating boundaries can be discerned. A Pt layer (100 nm thick), deposited by direct current (DC) sputtering, served as the cathode current collector. The EDS map of Si clearly shows the location of the quartz substrate.
[0110] For each charging potential, the cell exhibits a sloped voltage profile (FIGS. 17A-17C). Given the amorphous / nanocrystalline nature of the LRCO film, the lack of a flat voltage plateau characteristic of a two-phase reaction is expected. Using differential capacitance analysis (FIG. 31), a Ru 4+ / 5+ The contribution of the oxidized couple is resolved; this is responsible for the majority of the cathode capacity. 3+ / 4+ An oxidation peak of is also seen at 3.7 V. This data demonstrates that both Ru and Co redox contribute to the capacity of the cathode.
[0111] All cells demonstrated excellent performance over the first 100 cycles, but extended cycling reveals important differences in the failure modes of the LRCO cathodes charged to 3.9 V and 4.0 V (Figure 31). + The cell charged to 3.9 V vs. 10 V showed 71.9% capacity retention over 300 cycles (FIG. 32A), further demonstrating the stability of LRCO at this potential. Degradation of the Li metal coating over the long-term testing in the glove box (over 3 months) is, in part, responsible for the capacity fade. Without coating the Li metal with a protective layer, which is critical to achieving stable cycling over an extended time frame and / or thousands of cycles, chemical reactions of the Li metal were visually evident in the imperfect atmosphere of the glove box. At a charge potential of 4.0 V, long-term cycling up to 300 cycles was attempted. Several cells were fabricated and, rather than slow capacity fade, sudden failure was observed for each cell upon charging to 4.0 V. Representative cycling behavior of three cells is presented in FIG. 32B, which includes the champion cell data from FIG. 18B. Each of these cells suddenly failed through a short circuit, suggesting that the integrity of the LiPON layer was compromised. One possibility is that at high potentials, structural instability of the cathode, combined with potential molecular oxygen release, leads to structural collapse of the coating, causing the LiPON to break down. In these materials, two oxidation processes occur when charged at high potentials: TIFF2024538118000007.tif6170 anionic redox reaction followed by irreversible formation of molecular oxygen can be ensured. The high capacity of anionic redox active cathode materials comes from cumulative cationic and anionic redox processes. However, the appearance of peroxo / superoxol-like species during the anionic redox reaction leads to the nucleation of disordered phases, which further irreversibly modify the oxygen crystal network that develops in the next discharge step, resulting in permanent damage to the cathode structure. Although no clear evidence of oxygen release is observed in the profiles, possibly due to the nanocrystalline nature of the coating, the key conclusion from the cycling is that at 3.9 V, stable cycling is provided with state-of-the-art capacity, which is better than state-of-the-art thin film materials (see Figure 36). Charging to 4 V or higher can extract more capacity at the expense of stability.
[0112] To further understand the redox contributions of both Co and Ru in the cycling behavior of the cathode, additional electrochemical characterization of the as-deposited LiCoO was carried out. For comparison, non-annealed LiCoO 2 (LCO) thin films were also prepared and characterized. Cyclic voltammetry (CV) of both LRCO and LCO at a scan rate of 0.1 mV / s is provided in Figure 34. The small peak at about 3.5 V corresponds to the Ru 4+ / Ru 5+ The redox couple Ru and Co can be assigned to the redox couple Ru+ and Co+, and another sharp peak at about 3.7 V corresponds to the oxidation of Co from 3+ to 4+. The oxidation of Ru and Co compensates for charge neutrality as Li is extracted from the cathode during charging. During the cathode scan, Co 4+ / Co 3+ and Ru 5+ / Ru 4+ These two reduction peaks for O merge into a broad peak range from about 3.8 to 3.5 V. Importantly, there is no indication of oxygen oxidation in the voltammograms. Oxygen oxidation would be expected to appear if the anodic scan extended beyond 4.0 V, potentially resulting from the oxidation of O. 2This is accompanied by the formation of gases, which can irreversibly destroy the cathode structure or compromise the integrity of the thin-film battery. + An upper limit of 3.9 V vs. LiCoO is considered to be a safety limit for these cells, which not only provides approximately the same capacity as a 4.0 V charge, but also ensures that only transition metal redox reactions occur. As a reference, the LCO thin film exhibits a similar redox trend starting at about 3.5 V, with the broad anodic peak attributed to Li-ion deintercalation. The differential charge capacity data in Figure 33B shows that the as-deposited LiCoO 2 It shows that lithium desorption of 1000 volts can provide a charge capacity of 8.6 μAh. The reduction peak at about 3.6 V can be attributed to the intercalation of Li ions (Figure 34). Furthermore, the CV curve of the as-deposited LCO can be found in Figure 33A, which shows a voltage range of 3.0-4.2 V at a scan rate of 0.1 mV / s, but exhibits a sluggish electrochemical activity and low current density compared to LRCO.
[0113] In addition to CV, we also cycled TFB with 300 nm thick as-deposited LCO films; the results are reported in Figure 35. Under the same current density as LRCO, LCO shows comparable capacity retention of 90.6%, but after 175 cycles, it is only 38.6 μAh / cm 2 The performance of these as-deposited LCO thin film cathodes is similar to that reported previously. The low capacity is attributed to the disordered crystalline microstructure and slow Li-ion diffusivity.
[0114] The comparative graph in Figure 36 summarizes the electrochemical performance comparison between typical inorganic thin film cathodes along with the annealing temperature. Most inorganic thin film cathodes are polycrystalline and undergo high temperature annealing during or after deposition to obtain the electrochemically optimal crystal structure and film texture. In LCO films, for example, annealing above 600 °C results in a favorable microstructure with the (101) / (104) plane perpendicular to the substrate, providing efficient ion transport and high discharge capacity. Under optimal fabrication processing reported by the Oak Ridge National Laboratory group, high temperature annealed LCO achieves a current of 100 μA / cm 2 At a current density of 60 μAh / cm 2 The LCO thin film cathode exhibits an initial discharge capacity of 10 μA / cm and achieves a capacity retention of over 99.0% over 1000 cycles (Figure 36). The LCO thin film cathode annealed at less than 500 °C exhibits a current of 10 μA / cm 2 At a current density of only 54 μAh / cm 2 The LRCO thin-film cathode provides a specific capacity of 100-μm and 92.6% capacity retention over 140 cycles. Although annealing is important for optimizing performance, it also constrains the substrate material and increases the number of processing steps in thin-film battery fabrication. On the other hand, the as-deposited LRCO thin-film cathode does not require thermal annealing and provides a capacity of 104.2 μAh / cm when charged to 3.9 V. 2 36. On the other hand, the as-deposited LiV gave exceptional specific capacitance of 1.0-μm and 94.4% capacity retention over 100 cycles, outperforming other common inorganic thin film cathodes presented in Figure 36. 3 O 8 is 10μA / cm 2 At a rate of 133 μAh / cm 2 It can provide an initial discharge capacity of 100-μm, but a lower capacity retention of 78.8% over 100 cycles. 2 O 5 is 5μA / cm 2 At a current density of 109 μAh / cm 2Although it exhibits a low capacitance retention over 100 cycles, a low capacitance retention of 90.5% is achieved for LRCO. 2 O 5 Because the cathode is not naturally lithiated and, as such, is incompatible with anode-free cell designs, the as-deposited LRCO cathode offers a compelling combination of specific capacity and reversibility (capacity retention).
[0115] Demonstration of flexible TFB By possessing high specific capacity in as-deposited nanocrystalline morphology, LRCO expands the range of compatible substrates for thin-film batteries. Besides typical rigid inorganic substrates such as silicon, quartz and alumina, low-cost flexible thermoplastic substrates can be used as substrates. This has been demonstrated using polyethylene terephthalate (PET) and polyimide (Kapton®) coatings as substrates. Figure 38A shows the cycling performance of a thin-film battery fabricated on a PET substrate. When bending is imposed on the PET throughout the cycling process, LRCO achieves a specific capacity of 101.5 μAh / cm 2 The TFB provides a discharge capacity of 100-μm and 97.5% capacity retention over 120 cycles. To further demonstrate the stability and flexibility of the cells on these flexible substrates, the same cells (after 120 cycles) were used to power micro-LEDs. The TFB successfully powered LEDs in flat (FIG. 39A) or bent configurations (FIG. 39B), demonstrating the versatility of the LRCO material for many applications. The continuous operation of the LED as a function of various bending angles, as well as the evolution of the open circuit voltage under bending and at rest, are shown in FIG. 37.
[0116] As another attractive alternative, Kapton® coating can be used over a much wider temperature range (-250 to 400°C). To further demonstrate the exceptional flexibility and mechanical stability of the as-deposited LRCO TFB, Kapton® coating was also used as the substrate layer. To add and compare the effect of bending on the cell operation, the Kapton®-based TFB was left in a flat conformation for the first 60 cycles and then bent for the subsequent cycles (Figure 38B). No obvious change in capacity or capacity retention was observed after the first 60 cycles, further providing flexibility to the battery. A capacity retention of 93.0% over 120 cycles was obtained, which is slightly lower than the 97.5% using PET. The comparable and competitive performance on both substrates, especially against traditional inorganic substrates, reinforces the importance of low-temperature preparation of LRCO.
[0117] The capacity retention vs. capacity diagram in Figure 40 represents an electrochemical performance comparison between inorganic thin film cathodes on flexible substrates. In some instances, high temperature annealing was still used and these annealing temperatures are included in the plot. High temperature annealing is used to improve the electrochemical properties of inorganic substrates, e.g., LiMn 2 O 4 Stainless steel foil (annealed at 700°C) in the case of Li 4 Ti 5 O 12 This is possible using zirconia sheets (annealed at 800 °C) in the case of LCO. Another strategy uses a coating peeling and transfer method. LCO deposited on mica and annealed at 700 °C was transferred to a flexible polydimethylsiloxane (PMDS) substrate, resulting in a reasonable but reduced cathode capacity (67 μAh / cm for LCO). 2 The authors provide a novel fabrication technique to obtain a theoretical volume of 100-200 μm. However, high temperature annealing limits the alternative options for a variety of flexible, low-cost thermoplastic sheets. When fabricated at room temperature on a polyimide substrate, LiNi 0.5 Mn 1.5 O 4has a reasonable capacity retention of 87.5% after 20 cycles, but 2 -μm. 3 is the specific capacity (155 μAh / cm in the first cycle) 2 LRCO is the only room temperature prepared cathode with a capacity (104.1 μAh / cm) superior to LRCO, but is marred by a limited capacity retention of 51% after 100 cycles. In comparison, as-deposited LRCO can be simply fabricated directly on flexible thermoplastic substrates (PET and Kapton®) and has an initial capacity (104.1 μAh / cm 2 The nanotube nanofibers offer a desirable combination of 0.1-μm nanofibers and high capacity retention of 95.3% over 100 cycles.
[0118] Developing a high specific capacity, long cycle life cathode that does not require high temperature post-deposition treatment will enable multi-cell vertically stacked battery configurations. The ionic conductivity of LiPON is known to degrade significantly above about 350 °C. If post-deposition annealing of the cathode is required, this high temperature treatment would prevent the sequential deposition of multiple cells into high voltage series batteries. By using a non-annealing LRCO cathode in the cell design, multiple cells can be sequentially deposited on a single substrate to produce a multi-cell TFB. In such a design, the mass ratio of substrate to active material can be dramatically reduced, resulting in a higher overall battery specific energy.
[0119] result LRCO thin film cathodes were successfully fabricated and demonstrated in thin film cells. As the distance between the sputtering target and the substrate increased, a smooth isotropic film was deposited, which is important for the uniformity of ion transport. XRD suggests that the LRCO film is nanocrystalline due to the presence of characteristic LRCO reflections. The oxidation states of 3+ and 4+ for cobalt and ruthenium were confirmed by XPS, respectively. After fabricating the LRCO TFB on the fused quartz substrate, the highest charging potential for optimal cycle life was also tested. Starting from 3.8 V, the specific capacity and capacity retention increased as the charging cutoff potential increased, and the Li / Li + At a charging potential of 4 V, 2 At a current density of up to 111.7 μAh / cm 2 94.4% over 100 cycles at 100 μm. To avoid the structural instability of LRCO at high potentials, the Li / Li + The charging potential of 3.9 V vs. 0.1 V provides a stable compromise between specific capacity and reversibility. Given the low temperature preparation of the as-deposited LRCO, completed thin-film batteries were also fabricated directly on flexible plastic substrates without further ex situ annealing. 2 Excellent specific capacity and capacity retention, as high as 97.5%, were achieved over 120 cycles. The excellent performance of as-deposited LRCO, substrate versatility, and potential for non-annealing multi-cell battery configurations may enable the utilization of TFB in future flexible applications.
[0120] conclusion As discussed herein, LRCO thin film cathodes have been shown to have improved performance when incorporated into solid-state thin film batteries. As-deposited amorphous LRCO films have been shown to provide good charge capacity and electrochemical reversibility. Non-annealed LRCO has a charge capacity of 110 μAh / cm 2It has been shown that annealed LRCO films provide discharge capacities of over 100-μm, which is nearly twice the specific energy of LCO thin film cathodes. Non-annealed LRCO films also offer the possibility of developing thin film batteries on flexible / polymeric substrates. Improvements in LRCO energy storage properties can be achieved through crystallization. However, annealed films have been shown to exhibit rapid grain growth and a coarse, particulate film morphology.
[0121] The absence of high temperature annealing associated with traditional lithium battery cathode production allows for the use of a wide variety of substrate materials, including substrates made from flexible thermoplastic materials. Lithium batteries with flexible substrate cathodes can be used in traditional battery applications. Lithium batteries with flexible substrate cathodes can also be used in new applications requiring device flexibility, such as wearable, flexible consumer electronics. The novel flexible cathode materials disclosed herein enable the development of flexible electronic devices requiring battery components to be flexible.
[0122] The energy density of existing flexible batteries remains low due to limitations on material thickness and total electrolyte loading.The emergence of high-performance flexible thin-film batteries will accelerate the development of next-generation fully flexible electronic systems in combination with existing flexible components such as displays, memory, interactive user interfaces and LEDs.The flexible batteries disclosed herein exhibit high electrochemical performance and excellent mechanical deformability by being provided on flexible low melting temperature substrates.
[0123] It will be understood that variations of the above-disclosed and other features and functions, or alternatives thereof, may be combined into many other different systems or applications. Various presently unforeseen or unanticipated alternatives, modifications, variations or improvements thereon may subsequently be made by those skilled in the art which are intended to be encompassed by the following claims.
[0124] While the forgoing is directed to embodiments of the present disclosure, other and further embodiments of the disclosure may be devised without departing from the basic scope thereof, which is determined by the following claims. Tables 3 and 4 References TIFF2024538118000008.tif215170TIFF2024538118000009.tif87170
Claims
1. 1. An energy storage device, comprising: a cathode comprising an anion redox active material, the anion redox active material comprising one or more of lithiated ruthenium oxide and lithiated iridium oxide, and one or more lithium metal oxides, the lithium metal oxides comprising one or more of iron, cobalt, nickel, manganese, tin, titanium, palladium, silver, zinc, gallium, indium, and vanadium; an anode disposed adjacent to the cathode; and An electrolyte disposed between the cathode and the anode 16. An energy storage device comprising:
2. 10. The energy storage device of claim 1 , wherein the lithium metal oxide comprises one or more of iron, cobalt, nickel, manganese, tin, titanium, and vanadium.
3. 3. The energy storage device of claim 2, wherein the anion redox active material comprises lithiated ruthenium oxide and the lithium metal oxide is lithium cobalt oxide.
4. 10. The energy storage device of claim 1 , wherein the electrolyte has an electrolyte thickness of about 0.05 μm to about 3 μm.
5. 5. The energy storage device of claim 4, further comprising a current collector, the cathode being disposed between the current collector and the electrolyte.
6. 10. The energy storage device of claim 1 , wherein the cathode is amorphous or nanocrystalline.
7. 10. The energy storage device of claim 1 , wherein the cathode is deposited using PVD.
8. 4. The energy storage device of claim 3, wherein the atomic ratio of lithium to ruthenium is from about 5:1 to about 2:
1.
9. 4. The energy storage device of claim 3, wherein the atomic ratio of lithium to cobalt is from about 21:1 to about 5:
1.
10. 4. The energy storage device of claim 3, wherein the atomic ratio of ruthenium to cobalt is from about 10:1 to about 1:
1.
11. 1. An energy storage device, comprising: Supporting base material; a platinum coating disposed on a portion of a support substrate; a cathode disposed on the platinum coating and comprising lithium, ruthenium, cobalt and oxygen; an anode disposed adjacent to the cathode and comprising lithium; and An electrolyte disposed between the cathode and the anode 16. An energy storage device comprising:
12. 12. The energy storage device of claim 11, wherein the electrolyte is a solid lithium ion conductor.
13. 12. The energy storage device of claim 11, wherein the atomic ratio of ruthenium to cobalt in the cathode is from about 10:1 to about 1:
1.
14. 1. A method of forming an energy storage device, comprising: depositing a cathode coating on a support substrate in a processing region of the processing chamber, the cathode coating comprising lithium, ruthenium, cobalt and oxygen; depositing an electrolyte over the cathode coating; and Depositing an anode over the electrolyte A method comprising:
15. The method of claim 14, wherein the support substrate is separated from the sputtering target in the processing chamber by a sputtering distance of about 5 cm to about 20 cm during deposition of the cathode coating.
16. The method of claim 14 , wherein the process temperature in the process chamber during deposition of the cathode coating is less than about 700° C.
17. 15. The method of claim 14, wherein the cathode coating is deposited using physical vapor deposition, a sputtering target is disposed on an opposing side of the support substrate, the sputtering target comprising lithium, ruthenium, cobalt, and oxygen.
18. The method of claim 14, wherein the atomic ratio of ruthenium to cobalt in the cathode coating is from about 10:1 to about 1:
1.
19. The method of claim 18, wherein the cathode coating has a cathode thickness in the range of about 50 nm to about 40,000 nm.
20. 15. The method of claim 14, wherein the anode is a lithium anode and the electrolyte is a solid lithium ion conductor.
Citation Information
Patent Citations
Lithium ion secondary battery cathode material, preparation method and lithium ion battery
CN104134781A
Battery
CN104638300A
Positive pole material for lithium ion battery and modification method thereof
CN105006564A
Lithium ion power storage device and manufacturing method thereof
CN113035582A
Nonaqueous electrolyte secondary battery
JP1992328259A