Martensitic heat-resistant steel for use at 630°C or higher and its manufacturing method

A specially formulated martensitic heat-resistant steel with controlled microstructure and composition addresses the limitations of existing materials, providing enhanced high-temperature strength and oxidation resistance for ultra-supercritical steam turbine rotors.

JP2024539727AActive Publication Date: 2024-10-29CHINA FIRST HEAVY IND +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024526892
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-06-22
Filing Date
2023-06-01
Publication Date
2024-10-29
Estimated Expiration
2043-06-01

AI Technical Summary

Technical Problem

Current martensitic heat-resistant steel materials for steam turbine rotors in ultra-supercritical steam turbines are limited by high-temperature durability and oxidation resistance, hindering the development of advanced thermal power generation technologies.

Method used

A martensitic heat-resistant steel with a composition including C, Si, Mn, Cr, W, Mo, Nb, V, Co, Cu, Ni, B, N, and Ta, featuring a microstructure with finely dispersed M23C6 carbide, CrTaN phase, and nanodispersion-strengthened Cu phase, produced through controlled manufacturing processes to enhance high-temperature strength and oxidation resistance.

Benefits of technology

The steel exhibits excellent high-temperature strength, creep resistance, and oxidation resistance, suitable for ultra-supercritical steam turbine rotors, with yield strength of 660 MPa at room temperature and 280 MPa at 630°C, and improved durability and toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539727000001_ABST
    Figure 2024539727000001_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of metallic materials, and discloses a martensitic heat-resistant steel for use at temperatures of 630° C. or higher and a manufacturing method thereof. The heat-resistant steel contains, by mass percentage, 0.01-0.14% C, 0.05-0.50% Si, 0.05-0.70% Mn, 8.5-13% Cr, 2.0-3.5% W, 0.1-0.7% Mo, 0.03-0.07% Nb, 0.1-0.3% V, 2.8-5% Co, 0.8-1.5% Cu, 0.1-0.5% Ni, 0.01-0.015% B, 0.01-0.08% N, 0.2-0.5% Ta, 0.1-0.5% Zr, and 0.01-0.3% Ce+Y, with the remaining components being Fe and unavoidable impurities. The heat-resistant steel of the present invention has good overall performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to a Chinese patent application filed with the State Intellectual Property Office of the People's Republic of China on June 22, 2022, bearing application number 2022107134571 and entitled "Martensitic heat-resistant steel for use at temperatures above 630°C and its manufacturing method," the entire contents of which are incorporated herein by reference.

[0002] The present invention belongs to the technical field of metallic materials, and more specifically, to a martensitic heat-resistant steel for use at temperatures of 630° C. or higher and a method for producing the same. [Background technology]

[0003] At present, in order to achieve the goal of energy saving and emission reduction, thermal power generation technology is developing towards hyperparameterization, two-stage reheating, and clean and highly efficient, and advanced ultra-supercritical coal-fired power generation technology is being fully used. For example, in thermal power generation, when the subcritical state is upgraded to the ultra-supercritical state, 68g of coal is saved per kilowatt-hour of electricity, and the coal consumption for power supply can be reduced by 21%, so that China can save 232 million tons of coal every year, which will reduce the annual emission of CO2.51 billion tons. However, at present, martensitic heat-resistant steel materials for large castings and forgings of hyperparameterized steam turbines are still a technical bottleneck that restricts the parameter improvement of power plants, and especially for the rotor forgings of steam turbines for 630℃, there are currently no mature products at home or abroad, and most of the rotors of steam turbines for 620℃ are imported.

[0004] Therefore, in order to break through the important core technologies, it is urgent to domestically produce high-performance and reliable heat-resistant steel materials and products. With the improvement of unit parameters, the performance requirements of materials are also increasing, especially the requirements for strength, toughness and durability under high stress and high temperature conditions. Currently, domestic and international research mainly focuses on adding W, Co, B and N elements to further improve the high-temperature durability and oxidation resistance of heat-resistant steel. However, even if elements such as W, Co, B, Nb and N are adjusted, there is a limit to how much the high-temperature durability and oxidation resistance of heat-resistant steel can be improved, so it is urgent to develop a new strengthening method to further improve the high-temperature properties and oxidation resistance of heat-resistant steel. Summary of the Invention [Problem to be solved by the invention]

[0005] Based on the above analysis, an object of the present invention is to provide a martensitic heat-resistant steel for use at 630°C or above, which has good overall performance in terms of high-temperature strength, impact resistance, permanent creep strain resistance, oxidation resistance, etc., and is suitable for rotors of ultra-supercritical steam turbines whose operating temperatures are 630°C or above, and a manufacturing method thereof.

[0006] In the present invention, a large number of experimental studies have been conducted on the material selection requirements for heat-resistant steels for steam turbine units in power plants under supercritical conditions. From the viewpoint of restricting the micromorphology of the nitride precipitation phase in 10-12% Cr steel, a new martensitic heat-resistant steel has been developed, in which tantalum element is added to make fine chromium tantalum nitrides stable at high temperatures the precipitation strengthening phase instead of MX.

[0007] The objectives of the present invention are mainly achieved by the following technical solutions: The present invention provides a martensitic heat-resistant steel for use at 630°C or higher, and its components, by mass percentage, include 0.01-0.14% C, 0.05-0.50% Si, 0.05-0.70% Mn, 8.5-13% Cr, 2.0-3.5% W, 0.1-0.7% Mo, 0.03-0.07% Nb, 0.1-0.3% V, 2.8-5% Co, 0.8-1.5% Cu, 0.1-0.5% Ni, 0.01-0.015% B, 0.01-0.08% N, 0.2-0.5% Ta, 0.1-0.5% Zr, and 0.01-0.3% Ce+Y, with the remaining components being Fe and unavoidable impurities.

[0008] Furthermore, there is provided a martensitic heat-resistant steel for use at 630°C or higher, the components of which, by mass percentage, are 0.01-0.14% C, 0.05-0.50% Si, 0.05-0.70% Mn, 8.5-13% Cr, 2.0-3.5% W, 0.1-0.7% Mo, 0.03-0.07% Nb, 0.1-0.3% V, 2.8-5% Co, 0.8-1.2% Cu, 0.1-0.5% Ni, 0.01-0.015% B, 0.01-0.08% N, 0.28-0.45% Ta, 0.1-0.5% Zr, and 0.1-0.2% Ce+Y, with the remaining components being Fe and unavoidable impurities.

[0009] Furthermore, the microstructure of the heat-resistant steel is a fully tempered martensite structure and a precipitate phase, and the precipitate phase is a dispersedly distributed M 23 Contains C6 type carbide, CrTaN phase, Laves phase and nano-dispersion strengthened Cu phase.

[0010] Compared with the conventional technology, the martensitic heat-resistant steel of the present invention for use at temperatures above 630°C has the following advantages: On the other hand, in addition to small amounts of V and Nb, 0.2 to 0.5% Ta is also added. The appropriate amount of Ta forms the CrTaN phase, which is resistant to coarsening. This prevents the formation of the Cr(V,Nb)N phase, which is very susceptible to coarsening over the long term. The coarsening of this phase reduces durability. In addition, during the long-term use of the steel, MX is transformed into Cr(Nb,V)N and coarsens, which can cause a sudden decrease in performance. On the other hand, in the present invention, the carbon content is limited to a relatively low level, and finely dispersed M with a relatively low C content is obtained. 23 The formation of C6 plays a role in dispersion strengthening, and a certain amount of Cu element is added to suppress the formation of high-temperature ferrite. In addition, the precipitation of nano-copper-rich phase compensates for the lack of V and Nb, plays a role in precipitation strengthening, and can improve the durability of heat-resistant steel. The addition of an appropriate amount of B element can improve the durability of heat-resistant steel. 23 Substitution at the C atom position of C6 gives M 23 (C,B)6 is formed, which results in M ​​near the prior austenite grain boundary. 23 The coarsening rate of C6 is reduced to significantly improve the creep strength, an appropriate amount of W element is used to improve the endurance limit, and a small amount of Ni element is used to improve the matrix toughness with a relatively high Co content. The rational element composition can largely avoid the formation of high temperature ferrite, which provides a wider temperature range for the forging and heat treatment process in actual production.

[0011] The present invention also provides a method for producing a martensitic heat-resistant steel for use at 630° C. or higher, comprising the following steps: Step S1: weighing raw materials according to the content of each component in the composition, smelting and pouring in a vacuum induction furnace to obtain an ingot, and strictly restricting the content of impurity elements, the composition is, on a mass percentage basis, C 0.01-0.14%, Si 0.05-0.50%, Mn 0.05-0.70%, Cr 8.5-13%, W 2.0-3.5%, Mo 0.1-0.7%, Nb 0.03-0.07%, V 0.1-0.3%, Co 2.8-5%, Cu 0.8-1.5%, Ni 0.1-0.5%, B 0.01-0.015%, N 0.01-0.08%, Ta 0.2-0.5%, Zr 0.1-0.5%, Ce+Y The content is 0.01 to 0.3%, and the remaining components are Fe and unavoidable impurities. In step S2, the ingot obtained in step S1 is subjected to high-temperature homogenization treatment, kept warm, and then cooled to room temperature in each furnace to obtain a blank. In step S3, the blank obtained in step S2 is forged by a rolling method, a swaging method or a stretching method, and when the temperature in the forging process is lower than the finish forging temperature, it is returned to the furnace to be heated and then forged again, and after forging, it is furnace-cooled to room temperature. In step S4, the forged bar obtained in step S3 is subjected to normalizing and two tempering heat treatments to obtain a chromium-tantalum nitride reinforced martensitic heat-resistant steel, in which the first tempering temperature is lower than the second tempering temperature.

[0012] Furthermore, in step S2, the temperature of the high-temperature homogenization treatment is 1160 to 1200° C., and the temperature retention time is 4 to 8 hours.

[0013] Furthermore, in the step S3, the rough forging temperature is 1160 to 1200°C, and the finish forging temperature is 850 to 950°C in the forging process.

[0014] Furthermore, the step S4 includes the following steps. Step S401 is normalizing, and the normalizing process involves heating the forged bar to 1050 to 1150° C., keeping the temperature, and then air-cooling it to room temperature. Step S402 is a first tempering step, in which the forged bar is heated to 600 to 700° C., kept at that temperature, and then air-cooled to room temperature. Step S403 is the second tempering, and the second tempering step involves heating the forged bar to 680 to 780° C., keeping the temperature, and then air-cooling it to room temperature.

[0015] Furthermore, in step S401, the temperature increase rate is 100° C. / hour or less, and the temperature retention time is 1 to 10 hours.

[0016] Furthermore, in step S402, the warming time is 5 to 10 hours.

[0017] Furthermore, in step S403, the warming time is 5 to 10 hours. Effect of the Invention

[0018] Compared with the prior art, the manufacturing process of martensitic heat-resistant steel for use above 630°C provided by the present invention precisely limits the process parameters such as the time and temperature of high-temperature homogenization, the temperature of forging, the temperature and time of normalizing, and the temperature and time of two temperings, thereby ensuring that the microstructure obtained is a complete tempered martensite structure and precipitates, and the precipitates are finely dispersed and distributed M. 23 Contains C6 carbide, CrTaN phase, a small amount of fine Laves phase, and nano-dispersion strengthened Cu phase. The heat-resistant steel has excellent room temperature strength, high temperature strength, permanent creep resistance, and oxidation resistance, making it suitable for rotors of ultra-supercritical steam turbines used at temperatures above 630°C.

[0019] Additional features and advantages of the invention will be set forth in the specification which follows, and in part will be obvious from the specification, or may be learned by practice of the invention. The objectives and other advantages of the invention may be realized and obtained as particularly pointed out in the written description and drawings. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 shows the as-cast structure of the heat-resistant steel according to Example 1 of the present invention. [Diagram 2] FIG. 2 shows the homogenized structure of the heat-resistant steel according to Example 1 of the present invention. [Diagram 3] FIG. 3 shows the structure of the heat-resistant steel according to Example 1 of the present invention after quenching and tempering. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings. The drawings are a part of the present invention and serve to explain the principles of the present invention together with an outline of the invention according to the present invention.

[0022] The present invention provides a martensitic heat-resistant steel for use at 630°C or higher, and its components, by mass percentage, include 0.01-0.14% C, 0.05-0.50% Si, 0.05-0.70% Mn, 8.5-13% Cr, 2.0-3.5% W, 0.1-0.7% Mo, 0.03-0.07% Nb, 0.1-0.3% V, 2.8-5% Co, 0.8-1.5% Cu, 0.1-0.5% Ni, 0.01-0.015% B, 0.01-0.08% N, 0.2-0.5% Ta, 0.1-0.5% Zr, and 0.01-0.3% Ce+Y, with the remaining components being Fe and unavoidable impurities.

[0023] In general, after long-term use, coarse chromium vanadium or chromium niobium nitride phases, i.e., CrVN and CrNbN, are formed in 9-12% Cr steel. Compared with the prior art, the heat-resistant steel provided by the present invention has a relatively low C content, a relatively high Co content, and is added with strengthening elements such as Ta and Cu and rare earth elements Ce+Y. The heat-resistant steel provided by the present invention does not contain V and Nb elements, and can avoid the formation of the coarsening Cr(V,Nb)N phase, which is very likely to form in the long-term process, and the coarsening of this phase reduces durability.

[0024] In the present invention, 0.2 to 0.5% of Ta element is added, and an appropriate amount of Ta element forms a CrTaN phase that is difficult to coarsen, and in the process of long-term use, it is possible to avoid a sudden decrease in performance caused by the transformation of MX into Cr(Nb,V)N and coarsening.

[0025] The heat-resistant steel provided by the present invention has a relatively low C content and finely dispersed M 23 The formation of C6 plays a role in dispersion strengthening. 0.8 to 1.5% Cu element is added. On the one hand, Cu element is an austenite forming element that suppresses the formation of high temperature ferrite. On the other hand, the precipitation of nano-copper rich phase compensates for the lack of V and Nb, plays a role in precipitation strengthening, and improves the durability limit of heat-resistant steel. An appropriate amount of B element is added to M. 23 Substitution at the C atom position of C6 gives M 23 (C,B)6 can be formed, which results in M ​​near the prior austenite grain boundary. 23 The coarsening rate of C6 is reduced to significantly improve the creep strength, an appropriate amount of W element is used to improve the endurance limit, and a small amount of Ni element is used to improve the matrix toughness with a relatively high Co content. The rational element composition can also largely avoid the formation of high temperature ferrite, which provides a wider temperature range for the forging and heat treatment processes in actual production.

[0026] The heat-resistant steel provided by the present invention has properties such as high strength, resistance to permanent creep strain, and oxidation resistance. The martensitic heat-resistant steel manufactured by the present invention has a yield strength of more than 660 MPa, a tensile strength of more than 850 MPa, an elongation of 16% or more, a cross-sectional shrinkage of 50% or more, and an impact energy of 20 J or more at room temperature. At 630°C, the yield strength is more than 280 MPa, the tensile strength is more than 380 MPa, the elongation is 22% or more, and a cross-sectional shrinkage of 62% or more. At 650°C, the creep rupture time at 650°C and 180 MPa is more than 3500 hours, and the weight gain due to oxidation resistance at 650°C (400 hours) is 0.3 mg / m 2 The overall performance is excellent.

[0027] Specifically, in the above martensitic heat-resistant steel for temperatures above 630°C, the roles of each component are as follows: C is an important precipitate strengthening element, and M 23 C6 and MX strengthen the dispersion and improve the permanent creep strain resistance. C is a strong austenite stabilizing element, which can reduce the formation of δ-ferrite and improve the hardenability and precipitation strengthening. If the carbon content is too high, it will lead to excessive consumption of solid solution elements (e.g., Cr, W), which will reduce the intergranular corrosion resistance, reduce the welding performance, and negatively affect the permanent creep strain resistance. If it is too low, the strengthening will be insufficient, which will reduce the strength and hardness, so the mass percentage of C is limited to 0.01-0.14% in the present invention.

[0028] Silicon helps to improve the strength and steam corrosion resistance of the matrix of the material. With increasing Si content, the oxidation resistance is improved rapidly. Increasing the Si content promotes the formation of ferrite at high temperatures and lowers the formation temperature of high-temperature ferrite, which has a negative effect on the forging temperature range. In addition, too high a Si content is detrimental to the impact strength of the material, and the endurance limit of the material decreases with increasing Si content. Therefore, in the present invention, the mass percentage of Si is limited to 0.05-0.50%.

[0029] Mn improves strength, improves hot workability, and stabilizes P, S, etc. If the content is lower than 0.2%, Mn cannot play an obvious role. If the content is higher than 1%, a second phase may appear in the structure, which is detrimental to the impact strength of the material. Therefore, the mass percentage of Mn is limited to 0.05-0.70% in the present invention.

[0030] Cr is the most important corrosion-resistant and oxidation-resistant element. Cr element itself has excellent creep strain resistance properties, and is also the main element for improving the steam oxidation and corrosion resistance performance of heat-resistant steels, and can also improve the high-temperature strength of steels. When there is sufficient Cr, it can react with O to form a Cr2O3 protective film on the surface of the alloy matrix, preventing the diffusion of O atoms and metal ions, and thus slowing down the progress of oxidation. Cr is also an important precipitate strengthening element, and is a major component of C and M. 23 It can form C6 precipitates to strengthen the steel. If the Cr content is too high, δ ferrite will be formed, which will reduce the high temperature strength. Therefore, the Cr content range is set to 9-13%.

[0031] W is a typical solid solution strengthening element, and its solid solution strengthening effect is more obvious than that of Mo. 23 It can stabilize the fine distribution of C6 and promote its precipitation strengthening. Increasing W element can significantly improve the high temperature strength and creep properties of heat-resistant steel. If W element is less than 2.0%, the long-term creep requirements of heat-resistant steel for temperatures above 630°C cannot be met, and if W exceeds 3.5%, ferrite formation occurs at high temperatures, and the welding performance of heat-resistant steel gradually deteriorates with increasing W content. Therefore, the mass percentage of W is limited to 2.0-3.5% in the present invention.

[0032] As for Mo, the combined addition of W and Mo can improve the toughness and plasticity of the material, the hot workability is good, and the impact strength is improved.

[0033] Co is an austenite stabilizing element that suppresses the formation of δ-ferrite, improves the high-temperature strength of the material, and 23 Coarsening of C6 is suppressed. In the present invention, the mass percentage of Co is limited to 2.8 to 5%.

[0034] Regarding Cu, Cu element can suppress the formation of δ-ferrite. In addition, adding Cu helps to improve the role of solid solution strengthening of W, and can improve the high-temperature creep strength of W-containing martensitic heat-resistant steel. Cu itself can also play the role of precipitation strengthening by existing as nano Cu-rich particles. When the content is relatively low, Cu mainly exists in a solid solution form, and the strengthening effect is relatively weak, but when the Cu content is relatively high, it has a great impact on the thermoplasticity at high temperatures. Therefore, the mass percentage of Cu is limited to 0.5-1.5% in the present invention.

[0035] Ni is a typical austenite-forming element, which can improve toughness and balance with the Cr equivalent of the material. In the present invention, the mass percentage of Ni is limited to 0.1 to 0.5%.

[0036] Regarding B, in the case of high Cr martensitic heat-resistant steel, the B element is M 23 Substitution at the C atom position of C6 gives M 23 (C,B)6 can be formed, M 23 (C,B)6 has a slow aging rate and good durability, which allows the M near the prior austenite grain boundaries to be 23 By reducing the coarsening rate of C6, M 23 Suppresses the coarsening of C6 and improves the creep strength of steel. B purifies the grain boundary and forms carbon boride M 23 (C 0.85 B 0.15 If the B content is too high, the thermoplasticity at high temperatures is reduced and the risk of cracking during forging increases. Therefore, in the present invention, the mass percentage of B is limited to 0.01 to 0.015%.

[0037] N forms finely dispersed second phase particles together with V, Nb, and Ta, and can significantly improve the high temperature endurance limit of the material. However, if the N content is too high, it will combine with B element to form coarse BN particles, significantly weakening the strength and toughness of the steel, and consuming B element for grain boundary strengthening, significantly reducing the high temperature endurance limit of the steel. Therefore, in the present invention, the mass percentage of N is limited to 0.01 to 0.08%.

[0038] Ta increases the Cr content to about 12% in this steel, and when it is aged and used for a long time at 600-650℃, the Cr in the matrix aggregates to MX and further forms Cr(Nb,V)N, which consumes the Cr element in the matrix, causing the precipitate phase to coarsen, and further promotes the formation of Cr(Nb,V)N. 12Cr is more likely to form coarse chromium vanadium or chromium niobium nitride phases than 9Cr steel, which is unfavorable for dislocation pinning and lath, and affects the durability of the steel. Adding an appropriate amount of Ta suppresses the transformation of MX to Cr(Nb,V)N and forms a phase mainly composed of CrTaN, which is less likely to coarsen than the Cr(Nb,V)N phase and exists as a finely dispersed precipitate phase, playing the role of precipitation strengthening, thereby solving the problems associated with the increase in the Cr content. If the Ta content is too high, it becomes difficult to completely dissolve in the matrix, and exists as Ta-rich particles, which increases the difficulty of smelting. Therefore, in the present invention, the mass percentage of Ta is limited to 0.2 to 0.5%.

[0039] Zr tends to reduce the growth of austenite grains with increasing Zr content and reduces the size of inclusions, therefore, in the present invention, the mass percentage of Zr is limited to 0.1 to 0.5%.

[0040] Regarding rare earth elements, Ce+Y are rare earth elements, and adding a small amount of them can improve the mechanical properties and corrosion resistance of heat-resistant steel at high temperatures. The mixed addition of rare earth elements exerts a synergistic effect, purifies and strengthens grain boundaries, and limits the number and shape of inclusions, thereby improving high-temperature strength and oxidation resistance. The total amount of rare earth added in the present invention is 0.01-0.3%.

[0041] Preferably, in a martensitic heat resistant steel for use at 630°C or higher, the components, by mass percentage, include 0.01-0.14% C, 0.05-0.50% Si, 0.05-0.70% Mn, 8.5-13% Cr, 2.0-3.5% W, 0.1-0.7% Mo, 0.03-0.07% Nb, 0.1-0.3% V, 2.8-5% Co, 0.8-1.2% Cu, 0.1-0.5% Ni, 0.01-0.015% B, 0.01-0.08% N, 0.28-0.45% Ta, 0.1-0.5% Zr, and 0.1-0.2% Ce+Y, with the remaining components being Fe and unavoidable impurities.

[0042] The present invention also provides a method for producing a martensitic heat-resistant steel for use at 630° C. or higher, comprising the following steps: Step S1: weighing raw materials according to the content of each component in the composition, smelting and pouring in a vacuum induction furnace to obtain an ingot, and strictly restricting the content of impurity elements, the composition is, on a mass percentage basis, C 0.01-0.14%, Si 0.05-0.50%, Mn 0.05-0.70%, Cr 8.5-13%, W 2.0-3.5%, Mo 0.1-0.7%, Nb 0.03-0.07%, V 0.1-0.3%, Co 2.8-5%, Cu 0.8-1.5%, Ni 0.1-0.5%, B 0.01-0.015%, N 0.01-0.08%, Ta 0.2-0.5%, Zr 0.1-0.5%, Ce+Y The content is 0.01 to 0.3%, and the remaining components are Fe and unavoidable impurities. In step S2, the ingot obtained in step S1 is subjected to high-temperature homogenization treatment, kept warm, and then cooled to room temperature in each furnace to obtain a blank. In step S3, the blank obtained in step S2 is forged by a rolling method, a swaging method or a stretching method, and when the temperature in the forging process is lower than the finish forging temperature, it is returned to the furnace to be heated and then forged again, and after forging, it is furnace-cooled to room temperature. In step S4, the forged bar obtained in step S3 is subjected to normalizing and two tempering heat treatments to obtain a chromium-tantalum nitride reinforced martensitic heat-resistant steel, in which the first tempering temperature is lower than the second tempering temperature.

[0043] Specifically, in the above step S2, the purpose of the high-temperature homogenization treatment is to eliminate the high-temperature ferrite, precipitated phases, and segregation of alloy elements in the ingot. If the temperature of the high-temperature homogenization is too high, the grains will be significantly coarsened and high-temperature ferrite will be formed, and if it is too low, the precipitated phases and element segregation such as δ ferrite, M3B2, etc. in the cast structure cannot be effectively eliminated. From a large amount of experimental research, the temperature of the high-temperature homogenization is limited to 1160-1200°C. The heat-holding time is limited to 4-8 hours, and if the heat-holding time is too short, it is insufficient to eliminate the high-temperature ferrite, precipitated phases, element segregation, etc. in the ingot, and if the time is too long, it may cause overheating or overburning, which causes the grains to become coarse.

[0044] Specifically, the forging in step S3 above can achieve the purpose of crushing defects, refining grains, and homogenizing the structure (the structure of the heat-resistant steel according to Example 1 after quenching and tempering is as shown in FIG. 3), which lays a good foundation for improving the overall performance of the heat-resistant steel. If the rough pressing temperature is higher than 1200°C, high-temperature ferrite will be formed, increasing the risk of forging cracks, and if the rough pressing temperature is too high, the grains will be significantly coarsened, which increases the difficulty of limiting the grain size in the subsequent forging process, and if the grains are too large or mixed crystals exist after forging, on the one hand, it will affect the final mechanical properties, and on the other hand, it will also affect flaw detection. Therefore, in the present invention, the rough pressing temperature is limited to 1160-1200°C and the finish pressing temperature is limited to 850-950°C, and in the forging temperature range shown in the present invention, the steel has good plasticity. Compared with the prior art, the rough pressing temperature in the present invention is about 100°C higher than the same type of steel, so the forging temperature range is significantly expanded.

[0045] Specifically, the above step S4 includes the following steps. Step S401 is normalizing. The normalizing process involves heating a forged bar to 1050 to 1150° C., keeping the temperature, and then air-cooling it to room temperature. Step S402 is the first tempering, and the first tempering step involves heating the forged bar to 600 to 700° C., keeping the temperature, and then air-cooling it to room temperature. Step S403 is the second tempering, and the second tempering process involves heating the forged bar to 680 to 780° C., keeping the temperature, and then air-cooling it to room temperature.

[0046] Specifically, in the above S401, in the heat treatment of large forgings, if the heating rate is too fast, the temperature difference between the inside and outside will be very large, and if the heating rate is too fast, thermal cracking may occur. Based on the actual rules of heat treatment of large forgings, the forged bar is placed in a heating furnace at room temperature, and the heating rate is not more than 100°C / hour.

[0047] Specifically, in the above S401, if the heat-retention time is too long, the grains will become significantly coarsened, and if it is too short, the heat treatment of the forged product will be insufficient. Therefore, the heat-retention time is limited to 1 to 10 hours.

[0048] Specifically, in the above S402, the role of the first tempering is to promote the precipitation of CrTaN and fix the N element in the CrTaN phase. This is because around 650°C is the temperature range in which CrTaN in 12% Cr steel is most likely to precipitate. Tempering at this temperature allows the formation of extremely finely dispersed CrTaN phases, which then disperse and bind together with other MX, Cr 23 It is more difficult to grow than precipitates such as C6 and Laves. If the tempering temperature is too high, a large amount of carbides will precipitate, the martensite structure will widen in lath width, and the dislocation density will decrease, resulting in a significant decrease in strength. If the tempering temperature is too low, it will be insufficient to promote the precipitation of CrTaN. If the heat-holding time is too long, performance will decrease, and if it is too short, it will be insufficient for heat treatment and element diffusion. Therefore, the tempering temperature is limited to 600-700°C and the heat-holding time to 5-10 hours.

[0049] Specifically, in the above S403, the role of the second tempering is to form a complete tempered martensite structure to obtain good overall performance. If the tempering temperature is too high, the strength is insufficient; if the tempering temperature is too low, the impact strength is greatly reduced; if the heat-holding time is too long, the size of the precipitated phase is large, and both the strength and impact value cannot meet the performance requirements; if the heat-holding time is too short, the heat treatment of the forging and the formation of tempered martensite are insufficient. Therefore, the tempering temperature is limited to 680-780°C and the heat-holding time is limited to 5-10 hours.

[0050] The normalizing temperature mentioned above is M 23 The precipitates such as C6, M3B2, Laves, etc. can be completely eliminated, the alloy elements can be completely dissolved in the matrix, the grain size is limited within grade 2, and δ ferrite is not formed. The first low-temperature tempering can promote the precipitation of CrTaN and fix N element in CrTaN phase, and the second high-temperature tempering tempers the newly transformed martensite, and finally ensures that the structure is all uniform tempered martensite + precipitate phase, the proportions of tempered martensite and precipitate phase are 98% and 2% respectively, and the precipitate phase is finely dispersed and distributed in lath boundaries and grain boundaries, which plays a good strengthening role.

[0051] The structure of the heat-resistant steel that has undergone the above heat treatment is a fully tempered martensite structure + precipitate phase. The precipitate phase is mainly finely dispersed M 23 C6, CrTaN, a small amount of fine Laves phase and nano-dispersion strengthened Cu phase.

[0052] The heat-resistant steel that has undergone the above heat treatment has a yield strength of more than 660 MPa, a tensile strength of more than 850 MPa, an elongation of 16% or more, a cross-sectional shrinkage of 50% or more, and an impact energy of 20 J or more at room temperature. At 630°C, the yield strength is more than 280 MPa, the tensile strength is more than 380 MPa, the elongation is more than 22%, and the cross-sectional shrinkage is more than 62%, the creep rupture time at 650°C and 180 MPa is more than 3500 hours, and the weight gain due to oxidation resistance at 650°C (400 hours) is 0.3 mg / m 2 Below is the result: Excellent performance.

[0053] The following specific examples and comparative examples demonstrate the advantages of the precise limits of the composition and process parameters of the steel according to the invention.

[0054] Example 1 This embodiment provides a martensitic heat-resistant steel for use at temperatures of 630° C. or higher and a method for manufacturing the same.

[0055] The chemical composition of this example is, by weight percentage, C 0.05%, Si 0.30%, Mn 0.50%, Cr 12.0%, W 3.0%, Mo 0.2%, Nb 0.05%, V 0.2%, Co 4.5%, Ni 0.2%, Cu 1.0%, B 0.01%, N 0.045%, Ta 0.32%, Zr 0.3%, Ce+Y 0.15%, and the remaining components are Fe and unavoidable impurities.

[0056] The manufacturing method of heat-resistant steel includes the following: In step S1, the alloy is smelted in a vacuum induction furnace according to the composition ratio, and an ingot is obtained by pouring the alloy into the vacuum induction furnace, and the content of impurity elements is strictly limited. In step S2, the ingot obtained in step S1 is subjected to high-temperature homogenization treatment, and then cooled to room temperature in each furnace to obtain a blank, where the temperature of high-temperature homogenization is 1180°C and the heat retention time is 5 hours. In step S3, the blank obtained in step S2 is forged by the rolling method, the upsetting method or the stretching method. The rough forging temperature is 1180°C, and the finish forging temperature is 950°C. If the temperature in the forging process is lower than the finish forging temperature, it needs to be returned to the furnace to be heated and then forged again. In step S4, the forged bar obtained in step S3 is subjected to normalizing and two tempering heat treatments to obtain a chromium-tantalum nitride reinforced martensitic heat-resistant steel, in which the normalizing temperature is 1100°C, the heat retention time is 5 hours, the first tempering temperature is 650°C, the heat retention time for the first tempering is 6 hours, the second tempering temperature is 740°C, and the heat retention time for the second tempering is 6 hours.

[0057] The chemical compositions of the steels according to Examples 1 to 4 and Comparative Examples 1 and 2 are shown in Table 1. The process steps of Examples 2 to 4 are the same as those of Example 1, and the specific process parameters are shown in Table 2. The performances of Examples 1 to 4 and Comparative Examples 1 and 2 are shown in Tables 3 and 4, and the metal structures of Examples 1 to 4 and Comparative Examples 1 and 2 are shown in Table 5.

[0058] Comparative Example 1 does not have Cu, Ta, Zr or rare earth elements added to its chemical composition, and Comparative Example 2 has Ta element added to its chemical composition, and the specific chemical composition is as shown in Table 1. The process steps of Comparative Examples 1 and 2 are the same as those of Example 1, and the specific process parameters are shown in Table 2, and the comparison of each performance index with Examples 1 to 4 is as shown in Table 3. As can be seen from Table 3, the Examples are superior in each performance compared to the Comparative Examples. JPEG2024539727000002.jpg37170JPEG2024539727000003.jpg252170JPEG2024539727000004.jpg123170

[0059] The above are only specific preferred embodiments of the present invention, and the scope of protection of the present invention is not limited thereto. Any changes or replacements that are easily thought of by a person skilled in the art within the technical scope disclosed in the present invention are intended to be included in the scope of protection of the present invention.

Claims

1. A martensitic heat-resistant steel for use at 630°C or higher, The components, on a mass percentage basis, are C 0.01-0.14%, Si 0.05-0.50%, Mn 0.05-0.70%, Cr 8.5-13%, W 2.0-3.5%, Mo 0.1-0.7%, Nb 0.03-0.07%, V 0.1-0.3%, Co 2.8-5%, Cu 0.8-1.5%, Ni 0.1-0.5%, B 0.01-0.015%, N 0.01-0.08%, Ta 0.2-0.5%, Zr 0.1-0.5%, Ce+Y 0.01-0.3%, and the remaining components are Fe and inevitable impurities. Martensitic heat-resistant steel for temperatures above 630°C.

2. The components, expressed as mass percentages, are C 0.01-0.14%, Si 0.05-0.50%, Mn 0.05-0.70%, Cr 8.5-13%, W 2.0-3.5%, Mo 0.1-0.7%, Nb 0.03-0.07%, V 0.1-0.3%, Co 2.8-5%, Cu 0.8-1.2%, Ni 0.1-0.5%, B 0.01-0.015%, N 0.01-0.08%, Ta 0.28-0.45%, Zr 0.1-0.5%, Ce+Y 0.1-0.2%, and the remaining components are Fe and inevitable impurities. The martensitic heat-resistant steel for use at temperatures of 630°C or higher according to claim 1.

3. The microstructure of the heat-resistant steel is a fully tempered martensite structure and a precipitate phase, and the precipitate phase is a dispersed M phase. 23 C 6 type carbides, CrTaN phase, Laves phase and nano-dispersion strengthened Cu phase, The martensitic heat-resistant steel for use at temperatures of 630° C. or higher according to claim 1 or 2.

4. The raw materials are weighed according to the content of each component in the composition, smelted in a vacuum induction furnace, and poured to obtain an ingot. The content of impurity elements is strictly limited. The composition is, by mass percentage, C 0.01-0.14%, Si 0.05-0.50%, Mn 0.05-0.70%, Cr 8.5-13%, W 2.0-3.5%, Mo 0.1-0.7%, Nb 0.03-0.07%, V 0.1-0.3%, Co 2.8-5%, Cu 0.8-1.5%, Ni 0.1-0.5%, B 0.01-0.015%, N 0.01-0.08%, Ta 0.2-0.5%, Zr 0.1-0.5%, Ce+Y Step S1, comprising 0.01 to 0.3% of Fe and the remaining components being Fe and inevitable impurities; Step S2: subjecting the ingot obtained in step S1 to a high-temperature homogenization treatment, keeping it warm, and then cooling it to room temperature in each furnace to obtain a blank; Step S3: forging the blank obtained in step S2 by a rolling method, a swaging method, or a stretching method, and when the temperature in the forging process is lower than the finishing temperature, returning it to the furnace to heat it and forging it again, and then cooling it to room temperature after forging; Step S4, the forged bar obtained in step S3 is subjected to normalizing and two tempering heat treatments to obtain a chromium-tantalum nitride reinforced martensitic heat-resistant steel, where the first tempering temperature is lower than the second tempering temperature. The method for producing a martensitic heat-resistant steel for use at 630° C. or higher according to any one of claims 1 to 3.

5. In step S2, the temperature of the high-temperature homogenization treatment is 1160 to 1200 ° C, and the heat retention time is 4 to 8 hours; The method for producing the martensitic heat-resistant steel for use at temperatures of 630° C. or higher according to claim 4.

6. In step S3, the rough forging temperature is 1160 to 1200 ° C., and the finish forging temperature is 850 to 950 ° C. The method for producing the martensitic heat-resistant steel for use at temperatures of 630° C. or higher according to claim 4.

7. The step S4 is Step S401: Normalizing. The normalizing process is to heat the forged bar to 1050-1150°C, keep the temperature, and then air-cool it to room temperature; Step S402: the first tempering step is to heat the forged bar to 600 to 700 ° C., keep the temperature, and then air-cool the bar to room temperature; A second tempering step includes a step S403 of heating the forged bar to 680 to 780 ° C., keeping the temperature, and then air-cooling the bar to room temperature. The method for producing the martensitic heat-resistant steel for use at temperatures of 630° C. or higher according to claim 4.

8. In step S401, the heating rate is 100° C. / hour or less, and the heat retention time is 1 to 10 hours. The method for producing the martensitic heat-resistant steel for use at temperatures of 630° C. or higher according to claim 7.

9. In step S402, the warming time is 5 to 10 hours. The method for producing the martensitic heat-resistant steel for use at temperatures of 630° C. or higher according to claim 7.

10. In step S403, the warming time is 5 to 10 hours. The method for producing the martensitic heat-resistant steel for use at temperatures of 630° C. or higher according to claim 7.

Citation Information

Patent Citations

  • Heat-resistant steel for ultra-supercritical steam turbine casting at temperature of 630 DEG C or above and preparation method of heat-resistant steel

    CN114622132A

  • Heat-resistant steel for ultra-supercritical steam turbine rotor forge piece and preparation method of heat-resistant steel

    CN114622133A

  • Heat-resistant steel for ultra-supercritical steam turbine forgings at temperature of 630 DEG C or above and preparation method thereof

    CN114622142A

  • High chromium ferritic heat resistant steel

    JP1996085850A

  • Production of ferritic iron base alloy, production of ferritic heat resistant steel and ferritic heat resistant steel

    JP1997184050A