Adsorbents containing boron oxide and related methods and devices - Patents.com
A boron oxide-coated porous adsorbent base effectively adsorbs impurities from semiconductor gases, addressing the challenge of delivering ultra-pure feedstock gases to reduce defects in microelectronic devices.
Patent Information
- Application Number
- JP2024523958
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-27
- Filing Date
- 2022-10-24
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The semiconductor manufacturing industry faces challenges in delivering feedstock gases with extremely low levels of impurities due to atmospheric and system-generated contaminants, which can cause defects in microelectronic devices, despite the use of specialized storage and delivery systems.
A novel adsorbent material comprising a porous adsorbent base with boron oxide on its surface, particularly using activated carbon or pyrolytic carbon, effectively adsorbs trace amounts of moisture, metals, and hydrocarbons from gases like halides and hydrides by applying boric acid to form boron oxide on the surface of the base.
The boron oxide-containing adsorbent significantly reduces impurities in feedstock gases by at least 20-60%, ensuring high-purity delivery to semiconductor processing tools, thereby minimizing defects in microelectronic devices.
Smart Images

Figure 2024539921000001_ABST
Abstract
Description
[Technical field]
[0001] The present specification relates to a porous adsorbent base and a boron oxide-containing adsorbent comprising boron oxide on a surface of the base, as well as devices comprising the boron oxide-containing adsorbent, and related methods of preparing and using the boron oxide-containing adsorbent. [Background technology]
[0002] The semiconductor manufacturing industry uses source gases in the processing of semiconductor wafers and the production of microelectronic devices. These gases include halogens, hydrides, hydrogen halides, and other halogen-containing and non-halogen-containing gases.
[0003] Source gases must be used in high purity form. Impurities in the source gas will cause defects in the semiconductor wafers or microelectronic devices that are processed using the source gas. As advanced microelectronic devices become smaller and smaller, their sensitivity to the presence of impurities continues to increase, and source gases must be delivered to the semiconductor processing tools with lower and lower levels of impurities.
[0004] The steps of synthesizing, isolating, purifying, handling, storing, transporting, and delivering the source gases to the semiconductor processing tools are carried out using highly contaminant-free conditions. Specialized storage and delivery systems have been developed to store, handle, and deliver the source gases to the semiconductor processing tools without allowing atmospheric contaminants to be carried in the gases.
[0005] However, even with high levels of precautions, small amounts of impurities from atmospheric or non-atmospheric sources are typically present in purified gases. Impurities can be present not only through exposure to atmospheric impurities, but can also potentially arise within the gas handling or storage system. Impurities can be generated during handling or storage of the feed gas by interaction of the feed gas with the handling or storage equipment. Impurities can also be generated by interaction of the gas with different impurities in the system, e.g., water. Because many feed gases are highly reactive (including halogens, hydrides, and hydrogen halides), impurities can arise during storage by chemically interacting the highly reactive feed gas with contaminants such as water, or with metallic parts of the storage or gas handling system, such as metallic flow control devices (pipes or conduits), vessel bodies, valves, etc.
[0006] Specific contaminants that may be present in the source gas at the point of use, i.e., delivery of the gas to the semiconductor processing tool, include water, metals, and hydrocarbons. Possible metal contaminants include elemental metals present in metal storage containers or metal conduits used to contain, transport, or handle the reagent gas, such as copper, molybdenum, nickel, iron, or cobalt. In the specific case of hydrogen chloride (HCl) gas, the hydrocarbon 2-chloropropane may be present and is known to cause defects on wafers. These contaminants can cause defects in the processed microelectronic devices even when the contaminants are present in only trace amounts, such as concentrations in the parts per billion (volume) range or less.
[0007] Suppliers and users of feed gases have a continuing need to reduce or eliminate trace impurities (e.g., metals, water, hydrocarbons) found in feed gases supplied to semiconductor processing tools at the point of use, i.e., at the tool. "Gas purifier" products have been developed and are commercially available that improve the final purity of the gaseous feed (i.e., the purity as it is delivered to the semiconductor processing tool) as the gas is supplied to the tool. Examples include the family of products sold by Entegris under the trade name GateKeeper® GPU Media Gas Purifiers. These products are useful for performing a final purification step on feed gases including halides, hydrides, hydrogen halides, and the like, such as: HCl, Cl2, B2H6, BCl3, CClH3, GeCl4, GeH4, H2S, H2Se, HBr, NF3, SiCl4, SiF4, SiH2Cl2, SiHCl3, SO2, CHClF2, BF3, HF, and HBr. Impurities that can be removed using these gas purifiers include traces of water, hydrocarbons (eg, toluene), and metals such as Fe, Ni, Mo, Cr and Mn, among others. Summary of the Invention
[0008] The following description relates to a novel sorbent material (or "purification material") for use in a method for adsorbing impurity gases present in a high purity reagent gas. The novel sorbent material includes a porous sorbent base structure (e.g., a particle or "monolith"), and boron oxide on a surface of the porous sorbent base. The novel sorbent material is referred to herein as a "boron oxide-containing sorbent," e.g., a "boron oxide-containing particle," or, for certain exemplary sorbents in the form of particles, simply as a "particle" or "sorbent particle," where the context permits.
[0009] The novel adsorbent material comprises an effective combination of a porous base structure (sometimes simply referred to as a "base"), which may be effective as an adsorbent material by itself, but the addition of boron oxide to the surface of the base structure provides added adsorption properties. In particular, the novel adsorbent material is effective in adsorbing trace amounts of moisture, metals, hydrocarbons, or combinations thereof, that would otherwise be present in pure feed gases, such as halides, hydrides, and hydrogen halides.
[0010] Particularly preferred boron oxide-containing adsorbents can be prepared using carbon-based adsorbent materials, such as activated carbon or pyrolytic carbon, in the form of porous adsorbent particles or monoliths as the base material. Activated carbon and pyrolytic carbon can function as very effective base materials for adsorbing impurity gas molecules due to the high surface area and high porosity of various activated carbon and pyrolytic carbon products. The highly inert and hygroscopic nature of boron oxide (B2O3) added to the carbon base results in a boron oxide-containing adsorbent that is very effective for adsorbing gaseous impurities, including water, gaseous metals, and hydrocarbons.
[0011] In one aspect, the present disclosure relates to a boron oxide-containing adsorbent, the adsorbent comprising a porous adsorbent base and boron oxide on a surface of the porous adsorbent base.
[0012] In another aspect, the invention relates to a purifier device that includes a purifier vessel having an interior, an inlet, an outlet, and a sorbent therein that contains the boron oxide described.
[0013] In another aspect, the present disclosure relates to a method of forming boron oxide on a surface of a porous adsorbent base, the method including applying an aqueous solution of boric acid to a surface of a porous adsorbent base, removing water from the boric acid solution, and forming boron oxide on the surface from the boric acid.
[0014] In yet another aspect, the present disclosure relates to a method of forming a porous adsorbent base having a surface coated with a boric acid solution, the method comprising applying an aqueous solution of boric acid to a surface of the porous adsorbent base.
[0015] In another aspect, the disclosure relates to a method for removing impurities from a reagent gas, the method comprising contacting the reagent gas with a porous adsorbent base and a boron oxide-containing adsorbent comprising boron oxide on a surface of the porous adsorbent base. [Brief description of the drawings]
[0016] [Figure 1] 1 shows an example of a process for preparing the described adsorbents. [Diagram 2] 1 shows a purifier device as described. [Diagram 3] A system is shown in which the described purifier device is used in the final purification step of reagent gases delivered to a semiconductor processing tool. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The figures are schematic and not necessarily to scale.
[0018] The following is a description of a porous sorbent base (e.g., base particle or monolith) that includes a porous surface, and a novel boron oxide-containing sorbent material that includes boron oxide located on the surface of the porous sorbent base. Also described are methods for preparing the novel sorbent material (e.g., particle or monolith), methods of using the novel sorbent material, and systems and devices, such as purifier devices and semiconductor processing tools, that include the novel sorbent material.
[0019] The novel sorbent material is in the form of a porous sorbent base structure that can be used as a porous base to support boron oxide on the surface of the base structure in a manner that allows the boron oxide to be effective as an adsorbent or purifier for removing gaseous impurities from a gas. In certain examples, the porous sorbent base can be in the form of individual porous particles (e.g., "inner particles," "core particles," or "base particles") that can be used as a porous base to support boron oxide on the surface of the particles in a manner that allows the boron oxide to be effective as an adsorbent or purifier for removing gaseous impurities from a gas. The base can be small granular particles, or in other examples, the base can be a "monolith" or "pack" of larger dimensions that can be used as a porous substrate to support boron oxide on the surface of the particles in a manner that allows the boron oxide to be effective as an adsorbent or purifier for removing gaseous impurities from a gas.
[0020] The boron oxide-containing sorbents described are not intended to include boron oxide granules, i.e., granules (or particles, or monolith structures) made solely of boron oxide. Boron oxide granules, i.e., granules containing substantially only boron oxide (as compared to the boron oxide-containing sorbents herein, which contain boron oxide formed on the surface of a different (non-boron oxide) type of porous sorbent base), are known for use, for example, in purifier products sold by Entegris as the "CR Series" of GateKeeper® GPU Media Gas Purifiers.
[0021] The boron oxide-containing sorbents described herein, including boron oxide-containing sorbent particles, differ from boron oxide granules at least because the boron oxide-containing sorbents described herein include a porous base structure (particle or "monolith") that may differ from boron oxide and may have different physical properties than those of boron oxide granules, e.g., higher porosity and higher surface area compared to boron oxide granules; and also because the boron oxide on the surface of the boron oxide-containing sorbents described herein is added separately to the surface of the porous sorbent base structure, i.e., applied to the surface of the porous sorbent base after the base is formed using a separate (prior) formation step.
[0022] The porous sorbent base may be any useful porous sorbent material upon which a quantity of boron oxide may be formed by the methods described, after which the porous sorbent base and the applied boron oxide become effective as a purifier or sorbent material for removing gas impurities from a reagent gas, such as a halide, hydride, or hydrogen halide.
[0023] Examples of adsorbent materials that may be useful as the porous adsorbent base include known types of porous adsorbent materials. Examples include carbon-based adsorbent media, polymeric adsorbent media, silica, etc. Specific examples include metal-organic frameworks ("MOFs"), including zeolite materials, particularly including zeolite imidazolate framework ("ZIF") adsorbents; silica and silica-based particles; alumina and alumina-based particles; and porous carbon adsorbent particles (sometimes referred to as "porous carbon particles" for short), including carbon adsorbent materials commonly referred to as "activated carbon particles," among other types of carbon particles.
[0024] Non-limiting examples of porous carbon sorbent materials useful as the porous sorbent base include carbon formed by pyrolysis of synthetic polymers, such as hydrocarbon, halocarbon (e.g., chlorocarbon), or hydrohalocarbon resins, such as polyacrylonitrile, polystyrene, sulfonated polystyrene-divinylbenzene, polyvinylidene chloride (PVDC), and the like; polymeric structure (PF) materials; porous organic polymers (POP); cellulose char; charcoal; and activated carbons formed from natural source materials, such as coconut shells, pitch, wood, petroleum, coal, and the like.
[0025] The porous sorbent base may be of any shape, form, size, etc. to support boron oxide on the surface of the base, and the combined structure of the base with the added boron oxide is effective such that the combination of the base and boron oxide is useful for adsorbing impurity gases from impurity-containing reagent gases. The size, shape and physical properties of the porous sorbent base, such as pore characteristics (pore size, porosity), can affect the ability of the base to adsorb impurities from impurity-containing reagent gases after boron oxide is applied to the surface of the base, and the packing density and void (interstitial) volume of the sorbent when contained in a purifier device.
[0026] The base (prior to forming boron oxide on the surface of the base) may have any suitable form, such as a granule or a structure referred to as a "monolith." Granules, also referred to as "particles," are an assembly of many individual pieces of porous adsorbent, each piece having a relatively small size, such as less than 3 centimeters, or less than 2 or 1 centimeter. The particles may have any useful particle size, shape, porosity, and size range. Examples of useful shapes and forms of the base structure include beads, granules, pellets, platelets, shells, saddles, powders, irregularly shaped particulate matter, pressed monoliths, extrudates of any shape and size, fabric or web-form material, honeycomb matrix monoliths, and composites (of adsorbent with other components), as well as crushed or crushed forms of the aforementioned types of adsorbent materials.
[0027] Useful or preferred base particles can have an average size in the range of 0.5 to 20 millimeters, e.g., 1 to 15 or 1 to 10 millimeters (mm). The average particle size of a collection of adsorbent particles can be measured by standard techniques including randomly selecting particles from the collection of particles and measuring the size (e.g., diameter) using a micrometer.
[0028] Useful or preferred particles may also have a shape that, in combination with the average size of the particles, results in a useful packing density and amount of void space between the particles when the particles are included in a purifier device. Exemplary shapes include rounded shapes, including substantially rounded, substantially spherical, or cylindrical particles. Exemplary preferred amounts of void space between sorbent particles (not including the headspace of the container) when the particles are included as sorbent particles in a purifier device (see Figures 2 and 3) may be less than 50 percent, e.g., less than 40, 30, or 25 percent.
[0029] As an alternative to a porous sorbent base in the form of particles having a relatively small size, e.g., dimensions less than 2 centimeters, the porous sorbent base may instead be larger in size and fewer sorbent structures may be accommodated in the purifier. In the sorbent art, sorbent structures that are larger in size or sized to closely fit the interior space of a storage vessel may in some cases be referred to as "monolith" type sorbent materials. Monolith sorbents have at least one dimension greater than 2 centimeters and may be in the form of a three-dimensional cylinder or "pack." Typically, one single monolith or a small number (e.g., 3-10) of monoliths are sized to fit into the purifier vessel.
[0030] Another characteristic of useful porous adsorbent bases (e.g., in the form of particles or as monoliths) is high surface area. Porous adsorbent bases, such as porous adsorbent carbon particles, may be characterized by the surface area of the porous adsorbent material. This type of surface area measurement may be performed by known nitrogen BET surface area measurement methods, for example, by using an Autosorb iQ instrument available from Anton-Paar, configured to use the BET (Brunauer, Emmett and Teller) method. According to useful or preferred examples, the porous adsorbent base material may exhibit a relatively high surface area, for example, a surface area of at least 500, 600 or 700 square meters per gram, for example, a surface area in the range of 700 to 1000 square meters per gram, or more.
[0031] The porous adsorbent base may be porous and may include an interconnected network of pores extending through the interior of the base structure. The pores may have any useful pore size, i.e., any pore size that allows for the desired adsorption performance of the base after boron oxide is formed on the surface of the base.
[0032] Pore sizes of adsorbent materials are classified into general ranges based on the average pore size of a collection of particles. Particles having an average pore size greater than 50 nanometers (nm) are typically referred to as macroporous. Particles having an average pore size in the range of 2-50 nanometers (nm) are typically referred to as mesoporous particles. Particles having an average pore size less than 2 nanometers are typically referred to as microporous. These terms are defined by IUPAC terminology. Base particles used in accordance with this specification may have an average pore size, or pore size range, that falls within any of these size range designations.
[0033] The porous adsorbent base may have pores in the macroporous range, pores in the mesoporous range, and pores in the microporous range. Desirably, for useful removal of impurities as described herein, the base may have a useful amount of pores in the microporous range, and even a useful amount of pores in the mesoporous range. Impurities have faster mass transfer rates in pores in the microporous or mesoporous size ranges compared to mass transfer rates in pores in the macroporous size range; for this reason (at least), the porous adsorbent base may preferably have a significant pore size distribution of pores in the microporous size range, mesoporous size range, or both.
[0034] Another characteristic of a porous adsorbent base material is porosity (sometimes referred to as "pore volume"), which is the amount (volume) of the porous adsorbent base occupied by pores per mass of the particle. Exemplary base particles may have a porosity of at least 0.2 milliliters per gram, for example, at least 0.35 milliliters per gram, and preferably at least 0.40 milliliters per gram.
[0035] Useful or preferred porous sorbent base materials include porous carbon sorbent particles, such as particles of activated charcoal and pyrolytic carbon. Activated charcoal is a granular material produced by a process that involves heating charcoal derived from natural sources (e.g., coconut shells or coal) to temperatures in the range of 800-1000 degrees Celsius to "activate" the material. After heating, impurities are removed from the material by acid washing. Generally, activated charcoal may have pore sizes in the range of 500-1000 nm, and a surface area of at least about 1000 square meters per gram.
[0036] Useful activated carbon particles may be of any effective size and shape, with typical forms being substantially rounded spherical beads, pellets, or granules. Preferred activated carbon particles may have good adsorption properties for various gases, even before boron oxide is formed on the particle surface, as described herein. Preferred particles may have relatively high porosity (e.g., at least 35 or 40 cubic centimeters per gram) and relatively high surface area (e.g., at least 400, 500, 600, or 700 square meters per gram).
[0037] Many types of activated carbon particles prepared from a variety of carbon sources are well known and many are commercially available, such as the beaded activated carbon products sold by Kureha Corporation of Japan.
[0038] According to the method of the present disclosure, boron oxide (BO) is formed on the surface of the porous adsorbent base. Since boron oxide is reactive with protic solvents such as water and has low solubility in other organic solvents, applying boron oxide directly to the surface of the adsorbent porous base as boron oxide is not a valid option. To overcome this difficulty in handling boron oxide in its boron oxide form, and to avoid the need to apply boron oxide directly to the surface of the porous adsorbent base, the present disclosure includes a method of forming boron oxide on the surface of the porous adsorbent base by applying a boric acid (ortho- or meta-boric acid) solution to the surface of the base, and then removing the solvent (e.g., water) from the applied boric acid solution, thereby chemically forming boron oxide on the surface, which may remain on the surface.
[0039] Boron oxide is a known chemical and may be formed from boric acid according to the following reaction: 2H3BO3→B2O3+3H2O(I)
[0040] This reaction is well known and is described, for example, in "Inorganic Syntheses" by W. Conard Fernelius, Vol. 2, McGraw-Hill, 1946, pp. 22-23; see also U.S. Pat. No. 6,522,457, the entire contents of which are incorporated herein by reference. The starting component is identified as orthoboric acid, H3BO3, although the intermediate reaction product, metaboric acid, HBO2, also serves well as a starting component. Hereinafter, reference to boric acid is intended to refer to both orthoboric acid and metaboric acid, unless otherwise specified.
[0041] To form boron oxide on the surface of a sorbent base (e.g., a particle monolith) as described, a boric acid solution is prepared and applied to the surface of the sorbent base. The method used to apply the solution to the surface of the sorbent base may be any useful application method, such as by spraying or otherwise coating the solution onto the base particles, or by dipping or soaking the base in the solution. After the boric acid solution is applied to the surface, the solvent (e.g., the original water) is removed from the solution, leaving behind boric acid, B(OH)3, on the surface.
[0042] The base and the boric acid coating on the surface of the base are substantially dry of moisture (i.e., liquid water) present in the applied boric acid solution. However, molecular water remains in the boric acid present on the surface of the base. To remove the water from the boric acid and chemically convert the boric acid to boron oxide, the base with the boric acid (from the dried boric acid solution) on its surface is further heated for a time and temperature effective to remove the water from the boric acid, thereby converting the boric acid to boron oxide, B2O3. This process may be referred to as a "dehydration" process. The resulting boric oxide forms a highly conformal coating on the surfaces of the pores of the porous adsorbent base. The boric acid solution may include boric acid in any solvent, with water being an effective solvent. The concentration of boric acid in the solution may be any concentration effective to apply a desired amount of boric acid to the surface of the adsorbent base to form a desired amount of boron oxide on the surface. An example of a useful concentration of boric acid (whether orthoboric or metaboric acid) may range from 0.1 to 10 M. Because water is an effective solvent for boric acid, the solvent used to form boron oxide on the surface of the base is referred to as water as an exemplary solvent.
[0043] After the boric acid solution is applied to the surface of the base, water is removed from the solution in a manner that chemically converts the boric acid to boron oxide according to Formula I, leaving the boron oxide on the surface of the porous adsorbent base in a desired amount. Converting the boric acid to boron oxide involves removing water from the solution and applying an amount of heat that is also sufficient to produce boron oxide according to Formula I.
[0044] The method of removing water and heating the solution to form boron oxide may be any effective method. Examples of useful equipment may be heaters, ovens, rotary evaporators, ovens with radiant or convection heat and optional agitation, etc. The dehydration step to convert the applied boric acid to boron oxide may be carried out in a dry atmosphere, preferably of high purity and substantially free of contaminants, optionally in the presence of an inert gas such as nitrogen, helium, etc.
[0045] Forming boron oxide according to the reaction of formula I does not require that all or substantially all of the water from the boric acid solution be removed from the solution or from the boron oxide reaction product at the surface of the porous adsorbent base. However, the methods herein may preferably include heating the boron oxide reaction product at a temperature and for a time useful for removing substantially all of the water from the boron oxide reaction product formed on the porous adsorbent base; this step of removing residual water from the boron oxide reaction product may be referred to as a "dehydration" step. Temperatures useful for removing residual water from the boron oxide reaction product, i.e., dehydrating the porous adsorbent base containing boron oxide, may be at least 120 degrees Celsius, e.g., 130 or 150 degrees Celsius, up to about 200 degrees Celsius.
[0046] The amount of water that remains present in the boron oxide containing adsorbent (e.g., particles or monolith) after boron oxide formation and after the dehydration step may be an amount of less than 0.5 weight percent water per total weight of the boron oxide containing adsorbent, such as less than 0.1 weight percent water per total weight of the boron oxide containing adsorbent.
[0047] The amount of boron oxide applied to the sorbent base may be an amount that produces a boron oxide-containing sorbent that is effective as an adsorbent for removing impurities from an impure reagent gas, for example by adsorbing the impurities. The amount is sufficient to provide effective adsorption properties of the boron oxide-containing sorbent, while not unduly interfering with the porosity of the porous sorbent base, i.e., not unduly filling the pores, particularly pores in the mesoporous or microporous size range of less than 10 or 2 nanometers. Examples of currently recognized useful amounts of boron oxide may be at least 2 weight percent boron oxide per gram of boron oxide-containing sorbent, for example, amounts in the range of 5 to 30 weight percent boron oxide per gram of boron oxide-containing sorbent.
[0048] The properties of the porous adsorbent base when boron oxide is applied to the surface of the porous adsorbent base are not unduly affected by the presence of the added boron oxide formed on the surface of the base, specifically, the physical characteristics of the boron oxide-containing adsorbent, i.e., the porous adsorbent base with boron oxide formed on its surface, may be comparable to the physical characteristics of the base particle before boron oxide is applied to its surface.
[0049] Useful or preferred boron oxide-containing sorbents may have shapes equivalent to the shape of the sorbent base.
[0050] When the base adsorbent is made from particles, the adsorbent particles containing boron oxide, when included as adsorbent particles in a purifier device (see Figures 2 or 3), exhibit voids between the adsorbent particles (not including the headspace of the container) that are comparable to that of the base particles, e.g., less than 50 percent, e.g., less than 40, 30 or 25 percent.
[0051] The boron oxide containing adsorbents can exhibit a relatively high surface area comparable to the surface area of the porous adsorbent base from which the boron oxide containing adsorbents are formed, e.g., a surface area of at least 400, 500, 600, or 700 square meters per gram, e.g., a surface area ranging from at least 400, 500, 700, or 1000 square meters per gram, or greater than 1000 square meters.
[0052] The boron oxide containing sorbent, like the porous sorbent base, is preferably porous and can include an interconnected network of pores that extend throughout the interior of the base structure. The pores can have any useful pore size and pore size distribution, meaning any pore size that allows for the desired adsorption of impurities onto the boron oxide containing sorbent.
[0053] The pore size of the boron oxide-containing adsorbent may be comparable to the pore size of the porous adsorbent base used to form the boron oxide-containing adsorbent prior to the formation of boron oxide on the surface of the porous adsorbent base. The boron oxide-containing adsorbent may have an average pore size greater than 50 nanometers (nm) (e.g., may be macroporous particles); may have an average pore size in the range of 2 to 50 nanometers (nm) (e.g., may be mesoporous particles); or may have an average pore size less than 2 nanometers (e.g., may be microporous). Desirably, the boron oxide-containing porous adsorbent may have a significant pore size distribution of pores in the microporous size range, the mesoporous size range, or both.
[0054] The porosity of the boron oxide-containing sorbent particles may be comparable to the porosity of the base particle prior to the formation of boron oxide at the surface of the base particle. Exemplary boron oxide-containing sorbent particles may have a porosity of at least 0.2-0.8 milliliters per gram.
[0055] FIG. 1 shows exemplary steps of a method for forming boron oxide on a base particle (alternatively, a monolithic porous sorbent base), such as activated carbon particles. In step 2, an aqueous solution of boric acid is applied to the base particle, which may be a carbon sorbent particle, e.g., activated carbon particles, pyrolytic carbon, or the like. A quantity of water may be removed from the aqueous solution disposed on the particle surface by any useful technique, and the aqueous solution and base particle may be exposed to an elevated temperature to cause the formation of boric acid. This initial water removal step may be carried out using any useful equipment and technique, such as the use of an oven, vacuum, or rotary evaporator.
[0056] The particles comprising a surface having a coating of boric acid can be further dried by any useful method to convert the boric acid to boron oxide. As shown in FIG. 1, the particles can first be placed inside a container of a purifier device (see FIGS. 2 and 3 and related description herein), and the purifier device and contained particles can be heated in an oven at a temperature of 140 degrees Celsius for a time sufficient to remove most of the remaining water from the particles, for example, to reduce the water content of the boron oxide-containing sorbent particles to less than about 2 weight percent, or less than 1 or 0.5 weight percent based on the total weight of the boron oxide-containing sorbent particles. This results in a purifier device container containing boron oxide-containing sorbent particles that have been dehydrated while in the purifier device, i.e., in situ.
[0057] The described boron oxide-containing adsorbents may be used to remove one or more impurity gases from a reagent gas that contains one or more impurity gases by contacting the reagent gas and the impurity gas with the boron oxide-containing adsorbent, the impurity gas being adsorbed onto the boron oxide-containing adsorbent but not the reagent gas, removing the impurities from the reagent gas and processing the reagent gas into a higher purity form with reduced levels of the impurities removed.
[0058] The process of purifying a reagent gas by removing impurities from the reagent gas, i.e., removing trace levels of contaminants, requires that when the reagent gas contacts a boron oxide-containing adsorbent, the contaminants (i.e., impurities) are effectively adsorbed to the surface of the boron oxide-containing adsorbent, but the reagent gas is not adsorbed. The reagent gas itself is not effectively adsorbed to the surface of the boron oxide-containing adsorbent when the reagent gas contacts the particles under process conditions, i.e., conditions that purify the reagent gas. Examples of reagent gases that are not substantially adsorbed to boron oxide-containing adsorbents as described include halides, hydrides, and hydrogen halides, such as HCl, Cl2, B2H6, BCl3, CClH3, GeCl4, GeH4, H2S, H2S3, NF3, SiCl4, SiF4, SiH2Cl2, SiHCl3, SO2, CHClF2, BF3, and HBr.
[0059] The impurity gases that may be removed from the reagent gas are those that are effectively adsorbed onto the surface of the boron oxide-containing adsorbent particles when the reagent gas (including the impurities) contacts the boron oxide-containing adsorbent particles under process conditions, i.e., conditions for purifying the reagent gas. Examples of impurities that may be adsorbed onto these particles include water, metals (e.g., copper, molybdenum, nickel, iron or cobalt), and hydrocarbons such as 2-chloropropane and toluene. When using boron oxide-containing adsorbent particles in a method for purifying a reagent gas, the particles may be contained within a vessel (a "purifier" vessel) that includes a vessel body defining an interior volume, an inlet (conduit, passage, opening, etc.) leading from the exterior to the interior, an outlet (conduit, passage, opening, etc.) leading from the interior to the exterior, and a collection of boron oxide-containing adsorbent particles therein.
[0060] 2, an exemplary purifier device 60 includes a vessel body 40 defining an interior 42 and containing a mass of boron oxide-containing sorbent particles 44 (alternatively, a monolithic boron oxide-containing sorbent). The vessel body 40 may be made from a material that is chemically resistant to the reagent gases that pass through the body 40 during use of the device 60 in a purification process. Examples of useful materials include stainless steel, nickel alloys, and Hastelloy metal alloys. Useful or preferred inner surfaces of the vessel may also be smoothed by polishing or electropolishing, for example, to a roughness of 20 Ra or 10 Ra.
[0061] 2, inlet 46 allows reagent gas 50 to enter interior 42. Reagent gas 50 may be any reagent gas that contains, for example, trace levels of impurities that may be adsorbed to particles 44 while the reagent gas passes through interior 42, and then exits interior 42 through outlet 52 with a reduced amount of impurities. The impurities remain adsorbed to particles 44, and purified reagent gas 52 passes through outlet 48.
[0062] 3 shows a semiconductor processing system 100 including a stored reagent gas 102 (containing trace levels of impurities), a purifier 104 including sorbent particles 108 containing boron oxide, and a semiconductor processing tool 106. The container 120 may be any storage container or other type of source of the reagent gas 102. The container 120 may be a pressurized or non-pressurized (e.g., sorbent-containing) storage container used to transport and store the reagent gas 102 and then connected to the tool 106 to deliver the reagent gas 102 to the tool 106 for processing. The container 120 may alternatively be a permanent or semi-permanent container housed in a clean room with the tool 106 or that is a component of the tool 106.
[0063] The container 120 contains the reagent gas 102 in a highly purified form for use in the tool 106. The gas 102 may be any reagent gas, such as a halogen, hydride, or hydrogen halide, of high purity, e.g., at least 99.9 or 99.99 percent pure by volume. The gas 102 may contain trace levels of impurities, such as water in an amount of less than 100 ppbv, one or more metals in an amount of less than 100 ppbv (of total metals), and hydrocarbons in an amount of less than 100 ppbv (of total hydrocarbons).
[0064] According to this specification, the gas 102 may pass through a purification device 104 and particles 108 for a "final filtration step" or "final purification step" to remove a certain amount of trace impurities from the gas 102 before delivering the purified form of the gas 102a to the tool 106. The gas 102a contains a reduced amount of one or more trace impurities, e.g., a reduced amount of water, hydrocarbon, or metal impurities, compared to the stored gas 102. The reduced amount of any single impurity (water, hydrocarbon or single hydrocarbon species, metal or single metal species) present in the purified gas 102a may be at least 20, 40, 50, or 60 percent (molar) reduced relative to the amount of a single impurity present in the stored gas 102.
[0065] In a particular example, the reagent gas 102 may be hydrogen fluoride (HF) of at least 99.99 percent (by volume) purity, which includes water as an impurity in an amount less than 100 ppbv. The reagent gas 102a delivered to the tool 106 has a reduced amount of water compared to the reagent gas 102 stored in the container 120 after being purified by passing through the purifier 104 and contacting the particles 108. The tool 106 may be an HF furnace, an etching tool, a cleaning tool, or another tool that uses hydrogen fluoride. In a different example, the reagent gas 102 may be hydrogen chloride gas (HCl) of at least 99.99 percent (by volume) purity, which includes 2-chloropropane as an impurity in an amount less than 100 ppbv. The reagent gas 102a delivered to the tool 106 has a reduced amount of 2-chloropropane compared to the reagent gas 102 stored in the container 120 after being purified by passing through the purifier 104 and contacting the particles 108. Tool 106 may be an etch tool or an epitaxy tool.
[0066] In a first embodiment, the boron oxide containing adsorbent comprises a porous adsorbent base and boron oxide on a surface of the porous adsorbent base.
[0067] In a second embodiment according to the first aspect, the porous adsorbent base comprises porous adsorbent carbon particles.
[0068] In a third embodiment according to the second embodiment, the porous adsorbent carbon particles are derived from natural carbon sources or synthetic hydrocarbon polymers.
[0069] The fourth embodiment according to any preceding embodiment, further comprising 70 to 95 weight percent of the porous adsorbent base, and 5 to 30 weight percent of boron oxide, based on the total weight of the porous adsorbent base and boron oxide.
[0070] In a fifth embodiment according to any preceding embodiment, the adsorbent consists essentially of a porous adsorbent base and boron oxide.
[0071] A sixth embodiment according to any preceding embodiment, having a surface area of at least 500 square meters per gram.
[0072] In a seventh embodiment according to any preceding embodiment, the porous adsorbent base comprises particles having an average diameter of less than 1 centimeter.
[0073] In an eighth embodiment according to any preceding embodiment, the porous adsorbent base comprises a monolith having a dimension of at least 2 centimeters.
[0074] A 9th embodiment, further comprising less than 1 weight percent water, based on the total weight of the boron oxide-containing adsorbent.
[0075] In a tenth embodiment according to any preceding embodiment, the adsorbent is prepared by a method comprising applying an aqueous solution of boric acid to a surface of a porous adsorbent base, removing water from the boric acid solution, and forming boron oxide on the surface from the boric acid.
[0076] In an eleventh embodiment according to the tenth embodiment, the method further comprises removing a quantity of water from the boric acid solution to leave boric acid on the surface, and heating the boric acid on the surface to remove the water from the boric acid and convert the boric acid to boric oxide.
[0077] In a twelfth embodiment, a purifier device includes an interior, an inlet, an outlet, and a purifier vessel containing therein a boron oxide-containing sorbent of any of the preceding embodiments.
[0078] In a thirteenth embodiment, there is provided a method of forming boron oxide on a surface of a porous adsorbent base, the method comprising applying an aqueous solution of boric acid to a surface of a porous adsorbent base, removing water from the boric acid solution, and forming boron oxide on the surface from the boric acid.
[0079] In a fourteenth embodiment according to the thirteenth embodiment, the porous adsorbent base comprises a porous carbon adsorbent.
[0080] A fifteenth embodiment according to the thirteenth or fourteenth embodiment, further comprising removing water from the boric acid solution using a rotary evaporator.
[0081] A sixteenth aspect according to any of the thirteenth to fifteenth aspects further includes, after removing water from the boric acid solution, placing the porous sorbent base within a container of a purifier device, and heating the purifier device and particles contained within the purifier device to a temperature in the range of 120-200 degrees Celsius to remove water from the boric acid and convert the boric acid to boric oxide.
[0082] In a seventeenth embodiment according to any of the thirteenth to sixteenth embodiments, the porous adsorbent base has a surface area of at least 500 square meters per gram.
[0083] In an eighteenth aspect according to any of the thirteenth to seventeenth aspects, an aqueous boric acid solution having a boric acid concentration in the range of 0.1 to 10 moles per liter.
[0084] In a nineteenth embodiment, a method of forming a porous adsorbent base having a surface coated with a boric acid solution comprises applying an aqueous solution of boric acid to a surface of the porous adsorbent base.
[0085] The twentieth embodiment according to the nineteenth embodiment further comprises removing water from the boric acid solution in a rotary evaporator using the porous adsorbent base.
[0086] In a twenty-first embodiment according to the nineteenth or twentieth embodiment, the porous adsorbent base comprises carbon particles.
[0087] In a twenty-second embodiment according to any of the nineteenth to twenty-first embodiments, the porous adsorbent base has a surface area of at least 500 square meters per gram.
[0088] In a twenty-third embodiment, a method for removing impurities from a reagent gas includes contacting the reagent gas with a boron oxide-containing adsorbent comprising a porous adsorbent base and boron oxide on a surface of the porous adsorbent base.
[0089] In a twenty-fourth embodiment according to the twenty-third embodiment, the porous adsorbent base comprises carbon particles.
[0090] In a twenty-fifth embodiment according to the twenty-third or twenty-fourth embodiment, the boron oxide-containing sorbent comprises 70 to 95 weight percent of the porous sorbent base, and 5 to 30 weight percent of the boron oxide, based on the total weight of the porous sorbent particles and the boron oxide.
[0091] In a twenty-sixth embodiment according to any of the twenty-third to twenty-fifth embodiments, the boron oxide containing adsorbent has a surface area of at least 500 square meters per gram.
[0092] In a 27th embodiment according to any of the 23rd to 26th embodiments, the reagent gas comprises a halide, hydride, or hydrogen halide, impurities comprise water, a metal, or a hydrocarbon.
[0093] In a 28th embodiment according to any of the 23rd to 27th embodiments, the reagent gas comprises HCl, Cl2, B2H6, BCl3, CClH3, GeCl4, GeH4, H2S, H2S3, NF3, SiCl4, SiF4, SiH2Cl2, SiHCl3, SO2, CHClF2, BF3, and HBr.
[0094] In a 29th embodiment according to any of the 23rd to 27th embodiments, the reagent gas is hydrogen chloride gas (HCl) and the impurity is 2-chloropropane.
[0095] In a 30th embodiment according to any of the 23rd to 27th embodiments, the reagent gas is hydrogen fluoride (HF) and the impurity is water.
Claims
1. An adsorbent containing boron oxide, Porous adsorbent-based, and Boron oxide on porous adsorbent-based surfaces An adsorbent comprising:
2. 10. The sorbent of claim 1, wherein the porous sorbent base comprises porous sorbent carbon particles.
3. 3. The adsorbent of claim 2, wherein the porous adsorbent carbon particles are derived from natural carbon sources or synthetic hydrocarbon polymers.
4. Based on the total weight of the porous adsorbent base and boron oxide, 70 to 95 weight percent of a porous adsorbent base; and 5 to 30 weight percent boron oxide The adsorbent of claim 1 , further comprising:
5. 5. The adsorbent of any one of claims 1 to 4, consisting essentially of a porous adsorbent base and boron oxide.
6. 6. The adsorbent of any one of claims 1 to 5, having a surface area of at least 500 square meters per gram.
7. 7. The adsorbent of any one of claims 1 to 6, wherein the porous adsorbent base comprises particles having an average diameter of less than 1 centimeter.
8. 7. The adsorbent of any one of claims 1 to 6, wherein the porous adsorbent base comprises a monolith having a dimension of at least 2 centimeters.
9. 9. The adsorbent of any one of claims 1 to 8, comprising less than 1 weight percent water, based on the total weight of the adsorbent containing boron oxide.
10. applying an aqueous solution of boric acid to a surface of the porous adsorbent base; removing water from the boric acid solution; and Forming boron oxide on the surface from boric acid 10. The adsorbent of claim 1 , prepared by a process comprising:
11. The method is removing a quantity of water from the boric acid solution to leave the boric acid on the surface; and Heating the boric acid on the surface to remove water from the boric acid and convert it to boric oxide The adsorbent of claim 10 further comprising:
12. 12. A purifier device comprising an interior, an inlet, an outlet, and a purifier vessel containing therein a boron oxide-containing sorbent according to any one of claims 1 to 11.
13. 1. A method for forming boron oxide on a surface of a porous adsorbent base, comprising: applying an aqueous solution of boric acid to a surface of the porous adsorbent base; removing water from the boric acid solution; and Forming boron oxide on the surface from boric acid A method comprising:
14. The method of claim 13 , wherein the porous adsorbent base comprises a porous carbon adsorbent.
15. 15. The method of claim 13 or 14, comprising removing water from the boric acid solution using a rotary evaporator.
16. placing the porous adsorbent base in a container of a purifier device after removing water from the boric acid solution; and heating the purifier device and particles contained therein to a temperature in the range of 120-200 degrees Celsius to remove water from the boric acid and convert the boric acid to boric oxide.
16. The method of any one of claims 13 to 15, further comprising:
17. 17. The method of any one of claims 13 to 16, wherein the porous adsorbent base has a surface area of at least 500 square meters per gram.
18. 18. The method according to any one of claims 13 to 17, wherein the aqueous boric acid solution has a boric acid concentration in the range of 0.1 to 10 moles per liter.
19. A method for forming a porous adsorbent base having a surface coated with a boric acid solution, the method comprising applying an aqueous solution of boric acid to a surface of the porous adsorbent base.
20. 20. The method of claim 19, further comprising removing water from the boric acid solution by rotary evaporating the porous adsorbent base.
21. 21. The method of claim 19 or 20, wherein the porous adsorbent base comprises carbon particles.
22. 22. The method of any one of claims 19 to 21, wherein the porous adsorbent base has a surface area of at least 500 square meters per gram.
23. A method for removing impurities from a reagent gas, the method comprising contacting the reagent gas with a boron oxide-containing adsorbent comprising a porous adsorbent base and boron oxide on a surface of the porous adsorbent base.
24. 24. The method of claim 23, wherein the porous adsorbent base comprises carbon particles.
25. The boron oxide-containing adsorbent has a total weight of: 70 to 95 weight percent of a porous adsorbent base; and 5 to 30 weight percent boron oxide 25. The method of claim 23 or 24, comprising:
26. 26. The method of any one of claims 23 to 25, wherein the boron oxide containing adsorbent has a surface area of at least 500 square meters per gram.
27. the reagent gas comprises a halide, hydride, or hydrogen halide; 27. The method of any one of claims 23 to 26, wherein the impurities comprise water, metals, or hydrocarbons.
28. The reagent gases are HCl, Cl 2 , B 2 H 6 , BCl 3 , CClH 3 , GeCl 4 , GeH 4 , H 2 S, H 2 S 3 , N.F. 3 , SiCl 4 , SiF 4 , SiH 2 C 2 , SiHCl 3 , S.O. 2 , CHClF 2 , B.F. 3 and HBr.
29. 28. The method of any one of claims 23 to 27, wherein the reagent gas is hydrogen chloride gas (HCl) and the impurity is 2-chloropropane.
30. 28. The method of any one of claims 23 to 27, wherein the reagent gas is hydrogen fluoride (HF) and the impurity is water.
Citation Information
Patent Citations
JP1975131891A
Large-sized video image display device
JP1984039180A
Method for removing moisture from evacuated room or gas
JP2000005552A
Gas adsorption composition and device, and method for producing them
JP2006519098A
Process for the removal of water from evacuated chambers or from gases
US20020044334A1