Flame-retardant heat insulating and fire-resistant materials for batteries
The flame-retardant heat-insulating fire protection material for batteries addresses the instability of ceramicized silicone rubbers by using glass powders with varying melting temperatures to maintain a continuous ceramic layer, ensuring effective fire protection and insulation up to 1500°C.
Patent Information
- Application Number
- JP2024506941
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-18
- Filing Date
- 2023-09-21
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-09-21
AI Technical Summary
Existing ceramicized silicone rubbers used in battery packs fail to form a continuous, dense ceramic body structure due to varying reaction temperatures of components, leading to structural instability and vulnerability to thermal shock and high temperatures, which compromises their fire protection efficacy.
A flame-retardant heat-insulating fire protection material for batteries is developed, incorporating glass powders with multiple initial melting temperatures ranging from 300°C to 1500°C, ensuring a continuous ceramic layer by timely filling pores and cracks, and comprising an impact-resistant layer with a specific thickness ratio to maintain integrity and compactness.
The material effectively maintains a continuous, dense ceramic layer even at high temperatures up to 1500°C, ensuring robust fire protection and insulation by continuously filling gaps with molten glass powders, thereby preventing structural failure under thermal shock.
Smart Images

Figure 2024539811000001_ABST
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to Chinese Patent Application No. 202211274999.X, filed in China on October 18, 2022, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a silicone rubber flame-retardant heat insulating and fire-resistant material, in particular to a flame-retardant heat insulating and fire-resistant material for new energy vehicle battery packs. [Background technology]
[0003] Generally, the probability of a battery's thermal runaway is one in ten million, but when an electric vehicle is equipped with thousands of batteries to form a battery pack, the probability of the battery pack's thermal runaway increases to one in ten thousand, and the thermal runaway of one battery can cause the thermal runaway of the entire battery pack, and the combustion temperature after the thermal runaway of the battery pack can reach 1500°C, which is even more shocking, posing a major challenge to the safety of electric vehicles. Research has shown that ceramized silicone rubber is currently the best material solution for new energy vehicle battery packs to prevent the continuous thermal runaway of the battery core and avoid the ignition of adjacent modules.
[0004] Ceramic silicone rubber is a polymer composite material that can be porcelainized. This material has the excellent properties of ordinary polymers at room temperature, and can form a dense ceramic structure at high temperatures, so it exhibits ceramic properties. In silicone rubber, the bond energy of the Si-O bond is high, so the silicone rubber itself has good thermal stability. Furthermore, when it is burned in a high-temperature flame, the Si-O bonds are connected to form a network of SiO, which is oxidation-resistant and insulating. 2 Ash is formed and covers the surface of the battery core, effectively preventing further combustion of the flame. In addition, the smoke generated during the combustion process of the silicone rubber matrix is mainly CO generated by the combustion of the side groups. 2 and H 2O, no toxic gases are produced, and there is no risk of environmental pollution. The use of organic silicone polymers to produce ceramic silicone rubber has unique advantages in terms of process and raw material selection, as well as the high temperature resistance and mechanical properties of ceramic products.
[0005] The main principle of ceramicized silicone rubber flame retardant, heat insulation and fire protection is to improve the thermal stability of silicone rubber by adding catalysts, heat stabilizers, fireproof fillers, glass powder, etc., and promote the formation and stabilization of the ceramic layer. Usually, after ceramicized silicone rubber is burned, the specific process of ceramicization is as follows: When burned or heated, the silicone rubber matrix first transforms into amorphous SiO 2 Then, with the increase in temperature, the low-melting glass powder (ceramic powder, porcelain-forming melting aid) melts gradually first, forming a liquid phase material in the silicone rubber system, and the amorphous SiO 2 formed in the matrix. 2 and temperature-resistant porcelain-forming fillers (mica, kaolin, wollastonite, etc.) to form a "hypoeutectic mixture" at the filler interface, called a co-crystalline reaction. The hypoeutectic mixture forms amorphous SiO 2 Finally, as time progresses, the temperature increases further and the porcelain-forming fillers and amorphous SiO 2 and the low eutectic mixture, the filler boundaries disappear and new inorganic phases are generated, forming a continuous, complete, dense ceramic body structure.
[0006] Chinese patent CN110845850A discloses porcelainizable halogen-free flame-retardant silicone rubber and its manufacturing method. Chinese patent CN107286636A discloses low smoke flame retardant ceramizable thermoplastic polyurethane elastomer composite material, its manufacturing method and application. Chinese patent CN202111191443.X discloses ceramified flame retardant heat insulation and fire protection material, its manufacturing method and application. Although the above patents all disclose ceramified silicone rubber and its application method, there are still deficiencies in protecting battery packs.
[0007] Normally, when ceramic silicone rubber is burned at high temperatures, the reaction temperatures of each component are significantly different. For example, silicone rubber starts to decompose at 350℃, and amorphous SiO 2 , which produces a large number of pores of different sizes on its surface. Muscovite (a common porcelain-forming filler) begins to decompose only above 700℃. Ordinary glass powders of different components have initial melting temperatures between 300℃ and 700℃. When the battery goes into thermal runaway, the combustion temperature gradually reaches 1500℃, and is accompanied by thermal shock. Therefore, the initial melting temperature of the glass powder is high (above 700℃), and within the low temperature range (350℃ to 700℃), the silicone rubber cannot form a continuous, complete, dense ceramic body structure together with the porcelain-forming filler and glass powder, and the amorphous SiO with pores is formed. 2 If the initial melting temperature of the glass powder is low (less than 700℃), the glass powder vaporizes in the high temperature range (above 1200℃), creating pores in the ceramic body skeleton structure, reducing the density of the ceramic body structure and making it susceptible to thermal shock, which results in melting.
[0008] All currently disclosed ceramic silicone rubbers only contain glass powder with one initial melting temperature, that is, the glass powder in the conventional materials cannot completely cover the temperature range of 300°C to 1500°C in the melting state, so the above problem always occurs. Summary of the Invention
[0009] In view of the shortcomings of the prior art, the present invention provides a flame-retardant heat insulating fire-resistant material for batteries. The present invention adds various glass powders having different melting temperature ranges, so that when the fire-resistant material burns at 300°C to 1500°C, it always has molten glass powder inside, and these molten glass powders are SiO 2The pores and cracks generated at different temperatures in the ceramic layer formed by the co-crystallization of ash and refractory filler can be filled in a timely manner, and the continuity, integrity and density of the ceramic layer can be maximized, and the fireproof material also has the characteristics of quickly forming porcelain at low temperatures and being resistant to high temperatures of over 1500° C. Conventional materials have the problem that the temperature range of the molten state of glass powder is single, and the high-melting glass powder cannot melt in a timely manner at low temperatures to fill the gaps in the ceramic layer, and the low-melting glass powder is easily vaporized at high temperatures, causing pores in the ceramic phase, which reduces the density of the structure and makes it easy to burn through.
[0010] In order to solve the above technical problems, the present invention provides the following technical solution: A flame-retardant heat-insulating and fire-protecting material for batteries, comprising an impact-resistant layer and a flame-retardant heat-insulating layer, which, in addition to comprising organic silicone rubber, a porcelain-forming filler, a flame retardant and an auxiliary, further comprises glass powders having different initial melting temperatures, the flame-retardant heat-insulating layer is applied to the surface of the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer is (2-10):1, and the temperature range of the molten state of the glass powders covers 300℃-1500℃.
[0011] In the above technical solution, optionally, the impact-resistant layer is a glass fiber cloth.
[0012] In the above technical solution, optionally, the impact-resistant layer is a multi-layer composite of glass fiber cloth.
[0013] In the above technical solution, optionally, the glass powder includes glass powder A having a temperature range in a molten state of 300° C. to 700° C. and glass powder B having a temperature range in a molten state of 700° C. to 1500° C. The mass ratio of glass powder A to glass powder B is 1-2:1-3.
[0014] In the above technical solution, the glass powder optionally includes glass powder C having a temperature range in a molten state of 300° C. to 550° C., glass powder D having a temperature range in a molten state of 550° C. to 900° C., and glass powder E having a temperature range in a molten state of 900° C. to 1500° C. In terms of mass ratio, the ratio of glass powder C, glass powder D and glass powder E is 1-2:1-2:2-3.
[0015] In the above technical solution, the glass powders selectively include glass powder F, which has a temperature range in a molten state covering 300° C. to 800° C., glass powder G, which has a temperature range in a molten state covering 600° C. to 1000° C., glass powder H, which has a temperature range in a molten state covering 700° C. to 1250° C., and glass powder I, which has a temperature range in a molten state covering 1000° C. to 1500° C. In terms of mass ratio, the ratio of glass powder F, glass powder G, glass powder H, and glass powder I is 1-3:1-3:1-3:1-3:1-3.
[0016] In the above technical solution, optionally, the raw material of the glass powder includes one or more selected from silicon oxide, boron oxide, and metal oxide, and the metal oxide includes one or more selected from lead oxide, aluminum oxide, lithium oxide, zinc oxide, titanium oxide, magnesium oxide, vanadium oxide, barium oxide, sodium oxide, calcium oxide, strontium oxide, tin oxide, bismuth oxide, and antimony oxide.
[0017] In the above technical solution, optionally, the raw material of the glass powder further comprises stannous fluoride.
[0018] In the above technical solution, optionally, it includes 40 parts to 60 parts of organic silicone rubber, 20 parts to 30 parts of porcelain forming filler, 15 parts to 25 parts of flame retardant, 2 parts to 10 parts of glass powder, and 2 parts to 5 parts of auxiliary agent.
[0019] In the above technical solution, optionally, the composition further comprises 10 parts to 17 parts of an extending filler. In the above technical solution, optionally, the flame-retardant heat insulating fire-resistant material will not melt down under the flame impact of 1500℃ for at least 30 minutes.
[0020] The glass powder is generally SiO 2 , B 2 O 3 , Al 2 O 3 It is made by thoroughly mixing PbO, PbO and some metal oxides in a certain ratio, melting, water quenching and grinding. Due to the adjustment of the ratio of different components and the addition of different metal oxides, the initial melting temperature and the temperature range of the molten state of the glass powder will be slightly different.
[0021] When a lithium battery experiences thermal runaway, a deflagration phenomenon occurs, i.e. high-temperature combustion is accompanied by impact. Silicone rubber begins to decompose at 350℃, forming amorphous SiO 2 In this case, the glass powder melts, forms a liquid phase, fills the pores, and forms amorphous SiO 2 and the porcelain forming filler must be connected to maintain stability under combustion and impact. Thus, the initial melting temperature of the glass powder in the conventional material is often selected between 300°C and 700°C so that it melts when the silicone rubber starts to decompose and fills the pores as soon as possible, but the temperature range of the molten state of the glass powder with the initial melting temperature between 300°C and 700°C does not basically exceed 1000°C, that is, when the burning temperature is higher than the temperature range of the molten state of the glass powder, the glass powder will volatilize in gas phase, that is, pores will be generated in the formed ceramic layer, so that the density of the entire structure of the ceramic layer will decrease, and under the synergistic effect of thermal shock and combustion, the conventional fireproof material will melt down in the flame of 1000°C to 1500°C, and the fireproof material will be ineffective. Moreover, thermal shocks occur during the entire burning process, which are very likely to cause cracks in the ceramic layer. If the cracks are not repaired, the entire fire-protection material will fail. That is, the molten glass powder needs to fill the pores and cracks from time to time during the entire burning process of the fire-protection material, so that the ceramic layer remains continuous, complete and dense up to 1500°C.
[0022] Therefore, the present invention has various molten temperature ranges, covering 300°C to 1500°C, by mixing glass powders with various initial melting temperatures. Therefore, no matter how high the burning temperature of the fireproof material is, there is always glass powder in a molten state to fill the pores and cracks in the ceramic layer, and the continuity, completeness, and denseness of the ceramic layer are maximized, allowing the ceramic layer to maximize its thermal insulation and flame retardancy.
[0023] Compared with the prior art, the present invention adds various glass powders having different melting temperature ranges to always have molten glass powder within the temperature range of 300°C to 1500°C, and the molten glass powder can timely fill pores and cracks generated in the ceramic layer at different temperatures, maximizing the continuity, completeness, and denseness of the ceramic layer, and the flame-retardant heat insulating fireproof material for batteries is characterized by quickly forming porcelain at low temperatures and enduring high temperatures of about 1500°C. Conventional materials have a single temperature range for the melting state of the glass powder, and the high-melting glass powder cannot melt at low temperatures to timely fill gaps in the ceramic layer, and the low-melting glass powder is easily vaporized at high temperatures, causing pores in the ceramic layer, reducing the denseness of the structure and making it easy to melt down. [Brief description of the drawings]
[0024] [Figure 1] FIG. 11 is an actual image showing the complete ceramicization state of the flame-retardant heat insulating and fire-resistant material for batteries prepared according to Example 17 of the present invention after undergoing a flame shock test at 1500° C. for 15 minutes and a deflagration test at 5 standard atmospheric pressure. [Diagram 2] 11 is an actual image showing the ceramic crack state of the flame-retardant heat insulating and fire-resistant material for batteries prepared according to Example 17 of the present invention after undergoing a flame shock test at 1500°C for 15 minutes and a deflagration test at 7 standard atmospheric pressure. [Diagram 3] 1 is an actual image showing the ceramic destruction state of the flame-retardant heat insulating and fire-resistant material for batteries prepared according to Example 17 of the present invention after undergoing a flame shock test at 1500°C for 15 minutes and a deflagration test at 10 standard atmospheric pressure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] In order to facilitate understanding of the present invention, the present invention is listed in the following examples. Those skilled in the art should understand that the above examples are merely to aid in understanding the present invention, and are not intended to specifically limit the present invention.
[0026] In the embodiments of the present application, the organic silicone rubber is any one or a combination of at least two selected from liquid silicone rubber, methylvinyl silicone rubber, or methylphenylvinyl silicone rubber. In the following examples and comparative examples, the organic silicone rubber is methylvinyl silicone rubber: 1103 from Guangzhou Sekiyou New Materials Technology Co., Ltd. ("Seki" is the Chinese character consisting of "stone" and "evening"). In practical applications, it is not limited to methylvinyl silicone rubber.
[0027] The porcelain-forming filler is any one or a combination of at least two selected from muscovite, phlogopite, kaolin, brucite and talc. In the following examples and comparative examples, the porcelain-forming filler is muscovite from Guangdong Yongfeng Chemical Co., Ltd. In practical application, it is not limited to muscovite.
[0028] The extending filler is any one or a combination of at least two selected from diatomaceous earth, wollastonite, calcium carbonate and fumed silica. In the following examples and comparative examples, the extending filler includes diatomaceous earth from Guangzhou Haozhao Chemical Co., Ltd., calcium carbonate of 325-6250 (mesh) from Dongguan Kinke New Materials Co., Ltd. ("kin" is the Chinese character consisting of "sun" and "jin"), and nanosilica KS-8200 from Jinan Kasong Chemical Co., Ltd. ("ka" is the Chinese character consisting of "up" and "to"). The mass ratio of diatomaceous earth, calcium carbonate and nanosilica is 0.8:1:3, and is not limited to the mixture of the above materials in practical application.
[0029] The flame retardant is any one or a combination of at least two selected from antimony trioxide, aluminum hydroxide, magnesium hydroxide, phosphorus-containing inorganic flame retardant, boron-containing inorganic flame retardant, and phosphorus-containing organic flame retardant. In the following examples and comparative examples, the flame retardant includes aluminum hydroxide from Hefei Zhongke Flame Retardant New Materials Co., Ltd., phosphorus-containing inorganic flame retardant from Shijiazhuang Jinsheng Chemical Co., Ltd. ("Jin" is the Chinese character consisting of three "gold"), and phosphorus-containing organic flame retardant from Zhengzhou Hanshuo Chemical Raw Materials Co., Ltd. The mass ratio of aluminum hydroxide, phosphorus-containing inorganic flame retardant, and phosphorus-containing organic flame retardant is 3:0.9:1.3, and is not limited to the mixture of the above materials in practical application.
[0030] The auxiliary includes a silane coupling agent, silicone oil and a vulcanizing agent, where the vulcanizing agent is one selected from benzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di-tert-butylhexane peroxide and platinum vulcanizing agent. In the following examples and comparative examples, the auxiliary is a silane coupling agent and silicone oil from Jiangsu Quanli Chemical Co., Ltd., and the vulcanizing agent is benzoyl peroxide. The mass ratio of the silane coupling agent, silicone oil and benzoyl peroxide is 0.5:5:1.8, and is not limited to the mixture of the above materials in practical application.
[0031] The glass powder is any one or a combination of at least two selected from silicon oxide, boron oxide, and metal oxide. Here, the metal oxide is any one or a combination of at least two selected from lead oxide, aluminum oxide, lithium oxide, zinc oxide, titanium oxide, magnesium oxide, vanadium oxide, barium oxide, sodium oxide, calcium oxide, strontium oxide, tin oxide, bismuth oxide, and antimony oxide. Some glass powders further contain stannous fluoride. Depending on the components and the compounding ratio, the glass powder has various initial melting temperatures and temperature coverage intervals of the molten state. In the present application, the temperature coverage interval of the molten state only indicates that the glass powder is in a molten state within this interval, and the temperatures at both ends are not the melting point and the boiling point, and the glass powder may be in a molten state outside the temperature coverage interval. In the following examples and comparative examples, the glass powder is provided by Guangzhou Yifeng Chemical Technology Co., Ltd. according to the applicant's request, or is self-disposed by the applicant.
[0032] In the examples of the present application, the components of glass powder A are SnF 2 , P 2 O 5 , SiO 2 , Sb 2 O 3 , Bi 2 O 3 Including 40 to 50 parts by mass of SnF 2 , 35th to 45th part P 2 O 5 , 1 part ~ 7 parts SiO 2 , Parts 1 to 7 Sb 2 O 3 and Part 1 to Part 7 Bi 2 O 3 Optionally, the glass powder A component contains 45 parts SnF 2 , 40 parts P 2 O 5 , 5 parts SiO 2 , 5 parts Sb 2 O 3 and 5th Division Bi 2 O 3The temperature range of the molten state of glass powder A covers 300°C to 700°C, and in practical applications, regardless of the components of glass powder A, the temperature range of the molten state of glass powder A only needs to cover 300°C to 700°C, and the above is only an example of one component of glass powder A.
[0033] The component of glass powder B is SiO 2 , B 2 O 3 , PbO, and 25 to 35 parts by mass of SiO 2 , Part 10 to Part 15 B 2 O 3 Optionally, glass powder B contains 30 parts SiO 2 , Part 11 B 2 O 3 , and 22 parts PbO. The temperature range of glass powder B in the molten state covers 700°C to 1500°C, and in actual application, regardless of the components of glass powder B, it is only necessary that the temperature range of glass powder B in the molten state covers 700°C to 1500°C, and the above is only an example of one component of glass powder B.
[0034] The composition of glass powder C is SnF 2 , P 2 O 5 , V 2 O 5 , Sb 2 O 3 , Bi 2 O 3 Including 45 to 55 parts by mass of SnF 2 , 30 to 40 copies of P 2 O 5 , Part 1 to Part 7 V 2 O 5 , 1st to 7th parts of Sb 2 O 3 and Bi from 1st to 7th divisions 2 O 3 Optionally, glass powder C contains 50 parts SnF 2 , 35th P 2 O 5 , 5th part V 2 O 5 , 5 parts Sb 2 O 3and 5th Division Bi 2 O 3 The temperature range of the molten state of the glass powder C covers 300°C to 550°C, and in practical application, regardless of the composition of the glass powder C, the temperature range of the molten state of the glass powder C only needs to cover 300°C to 550°C, and the above is only an example of one composition of the glass powder C.
[0035] The composition of glass powder D is SiO 2 , TiO 2 , B 2 O 3 , PbO, and 10 to 15 parts by mass of SiO 2 , 1 part to 5 parts of TiO 2 , Part 10 to Part 15 B 2 O 3 Optionally, glass powder D contains 14 parts SiO 2 , 2 parts TiO 2 , Part 12 B 2 O 3 , and 17 parts PbO. The temperature range of the molten state of glass powder D covers 550°C to 900°C, and in practical applications, regardless of the components of glass powder D, it is only necessary that the temperature range of the molten state of glass powder D covers 550°C to 900°C, and the above is only an example of one component of glass powder D.
[0036] The composition of glass powder E is SiO 2 , PbO, 30 to 40 parts by mass of SiO 2 Optionally, glass powder E contains 35 parts SiO 2 , and 20 parts PbO. The temperature range of the molten state of the glass powder E covers 900°C to 1500°C, and in practical applications, regardless of the components of the glass powder E, it is only necessary that the temperature range of the molten state of the glass powder E covers 900°C to 1500°C, and the above is only an example of one component of the glass powder E.
[0037] The components of glass powder F are SnF 2 , P 2 O 5 , SiO 2 , Bi2 O 3 , V 2 O 5 Contains 35 to 45 parts by mass of SnF 2 , 35th to 45th part P 2 O 5 , Part 1 to Part 7 V 2 O 5 , 5 parts to 15 parts of SiO 2 , Part 1 to Part 7 Bi 2 O 3 Optionally, the glass powder F contains 40 parts SnF 2 , 40 parts P 2 O 5 , 5th part V 2 O 5 , 10 parts SiO 2 and 5th Division Bi 2 O 3 The temperature range of the glass powder F in the molten state covers 300°C to 800°C, and in practical applications, regardless of the composition of the glass powder F, it is only necessary that the temperature range of the glass powder F in the molten state covers 300°C to 800°C, and the above is only an example of one composition of the glass powder F.
[0038] The component of glass powder G is SiO 2 , TiO 2 , B 2 O 3 , PbO, and 10 to 20 parts by mass of SiO 2 , 7 to 13 parts of TiO 2 , Part 10 to Part 15 B 2 O 3 Optionally, the glass powder G contains 15 parts of SiO 2 , 10 parts TiO 2 , Part 13 B 2 O 3 , and 12 parts PbO. The temperature range of the molten state of the glass powder G covers 600°C to 1000°C, and in practical applications, regardless of the components of the glass powder G, it is only necessary that the temperature range of the molten state of the glass powder G covers 600°C to 1000°C, and the above is only an example of one component of the glass powder G.
[0039] The composition of glass powder H is SiO2 , B 2 O 3 , TiO 2 , PbO. 15 to 20 parts by mass of SiO 2 , 10 to 15 parts of TiO 2 , 10th to 20th part B 2 O 3 Optionally, the glass powder H contains 17 parts SiO 2 , 12 parts TiO 2 , Part 15 B 2 O 3 , and 20 parts PbO. The temperature range of the molten state of the glass powder H covers 700°C to 1250°C, and in practical applications, regardless of the components of the glass powder H, it is only necessary that the temperature range of the molten state of the glass powder H covers 700°C to 1250°C, and the above is only an example of one component of the glass powder H.
[0040] The composition of glass powder I is SiO 2 , PbO. 25 to 35 parts by mass of SiO 2 Optionally, glass powder I contains 30 parts SiO 2 , and 13 parts PbO. The temperature range of the molten state of Glass Powder I covers 1000°C to 1500°C, and in practical application, regardless of the components of Glass Powder I, it is only necessary that the temperature range of the molten state of Glass Powder I covers 1000°C to 1500°C, and the above is only an example of one component of Glass Powder I.
[0041] Example 1: By weight, the composition contained 40 parts of organic silicone rubber, 20 parts of porcelain-forming filler, 10 parts of extending filler, 15 parts of flame retardant, 2 parts of glass powder and 2 parts of auxiliary agent. The glass powder contained glass powder A and glass powder B. The mass ratio of glass powder A to glass powder B was 1:1. The impact-resistant layer was a single-ply glass fiber cloth, and the flame-retardant heat-insulating layer was composited with the impact-resistant layer, and the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 10:1, and the total thickness of the material was 2 mm.
[0042] Example 2: by weight, it contains 60 parts of organic silicone rubber, 30 parts of porcelain-forming filler, 17 parts of extending filler, 25 parts of flame retardant, 10 parts of glass powder and 5 parts of auxiliary. The glass powder contains glass powder C, glass powder D and glass powder E. The mass ratio of glass powder C, glass powder D and glass powder E was 1:1:2. The impact-resistant layer was a three-layer glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer was 2:1, and the total thickness of the material was 1 mm.
[0043] Example 3: by weight, it contains 50 parts of organic silicone rubber, 25 parts of porcelain-forming filler, 15 parts of extending filler, 20 parts of flame retardant, 6 parts of glass powder and 3 parts of auxiliary. The glass powder contains glass powder F, glass powder G, glass powder H and glass powder I. The mass ratio of glass powder F, glass powder G, glass powder H and glass powder I was 1:1:1:1. The impact-resistant layer was a two-layer glass fiber cloth, and the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer was 6:1, and the total thickness of the material was 2.5 mm.
[0044] Example 4: by weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder contained glass powder A and glass powder B, and the mass ratio of glass powder A to glass powder B was 1:1. The impact-resistant layer was a single-ply glass fiber cloth, and the flame-retardant heat-insulating layer was composited with the impact-resistant layer, and the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0045] Example 5: by weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder contained glass powder A and glass powder B, and the mass ratio of glass powder A to glass powder B was 1:2. The impact-resistant layer was a single-ply glass fiber cloth, and the flame-retardant heat-insulating layer was composited with the impact-resistant layer, and the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0046] Example 6: by weight, containing 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder contained glass powder A and glass powder B, and the mass ratio of glass powder A to glass powder B was 2:3. The impact-resistant layer was a single-ply glass fiber cloth, and the flame-retardant heat-insulating layer was composited with the impact-resistant layer, and the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0047] Example 7: by weight, it contains 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder contains glass powder C, glass powder D and glass powder E. The mass ratio of glass powder C, glass powder D and glass powder E was 1:1:2. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0048] Example 8: by weight, it contains 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder contains glass powder C, glass powder D and glass powder E. The mass ratio of glass powder C, glass powder D and glass powder E was 1:2:3. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0049] Example 9: By weight, it contains 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder contains glass powder C, glass powder D and glass powder E. The mass ratio of glass powder C, glass powder D and glass powder E was 2:2:3. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0050] Example 10: by weight, containing 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder includes glass powder F, glass powder G, glass powder H and glass powder I. The mass ratio of glass powder F, glass powder G, glass powder H and glass powder I was 1:1:1:1. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0051] Example 11: By weight, it contains 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder contains glass powder F, glass powder G, glass powder H and glass powder I. The mass ratio of glass powder F, glass powder G, glass powder H and glass powder I was 1:1:2:2. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0052] Example 12: by weight, it contains 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder contains glass powder F, glass powder G, glass powder H and glass powder I. The mass ratio of glass powder F, glass powder G, glass powder H and glass powder I was 1:2:2:3. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0053] Example 13: By weight, it contains 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder and 2 parts of auxiliary. The glass powder contains glass powder F, glass powder G, glass powder H and glass powder I. The mass ratio of glass powder F, glass powder G, glass powder H and glass powder I was 1:1:1:2. The impact-resistant layer is a single-ply glass fiber cloth, the flame-retardant heat-insulating layer is composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer is 4:1, and the total thickness of the material is 1 mm.
[0054] Example 14: By weight, it contains 52 parts of organic silicone rubber, 27 parts of porcelain forming filler, 17 parts of extending filler, 23 parts of flame retardant, 5 parts of glass powder and 2 parts of auxiliary. The other contents are the same as those of Example 12.
[0055] Example 15: In parts by weight, it contains 47 parts of organic silicone rubber, 25 parts of porcelain forming filler, 15 parts of extending filler, 20 parts of flame retardant, 4 parts of glass powder and 2 parts of auxiliary agent. The other contents are the same as those of Example 12.
[0056] In the above embodiment, the number of glass powders with different initial melting temperatures is not limited to the contents disclosed in the present application, and the molten state temperature of the glass powders only needs to cover 300°C to 1500°C. That is, the mixing of glass powders is not limited to the mixing of glass powder A and glass powder B, and the mixing of glass powder C, glass powder D, and glass powder E, and the mixing of glass powder F, glass powder G, glass powder H, and glass powder I can be mixed with each other as long as they meet the requirements. And, it is not limited to the glass powder A, glass powder B, glass powder C, glass powder D, glass powder E, glass powder F, glass powder G, glass powder H, and glass powder I disclosed in the present application, and the glass powders can be mixed with each other as long as they meet the requirements of the temperature range of the molten state.
[0057] Example 16: by weight, it contains 47 parts of organic silicone rubber, 25 parts of porcelain-forming filler, 15 parts of extending filler, 20 parts of flame retardant, 4 parts of glass powder and 2 parts of auxiliary. The glass powder contains glass powder A, glass powder G, glass powder H and glass powder I. The mass ratio of glass powder A, glass powder G, glass powder H and glass powder I was 1:1:2:2. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0058] Example 17: by weight, it contains 47 parts of organic silicone rubber, 25 parts of porcelain-forming filler, 15 parts of extending filler, 20 parts of flame retardant, 4 parts of glass powder and 2 parts of auxiliary. The glass powder contains glass powder A, glass powder G, glass powder H and glass powder E. The mass ratio of glass powder A, glass powder G, glass powder H and glass powder E was 1:1:1:2. The impact-resistant layer is a single-ply glass fiber cloth, the flame-retardant heat-insulating layer is composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer and the impact-resistant layer is 4:1, and the total thickness of the material is 1 mm.
[0059] In the above embodiments, the glass powders having different initial melting temperatures are mixed with the organic silicone rubber, the porcelain-forming filler, the extending filler or the flame retardant alone, and the glass powders having different initial melting temperatures should not be mixed with the organic silicone rubber, the porcelain-forming filler, the extending filler or the flame retardant after mixing.
[0060] Comparative Example 1: By weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder, and 2 parts of auxiliary. The glass powder was glass powder A. The impact-resistant layer was a single-ply glass fiber cloth, and the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0061] Comparative Example 2: By weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder, and 2 parts of auxiliary. The glass powder was glass powder B. The impact-resistant layer was a single-ply glass fiber cloth, and the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0062] Comparative Example 3: By weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder, and 2 parts of auxiliary. The glass powder was glass powder C. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0063] Comparative Example 4: By weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder, and 2 parts of auxiliary. The glass powder was glass powder D. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0064] Comparative Example 5: By weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder, and 2 parts of auxiliary. The glass powder was glass powder E. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0065] Comparative Example 6: By weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder, and 2 parts of auxiliary. The glass powder was glass powder F. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0066] Comparative Example 7: By weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder, and 2 parts of auxiliary. The glass powder was glass powder G. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0067] Comparative Example 8: By weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder, and 2 parts of auxiliary. The glass powder was glass powder H. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0068] Comparative Example 9: By weight, it contained 45 parts of organic silicone rubber, 27 parts of porcelain-forming filler, 14 parts of extending filler, 22 parts of flame retardant, 8 parts of glass powder, and 2 parts of auxiliary. The glass powder was glass powder I. The impact-resistant layer was a single-ply glass fiber cloth, the flame-retardant heat-insulating layer was composited with the impact-resistant layer, the thickness ratio of the flame-retardant heat-insulating layer to the impact-resistant layer was 4:1, and the total thickness of the material was 1 mm.
[0069] The composite of the flame-retardant heat insulating layer and the impact resistant layer in all the examples and comparative examples was obtained by the following manufacturing method.
[0070] S1: Glass powders having different initial melting temperatures were mixed alone with organic silicone rubber, porcelain-forming filler, extender filler, flame retardant, and other auxiliary agents other than vulcanizing agent in an internal mixer in several batches, and further kneaded to obtain a rubber mixture.
[0071] S2: The rubber mixture was placed in a vulcanizer and a vulcanizing agent was added to obtain a flame-retardant, heat-insulating, fire-resistant silicone rubber.
[0072] S3: The flame-retardant heat-insulating fire-resistant silicone rubber was applied to the impact-resistant layer (i.e., glass fiber cloth), rolled, and the vulcanization temperature was controlled at 130℃~160℃.
[0073] Finally, a flame-retardant heat insulating and fire-preventing material for batteries was obtained.
[0074] Performance tests were carried out on Examples 4 to 17, and the test criteria and results were as follows.
[0075] Density: ASTM D792-2013, density meter. In Examples 4 to 17, the density was 1.6±0.1 g / cm 3 It was.
[0076] Tensile strength: ASTM D412, tensile machine. In examples 4 to 17, the tensile strength exceeded 15 MPa.
[0077] Flame retardancy: UL94, horizontal and vertical combustion tester. In Examples 4 to 17, the flame retardancy was V0.
[0078] Thermal conductivity: ASTM D5470, thermal conductivity tester. In Examples 4 to 17, the thermal conductivity was 0.3 W / (m·K) or less.
[0079] Withstand voltage: voltage adjusted to 2700 V DC, time 60 s, leakage current, withstand voltage tester. In Examples 4 to 17, the leakage current was less than 1 mA.
[0080] Insulation: voltage adjusted to 1000 V DC, time 60 s, resistance, insulation tester. In Examples 4 to 17, the resistance exceeded 1 GΩ.
[0081] Voltage Breakdown: ASTM D149, Voltage Breakdown Tester. Examples 4 to 17 had a breakdown voltage of over 20 kv.
[0082] Hardness: ASTM D2240, hardness tester. Examples 4 to 17 had a hardness of 65±7 Shore A.
[0083] Water absorption: 24-h water absorption mass ratio. In Examples 4 to 17, the water absorption was 3% or less.
[0084] Ozone aging resistance: ASTM D1171, ozone concentration 2 ppm, temperature 23° C., humidity 65%, tensile 15%, moisturizing 46 h. In Examples 4 to 17, there were no cracks.
[0085] Low temperature properties: -40°C / 24 hours, folded 180°. No cracks were observed in Examples 4 to 17.
[0086] Long-term weather resistance: 500 cycles between -40℃ and 85℃ with a temperature gradient of 5℃ / min or less, and in each cycle, the maximum and minimum temperatures were held for 15min respectively. 85℃, 85% humidity, 1000h. Aged at 120℃ for 1200h. In Examples 4 to 17, all the above performances can still meet the standard requirements after undergoing high and low temperature cycles, high temperature and high humidity, and high temperature aging, respectively.
[0087] Deflagration tests were carried out at different pressures for Examples 4 to 17 and Comparative Examples 1 to 9. The results are shown in Table 1.
[0088] Table 1: Deflagration test of Examples 4 to 17 and Comparative Examples 1 to 9 in a state where they are combined with glass fibers [Table 1] JPEG2024539811000003.jpg92124JPEG2024539811000004.jpg24124JPEG2024539811000005.jpg103124
[0089] The term "ceramic complete" means that the surface of the flame-retardant heat insulating and fire-protecting material for batteries prepared in the examples is relatively complete after the deflagration test, and has no obvious defects.
[0090] The term "ceramic cracking" means that obvious cracks appear on the surface of the flame-retardant heat insulating and fire-protecting material for batteries prepared in the examples after the deflagration test.
[0091] The term "ceramic destruction" means that obvious pores and cracks are generated on the surface of the flame-retardant heat insulating and fire-protecting material for batteries prepared in the examples after the deflagration test.
[0092] The ceramic completeness, ceramic cracks and ceramic destruction can be seen in Figures 1 to 3, and the states of each embodiment and comparative example are actually slightly different after the deflagration test. As can be seen from Table 1, at 30 min, 1500°C flame shock, and 3 standard atmospheric pressure, the body integrity of the embodiments 4 to 17 can be guaranteed, while the insulation and fire protection functions of the comparative examples 1 to 9 have already been partially lost.
[0093] At 30 min, 1500°C flame impact, and 5 standard atmospheric pressure, the heat insulating and fireproofing performance of Examples 4 to 17 was reduced, but still had a certain heat insulating and fireproofing function. Comparative Examples 1 to 9 all lost their heat insulating and fireproofing functions.
[0094] At 15 min, 1500° C. flame shock, and 5 standard atmospheric pressure, most of the examples 4 to 17 still had their heat insulating and fireproofing functions, while all of the comparative examples 1 to 9 lost their heat insulating and fireproofing functions.
[0095] At 15 min, 1500° C. flame shock, and 7 standard atmospheric pressure, some of the examples 4 to 17 lost their heat insulating and fireproofing functions, and all of the comparative examples 1 to 9 lost their heat insulating and fireproofing functions.
[0096] After 15 minutes of flame shock at 1500° C. and 10 standard atmospheric pressure, all of the heat insulating and fireproofing functions of Examples 4 to 17 and Comparative Examples 1 to 9 were lost.
[0097] As can be seen from Table 1, Examples 4 to 17 have completely superior performance to Comparative Examples 1 to 9, and show that the performance of the heat insulating fireproof material that completely covers in the molten state is superior to the heat insulating fireproof material that partially covers. As can be seen from the different temperature and atmospheric pressure conditions in Examples 4 to 17, when the content of high melting point glass powder is higher than that of low melting point glass powder, the performance of the heat insulating fireproof material is better as in Examples 12 to 17. When the content of high melting point glass powder and low melting point glass powder are equal, the performance is reduced. Due to the fast deflagration temperature rise, the temperature quickly reaches 1500 ° C., and it was presumed that in order to burn at 1500 ° C. for a long time, the glass powder needs to be in a molten state at 1500 ° C. for a long time.
[0098] In Example 4 to Example 17 and Comparative Example 1 to Comparative Example 9, the flame-retardant heat insulating layer was produced by itself according to the blending ratio of the raw materials for forming the flame-retardant heat insulating layer, and the deflagration test was carried out under different pressures. The details are shown in Table 2.
[0099] Table 2: Deflagration test of Examples 4 to 17 and Comparative Examples 1 to 9 without glass fiber [Table 2] JPEG2024539811000007.jpg88124
[0100] As can be seen from Table 2, without the impact-resistant layer, Examples 4 to 17 and Comparative Examples 1 to 9 could not withstand the deflagration test at 15 min, 1500 ° C flame impact, and 2 standard atmospheric pressure, i.e., when the flame-retardant heat-insulating layer is not combined with the impact-resistant layer, its heat-insulating and fire-resistant performance is insufficient. At the same time, in the deflagration test at 15 min, 1500 ° C flame impact, and 1 standard atmospheric pressure, the main body structure of most of the flame-retardant heat-insulating layers of Comparative Examples 1 to 9 was already incomplete and could not be used normally. On the contrary, in Examples 4 to 17, cracks and destruction of the ceramic phase occurred only in the deflagration test at 15 min, 1500 ° C flame impact, and 1.5 standard atmospheric pressure.
[0101] Deflagration tests were carried out at different temperatures for Examples 4 to 17. The results are shown in Table 3.
[0102] Table 3: Deflagration tests at different temperatures after compounding with glass fibers of Examples 4 to 17 and Comparative Examples 1 to 9. [Table 3] JPEG2024539811000009.jpg65124JPEG2024539811000010.jpg53124
[0103] As can be seen from Table 3, at 15 min, 700°C flame shock, 5 standard atmospheric pressure and 15 min, 1000°C flame shock, 5 standard atmospheric pressure, Examples 4 to 17 can guarantee basic heat insulation and fire retardancy. Comparative Examples 1 to 9 have different conditions due to the different glass powders added. At 700°C, the comparative example with low melting point glass powder added can still guarantee basic heat insulation and fire retardancy, while the comparative example with high melting point glass powder added cannot form a complete ceramic layer after low temperature combustion for a long time. Adding high melting point glass powder alone is effective only when the temperature rises rapidly to 1500°C.
[0104] As can be seen from the above experiments, the flame-retardant heat insulating material in which the temperature range of the molten state of the glass powder covers 300°C to 1500°C in the present application has better performance than the flame-retardant heat insulating material in which the initial melting temperature of the glass powder is single. The principle of being able to withstand a high temperature of 1500°C for a long time in a high pressure environment is that a part of the glass powder can always be kept in a molten state at 350°C or higher, and the silica substrate and the glass powder are seamlessly combined to maximize the continuity, integrity and density of the ceramic layer. If only glass powder with a single initial melting temperature is added, it will only be able to withstand low temperature combustion, or the ceramic layer will be destroyed during low temperature combustion.
[0105] Generally, the thicker the total thickness of the material, the better the impact resistance and flame retardant heat insulation performance of the material, and in this specific embodiment, the total thickness of the material to be tested is about 1 mm. However, the thickness of the material in this application is not limited to the thickness disclosed in the specific embodiment, and in different application scenarios, the thickness of the impact resistance layer, the thickness of the flame retardant heat insulation layer, and the total thickness of the material can be set according to actual needs.
Claims
1. A flame-retardant heat insulating and fire-resistant material for batteries, comprising: In addition to containing organic silicone rubber, porcelain-forming filler, flame retardant and auxiliary, the flame retardant heat-insulating layer further contains glass powders having several different initial melting temperatures, and an impact-resistant layer, the flame retardant heat-insulating layer is applied on the surface of the impact-resistant layer, the thickness ratio of the flame retardant heat-insulating layer to the impact-resistant layer is (2-10):1, and the temperature range of the melting state of several glass powders covers 300°C to 1500°C. A flame-retardant heat insulating and fireproof material for batteries.
2. The impact resistant layer is a glass fiber cloth.
2. The flame-retardant heat insulating and fireproof material for batteries according to claim 1.
3. The impact-resistant layer is a multi-layer composite of glass fiber cloth.
3. The flame-retardant heat insulating and fireproof material for batteries according to claim 2.
4. The glass powder includes glass powder A having a temperature range in a molten state of 300°C to 700°C and glass powder B having a temperature range in a molten state of 700°C to 1500°C, and the mass ratio of glass powder A to glass powder B is 1-2:1-3.
2. The flame-retardant heat insulating and fireproof material for batteries according to claim 1.
5. The glass powder includes glass powder C having a temperature range in a molten state of 300°C to 550°C, glass powder D having a temperature range in a molten state of 550°C to 900°C, and glass powder E having a temperature range in a molten state of 900°C to 1500°C, and the mass ratio of glass powder C, glass powder D, and glass powder E is 1-2:1-2:2-3.
2. The flame-retardant heat insulating and fireproof material for batteries according to claim 1.
6. The glass powder includes glass powder F having a temperature range in a molten state of 300°C to 800°C, glass powder G having a temperature range in a molten state of 600°C to 1000°C, glass powder H having a temperature range in a molten state of 700°C to 1250°C, and glass powder I having a temperature range in a molten state of 1000°C to 1500°C, and the ratio of glass powder F, glass powder G, glass powder H, and glass powder I is 1-3:1-3:1-3:1-3:1-3 by mass.
2. The flame-retardant heat insulating and fireproof material for batteries according to claim 1.
7. The raw material of the glass powder includes one or more selected from silicon oxide, boron oxide, and metal oxide; The flame-retardant heat insulating and fireproof material for batteries according to any one of claims 1 to 6.
8. The metal oxide includes one or more selected from lead oxide, aluminum oxide, lithium oxide, zinc oxide, titanium oxide, magnesium oxide, vanadium oxide, barium oxide, sodium oxide, calcium oxide, strontium oxide, tin oxide, bismuth oxide, and antimony oxide; The flame-retardant heat insulating and fireproof material for batteries according to any one of claims 6 to 8.
9. The glass powder raw material further includes stannous fluoride; The flame-retardant heat insulating and fireproof material for batteries according to any one of claims 6 to 8.
10. In parts by weight, the flame-retardant heat-insulating layer comprises 40 parts to 60 parts of an organic silicone rubber, 20 parts to 30 parts of a porcelain-forming filler, 15 parts to 25 parts of a flame retardant, 2 parts to 10 parts of a glass powder, and 2 parts to 5 parts of an auxiliary agent; The flame-retardant heat insulating and fireproof material for batteries according to any one of claims 1 to 6.
11. The flame retardant insulation layer further comprises 10 to 17 parts of an extending filler; The flame-retardant heat insulating and fireproof material for batteries according to claim 10.
12. Flame-retardant heat insulation and fire protection materials will not melt down for at least 30 minutes when exposed to a flame shock of 1500℃.
2. The flame-retardant heat insulating and fireproof material for batteries according to claim 1.
Citation Information
Patent Citations
Preparation method of ceramic fire-resistant silicone rubber composite material
CN110862687A
Reactive flame-retardant porcelainized powder and reinforced flame-retardant porcelainized organic silicon elastomer using same
CN113087969A
Ceramic flame-retardant heat-insulating fireproof material and preparation method and application thereof
CN113829701A
Preparation method of silicon-ceramic composite material and high-performance fireproof silicon-ceramic / mica composite material
CN114921968A
Blending production method of flame-retardant heat-insulation fireproof material for battery
CN115491037A