Advanced refining cell for aluminum scrap recycling

By employing a non-carbonaceous substrate with guiding mechanisms to direct wettable materials in aluminum refining cells, the inefficiencies in aluminum production are addressed, achieving higher purity and lower energy consumption.

JP2024540305APending Publication Date: 2024-10-31ALCOA USA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024526618
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-02-17
Filing Date
2022-11-07
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing aluminum production methods from alumina face inefficiencies and challenges in purifying aluminum, particularly in the refinement process, leading to high energy consumption and material wastage.

Method used

The use of a non-carbonaceous substrate with guiding mechanisms, such as TiB2, to direct wettable materials like aluminum and magnesium in a predetermined direction within an aluminum refining cell, reducing corrosion and enhancing the efficiency of the refining process.

Benefits of technology

This approach improves the energy efficiency of aluminum refinement by minimizing corrosion and optimizing material usage, resulting in higher purity aluminum production with reduced energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540305000001_ABST
    Figure 2024540305000001_ABST
Patent Text Reader

Abstract

The present application is directed to products and methods relating to an aluminum purification cell having a non-carbonaceous substrate with a directing mechanism. The directing mechanism can be configured to direct a wettable material in a predetermined direction. The non-carbonaceous substrate can be at least partially covered with solid aluminum metal. The wettable material can be aluminum metal.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is the subject of a patent application Ser. 2 This application claims priority to U.S. Provisional Patent Application No. 63 / 276,892, filed November 8, 2021, entitled "Advanced Purification Cell for Aluminum Scrap Recycling," which is a continuation of U.S. Provisional Patent Application No. 63 / 311,366, filed February 17, 2022, entitled "Advanced Purification Cell for Aluminum Scrap Recycling," each of which is incorporated herein by reference in its entirety. [Background technology]

[0002] Aluminum has traditionally been produced as alumina (Al 2 O 3 ) has been made from alumina (Al 2 O 3 The conversion of aluminium to alumina (Al 2 O 3 ) is dissolved in cryolite, a flux, and then an electric current is passed through the mixture, dissolving the carbon from the carbon anode into dissolved alumina (Al 2 O 3 ) to obtain aluminum and carbon dioxide as by-products. Various efforts have been made to purify aluminum, including the "Hoopes process" (see U.S. Pat. No. 1,534,315), as well as the method described in commonly owned WO 2016 / 130823. Summary of the Invention

[0003] In general, the present disclosure relates to methods and systems for refining aluminum in an aluminum refining cell. In some embodiments, the aluminum refining cell includes at least one electrode having an induction mechanism. Various induction mechanisms are described in "Methods and Systems of TiB 2 No. 63 / 276,892, filed November 8, 2021, entitled "Infiltrated Solid Aluminum Products," which is hereby incorporated by reference in its entirety.

[0004] In some aspects, the technology described herein relates to an aluminum purification cell comprising a non-carbonaceous substrate, the non-carbonaceous substrate comprising a guiding mechanism configured to guide a wettable material in a predetermined direction.

[0005] In some aspects, the technology described herein relates to a cell comprising a cell chamber, at least one anode within the cell chamber, and at least one cathode within the cell chamber, the at least one cathode at least partially overlying a top portion of the at least one anode.

[0006] In some aspects, the technology described herein relates to a cell, where at least a portion of the wettable material is disposed within and / or on a guidance feature.

[0007] In some aspects, the technology described herein relates to a cell, wherein the wettable material is a molten metal.

[0008] In some aspects, the technology described herein relates to a cell, wherein the wettable material comprises a metal.

[0009] In some aspects, the technology described herein relates to a cell, wherein the metal comprises at least aluminum and magnesium.

[0010] In some aspects, the technology described herein relates to a cell, wherein the metal comprises aluminum.

[0011] In some embodiments, the technology described herein relates to a cell where the metal comprises at least 50 weight percent aluminum, or at least 55 weight percent aluminum, or at least 60 weight percent aluminum, or at least 65 weight percent aluminum, or at least 70 weight percent aluminum, or at least 75 weight percent aluminum, or at least 80 weight percent aluminum, or at least 85 weight percent aluminum, or at least 90 weight percent aluminum, or at least 95 weight percent aluminum.

[0012] In some aspects, the technology described herein relates to a cell, wherein the metal is selected from the group consisting of an aluminum alloy, aluminum metal, and combinations thereof.

[0013] In some aspects, the technology described herein relates to a cell in which a surface of a non-carbonaceous substrate is at least partially covered with solid aluminum metal.

[0014] In some aspects, the technology described herein relates to a cell, wherein the guiding features are selected from the group consisting of slots, grooves, pores, and combinations thereof.

[0015] In some aspects, the technology described herein relates to a cell, wherein the non-carbonaceous substrate comprises a cermet or a ceramic.

[0016] In some aspects, the technology described herein relates to a cell, the non-carbonaceous substrate being TiB 2 Includes.

[0017] In some aspects, the technology described herein relates to a cell, the non-carbonaceous substrate being TiB 2 It essentially consists of:

[0018] In some aspects, the technology described herein relates to a cell and the predetermined direction is vertical and / or horizontal.

[0019] In some aspects, the technology described herein relates to a cell, and the predetermined direction is an upward direction toward the electrolyte of an aluminum refining cell.

[0020] In some aspects, the technology described herein relates to a cell, where the non-carbonaceous substrate is not an electrode.

[0021] In some aspects, the technology described herein relates to a cell, where the non-carbonaceous substrate is an electrode.

[0022] In some aspects, the technology described herein relates to a cell where the non-carbonaceous substrate is an anode or a cathode.

[0023] In some aspects, the technology described herein relates to a cell, wherein the non-carbonaceous substrate is a first substrate and the cell includes a second substrate.

[0024] In some aspects, the technology described herein relates to a cell, wherein the second substrate is a carbonaceous substrate.

[0025] In some aspects, the technology described herein relates to a cell, wherein the second substrate is a non-carbonaceous substrate.

[0026] In some aspects, the technology described herein relates to a cell, wherein the second substrate comprises a cermet or a ceramic.

[0027] In some aspects, the technology described herein relates to a cell, wherein the second substrate is TiB 2 Includes.

[0028] In some aspects, the technology described herein relates to a cell, wherein the second substrate is TiB 2 It essentially consists of:

[0029] In some aspects, the technology described herein relates to a cell, wherein the second substrate comprises a guide mechanism.

[0030] In some aspects, the technology described herein relates to a cell where the second substrate is devoid of a directing mechanism.

[0031] In some aspects, the technology described herein relates to a cell, wherein the second substrate is an anode.

[0032] In some aspects, the technology described herein relates to a cell, wherein the second substrate is a cathode.

[0033] In some aspects, the technology described herein relates to an aluminum purification cell that includes: (a) a non-carbonaceous substrate comprising at least one directing feature; and (b) solid aluminum metal at least partially covering a surface of the non-carbonaceous substrate.

[0034] In some aspects, the technology described herein relates to a cell comprising a cell chamber, at least one anode within the cell chamber, and at least one cathode within the cell chamber, the at least one cathode at least partially overlying a top portion of the at least one anode.

[0035] In some aspects, the technology described herein relates to a cell, wherein at least a portion of the solid aluminum metal is disposed within and / or on an induction feature.

[0036] In some aspects, the technology described herein relates to a cell, wherein the solid aluminum metal is at least partially contained within at least one induction feature.

[0037] In some aspects, the technology described herein relates to a cell, wherein a non-carbonaceous substrate comprises a surface region, a first portion of the surface region comprising at least one directing feature and a second portion of the surface region is devoid of any directing features.

[0038] In some aspects, the technology described herein relates to a cell, wherein a first portion of the surface region is at least partially covered by solid aluminum metal.

[0039] In some aspects, the technology described herein relates to a cell, wherein a first portion of the surface area is at least 1% covered by solid aluminum metal.

[0040] In some aspects, the technology described herein relates to a cell, wherein a second portion of the surface region is at least partially covered by solid aluminum metal.

[0041] In some aspects, the technology described herein relates to a cell, wherein the second portion of the surface area is at least 1% covered by solid aluminum metal.

[0042] In some aspects, the technology described herein relates to a method of using any of the cells, wherein a surface of a non-carbonaceous substrate is at least partially covered with solid aluminum metal, and the method includes heating the non-carbonaceous substrate above a melting point temperature of the solid aluminum metal.

[0043] In some aspects, the technology described herein relates to methods of using any cell, including limiting or preventing electrolyte-mediated corrosion of non-carbonaceous substrates in an aluminum refining cell.

[0044] In some aspects, the technology described herein relates to methods, wherein the limiting or preventing includes at least partially covering the non-carbonaceous substrate with a wettable material.

[0045] In some embodiments, the technology described herein relates to methods, wherein limiting or preventing includes covering at least 50%, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, at least 85%, at least 90%, at least 95%, or at least 99% of a surface area of ​​the non-carbonaceous substrate with the wettable material.

[0046] In some aspects, the technology described herein relates to a method, wherein the wettable material limits or prevents the electrolyte from contacting the exterior surface of the substrate.

[0047] In some aspects, the technology described herein relates to a method of using any of the cells, including limiting or preventing corrosion of the non-carbonaceous substrate when the temperature of the non-carbonaceous substrate is below the melting point temperature of solid aluminum metal.

[0048] In some aspects, the technology described herein relates to a method, wherein the limiting or preventing includes at least partially covering the non-carbonaceous substrate with solid aluminum.

[0049] In some embodiments, the technology described herein relates to methods, where limiting or preventing includes covering at least 50%, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, at least 85%, at least 90%, at least 95%, or at least 99% of a surface area of ​​the non-carbonaceous substrate with solid aluminum.

[0050] In some aspects, the technology described herein relates to a method, wherein the solid aluminum limits or prevents the electrolyte from contacting the exterior surface of the substrate.

[0051] In some aspects, the technology described herein relates to a method, the method including: (a) providing an aluminum feedstock to an aluminum refining cell, the aluminum feedstock comprising aluminum metal, the aluminum refining cell comprising a molten metal pad and an electrolyte, the molten metal pad having a density greater than a density of the electrolyte; (b) passing a current through at least one anode, through the electrolyte, and to at least one cathode, where (i) the at least one anode and the at least one cathode are partially disposed within the electrolyte, (ii) the at least one anode is partially disposed within the molten metal pad, (iii) the at least one anode and / or the at least one cathode are non-carbonaceous substrates comprising a directing mechanism, and (iv) the directing mechanism is configured to direct a wettable material in a predetermined direction; (c) directing aluminum metal from the molten metal pad into the electrolyte by the directing mechanism; (d) generating at least some aluminum ions in the electrolyte; and (e) producing a refined aluminum product.

[0052] In some aspects, the technology described herein relates to a cell, where the directing mechanism is within or on a substrate (e.g., a non-carbonaceous substrate).

[0053] Although the present disclosure is generally directed to refining aluminum, the devices, systems, and methods described herein are applicable to refining other metals (e.g., magnesium).

[0054] In some embodiments, the guidance mechanism comprises at least one slot that is open or closed, and at least one slot is a TiB 2 In some embodiments, the dimensions of the at least one slot are predetermined. In some embodiments, the TiB 2The substrate comprises a first protrusion and a second protrusion, and the guiding mechanism comprises a slot defined between an inner surface of the first protrusion and an inner surface of the second protrusion. In some embodiments, the slot extends the entire length (l) of the first protrusion and the entire length (l) of the second protrusion. In some embodiments, the entire length (l) of the first protrusion and the entire length (l) of the second protrusion range from about 0.01 meters to about 1 meter. In some embodiments, the thickness (t) of the first protrusion and the thickness (t) of the second protrusion range from about 1 mm to about 20 mm. In some embodiments, the slot extends a distance (d) between the inner surface of the first protrusion and the inner surface of the second protrusion. In some embodiments, the distance (d) ranges from about 20 μm to about 20 mm. In some embodiments, the width (w) of the first protrusion and the width (w) of the second protrusion range from about 1 mm to about 20 mm.

[0055] As noted above, in some embodiments, the slots are fully closed. In some embodiments, when the slots are fully closed, the guide mechanism is a fully closed channel. In some embodiments, at least one slot is partially closed, i.e., a partially closed slot. In some embodiments, the partially closed slot comprises a closed lateral width opening. When at least one slot is partially closed, the lateral width opening of the at least one slot can be fully closed and extend continuously over a portion of the length of the slot. When at least one slot is partially closed, the lateral width opening of the at least one slot can be partially closed over the entire length of the slot. When at least one slot is partially closed, the amount of closure of the lateral width opening of the at least one slot can vary along the length of the slot.

[0056] As described above, the substrate may include at least one channel. The channel may be of any length, width, size, or shape. In some embodiments, the channel extends substantially parallel to the longitudinal axis of the substrate. In some embodiments, the channel extends at an angle to the longitudinal axis of the substrate. In some embodiments, multiple channels may be combined into a single channel. In some embodiments, a single channel may be split into multiple channels. The cross-section of the channel may be of any shape or size. In some embodiments, the cross-section is substantially constant throughout the length of the channel. In some embodiments, the cross-section is substantially variable throughout the length of the channel. In some embodiments, the cross-section may increase and / or decrease along the length of the channel.

[0057] This disclosure generally relates to TiB 2 Although the term refers to a substrate, other ceramic and / or cermet substrates with guiding features may be used. Any ceramic and / or cermet substrate with guiding features may be used with any wettable metal. In some embodiments, any wettable metal may be any suitable metal for transfer through the ceramic and / or cermet substrate. In some embodiments, a suitable metal may be aluminum, e.g., aluminum alloys, metallic aluminum, and combinations thereof. In some embodiments, a suitable metal may be copper, e.g., copper alloys, metallic copper, and combinations thereof. In some embodiments, the wettable material consists essentially of aluminum, magnesium, copper, and combinations thereof. In some embodiments, the wettable material is primarily aluminum. In one aspect, the present disclosure relates to products having a ceramic or cermet substrate with guiding features, the guiding features configured to guide the ceramic or cermet wettable material in a predetermined direction. In some embodiments, the substrate is a ceramic substrate. In some embodiments, the ceramic substrate is TiB 2 Base material, ZrB 2Substrate, or HfB 2 In some embodiments, the ceramic wettable material is aluminum, such as aluminum alloys, aluminum metal, and combinations thereof.

[0058] The above disclosure is 2 and aluminum, the apparatus, systems, and methods described herein are directed to TiB 2 For example, the disclosure herein may be applicable to other ceramic and / or cermet materials other than those described above. For example, the disclosure herein may be applicable to other metal borides (e.g., metal diborides) that have metal wettability capabilities, such as ZrB, to name just two examples. 2 and HfB 2 are equally applicable to both, both of which are aluminum wettable materials.

[0059] In some embodiments, the substrate can be a carbon-based (carbonaceous) material. In some embodiments, the carbon-based material can be an inorganic carbon-based material. Suitable carbon-based materials can include, for example, amorphous and crystalline forms of carbon. In some embodiments, the carbon-based material includes graphite. In some embodiments, the substrate includes a pre-fired carbon electrode material. The carbon-based substrate can include a plating material to promote wettability of a suitable metal, for example aluminum.

[0060] In some embodiments, the substrate can be a non-carbonaceous material. A non-carbonaceous material is any material that is not carbon-based. Non-carbonaceous materials include, for example, ceramic and cermet materials. In some embodiments, the substrate can be a ceramic or a cermet.

[0061] The ceramic material includes an inorganic, non-metallic material. The inorganic, non-metallic material can include a boride, oxide, nitride, or carbide material. In some embodiments, the ceramic material includes titanium. In some embodiments, the ceramic material includes a metal boride (e.g., a metal diboride). In some embodiments, the metal diboride material is TiB 2 , ZrB 2 , HfB 2 , or SrB 2 Includes.

[0062] A cermet material is a material of ceramic and metallic materials. A cermet material may include a ceramic matrix bonded by a metallic binder. In some embodiments, the cermet material includes copper (Cu), nickel (Ni), chromium (Cr), tungsten (W), molybdenum (Mo), iron (Fe), cobalt (Co), or alloys or combinations thereof. In some embodiments, the cermet material includes nickel-titanium carbide or nickel-titanium diboride.

[0063] In some embodiments, the substrate comprises, consists essentially of, or consists of the described materials. In one embodiment, the substrate consists essentially of, or consists of a ceramic. In one embodiment, the substrate consists essentially of, or consists of a cermet. In one embodiment, the substrate consists essentially of, or consists of a carbon-based material.

[0064] In some embodiments, the substrate is a plating material that promotes wettability. In some embodiments, the plating material is a ceramic and / or a cermet, such as any of the ceramic or cermet materials described herein. In some embodiments, the substrate is a ceramic, such as TiB 2 The carbon-based material is plated with [Brief description of the drawings]

[0065] [Figure 1A]FIG. 1A illustrates one embodiment of a method for directing a TiB 2 wettable material in a predetermined direction using a directing mechanism.

[0066] [Figure 1B] FIG. 1B illustrates another embodiment of a method for directing a TiB 2 wettable material in a predetermined direction using a directing mechanism.

[0067] [Figure 2A] FIG. 2A is a perspective view of one embodiment of the product, in which a TiB2 substrate has multiple slots as guiding features.

[0068] [Figure 2B] FIG. 2B is a first side view of the embodiment shown in FIG. 2A.

[0069] [Figure 2C] 2C is an enlarged partial top cross-sectional view of the embodiment shown in FIG. 2A, indicated by the dashed circle in FIG. 2A.

[0070] [Figure 3A] FIG. 3A is a front view of one embodiment of the product, in which the TiB2 substrate has slots as a guiding feature.

[0071] [Figure 3B] FIG. 3B is a cross-sectional view of the section taken along dashed line 3B shown in FIG. 3A.

[0072] [Figure 3C] FIG. 3C is a first side view of the embodiment shown in FIG. 3A.

[0073] [Figure 4A] FIG. 4A is a front view of one embodiment of the product, in which the TiB2 substrate has multiple grooves as guiding features.

[0074] [Figure 4B] FIG. 4B is a first side view of the embodiment shown in FIG. 4A.

[0075] [Figure 4C] 4C is an enlarged partial cross-sectional view of the embodiment shown in FIG. 4A, indicated by the dashed circle in FIG. 4A.

[0076] [Figure 4D] FIG. 4D is an alternative configuration of grooves for the embodiment shown in FIG. 4C.

[0077] [Figure 5A] FIG. 5A is a side view of another embodiment of an article in which a TiB2 substrate has a plurality of pores as guide features.

[0078] [Figure 5B] FIG. 5B is an enlarged view of a portion of the embodiment shown in FIG. 5A that is indicated by the dashed lines in FIG. 5A.

[0079] [Figure 6A] FIG. 6A is a perspective view of one embodiment of the product, in which a TiB2 substrate has multiple slots as guiding mechanisms and a solid aluminum metal covers the TiB2 substrate.

[0080] [Figure 6B] FIG. 6B is a first side view of a cross section taken along arrow 6B shown in FIG. 6A.

[0081] [Figure 6C] FIG. 6C is an enlarged partial cross-sectional view of the embodiment shown in FIG. 6A, indicated by the dashed circle in FIG. 6A.

[0082] [Figure 6D] FIG. 6D is a cross-sectional side view of one embodiment of the product, in which a TiB2 substrate has multiple slots as guiding mechanisms and solid aluminum metal covers the top of the TiB2 substrate.

[0083] [Figure 6E]Figure 6E is a partial cross-sectional view taken along dashed line 6E shown in Figure 6D, where only one of the slots is shown. The cross section is along the top of the TiB2 substrate where the solid aluminum metal is present.

[0084] [Figure 6F] Figure 6F is a partial cross-sectional view taken along dashed line 6F shown in Figure 6D, where only one of the slots is shown, and the cross section is taken along the bottom of the TiB2 substrate where there is no solid aluminum metal.

[0085] [Figure 6G] FIG. 6G is a cross-sectional side view of one embodiment in which a TiB2 substrate has multiple slots as guiding mechanisms and solid aluminum metal covers the front half of the TiB2 substrate.

[0086] [Figure 6H] FIG. 6H is a partial cross-sectional view taken along dashed line 6H shown in FIG. 6G, where only one of the slots is shown.

[0087] [Figure 6I] FIG. 6I is a side view of one embodiment, where a TiB2 substrate has slots and solid aluminum metal within the slots as a guide mechanism.

[0088] [Figure 6J] FIG. 6J is a partial cross-sectional view taken along dashed line 6J shown in FIG. 6I, with only one of the slots being shown in FIG. 6J.

[0089] [Figure 6K] FIG. 6K is a front view of one embodiment in which a TiB2 substrate has multiple slots as guiding features with solid aluminum metal covering some or none of the slots.

[0090] [Figure 6L] FIG. 6L is a first side view of the embodiment shown in FIG. 6K.

[0091] [Figure 6M] FIG. 6M is a front view of one embodiment of a TiB2 substrate having a surface region having a first portion of the surface region having a plurality of slots as guiding features and a second portion of the surface region without any guiding features.

[0092] [Figure 6N] FIG. 6N is a first side view of the embodiment shown in FIG. 6M, where a second portion of the surface area is devoid of any guidance features.

[0093] [Figure 7A] FIG. 7A is a front view of one embodiment of the product, in which a TiB2 substrate has slots as guiding features and solid aluminum metal covers the TiB2 substrate.

[0094] [Figure 7B] FIG. 7B is a cross section taken along dashed line 7B shown in FIG. 7A.

[0095] [Figure 7C] FIG. 7C is a first side view of a cross section taken along line 7C shown in FIG. 7A.

[0096] [Figure 7D] FIG. 7D is a front view of one embodiment of the product, in which the TiB2 substrate has a slot as a guide mechanism and solid aluminum metal covers a portion of the slot.

[0097] [Figure 7E] FIG. 7E is a cross section taken along dashed line 7E shown in FIG. 7D.

[0098] [Figure 7F] FIG. 7F is a first side view of the embodiment shown in FIG. 7F.

[0099] [Figure 8A] FIG. 8A is a front view of one embodiment of the product, in which a TiB2 substrate has multiple grooves as guiding features and solid aluminum metal covers the TiB2 substrate.

[0100] [Figure 8B] FIG. 8B is a first side view of a cross section taken along line 8B shown in FIG. 8A.

[0101] [Figure 8C] FIG. 8C is an enlarged partial cross-sectional view of the embodiment shown in FIG. 8A, indicated by the dashed circle in FIG. 8A.

[0102] [Figure 8D] FIG. 8D is a back view of one embodiment of the product, in which the TiB2 substrate has multiple grooves as guiding features and solid aluminum metal covers the front half of the TiB2 substrate.

[0103] [Figure 8E] FIG. 8E is a first side view of the cross section taken along line 8E shown in FIG. 8D.

[0104] [Figure 8F] FIG. 8F is an enlarged partial cross-sectional view of the embodiment shown in FIG. 8D, indicated by the dashed circle in FIG. 8F.

[0105] [Figure 9] FIG. 9 is a close-up view of a portion of an embodiment having pores and solid aluminum metal, according to some embodiments.

[0106] [Figure 10] FIG. 10 is a front view of the final sintered TiB2 foam product used in the laboratory-scale tests.

[0107] [Figure 11]FIG. 11 shows a front view of four TiB2 foam samples used in the lab-scale testing, the samples having porosities of approximately 10, 20, 30, and 45 pores per inch ("PPI").

[0108] [Figure 12] FIG. 12 is a schematic cutaway side view of the three crucibles used in the laboratory-scale testing, each containing four TiB2 foam samples that were immersed (partially or fully) in molten aluminum for 48 hours.

[0109] [Figure 13A] FIG. 13A is a front view of a TiB2 foam sample from the crucible used in the lab-scale testing after being fully immersed in molten aluminum for about 48 hours.

[0110] [Figure 13B] FIG. 13B is a front view of a TiB2 foam sample from the crucible used in the lab-scale testing after being partially immersed in molten aluminum for about 48 hours.

[0111] [Figure 14] FIG. 14 illustrates one embodiment of a method for refining aluminum metal, such as aluminum scrap, in an aluminum refining cell.

[0112] [Figure 15A] FIG. 15A is a schematic cross-sectional side view of one embodiment of an aluminum refining cell for refining aluminum according to some embodiments.

[0113] [Figure 15B] FIG. 15B is an expanded view of a representative electrode pair shown in FIG. 15A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0114] This document includes several sections. Section i describes an aluminum refining cell. Section ii describes a substrate having an induction mechanism. Section iii describes the start-up of an aluminum refining cell. Section iv describes the use of a substrate having an induction mechanism of section ii in an aluminum refining cell of section i. Definitions are also included below.

[0115] The present disclosure is further described with reference to the accompanying drawings, in which like structures are referenced with like reference numerals throughout the several views. The drawings constitute a part of this specification and include exemplary embodiments of the present disclosure, illustrating various objects and features thereof. Moreover, the drawings are not necessarily to scale, and some features may be exaggerated to show details of particular components. Moreover, any dimensions, specifications, etc. shown in the figures are for illustrative purposes and not limiting. Therefore, specific structural and functional details disclosed herein should not be interpreted as limiting, but merely as a representative basis for teaching those skilled in the art to various uses of the present disclosure.

[0116] Among these disclosed advantages and improvements, other objects and advantages of the present disclosure will become apparent from the following description taken in conjunction with the accompanying drawings. Detailed embodiments of the present disclosure are disclosed herein. However, it should be understood that the disclosed embodiments are merely exemplary of the present disclosure, which may be embodied in various forms. Moreover, each of the examples given in connection with the various embodiments of the present invention are intended to be illustrative and not limiting.

[0117] Throughout this specification and the claims, the following terms have the meanings expressly associated therewith, unless the context clearly dictates otherwise. As used herein, the phrases "in one embodiment" and "in some embodiments" may refer to the same embodiment, but do not necessarily refer to the same embodiment. Additionally, as used herein, the phrases "in another embodiment" and "in some other embodiments" may refer to different embodiments, but do not necessarily refer to different embodiments. Thus, as described below, various embodiments of the invention can be readily combined without departing from the scope or spirit of the invention.

[0118] Additionally, the term "or" as used herein is an inclusive "or" operator and is equivalent to the term "and / or" unless the context clearly dictates otherwise. The term "based on" is not exclusive and acknowledges that a term may be based on other unrecited factors unless the context clearly dictates otherwise. Additionally, throughout this specification, the meanings of "a," "an," and "the" include plural referents. "In" includes "in" and "on."

[0119] As used herein, "aluminum source" means a material having at least 50% aluminum by weight.

[0120] As used herein, "refined aluminum" means a material having at least 99.5% aluminum by weight.

[0121] As used herein, "refined molten aluminum" means a material having at least 99.5% by weight molten aluminum.

[0122] As used herein, "raffinate" means aluminum that contains a very high impurity content.

[0123] As used herein, "molten metal pad" means a reservoir of molten material disposed beneath the electrolyte, the molten material comprising aluminum.

[0124] As used herein, "sludge" refers to the sludge that settles during aluminum refining. In some embodiments, the sludge comprises solid material.

[0125] As used herein, "aluminum wettable" means that the contact angle with molten aluminum is 90 degrees or less.

[0126] As used herein, "wettable material" means that it has a contact angle with a non-carbonaceous material of 90 degrees or less.

[0127] As used herein, "electrolyte" refers to a medium through which electric current flows by the movement of ions / ionic species. In one embodiment, the electrolyte can include a molten salt.

[0128] As used herein, "energy efficiency" means the amount of energy (in kilowatt-hours) consumed by an aluminum refining cell per kilogram of refined aluminum produced by the aluminum refining cell. Energy efficiency can therefore be expressed in kilowatt-hours per kilogram (kWh / kg) of aluminum produced.

[0129] As used herein, "anode-cathode overlap" (ACO) means the vertical distance from the distal end of an anode (e.g., an elongated vertical anode) to the distal end of each cathode (e.g., an elongated vertical cathode).

[0130] As used herein, "anode-cathode distance" (ACD) means the horizontal distance separating an anode (eg, an elongated vertical anode) from each cathode (eg, an elongated vertical cathode).

[0131] i. Aluminum refining cell with substrate using induction mechanism The present disclosure relates to an aluminum refining cell having a substrate with one or more induction features. Such substrates are described in detail in section ii below and further described in commonly owned U.S. Provisional Patent Application No. 63 / 276,892, the contents of which are incorporated herein by reference in their entirety. The aluminum refining cell disclosed herein can include any of the substrates described in section ii, and in any combination. In some embodiments, the substrate is not an electrode. In some embodiments, the substrate is an electrode. For example, a first electrode may comprise a substrate with at least one groove, while a second electrode may comprise a substrate with a slot or void. As another example, a first electrode may comprise a substrate without induction features and a second electrode may comprise a substrate with a groove. As another example, a first electrode may comprise a substrate with a groove or void, and a second electrode may comprise a substrate without induction features. As another example, a first electrode may comprise a substrate with voids, and a second electrode may comprise a substrate with voids. Any of the substrates can be used in any combination with any carbonaceous or non-carbonaceous electrode.

[0132] FIG. 14 illustrates one embodiment of a method for refining aluminum metal, e.g., aluminum scrap, in an aluminum refining cell. In some embodiments, the method of refining aluminum in an aluminum refining cell includes using at least one electrode, e.g., an anode or a cathode. FIG. 14 shows some steps as dashed boxes to indicate that these steps are optional. In some embodiments, the method includes feeding an aluminum feedstock to the aluminum refining cell (feeding step 10100), inducing the aluminum metal into an electrolyte (inducing step 10200), and producing a refined aluminum product (producing step 10300). In some embodiments, the method includes energizing the electrodes (e.g., the anode and / or cathode) (energizing step 10420) and / or generating ions in the electrolyte (ion generating step 10440).

[0133] 15A is a schematic cross-sectional side view of one embodiment of an aluminum refining cell 1000 for refining aluminum according to some embodiments. The aluminum refining cell 1000 is an exemplary embodiment of a refining cell for the apparatus, systems, and methods described herein.

[0134] FIG. 15B is an enlarged view of a portion of an electrode, for example, anode 1090 and cathode 1150 of FIG. 15A.

[0135] The aluminum refining cell 1000 comprises a cell chamber 1210 having a cell bottom 1060, a heat resistant sidewall 1030, and a heat resistant top cover 1040, at least one anode 1090 extending upwardly from the cell bottom 1060, a cathode connector 1140 disposed proximate the heat resistant top cover 1040, at least one cathode 1150 extending downwardly from the cathode connector 1140, an extraction port 1200 for withdrawing purified aluminum 1120 from the cell chamber 1210, and a cell access channel 1160 comprising an access port 1170 through which aluminum feedstock 1180 can access into the cell chamber 1210. The cell chamber 1210 is at least partially defined by the heat resistant sidewall 1030, the heat resistant top cover 1040, and the cell bottom 1060. The base 1010 is disposed proximate the cell bottom 1060. In some embodiments, the cell chamber 1210 comprises an extraction port 1200 and an access port 1170 in the heat-resistant sidewall 1030 .

[0136] In some embodiments, the aluminum purification cell 1000 includes a cell access channel 1160 that penetrates the cell chamber 1210, thereby providing access to a lower portion of the cell chamber 1210. The cell access channel 1160 can include an access port 1170. Aluminum feedstock 1180 can enter the aluminum purification cell 1000 through the access port 1170.

[0137] In some embodiments, the aluminum purification cell 1000 includes an extraction port 1200 that extends through the heat-resistant sidewall 1030, allowing access to the top of the cell chamber 1210. The refined aluminum 1120 can be extracted from the aluminum purification cell 1000 through the extraction port 1200.

[0138] In some embodiments, the aluminum purification cell 1000 includes an inert gas inlet 1220 formed in the heat resistant top cover 1040. The inert gas inlet 1220 is configured to supply an inert atmosphere to the cell chamber 1210. Examples of inert gases include helium, argon, and nitrogen.

[0139] The cell bottom 1060 comprises an upper surface 1080 and a lower surface 1070. In some embodiments, the cell bottom 1060 is flat. In some embodiments, the cell bottom 1060 slopes downwardly towards the access port 1170. In some embodiments, the slope of the cell bottom 1060 has an angle of less than 10 degrees. In some embodiments, the slope of the cell bottom 1060 has an angle of between 3 and 5 degrees.

[0140] The aluminum purification cell 1000 includes a cathode connector 1140 adjacent the heat resistant top cover 1040. The cathode connector 1140 includes an upper connecting rod 1130 configured to connect to an external power source. The cathode connector 1140 includes a lower surface 1142 and an upper surface 1144. Opposite the cathode connector 1140, the aluminum purification cell 1000 includes an anode connector 1050 that electrically connects to the cell bottom 1060. The anode connector 1050 is configured to connect to an external power source.

[0141] The anode 1090 and the cathode 1150 are electrodes. In some embodiments, some of the electrodes are made of the same material and some are made of different materials. In some embodiments, all of the electrodes are made of different materials. In some embodiments, all of the electrodes are made of the same material. In some embodiments, some of the electrodes are made of a carbonaceous material and some of the electrodes are made of a non-carbonaceous material.

[0142] The electrodes (i.e., the anode 1090 and the cathode 1150) can be made of an aluminum wettable material. In some embodiments, the electrodes are made of TiB 2 , ZrB 2 , HfB 2 , SrB 2 , a carbonaceous material (e.g., graphite), tungsten (W), molybdenum (Mo), steel, or a combination thereof. In some embodiments, the electrode is made of a non-carbonaceous material. In some embodiments, the electrode is made of a cermet or ceramic. In some embodiments, the electrode is ceramic. In some embodiments, the electrode is made of titanium. In some embodiments, the electrode is made of TiB 2 In some embodiments, the electrode comprises TiB 2 In some embodiments, the electrode is made of multiple layers.

[0143] The anode 1090 is disposed on the cell bottom 1060 of the aluminum refining cell 1000. The anode 1090 has a proximal end 1094 that connects to the top surface 1080 of the cell bottom 1060. The anode 1090 has a distal end 1092 that extends upwardly toward the heat resistant top cover 1040 of the aluminum refining cell 1000. The anode 1090 has an intermediate portion between the distal end 1092 and the proximal end 1094. In some embodiments, the anode 1090 is a vertical anode.

[0144] The cathode 1150 includes a proximal end 1154 that connects to the cathode connector 1140 and a distal end 1152 that extends downward toward the base 1010. The cathode 1150 includes an intermediate portion between the proximal end 1154 and the distal end 1152. In some embodiments, the cathode 1150 is a vertical cathode. The anodes 1090 may be interleaved with the cathodes 1150.

[0145] In some embodiments, the anode 1090 overlaps the cathode 1150, thereby defining an anode-cathode overlap (ACO) 1290. In FIG. 15B, the distal end 1092 of the anode 1090 partially overlaps the distal end 1152 of the cathode 1150. In some embodiments, the distal end 1152 of the cathode 1150 is near the middle of the anode 1090, and the distal end 1092 of the anode 1090 is near the middle of the cathode 1150. In some embodiments, the anode-cathode overlap (ACO) 1290 is between 0 and 50 inches. In some embodiments, the anode-cathode overlap 1290 is between 1 and 50 inches. In some embodiments, the anode-cathode overlap 1290 is between 5 and 50 inches. In some embodiments, the anode-cathode overlap 1290 is between 10 and 50 inches. In some embodiments, the anode-cathode overlap 1290 is between 20 and 50 inches. In some embodiments, the anode-cathode overlap 1290 is between 25 and 50 inches. In some embodiments, the anode-cathode overlap 1290 has at least some overlap, up to 12 inches of overlap. In some embodiments, the anode-cathode overlap 1290 is at least 2 inches of overlap to 10 inches of overlap. In some embodiments, the anode-cathode overlap 1290 is at least 3 inches of overlap to 8 inches of overlap. In some embodiments, the anode-cathode overlap 1290 is at least 3 inches of overlap to 6 inches of overlap.

[0146] The lateral separation between the anode 1090 and the cathode 1150 can be designated as the anode-cathode distance (ACD) 1280. In some embodiments, the anode-cathode distance 1280 can be between 1 / 8 inch and 3 inches. In some embodiments, the anode-cathode distance 1280 can be between 1 / 8 inch and 2 inches. In some embodiments, the anode-cathode distance 1280 can be between 1 / 8 inch and 1 inch. In some embodiments, the anode-cathode distance 1280 can be between 1 / 8 inch and 1 / 4 inch. In some embodiments, the anode-cathode distance 1280 can be between 1 / 4 inch and 1 / 2 inch. In some embodiments, the anode-cathode distance 1280 can be between 1 / 8 inch and 3 / 4 inch. In some embodiments, the anode-cathode distance 1280 can be between 1 / 8 inch and 1 inch. In some embodiments, the anode-cathode distance 1280 may be between 1 / 8 inch and 1 / 2 inch.

[0147] In some embodiments, the aluminum purification cell 1000 comprises an outer shell 1020. The outer shell 1020 may comprise steel or other suitable material. In some embodiments, the outer shell 1020 may comprise a shell floor disposed below the base 1010 (shell floor not shown). In some embodiments, the outer shell 1020 may comprise a shell sidewall spaced apart from and surrounding the heat resistant sidewall 1030.

[0148] In some embodiments, the aluminum purification cell 1000 includes a cell lining to insulate the cell chamber 1210. The cell lining may be disposed between the heat resistant sidewall 1030 and the outer shell 1020, and between the base 1010 and the cell bottom 1060. In some embodiments, the cell lining may seal substantially all of the cell chamber 1210, or only a portion of the cell chamber 1210. The cell lining can facilitate high electrical efficiency of the aluminum purification cell 1000.

[0149] In some embodiments, the cell chamber 1210 includes a molten metal pad 1100, refined aluminum 1120, and an electrolyte 1110. The molten metal pad 1100 is in contact with the cell bottom 1060. The electrolyte 1110 separates the refined aluminum 1120 from the molten metal pad 1100. The anode 1090 extends upward from the cell bottom 1060 through the molten metal pad 1100 and terminates in the electrolyte 1110. The cathode 1150 extends downward from the cathode connector 1140 and terminates in the electrolyte 1110 such that the cathode 1150 overlaps the anode 1090 in the electrolyte 1110. Thus, the cathode 1150 is separated from the anode 1090 by the electrolyte 1110.

[0150] In an exemplary embodiment, the refined aluminum 1120 has a lower density than the electrolyte 1110 of the aluminum refinement cell 1000. The electrolyte 1110 has a lower density than the molten metal pad 1100 of the aluminum refinement cell 1000. The electrolyte 1110 separates a top layer of the refined aluminum 1120 from the molten metal pad 1100. In this regard, the composition of the electrolyte 1110 can be selected such that the electrolyte 1110 has a lower density than the molten metal pad 1100 and a higher density than the refined aluminum 1120. In some embodiments, the electrolyte 1110 includes a molten salt. In some embodiments, the electrolyte 1110 includes at least one of a fluoride and / or a chloride. In some embodiments, the electrolyte 1110 includes at least one of a fluoride and / or a chloride, such as Na, K, Al, Ba, Ca, Ce, La, Cs, Rb, or a combination thereof.

[0151] In some embodiments, the molten metal pad 1100 comprises at least 50% by weight aluminum metal, or at least 55% by weight aluminum metal, or at least 60% by weight aluminum metal, or at least 65% by weight aluminum metal, or at least 70% by weight aluminum metal, or at least 75% by weight aluminum metal, or at least 80% by weight aluminum metal, or at least 85% by weight aluminum metal, or at least 90% by weight aluminum metal, or at least 95% by weight aluminum metal.

[0152] In some embodiments, the molten metal pad 1100 comprises at least one alloy containing one or more of Al, Si, Cu, Fe, Sb, Gd, Cd, Sn, Pb, and impurities. In some embodiments, the composition of the wettable material on the anode 1090 in the aluminum purification cell 1000 is the same as or substantially similar to the molten metal pad 1100 (see section ii for a discussion of wettable materials). In some embodiments, the composition of the wettable material is a metal. In some embodiments, the metal comprises aluminum, or at least aluminum and magnesium. In some embodiments, the metal comprises at least 50 weight percent aluminum, or at least 55 weight percent aluminum, or at least 60 weight percent aluminum, or at least 65 weight percent aluminum, or at least 70 weight percent aluminum, or at least 75 weight percent aluminum, or at least 80 weight percent aluminum, or at least 85 weight percent aluminum, or at least 90 weight percent aluminum, or at least 95 weight percent aluminum. In some embodiments, the metal is selected from the group consisting of aluminum alloys, metallic aluminum, and combinations thereof.

[0153] The aluminum refining cell 1000 comprises a molten metal pad 1100 and an electrolyte 1110. In some embodiments, the step 10100 of providing an aluminum feedstock 1180 includes flowing the aluminum feedstock 1180 through the cell access channel 1160 and into the molten metal pad 1100.

[0154] In some embodiments, impurities of the aluminum feedstock 1180 can include Cr, Cu, Fe, Mg, Mn, Ni, Si, Ti, and Zn. In some embodiments, the aluminum feedstock 1180 can include aluminum with up to 2 wt.% Mg in addition to other impurities.

[0155] In some embodiments, additives (e.g., copper) are added to the aluminum feedstock 1180 to densify and retain the metal of the aluminum feedstock 1180 in the molten metal pad 1100 on the bottom of the aluminum refining cell 1000. In some examples, the aluminum feedstock 1180 includes at least 5% copper by weight, at least 10% copper by weight, at least 15% copper by weight, at least 20% copper by weight, at least 25% copper by weight, at least 30% copper by weight, at least 35% copper by weight, at least 40% copper by weight, at least 45% copper by weight, or at least 50% copper by weight. Thus, the molten metal pad 1100 may include a relatively large amount of copper. In some embodiments, the molten metal pad 1100 includes at least 5% copper by weight, at least 10% copper by weight, at least 15% copper by weight, at least 20% copper by weight, at least 25% copper by weight, at least 30% copper by weight, at least 35% copper by weight, at least 40% copper by weight, or more.

[0156] In some embodiments, the feeding step 10100 includes continuously feeding the aluminum feedstock 1180 during operation of the aluminum purification cell 1000. In some embodiments, the feeding step 10100 includes periodically adding the aluminum feedstock 1180 into the aluminum purification cell 1000. In some embodiments, the feeding step 10100 includes feeding the aluminum feedstock 1180 into the aluminum purification cell 1000 at a first feed rate. The first feed rate may be kept constant or may vary, including stopping and starting the feeding of the aluminum feedstock 1180 to the aluminum purification cell 1000. In some embodiments, the feeding step 10100 includes periodically adding the aluminum feedstock 1180 to the aluminum purification cell 1000.

[0157] As described above, the aluminum feedstock 1180 providing step 10100 can be performed by the aluminum purification cell 1000. In some embodiments, the aluminum feedstock 1180 includes aluminum metal. In some embodiments, the aluminum feedstock 1180 includes at least one metal other than aluminum metal. In some embodiments, the aluminum feedstock 1180 includes a transition metal. In some embodiments, the aluminum feedstock 1180 includes at least 50% aluminum metal by weight. In some embodiments, the aluminum feedstock 1180 includes at least 55% aluminum metal by weight. In some embodiments, the aluminum feedstock 1180 includes at least 60% aluminum metal by weight. In some embodiments, the aluminum feedstock 1180 includes at least 65% aluminum metal by weight. In some embodiments, the aluminum feedstock 1180 includes at least 70% aluminum metal by weight. In some embodiments, the aluminum feedstock 1180 includes at least 75% aluminum metal by weight. In some embodiments, the aluminum feedstock 1180 includes at least 80% aluminum metal by weight. In some embodiments, the aluminum feedstock 1180 includes at least 85% aluminum metal by weight. In some embodiments, aluminum feedstock 1180 comprises at least 90% aluminum metal by weight. In some embodiments, aluminum feedstock 1180 comprises at least 95% aluminum metal by weight.

[0158] In some embodiments, the aluminum feedstock 1180 includes impurities. In some embodiments, the aluminum feedstock 1180 includes impurities between 0.5% and 50.0% by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes impurities between 5.0% and 50.0% by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes impurities between 10.0% and 50.0% by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes impurities between 15.0% and 50.0% by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes impurities between 20.0% and 50.0% by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes impurities between 25.0% and 50.0% by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes 30.0% to 50.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes 35.0% to 50.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes 40.0% to 50.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes 45.0% to 50.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes 0.5% to 45.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes 0.5% to 40.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes 0.5% to 35.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes between 0.5% and 30.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes between 0.5% and 25.0% impurities by weight of the aluminum feedstock 1180.In some embodiments, the aluminum feedstock 1180 includes between 0.5% and 20.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes between 0.5% and 15.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes between 0.5% and 10.0% impurities by weight of the aluminum feedstock 1180. In some embodiments, the aluminum feedstock 1180 includes between 0.5% and 5.0% impurities by weight of the aluminum feedstock 1180.

[0159] In some embodiments, the aluminum feedstock 1180 is aluminum alloy scrap. In some embodiments, the aluminum alloy scrap includes at least one of a 1xxx series aluminum alloy, a 2xxx series aluminum alloy, a 3xxx series aluminum alloy, a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, a 6xxx series aluminum alloy, a 7xxx series aluminum alloy, an 8xxx series aluminum alloy, or any combination thereof.

[0160] In some embodiments, the ion generating step 10440 includes generating aluminum ions in the electrolyte 1110 and reducing at least a portion of the aluminum ions at or near at least one cathode 1150 of the aluminum purification cell 1000. In some embodiments, the ion generating step 10440 includes migrating the aluminum ions through the electrolyte 1110 toward the cathode 1150.

[0161] The disclosed method includes producing refined aluminum 1120 from aluminum feedstock 1180 by passing an electric current through the anode 190 and through the electrolyte 1110 to the cathode 1150. In some embodiments, the current passing step 10420 includes passing a direct current from the anode 1090 through the electrolyte 1110 to the cathode 1150. In the production step 10300, the anode 1090 and the cathode 1150 can be partially disposed in the electrolyte 1110, and the anode 1090 can be partially disposed in the molten metal pad 1100. Directing the aluminum metal of the molten metal pad 1100 toward the electrolyte 1110 (e.g., directing step 10200) can include flowing the aluminum metal toward the electrolyte 1110 and providing an electric current to the anode 1090 (e.g., current passing step 10420).

[0162] In some embodiments, the method may include transferring at least a portion of the top layer of the refined aluminum 1120 from the aluminum purification cell 1000 through the extraction port 1200. In some embodiments, the refined aluminum 1120 may be transferred substantially continuously during operation of the aluminum purification cell 1000. In some embodiments, the first transfer rate may be controlled, for example, based at least in part on the second transfer rate. In some embodiments, the refined aluminum 1120 may be transferred periodically during operation of the aluminum purification cell 1000. In some embodiments, the transferring step may be performed using equipment (e.g., alumina, graphite, and / or TiB) configured to transfer the refined aluminum 1120 product without contaminating the product. 2 This is completed using a tapping device.

[0163] The refined aluminum 1120 product above the electrolyte 1110 defines a top layer. In some embodiments, the refined aluminum 1120 product comprises an aluminum purity of at least 99.5% by weight. In some embodiments, the refined aluminum 1120 product comprises an aluminum purity of at least 99.5% by weight and up to 99.999% by weight. In some embodiments, the refined aluminum 1120 product comprises an aluminum purity of at least 99.8% by weight and up to 99.999% by weight. In some embodiments, the refined aluminum 1120 product comprises an aluminum purity of at least 99.9% by weight and up to 99.999% by weight. In some embodiments, the refined aluminum 1120 product comprises an aluminum purity of at least 99.9% by weight and up to 99.999% by weight. For example, the refined aluminum 1120 product can have at least 99.5% by weight aluminum, or at least 99.75% by weight aluminum, or at least 99.8% by weight aluminum, or at least 99.85% by weight aluminum, or at least 99.9% by weight aluminum, or at least 99.95% by weight aluminum.

[0164] In some embodiments, the purified aluminum 1120 product can be produced by the aluminum purification cell 1000 at an energy efficiency of 1-15 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 120 product can be produced by the aluminum purification cell 1000 at an energy efficiency of 1-10 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 1120 product can be produced by the aluminum purification cell 1000 at an energy efficiency of 1-8 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 1120 product can be produced by the aluminum purification cell 1000 at an energy efficiency of 1-6 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 1120 product can be produced by the aluminum purification cell 1000 at an energy efficiency of 1-4 kWh / kg of purified aluminum. In some embodiments, the purified aluminum 1120 product can be produced by the aluminum purification cell 1000 at an energy efficiency of 5-15 kWh / kg of purified aluminum. In some embodiments, the refined aluminum 1120 product can be produced by the aluminum purification cell 1000 at an energy efficiency of 10-15 kWh / kg of refined aluminum. In some embodiments, the refined aluminum 1120 product can be produced by the aluminum purification cell 1000 at an energy efficiency of 12-15 kWh / kg of refined aluminum.

[0165] In some embodiments, the sludge 1190 may be produced, at least in part, by the current application process 10420. The sludge 1190 may have a higher density than the molten metal pad 1100. As described above, the top surface 1080 of the cell bottom 1060 may be sloped. In some embodiments, the slope may extend downward from the refractory sidewall 1030 toward the cell access channel 1160. Thus, the sludge 1190 may be drained along the top surface 1080 toward the cell access channel 1160. In some embodiments, the sludge 1190 may be removed from the cell chamber 1210 through the cell access channel 1160. In some embodiments, impurities may tend to collect in the molten metal pad 1100. Thus, the cell access channel 1160 may facilitate removal of at least a portion of the molten metal pad 1100.

[0166] ii. Substrate with induction mechanism As explained above, the present disclosure relates to an aluminum refining cell having a substrate with one or more induction features, such substrates being described below in this section.

[0167] The present disclosure relates to titanium diboride (TiB 2 ) substrate, or using an induction mechanism to 2 In some embodiments, the TiB 2 The substrate structure is TiB 2 It can be covered with solid aluminum metal before contacting the wettable material. 2 Wettability material is TiB 2 When in contact with the substrate, the induction mechanism is TiB 2 The guiding features guide the wettable material in a predetermined direction. The guiding features can take many shapes and sizes. In some embodiments, the guiding features can be slots, grooves, pores, or combinations thereof. The TiB having at least one guiding feature 2The substrate can be used in a variety of applications, including the movement of fluids within an article. In some embodiments, TiB 2 The wettable material is TiB 2 It may be any metal suitable for transport through the substrate. In some embodiments, TiB 2 The wettable material is aluminum, for example, aluminum alloys, aluminum metal, and combinations thereof.

[0168] In one aspect, the present disclosure provides a TiB having an induction mechanism. 2 The article includes a substrate, and the induction mechanism is TiB 2 The TiB 2 The wettable material includes aluminum. In some embodiments, the aluminum is selected from the group consisting of an aluminum alloy, metallic aluminum, and combinations thereof. In some embodiments, TiB 2 The surface of the substrate is at least partially covered with solid aluminum metal. In some embodiments, the inducing mechanism is a structure, e.g., TiB 2 In some embodiments, the TiB 2 The substrate has a three-dimensional geometric shape. In some embodiments, the three-dimensional geometric shape has at least one of the following three-dimensional features: a rectangular shape, a square shape, a triangular shape, an elliptical shape, or an oblong shape. In some embodiments, the TiB 2 The substrate has an asymmetric shape. In some embodiments, the TiB 2 The substrate is in the form of a plate.

[0169] In some embodiments, TiB 2 The substrate is configured for use in an aluminum refining cell. In some embodiments, the induction mechanism is to induce TiB 2 In some embodiments, the inducing features include pores. In some embodiments, the inducing features include TiB 2The porosity of the substrate is included. In some embodiments, the porosity ranges from about 1 to about 200 pores per inch (PPI). In some embodiments, the porosity is at least about 5 pores per inch (PPI), or at least about 10 pores per inch (PPI), or at least about 15 pores per inch (PPI), or at least about 20 pores per inch (PPI). In some embodiments, the porosity is about 175 pores per inch (PPI) or less, or about 150 pores per inch (PPI) or less, or about 125 pores per inch (PPI) or less, or about 100 pores per inch (PPI) or less, or about 80 pores per inch (PPI) or less, or about 60 pores per inch (PPI) or less, or about 50 pores per inch (PPI) or less.

[0170] In some embodiments, the guidance mechanism comprises a structure having at least one groove. In some embodiments, the at least one groove comprises a TiB 2 The at least one groove extends partially into the substrate. In some embodiments, the dimensions of the at least one groove are predetermined. In some embodiments, the size and / or shape of the at least one groove are predetermined. In some embodiments, the width (w) of the at least one groove is in the range of about 10 μm to about 20 mm. In some embodiments, the groove depth (gd) of the at least one groove is in the range of about 1 mm to about 10 mm. In some embodiments, the length (l) of the at least one groove is in the range of about 1 cm to about 1 m. In some embodiments, the TiB 2 The thickness (t) of the substrate ranges from about 5 mm to about 30 mm. In some embodiments, the induction mechanism is TiB 2 The substrate comprises at least two grooves, hi some embodiments, the edge-to-edge distance (d) between the at least two grooves is in the range of about 1 mm to about 20 mm.

[0171] In another aspect, the present disclosure provides a TiB2 having (a) at least one induction mechanism. 2 (b) the substrate and (b) TiB 2and solid aluminum metal at least partially covering a surface of the substrate. In some embodiments, the solid aluminum metal is at least partially contained within at least one induction feature. In some embodiments, TiB 2 The substrate comprises a structure having a surface region, a first portion of the surface region comprising at least one induction feature and a second portion of the surface region free of any induction features. In some embodiments, the first portion of the surface region is at least partially covered by solid aluminum metal. In some embodiments, the first portion of the surface region is at least 1% covered by solid aluminum metal. In some embodiments, the second portion of the surface region is at least partially covered by solid aluminum metal. In some embodiments, the second portion of the surface region is at least 1% covered by solid aluminum metal. In some embodiments, the solid aluminum metal covering the second portion of the surface region is in the form of a film. In some embodiments, the film comprises a thickness of 1 μm to 500 μm. In some embodiments, the second portion of the surface region is free of solid aluminum metal.

[0172] In some embodiments, the at least one guiding feature comprises a void volume, and at least 1% of the void volume comprises solid aluminum metal. In some embodiments, the at least one guiding feature is a structure having a slot, and the solid aluminum metal is at least partially within the slot. In some embodiments, the at least one slot comprises a slot volume, and the solid aluminum metal occupies at least 1% of the slot volume. In some embodiments, the at least one guiding feature is a groove, and the solid aluminum metal is at least partially within the groove. In some embodiments, the at least one groove comprises a groove volume, and the solid aluminum metal occupies at least 1% of the groove volume.

[0173] In another aspect, the present disclosure provides a method for producing a TiB 2 Web of Science and Technology, and (b) TiB 2and solid aluminum metal at least partially covering a surface of the web of TiB. 2 The web is TiB 2 In some embodiments, the solid aluminum metal comprises the voids. In some embodiments, the TiB 2 The web voids are TiB 2 wherein the solid aluminum metal occupies at least 1% of the pore volume.

[0174] In another aspect, the present disclosure provides a TiB having at least one induction mechanism. 2 A product is manufactured, and TiB is guided in a predetermined direction by at least one guidance mechanism. 2 In some embodiments, the method includes forming a TiB2 layer having a plurality of pores. 2 In some embodiments, the manufacturing process includes forming a geometric feature. In some embodiments, the manufacturing process includes forming a TiB 2 Product or TiB 2 In some embodiments, the manufacturing process includes machining the product precursor to form at least one inducing feature. 2 The raw material is TiB 2 and extruding the TiB 2 The product precursor comprises at least one induction mechanism. In some embodiments, TiB 2 The product precursor is unsintered TiB 2 In some embodiments, the method includes preparing an unsintered TiB 2 The material is exposed to high temperatures, which causes TiB 2 In some embodiments, the substrate is formed of TiB 2 The at least one guide feature in the substrate may comprise a groove, a slot, a channel, or a combination thereof.

[0175] In another aspect, the present disclosure provides a TiB 2In some embodiments, the aluminum refining cell includes a TiB 2 At least one of the substrates is an electrode. In some embodiments, TiB 2 At least one of the substrates is an induction device configured to induce liquid aluminum metal (eg, molten aluminum metal) in a predetermined direction when no electrical current is applied thereto.

[0176] As used herein, a "slot" is a TiB 2 It means a geometric feature that penetrates the thickness of a substrate.

[0177] As used herein, a "groove" refers to a TiB 2 It means a geometric feature that extends partially through, but not completely through, the thickness of a substrate.

[0178] As used herein, "geometric features" refers to TiB 2 It means a predetermined shape formed in a substrate. Examples include slots and grooves of any shape or size.

[0179] As used herein, "TiB 2 The wettable material is TiB 2 This means that the contact angle with the surface is 90 degrees or less.

[0180] As used herein, "TiB 2 "Substrate" refers to TiB2 that can be equipped with at least one induction mechanism. 2 This refers to a substrate made of TiB 2 An example of a substrate is TiB 2 In one embodiment, TiB 2 The base material is TiB 2 It essentially consists of:

[0181] As used herein, "aluminum-coated TiB 2The "substrate" is a TiB2 substrate at least partially coated with aluminum metal. 2 By substrate, the aluminum metal is meant aluminum metal and / or an aluminum alloy. In one embodiment, the aluminum metal is TiB 2 At least partially contained within at least one inductive feature of the substrate. In one embodiment, the aluminum metal is TiB 2 At least partially covering the outer surface of the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 5% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 10% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 15% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 20% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 25% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 30% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 35% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 40% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 45% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 50% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 55% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 60% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 65% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 70% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2Covers at least 75% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 80% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 85% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 90% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 91% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 92% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 93% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 94% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 95% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 96% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 97% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 98% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 99% of the surface area of ​​the substrate. In one embodiment, the aluminum metal is TiB 2 Covers at least 100% of the surface area of ​​the substrate.

[0182] As used herein, "plating material" and the like means a film, coating, or other thin film in contact with at least a portion of an exterior surface of a substrate, regardless of how the plating material is produced on the substrate; i.e., plating includes all methods of applying a film, coating, or thin film to a substrate.

[0183] Figure 1A shows TiB 21 illustrates one embodiment of a method 100 for directing a wettable material in a predetermined direction using a directing mechanism. Step 102 is an optional step illustrated in FIG. 1A by a dashed box. Step 102 includes: 2 The substrate is coated with solid aluminum metal. 2 The substrate may be covered with solid aluminum metal. In some embodiments, TiB 2 The entire substrate can be covered. 2 Part of the substrate can be covered with solid aluminum metal, but TiB 2 The rest of the substrate is free of solid aluminum. The coverage of solid aluminum metal is 2 It depends on the application of the substrate. 2 The substrate is TiB 2 Step 106 includes contacting the TiB 2 This involves directing the wettable material in a desired direction.

[0184] Figure 1B shows TiB 2 1 illustrates another embodiment of a method 110 for directing a wettable material in a predetermined direction using a directing mechanism. A manufacturing process 112 includes forming a TiB 2 The manufacturing process 112 includes manufacturing a TiB2 having a plurality of pores. 2 The manufacturing process 112 may include forming a product structure. The manufacturing process 112 may include forming a geometric feature. The manufacturing process 112 may include forming a TiB 2 Product or TiB 2 The method can include machining the product precursor structure to form at least one guide feature. The guide features in or on the product or product precursor structure can be slots, grooves, pores, and combinations thereof. The guide features can include void volume. In some embodiments, at least 1% of the void volume includes solid aluminum metal. The guide features can be formed by capillary action to form TiB 2 Wettability of the material can be induced.

[0185] Manufacturing process 112 is TiB2 The raw material is TiB 2 and extruding the TiB 2 The product precursor comprises at least one induction mechanism. In some embodiments, TiB 2 The product precursor is unsintered TiB 2 The manufacturing process 112 is unsintered TiB 2 The material is exposed to high temperatures, which causes TiB 2 The inducing step 114 may include forming a substrate using TiB 2 The method includes directing the wettable material in a predetermined direction by at least one directing mechanism.

[0186] FIG. 2A is a perspective view of one embodiment of a product 200. 2 The substrate 202 has a number of slots 206 as a guide mechanism. The slots 206 are defined between the protrusions 204. 2 The substrate 202 also includes a base portion 208 and a tip portion 210. The slot 206 is 2 The TiB is configured to direct the wettable material in a predetermined direction. 2 The wettable material can include aluminum, for example, aluminum alloys, aluminum metal, and combinations thereof.

[0187] Figure 2B is a first side view of the embodiment shown in Figure 2A. Figure 2B shows a side view of product 200 showing protrusion 204. Protrusion 204 has a length (l) that extends from the top of base 208 to the end of tip 210. Tip 210 can have any of a variety of shapes, including a pointed shape, a rounded curve, or a jagged edge, etc.

[0188] Figure 2C is an enlarged partial cross-sectional view of the embodiment shown in Figure 2A, indicated by the dashed circle in Figure 2A. The partial top view shows only two of the protrusions 204. Namely, Figure 2C shows a first protrusion 204A and a second protrusion 204B, which define a first slot 206A. The first slot 206A is defined by an inner surface of the first protrusion 204A and an inner surface of the second protrusion 204B.

[0189] FIG. 3A is a front view of one embodiment of a product 300. 2 The substrate 302 has a slot 306 as a guide mechanism. The slot 306 is defined by a first protrusion 304A and a second protrusion 304B (collectively, protrusions 304). 2 The substrate 302 also includes a base portion 308 and a tip portion 310. The slot 306 is 2 The width (w) of one of the protrusions is also shown, the width being configured to direct the wettable material in a predetermined direction.

[0190] Figure 3B is a cross-sectional view of a section taken along dashed line 3B shown in Figure 3A. Figure 3B shows the thickness (t) of the protrusion 304 and the distance (d) that the slot 306 extends between the inner surface of the first protrusion 304A and the inner surface of the second protrusion 304B. Figure 3C is a first side view of the embodiment (e.g., product 300) shown in Figure 3A. Figure 3C shows the length (l) of the protrusion 304.

[0191] Figures 2A-2C and 3A-3C are similar and will be described together. The embodiment of Figures 2A-2C differs from the embodiment of Figures 3A-3C in the number of protrusions 204 / 304, the number of slots 206 / 306, and the thickness (t) of the protrusions 204 / 304.

[0192] The dimensions of the slot 206 / 306 are pre-determined. In some embodiments, the slot 206A / 306 extends the entire length (l) of the first protrusion 206A / 306A and the entire length (l) of the second protrusion 206B / 306B. The entire length (l) of the first protrusion 206A / 306A and the entire length (l) of the second protrusion 204B / 304B can range from about 0.01 meters to about 1 meter. The thickness (t) of the first protrusion 204A / 304A and the thickness (t) of the second protrusion 204B / 304B can range from about 1 mm to about 20 mm. The slot 206A / 306 extends a distance (d) between the inner surface of the first protrusion 204A / 304A and the inner surface of the second protrusion 204B / 304B. In some embodiments, the distance (d) ranges from about 20 μm to about 20 mm. The width (w) of the protrusions 204 / 304 (eg, the first protrusions 204A / 304A and the second protrusions 204B / 304B) can range from about 1 mm to about 20 mm.

[0193] The protrusions 204 / 304 can differ from one another in dimensions. The protrusions 204 / 304 can differ from one another in length (l), thickness (t), and width (w). Similarly, the distance (d) of the slots 206 / 306 can differ from one another. In some embodiments, the first protrusion 204A / 304A can have a longer length (l) and a wider width (w) and a thinner thickness (t) compared to the second protrusion 204B / 304B.

[0194] Slot 206 / 306 is TiB 2 The slots extend through the thickness of the substrate 202 / 302. The number of slots may vary. In some embodiments, there may be one slot, as shown in the examples of Figures 3A, 3B, and 3C. There may also be two or more slots. The number of slots is determined by the TiB 2 This may vary depending on the intended use of the substrate 202 / 302. In the example shown in Figures 2A, 2B, and 2C, there are six slots.

[0195] TiB 2The substrate 202 / 302 may be at least partially covered with solid aluminum metal. The slot 206 / 306 may be filled with TiB 2 The guiding features of the substrate 202 / 302. Other guiding features, such as grooves, pores, and combinations thereof, may be used in the TiB 2 A substrate 202 may be provided.

[0196] TiB 2 The substrate 202 / 302 can have any suitable configuration, size, or shape depending on the application. 2 The substrate 202 / 302 can have a three-dimensional geometric shape. The geometric shape surface can include at least one of a rectangular shape, a square shape, a triangular shape, an elliptical shape, or an oblong shape surface, etc. 2 The substrate 202 / 302 may also have an asymmetric shape. 2 The substrate 202 / 302 may also be plate-shaped. 2 The substrate 202 / 302 is adapted to guide the TiB2 through capillary action using the slot 206 / 306 as a guide mechanism. 2 Wettability of the material can be induced.

[0197] TiB 2 The substrate 202 / 302 can be used in a variety of applications. In some embodiments, TiB 2 The substrate 202 / 302 can be configured for use in an aluminum refining cell where a cathode is at the top of the cell, an anode is at the bottom of the cell, and refined aluminum migrates to the top of the cell. An example of an aluminum refining cell is described in commonly owned U.S. Patent No. 10,407,786, filed February 11, 2016, entitled "Systems and Methods for Purifying Aluminum."

[0198] FIG. 4A is a front view of one embodiment of a product 400. 2The substrate 402 has a plurality of grooves 406 as a guiding feature. Figure 4B is a first side view of the embodiment shown in Figure 4A. Figure 4C is an enlarged partial cross-sectional view of the embodiment shown in Figure 4A, indicated by the dashed circle in Figure 4A. Figure 4D is another configuration of the plurality of grooves of the embodiment shown in Figure 4C.

[0199] Product 400 is similar to products 200 / 300. The differences will now be described. In some embodiments, the guiding feature of product 200 / 300 is a slot 206 / 306, in contrast to the guiding feature of product 400 being at least one groove 406.

[0200] Groove 406 is TiB 2 The groove 406 extends partially into the substrate 402. The dimensions of the groove 406 are pre-determined. In some embodiments, the size and / or shape of the groove 406 is pre-determined. The width (w) of the groove 406 ranges from about 10 μm to about 20 mm. The groove depth (gd) of the groove 406 ranges from about 1 mm to about 10 mm. The length (l) of the groove 406 ranges from about 1 cm to about 1 m. 2 The thickness (t) of the substrate 402 ranges from about 5 mm to about 30 mm. The edge-to-edge distance (d) between the grooves 406 ranges from about 1 mm to about 20 mm.

[0201] As shown in Figure 4C, the induction mechanism is TiB 2 The substrate 402 includes at least two grooves 406. Specifically, the guiding mechanism includes three grooves 406. Figure 4C shows a first groove 406A, a second groove 406B, and a third groove 406C (collectively, grooves 406).

[0202] The grooves 406 can be arranged in any pattern. The grooves 406 can also have the same dimensions as one another or different dimensions from one another. The grooves 406 can also be arranged on the front and back surfaces as shown in FIG. 4C, as well as on the TiB 2The grooves 406 may also be disposed on the side of the substrate 402. FIG. 4D shows a first groove 406A', a second groove 406B', and a third groove 406C' (collectively, grooves 406'). FIG. 4D shows grooves 406' of different dimensions and arrangement compared to groove 406 in FIG. 4C. FIG. 4C shows grooves 406 having the same dimensions as each other, but with TiB 2 FIG. 4D illustrates that the grooves 406′ can have different dimensions. In some embodiments, the second groove 406B′ has a groove depth of TiB 2 It is the largest groove, extending more than halfway through the substrate 402. The third groove 406C' is the smallest groove and is 2 It extends less than halfway through the substrate 402'.

[0203] FIG. 5A is a side view of another embodiment of a product 500. 2 The substrate 502 has a plurality of pores as guide features. Figure 5B is an enlarged view of a portion of the embodiment shown in Figure 5A, which is indicated by the dashed lines in Figure 5A. As shown in Figure 5A, TiB 2 The base material is TiB 2 The pores 504 are TiB 2 Base material 502, TiB 2 The guide mechanism of the product 500 is defined by a web of TiB 2 It may be a void in the substrate 502. 2 The porosity of the substrate 502 can range from about 1 pore to about 200 pores per square inch (PPI). In some embodiments, the porosity is at least about 5 pores per square inch (PPI), or at least about 10 pores per square inch (PPI), or at least about 15 pores per square inch (PPI), or at least about 20 pores per square inch (PPI). In some embodiments, the porosity is about 175 pores per square inch (PPI) or less, or about 150 pores per square inch (PPI) or less, or about 125 pores per square inch (PPI) or less, or about 100 pores per square inch (PPI) or less, or about 80 pores per square inch (PPI) or less, or about 60 pores per square inch (PPI) or less, or about 50 pores per square inch (PPI) or less.

[0204] TiB 2 The porosity of the substrate 502 can have any suitable porous structure. 2 The voids in the substrate 502 may be an interconnected porous structure, with at least a portion of the pores in fluid communication with one another to facilitate the movement of the wettable material from a first location to a second location (e.g., from a first predetermined location to a second predetermined location). Thus, the interconnected porous structure may be considered an open pore structure. In some embodiments, TiB 2 The voids in the substrate 502 provide a random porous structure. 2 The porosity of the substrate 502 may result in an oriented porous structure. In some embodiments, TiB 2 The pores in the oriented porous structure of the substrate 502 may have a porosity gradient. 2 The porosity gradient of the oriented porous structure of the substrate 502 can vary along a three-dimensional gradient (i.e., the porosity gradient can vary along a three-dimensional gradient). 2 (The thickness of the TiB 2 The porosity gradient of the oriented porous structure of the substrate 502 is 2 In some embodiments, the TiB 2 The porosity gradient of the oriented porous structure of the substrate 502 is 2 The TiB 2 The porosity gradient of the oriented porous structure of the substrate 502 is 2 From one end of the substrate 502, TiB 2 It may increase, decrease, and then increase to the other end of the substrate 502 .

[0205] FIG. 6A is a perspective view of one embodiment of a product 600. 2 The substrate 602 has a number of slots 606 as a guide mechanism, and the solid aluminum metal 612 is TiB 26A , a portion of solid aluminum metal 612 is shown peripherally or transparently to reveal the surface structure of substrate 602. Product 600 includes protrusions 604, base 608, and tip 610. FIG. 6B is a first side view of a cross section taken along arrow 6B shown in FIG. 6A . FIG. 6C is an enlarged partial cross-sectional view of the embodiment shown in FIG. 6A , indicated by the dashed circle in FIG. 6A . The embodiments shown in FIGS. 2A , 2B, and 2C are the same as or similar to the embodiments of FIGS. 6A , 6B, and 6C , except for the differences described herein. In some embodiments, the structures shown in FIGS. 6A , 6B, and 6C may be formed by forming TiB 612 on the TiB 612 shown in FIGS. 2A , 2B, and 2C . 2 Substrate structure (e.g., TiB 2 2A, 2B, and 2C. Similar features of FIGS. 6A, 6B, and 6C to those of FIGS. 2A, 2B, and 2C will not be repeated. FIGS. 6A and 6B show the TiB 2 Solid aluminum metal 612 is shown completely covering substrate 602. Figure 6C shows solid aluminum metal 612 completely occupying slot 606A between first protrusion 604A and second protrusion 604B.

[0206] In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 at least partially covers the surface of the substrate 602 and / or is at least partially within the slots 606. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 1% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 5% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 10% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 15% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2The solid aluminum metal 612 covers at least 20% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 25% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 30% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 35% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 40% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 45% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 50% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 55% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 60% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 65% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 70% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 75% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 80% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 85% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 The solid aluminum metal 612 covers at least 90% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2The solid aluminum metal 612 covers at least 95% of the surface of the substrate 602. In some embodiments, the solid aluminum metal 612 is TiB 2 It covers at least 100% of the surface of the substrate 602 .

[0207] In some embodiments, the solid aluminum metal 612 is at least partially within the slot 606. In some embodiments, if the slot 606 has a slot volume, the solid aluminum metal 612 occupies at least 1% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 5% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 10% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 15% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 20% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 25% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 30% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 35% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 40% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 45% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 50% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 55% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 60% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 65% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 70% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 75% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 80% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 85% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 90% of the slot volume.In some embodiments, the solid aluminum metal 612 occupies at least 95% of the slot volume. In some embodiments, the solid aluminum metal 612 occupies at least 100% of the slot volume.

[0208] In the embodiments shown in FIGS. 6A-6N, various amounts of solid aluminum metal 612 are inserted into the slots 606 and TiB 2 Occupying a substrate 602 .

[0209] FIG. 6D is a cross-sectional side view of one embodiment of a product 600′. 2 The substrate 602' has a number of slots 606A' as a guide mechanism, and the solid aluminum metal 612' is TiB 2 6E is a partial cross-sectional view taken along dashed line 6E shown in FIG. 6D, where only one of the slots 606A' is shown. The cross-section shows the TiB 2 6A is a partial cross-sectional view taken along dashed line 6F shown in FIG. 6D, where only one slot 606A' of the plurality of slots 606A' is shown in FIG. 6F. The cross-section shows the TiB 2 Along the bottom of the substrate 602'.

[0210] FIG. 6G illustrates a TiB having multiple slots 606A′ as a guidance mechanism. 2 Substrate 602'' and TiB 2 FIG. 6H is a cross-sectional side view of an embodiment with solid aluminum metal 612'' covering one half, or front, of substrate 602''. Solid aluminum metal 612'' covers the front half of base 608'' and tip 610''. FIG. 6H is a partial cross-sectional view taken along dashed line 6H shown in FIG. 6G, where only one slot 606A'' of multiple slots 606A'' is shown. Solid aluminum metal 612'' covers the front half of slot 606A''.

[0211] FIG. 6I illustrates a TiB having a base 608''' and a tip 610''' with multiple slots 606A''' as a guidance mechanism, and solid aluminum metal 612'''' in the multiple slots 606A'''. 2 FIG. 6J is a side view of an embodiment of a substrate 602'''. FIG. 6J is a partial cross-sectional view taken along dashed line 6J shown in FIG. 6I, where only one slot 606A''' of the plurality of slots 606A'' is shown. In the embodiments of FIGS. 6I and 6J, the TiB 2 There is no solid aluminum metal 612''' on the outer surface of substrate 602'''. Solid aluminum metal 612''' completely fills the slot volume of slot 606A''''.

[0212] FIG. 6K is a front view of one embodiment of the TiB 2 A substrate 602'''' has multiple slots 606A, 606B, 606B (collectively, slots 606'''') as a guide mechanism, with solid aluminum metal 612'''' covering some or none of the slots 606. FIG. 6L is a first side view of the embodiment shown in FIG. 6K. FIG. 6K shows a TiB having a base 608'''' and a tip 610''''. 2 Substrate 602'''' is shown. Slots 606'''' have various lengths, thicknesses, and amounts of solid aluminum metal 612''''.

[0213] For slot 606A, the slot length is TiB 2 6A. The top of slot 606A does not include solid aluminum metal 612''''. The bottom of slot 606A includes solid aluminum metal 612''''. For slot 606B, the slot length extends from the top of base 608'''' to tip 610''''. Slot 606B does not include solid aluminum metal 612''''. Slot 606C does not start in the same location as slots 606A and 606B. The beginning of slot 606C begins at the TiB 2Starting further up the substrate 602'''', the slot 606C has solid aluminum metal 612'''' on the bottom and top, but not in the center of the slot 606C.

[0214] Figure 6M shows TiB 2 FIG. 6N is a front view of an embodiment of a substrate 602''''', where surface region 620''''' has a first portion 622'''''' of surface region 620'''''' having a plurality of slots 606'''''' as guiding features and a second portion 624'''''' of surface region 620'''''' without any guiding features. Protrusions 604'''''' define a plurality of slots 606''''''. FIG. 6N is a first side view of the embodiment shown in FIG. 6M, where second portion 624'''''' of surface region 620'''''' is without any guiding features.

[0215] TiB 2 Substrate 602''''' has a surface region 620'''''', a first portion 622'''''' of surface region 620''''' has at least one guiding feature and a second portion 624'''''' of surface region 620''''' is devoid of any guiding feature.

[0216] In some embodiments, first portion 622''''' of surface region 620'''''' is at least partially covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 1% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 5% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 10% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 15% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 20% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 25% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 30% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 35% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 40% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 45% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 50% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 55% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 60% covered by solid aluminum metal.In some embodiments, first portion 622''''' of surface region 620'''''' is at least 65% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 70% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 75% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 80% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 85% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 90% covered by solid aluminum metal. In some embodiments, first portion 622''''' of surface region 620'''''' is at least 95% covered by solid aluminum metal. In some embodiments, the first portion 622'''''' of the surface area 620'''''' is at least 100% covered by solid aluminum metal.

[0217] In some embodiments, second portion 624''''' of surface region 620'''' is at least partially covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 1% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 5% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 10% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 15% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 20% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 25% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 30% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 35% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 40% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 45% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 50% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 55% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 60% covered by solid aluminum metal.In some embodiments, second portion 624''''' of surface region 620'''' is at least 65% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 70% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 75% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 80% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 85% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 90% covered by solid aluminum metal. In some embodiments, second portion 624''''' of surface region 620'''' is at least 95% covered by solid aluminum metal. In some embodiments, the second portion 624'''''' of the surface area 620'''' is at least 100% covered by solid aluminum metal.

[0218] In some embodiments, the solid aluminum metal covering first portion 622'''''' and / or second portion 624'''''' of surface region 620'''''' is in the form of a film. In some embodiments, the film has a thickness between 1 μm and 500 μm. In some embodiments, first portion 622'''''' and / or second portion 624'''''' of surface region 620'''''' is free of solid aluminum metal.

[0219] FIG. 7A is a front view of one embodiment of a product 700. 2 The substrate 702 has slots 706 as a guide mechanism, and the solid aluminum metal 712 is TiB 27A , a portion of solid aluminum metal 712 is shown peripherally or transparently to reveal the surface structure of substrate 702. First protrusion 704A and second protrusion 704B define a slot 706 that extends upwardly from base 708. FIG. 7B is a cross section taken along dashed line 7B shown in FIG. 7A. FIG. 7C is a first side view of the cross section taken along dashed line 7C shown in FIG. 7A.

[0220] FIG. 7D is a front view of one embodiment of a product 700′. 2 The substrate 702' has a slot 706' as a guide feature, with solid aluminum metal 712' covering a portion of the slot 706'. A first protrusion 704A' and a second protrusion 704B' extend upwardly from a base 708', thereby defining a slot 706'. FIG. 7E is a cross-section taken along dashed line 7E shown in FIG. 7D. As shown in FIG. 7E, a middle portion 714' of the slot 706' is free of solid aluminum metal 712'. The front and back of the slot 706' are shown as having solid aluminum metal 712'. FIG. 7F is a first side view of the embodiment shown in FIG. 7D.

[0221] The embodiments shown in Figures 7D, 7E, and 7F and the embodiments shown in Figures 7A, 7B, and 7C are the same or similar, except for the differences described herein. 2 The amount of solid aluminum metal 712 / 712' covering the substrate 702 / 702' varies depending on the embodiment. In the embodiments of FIGS. 7A, 7B, and 7C, the solid aluminum metal 712 is TiB 2 7D, 7E, and 7F show a TiB 2 There is no solid aluminum metal 712' on the outside of the substrate 702'. Only a portion of the slot 706' is filled with solid aluminum metal 712'.

[0222] Figures 7A, 7B, 7C, 7D, 7E, and 7F are the same as or similar to the embodiments of Figures 3A, 3B, and 3C. One difference is that Figures 3A, 3B, and 3C do not show solid aluminum metal on the TiB2 substrate surface or at least partially covering them. The description of the solid aluminum metal in the embodiments of Figures 6A-6N also applies to the solid aluminum metal in Figures 7A-7F.

[0223] FIG. 8A is a front view of one embodiment of a product 800. 2 The substrate 802 has a number of grooves 806 as guiding features, and the solid aluminum metal 812 is TiB 2 8A , a portion of solid aluminum metal 812 is shown peripherally or transparently to reveal the surface structure of substrate 802. FIG. 8B is a first side view of a cross section taken along line 8B shown in FIG. 8A . FIG. 8C is an enlarged partial cross-sectional view of the embodiment shown in FIG. 8A , as indicated by the dashed line in FIG. 8A . FIG. 8C includes views of first groove 806A, second groove 806B, and third groove 806C.

[0224] FIG. 8D is a rear view of one embodiment of a product 800′. 2 The substrate 802' has a number of grooves 806' as guide features, and the solid aluminum metal 812' is TiB 2 It covers the front half of the substrate 802'. Figure 8E is a first side view of a cross section taken along line 8E shown in Figure 8D. Figure 8F is an enlarged partial cross-sectional view of the embodiment shown in Figure 8D, indicated by the dashed circle in Figure 8F.

[0225] The embodiments shown in Figures 8D, 8E, and 8F and the embodiments shown in Figures 8A, 8B, and 8C are the same or similar, except for the differences described herein. 2 The amount of solid aluminum metal 812 / 812' covering the substrate 802 / 802' varies depending on the embodiment. In the embodiments of FIGS. 8A, 8B, and 8C, the solid aluminum metal 812 is TiB 2In contrast, the solid aluminum metal 812′ in FIGS. 8D, 8E, and 8F is a TiB 2 Only the front half of the substrate 802' is covered.

[0226] The embodiments of Figures 8A, 8B, 8C, 8D, 8E, and 8F are the same as or similar to the embodiments of Figures 4A, 4B, 4C, and 4D. One difference is that Figures 4A, 4B, 4C, and 4D do not include a TiB 2 Solid aluminum metal on the substrate surface is not shown. 2 Solid aluminum metal 812 / 812' is shown on the substrate. The descriptions of solid aluminum metal 612 / 712 of the embodiments of Figures 6A-6N and 7A-7F also apply to solid aluminum metal 812 / 812' of Figures 8A-8F.

[0227] In FIGS. 8A-8F, the at least one guiding feature is a groove 806 / 806', and the solid aluminum metal 812 / 812' is at least partially contained within the groove 806 / 806'. The at least one groove 806 / 806' comprises a groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 1% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 5% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 10% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 15% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 20% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 25% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 30% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 35% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 40% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 45% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 50% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 55% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 60% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 65% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 70% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 75% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 80% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 85% of the groove volume.In some embodiments, the solid aluminum metal 812 / 812' occupies at least 90% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 95% of the groove volume. In some embodiments, the solid aluminum metal 812 / 812' occupies at least 100% of the groove volume.

[0228] FIG. 9 illustrates a TiB2B substrate having pores 904 and solid aluminum metal 906 according to some embodiments. 2 FIG. 9 is a close-up view of a portion of an embodiment of an article 900 of a substrate 902. 2 The substrate 902 is TiB 2 The web is, for example, a sponge-like structure.

[0229] In some embodiments, the product 900 is TiB 2 TiB of Web 2 Base material 902 and TiB 2 and a solid aluminum metal 906 at least partially covering a surface of the web of substrate 902. 2 The web of the substrate 902 is TiB 2 The web defines pores 904.

[0230] In some embodiments, the solid aluminum metal 906 has voids. The solid aluminum metal 906 may be hot when the solid aluminum metal 906 fills the pores 904. When the solid aluminum metal 906 cools, the solid aluminum metal 906 and TiB 2 There may be spaces (e.g., pores or voids) between the pores of the substrate 902. The pores 904 are filled with TiB 2 The pore volume of the substrate 902 is defined by TiB 2The substrate 902 has web voids. In some embodiments, the solid aluminum metal 906 occupies at least 1% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 5% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 10% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 15% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 20% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 25% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 30% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 35% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 40% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 45% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 50% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 55% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 60% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 65% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 70% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 75% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 80% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 85% of the pore volume. In some embodiments, the solid aluminum metal 906 occupies at least 90% of the pore volume.

[0231] TiB 2 The porosity of the substrate 902 can have any suitable porous structure. 2The voids of the substrate 902 may be an interconnected porous structure, with at least a portion of the pores in fluid communication with one another to facilitate the movement of the wettable material from a first location to a second location (e.g., from a first predetermined location to a second predetermined location). Thus, the interconnected porous structure may be considered an open pore structure. In some embodiments, TiB 2 The voids in the substrate 902 provide a random porous structure. 2 The porosity of the substrate 902 may result in an oriented porous structure. 2 The porosity of the oriented porous structure of the substrate 902 may be a porosity gradient. 2 The porosity gradient of the oriented porous structure of the substrate 902 can vary along a three-dimensional gradient (i.e., the porosity gradient can vary along a three-dimensional gradient). 2 (which may vary along the X, Y, and Z axes of the substrate 902). In some embodiments, TiB 2 The porosity gradient of the oriented porous structure of the substrate 902 is 2 In some embodiments, the TiB 2 The porosity gradient of the oriented porous structure of the substrate 902 is 2 The TiB 2 The porosity gradient of the oriented porous structure of the substrate 902 is 2 From one end of the substrate 902, TiB 2 It may increase, decrease, and then increase to the other end of the substrate 902 .

[0232] The aluminum purification cell comprises the TiB 2 In some embodiments, the substrate may comprise any of the TiB 2 At least one of the substrates is an electrode of an aluminum refining cell. In some embodiments, TiB 2At least one of the substrates is an induction device configured to induce the liquid aluminum metal in a predetermined direction in the absence of an applied electrical current.

[0233] The product comprises at least one induction mechanism and TiB 2 The TiB2 substrate described herein has solid aluminum metal at least partially covering a surface of the substrate. 2The substrate may comprise a substrate. The solid aluminum metal may be at least partially contained within the at least one directing feature. In some embodiments, the at least one directing feature comprises a void volume. In some embodiments, at least 1% of the void volume comprises solid aluminum metal. In some embodiments, at least 5% of the void volume comprises solid aluminum metal. In some embodiments, at least 10% of the void volume comprises solid aluminum metal. In some embodiments, at least 15% of the void volume comprises solid aluminum metal. In some embodiments, at least 20% of the void volume comprises solid aluminum metal. In some embodiments, at least 25% of the void volume comprises solid aluminum metal. In some embodiments, at least 30% of the void volume comprises solid aluminum metal. In some embodiments, at least 35% of the void volume comprises solid aluminum metal. In some embodiments, at least 40% of the void volume comprises solid aluminum metal. In some embodiments, at least 45% of the void volume comprises solid aluminum metal. In some embodiments, at least 50% of the void volume comprises solid aluminum metal. In some embodiments, at least 55% of the void volume comprises solid aluminum metal. In some embodiments, at least 60% of the void volume comprises solid aluminum metal. In some embodiments, at least 65% of the void volume comprises solid aluminum metal. In some embodiments, at least 70% of the void volume comprises solid aluminum metal. In some embodiments, at least 75% of the void volume comprises solid aluminum metal. In some embodiments, at least 80% of the void volume comprises solid aluminum metal. In some embodiments, at least 85% of the void volume comprises solid aluminum metal. In some embodiments, at least 90% of the void volume comprises solid aluminum metal. In some embodiments, at least 95% of the void volume comprises solid aluminum metal. In some embodiments, at least 100% of the void volume comprises solid aluminum metal.

[0234] This disclosure generally relates to TiB2 Although the term refers to a substrate, other ceramic and / or cermet substrates with guiding mechanisms may be used. Any ceramic and / or cermet substrate with guiding mechanisms may be used with any wettable metal. In some embodiments, any wettable metal may be any suitable metal for transfer through the ceramic and / or cermet substrate. In some embodiments, a suitable metal may be aluminum, e.g., aluminum alloys, metallic aluminum, and combinations thereof. In one aspect, the present disclosure relates to products having a ceramic or cermet substrate with guiding mechanisms, the guiding mechanisms configured to guide the ceramic or cermet wettable material in a predetermined direction. In some embodiments, the substrate is a ceramic substrate. In some embodiments, the ceramic substrate is TiB 2 Base material, ZrB 2 Substrate, or HfB 2 In some embodiments, the ceramic wettable material is aluminum, such as aluminum alloys, aluminum metal, and combinations thereof.

[0235] Some of the above disclosures are 2 and aluminum, the apparatus, systems, and methods described herein also apply to TiB 2 For example, the disclosure herein may be applicable to other ceramic and / or cermet materials other than those described above. For example, the disclosure herein may be applicable to other metal borides (e.g., metal diborides) that have metal wettability capabilities, such as ZrB, to name just two examples. 2 and HfB 2 are equally applicable to both, both of which are aluminum wettable materials.

[0236] iii. Start-up of Aluminum Refining Cell 1000 During start-up of the aluminum refining cell 1000, the electrodes of the aluminum refining cell 1000 (e.g., anode 1090 and / or cathode 1150) may be damaged. If the electrodes are not protected, external contaminants, e.g., electrolyte 1110, may damage the electrodes. When the aluminum refining cell 1000 is operating at steady state, protection can be provided by the wettability of the electrodes via the molten metal of the molten metal pad 1100. In some embodiments, when the aluminum refining cell 1000 has gone through the start-up phase and is operating at or near steady state, the molten metal of the molten metal pad 1100 can wet and cover the electrodes, protecting them from contaminants. In some embodiments, the molten metal pad 1100 of the aluminum refining cell 1000 can be either a bottom liquid (protecting the anode 1090) or a top liquid (protecting the cathode 1150).

[0237] In some embodiments, before the aluminum purification cell 1000 can reach a steady state, the electrodes of the aluminum purification cell 1000 can be protected by other methods. For example, the electrodes can be covered with solid aluminum metal as described in section ii. The solid aluminum metal on the electrodes can be a barrier against external contaminants. During start-up, the temperature of the electrodes of the aluminum purification cell 1000 begins to increase. As the temperature increases above the melting point temperature of the solid aluminum metal on the electrodes, the solid aluminum metal undergoes a phase transition from solid to liquid. During the phase transition from solid to liquid, the liquid begins to preferentially wet the electrodes and moves in a predetermined direction via the induction mechanism of the electrodes (e.g., the predetermined direction is vertical and / or horizontal). The liquid aluminum metal covering the previously solid electrodes will facilitate the flow of the molten metal from the molten metal pad 1100. During the steady state operation of the aluminum purification cell 1000, the solid aluminum metal and the liquid metal from the molten metal pad 1100 cover the electrodes and protect them from external contaminants.

[0238] In some embodiments, the aluminum refining cell 1000 is first heated in an empty state, after which a liquid bath and liquid aluminum are placed into the aluminum refining cell 1000. In some embodiments, start-up of the aluminum refining cell 1000 may include a dry bath (i.e., an unmolten bath) since the electrodes are protected by a solid aluminum metal coating during the initial start-up. During start-up of the aluminum refining cell 1000, the dry bath within the aluminum refining cell 1000 may be melted during a cell pre-heat cycle.

[0239] In some embodiments, a method of using the aluminum purification cell 1000 includes limiting or preventing corrosion of the anode 1090 and / or cathode 1150 (e.g., a non-carbonaceous substrate) by the electrolyte 1110 of the aluminum purification cell 1000. In some embodiments, the limiting or preventing includes at least partially covering the anode 1090 and / or cathode 1150 with a wettable material (e.g., molten material from the molten metal pad 1100). The limiting or preventing includes covering at least 50%, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, at least 85%, at least 90%, at least 95%, or at least 99% of the surface area of ​​the anode 1090 and / or cathode 1150 with the wettable material. The wettable material can limit or prevent contact of an exterior surface of the anode 1090 and / or cathode 1150 by the electrolyte 1110.

[0240] In some embodiments, limiting or preventing corrosion of the anode 1090 and / or cathode 1150 (e.g., non-carbonaceous substrate) includes when the temperature of the non-carbonaceous substrate is below the melting point temperature of solid aluminum metal. In some embodiments, limiting or preventing can be achieved by at least partially covering the anode 1090 and / or cathode 1150 (e.g., non-carbonaceous substrate) with solid aluminum. For example, limiting or preventing can include covering at least 50%, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, at least 85%, at least 90%, at least 95%, or at least 99% of the surface area of ​​the anode 1090 and / or cathode 1150 (e.g., non-carbonaceous substrate) with solid aluminum. The solid aluminum can limit or prevent contact of the exterior surface of the anode 1090 and / or cathode 1150 (e.g., non-carbonaceous substrate) with the electrolyte 1110.

[0241] iv. Using a substrate having an induction mechanism in an aluminum refining cell One embodiment of a method for purifying aluminum includes supplying an electric current to the anode 1090. Molten material, including molten aluminum from the molten metal pad 1100, may creep up the vertical surface of the anode 1090. In some embodiments, creeping of molten material from the molten metal pad 1100 may occur continuously during operation of the aluminum refining cell 1000. In some embodiments, the molten material may cover essentially all of the exposed surface of the anode 1090. The molten aluminum on the surface of the anode 1090 may be anodized by the anode 1090, thereby producing aluminum ions. At least a portion of the aluminum ions may be transported through the electrolyte 1110 onto the surface of the cathode 1150. At least a portion of the aluminum ions may be reduced by the cathode 1150, thereby producing purified aluminum on the surface of the cathode 1150.

[0242] Without being bound to a particular mechanism or theory, one possible explanation is that the refined aluminum 1120 climbs up the surface of the cathode 1150 due to the buoyancy of the refined aluminum 1120 within the electrolyte 1110. Thus, the refined aluminum 1120 may tend to collect as a layer above the electrolyte 1110. For example, based on density differences between the refined aluminum 1120 product, the electrolyte 1110 (e.g., bath components within the electrolyte 1110), and the molten metal pad 1100 (including aluminum feedstock 1180 with aluminum metal, impurities, and / or densification aids (e.g., additives to increase density)), the molten metal pad 1100 is configured with a greater density than the electrolyte 1110 such that the molten metal pad zone is configured below the electrolyte zone.

[0243] In some embodiments, the anode 1090 and / or the cathode 1150 can include a guiding mechanism as described in section ii. The guiding mechanism can assist the wettable material (e.g., the molten material of the molten metal pad 1100) in creeping up the anode 1090 and the cathode 1150, as described in section ii. EXAMPLES

[0244] Example 1 - Laboratory scale testing <Porous TiB 2 Base material (TiB 2 Manufacturing of foams

[0245] Four different TiBs, each measuring approximately 3 inches (H) x 2 inches (W) x 0.5 inches (D) 2 The foam samples were fabricated with porosities of approximately 10, 20, 30 and 45 PPI, respectively. 2 The foam samples were made of polyurethane foams with various pore sizes, with TiB 2 The TiB particles were then immersed in an aqueous slurry. 2The coated foam was rolled between a set of parallel rollers with a defined gap thickness, which compressed the infiltrated foam and expelled the unwanted slurry. The rolled TiB 2 The foam was hung in a drying oven. In some cases, the process was repeated, re-immersing the coated foam in the aqueous slurry and then air drying. The final dried TiB 2 The foams were sintered by heating at a temperature of about 1850° C. FIG. 10 shows an example of the sintered final product. The sintered final product had continuous interconnected pores with pore sizes of about 10, 20, 30, and 45 PPI corresponding to the pore sizes of the respective polyurethane foams. As shown in FIG. 10, the pore structure is an open pore structure that allows fluid to move from one predetermined location to another.

[0246] <Water Wetness Test> As shown in Figure 11, four TiB (approximately 10, 20, 30, and 45 PPI) 2 Each foam sample was wrapped with two pieces of tissue paper, one on the top of the sample and one in the middle. 2 The bottom of the sample was placed in 0.25 inches of water well below the center of the sample to test the sample's ability to promote water mass transfer via capillary action. After approximately 12 hours, the samples were evaluated. None of the tissues in the approximately 10 PPI sample were damp or wet, indicating that capillary action was not occurring. In the approximately 20 PPI sample, the center tissue was wet and the top tissue was dry, indicating that some capillary action was occurring. In both the approximately 30 and 45 PPI samples, the center and top tissues were wet, indicating that significant capillary action was occurring.

[0247] <TiB 2 Aluminum metal penetration into foam > Sintered TiB 2 The foam was immersed in molten aluminum for 1 min and then air cooled. After complete cooling, the four TiB2 Each of the foam samples was placed in a approximately 0.5 inch deep slot in the graphite pedestal of three separate crucibles (Crucible #1, Crucible #2, and Crucible #3, described further below). Each of the three crucibles was placed in a furnace and heated to 900° C. in argon. A purified molten aluminum composition (pure aluminum pellets) and a molten bath composition were placed in each crucible. The molten bath composition was cryolite-based and contained NaF, AlF 3 , and CaF 2 It contained ingredients.

[0248] 4 TiB 2 The crucibles with the foam samples, molten aluminum, and cryolite were held at 900° C. for about 48 hours. As shown in FIG. 12, in crucible #1, four TiB 2 The foam samples were completely immersed in molten aluminum for 48 hours. In crucibles #2 and #3, four TiB 2 The foam samples were partially immersed in approximately 1 and 2 inches of molten aluminum, respectively, and the remainder of the foam was exposed to the molten bath for 48 hours.

[0249] As shown in Figures 13A and 13B, after 48 hours of testing at 900°C, four TiB 2 No corrosion was observed on the foam samples, indicating that the samples were wetted by the molten aluminum through capillary action promoted by the pores of the foam. 2 Protects against corrosion by cryolite.

[0250] Example 2 - Larger Laboratory Scale Testing <TiB 2 Preparation of foam samples>

[0251] Two separate TiBs, each measuring approximately 16 inches (H) x 2 inches (W) x 0.5 inches (D). 2 The foam samples were produced by the process of the foam samples of Example 1. Two TiB 2The sintered final product of the foam samples had continuous interconnected pores with pore sizes of approximately 20 and 30 PPI corresponding to the pore sizes of the respective polyurethane foams.

[0252] <TiB 2 Aluminum metal penetration into foam > Two untreated TiB 2 The foam sample was placed in a slot about 2 inches deep in the graphite platform of the crucible. Prior to being placed in the graphite platform, purified molten aluminum compositions (pure aluminum pellets) and (cryolite-based, NaF, AlF 3 , and CaF 2 A molten bath composition (containing the TiB2O3 component) was placed in each crucible, and each crucible was placed in a furnace and heated to 900° C. in argon. After heating, two TiB2O3 melted into the melt. 2 Each of the foam samples was placed in a crucible. 2 The crucibles containing the foam samples, molten aluminum, and cryolite were held at 900° C., and after approximately 10 minutes of testing, the two TiB 2 The foam sample was removed from the crucible and molten aluminum was detected at the top of the sample. 2 No corrosion was observed on any of the foam samples, indicating that the samples were wetted by approximately 14 inches of molten aluminum through capillary action promoted by the pores in the foam. 2 Protects against corrosion by cryolite.

[0253] While a number of embodiments of the present disclosure have been described, it will be understood that these embodiments are illustrative and not limiting, and that numerous modifications will become apparent to those skilled in the art. The various steps may be performed in any desired order (and any desired steps may be added and / or any desired steps may be removed). For example, the shape and characteristics of the guide features (e.g., slots, pores, or grooves) may vary from product to product comprising an aluminum refining cell and / or TiB 2The solid aluminum metallization may be used with any of the substrates or alone. The solid aluminum metallization features and properties described in any of the embodiments may be used in any other embodiment described herein. The exemplary embodiments of the guidance mechanism and solid aluminum metallization are not intended to be exhaustive. The features and properties of the present disclosure may be combined in any manner.

Claims

1. 1. An aluminum refining cell comprising: a non-carbonaceous substrate, the non-carbonaceous substrate comprising an induction mechanism; The aluminum refining cell, wherein the guiding mechanism is configured to guide the wettable material in a predetermined direction.

2. The cell is A cell chamber; at least one anode within the cell chamber; 10. The cell of claim 1 comprising: at least one cathode within the cell chamber, the at least one cathode at least partially overlying a top portion of the at least one anode.

3. The cell of claim 1 or 2, wherein at least a portion of the wettable material is disposed within and / or on the guidance feature.

4. The cell of any one of claims 1 to 3, wherein the wettable material is a molten metal.

5. The cell of any one of claims 1 to 4, wherein the wettable material comprises a metal.

6. 6. The cell of claim 5, wherein the metal comprises at least aluminum and magnesium.

7. The cell of claim 5 , wherein the metal comprises aluminum.

8. 6. The cell of claim 5, wherein the metal comprises at least 50 weight percent aluminum, or at least 55 weight percent aluminum, or at least 60 weight percent aluminum, or at least 65 weight percent aluminum, or at least 70 weight percent aluminum, or at least 75 weight percent aluminum, or at least 80 weight percent aluminum, or at least 85 weight percent aluminum, or at least 90 weight percent aluminum, or at least 95 weight percent aluminum.

9. 6. The cell of claim 5, wherein the metal is selected from the group consisting of an aluminum alloy, aluminum metal, and combinations thereof.

10. The cell of any one of claims 1 to 9, wherein a surface of the non-carbonaceous substrate is at least partially covered with solid aluminum metal.

11. The cell of any one of claims 1 to 10, wherein the guiding features are selected from the group consisting of slots, grooves, pores, and combinations thereof.

12. The cell of any one of claims 1 to 11, wherein the non-carbonaceous substrate comprises a cermet or a ceramic.

13. The non-carbonaceous substrate is TiB 2 The cell according to any one of claims 1 to 12, comprising:

14. The non-carbonaceous substrate is TiB 2 The cell of any one of claims 1 to 12, consisting essentially of

15. The cell according to any one of claims 1 to 14, wherein the predetermined direction is vertical and / or horizontal.

16. The cell of any one of claims 1 to 14, wherein the predetermined direction is an upward direction towards an electrolyte of the aluminium refining cell.

17. The cell of any one of claims 1 to 16, wherein the non-carbonaceous substrate is not an electrode.

18. The cell of any one of claims 1 to 17, wherein the non-carbonaceous substrate is an electrode.

19. 20. The cell of claim 18, wherein the non-carbonaceous substrate is an anode or a cathode.

20. The cell of any one of claims 1 to 19, wherein the non-carbonaceous substrate is a first substrate and the cell comprises a second substrate.

21. 21. The cell of claim 20, wherein the second substrate is a carbonaceous substrate.

22. 21. The cell of claim 20, wherein the second substrate is a non-carbonaceous substrate.

23. The cell of claim 20 , wherein the second substrate comprises a cermet or a ceramic.

24. The second substrate is TiB 2 21. The cell of claim 20 comprising:

25. The second substrate is TiB 2 21. The cell of claim 20 consisting essentially of:

26. The cell of claim 20 , wherein the second substrate comprises a guidance mechanism.

27. The cell of claim 20 , wherein the second substrate is devoid of a guidance mechanism.

28. 21. The cell of claim 20, wherein the second substrate is an anode.

29. 21. The cell of claim 20, wherein the second substrate is a cathode.

30. (a) a non-carbonaceous substrate having at least one induction feature; (b) solid aluminum metal at least partially covering a surface of the non-carbonaceous substrate.

31. The cell is A cell chamber; at least one anode within the cell chamber; 31. The cell of claim 30 comprising: at least one cathode within the cell chamber, the at least one cathode at least partially overlying a top portion of the at least one anode.

32. 32. The cell of claim 30 or 31, wherein at least a portion of the solid aluminum metal is disposed within and / or on the guidance feature.

33. The cell of any one of claims 1 to 32, wherein the solid aluminum metal is at least partially contained within the at least one induction feature.

34. 34. The cell of any one of claims 1 to 33, wherein the non-carbonaceous substrate comprises a surface region, a first portion of the surface region comprising the at least one inductive feature, and a second portion of the surface region is free of any inductive features.

35. 35. The cell of claim 34, wherein the first portion of the surface region is at least partially covered by the solid aluminum metal.

36. 35. The cell of claim 34, wherein the first portion of the surface area is at least 1% covered by the solid aluminum metal.

37. The cell of any one of claims 34 to 36, wherein the second portion of the surface region is at least partially covered by the solid aluminum metal.

38. The cell of any one of claims 34 to 36, wherein the second portion of the surface area is at least 1% covered by the solid aluminum metal.

39. 39. A method of using any of the aluminum purification cells of claims 1 to 38, wherein a surface of the non-carbonaceous substrate is at least partially covered with solid aluminum metal, the method comprising: heating the non-carbonaceous substrate above a melting point temperature of the solid aluminum metal.

40. A method of using any of the aluminium refining cells according to claims 1 to 38, comprising the steps of: limiting or preventing corrosion of the non-carbonaceous substrate by an electrolyte of the aluminum refining cell.

41. 41. The method of claim 40, wherein the limiting or preventing comprises at least partially covering the non-carbonaceous substrate with the wettable material.

42. 41. The method of claim 40, wherein the limiting or preventing comprises covering at least 50%, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, at least 85%, at least 90%, at least 95%, or at least 99% of the surface area of ​​the non-carbonaceous substrate with the wettable material.

43. The method of claims 40-42, wherein the wettable material limits or prevents contact of the exterior surface of the substrate by the electrolyte.

44. A method of using any of the aluminium refining cells according to claims 1 to 38, comprising the steps of: limiting or preventing corrosion of the non-carbonaceous substrate when the temperature of the non-carbonaceous substrate is below a melting point temperature of the solid aluminum metal.

45. 45. The method of claim 44, wherein said limiting or preventing comprises at least partially covering said non-carbonaceous substrate with said solid aluminum.

46. 45. The method of claim 44, wherein the limiting or preventing comprises covering at least 50%, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, at least 85%, at least 90%, at least 95%, or at least 99% of the surface area of ​​the non-carbonaceous substrate with the solid aluminum.

47. The method of claims 44-46, wherein the solid aluminum limits or prevents contact of the exterior surface of the substrate with an electrolyte.

48. A method according to any one of claims 39 to 47, comprising the steps of: (a) supplying an aluminum source to the aluminum refining cell, the aluminum source comprising aluminum metal, the aluminum refining cell comprising a molten metal pad and an electrolyte, the molten metal pad having a density greater than a density of the electrolyte; (b) passing a current through the at least one anode, through the electrolyte, and to the at least one cathode; (i) the at least one anode and the at least one cathode are partially disposed in the electrolyte; (ii) the at least one anode is partially disposed in the molten metal pad; (iii) the at least one anode and / or the at least one cathode are non-carbonaceous substrates having an induction mechanism; (iv) energizing the guiding mechanism, the guiding mechanism being configured to guide the wettable material in a predetermined direction; (c) directing the aluminum metal from the molten metal pad into the electrolyte by the directing mechanism; (d) generating at least some aluminum ions in the electrolyte; and (e) producing a refined aluminum product.

49. The non-carbonaceous substrate is TiB 2 The cell of any one of claims 1 to 38, comprising a carbon-based material plated with

50. The cell of any one of claims 1 to 38, wherein the non-carbonaceous substrate comprises a plating material that promotes wettability.

51. 51. The cell of claim 50, wherein the plating material comprises a ceramic and / or a cermet.

52. The plating material is TiB 2 52. The cell of claim 51 , comprising:

53. The non-carbonaceous substrate is TiB 2 The method of any one of claims 39 to 48, comprising a carbon-based material plated with

54. The method of any one of claims 39 to 48, wherein the non-carbonaceous substrate comprises a plating material that promotes wettability.

55. 55. The method of claim 54, wherein the plating material comprises a ceramic and / or a cermet.

56. The plating material is TiB 2 56. The method of claim 55, comprising:

57. The cell of any one of claims 1 to 38 or 49 to 52, wherein the guidance mechanism comprises at least one channel.

58. 58. The cell of claim 57, wherein the at least one channel has a cross-section, the cross-section being substantially constant throughout the length of the at least one channel.

59. 58. The cell of claim 57, wherein the at least one channel comprises a cross-section, the cross-section varying over a length of the at least one channel.

60. 57. The method of any one of claims 39-48 or 53-56, wherein the guidance mechanism comprises at least one channel.

61. 61. The method of claim 60, wherein the at least one channel has a cross-section, the cross-section being substantially constant throughout the length of the at least one channel.

62. 61. The method of claim 60, wherein the at least one channel comprises a cross-section, the cross-section being variable over a length of the at least one channel.

63. 60. The cell of any one of claims 1-38, 49-52, or 57-59, wherein the directing feature comprises an oriented porous structure.

64. 64. The cell of claim 63, wherein the oriented porous structure has a porosity gradient.

65. 63. The method of any one of claims 39-48, 53-56, or 60-62, wherein the directing features comprise an oriented porous structure.

66. 66. The method of claim 65, wherein the oriented porous structure has a porosity gradient.

67. 65. The cell of any one of claims 1-38, 49-52, 57-59, 63, or 64, wherein the induction feature is in or on the non-carbonaceous substrate.

68. 70. The method of any one of claims 39-48, 53-56, 60-62, 65, or 66, wherein the induction mechanism is within or on the non-carbonaceous substrate.