Method for producing water-based polyurethane dispersion and its application
The production of aqueous polyurethane dispersants for liquid indigo dyes improves grinding efficiency and dyeing stability, reducing environmental impact and health risks, while ensuring uniform dyeing and reduced water consumption.
Patent Information
- Application Number
- JP2024525004
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-04
- Filing Date
- 2022-01-20
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-01-20
Smart Images

Figure 2024539695000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention is in the field of polymeric dispersants and relates to a method for producing an aqueous polyurethane dispersion and its application in the production of liquid indigo. [Background technology]
[0002] Indigo dye is a kind of dye with simple structure and very low water solubility, mainly used for dyeing and printing jeans.Current indigo dye is mainly in powder form, and powder disperse dye has the advantages of simple packaging, easy transport, good storage stability, strong adaptability to processing equipment, and easy operation.However, indigo dye does not have strong affinity to cotton fiber and is difficult to dye in deep colors, so most of the dye is concentrated on the surface of the fiber.In fact, in the jeans production process in the factory, it is necessary to carry out more than 20 water washing processes to remove color floating and related auxiliaries on the surface of the fabric, which causes a large amount of water consumption and water pollution.In addition, powder indigo dye has the defects of dust pollution during the chemical reaction process and inaccurate paste preparation or liquid preparation measurement, which causes certain harm to people's health.
[0003] As the global trend of green environmental protection is promoted, the concept of ecological environmental protection is gradually incorporated into various industries in society, and the lifestyle of "return to nature, green environmental protection, ecological health" has begun to be advocated by more and more people, and the ecological pollution problem caused by the textile and apparel industry, as a traditional industry that people rely on very much, has always been the focus of global attention, and as the most polluting in the textile and apparel industry, the dyeing and washing process of denim products causes extremely serious pollution of the ecological environment. Liquid indigo dye can eliminate some of the defects of powder disperse dyes, can achieve good dispersion effect with less dispersant, improve the dye utilization rate, and in terms of dyeing or printing, because its dye particles are small, it can improve the dyeing rate and dye deeper colors, and at the same time, make the dye easier to diffuse into the fiber, reduce the color floating on the surface of the fiber, and further reduce the subsequent washing process, and greatly reduce the discharge of printing dyeing wastewater from the source, thereby reducing the amount of dye and related auxiliary agents in the dyeing wastewater, and reduce the environmental damage caused by the dyeing process, realizing the development concept of energy-saving and environmental protection. Therefore, the preparation of liquid dyes has become a hot research topic in recent years. However, there are currently very few studies on the preparation of liquid indigo dyes, and there are problems such as low grinding efficiency during the preparation of liquid dyes, and the nanoscale liquid indigo dyes produced will grow larger during storage, leading to aggregation and precipitation, which causes problems such as non-uniform dyeing and poor reproducibility.
[0004] The key factor to solve the above problem is the structure of the dispersant, and a suitable dispersant structure can not only improve the grinding efficiency of liquid dyes, but also make the liquid dyes have good stability. At present, most of the dispersants used to produce liquid indigo dyes are some low molecular weight anionic and nonionic dispersants, such as naphthalene-based, lignin sulfonate salts, and different polyoxyethylene ether-type dispersants, which can produce nanoscale liquid dyes, but the problems of low grinding efficiency and poor stability still exist. Polymer dispersants have a special anchor group structure, which can not only be firmly adsorbed on the surface of particles, but also provide solvation segments that make the system stable, and have attracted attention. Current polymer dispersants have achieved many beneficial results in the production of liquid pigments and paints. For example, the Chinese Patent Application for Invention with application number CN201910844629.7 (publication number CN110540639A) discloses a parallel-type polymeric aqueous pigment dispersant, the synthesized parallel-type polymeric aqueous pigment dispersant has a comb-shaped branched structure, and contains a naphthalene ring and a peripheral ethylene oxide / propylene oxide polymer long chain, the parallel-type polymeric aqueous pigment dispersant has excellent dispersion stability, storage stability and resolubility for organic pigments, has high grinding efficiency, strong viscosity reduction, and good color development. The Chinese Patent Application for Invention with application number CN202110585011.0 (publication number CN113278111A) discloses a ternary copolymer dispersant, the dispersant of this structure has high grinding efficiency when producing liquid disperse dyes, and good dye storage stability. However, at present, there is little research on polymeric dispersants in the production of liquid indigo, and there is an urgent need to further research and develop new products. Summary of the Invention [Means for solving the problem]
[0005] The object of the invention is as follows: The object of the present invention is to provide a method for preparing a designed and synthesized aqueous polyurethane dispersant and its application, specifically, to successfully prepare a liquid indigo dye with good storage stability by mechanically grinding the synthesized dispersant and powdered indigo dye.
[0006] The technical solution is as follows: The preparation method of the aqueous polyurethane dispersion according to the present invention, the specific operation steps are as follows: (1) Weigh out an isocyanate group-containing compound as an initiator, and react it with polyethylene glycol of a certain molecular weight in the presence of nitrogen and a catalyst at 75 to 80°C for 2 to 2.5 hours to produce a polyurethane prepolymer; Add an appropriate amount of organic solvent to the reaction system to control the viscosity. (2) While keeping the temperature constant, add chain extender 1 and carry out the chain extension reaction for 2 to 2.5 hours. (3) The temperature is kept constant, chain extender 2 is added, and the chain extension reaction is continued for 2 to 2.5 hours. (4) The temperature is lowered to 50 to 55°C, a terminal blocking agent is added, and the terminal blocking reaction is carried out for 1 to 1.5 hours. (5) After the reaction is completed, add an equimolar amount of triethylamine to the chain extender 1 and carry out a neutralization reaction for 1 hour, add an appropriate amount of deionized water and emulsify at high speed for 20 to 30 minutes, and then remove the organic solvent by vacuum distillation at room temperature to finally obtain an aqueous polyurethane dispersion.
[0007] Further, in step (1), the initiator is any one of hexamethylene diisocyanate and isophorone diisocyanate; the polyethylene glycol is either PEG 400 or PEG 600; The molar ratio of the initiator to polyethylene glycol is 4:1 to 1.2.
[0008] Further, in step (1), the catalyst is dibutyltin dilaurate; The amount of the monomer used is 2% by mass to 3% by mass of the two monomers, the initiator and polyethylene glycol.
[0009] Further, in step (1), the organic solvent is either acetone or butanone.
[0010] Furthermore, in step (2), the chain extender 1 is either 2,2-hydroxymethylpropionic acid or 2,2-hydroxymethylbutyric acid; The molar ratio of the initiator, polyethylene glycol, and chain extender 1 is 4:1-1.2:1.2-1.5.
[0011] Furthermore, in step (3), the chain extender 2 is 1-phenyl-1,2-ethylene glycol; The molar ratio of the initiator, the polyethylene glycol, the chain extender 1, and the chain extender 2 is 4:1 to 1.2:1.2 to 1.5:1.2.
[0012] Furthermore, in step (4), the end-capping agent is methyl ethyl ketone oxime, The molar ratio of the initiator, polyethylene glycol, chain extender 1, chain extender 2 and end capping agent is 4:1-1.2:1.2-1.5:1.2:0.2-1.2.
[0013] Further, the aqueous polyurethane dispersion prepared by the above-mentioned preparation method is applied in the preparation of liquid indigo dye.
[0014] Furthermore, the specific process includes the steps of mixing indigo dye, aqueous polyurethane dispersion and water, first pre-grinding in a grinding cup at 1500r / min for 5-10min, then adding zirconia beads, and then continuing to grind in a sand mill at 3000r / min for 1-2 hours to obtain liquid indigo dye.
[0015] Furthermore, the aqueous polyurethane dispersion accounts for 25% to 35% of the dry weight of the indigo dye, the dye content in the liquid indigo dye is 25%, the rotation speed of the sand mill is 3000 to 3500 r / min, and the diameter of the zirconia beads is 1 to 2 mm.
[0016] The beneficial effects are as follows. Comparing the present invention with the prior art, the present invention has the following features: 1. The aqueous polyurethane dispersant prepared in the present invention has a transparent appearance and only a very light yellow color, while the dispersants used in the preparation process of liquid indigo in the current relevant literature are naphthalene-based and lignin-based dispersants, which themselves have a certain color, and the prepared liquid indigo dye inevitably has a coloring effect on the fabric during subsequent dyeing or printing, and the pale yellow and transparent aqueous polyurethane can greatly solve this problem. 2. The liquid indigo dye prepared in the present invention can greatly improve the production environment of the factory, and solve the defects that the dust pollution occurs when the traditional powder dye is weighed, used and transported in large quantities in the factory, which harms the environment, and the weighing and rapid material blending cannot be accurately controlled, and can ensure the physical health of the workers in the workplace and lay the foundation for clean automated production in the future workplace. 3. The aqueous polyurethane dispersant designed and synthesized in the present invention can eliminate the multiple COO in the chain extension process. - As an anchor group, the multi-point anchor of the polymer dispersant can greatly improve the anchoring effect with the dye, and at the same time, the polyethylene glycol chain end is connected to the polyurethane dispersant as a solvation segment, and the chain end can function as a good solvation chain end, which not only has good compatibility with the aqueous medium, but also can generate sufficient steric hindrance and effectively prevent the re-aggregation of dye particles. At the same time, the NH, C=O structure of the carbamate structure of the polyurethane forms a hydrogen bond with the NH, C=O of the indigo dye structure, which can further improve the binding force between the dispersant and the dye particles, and the introduction of 1-phenyl-1,2-ethylene glycol introduces a benzene ring structure with strong planarity and containing π-π bonds, which further increases the steric hindrance of the dispersant, thereby preventing the collision and aggregation between the dye particles and obtaining a stable system. 4. The dispersant designed and synthesized in the present invention has high grinding efficiency when producing liquid disperse dyes, and the storage stability of the nano-scale dye is good, and its dyeability is greatly improved compared with that of powder dyes. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is an operational flow chart of the present invention. [Diagram 2] FIG. 2 is an infrared spectrum diagram of the aqueous polyurethane dispersion prepared in Example 1 of the present invention. [Diagram 3] FIG. 3 is a particle size diagram and an SEM photograph of the liquid indigo dye particles according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will now be further described with reference to the drawings and specific examples.
[0019] As shown in the figure, the method for preparing the aqueous polyurethane dispersion according to the present invention is as follows: (1) Weigh out an isocyanate group-containing compound as an initiator, and react it with polyethylene glycol of a certain molecular weight in the presence of nitrogen and a catalyst at 75 to 80°C for 2 to 2.5 hours to produce a polyurethane prepolymer; Add an appropriate amount of organic solvent to the reaction system to control the viscosity. (2) The temperature is kept constant (75 to 80°C), chain extender 1 is added, and the chain extension reaction is carried out for 2 to 2.5 hours. (3) The temperature is kept constant (75 to 80°C), chain extender 2 is added, and the chain extension reaction is continued for 2 to 2.5 hours. (4) The temperature is lowered from 75 to 80°C to 50 to 55°C, a terminal blocking agent is added, and the terminal blocking reaction is carried out for 1 to 1.5 hours. (5) After the reaction is completed, add an equimolar amount of triethylamine to the chain extender 1 and carry out a neutralization reaction for 1 hour, add an appropriate amount of deionized water and emulsify at high speed for 20 to 30 minutes, and then remove the organic solvent by vacuum distillation at room temperature (the normal temperature is 25°C) to finally obtain an aqueous polyurethane dispersion.
[0020] Further, in step (1), the initiator is either hexamethylene diisocyanate or isophorone diisocyanate, preferably isophorone diisocyanate; The polyethylene glycol is either PEG 400 or PEG 600, preferably PEG 400; The molar ratio of the initiator to polyethylene glycol is 4:1 to 1.2, and preferably 4:1.
[0021] Further, in step (1), the catalyst is dibutyltin dilaurate; The amount of the monomer used is 2% by mass to 3% by mass of the two monomers, the initiator and polyethylene glycol, and is preferably 2% by mass.
[0022] Further, in step (1), the organic solvent is either acetone or butanone, preferably acetone.
[0023] Furthermore, in step (2), the chain extender 1 is either 2,2-hydroxymethylpropionic acid or 2,2-hydroxymethylbutyric acid, preferably 2,2-hydroxymethylbutyric acid; The molar ratio of the initiator, polyethylene glycol, and chain extender 1 is 4:1 to 1.2:1.2 to 1.5, and preferably 4:1:1.5.
[0024] Furthermore, in step (3), the chain extender 2 is 1-phenyl-1,2-ethylene glycol; The molar ratio of the initiator, polyethylene glycol, chain extender 1, and chain extender 2 is 4:1 to 1.2:1.2 to 1.5:1.2, and preferably 4:1:1.5:1.2.
[0025] Furthermore, in step (4), the end-capping agent is methyl ethyl ketone oxime, The molar ratio of the initiator, polyethylene glycol, chain extender 1, chain extender 2 and end capping agent is 4:1-1.2:1.2-1.5:1.2:0.2-1.2, and preferably 4:1:1.5:1.2:0.6.
[0026] Further, the aqueous polyurethane dispersion prepared by the above-mentioned preparation method is applied in the preparation of liquid indigo dye.
[0027] Furthermore, the specific process includes the steps of mixing indigo dye, aqueous polyurethane dispersion and water, first pre-grinding in a grinding cup at 1500r / min for 5-10min, then adding zirconia beads, and then continuing to grind in a sand mill at 3000r / min for 1-2 hours to obtain liquid indigo dye.
[0028] Furthermore, the aqueous polyurethane dispersion occupies 25% to 35% of the dry weight of the indigo dye, preferably 27%, the dye content in the liquid indigo dye is 25%, the rotation speed of the sand mill is 3000 to 3500 r / min, preferably 3000 r / min, and the diameter of the zirconia beads is 1 to 2 mm, preferably 1 mm.
[0029] Example 1 (1) Synthesis of aqueous polyurethane dispersion The molar ratio of six monomers, namely initiator, polyethylene glycol, chain extender 1, chain extender 2, end capping agent, and neutralizer, was calculated to be 4:1:1.5:1.2:0.6:1.5. 1 mol of polyethylene glycol 400 was added to a three-neck flask equipped with a stirrer and a reflux condenser. The three-neck flask was fixed to an oil bath, the temperature was raised to 120°C and vacuum dehydrated for 1 h, then the temperature was lowered to 75°C, 4 mol of isophorone diisocyanate and 2% by mass of dibutyltin dilaurate of the above two monomers were added, and nitrogen was blown in for 5 min to react for 2 h to produce a polyurethane prepolymer. Add an appropriate amount of acetone to control the viscosity, keep the temperature constant, add 1.5 mol of chain extender 2,2-hydroxymethylbutyric acid to carry out chain extension reaction for 2 hours, add 1.2 mol of chain extender 1-phenyl-1,2-ethylene glycol to carry out chain extension reaction for 2 hours at the same temperature, lower the temperature to 50°C, add 0.6 mol of methyl ethyl ketone oxime to carry out end-capping reaction for 1 hour, add 1.5 mol of triethylamine to carry out neutralization reaction for 1 hour after the reaction is completed, add an appropriate amount of deionized water to emulsify at high speed for 20 minutes, and remove acetone by vacuum distillation at room temperature to obtain an aqueous polyurethane dispersant.
[0030] The infrared spectrum of the aqueous polyurethane dispersion prepared in Example 1 is shown in FIG. 2. As can be seen from FIG. 2, -1 is the urea bond, urethane bond, and C=O stretching vibration peak on DMBA, and 2970 cm -1 belongs to the inverse symmetric stretching vibration peak of CH in 1-phenyl-1,2-ethylene glycol and IPDI, and is located at 1090 cm -1 The peak at 1,460 cm corresponds to the polyethylene glycol C-O-C bond stretching vibration peak. These characteristic peaks prove the presence of a carbamate structure. -1 The peak at 1560 cm corresponds to the CH deformation vibration peak of the methyl group and the CH shear vibration peak of the methylene group. -1 The peak at 2260 cm corresponds to the mixed peak of CC stretching vibration, CN stretching vibration, and NH in-plane bending vibration. -1The areas before and after this are characteristic absorption peaks of -NCO, and the peak values are weak, indicating that -NCO in IPDI was almost completely involved in the reaction.
[0031] Comparing the aqueous solution of the aqueous polyurethane dispersion prepared in Example 1 with the aqueous solutions of conventional dispersants, the aqueous polyurethane dispersions are generally transparent and pale yellow in appearance, whereas the naphthalene-based and lignin-based dispersants are dark brown in color.
[0032] (2) Application of aqueous polyurethane dispersion in the production of liquid indigo dye The polymer dispersant prepared in step (1) and deionized water were put into a grinding cup, and the mixture was pre-ground at 1500 r / min for 10 min, then indigo dye was added, zirconia beads were added, and the mixture was ground at 3000 r / min for 1 hour to obtain liquid indigo dye. The dry weight of the indigo dye was 15 g, the aqueous polyurethane dispersant accounted for 27% of the dry weight of the indigo, and deionized water was added to make up to 60 g, the concentration of the dye in the liquid indigo was 25%, and the diameter of the zirconia beads was 1 mm.
[0033] In step (2), the particle size distribution diagram and SEM photograph of the liquid indigo dye prepared with the aqueous polyurethane dispersant are shown in Figure 3. It can be seen that the D90 of the liquid indigo suspension is about 280 nm, the particle size distribution is uniform, and there are no large particles. The SEM photograph also shows that the particles of the liquid indigo suspension are small and there is no obvious aggregation phenomenon. The particle size of the prepared liquid indigo dye when stored at room temperature for 7 days and at 60°C for 7 days is shown in Table 1. It can be seen that the dispersant with this structure has high grinding efficiency when preparing the liquid disperse dye, and the storage stability of the dye is good, and the particle size of the dye particles does not change significantly before and after storage.
[0034] [Table 1]
[0035] The above are merely preferred embodiments of the present invention, and the scope of protection of the present invention is not limited to the above embodiments, and all technical solutions within the concept of the present invention are within the scope of protection of the present invention. In addition, any improvements and modifications made by those skilled in the art without departing from the principles of the present invention should be considered as within the scope of protection of the present invention.
Claims
1. The preparation method of the aqueous polyurethane dispersion is as follows: (1) Weigh out an isocyanate group-containing compound as an initiator, and react it with polyethylene glycol of a certain molecular weight in the presence of nitrogen and a catalyst at 75 to 80° C. for 2 to 2.5 hours to produce a polyurethane prepolymer; Add an appropriate amount of organic solvent to the reaction system to control the viscosity. (2) Keep the temperature constant, add chain extender 1, and carry out the chain extension reaction for 2 to 2.5 hours. (3) Keep the temperature constant, add chain extender 2, and continue the chain extension reaction for 2 to 2.5 hours. (4) The temperature is lowered to 50-55°C, a terminal blocking agent is added, and the terminal blocking reaction is carried out for 1-1.5 hours. (5) After the reaction is completed, an equimolar amount of triethylamine is added to the chain extender 1 to carry out a neutralization reaction for 1 hour, deionized water is added to emulsify the mixture at high speed for 20 to 30 minutes, and the mixture is distilled under reduced pressure at room temperature to remove the organic solvent, thereby finally obtaining an aqueous polyurethane dispersion.
2. In step (1), the initiator is either hexamethylene diisocyanate or isophorone diisocyanate; The polyethylene glycol is either PEG 400 or PEG 600; 2. The method for producing an aqueous polyurethane dispersion according to claim 1, wherein the molar ratio of the initiator to the polyethylene glycol is 4:1 to 1.
2.
3. In step (1), the catalyst is dibutyltin dilaurate; The method for producing an aqueous polyurethane dispersion according to claim 1, characterized in that the amount of the initiator and polyethylene glycol used is 2% by weight to 3% by weight of the two monomers.
4. 2. The method for producing an aqueous polyurethane dispersion according to claim 1, wherein in step (1), the organic solvent is either acetone or butanone.
5. In step (2), the chain extender 1 is either 2,2-hydroxymethylpropionic acid or 2,2-hydroxymethylbutyric acid; The method for producing an aqueous polyurethane dispersion according to claim 1, wherein the molar ratio of the initiator, the polyethylene glycol, and the chain extender 1 is 4:1 to 1.2:1.2 to 1.
5.
6. In step (3), the chain extender 2 is 1-phenyl-1,2-ethylene glycol; The method for producing an aqueous polyurethane dispersion according to claim 1, wherein the molar ratio of the initiator, the polyethylene glycol, the chain extender 1, and the chain extender 2 is 4:1 to 1.2:1.2 to 1.5:1.
2.
7. In step (4), the endcapping agent is methyl ethyl ketone oxime; The method for producing an aqueous polyurethane dispersion according to claim 1, wherein the molar ratio of the initiator, the polyethylene glycol, the chain extender 1, the chain extender 2, and the end capping agent is 4:1-1.2:1.2-1.5:1.2:0.2-1.
2.
8. Application of the aqueous polyurethane dispersion produced by the process according to any one of claims 1 to 7 in the production of liquid indigo dyes.
9. The application of claim 8, wherein the specific process includes: mixing indigo dye, aqueous polyurethane dispersion and water, first pre-grinding in a grinding cup at 1500 r / min for 5-10 min, then adding zirconia beads, and then continuing to grind in a sand mill at 3000 r / min for 1-2 hours to obtain liquid indigo dye.
10. The application of claim 9, wherein the aqueous polyurethane dispersion accounts for 25%-35% of the dry weight of the indigo dye, the dye content in the liquid indigo dye is 25%, the rotation speed of the sand mill is 3000-3500 r / min, and the diameter of the zirconia beads is 1-2 mm.
Citation Information
Patent Citations
Pigment dispersants formed by reacting isocyanates with poly(ethylene glycol) alkyl ethers, polyesters or polyacrylates, and diamines.
JP2003506538A
Polyurethane-based pigment dispersant containing reactive double bonds
JP2008542523A
Urethane prepolymer, polyurethane, and powder dispersant comprising said polyurethane, and production method for urethane prepolymer and polyurethane
WO2021020194A1