Lithium secondary battery
A non-aqueous electrolyte with a phosphonate additive forms stable films on lithium-ion battery electrodes, addressing deterioration issues and improving high-temperature performance.
Patent Information
- Application Number
- JP2024526910
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-09
- Filing Date
- 2023-03-10
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-03-10
AI Technical Summary
Lithium-ion batteries face issues with electrode deterioration due to transition metal elution and SEI layer degradation, leading to increased resistance and reduced capacity at high temperatures, especially when using silicon-based negative electrodes.
Incorporating a non-aqueous electrolyte with an additive that forms a firm film on the electrode surfaces, containing a compound represented by Chemical Formula 1, which includes a phosphonate group to stabilize the SEI and CEI films, preventing metal elution and electrolyte decomposition.
The solution enhances the battery's cycle characteristics and high-temperature storage stability by forming stable films on the electrodes, reducing resistance and maintaining capacity.
Smart Images

Figure 2024540381000001 
Figure 2024540381000002 
Figure 2024540381000003
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0033019 filed on March 16, 2022 and Korean Patent Application No. 10-2023-0031448 filed on March 9, 2023, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference. The present invention relates to a lithium secondary battery having improved high-temperature storage characteristics and high-temperature cycle characteristics. [Background technology]
[0002] 2. Description of the Related Art As modern society becomes increasingly dependent on electrical energy, there is a demand for increased electrical energy production, and large-capacity power storage devices capable of stably supplying power are being developed.
[0003] Lithium-ion batteries have been attracting attention as the device that exhibits the highest energy density among commercially available power storage devices.
[0004] A lithium-ion battery is composed of a positive electrode made of a transition metal oxide containing lithium, a negative electrode capable of storing lithium, an electrolyte solution containing an organic solvent containing a lithium salt, and a separator.
[0005] Among these, the positive electrode stores energy through the oxidation-reduction reaction of transition metals, which ultimately means that the positive electrode material must contain a transition metal.
[0006] However, repeated charging and discharging may cause the collapse of a particular positive electrode structure, resulting in the elution of the transition metal, or the elution of the transition metal due to an acid formed by a side reaction of the electrolyte or hydration / thermal decomposition of lithium salt under a high operating potential. The eluted transition metal is not only re-deposited on the positive electrode, thereby increasing the resistance of the positive electrode, but is also electrodeposited on the negative electrode through the electrolyte, thereby causing self-discharge of the negative electrode, and is known to be a factor in increasing the interface resistance of the negative electrode by destroying the solid electrolyte interphase (SEI) film on the surface of the negative electrode and promoting additional electrolyte decomposition reactions.
[0007] Furthermore, when a silicon-based negative electrode active material is used as a negative electrode component of the lithium ion battery, the SEI layer is lost due to electrode expansion as the cycle progresses, which may lead to an increase in resistance and an increase in electrolyte side reactions, and such problems may cause damage to the electrode structure.
[0008] Therefore, there is a need for research into methods that can prevent the deterioration of secondary batteries by forming a strong passivation film on the electrode surface. Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide a lithium secondary battery having improved high-temperature storage characteristics and high-temperature cycle characteristics by including a non-aqueous electrolyte solution containing an additive capable of forming a strong coating on the electrode surface. [Means for solving the problem]
[0010] In one embodiment of the present invention to achieve the above object, positive electrode, a negative electrode including a silicon-based negative electrode active material; A separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte solution including a lithium salt, an organic solvent, and an additive; The additive provides a lithium secondary battery containing a compound represented by the following Chemical Formula 1.
Chem.
[0011] On the other hand, the silicon-based negative electrode active material may be at least one selected from the group consisting of silicon, silicon chloride, silicon oxide (SiO x (0 < x < 2)), and silicon-carbon composite (SiC). Specifically, the silicon-based negative electrode active material may be silicon oxide.
[0012] On the other hand, the negative electrode may further contain a carbon-based negative electrode active material. In this case, the mixing ratio of the silicon-based negative electrode active material and the carbon-based negative electrode active material may be 1:99 to 20:80 by weight, specifically 1:99 to 10:90.
[0013] On the other hand, the positive electrode may contain a positive electrode active material containing at least one metal selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), and aluminum (Al) and lithium.
[0014] On the other hand, in the Chemical Formula 1, R 1 ~R 3 may each independently be an alkyl group having 1 to 8 carbon atoms. Specifically, in the Chemical Formula 1, R 1 is an alkyl group having 1 to 5 carbon atoms, and the R 2 ~R 3 may each independently be an alkyl group having 2 to 6 carbon atoms. More specifically, in the Chemical Formula 1, the R 1 is an alkyl group having 1 to 3 carbon atoms, and the R 2 ~R 3 may each independently be an alkyl group having 2 to 5 carbon atoms.
[0015] Meanwhile, the compound represented by Formula 1 may be included in an amount of 0.1 wt % to 5.0 wt % based on the total weight of the nonaqueous electrolyte. Effect of the Invention
[0016] In order to solve the above problems, the present invention provides a negative electrode containing a silicon-based negative electrode active material and a phosphonate (-PO(OR) 2 By using a non-aqueous electrolyte solution containing a compound having a silicon-based functional group as an additive, a strong coating of an inorganic component can be formed on the surface of a negative electrode containing a silicon-based negative electrode active material, thereby preventing deterioration of the battery, and thus providing a lithium secondary battery that can realize excellent cycle characteristics and high-temperature storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will now be described in more detail. The terms and phrases used in the present specification and claims are merely used to describe exemplary embodiments and are not intended to limit the present invention.
[0018] For example, in this specification, terms such as "including," "comprising," or "having" are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and other parts may be added, unless "only" is used.
[0019] In this specification, "%" means "% by weight" unless otherwise specified.
[0020] In this specification, unless otherwise defined, the term "substituted" means that at least one hydrogen bonded to a carbon is replaced with an element other than hydrogen, for example, replaced with an alkyl group having 1 to 5 carbon atoms or a fluorine element.
[0021] Generally, the passivation performance of the SEI film formed on the negative electrode surface by the decomposition of the electrolyte and the CEI film formed on the positive electrode surface at high potential is a factor that has a significant impact on the improvement of the storage performance of secondary batteries. On the other hand, the lithium salt (LiPF 6 Lewis acid substances generated by the thermal decomposition of the cathode are known to cause the deterioration of the anode coating (SEI) and cathode coating (CEI). That is, when the cathode surface is deteriorated by the attack of the Lewis acid substance, a side reaction with the electrolyte occurs, which causes the transition metal to dissolve and the local structure of the cathode surface changes, which may increase the surface resistance of the electrode and reduce the capacity. In addition, transition metal ions dissolve from the cathode due to the structural change of the cathode caused by repeated charging and discharging. The dissolved transition metal ions move to the anode via the electrolyte and are then electrodeposited on the anode, causing the anode to self-discharge and destroy the coating (SEI), which promotes an additional electrolyte decomposition reaction and increases the interface resistance between the anode and the cathode.
[0022] The present invention provides a lithium secondary battery that can realize excellent cycle characteristics and high-temperature storage stability by using a negative electrode containing a silicon-based negative electrode active material in combination with a non-aqueous electrolyte solution containing an additive that can form a strong coating on the negative electrode surface and the positive electrode surface to suppress deterioration of the positive electrode and the negative electrode during rapid charging.
[0023] Lithium secondary battery According to an embodiment of the present invention, the lithium secondary battery of the present invention comprises: positive electrode, a negative electrode including a silicon-based negative electrode active material; A separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte solution including a lithium salt, an organic solvent, and an additive; The additive may include a compound represented by the following Chemical Formula 1: [ka] In the above Chemical Formula 1, R 1 ~R 3are each independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.
[0024] The configuration of the lithium secondary battery of the present invention will be specifically described below. (1) Positive electrode The positive electrode according to the present invention may contain a positive electrode active material, and may further contain a conductive material and / or a binder, if necessary.
[0025] The positive electrode active material may include a compound capable of reversible intercalation and deintercalation of lithium, specifically, a lithium transition metal oxide represented by the following Chemical Formula 2, which includes at least one metal selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), and aluminum (Al) and lithium. [Chemical formula 2] Li 1+a Ni x Co y M 1 z M 2 w O 2 In the above Chemical Formula 2, M 1 is Mn, Al or a combination thereof, M 2 is at least one selected from the group consisting of Al, Zr, W, Ti, Mg, Ca and Sr, 0≦a≦0.5, 0 <x≦0.6、0<y≦0.4、0<z≦0.4、0≦w≦0.1である。
[0026] The 1+a represents the atomic fraction of lithium in the lithium transition metal oxide, and may be 0≦a≦0.5, preferably 0≦a≦0.2, and more preferably 0≦a≦0.1. When the atomic fraction of lithium satisfies the above range, the crystal structure of the lithium transition metal oxide can be stably formed.
[0027] The x represents the atomic fraction of nickel among all the transition metal elements in the lithium transition metal oxide, where 0 < x ≤ 0.6, specifically 0.55 < x < 1.0, more specifically 0.6 ≤ x ≤ 0.98, and even more specifically 0.6 ≤ x ≤ 0.95. When the atomic fraction of nickel satisfies the above range, it shows a high energy density, so it is possible to realize a high capacity.
[0028] The y represents the atomic fraction of cobalt among all the transition metal elements in the lithium transition metal oxide, where 0 < y ≤ 0.4, specifically 0 < y ≤ 0.3, and more specifically 0.05 ≤ y ≤ 0.3. When the atomic fraction of cobalt satisfies the above range, good resistance characteristics and output characteristics can be realized.
[0029] The z represents the atomic fraction of the M 1 element among all the transition metal elements in the lithium transition metal oxide, where 0 < z ≤ 0.4, preferably 0 < z ≤ 0.3, and more preferably 0.01 ≤ z ≤ 0.3. 1 When the atomic fraction of the M
[0030] element satisfies the above range, the structural stability of the positive electrode active material is excellent. 2 The w represents the atomic fraction of the M
[0031] element among all the transition metal elements in the lithium transition metal oxide, where 0 < w ≤ 0.1, preferably 0 < w ≤ 0.05, and more preferably 0 < w ≤ 0.02. 0.6 Specifically, in order to realize a high-capacity battery, the positive electrode active material has a Ni content of 0.55 atm% or more, such as Li(Ni 0.2 Mn 0.2 )O 2 , Li(Ni 0.7 Mn 0.15 Co 0.15 )O 2 , Li(Ni 0.7 Mn 0.2 Co 0.1 )O 2 , Li(Ni 0.8 Mn 0.1 Co 0.1 )O 2 , Li(Ni0.8 Co 0.15 Al 0.05 )O 2 、Li(Ni 0.86 Mn 0.07 Co 0.05 Al 0.02 )O 2 、又はLi(Ni 0.90 Mn 0.05 Co 0.05 )O 2 may include lithium composite transition metal oxides such as these.
[0032] In addition, the positive electrode active material may be used in combination with a lithium-manganese-based oxide (for example, LiMnO 2 、LiMn 2 O 4 etc.), a lithium-cobalt-based oxide (for example, LiCoO 2 etc.), a lithium-nickel-based oxide (for example, LiNiO 2 etc.), a lithium-nickel-manganese-based oxide (for example, LiNi 1-Y Mn Y O 2 (0 < Y < 1), LiMn 2-z Ni z O 4 (0 < Z < 2), a lithium-nickel-cobalt-based oxide (for example, LiNi 1-Y1 Co Y1 O 2 (0 < Y1 < 1), a lithium-manganese-cobalt-based oxide (for example, LiCo 1-Y2 Mn Y2 O 2 (0 < Y2 < 1), LiMn 2-z1 Co z1 O 4 (0 < Z1 < 2), or Li(Ni p1 Co q1 Mn r2 )O 4 (0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2), etc. may be used in combination.
[0033] Next, the conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing chemical changes in the battery that is constructed.Specific examples include carbon powders such as carbon black, acetylene black (or denka black), ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, and graphite with highly developed crystal structures; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in mixture.
[0034] Secondly, the binder serves to improve adhesion between particles of the positive electrode active material and between the positive electrode active material and the current collector.
[0035] Examples of such binders include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders. One or a mixture of two or more of these binders may be used.
[0036] Meanwhile, the positive electrode of the present invention may be manufactured by a method for manufacturing a positive electrode known in the art. For example, the positive electrode may be manufactured by a method of coating a positive electrode slurry prepared by dissolving or dispersing a positive electrode active material, a binder, and / or a conductive material in a solvent on a positive electrode current collector, drying and rolling the cathode slurry, or a method of casting the positive electrode slurry on a separate support to form a film, peeling off the support, and laminating the film on a positive electrode current collector.
[0037] The positive electrode active material may be included in an amount of 80 wt% to 98 wt%, more specifically, 85 wt% to 98 wt%, based on the total weight of the positive electrode slurry. When the positive electrode active material is included in this range, excellent capacity characteristics can be exhibited.
[0038] The conductive material may be included in an amount of 0.1 wt % to 10 wt %, preferably 0.1 wt % to 5 wt %, based on the total weight of the positive electrode slurry, and the binder may be included in an amount of 0.1 wt % to 15 wt %, preferably 0.1 wt % to 10 wt %, based on the total weight of the positive electrode active material layer.
[0039] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The positive electrode current collector may generally have a thickness of 3 μm to 500 μm, and fine irregularities may be formed on the collector surface to increase the adhesive strength of the positive electrode material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0040] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, etc. One of these alone or a mixture of two or more may be used. The amount of the solvent used may be adjusted so that the positive electrode composite material has an appropriate viscosity in consideration of the coating thickness of the positive electrode composite material, production yield, workability, etc., and is not particularly limited.
[0041] (2) Negative electrode The negative electrode according to the present invention contains a negative electrode active material and may further contain a conductive material and / or a binder as necessary.
[0042] As the negative electrode active material, a silicon-based negative electrode active material used in the industry may be used, and further, a carbon-based negative electrode active material may be mixed and used together with the silicon-based negative electrode active material.
[0043] The silicon (Si)-based negative electrode active material is, for example, silicon (Si), silicon carbide (SiC), silicon chloride, and silicon oxide (SiO x , where 0 < x < 2), Si-Y alloy (where Y is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), and may include one or more selected from the group consisting of. As the element Y, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db (dubnium), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof may be selected.
[0044] Specifically, the negative electrode active material is silicon dioxide (SiO 2) and amorphous silicon in a 1:1 mixture ratio based on weight ratio.
[0045] * Meanwhile, the silicon-based negative electrode active material can obtain higher capacity characteristics than the carbon-based negative electrode active material. However, in the case of a negative electrode containing a silicon-based negative electrode active material, an SEI film containing more oxygen (O)-rich components than a graphite negative electrode is formed on the surface due to a reaction with a non-aqueous electrolyte during initial charging and discharging, and such an SEI film is formed when HF or PF is added to the electrolyte. 5 In the presence of such Lewis acids, the electrolyte is easily decomposed, which may cause side reactions in the electrolyte or induce consumption of the electrolyte. Therefore, when using a silicon-based negative electrode active material as the negative electrode component, it is important to form a robust SEI film containing inorganic components in order to suppress the decomposition of Si by HF. In other words, when using a negative electrode containing a silicon-based negative electrode active material, the non-aqueous electrolyte used in combination must contain HF and PF in the electrolyte in order to stably maintain the SEI film. 5 There is a need to include an additive capable of suppressing the generation of such Lewis acids or scavenging the generated Lewis acids while forming an inorganic coating.
[0046] In addition, the carbon-based negative electrode active material that can be used in combination with the silicon-based negative electrode active material may be any of various carbon-based negative electrode active materials used in the art, for example, graphite-based materials such as natural graphite, artificial graphite, and Kish graphite; pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes, soft carbon, hard carbon, etc. The shape of the carbon-based negative electrode active material is not particularly limited, and materials of various shapes such as amorphous, plate-like, scaly, spherical, or fibrous may be used.
[0047] Meanwhile, the silicon-based negative electrode active material and the carbon-based negative electrode active material may be mixed and used in a weight ratio of 1:99 to 20:80. When the mixing ratio of the silicon-based negative electrode active material and the carbon-based negative electrode active material is satisfied, the volume expansion of the silicon-based negative electrode active material is suppressed while improving the capacity characteristics, and excellent cycle performance of the battery can be secured, and high capacity can be realized. When the mixing ratio of the silicon-based negative electrode active material is less than 1 weight ratio, it is difficult to increase the energy density and to increase the capacity of the battery, and when it exceeds 20 weight ratio, the degree of volume expansion of the negative electrode may increase. Specifically, the mixing ratio of the silicon-based negative electrode active material and the carbon-based negative electrode active material may be 1:99 to 10:90 by weight ratio, specifically 3:97 to 5:95, more specifically 5:95 to 3:9.
[0048] Next, the conductive material is not particularly limited as long as it is a component for further improving the conductivity of the negative electrode active material and has conductivity without causing a chemical change in the battery. Specifically, the conductive material may be carbon powder such as carbon black, acetylene black (or denka black), ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive fiber such as carbon fiber or metal fiber; conductive powder such as carbon fluoride powder, aluminum powder, or nickel powder; conductive whisker such as zinc oxide or potassium titanate; conductive metal oxide such as titanium oxide; conductive material such as polyphenylene derivative, and the like, and may be the same as or different from the conductive material applied to the positive electrode.
[0049] The binder is a component that aids in adhesion between the conductive material, the active material, and the current collector. Representative examples of the binder include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders. The binder may be the same as or different from the binder applied to the positive electrode.
[0050] The negative electrode may be manufactured by a method for manufacturing a negative electrode known in the art. For example, the negative electrode may be manufactured by applying a negative electrode slurry, which is prepared by dissolving or dispersing a negative electrode active material and, optionally, a binder and a conductive material in a solvent, onto a negative electrode current collector, followed by drying and rolling, or by casting the negative electrode slurry onto a separate support to form a film, and then peeling off the support to form a film, which is then laminated onto the negative electrode current collector.
[0051] The negative electrode active material may be included in an amount of 80 wt % to 99 wt % based on the total weight of the negative electrode slurry. When the content of the negative electrode active material is in this range, excellent capacity characteristics and electrochemical characteristics can be obtained.
[0052] The conductive material may be added in an amount of 10 wt % or less, preferably 5 wt % or less, based on the total weight of the negative electrode slurry, and the binder may be included in an amount of 0.1 to 15 wt %, preferably 0.1 to 10 wt %, based on the total weight of the negative electrode slurry.
[0053] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of typically 3 μm to 500 μm, and may have fine irregularities formed on the surface of the current collector to strengthen the binding force of the negative electrode active material, as in the case of the positive electrode current collector. For example, the negative electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.
[0054] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and one or a mixture of two or more of these may be used. The amount of the solvent used is not particularly limited as long as it can be adjusted to an appropriate viscosity of the negative electrode slurry in consideration of the coating thickness of the negative electrode composite, production yield, workability, etc.
[0055] (3) Separator The lithium secondary battery according to the present invention includes a separator between the positive electrode and the negative electrode. The separator separates the negative electrode and the positive electrode to provide a path for lithium ion migration. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion migration of a lithium salt and excellent moisture-absorbing ability for an electrolyte is preferred.
[0056] Specifically, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof. Also, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used. Also, in order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be selectively used as a single layer or a multilayer structure.
[0057] (4) Non-aqueous electrolyte The lithium secondary battery according to the present invention comprises a non-aqueous electrolyte solution containing a lithium salt, an organic solvent, and an additive.
[0058] (4-1) Lithium salt First, in the non-aqueous electrolyte of the present invention, the lithium salt may be any one that is commonly used in non-aqueous electrolytes for lithium secondary batteries without any limitations. For example, Li + The anion is F - , Cl - , Br - , I - , NO 3 - , N(CN) 2 - , B.F. 4 - , ClO 4 - , B 10 Cl 10 - , AlCl 4 - , AlO 4 - , P.F. 6 - , C.F. 3 SO 3 - , C.H. 3 CO 2 - , C.F. 3 CO 2 - , AsF 6 - , SbF 6 - , C.H. 3 SO 3 - , (CF 3 CF 2 SO 2 ) 2 N - , (CF 3 SO 2 ) 2 N - , (FSO 2 ) 2 N - , B.F. 2 C 2 O 4 - , B.C. 4 O 8 - , P.F. 4 C 2 O 4- , P.F. 2 C 4 O 8 - , (CF 3 ) 2 PF 4 - , (CF 3 ) 3 PF 3 - , (CF 3 ) 4 PF 2 - , (CF 3 ) 5 PF - , (CF 3 ) 6 P - , C 4 F 9 SO 3 - , C.F. 3 CF 2 SO 3 - , C.F. 3 CF 2 (CF 3 ) 2 CO - , (CF 3 SO 2 ) 2 CH - , C.F. 3 (CF 2 ) 7 SO 3 - and SCN - At least one selected from the group consisting of:
[0059] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF 4 , LiClO 4 , LiB 10 Cl 10 , LiAlCl 4 , LiAlO 4 , LiPF 6 , LiCF 3 SO 3 , LiCH 3 CO 2 , LiCF 3 CO 2, LiAsF 6 , LiSbF 6 , LiCH 3 SO 3 , LiN(SO 2 F) 2 (lithium bis(fluorosulfonyl)imide, LiFSI), LiN(SO 2 CF 2 CF 3 ) 2 (lithium bis(pentafluoroethanesulfonyl)imide, LiBETI), and LiN(SO 2 CF 3 ) 2 (lithium bis(trifluoromethane sulfonyl)imide, LiTFSI) may be used alone or in combination of two or more. In addition, any lithium salt commonly used in the electrolyte of a lithium secondary battery may be used without limitation.
[0060] The lithium salt may be appropriately changed within a range that is normally usable, but in order to obtain the optimum effect of forming a corrosion prevention coating on the electrode surface, the lithium salt may be contained in the electrolyte at a concentration of 0.8 M to 4.0 M, specifically, at a concentration of 1.0 M to 3.0 M.
[0061] When the concentration of the lithium salt is within the above range, the viscosity of the non-aqueous electrolyte can be controlled to realize optimal impregnation, and the mobility of lithium ions can be improved, thereby improving the capacity characteristics and cycle characteristics of the lithium secondary battery.
[0062] (4-2) Organic Solvent The organic solvent is described below. As the non-aqueous organic solvent, various organic solvents commonly used in non-aqueous electrolytes may be used without limitation, and there is no limitation on the type of the organic solvent as long as it can minimize decomposition due to an oxidation reaction during the charge / discharge process of a secondary battery and can exhibit desired properties together with additives.
[0063] Specifically, the non-aqueous organic solvent may include (i) a cyclic carbonate organic solvent, (ii) a linear carbonate organic solvent, or (iii) a mixed organic solvent thereof.
[0064] The (i) cyclic carbonate organic solvent is a high-viscosity organic solvent having a high dielectric constant and capable of easily dissociating a lithium salt in a non-aqueous electrolyte solution, and specific examples thereof include at least one organic solvent selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and among these, at least one of ethylene carbonate and propylene carbonate may be included.
[0065] The (ii) linear carbonate organic solvent is an organic solvent having low viscosity and low dielectric constant, and specific examples thereof may include at least one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and specifically may include one of dimethyl carbonate and ethyl methyl carbonate.
[0066] In order to ensure high ionic conductivity, the (i) cyclic carbonate organic solvent and the (ii) linear carbonate organic solvent may be mixed in a volume ratio of 10:90 to 50:50, specifically 20:80 to 40:60.
[0067] In addition, the nonaqueous electrolyte solution according to the present invention may further include at least one organic solvent selected from the group consisting of (iv) a linear ester organic solvent and (v) a cyclic ester organic solvent, which have a lower melting point and higher stability at high temperatures than the cyclic carbonate organic solvent and / or the linear carbonate organic solvent, thereby further improving the ionic conductivity of the nonaqueous electrolyte solution according to the present invention.
[0068] A representative example of the (iv) linear ester organic solvent is at least one organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate, and specifically may include at least one of ethyl propionate and propyl propionate.
[0069] The (iv) cyclic ester organic solvent may contain at least one selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0070] Meanwhile, the organic solvent may be any organic solvent commonly used in electrolytes for lithium secondary batteries without limitation, if necessary, and may further include at least one organic solvent selected from the group consisting of ether-based organic solvents, amide-based organic solvents, and nitrile-based organic solvents.
[0071] Meanwhile, in the nonaqueous electrolyte solution of the present invention, the remaining components excluding the lithium salt, the additives, and other additives may be an organic solvent unless otherwise specified.
[0072] (4-3) Additives Meanwhile, the additive may include a compound represented by the following Chemical Formula 1:
[0073] [ka]
[0074] In the above Chemical Formula 1, R 1 ~R 3 are each independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.
[0075] As mentioned above, in the case of a negative electrode containing a silicon-based negative active material, the SEI film containing a large amount of oxygen (O)-rich components is formed on the surface of the negative electrode by reaction with the electrolyte. Therefore, in order to stably maintain such an SEI film, it is necessary to add HF or PF to the electrolyte. 5 There is a demand for the use of additives capable of suppressing the generation of such Lewis acids or removing (or scavenging) the generated Lewis acids.
[0076] The compound represented by the formula 1 has a phosphonate (-PO(OR) 2 ) group, a coating of an inorganic component can be formed on the surface of the negative electrode containing a silicon-based negative electrode active material, thereby preventing the decomposition of Si by HF and the resulting capacity loss, and mitigating the electrolyte consumption and the increase in coating thickness due to the decomposition and regeneration of the SEI film. In addition, the compound represented by Chemical Formula 1 contains an alkoxy group unsubstituted with fluorine as a terminal group, thereby preventing the terminal group from being detached under high temperature and high potential, and suppressing side reactions due to the detached substituent, such as gas generation. In addition, the compound represented by Chemical Formula 1 contains a cyanide (-CN) functional group in the structure, thereby forming a ligand with a transition metal to form a stable CEI film on the surface of the positive electrode, thereby preventing side reactions between the positive electrode and the electrolyte and suppressing metal elution during high-temperature storage.
[0077] Therefore, by using a non-aqueous electrolyte containing the compound represented by Formula 1 as a non-aqueous electrolyte additive, a lithium secondary battery having excellent cycle characteristics and high temperature storage stability can be manufactured.
[0078] On the other hand, in formula 1, R 1 ~R 3 However, when each of the alkyl groups has more than 10 carbon atoms, the solubility in an organic solvent may increase due to an increase in the molecular structure and molecular weight of the compound, and the electrolyte viscosity may increase, resulting in a decrease in electrolyte impregnation. 1 ~R 3However, independently, in the case of alkyl groups having more than 10 carbon atoms, there is a possibility that the amount of gas generated may increase during the additive decomposition reaction in which oxygen-phosphorus bonds, oxygen-carbon bonds, or carbon-carbon bonds are broken during charging and discharging.
[0079] Specifically, in the above Chemical Formula 1, the R 1 ~R 3 may each independently be an alkyl group having 1 to 8 carbon atoms. In addition, the R 1 is an alkyl group having 1 to 5 carbon atoms, 2 ~R 3 may each independently be an alkyl group having 2 to 6 carbon atoms. In addition, the R 1 is an alkyl group having 1 to 3 carbon atoms, 2 ~R 3 may each independently be an alkyl group having 2 to 5 carbon atoms.
[0080] More specifically, the compound represented by Chemical Formula 1 may include a compound represented by Chemical Formula 1a below.
[0081] [ka]
[0082] Meanwhile, the compound of Formula 1 may be included in an amount of 0.1 wt % to 5.0 wt % based on the total weight of the nonaqueous electrolyte.
[0083] When the compound represented by Formula 1 is contained within the above range, it is possible to manufacture a secondary battery with improved performance by forming a strong coating on the negative and positive electrodes while preventing side reactions caused by additives and effectively preventing deterioration of the negative electrode during rapid charging and discharging. Specifically, when the content of the compound represented by Formula 1 is 0.1 wt % or more, HF or PF is not generated during the battery operating time. 5The effect of removing the thermal decomposition products of the lithium salt such as 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 112, 123, 131, 142, 143, 154, 155, 165, 170, 171, 182, 193, 194, 195, 196, 197, 198, 199, 200, 20
[0084] More specifically, the compound represented by Chemical Formula 1 may be included in an amount of 0.1% by weight to 3.0% by weight, more preferably 0.3% by weight to 1.0% by weight.
[0085] (4-4) Other additives Meanwhile, the non-aqueous electrolyte may further include other additives in the non-aqueous electrolyte as needed to prevent the non-aqueous electrolyte from decomposing in a high-power environment, thereby causing the collapse of the negative electrode, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and battery expansion suppression effects at high temperatures.
[0086] Representative examples of such other additives include at least one selected from the group consisting of cyclic carbonate-based compounds, halogen-substituted carbonate-based compounds, sultone-based compounds, sulfate-based compounds, phosphate-based compounds, borate-based compounds, nitrile-based compounds, benzene-based compounds, amine-based compounds, silane-based compounds, and lithium salt-based compounds.
[0087] The cyclic carbonate compound may be vinylene carbonate (VC) or vinyl ethylene carbonate.
[0088] The halogen-substituted carbonate compound may be fluoroethylene carbonate (FEC).
[0089] The sultone compound may be at least one compound selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone, ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.
[0090] The sulfate-based compound may be ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyltrimethylene sulfate (MTMS).
[0091] The phosphate-based compound may be one or more compounds selected from the group consisting of lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tris(trimethylsilyl)phosphate, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphate.
[0092] Examples of the borate-based compound include tetraphenylborate and lithium oxalyl difluoroborate.
[0093] The nitrile compound may be at least one compound selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile.
[0094] The benzene-based compound may be fluorobenzene, the amine-based compound may be triethanolamine or ethylenediamine, and the silane-based compound may be tetravinylsilane.
[0095] The lithium salt-based compound is a compound different from the lithium salt contained in the non-aqueous electrolyte, and is LiPO 2 F 2 , LiODFB, LiBOB (Lithium Bis(oxalato)borate (LiB(C 2 O 4 ) 2 ), and LiBF 4 The compound may be one or more compounds selected from the group consisting of:
[0096] Among these other additives, when vinylene carbonate, vinyl ethylene carbonate, or succinonitrile is contained, a stronger SEI film can be formed on the negative electrode surface during the initial activation process of the secondary battery.
[0097] The other additives may be used in combination of two or more kinds, and may be included in an amount of 50% by weight or less, specifically 0.01% by weight to 10% by weight, and preferably 0.05% by weight to 5.0% by weight, based on the total weight of the non-aqueous electrolyte. If the content of the other additives is less than 0.01% by weight, the effect of improving the low-temperature output and high-temperature storage characteristics and high-temperature life characteristics of the battery is small, and if the content of the other additives is more than 50% by weight, side reactions may occur excessively in the electrolyte during charging and discharging of the battery. In particular, when the SEI film forming additive is added in an excessive amount, it may not be fully decomposed at high temperatures and may remain unreacted or precipitated in the electrolyte at room temperature. This may cause side reactions that reduce the life or resistance characteristics of the secondary battery.
[0098] Meanwhile, the lithium secondary battery of the present invention may be manufactured by a conventional method known in the art. Specifically, an electrode assembly in which a positive electrode, a negative electrode, and a separator are sequentially stacked between the positive electrode and the negative electrode are formed, and the electrode assembly is housed in a battery case, and then the nonaqueous electrolyte is injected into the battery case to manufacture the lithium secondary battery.
[0099] The external shape of the lithium secondary battery according to the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.
[0100] In addition, the lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but also as a unit battery for a medium- to large-sized battery module including a number of battery cells. Specifically, the lithium secondary battery according to the present invention can be usefully used in portable devices such as mobile phones, notebook computers, and digital cameras, and in electric vehicles such as hybrid electric vehicles (HEVs).
[0101] Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the present invention. However, the examples according to the present invention may be modified in various different forms, and the scope of the present invention should not be construed as being limited to the following examples. The examples of the present invention are provided to more completely explain the present invention to those having ordinary skill in the art.
[0102] Working Example Example 1. (Production of non-aqueous electrolyte) LiPF was added to an organic solvent consisting of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 30:70. 6 After dissolving the compound represented by Formula 1a to a concentration of 1.0M, 0.1 wt % of the compound represented by Formula 1a, 1.0 wt % of vinylene carbonate (VC), and 0.5 wt % of 1,3-propane sultone (PS) were added to prepare a non-aqueous electrolyte (see Table 1 below).
[0103] (Secondary battery manufacturing) The positive electrode active material particles were prepared using lithium nickel-cobalt-manganese oxide (Li(Ni 0.8 Co 0.1 Mn 0.1 )O 2 A positive electrode slurry (solid content 85.0 wt%) was prepared by adding the above-mentioned cation exchange resin, carbon black as a conductive material, and polyvinylidene fluoride as a binder in a weight ratio of 97.5:1:1.5 to a solvent, N-methyl-2-pyrrolidone (NMP). The positive electrode slurry was applied to a positive electrode current collector (aluminum thin film) having a thickness of 15 μm, dried, and roll pressed to prepare a positive electrode.
[0104] Anode active material (graphite and SiO = 95:5 weight ratio), binder (SBR-CMC), and conductive material (carbon black) were added to water as a solvent in a weight ratio of 95:3.5:1.5 to prepare anode slurry (solid content: 60 wt%). The anode slurry was applied to a copper (Cu) thin film as anode current collector with a thickness of 6 μm, dried, and then roll pressed to prepare anode.
[0105] A porous polypropylene separator was interposed between the positive and negative electrodes to prepare an electrode assembly, which was then housed in a battery case and the non-aqueous electrolyte was injected into the battery case to prepare a lithium secondary battery.
[0106] Example 2. In non-aqueous organic solvents, LiPF 6 A lithium secondary battery was manufactured in the same manner as in Example 1, except that a non-aqueous electrolyte solution was prepared by dissolving the compound represented by Formula 1a in an amount of 0.5 wt %, vinylene carbonate (VC) in an amount of 1.0 wt %, and 1,3-propane sultone (PS) in an amount of 0.5 wt % (see Table 1 below).
[0107] Example 3. In non-aqueous organic solvents, LiPF 6A lithium secondary battery was manufactured in the same manner as in Example 1, except that a non-aqueous electrolyte solution was prepared by dissolving the compound represented by Formula 1a in an amount of 1.0 wt %, vinylene carbonate (VC) in an amount of 1.0 wt %, and 1,3-propane sultone (PS) in an amount of 0.5 wt % (see Table 1 below).
[0108] Example 4. In non-aqueous organic solvents, LiPF 6 A lithium secondary battery was manufactured in the same manner as in Example 1, except that a non-aqueous electrolyte solution was prepared by dissolving the compound represented by Formula 1a in an amount of 5.0 wt %, vinylene carbonate (VC) in an amount of 1.0 wt %, and 1,3-propane sultone (PS) in an amount of 0.5 wt % (see Table 1 below).
[0109] Example 5. In non-aqueous organic solvents, LiPF 6 A lithium secondary battery was manufactured in the same manner as in Example 1, except that a non-aqueous electrolyte solution was prepared by dissolving the compound represented by Formula 1a in an amount of 6.0 wt %, vinylene carbonate (VC) in an amount of 1.0 wt %, and 1,3-propane sultone (PS) in an amount of 0.5 wt % (see Table 1 below).
[0110] Comparative Example 1 In non-aqueous organic solvents, LiPF 6 A lithium secondary battery was manufactured in the same manner as in Example 1, except that a non-aqueous electrolyte solution was prepared by adding 1.0 wt % vinylene carbonate (VC) and 0.5 wt % 1,3-propane sultone (PS) as additives (see Table 1 below).
[0111] Comparative Example 2 In non-aqueous organic solvents, LiPF 6A lithium secondary battery was manufactured in the same manner as in Example 2, except that a non-aqueous electrolyte solution was prepared by adding 0.5 wt % of a compound represented by the following Formula 3 instead of the compound represented by Formula 1a as an additive (see Table 1 below).
[0112] [ka]
[0113] Comparative Example 3. In non-aqueous organic solvents, LiPF 6 A lithium secondary battery was manufactured in the same manner as in Example 3, except that a non-aqueous electrolyte solution was prepared by adding 1.0 wt % of the compound represented by Formula 3 instead of the compound represented by Formula 1a as an additive (see Table 1 below).
[0114] Comparative Example 4. (manufacturing lithium secondary batteries) The positive electrode active material particles were prepared using lithium nickel-cobalt-manganese oxide (Li(Ni 0.8 Co 0.1 Mn 0.1 )O 2 A positive electrode slurry (solid content 85.0 wt%) was prepared by adding the above-mentioned cation exchange resin, carbon black as a conductive material, and polyvinylidene fluoride as a binder in a weight ratio of 97.5:1:1.5 to a solvent, N-methyl-2-pyrrolidone (NMP). The positive electrode slurry was applied to a positive electrode current collector (aluminum thin film) having a thickness of 15 μm, dried, and roll pressed to prepare a positive electrode.
[0115] Anode active material (graphite), binder (SBR-CMC), and conductive material (carbon black) were mixed in a weight ratio of 95:3.5:1.5 to water as a solvent to prepare anode slurry (solid content: 60 wt%). The anode slurry was applied to a 6 μm-thick copper (Cu) thin film as anode current collector, dried, and then roll pressed to prepare anode.
[0116] An electrode assembly was prepared by interposing a porous polypropylene separator between the prepared positive and negative electrodes, and then the electrode assembly was housed in a battery case. Thereafter, a lithium secondary battery was manufactured in the same manner as in Example 1, except that the nonaqueous electrolyte solution prepared in Example 3 was injected.
[0117] [Table 1]
[0118] Meanwhile, the abbreviations of the compounds in Table 1 have the following meanings. EC: Ethylene carbonate EMC: Ethyl methyl carbonate VC: Vinylene carbonate PS: 1,3-propane sultone
[0119] Experimental Example Experimental example 1. Performance evaluation after high-temperature storage The lithium secondary batteries of Examples 1 to 5 and Comparative Examples 1 to 4 were each charged at 0.2 C to 4.2 V in CC-CV mode, and then stored in a chamber at 60° C. for 30 days. The OCV was measured before storage, and then measured after 30 days of storage, and the change in OCV was expressed as dOCV. Next, each secondary battery was discharged at 0.2 C to 2.5 V in CC mode, and gas was extracted. The total amount of gas generated after high-temperature storage is shown in Table 2 below as the amount of gas generated. [Table 2]
[0120] From Table 2, it can be seen that the secondary batteries of Examples 1 to 5 using the non-aqueous electrolyte solution containing the compound of Formula 1a had reduced dOCV and gas generation amount compared to the secondary battery of Comparative Example 1.
[0121] In addition, when comparing the secondary batteries of Examples 2 and 3 containing the same amount of additive with the secondary batteries of Comparative Examples 2 and 3, it can be seen that the dOCV and gas generation amount of the secondary batteries of Examples 2 and 3, which use the non-aqueous electrolyte containing the compound of Chemical Formula 1a of the present invention, are reduced compared to the secondary batteries of Comparative Examples 2 and 3.
[0122] Considering these results, it can be confirmed that the compound of Formula 1a of the present invention forms a stable coating on the surface of the negative electrode and the positive electrode, thereby suppressing side reactions of the electrolyte during high-temperature storage, thereby reducing dOCV and gas generation.
[0123] In addition, when comparing the secondary battery of Example 3, which has a nonaqueous electrolyte containing the same amount of additive, with the secondary battery of Comparative Example 4, it can be seen that the secondary battery of Example 3 of the present invention, which uses a negative electrode containing a silicon-based negative electrode active material, has a reduced dOCV compared to the secondary battery of Comparative Example 4, and thus has an improved effect of suppressing the amount of gas generation.
[0124] Experimental example 2. Performance evaluation after rapid charging and discharging The lithium secondary batteries of Examples 1 to 5 and the lithium secondary batteries of Comparative Examples 1 to 4 were charged in CC-CV mode at 3 C to 4.2 V and discharged in CC mode at 0.2 C to 2.5 V as one cycle, and then rapid charge and discharge was carried out for 100 cycles. After that, the capacity retention rate (%) and the resistance increase rate (%) were calculated, and the results are shown in Table 3 below.
[0125] [Table 3]
[0126] From Table 3, it can be seen that the secondary batteries of Examples 1 to 4 using the nonaqueous electrolyte solution containing the compound of Formula 1a have a better capacity retention rate and a reduced resistance increase rate after rapid charging and discharging compared to the secondary battery of Comparative Example 1.
[0127] On the other hand, in the case of the secondary battery of Example 5 having a nonaqueous electrolyte containing a somewhat large amount of additive, it can be confirmed that the capacity retention rate is somewhat decreased and the resistance increase rate is somewhat increased compared to the secondary batteries of Examples 1 to 4 due to side reactions of the additive.
[0128] Meanwhile, when comparing the secondary batteries of Examples 2 and 3 containing the same amount of additives with the secondary batteries of Comparative Examples 2 and 3, it can be seen that the secondary batteries of Examples 2 and 3, which use the non-aqueous electrolyte containing the compound of Chemical Formula 1a of the present invention, have a higher capacity retention rate and a lower resistance increase rate after rapid charging and discharging than the secondary batteries of Comparative Examples 2 and 3.
[0129] In addition, when comparing the secondary battery of Example 3, which has a nonaqueous electrolyte containing the same amount of additive, with the secondary battery of Comparative Example 4, it can be seen that the capacity retention rate after rapid charging and discharging is increased and the resistance increase rate is decreased in the case of the secondary battery of Example 3 of the present invention, which uses a negative electrode containing a silicon-based negative electrode active material, compared to the secondary battery of Comparative Example 4.
Claims
1. A positive electrode and a negative electrode including a silicon-based negative electrode active material; a separator interposed between the positive electrode and the negative electrode; a non-aqueous electrolyte solution including a lithium salt, an organic solvent, and an additive; The additive comprises a compound represented by the following formula 1: [Formula 1] In the above Chemical Formula 1, R 1 ~R 3 are each independently a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.
2. The silicon-based negative electrode active material is silicon, silicon chloride, silicon oxide (SiO x 2. The lithium secondary battery according to claim 1, wherein the material is at least one selected from the group consisting of: (0<x<2)) and silicon-carbon composite (SiC).
3. 3. The lithium secondary battery according to claim 2, wherein the silicon-based negative electrode active material is silicon oxide (SiO).
4. The silicon oxide (SiO) is silicon dioxide (SiO 2 4. The lithium secondary battery according to claim 3, wherein the weight ratio of the amorphous silicon to the amorphous silicon is 1:
1.
5. The lithium secondary battery according to claim 1 , wherein the negative electrode further comprises a carbon-based negative electrode active material.
6. 6. The lithium secondary battery according to claim 5, wherein the mixing ratio of the silicon-based negative electrode active material and the carbon-based negative electrode active material is 1:99 to 20:80 by weight.
7. 6. The lithium secondary battery according to claim 5, wherein the mixing ratio of the silicon-based negative electrode active material and the carbon-based negative electrode active material is 1:99 to 10:90 by weight.
8. 2. The lithium secondary battery according to claim 1, wherein the positive electrode comprises a positive electrode active material including lithium and at least one metal selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), and aluminum (Al).
9. The R 1 ~R 3 and each independently represent an alkyl group having 1 to 8 carbon atoms.
10. The R 1 is an alkyl group having 1 to 5 carbon atoms, The R 2 ~R 3 and each independently represent an alkyl group having 2 to 6 carbon atoms.
11. The R 1 is an alkyl group having 1 to 3 carbon atoms, The R 2 ~R 3 and each independently represent an alkyl group having 2 to 5 carbon atoms.
12. The lithium secondary battery of claim 1 , wherein the compound represented by Chemical Formula 1 is a compound represented by Chemical Formula 1a: [Case 2]
13. The lithium secondary battery according to any one of claims 1 to 11, wherein the compound represented by Chemical Formula 1 is contained in an amount of 0.1 wt % to 5.0 wt % based on the total weight of the non-aqueous electrolyte.
14. 2. The lithium secondary battery of claim 1, wherein the non-aqueous electrolyte further comprises at least one other additive selected from the group consisting of cyclic carbonate-based compounds, halogen-substituted carbonate-based compounds, sultone-based compounds, sulfate-based compounds, phosphate-based compounds, borate-based compounds, nitrile-based compounds, amine-based compounds, silane-based compounds, and lithium salt-based compounds.
Citation Information
Patent Citations
Electrolyte for lithium ion battery and preparation method thereof
CN102637901A
Electrochemical device and electronic device comprising same
EP3907804A1
Non-aqueous electrolyte and lithium-ion batteries
JP2018525802A
Positive electrode, lithium ion secondary battery, positive electrode manufacturing method, and lithium ion secondary battery manufacturing method
JP2021106113A
Electrolyte and lithium secondary battery with the same
KR1020160002315A