Compositions and methods for selectively extracting lithium

Ion-selective separation membranes with polymer matrices and metal oxides enhance lithium extraction from brines by selectively transporting lithium while rejecting other cations, addressing inefficiencies in current methods and achieving high selectivity ratios.

JP2024540291AInactive Publication Date: 2024-10-31RGT UNIV OF CALIFORNIA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024526575
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-08
Filing Date
2022-11-07
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current lithium extraction methods from brine sources are costly, time-consuming, and environmentally unfriendly, and existing membrane technologies lack specific selectivity for lithium ions, limiting their efficiency and scalability.

Method used

Development of ion-selective separation membranes comprising a polymer matrix and dispersed metal compounds like lithium manganese or titanium oxides, which selectively transport lithium ions while rejecting other cations through a continuous membrane system.

Benefits of technology

The membranes achieve high selectivity for lithium ions over competing cations, with selectivity ratios up to 10,000, enabling efficient and scalable lithium extraction from brines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540291000003
    Figure 2024540291000003
  • Figure 2024540291000004
    Figure 2024540291000004
  • Figure 2024540291000005
    Figure 2024540291000005
Patent Text Reader

Abstract

An ion-selective separation membrane is provided that includes a polymer matrix and a metal compound dispersed within the polymer matrix. The metal compound is H a Li b X c O d wherein a is 1 to 1.5, b is 0 to 0.1, c is 1 to 2, d is 4 to 4.5, and X includes manganese or titanium.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority to U.S. Provisional Application No. 63 / 276921, filed November 8, 2021, the contents of which are incorporated herein by reference in their entirety.

[0002] Statement regarding government support This invention was made with Government support under Grant No. DE-EE0008391 awarded by the U.S. Department of Energy. The U.S. Government has certain rights in this invention.

[0003] FIELD OF THE DISCLOSURE Embodiments of the present disclosure relate generally to membranes for selectively extracting monovalent metal ions. More specifically, the present disclosure relates to membranes for selectively extracting lithium ions from a brine solution. [Background technology]

[0004] Lithium compounds are important components in many commercial applications including batteries, glasses, ceramics, lubricating greases, as well as other industrial products. Global lithium consumption has increased significantly in recent decades and is projected to reach 200,000 tonnes by 2030. Lithium resources exist primarily in solid form (e.g., minerals, ores, and lithium-ion battery recycling) and liquid form (e.g., seawater and other lithium-rich brines). Current commercial lithium production relies primarily on continental brine sources. Mainstream lithium extraction techniques such as evaporative precipitation and solvent extraction have been shown to be costly, time-consuming, and environmentally unfriendly. Recent advances in membrane-based separation technologies have provided promising and environmentally friendly alternatives for lithium recovery.

[0005] Membrane separation has the advantages of being energy efficient, scalable, and easy to operate in a continuous process. For example, nanofiltration (NF) uses the mechanisms of Donnan rejection, dielectric exclusion, and steric hindrance to make monovalent ions extractable. NF is a membrane liquid separation technology that shares many characteristics with reverse osmosis (RO). However, unlike RO, which removes high levels of virtually all dissolved solutes, NF removes high levels of multivalent ions such as sulfate and low levels of monovalent ions such as chloride.

[0006] Membrane distillation crystallization can recover minerals from high salinity brines using low-grade heat, and selective electrodialysis can efficiently separate monovalent cations under an electric field. Although the above membrane processes provide some bulk salt separation capability, they do not provide membranes with specific cation selectivity, especially between lithium and other monovalent cations, due to the presence of multiple competing cation concentrations in the brine. Lithium ion sieves (LIS) have been produced as adsorption media for lithium extraction, but the adsorption-desorption process can only be operated in batch mode. LIS known in the art are described in Xu et al., “Extraction of lithium with functionalized lithium ion-sieves.” Progress in Materials Science. Vol 84. December 2016, Pages 276-313. The slow adsorption rate also leads to poor lithium extraction efficiency, limiting the large-scale application of this process compared to the continuous mode. Therefore, there is a need for improved materials and processes for the selective extraction of lithium ions. [Prior art documents] [Non-patent literature]

[0007] [Non-Patent Document 1] Xu et al.,“Extraction of lithium with functionalized lithium ion-sieves.”Progress in Materials Science.Vol84.December2016,Pages276-313 Summary of the Invention [Means for solving the problem]

[0008] In various embodiments, the ion-selective separation membrane comprises a polymer matrix and a metal compound dispersed within the polymer matrix. a Li b X c O d wherein a is 1 to 1.5, b is 0 to 0.1, c is 1 to 2, d is 4 to 4.5, and X includes manganese or titanium.

[0009] In various embodiments, a method for making an ion-selective separation membrane is disclosed that provides a lithium manganese oxide or lithium titanium oxide. The lithium manganese oxide or lithium titanium oxide is delithiated to obtain a lithium adsorbent. The lithium adsorbent is dispersed in a polymer matrix to form a polymer adsorbent mixture. The polymer adsorbent mixture is heated to obtain the synthesized ion-selective separation membrane.

[0010] In various embodiments, a method for selectively separating ions in a polar solution containing a plurality of ions is disclosed, in which an ion-selective separation membrane is provided, the polar solution is contacted with the ion-selective separation membrane, and a potential difference is applied across the ion-selective separation membrane to selectively transport target ions through the membrane.

[0011] In various embodiments, an ion-selective separation membrane is provided that includes a polymer matrix having a polymer backbone and one or more functional groups, and a metal ion adsorbent dispersed within the polymer matrix, the metal ion adsorbent configured to allow transport of a target ion through the membrane and block the passage of one or more non-target ions upon application of a potential difference across the membrane. [Brief description of the drawings]

[0012] [Figure 1] 1 shows a cast anion exchange membrane (AEM) without lithium adsorbed particles according to one embodiment of the present disclosure. [Diagram 2] 1 illustrates a cast AEM including lithium adsorbed particles according to an embodiment of the present disclosure. [Diagram 3] 1 shows a graph of specific ion flux of Feed Solution A according to one embodiment of the present disclosure. [Figure 4] 1 shows a graph of specific ion flux of Feed Solution B according to one embodiment of the present disclosure. [Diagram 5] 1 illustrates an apparatus for rejecting lithium using an ion-selective separation membrane according to one embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention provides a method for effectively extracting lithium from complex aqueous solutions such as geothermal brines and acid extraction solutions in battery recycling operations by advantageously integrating highly lithium-selective materials into a continuous membrane system that are capable of passing targeted monovalent cations (e.g., lithium) while rejecting multivalent cations and certain monovalent cations.

[0014] More specifically, the present disclosure relates to methods for separating target metal ions from other cations, such as separating a target monovalent cation from other polyvalent or monovalent metal ions (e.g., Na +) are disclosed. Further disclosed herein are methods of synthesizing the ion-selective separation membranes and methods of separating ions using the ion-selective separation membranes. In various embodiments, the ion sieving material is synthesized by introducing a target ion (e.g., lithium) into an inorganic compound (e.g., a metal oxide) by a redox reaction or an ion exchange reaction. The synthesized ion sieving material includes a crystal structure in which the target ion is incorporated. After the target ion is incorporated into the crystal structure, it is eluted from the crystal site by an eluent, and the ion sieving material retains the vacant crystal site of the target ion, thereby allowing only the target ion (or ions with a smaller ionic radius) to pass through. In various embodiments, lithium is the target ion, and since lithium has the smallest ionic radius compared to other cations, only lithium ions can pass through the vacant crystal site. In various embodiments, the ion sieving material is combined with a polymer matrix, such as by dispersion or mixing.

[0015] In various embodiments, the ion exchange membrane comprises a polymer matrix (e.g., a polymer backbone) having one or more functional groups that provide fixed charge sites. In various embodiments, the polymer matrix is ​​selected from methacrylamide, polyaromatic, styrene-divinylbenzene copolymer, polyester, polyvinyl chloride, poly(ethylene), poly(propylene), polystyrene, polystyrene-divinylbenzene copolymer, fluorinated interpenetrating polymer network, low density polyethylene / high density polyethylene (interpenetrating polymer network), polystyrene-block-ethylenebutylene-block-polystyrene, polystyrene / butadiene, polyethylene oxide, alkoxysilane functionalized polyethylene oxide, alkoxysilane functionalized polyvinyl alcohol, poly(epichlorohydrin-co-ethylene oxide), polyvinyl alcohol, poly(epichlorohydrin), polyacrylic acid, chitosan, polybenzimidazole, glycidyl methacrylate, 3-(methacryloxypropyl)trimethoxysilane, alkoxysilane / acrylate, epoxyalkoxysilane, poly (vinylbenzyl chloride), poly(phenylene oxide), poly(methyl acrylate), polyethyleneimine, poly(1,1-dimethyl-3,5-dimethylenepiperidinium chloride), poly(diallyldimethylammonium chloride), poly(allylamine), poly(acrylonitrile-co-2-dimethylaminoethyl methacrylate), polychloromethylstyrene, poly(divinylbenzene), norbornene / dicyclopentadiene, cyclooctene, poly(phenylene), poly(methyl methacrylate), poly(butyl-acrylate), poly(methyl methacrylate-co-butyl-acrylate-co-vinylbenzyl), polyvinyl butyral, polyvinylidene fluoride, ethylene tetrafluoroethylene, fluorinated ethylene propylene, polytetrafluoroethylene, poly(4-vinylpyridine), polystyrene-ethylene-butylene sulfonic acid copolymer, epichlorohydrin / 1,4-diazabicyclo[2.2.2] Octane, polyethylene glycol, polysulfone, cardo polyethersulfone, poly(phthalazinone ether sulfone ketone), polysulfone polyphenylene sulfide sulfone, polyarylene, polydiallyldimethylammonium chloride, poly(etherimide), and / or sulfonated tetrafluoroethylene-based fluorinated polymer-copolymer.

[0016] In various embodiments, the functional groups include nitrogen-containing groups such as quaternary ammonium, tertiary diamine, (benzo)imidazolium, guanidinium, and / or pyridinium, In various embodiments, the functional groups include nitrogen-free groups such as phosphonium, sulfonium, ruthenium, nickel, and / or cobalt.

[0017] In terms of specific ion selectivity, LISs have shown satisfactory performance as a group of ion adsorption materials due to the "ion sieving effect". As mentioned above, ion sieving materials are synthesized by introducing target ions into inorganic compounds through redox reactions or ion exchange reactions. The target ions are eluted from their crystal sites by the eluent, leaving vacant crystal sites that can only accommodate template ions or ions with smaller ionic radii. In the case of LISs, lithium ions are eluted from the ... + , K + , Rb + , Cs + , Mg 2+ , Ca 2+ It selectively accesses vacancies due to its small ionic radius compared to competing cations such as

[0018] Generally, LIS materials include lithium manganese oxide (LMO) and lithium titanium oxide (LTO). In various embodiments, LMO includes lithium manganese oxide (e.g., LiMn2O4, Li2MnO3, LiMnO2, Li2MnO2). In various embodiments, LTO includes lithium titanate (Li2TiO3). In comparison, LMO-type LIS has high lithium selectivity and adsorption capacity, while LTO-type LIS has low dissolution loss and excellent recyclability.

[0019] In various embodiments, highly lithium selective materials can be integrated into a continuous membrane system to provide an efficient method for extracting lithium from a brine source (e.g., a polar solvent in which lithium and one or more other metal ions are dissolved). In a preferred embodiment, the solvent is water.

[0020] In some embodiments, the brine source is a continental brine, a geothermal brine, or an oil field brine. Continental brine deposits are found in underground reservoirs, typically in locations with arid climates. The brine is held within a closed basin, with the surrounding rock formations being the source of dissolved components in the brine. Geothermal brine deposits are found in underground layers of rock with high heat flow. Geothermal brines are highly concentrated and often contain large amounts of dissolved metals. Oil field brine deposits can be generated from land that has oil reserves below ground. Large amounts of brine are also brought to the surface during extraction of oil and gas from oil fields. These brines are rich in dissolved metals, and in some places may contain lithium.

[0021] In various embodiments, the polar solution comprises Li + ions and at least one additional cation. In various embodiments, the additional cation is a monovalent cation, a divalent cation, or a combination thereof. In various embodiments, the monovalent cation is an alkali metal ion (e.g., Na + , K + , Rb + , Cs +In some embodiments, the multivalent ion is a divalent ion. In certain embodiments, the divalent ion is Ca 2+ or Mg 2+ and other alkaline earth metal ions.

[0022] In various embodiments, the ion-selective separation membranes include any suitable embedded particles (e.g., ions) that promote specific interactions with target metal ions (e.g., monovalent ions). In various embodiments, the ion-selective separation membranes are formed of any suitable adsorbent (e.g., metal ion adsorbents) configured to allow target ions to pass through the membrane under the influence of an applied potential difference, while non-target ions cannot pass through the membrane (e.g., are too large). In various embodiments, the target ion is selected from the group consisting of alkali metals (lithium, sodium, potassium, rubidium, cesium, francium), alkaline earth metals (beryllium, magnesium, calcium, strontium, barium, radium), transition metals (scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, yttrium, zirconium, niobium, molybdenum, technetium, ruthenium, rhodium, palladium, silver, cadmium, lutetium, hafnium, tantalum, tungsten, rhenium, osmium, iridium, platinum, gold, mercury, lawrencium, rutherfordium, dubnium, seaborgium, bohrium, hassium, meitnerium, darmstadtium, roentgenium, copernium, fluorine, fluorine-containing ions, and the like. and / or at least one of the superactinides.

[0023] In various embodiments, the ion-selective separation membrane selectively separates a target monovalent ion from a polar solution containing the target ion and at least one competing ion. In various embodiments, the competing ion is Na +, K + , Rb + , Cs + Another monovalent ion, such as Ca 2+ Or Mg 2+ or any combination of monovalent and divalent ions.

[0024] In various embodiments, the selectivity of the target monovalent ion over the competing ion is at least 1.1. In various embodiments, the selectivity of the target monovalent ion over the competing ion is at least 2. In various embodiments, the selectivity of the target monovalent ion over the competing ion is at least 5. In various embodiments, the selectivity of the monovalent ion over the competing ion is at least 10. In various embodiments, the selectivity of the monovalent ion over the competing ion is at least 50. In various embodiments, the selectivity of the monovalent ion over the competing ion is at least 100. In various embodiments, the selectivity of the monovalent ion over the competing ion is at least 200. In various embodiments, the selectivity of the monovalent ion over the competing ion is at least 1,000. In various embodiments, the selectivity of the monovalent ion over the competing ion is at least 2,000. In various embodiments, the selectivity of the monovalent ion over the competing ion is at least 5,000. In various embodiments, the selectivity of the monovalent ion over the competing ion is at least 10,000. In various embodiments, the selectivity of a monovalent ion over a competing ion is at least 100,000.

[0025] In various embodiments, the target singly charged ion is Li + , Na + , K + , Rb + , Cs + , Ca +2 , Mg +2 , Sr +2 , Fe +2 , Mn +2 , Ni +2 , Fe +3 , Al +3In various embodiments, the target monovalent ion is one or more metal cations selected from the group consisting of Li + In various embodiments, the target ion is one of the alkali metals or a member of the alkaline earth metal, transition metal, post-transition metal, lanthanide, actinide, or superactinide families. In various embodiments, the competing ion is Na + , K + , Rb + , Cs + , Ca +2 , Mg +2 , Sr +2 , Fe +2 , Mn +2 , Ni +2 , Fe +3 , Al +3 The metal cations include one or more metal cations selected from the group consisting of:

[0026] In some embodiments, the proposed process includes the following steps:

[0027] Step 1. Preparation of the LIS Adsorbent In various embodiments, lithium manganese oxide (LMO) or lithium titanium oxide (LTO) is prepared by heat treating a first material at a predetermined temperature.

[0028] When making an LMO, the first material can be LiMnO2. In various embodiments, the predetermined temperature can be about 350° C. to about 600° C. In various embodiments, the predetermined temperature can be about 450° C. In various embodiments, the heat treatment can be performed in air. In various embodiments, the heat treatment can be performed in a particular gaseous environment, such as an oxygen-free environment (e.g., a nitrogen environment).

[0029] In various embodiments, the LMO or LTO is delithiated to remove most (e.g., substantially all) of the lithium ions from the resulting crystal structure. In various embodiments, the delithiation of the LMO or LTO removes Li + / H +In various embodiments, the LIS adsorbent is delithiated for a period of 1 hour to 24 hours. In various embodiments, the LIS adsorbent is delithiated for at least 24 hours. In various embodiments, the LIS adsorbent is dispersed in a strong acid (e.g., HCl) aqueous solution. In various embodiments, the molar ratio of protons (provided by the acid) to target metal ions (e.g., lithium in LMO) is at least 50. In various embodiments, the resulting material is a target ion (e.g., lithium) adsorbent. For example, the resulting adsorbent has the formula H a Li b X c O d (HMO). In various embodiments, the resulting particles are washed with deionized water until the pH of the wastewater is neutral. In various embodiments, the resulting particles are dried in an oven at between 30° C. and 80° C. In various embodiments, X is manganese or titanium. In various embodiments, a is 0-10, b is 0-10, c is 0-10, and d is 0-10. In various embodiments, a is 0.5-2, b is 0-0.2, c is 0.5-5, and d is 1-6. In various embodiments, a is 1-1.5, b is 0-0.1, c is 1-2, and d is 4-4.5. In various embodiments, a is 1-1.2, b is 0.07-0.09, c is 1.6-1.8, and d is 4-4.2. In various embodiments, a is about 1.1, b is about 0.8, c is about 1.73, and d is about 4.05. In certain embodiments, b is greater than 0 to about 0.1.

[0030] Step 2. Dispersion of LIS particles in polymer solution. In various embodiments, the resulting particles were dispersed in an ionomer solution composed of any of the combinations of polymer backbones and functional groups listed above. In some embodiments, the HMO particles were dispersed in a specific mass ratio in an ionomer solution of poly(p-phenylene oxide) backbones functionalized with quaternary ammonium groups by sonicating, stirring, or shear mixing the mixture in an ice bath for about 30 seconds to about 1 hour (e.g., 30 seconds, 60 seconds, 10 minutes, or 1 hour). In various embodiments, the resulting particles (e.g., HMO particles) are loaded onto the membrane at a loading range of about 1% to about 50% (corresponding HMO-polymer mass ratios in the range of 0.1:1 to 0.5:1).

[0031] In various embodiments, the resulting lithium adsorbent is mixed with a polymer matrix in a predetermined ratio. In various embodiments, the adsorbent may be about 0.10 to about 75% by weight of the combined polymer and adsorbent mixture (adsorbent to polymer ratio of about 1:999 to about 3:1). In various embodiments, the adsorbent may be about 1 to about 75% by weight of the combined polymer and adsorbent mixture (adsorbent to polymer ratio of about 1:99 to about 3:1). In various embodiments, the adsorbent may be about 5 to about 75% by weight of the combined polymer and adsorbent mixture (adsorbent to polymer ratio of about 1:19 to about 3:1). In various embodiments, the adsorbent may be about 1 to about 50% by weight of the combined polymer and adsorbent mixture (adsorbent to polymer ratio of about 1:99 to about 2:1). In various embodiments, the adsorbent may be about 25 to about 50 weight percent of the combined polymer and adsorbent mixture (adsorbent to polymer ratio of about 1:3 to about 2:1). In various embodiments, the adsorbent may be at least 1 weight percent of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 5 weight percent of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 10 weight percent of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 15 weight percent of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 20 weight percent of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 25 weight percent of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 30 weight percent of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 35 weight percent of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 40% by weight of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 45% by weight of the combined polymer and adsorbent mixture.In various embodiments, the adsorbent may be about 50% by weight of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 55% by weight of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 60% by weight of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 65% by weight of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 70% by weight of the combined polymer and adsorbent mixture. In various embodiments, the adsorbent may be about 75% by weight of the combined polymer and adsorbent mixture.

[0032] In various embodiments, the polymer-sorbent mixture may be mixed via an external device, such as an ultrasonicator. In various embodiments, the polymer-sorbent mixture may be mixed in an ice bath. In various embodiments, the polymer-sorbent mixture may be mixed for up to 1 minute (e.g., 30 seconds).

[0033] Step 3. Fabrication of mixed matrix membranes (MMMs) from the LIS polymer solution. In various embodiments, the polymer adsorbent mixture may be heated to evaporate the solvent from the polymer adsorbent mixture to obtain a synthesized ion-selective separation membrane. In various embodiments, the polymer adsorbent mixture is heated at a temperature of about 50° C. to about 100° C. In various embodiments, the polymer adsorbent mixture is heated at a temperature of 80° C. In various embodiments, the polymer adsorbent mixture is heated for about 1 hour to about 24 hours. In various embodiments, the polymer adsorbent mixture is heated for about 20 hours. In various embodiments, the synthesized ion-selective separation membrane may be immersed in a test solution (e.g., a brine solution) before use. In various embodiments, the synthesized ion-selective separation membrane may be immersed in deionized (DI) water before use.

[0034] Step 4. Application of a driving force (e.g., potential, concentration, or pressure difference) to the MMM system to continuously extract lithium from the brine. In various embodiments, the potential difference can be from about 10 mV to about 1 V. In various embodiments, the transport rate of ions through the membrane is a function of the potential difference applied across the membrane. In various embodiments, increasing the potential difference increases the transport rate of selected ions through the ion-selective separation membrane. In various embodiments, decreasing the potential difference decreases the transport rate of selected ions through the ion-selective separation membrane.

[0035] In various embodiments, the applied potential difference is at least 12 mV. In various embodiments, the applied potential difference is at least 14 mV. In various embodiments, the applied potential difference is at least 16 mV. In various embodiments, the applied potential difference is at least 18 mV. In various embodiments, the applied potential difference is at most 1.8 V. In various embodiments, the applied potential difference is at most 1.6 V. In various embodiments, the applied potential difference is at most 1.4 V. In various embodiments, the applied potential difference is at least 1.2 V. In various embodiments, the applied potential difference is at least 1 V. In various embodiments, the applied potential difference is at least 1 V. In various embodiments, the applied potential difference is at least 2 V. In various embodiments, the applied potential difference is at least 5 V. In various embodiments, the applied potential difference is at least 50 V. In various embodiments, the applied potential difference is at most 1.5 V. In various embodiments, the applied potential difference is at most 2 V. In various embodiments, the applied potential difference is up to 5 V. In various embodiments, the applied potential difference is at least 10 V. In various embodiments, the applied potential difference is at least 50 V.

[0036] In various embodiments, the current density associated with the applied potential difference is at least 0.1 A / m 2In various embodiments, the current density associated with the applied potential difference may be at least 1 A / m 2 In various embodiments, the current density associated with the applied potential difference is at least 10 A / m 2 In various embodiments, the current density associated with the applied potential difference is at least 50 A / m 2 In various embodiments, the current density associated with the applied potential difference is at least 100 A / m 2 In various embodiments, the current density associated with the applied potential difference is at least 200 A / m 2 In various embodiments, the current density may be about 0.1 A / m 2 ~about 1A / m 2 In various embodiments, the current density may be about 1 A / m 2 ~about 10A / m 2 In various embodiments, the current density may be about 10 A / m 2 ~about 50A / m 2 In various embodiments, the current density is about 50 A / m 2 ~about 100A / m 2 In various embodiments, the current density is about 50 A / m 2 ~about 200A / m 2 In various embodiments, the current density may be about 100 A / m 2 ~about 200A / m 2 may be also possible.

[0037] Figure 5 shows a device that uses an ion-selective separation membrane to reject lithium. In particular, a driving force (electromotive force, pressure difference, osmotic pressure difference) draws cations from the brine toward the cathode, allowing a Li+-rich solution to pass through the membrane while rejecting non-target ions. EXAMPLES

[0038] Step 1: Lithium manganese oxide (LMO) was prepared by heat treating lithium manganese dioxide (LiMnO2) powder at 450 °C in air. LMO was delithiated by Li+ / H+ ion exchange for 24 h. 1.5 g of LMO was dispersed in 1.5 L of strong acid (e.g., 0.5 M HCl) to obtain lithium adsorbent H 1.10 Li 0.08 Mn 1.73 O 4.05 (HMO) was obtained. The HMO particles were then thoroughly washed with deionized (DI) water until the pH was neutral, and then dried in an oven at 50 °C.

[0039] Step 2: The HMO particles were dispersed in the anion exchange polymer solution at a constant mass ratio by sonicating the mixture in an ice bath for 30 s. Three types of membranes with HMO loadings of 10%, 25%, and 50% (corresponding HMO-polymer ratios of 0.1:1, 0.25:1, and 0.5:1) were fabricated.

[0040] Step 3: Anion exchange membranes containing HMOs (HMO-AEMs) were synthesized by evaporating the solvent of the HMO polymer mixture in an oven at 80 °C for 20 h. The fabricated HMO-AEM membranes were immersed in the test solution for 24 h and then in DI water for 2 h before performance testing. Figure 1 shows the cast AEM without HMO particles. Figure 2 shows the cast AEM with HMO particles dispersed in it.

[0041] Step 4. The HMO-AEM membrane was sandwiched between two glass diffusion cells. A potential difference was applied as the driving force. The membrane performance was tested under constant current (0.1 A) conditions for 75 min. The membrane was tested using two different feed solutions. Feed solution A contained equimolar amounts of Na2SO4 (0.017 M), Li2SO4 (0.017 M), and MgSO4 (0.017 M). Feed solution B contained Na + , K + , Ca 2+ , and Mg 2+Feed solution B was made to have ionic strength and sulfate concentrations similar to Feed solution A: 0.003M Li2SO4, 0.217M Na2SO4, 0.018M K2SO4, 0.008M CaSO4, and 0.017M MgSO4.

[0042] result: The ion specific fluxes calculated from Equation 1 are shown in Figure 3 (feed solution A) and Figure 4 (feed solution B). The ion selectivities were calculated according to Equation 2, and the results are shown in Table 1.

number

Claims

1. A polymer matrix; a metal ion compound dispersed within the polymer matrix; An ion selective separation membrane comprising: The metal ion compound is H a Li b X c O d wherein a is 1 to 1.5, b is 0 to 0.1, c is 1 to 2, d is 4 to 4.5, and X contains manganese or titanium.

2. 2. The ion-selective membrane of claim 1, wherein X is manganese or titanium.

3. 2. The ion-selective membrane of claim 1, wherein X is manganese.

4. The ion-selective separation membrane according to any one of claims 1 to 3, wherein b is greater than 0 and about 0.

1.

5. The ion-selective membrane according to any one of claims 1 to 4, wherein the metal ion compound is a substantially crystalline compound.

6. The ion-selective separation membrane according to any one of claims 1 to 5, wherein the polymer matrix comprises an anion exchange polymer.

7. The anion exchange polymer may be selected from the group consisting of methacrylamide, polyaromatic, styrene-divinylbenzene copolymer, polyester, polyvinyl chloride, poly(ethylene), poly(propylene), polystyrene, polystyrene-divinylbenzene copolymer, fluorinated interpenetrating polymer networks, low density polyethylene / high density polyethylene (interpenetrating polymer networks), polystyrene-block-ethylenebutylene-block-polystyrene, polystyrene / butadiene, polyethylene oxide, alkoxysilane functionalized polyethylene oxide, alkoxysilane functionalized polyvinyl alcohol, poly(epichlorohydrin-co-ethylene oxide), polyvinyl alcohol, poly(epichlorohydrin), polyacrylic acid, chitosan, polybenzimidazole, glycidyl methacrylate, 3-(methacryloxypropyl)trimethoxysilane, alkoxysilane / acrylates, epoxyalkoxysilanes, Poly(vinylbenzyl chloride), poly(phenylene oxide), poly(methyl acrylate), polyethyleneimine, poly(1,1-dimethyl-3,5-dimethylenepiperidinium chloride), poly(diallyldimethylammonium chloride), poly(allylamine), poly(acrylonitrile-co-2-dimethylaminoethyl methacrylate), polychloromethylstyrene, poly(divinylbenzene), norbornene / dicyclopentadiene, cyclooctene, poly(phenylene), poly(methyl methacrylate), poly(butyl acrylate), poly(methyl methacrylate-co-butyl acrylate-co-vinylbenzyl), polyvinyl butyral, polyvinylidene fluoride, ethylene tetrafluoroethylene, fluorinated ethylene propylene, polytetrafluoroethylene, poly(4-vinylpyridine), polystyrene-ethylene-butylene sulfonic acid copolymer, epichlorohydrin / 1,The ion-selective separation membrane according to claim 6, comprising a polymer backbone selected from the group consisting of 4-diazabicyclo[2.2.2]octane, polyethylene glycol, polysulfone, cardo polyether sulfone, poly(phthalazinone ether sulfone ketone), polysulfone polyphenylene sulfide sulfone, polyarylene, polydiallyldimethylammonium chloride, poly(etherimide), and sulfonated tetrafluoroethylene-based fluorinated polymer-copolymer.

8. 8. The ion-selective separation membrane according to claim 6 or 7, wherein the anion exchange polymer contains a functional group selected from the group consisting of quaternary ammonium, tertiary diamine, (benzo)imidazolium, guanidinium, and pyridinium.

9. 8. The ion-selective membrane of claim 6 or 7, wherein the anion exchange polymer comprises nitrogen-free functional groups.

10. The ion-selective separation membrane according to any one of claims 6 to 9, wherein the anion exchange polymer contains a functional group selected from the group consisting of phosphonium, sulfonium, ruthenium, nickel, and cobalt.

11. The ion-selective separation membrane according to any one of claims 1 to 10, wherein X is manganese, a is about 1.10, b is about 0.08, c is about 1.73, and d is about 4.

05.

12. The ion-selective separation membrane according to any one of claims 1 to 11, further comprising a plurality of embedded ionic particles.

13. A method for producing an ion-selective separation membrane, comprising the steps of: Providing a lithium manganese oxide or a lithium titanium oxide; delithiating the lithium manganese oxide or the lithium titanium oxide to obtain a lithium adsorbent; dispersing the lithium adsorbent in a polymer matrix to form a polymer adsorbent mixture; heating the polymer-adsorbent mixture to obtain the synthesized ion-selective separation membrane; The method comprising:

14. Li + / H + 14. The method of claim 13, wherein delithiation is carried out by ion exchange.

15. 15. The method of claim 13 or 14, wherein the delithiation is carried out for at least 24 hours.

16. The delithiation is performed by Li + / H + 16. The method of any one of claims 13 to 15, comprising mixing the lithium manganese oxide or the lithium titanium oxide with a dispersion liquid after ion exchange.

17. The method of claim 16 , wherein the dispersion comprises an acid.

18. 20. The method of claim 17, wherein the acid comprises hydrochloric acid.

19. The method according to any one of claims 16 to 18, wherein the delithiation comprises mixing the lithium manganese oxide or the lithium titanium oxide with the dispersion liquid, followed by washing with a washing liquid.

20. 20. The method of claim 19, wherein the cleaning solution comprises deionized water.

21. 21. The method according to claim 19 or 20, wherein washing is carried out until the pH of the lithium adsorbent is neutral.

22. The method of any one of claims 13 to 21, wherein the delithiation further comprises drying the lithium adsorbent.

23. 14. The method of claim 13, wherein providing the lithium manganese oxide comprises heating lithium manganese dioxide.

24. The method of claim 23, wherein the heating is performed at a temperature of about 350° C. to about 600° C.

25. 25. The method of claim 24, wherein the temperature is about 450°C.

26. 26. The method of claim 24 or 25, wherein the heating is performed in air.

27. 14. The method of claim 13, wherein the polymer-sorbent mixture is heated to evaporate the solvent of the mixture.

28. 14. The method of claim 13, wherein the synthesized ion-selective separation membrane has a lithium adsorbent to polymer matrix ratio of about 1:99 to about 2:

1.

29. 14. The method of claim 13, wherein the synthesized ion-selective separation membrane has a lithium adsorbent to polymer matrix ratio of about 1:19 to about 2:

1.

30. 14. The method of claim 13, wherein the synthesized ion-selective separation membrane has a lithium adsorbent to polymer matrix ratio of about 1:3 to about 2:

1.

31. 1. A method for selectively separating ions in a polar solution containing a plurality of ions, comprising: Preparing an ion-selective separation membrane according to any one of claims 1 to 12; contacting the polar solution with the ion-selective separation membrane; applying a potential difference across said ion-selective separation membrane to selectively transport target ions through said membrane; The method comprising:

32. The target ion is Li + 32. The method of claim 31 , comprising ions.

33. The plurality of ions are Na + , K + , Ca 2+ , and Mg 2+ 32. The method of claim 31 , comprising at least one of:

34. 32. The method of claim 31 , wherein the potential difference is from about 1 V to about 50 V.

35. 32. The method of claim 31 , wherein a current associated with the potential difference is from about 0.01 A to about 0.5 A.

36. 32. The method of claim 31 , wherein a current associated with the potential difference is about 0.1 A.

37. 37. The method of any one of claims 31 to 36, wherein the polar solution comprises a continental brine, a geothermal brine, an oil field brine, a leachate obtained from a mining operation, a leachate obtained from a battery recycling operation, or any other leachate containing target ions to be separated.

38. The method of any one of claims 31 to 37, wherein the method is continuous.

39. a polymer matrix having a polymer backbone and one or more functional groups; a metal ion adsorbent dispersed within the polymer matrix; An ion selective separation membrane comprising: The ion-selective separation membrane, wherein the metal ion adsorbent is configured to allow transport of a target ion through the membrane and block the passage of one or more non-target ions when a potential difference is applied across the membrane.