Anti-fog paint, its manufacturing method, and anti-fog glass

A single-layer anti-fog coating using a hydrophilic copolymer and epoxy resin addresses the fogging issue on automotive glass, enhancing adhesion and durability while reducing energy consumption and production complexity.

JP2024539965AActive Publication Date: 2024-10-31FUYAO GLASS IND GROUP CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024524672
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-05
Filing Date
2022-11-04
Publication Date
2024-10-31
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

Automotive glass fogs up due to temperature and humidity differences, leading to reduced visibility and potential accidents, and existing anti-fog solutions like air-conditioning and electric heating have high energy consumption and complexity.

Method used

A single-layer anti-fog coating composed of a hydrophilic copolymer and epoxy resin with a coupling agent, forming a semi-interpenetrating network structure for improved adhesion and stress relief, eliminating the need for a base layer.

Benefits of technology

The single-layer coating effectively prevents fogging, extends service life, reduces energy consumption, and simplifies production by eliminating the need for a base layer, while maintaining excellent adhesion and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024539965000001_ABST
    Figure 2024539965000001_ABST
Patent Text Reader

Abstract

The present application relates to an anti-fog coating, a manufacturing method thereof, and an anti-fog glass, in which the manufacturing raw materials of the anti-fog coating include a hydrophilic copolymer, an epoxy resin, a coupling agent, a curing agent, and a first solvent, the manufacturing raw materials of the hydrophilic copolymer include a hydrophilic monomer, an initiator, and a second solvent, the solubility of the epoxy resin in water is about 90% or more, and the solubility of the hydrophilic copolymer in water is about 90% or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to a Chinese patent application filed on November 5, 2021, bearing application number 202111305548.3 and entitled "Anti-fog paint and its manufacturing method, and anti-fog glass," the entire text of which is incorporated herein by reference.

[0002] The present application relates to the technical field of vehicle glass, and in particular to an anti-fog coating material and a manufacturing method thereof, and an anti-fog glass. [Background technology]

[0003] Automotive glass is prone to fogging under conditions where there is a large difference in temperature and humidity between the inside and outside of the vehicle, and the fogging affects the driver's visibility and may even cause accidents. Air conditioning blowing and electric heating methods are commonly used to remove fog, but these methods have hysteresis and high energy consumption.

[0004] At present, a technical solution has been disclosed for eliminating the fogging phenomenon by producing two coating layers on the glass substrate of an automobile. In one technical solution, the two-layer structure includes a water-absorbent anti-fogging layer that plays the role of anti-fogging and a base layer that plays the role of connection buffer. The water-absorbent anti-fogging layer repeatedly absorbs and releases water during use, and the coating layer expands and contracts, generating large interfacial stress. If only a single layer of water-absorbent anti-fogging layer is used, the adhesive strength between the coating layer and the substrate will be reduced due to the interfacial stress, and peeling problems are likely to occur. Therefore, it is particularly important to add one layer of base layer, which can be tightly bonded to the substrate and relieve the interfacial stress caused by the water-absorbent anti-fogging layer, and further improve the overall peeling resistance. However, the process of forming two coating layers is complicated and increases the production cost. Summary of the Invention [Problem to be solved by the invention]

[0005] On this basis, according to various embodiments of the present application, an anti-fog paint is provided, the technical solutions of which are as follows: [Means for solving the problem]

[0006] An anti-fog paint, the manufacturing raw materials of which include a hydrophilic copolymer, an epoxy resin, a coupling agent, a curing agent and a first solvent, the manufacturing raw materials of the hydrophilic copolymer include a hydrophilic monomer, an initiator and a second solvent, the solubility of the epoxy resin in water is about 90% or more, and the solubility of the hydrophilic copolymer in water is about 90% or more.

[0007] In some embodiments, the hydrophilic monomer is a combination of an acrylate monomer and an acrylic acid amide monomer.

[0008] In some embodiments, the acrylic ester monomer is hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, glycidyl acrylate, glycidyl methacrylate, or a combination thereof.

[0009] In some embodiments, the acrylic acid amide monomer is acrylamide, N,N-dimethylacrylamide, 2-acrylamido-2-methylpropanesulfonic acid, or a combination thereof.

[0010] In some embodiments, the epoxy resin is an aliphatic glycidyl ether, and the aliphatic glycidyl ether is trimethylolpropane triglycidyl ether, glycerin triglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether, sorbitol glycidyl ether, or a combination thereof.

[0011] In some embodiments, the weight ratio of the hydrophilic copolymer to the epoxy resin is about (1-4:1).

[0012] In some embodiments, the ingredients of the antifog coating include, in parts by weight, about 1 part to about 80 parts of a hydrophilic copolymer, about 1 part to about 20 parts of an epoxy resin, about 0.1 parts to about 10 parts of a coupling agent, about 0.4 parts to about 15 parts of a curing agent, and about 20 parts to about 50 parts of a first solvent.

[0013] In some embodiments, the coupling agent is gamma-methacryloxypropyltrimethoxysilane, gamma-aminopropyltriethoxysilane, gamma-glycidoxypropyltrimethoxysilane, divinyltriaminopropyltrimethoxysilane, ureidopropyltriethoxysilane, or a combination thereof.

[0014] In some embodiments, the curing agent is diethylenetriamine, hydroxyethylethylenediamine, isophoronediamine, or a combination thereof.

[0015] In some embodiments, the initiator is a radical initiator that contains a nitrogen-nitrogen double bond.

[0016] In some embodiments, the first and second solvents are each independently an alcohol-based solvent or an ether-based solvent.

[0017] In some embodiments, the anti-fog coating material further comprises a silane hydrolysis catalyst, a filler, an antioxidant, an ultraviolet light absorber, a leveling agent, or a combination thereof.

[0018] In some embodiments, the silane hydrolysis catalyst is a base catalyst or an acid catalyst.

[0019] In some embodiments, the filler is nano-silica, nano-alumina, or a combination thereof.

[0020] In some embodiments, the antioxidant is triethylene glycol-bis(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, octyl-3,5-di-tert-butyl-4-hydroxy-hydrocinnamate, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-bis-3-(3'5'di-tert-butyl-4'-hydroxyphenyl)propionylhexamethylenediamine, or a combination thereof.

[0021] In some embodiments, the UV absorber is 2,2',4,4'-tetrahydroxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, or a combination thereof.

[0022] In some embodiments, the anti-fog coating material further comprises an accelerator, the accelerator being methyllithium, triethylaluminum, ethylmagnesium iodide, methylzinc chloride, trimethyllead hydride, or a combination thereof.

[0023] The present application further provides a method for producing the above anti-fog paint, the technical solution of which is as follows: The method for producing an anti-fog coating includes the steps of mixing a hydrophilic monomer, an initiator and a second solvent, carrying out a polymerization reaction to produce a hydrophilic copolymer, and mixing the hydrophilic copolymer, an epoxy resin, a coupling agent, a curing agent and a first solvent, carrying out a cross-linking reaction to produce an anti-fog coating.

[0024] The anti-fog glass includes a glass substrate and an anti-fog coating layer on the glass substrate, the anti-fog coating layer being formed from the above-mentioned anti-fog paint applied to the glass substrate, and the thickness of the anti-fog coating layer is about 5 μm to 30 μm.

[0025] In some embodiments, the glass substrate is a curved glass plate, the curved glass plate having a convex surface and a concave surface, the anti-fog coating layer is disposed on the concave surface, the anti-fog coating has a maximum thickness and a minimum thickness, and the difference between the maximum thickness and the minimum thickness is about 1 μm to 5 μm.

[0026] In some embodiments, the anti-fog glass further comprises an intermediate adhesive layer and another glass substrate, and the glass substrate coated with the anti-fog coating layer, the intermediate adhesive layer and the other glass substrate are laminated in order to form a laminated glass, and the anti-fog coating layer is located on the surface of the glass substrate opposite to the intermediate adhesive layer.

[0027] The details of one or more embodiments of the application are set forth below, and other features, objects and advantages of the application will become apparent from the description and claims.

[0028] In order to more clearly describe the technical solutions in the embodiments of the present application or the prior art, the drawings necessary for describing the embodiments or the prior art are briefly introduced below. It is obvious that the drawings described below are only the embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without any creative effort. [Brief description of the drawings]

[0029] [Figure 1] FIG. 2 is a structural schematic diagram of an anti-fogging glass manufactured in one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] The technical solutions in the embodiments of the present application are described below clearly and completely. It is obvious that the described embodiments are only some embodiments of the present application, but not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative labor are all included in the scope of protection of the present application.

[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terms used herein are for the purpose of describing the embodiments and examples only and are not intended to limit the present application.

[0032] term Terms and expressions used in this specification have the following meanings unless otherwise stated or contradicted:

[0033] As used herein, the scope of the term "and / or", "or / and", "and / or" includes any one of two or more of the associated listed items, and also includes any and all combinations of the associated listed items, including any two of the associated listed items, any further associated listed items, or all of the associated listed items.

[0034] In this specification, "one or more types" refers to any one type, any two types, or any two or more types of the listed items. Here, "multiple types" refers to two types or two or more types.

[0035] As used herein, "combinations thereof," "any combination thereof," "any manner of combination thereof," and the like include all appropriate combinations of any two of the listed items or any two or more of the items.

[0036] It should be understood that in this specification, "preferably" is merely intended to describe a more effective embodiment or example, and is not intended to limit the scope of protection of the present application.

[0037] In this application, technical features described in an open format include both closed technical means consisting of the recited features and open technical means comprising the recited features.

[0038] In this application, a numerical interval includes the two endpoints of the numerical interval, unless otherwise stated.

[0039] Percentage contents in this application refer to mass percentages for solid-liquid and solid-solid mixtures, and volume percentages for liquid-liquid mixtures, unless otherwise stated.

[0040] The percentage concentration in this application refers to the final concentration unless otherwise specified. The final concentration refers to the proportion of the added component in the system after the component is added.

[0041] Unless otherwise specified, the temperature parameters in this application may be constant temperature treatments or treatments within a constant temperature range, in which the temperature can vary within the precision range of the equipment control.

[0042] Unless otherwise specified, the "solubility" in this application is the mass of a solute that dissolves in water at 20°C when the solute reaches saturation.

[0043] The anti-fog paint includes, as manufacturing raw materials, a hydrophilic copolymer, an epoxy resin, a coupling agent, a curing agent and a first solvent, the manufacturing raw materials of the hydrophilic copolymer include a hydrophilic monomer, an initiator and a second solvent, the solubility of the epoxy resin in water is 90% or more, and the solubility of the hydrophilic copolymer in water is 90% or more.

[0044] The present invention uses a hydrophilic monomer to carry out a polymerization reaction under the action of an initiator to prepare a hydrophilic copolymer with high solubility. Then, the hydrophilic copolymer and an epoxy resin with high solubility are reacted under the action of a curing agent. Here, the hydrophilic copolymer is a linear polymer, and the hydrophilic copolymer with a linear structure can be crosslinked with the epoxy resin to form a strong semi-interpenetrating network structure, which is advantageous for improving surface adhesion, abrasion resistance, toughness and heat resistance. The semi-interpenetrating network structure releases the stress generated after the coating layer absorbs and releases water, making the coating layer less likely to peel off from the glass substrate. At the same time, the coupling agent can play an important role in connecting the coating material and the glass substrate, and the coating material produced can be directly applied to the glass substrate in a single layer and is not easily peeled off. By applying the anti-fog coating material of the present invention to the glass substrate in a single layer, the base layer between the anti-fog water-absorbing layer and the glass substrate layer can be omitted, and the hard coating layer on the outer surface of the anti-fog water-absorbing layer can also be omitted, simplifying the production process and reducing the production cost. In addition, the anti-fog coating layer of the present invention has excellent water absorption and good anti-fog effect, can realize active anti-fog of glass, has a long service life, and can significantly reduce the energy consumption of automobiles.

[0045] The higher the solubility, the more polar groups there are, and the easier it is to form a coating layer with higher water absorption.Preferably, the solubility of the hydrophilic copolymer in water is about 95% or more.

[0046] In one embodiment, the hydrophilic monomer is a combination of an acrylic acid ester monomer and an acrylic acid amide monomer.

[0047] By using a combination of an acrylic acid ester monomer and an acrylic acid amide monomer, both of which act as hydrophilic monomers and undergo a polymerization reaction under the action of an initiator, a hydrophilic copolymer having a linear structure and high solubility can be produced.

[0048] The acrylic acid ester polymer has good film-forming properties and good adhesion to the substrate, and the acrylic acid ester monomer can provide different functions according to different side chain structures. In one preferred embodiment, the side chains of the acrylic acid ester monomers used all contain hydrophilic groups, and can increase the hydrophilicity of the coating layer, and the monomers containing methyl groups can be used to ensure the hardness and water resistance of the coating layer. The acrylic acid amide monomer not only provides hydrophilic amide groups, but also plays a crosslinking role.

[0049] Optionally, the hydrophilic monomer may contain a hydroxyl group, a carboxyl group, an epoxy group, a primary amino group, a secondary amino group, a tertiary amino group, a cyano group, an amide group, or the like in its molecular structure.

[0050] Optionally, the acrylic ester monomer is hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, glycidyl acrylate, glycidyl methacrylate, or a combination thereof.

[0051] Optionally, the acrylic acid amide monomer is acrylamide, N,N-dimethylacrylamide, 2-acrylamido-2-methylpropanesulfonic acid, or a combination thereof.

[0052] The above hydrophilic monomers can be polymerized in the presence of an initiator to produce a hydrophilic copolymer.

[0053] Optionally, the initiator is a radical initiator containing a nitrogen-nitrogen double bond.

[0054] In some embodiments, the initiator is an azo-based initiator, including but not limited to azobisisobutyronitrile, azobisdimethylvaleronitrile, azobisisobutylamidine hydrochloride, azobisisobutylmidazoline hydrochloride, and 2-(carbamoylazo)isobutyronitrile. This type of initiator produces only one type of radical upon decomposition, with no other side reactions.

[0055] As can be seen, the polymerization reaction is carried out in a second solvent.

[0056] Optionally, the second solvent is an alcohol-based solvent or an ether-based solvent, including, but not limited to, n-butanol, isobutanol, ethanol, methanol, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol propyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, and propylene glycol butyl ether. These organic solvents are compatible with the hydrophilic monomers and can also be compatible with components such as epoxy resins, so that the final coating does not have problems such as phase separation.

[0057] As can be appreciated, the polymerization reaction is carried out under an inert atmosphere.

[0058] The gas providing the inert atmosphere may be nitrogen, argon or helium. The inert gas can avoid the effect of moisture in the air on the system reaction.

[0059] After preparing the hydrophilic copolymer, the hydrophilic copolymer, the epoxy resin, the coupling agent, the curing agent and the first solvent are mixed together to carry out a crosslinking reaction to prepare the anti-fog coating material.

[0060] Optionally, the epoxy resin is an aliphatic glycidyl ether.

[0061] The aliphatic glycidyl ether is trimethylolpropane triglycidyl ether, glycerin triglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether, sorbitol glycidyl ether, or a combination thereof.

[0062] The aliphatic glycidyl ether contains an epoxy group capable of ring-opening crosslinking in the molecular structure, and further contains a hydrophilic group.

[0063] Preferably, the aliphatic glycidyl ether contains at least two functional groups in its molecular structure.

[0064] In one embodiment, the mass ratio of the hydrophilic copolymer to the epoxy resin is (1-4):1.

[0065] Optionally, the coupling agent is a silane coupling agent, which is γ-methacryloxypropyltrimethoxysilane (KH570), γ-aminopropyltriethoxysilane (KH550), γ-glycidoxypropyltrimethoxysilane (KH560), divinyltriaminopropyltrimethoxysilane, ureidopropyltriethoxysilane, or a combination thereof. The silane coupling agent can be hydrolyzed to generate Si-OH to bond more tightly with the glass substrate.

[0066] Optionally, the raw material for producing the anti-fog coating further comprises a silane hydrolysis catalyst, which can accelerate the hydrolysis of the silane coupling agent.

[0067] Optionally, the silane hydrolysis catalyst is a base catalyst or an acid catalyst.

[0068] The base catalyst includes, but is not limited to, aqueous ammonia, sodium hydroxide, and potassium hydroxide.

[0069] The acid catalysts include, but are not limited to, nitric acid, hydrochloric acid, and acetic acid.

[0070] Optionally, the curing agent is diethylenetriamine, hydroxyethylethylenediamine, isophoronediamine, or a combination thereof.

[0071] Optionally, the first solvent is selected from alcohol-based solvents or ether-based solvents, including, but not limited to, n-butanol, isobutanol, ethanol, methanol, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol propyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, and propylene glycol butyl ether. These organic solvents are compatible with the hydrophilic monomer and can also be compatible with components such as epoxy resins, so that the final coating layer does not suffer from problems such as phase separation. The first solvent may be the same as or different from the second solvent.

[0072] In some embodiments, the ingredients of the anti-fog coating include, in parts by weight, about 1 part to about 80 parts of a hydrophilic copolymer, about 1 part to about 20 parts of an epoxy resin, about 0.1 parts to about 10 parts of a coupling agent, about 0.4 parts to about 15 parts of a curing agent, and about 20 parts to about 50 parts of a first solvent.

[0073] Optionally, the manufacturing raw materials of the anti-fog coating further include one or more of fillers, antioxidants, UV absorbers and leveling agents.

[0074] The addition of filler can improve the abrasion resistance and heat resistance of the coating layer. In one embodiment, the filler is nano silica, nano alumina, or a combination thereof. The primary particle size of the filler is preferably 20 nm or less, and examples of commercially available fillers include Evonik's AERROSIL A200, AEROXIDE ALU C, WACKER HDKV15, and N20.

[0075] The mass of the filler added is preferably 0.05% to 0.20% (total paint mass ratio: 100%).

[0076] The addition of an antioxidant and an ultraviolet absorber can improve the aging resistance of the coating layer and the weather resistance of the coating layer. The antioxidant is triethylene glycol-bis(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, octyl-3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-bis3-(3'5'di-tert-butyl-4'-hydroxyphenyl)propionylhexamethylenediamine, or a combination thereof. The ultraviolet absorber is 2,2',4,4'-tetrahydroxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, or a combination thereof.

[0077] In some preferred embodiments, the antioxidant is triethylene glycol-bis(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, the UV absorber is 2,2',4,4'-tetrahydroxybenzophenone, and the mass amounts of both are 0.5% to 1.5% and 0.1% to 0.5%, respectively (total paint mass ratio 100%).

[0078] The addition of a leveling agent can reduce problems such as orange peel and cissing in the coating layer, and can make the surface of the coating layer smoother and flatter. Examples of leveling agents include BYK-345, BYK-333, BYK-307, BYK337, and BYK341 manufactured by BYK of Germany.

[0079] Preferably, the amount of the leveling agent added may be 150 ppm to 600 ppm by total mass of the system.

[0080] Optionally, the raw material for manufacturing the anti-fog coating further includes an accelerator, which is an organic compound formed by directly bonding a metal atom with a carbon atom, and the addition of the accelerator can improve the toughness and abrasion resistance of the coating layer by utilizing the complexing effect of the metal. In one embodiment, the accelerator is methyllithium, triethylaluminum, ethylmagnesium iodide, methylzinc chloride, trimethyllead hydride, or a combination thereof.

[0081] In one embodiment, the mass of the accelerator added is 0.5% to 3%, preferably 1% to 1.8% (total paint mass ratio 100%).

[0082] As can be appreciated, other functional additives may be added to the anti-fog coating of the present invention, if desired.

[0083] One embodiment of the present application provides a method for manufacturing anti-fog glass, including the following steps.

[0084] Step 1: Preparation of the hydrophilic copolymer About 5 to 35 parts of a hydrophilic monomer and about 40 to 85 parts of a solvent are added to a reaction flask by weight, and then an inert gas is introduced to disperse the mixture by stirring. Then, an initiator is added and the mixture is reacted at a certain temperature for a certain period of time.

[0085] Step 2: Manufacturing the anti-fog coating By weight, about 1 to 80 parts of a hydrophilic copolymer, about 1 to 20 parts of an epoxy resin, about 0.1 to 10 parts of a coupling agent, about 0.5 to 15 parts of a curing agent, and about 20 to 50 parts of a first solvent are uniformly stirred and reacted at a certain temperature for a certain period of time to obtain an anti-fog coating material.

[0086] Step 3: Manufacture of anti-fog glass FIG. 1 shows a schematic diagram of the structure of the anti-fogging glass of this embodiment.

[0087] The surface of the glass substrate 01 is cleaned. Cleaning the glass thoroughly is advantageous for applying the coating solution more thoroughly and uniformly.

[0088] As can be understood, the cleaning process includes physical cleaning, chemical cleaning, and a combination of physical cleaning and chemical cleaning, and the physical cleaning in the cleaning process includes gauze wiping, powder polishing, plasma treatment, or a combination thereof. The polishing powder in the physical cleaning is nano cerium oxide, nano aluminum oxide, nano magnesium oxide, or a combination thereof. The chemical cleaning is alkaline cleaning, acid cleaning, immersion in fish eater solution, or a combination thereof. The cleaning process is intended to remove dust particles from the glass and activate the surface, and the cleaning method is not limited to the above, and may be any method that can achieve the purpose.

[0089] Then, an anti-fog paint is applied to the glass surface by a certain application method, and after the anti-fog paint is leveled on the glass surface, it is cured at a certain temperature for a certain time, and an anti-fog coating layer 02 is formed after curing, and the anti-fog coating layer 02 can be firmly attached to the surface of the glass substrate 01 by chemical bonding, and the thickness of the anti-fog coating layer is about 5 μm to 30 μm.

[0090] Optionally, the coating method is spin coating, shower coating, spray coating, dip coating or spray coating. In one embodiment, the coating is spray coating. By adopting a spray coating process, the thickness of the coating layer can be more precisely controlled and the overall thickness uniformity of the coating layer can be ensured.

[0091] Optionally, the curing temperature is about 120°C to 200°C, and the curing time is about 20 min to 720 min.

[0092] In one embodiment, the anti-fog paint can be manufactured and used as an anti-fog spray, and drivers can spray the anti-fog spray on their car windows, thereby achieving active anti-fog on the windows, prolonging their service life, and significantly reducing the energy consumption of the car.

[0093] An anti-fog glass includes a glass substrate and an anti-fog coating layer on the glass substrate, the anti-fog coating layer being formed from the above-mentioned anti-fog paint applied onto the glass substrate, and the thickness of the anti-fog coating layer is about 5 μm to 30 μm.

[0094] In one embodiment, the glass substrate may be a curved glass plate, the curved glass plate having a convex surface and a concave surface, the anti-fog coating layer is disposed on the concave surface, the anti-fog coating layer has a maximum thickness and a minimum thickness, and the difference between the maximum thickness and the minimum thickness is about 1 μm to 5 μm.

[0095] Forming the anti-fog coating layer on the concave surface can be achieved by a spray coating process, which allows for more accurate control of the thickness of the coating layer to ensure uniformity of the overall coating thickness.

[0096] In one embodiment, the anti-fog glass further includes an intermediate adhesive layer and another glass substrate, and the glass substrate coated with the anti-fog coating layer, the intermediate adhesive layer and the other glass substrate are laminated in order to form a laminated glass, and the anti-fog coating layer is located on the surface of the glass substrate opposite to the intermediate adhesive layer.

[0097] The present invention will be further described with reference to specific examples and comparative examples below. Unless otherwise specified, the raw materials in the following specific examples may be commercially available products, the equipment used may be commercially available products, and the processes involved may be those that are commonly selected by those skilled in the art, unless otherwise specified.

[0098] Example 1 This embodiment provides an anti-fog glass and its manufacturing method. The steps are as follows:

[0099] Step 1: Preparation of the hydrophilic copolymer 2g of hydroxyethyl acrylate, 4g of acrylamide, and 40g of propylene glycol methyl ether were weighed and placed in a reaction flask, protected by nitrogen gas and stirred uniformly, and then 0.15g of azobisisobutyronitrile was added. The reaction flask was placed in an oil bath at 70°C and reacted with stirring for 12 hours to obtain a hydrophilic copolymer with a solubility of 94%.

[0100] Step 2: Manufacturing the anti-fog coating 7.5 g of the hydrophilic copolymer prepared in step 1 and 5 g of epoxy resin EX-313 (a commercial product of Nagase ChemteX Japan Corporation, belonging to glycerin triglycidyl ether, solubility 99%) were taken, and the mass ratio of the two was 1.5:1. The two were uniformly mixed with 50 g of absolute ethanol, and 0.5 g of silane coupling agent KH550 and 0.6 g of diethylenetriamine were further added, and after uniform stirring, the mixture was reacted at room temperature for 2 hours to obtain anti-fog coating 1.

[0101] Step 3: Manufacture of anti-fog glass The surface of the glass substrate was cleaned, and the anti-fog coating material prepared in step 2 was applied to the glass substrate and cured at 150°C for 2 hours to obtain anti-fog glass.

[0102] Example 2 This embodiment provides an anti-fog glass and its manufacturing method. The steps are as follows:

[0103] Step 1: Preparation of the hydrophilic copolymer 2g of hydroxyethyl acrylate, 4g of acrylamide, and 40g of propylene glycol methyl ether were weighed and placed in a reaction flask, protected by nitrogen gas and stirred uniformly, and then 0.15g of azobisisobutyronitrile was added. The reaction flask was placed in an oil bath at 70°C and reacted for 12 hours with stirring to obtain a hydrophilic copolymer with a solubility of 94%.

[0104] Step 2: Manufacturing the anti-fog coating 12 g of the hydrophilic copolymer prepared in step 1 and 3 g of epoxy resin EX-614B (a commercial product of Japan Nagase ChemteX Corporation, belonging to sorbitol glycidyl ether, solubility 94%) were taken, and the mass ratio of the two was 4:1. The two were uniformly mixed with 50 g of absolute ethanol, and 0.5 g of silane coupling agent KH560 and 0.4 g of diethylenetriamine were further added, and after uniform stirring, the mixture was reacted at room temperature for 2 hours to obtain anti-fog coating 2.

[0105] Step 3: Manufacture of anti-fog glass The surface of the glass substrate was cleaned, and the anti-fog coating material prepared in step 2 was applied to the glass substrate and cured at 160°C for 2 hours to obtain anti-fog glass.

[0106] Example 3 This embodiment provides an anti-fog glass and its manufacturing method. The steps are as follows:

[0107] Step 1: Preparation of the hydrophilic copolymer 1 g of hydroxyethyl methacrylate, 4 g of N,N-dimethylacrylamide, and 40 g of propylene glycol methyl ether were weighed and placed in a reaction flask, protected by nitrogen gas and stirred uniformly, and then 0.1 g of azobisisobutyronitrile was added. The reaction flask was placed in an oil bath at 70°C and reacted with stirring for 12 hours to obtain a hydrophilic copolymer with a solubility of 92%.

[0108] Step 2: Manufacturing the anti-fog coating 7.5g of the hydrophilic copolymer prepared in step 1 and 5g of epoxy resin EX-313 (a commercial product of Japan Nagase ChemteX Corporation, belonging to glycerin triglycidyl ether, solubility 99%) were taken, and the mass ratio of the two was 1.5:1. The two were uniformly mixed with 50g of absolute ethanol, and 0.5g of silane coupling agent KH550 and 1.3g of hydroxyethylethylenediamine were further added, and after uniform stirring, the mixture was reacted at room temperature for 3 hours to obtain anti-fog coating 3.

[0109] Step 3: Manufacture of anti-fog glass The surface of the glass substrate was cleaned, and the anti-fog coating material prepared in step 2 was applied to the glass substrate and cured at 150°C for 2 hours to obtain anti-fog glass.

[0110] Example 4 This embodiment provides an anti-fog glass and its manufacturing method. The steps are as follows:

[0111] Step 1: Preparation of the hydrophilic copolymer 1.5g of hydroxyethyl methacrylate, 5g of N,N-dimethylacrylamide, and 55g of propylene glycol methyl ether were weighed and placed in a reaction flask, protected by nitrogen gas and stirred uniformly, and then 0.15g of azobisisobutyronitrile was added. The reaction flask was placed in an oil bath at 80°C and reacted with stirring for 1 hour to obtain a hydrophilic copolymer with a solubility of 93%.

[0112] Step 2: Manufacturing the anti-fog coating 6g of the hydrophilic copolymer prepared in step 1 and 6g of epoxy resin EX-512 (a commercial product of Japan Nagase ChemteX Corporation, belonging to polyglycerol polyglycidyl ether, solubility 100%) were taken, and the mass ratio of the two was 1:1. The two were uniformly mixed with 50g of absolute ethanol, and 0.5g of silane coupling agent KH550 and 1.2g of hydroxyethylethylenediamine were further added, and after uniform stirring, the mixture was reacted at room temperature for 1 hour to obtain anti-fog coating 4.

[0113] Step 3: Manufacture of anti-fog glass The surface of the glass substrate was cleaned, and the anti-fog coating material produced in step 2 was applied to the glass substrate and cured at 200°C for 1 hour to obtain anti-fog glass.

[0114] Example 5 This embodiment provides an anti-fog glass and its manufacturing method. The steps are as follows:

[0115] Step 1: Preparation of the hydrophilic copolymer 6 g of hydroxyethyl acrylate and 40 g of propylene glycol methyl ether were weighed and placed in a reaction flask, protected by nitrogen gas and stirred uniformly, and then 0.15 g of azobisisobutyronitrile was added. The reaction flask was placed in an oil bath at 70°C and reacted with stirring for 12 hours to obtain a hydrophilic copolymer with a solubility of 92%.

[0116] Step 2: Manufacturing the anti-fog coating 7.5g of the hydrophilic copolymer prepared in step 1 and 5g of epoxy resin EX-313 (a commercial product of Japan Nagase ChemteX Corporation, belonging to glycerin triglycidyl ether, solubility 99%) were taken, and the mass ratio of the two was 1.5:1. The two were uniformly mixed with 50g of absolute ethanol, and 0.5g of silane coupling agent KH550 and 0.6g of diethylenetriamine were further added, and after uniform stirring, the mixture was reacted at room temperature for 2 hours to obtain anti-fog coating 5.

[0117] Step 3: Manufacture of anti-fog glass The surface of the glass substrate was cleaned, and the anti-fog coating material prepared in step 2 was applied to the glass substrate and cured at 150°C for 2 hours to obtain anti-fog glass.

[0118] Comparative Example 1 This comparative example provides an anti-fog glass and its manufacturing method. The steps are as follows:

[0119] Step 1: Preparation of the hydrophilic copolymer 2g of hydroxyethyl acrylate, 4g of acrylamide, and 40g of propylene glycol methyl ether were weighed and placed in a reaction flask, protected by nitrogen gas and stirred uniformly, and then 0.15g of azobisisobutyronitrile was added. The reaction flask was placed in an oil bath at 70°C and reacted with stirring for 12 hours to obtain a hydrophilic copolymer with a solubility of 94%.

[0120] Step 2: Manufacturing the anti-fog coating 10 g of the hydrophilic copolymer prepared in step 1 and 5 g of epoxy resin EX-313 (a commercial product of Nippon Nagase ChemteX Corporation, belonging to glycerin triglycidyl ether, solubility 99%) were taken, and the mass ratio of the two was 2:1. The two were uniformly mixed with 50 g of absolute ethanol, and 1.5 g of isophoronediamine was further added. After uniform stirring, the mixture was reacted at room temperature for 2 hours to obtain anti-fog coating 6.

[0121] Step 3: Manufacture of anti-fog glass The surface of the glass substrate was cleaned, and the anti-fog coating material prepared in step 2 was applied to the glass substrate and cured at 150°C for 2 hours to obtain anti-fog glass.

[0122] Comparative Example 2 This comparative example provides an anti-fog glass and its manufacturing method. The steps are as follows:

[0123] Step 1: Making the anti-fog coating 6 g of epoxy resin EX-313 (a commercial product of Nippon Nagase Chemtex Corporation, belonging to glycerin triglycidyl ether, solubility 99%) was taken and mixed uniformly with 50 g of anhydrous ethanol, and 1.5 g of hydroxyethylethylenediamine was further added and stirred uniformly, and then reacted at room temperature for 2 hours to obtain anti-fog coating 7.

[0124] Step 2: Making anti-fog glass The surface of the glass substrate was cleaned, and the anti-fog coating material prepared in step 1 was applied to the glass substrate and cured at 120°C for 2 hours to obtain anti-fog glass.

[0125] The performance of each of the anti-fogging glasses manufactured as above was evaluated, and the evaluation requirements were as follows: Anti-fogging evaluation: The anti-fogging glass was left in an environment of 20°C and 50% RH for 1 hour, then transferred onto the surface of 100 ml or more of 35°C water (5 cm from the water surface), and the fogging time (s) was measured visually. Boiling resistance: Anti-fogging glass was placed in boiling water at 100°C for 2 hours, then removed and the appearance was observed. OK: No whitening, peeling, peeling or falling off of the coating layer is observed. NG: The coating layer is whitened, peeled, peeled off or fallen off. Alkaline resistance: Anti-fogging glass was immersed in 0.1N NaOH for 3 hours, taken out, washed with deionized water, dried, and the appearance was observed. OK: No whitening, peeling, peeling or falling off of the coating layer is observed. NG: The coating layer is whitened, peeled, peeled off or fallen off. Abrasion resistance: Anti-fog glass is abrasion-resistant tested using US Taber 5131, and the load is 4.9N / 400mm under the test conditions. 2 (20mm x 20mm friction surface), 40 cycles / min, 5000 abrasions, with the friction cloth replaced every 1000 abrasions. After the test, the appearance was observed and a haze test was performed using a Nippon Shinsha HZ-V3 haze meter. OK: No cracks, peeling or falling off was observed in the coating layer, and the haze change value was less than 2. NG: Cracks, peeling or falling off was observed in the coating layer, and the haze change value was less than 2.

[0126] The evaluation results are shown in Table 1.

[0127] [Table 1]

[0128] As is clear from Table 1, the single-layer anti-fogging glass of Examples 1 to 5 meets the requirements for anti-fogging evaluation, boiling resistance and alkali resistance, and reduces the number of processes and production costs. Specifically, it can delay the fogging time of the glass, has good anti-fogging properties, ensures driving safety and reduces the energy consumption of the automobile. At the same time, it has good boiling resistance and alkali resistance and is not easily peeled off. In addition, the single-layer anti-fogging glass of Examples 1 to 4 also has excellent abrasion resistance. In Example 5, only an acrylate-based monomer was used as the hydrophilic monomer, so the abrasion resistance of the coating layer was slightly reduced, which was because the crosslinking action of the acrylic acid amide-based monomer was insufficient, the crosslinking density was reduced, and the strength of the coating layer was reduced.

[0129] As a comparative example, Comparative Example 2 does not add hydrophilic copolymer and coupling agent, so the boiling resistance, alkali resistance, and wear resistance do not meet the requirements, the bonding strength between the anti-fogging coating layer and the glass substrate is poor, the coating layer absorbs water and expands and contracts, causing stress, and the coating layer is easily peeled off from the substrate, and the hydrophilic copolymer does not form a semi-interpenetrating network structure with the epoxy resin, so the network structure is not strong, and the surface is not easily peeled off. Comparative Example 1 does not add coupling agent, so the boiling resistance is poor, showing that the coupling agent plays an important role in connecting the coating layer and the substrate.

[0130] Each of the technical features of the above-mentioned embodiments can be combined in any manner, and for the sake of brevity, not all possible combinations of each of the technical features in the above-mentioned embodiments are described, but as long as there is no contradiction in the combination of these technical features, they should be considered within the scope described in this specification.

[0131] The above examples only show some embodiments of the present application, and the description is more specific and detailed, but should not be understood as limiting the scope of the claims. It should be noted that a person skilled in the art can make some modifications and improvements without departing from the spirit of the present invention, and all of these belong to the scope of protection of the present invention. Therefore, the scope of protection of the present application shall be subject to the scope of the attached claims.

Claims

1. An anti-fog paint comprising: The manufacturing raw materials of the anti-fog coating include a hydrophilic copolymer, an epoxy resin, a coupling agent, a curing agent and a first solvent; The raw materials for producing the hydrophilic copolymer include a hydrophilic monomer, an initiator, and a second solvent; The solubility of the epoxy resin in water is about 90% or more; An anti-fog coating, wherein the solubility of the hydrophilic copolymer in water is about 90% or more.

2. 2. The anti-fog coating according to claim 1, wherein the hydrophilic monomer is a combination of an acrylic acid ester monomer and an acrylic acid amide monomer.

3. 3. The anti-fog coating according to claim 2, wherein the acrylic acid ester monomer is hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, glycidyl acrylate, glycidyl methacrylate, or a combination thereof.

4. 3. The anti-fog coating according to claim 2, wherein the acrylic acid amide monomer is acrylamide, N,N-dimethylacrylamide, 2-acrylamido-2-methylpropanesulfonic acid, or a combination thereof.

5. The epoxy resin is an aliphatic glycidyl ether, The anti-fog coating material according to any one of claims 1 to 4, wherein the aliphatic glycidyl ether is trimethylolpropane triglycidyl ether, glycerin triglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether, sorbitol glycidyl ether, or a combination thereof.

6. The anti-fog coating according to any one of claims 1 to 5, characterized in that the mass ratio of the hydrophilic copolymer to the epoxy resin is about (1-4):

1.

7. 7. The anti-fog coating according to claim 6, wherein the raw materials for manufacturing the anti-fog coating include, in parts by weight, about 1 part to about 80 parts of a hydrophilic copolymer, about 1 part to about 20 parts of an epoxy resin, about 0.1 parts to about 10 parts of a coupling agent, about 0.4 parts to about 15 parts of a curing agent, and about 20 parts to about 50 parts of a first solvent.

8. The anti-fog coating according to any one of claims 1 to 7, characterized in that the coupling agent is γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, divinyltriaminopropyltrimethoxysilane, ureidopropyltriethoxysilane, or a combination thereof.

9. The anti-fog coating according to any one of claims 1 to 7, wherein the curing agent is diethylenetriamine, hydroxyethylethylenediamine, isophoronediamine, or a combination thereof.

10. The anti-fog coating material according to any one of claims 1 to 7, characterized in that the initiator is a radical initiator containing a nitrogen-nitrogen double bond.

11. The anti-fog coating according to any one of claims 1 to 7, wherein the first solvent and the second solvent are each independently an alcohol-based solvent or an ether-based solvent.

12. The anti-fog paint according to any one of claims 1 to 7, characterized in that the manufacturing raw materials of the anti-fog paint further comprise a silane hydrolysis catalyst, a filler, an antioxidant, an ultraviolet absorber, a leveling agent, or a combination thereof.

13. The anti-fog coating according to claim 12, characterized in that the silane hydrolysis catalyst is a base catalyst or an acid catalyst.

14. 13. The anti-fog coating of claim 12, wherein the filler is nano-silica, nano-alumina, or a combination thereof.

15. The anti-fog coating of claim 13, wherein the antioxidant is triethylene glycol-bis(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, octyl-3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-bis-3-(3'5'di-tert-butyl-4'-hydroxyphenyl)propionylhexamethylenediamine, or a combination thereof.

16. The anti-fog coating according to claim 12, wherein the ultraviolet absorber is 2,2',4,4'-tetrahydroxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, or a combination thereof.

17. The anti-fog paint according to any one of claims 1 to 16, wherein the manufacturing raw material of the anti-fog paint further comprises an accelerator, and the accelerator is methyllithium, triethylaluminum, ethylmagnesium iodide, methylzinc chloride, trimethyllead hydride, or a combination thereof.

18. A method for producing the anti-fog coating material according to any one of claims 1 to 17, mixing the hydrophilic monomer, the initiator and the second solvent and carrying out a polymerization reaction to prepare a hydrophilic copolymer; mixing the hydrophilic copolymer, the epoxy resin, the coupling agent, the curing agent and the first solvent, and carrying out a crosslinking reaction to produce an anti-fog coating.

19. An anti-fogging glass, A glass substrate and an anti-fog coating layer on the glass substrate, The anti-fog coating layer is formed from the anti-fog paint according to any one of claims 1 to 17 applied to a glass substrate, and the thickness of the anti-fog coating layer is about 5 μm to 30 μm.

20. The anti-fog glass according to claim 19, wherein the glass substrate is a curved glass plate, the curved glass plate having a convex surface and a concave surface, the anti-fog coating layer is provided on the concave surface, the anti-fog coating has a maximum thickness and a minimum thickness, and the difference between the maximum thickness and the minimum thickness is about 1 μm to 5 μm.

21. The anti-fogging glass according to any one of claims 19 to 20, further comprising an intermediate adhesive layer and another glass substrate, the glass substrate coated with the anti-fogging coating layer, the intermediate adhesive layer and the another glass substrate being laminated in this order to form a laminated glass, and the anti-fogging coating layer is located on a surface of the glass substrate opposite to the intermediate adhesive layer.

Citation Information

Patent Citations

  • Antifogging coating layer composition and preparation method and application method thereof

    CN106800855A

  • Antifogging coating liquid, antifogging glass window, and manufacturing method of antifogging glass window

    CN106978067A

  • JP1975001710A

  • Anti-fogging coating composition

    JP1994041519A

  • Anti-fogging article and method of manufacturing the same

    JP2013248849A