The non-aqueous electrolyte additive with an acetimidoyl-silyl structure addresses the deterioration issues in lithium secondary batteries by scavenging HF byproducts and forming a stable SEI film, enhancing high-temperature performance and stability.

JP2024540420AActive Publication Date: 2024-10-31LG ENERGY SOLUTION LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024527224
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-03
Filing Date
2023-08-03
Publication Date
2024-10-31
Estimated Expiration
2043-08-03

AI Technical Summary

Technical Problem

Lithium secondary batteries experience deterioration due to side reactions at the positive electrode, leading to the elution of transition metal ions, degradation of the Solid Electrolyte Interphase (SEI) film on the negative electrode, and swelling at high temperatures, which reduces battery performance and stability.

Method used

Incorporation of a non-aqueous electrolyte additive with an acetimidoyl group connected to a silyl group, which scavenges HF byproducts and forms a stable SEI film on the negative electrode, minimizing resistance and preventing electrode deterioration.

Benefits of technology

The additive enhances the stability of the electrode-electrolyte interface, improving high-temperature cycle and storage characteristics, and maintaining battery performance by reducing resistance and preventing swelling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540420000001_ABST
    Figure 2024540420000001_ABST
Patent Text Reader

Abstract

The present invention provides a non-aqueous electrolyte comprising a lithium salt, an organic solvent, and a compound represented by the following Chemical Formula 1 as an additive: JPEG2024540420000018.jpg41170 (In the above Chemical Formula 1, R1 is any one selected from the group consisting of an alkyl group having 1 to 5 carbon atoms, in which a hydrogen atom may be substituted with a fluorine atom, an aryl group having 6 to 8 carbon atoms, in which a hydrogen atom may be substituted with a fluorine atom, and a nitrile group, and R2 to R4 may each independently be an alkyl group having 1 to 5 carbon atoms.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0097613, filed on August 14, 2022, and all contents disclosed in the documents of that Korean patent application are incorporated as part of this specification.

[0002] The present invention relates to a non-aqueous electrolyte and a lithium secondary battery containing the same. [Background technology]

[0003] In recent years, the application fields of lithium secondary batteries have expanded to various technical fields, and accordingly, there is an increasing demand for secondary batteries with high capacity, high output, and high stability.

[0004] In particular, when a secondary battery is operated at a high voltage to increase its capacity, as charging and discharging proceeds, the coating formed on the surface of the positive / negative electrode or the structure of the electrode surface may deteriorate due to side reactions caused by the deterioration of the electrolyte, and transition metal ions may be eluted from the surface of the positive electrode. In this way, the eluted transition metal ions are electro-deposited on the negative electrode, which reduces the passivation ability of the SEI, causing the problem of the negative electrode being deteriorated.

[0005] Such deterioration of the secondary battery tends to be accelerated when the potential of the positive electrode is increased or when the battery is exposed to high temperatures.

[0006] In addition, when a lithium-ion battery is used continuously for a long period of time or left at high temperatures, gas is generated and the thickness of the battery increases, a phenomenon known as swelling. It is known that the amount of gas generated at this time depends on the state of the SEI.

[0007] Therefore, in order to solve such problems, research and development is being conducted on a method that can suppress the elution of metal ions in the positive electrode, form a stable SEI film in the negative electrode, reduce the swelling phenomenon of the secondary battery, and increase the stability at high temperatures. Summary of the Invention [Problem to be solved by the invention]

[0008] As a result of conducting extensive research to solve the above problems, an objective of the present invention is to provide an additive for a non-aqueous electrolyte that can suppress deterioration of a positive electrode, reduce side reactions between a positive electrode and an electrolyte, and form a stable SEI film on a negative electrode.

[0009] Another object of the present invention is to provide a non-aqueous electrolyte that contains the additive for a non-aqueous electrolyte and thereby has improved stability at high temperatures.

[0010] Another object of the present invention is to provide a lithium secondary battery containing the non-aqueous electrolyte, which has improved high-temperature cycle characteristics and high-temperature storage characteristics and thus improved performance. [Means for solving the problem]

[0011] In order to achieve the above object, one embodiment of the present invention provides a non-aqueous electrolyte comprising an additive for a non-aqueous electrolyte represented by the following Chemical Formula 1:

[0012] [ka]

[0013] In the above formula 1, R 1 is any one selected from the group consisting of an alkyl group having 1 to 5 carbon atoms, a hydrogen atom of which may be substituted with a fluorine atom, an aryl group having 6 to 8 carbon atoms, a hydrogen atom of which may be substituted with a fluorine atom, and a nitrile group; R 2 ~R 4 may each independently be an alkyl group having 1 to 5 carbon atoms.

[0014] In addition, an embodiment of the present invention provides a lithium secondary battery including the non-aqueous electrolyte. Effect of the Invention

[0015] HF, which is generated as a by-product when a secondary battery is operated, accelerates the breakdown of the positive and negative electrodes, which reduces the life and storage characteristics of the secondary battery, causing problems such as swelling of the secondary battery.

[0016] The compound represented by Formula 1, which is provided as an additive for a non-aqueous electrolyte according to the present invention, contains an acetimidoyl group linked to a silyl group in the structure. That is, the compound represented by Formula 1 according to the present invention has a CF 3 The presence of this group and its high bond energy with HF allows for effective scavenging of HF.

[0017] In addition, the compound represented by Formula 1 can minimize an increase in the resistance of a lithium secondary battery and form a stable SEI (Solid Electrolyte Interphase) film on the surface of the negative electrode. Therefore, the decrease in the passivation ability of the SEI at high temperatures can be suppressed, and deterioration of the negative electrode can be prevented, thereby improving the life characteristics of the battery.

[0018] Therefore, by using the nonaqueous electrolyte of the present invention containing the compound of Chemical Formula 1, an electrode-electrolyte interface that is stable even at high temperatures and has low resistance can be formed, thereby improving the high-temperature cycle characteristics and high-temperature storage characteristics, and realizing a lithium secondary battery with improved performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0020] As used herein, terms such as "comprise," "comprise," or "have" are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, but should not be understood as precluding the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.

[0021] In the present specification, in the description of "number of carbon atoms a to b," "a" and "b" refer to the number of carbon atoms contained in a specific functional group. That is, the functional group may contain "a" to "b" carbon atoms. For example, "an alkylene group having 1 to 5 carbon atoms" refers to an alkylene group containing 1 to 5 carbon atoms, i.e., -CH 2 -, -CH 2 CH 2 -, -CH 2 CH 2 CH 2 -, -CH 2 (CH 3 )CH-, -CH(CH 3 )CH 2 - and -CH(CH 3 )CH 2 CH 2 - etc.

[0022] In addition, in this specification, the alkyl group may be either substituted or unsubstituted. The term "substituted" means that at least one hydrogen bonded to a carbon atom is substituted with an element other than hydrogen, and means that the alkyl group has 1 to 20 carbon atoms, the alkenyl group has 2 to 20 carbon atoms, the alkynyl group has 2 to 20 carbon atoms, the alkoxy group has 1 to 20 carbon atoms, the cycloalkyl group has 3 to 12 carbon atoms, the cycloalkenyl group has 3 to 12 carbon atoms, the heterocycloalkyl group has 3 to 12 carbon atoms, the heterocycloalkenyl group has 3 to 12 carbon atoms, the aryloxy group has 6 to 12 carbon atoms, a halogen atom, a fluoroalkyl group has 1 to 20 carbon atoms, a nitro group, an aryl group has 6 to 20 carbon atoms, a haloaryl group has 6 to 20 carbon atoms, or the like.

[0023] The present invention will now be described in more detail.

[0024] Nonaqueous electrolyte The non-aqueous electrolyte according to the present invention contains, as an additive, a compound represented by the following chemical formula 1. A lithium secondary battery using a non-aqueous electrolyte containing the additive of the present invention is suppressed from deteriorating due to an interfacial reaction at high temperatures, and can have excellent high-temperature cycle characteristics and high-temperature storage characteristics.

[0025] [ka]

[0026] The compound of Formula 1 has a high bond energy with HF due to the presence of an acetimidoyl group linked to a silyl group in the structure, and therefore can effectively scavenge HF.

[0027] In addition, the compound of Formula 1 can minimize an increase in the resistance of a lithium secondary battery and form a stable LiF-containing SEI (Solid Electrolyte Interphase) film on the surface of the negative electrode, thereby preventing the deterioration of the negative electrode by suppressing the decrease in the passivation ability of the SEI at high temperatures.

[0028] In the above formula 1, R 1 may be any one selected from the group consisting of an alkyl group having 1 to 5 carbon atoms in which a hydrogen atom may be substituted with a fluorine atom, an aryl group having 6 to 8 carbon atoms in which a hydrogen atom may be substituted with a fluorine atom, and a nitrile group.

[0029] In addition, in the above-mentioned chemical formula 1, R 2 ~R 4 may each independently be an alkyl group having 1 to 5 carbon atoms.

[0030] Specifically, in the above formula 1, R 1 CF 3 Alternatively, the compound of Chemical Formula 1 may be a compound represented by the following Chemical Formula 1-1:

[0031] [ka]

[0032] In the above Chemical Formula 1-1, R 2 ~R 4 may each independently be an alkyl group having 1 to 5 carbon atoms.

[0033] In addition, in the above-mentioned chemical formula 1-1, R 6 ~R 10 may each independently be H or F. Preferably, R 6 ~R 10 When at least one of the groups is F, a better HF scavenging effect can be obtained.

[0034] Specifically, the compound of the present invention represented by Chemical Formula 1 may be any one selected from the group consisting of the following Chemical Formulae 1a to 1c.

[0035] [ka]

[0036] [ka]

[0037] [ka]

[0038] The additive for non-aqueous electrolyte according to the present invention may be included in an amount of 0.1 to 4 parts by weight, preferably 0.1 to 2.5 parts by weight, and more preferably 0.2 to 1.5 parts by weight, relative to 100 parts by weight of the non-aqueous electrolyte. When the content of the compound represented by Chemical Formula 1 satisfies the above range, a sufficient amount of SEI can be formed, the viscosity of the electrolyte can be maintained at an appropriate level, and there are effects of excellent rate characteristics and capacity characteristics during high-temperature storage.

[0039] The lithium salt contained in the non-aqueous electrolyte of the present invention is used as an electrolyte salt in a lithium secondary battery and is used as a medium for transferring ions. + and as an anion, F - , Cl - , Br - , I - , NO 3 - , N(CN) 2 - , B.F. 4 - , ClO 4 - , B 10 Cl 10 - , AlCl 4 - , AlO2 - 、PF 6 - 、CF 3 SO 3 - 、CH 3 CO 2 - 、CF 3 CO 2 - 、AsF 6 - 、SbF 6 - 、CH 3 SO 3 - 、(CF 3 CF 2 SO 2 ) 2 N - 、(CF 3 SO 2 ) 2 N - 、(FSO 2 ) 2 N - 、BF 2 C 2 O 4 - 、BC 4 O 8 - 、PF 4 C 2 O 4 - 、PF 2 C 4 O 8 - 、(CF 3 ) 2 PF 4 - 、(CF 3 ) 3 PF 3 - 、(CF 3 ) 4 PF 2 - 、(CF 3 ) 5 PF - 、(CF 3 ) 6 P - 、C 4 F 9 SO 3- , C.F. 3 CF 2 SO 3 - , C.F. 3 CF 2 (CF 3 ) 2 CO - , (CF 3 SO 2 ) 2 CH - , C.F. 3 (CF 2 ) 7 SO 3 - , and SCN - At least one selected from the group consisting of:

[0040] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF 4 , LiClO 4 , LiB 10 Cl 10 , LiAlCl 4 , LiAlO 2 , LiPF 6 , LiCF 3 SO 3 , LiCH 3 CO 2 , LiCF 3 CO 2 , LiAsF 6 , LiSbF 6 , LiCH 3 SO 3 , LiN(SO 2 F) 2 (Lithium bis(fluorosulfonyl)imide; LiFSI), LiN(SO 2 CF 2 CF 3 ) 2 (lithium bis(perfluoroethanesulfonyl)imide; LiBETI), and LiN(SO 2 CF 3 ) 2(lithium bis(trifluoromethanesulfonyl)imide; LiTFSI), or a mixture of two or more thereof. In addition to these, lithium salts that are commonly used in electrolytes for lithium secondary batteries can be used without any restrictions.

[0041] The lithium salt may be appropriately changed within a range that is normally usable, but in order to obtain an optimal effect of forming a corrosion prevention coating on the electrode surface, it may be contained in the electrolyte at a concentration of 0.5 M to 3 M, preferably a concentration of 0.5 M to 2.5 M, and more preferably a concentration of 0.8 M to 2 M. When the concentration of the lithium salt satisfies the above range, the effect of improving the cycle characteristics during high-temperature storage of the lithium secondary battery is sufficient, and the viscosity of the non-aqueous electrolyte is appropriate, so that the electrolyte impregnation can be improved.

[0042] The organic solvent contained in the nonaqueous electrolyte of the present invention may include at least one organic solvent selected from the group consisting of cyclic carbonate organic solvents, linear carbonate organic solvents, linear ester organic solvents, and cyclic ester organic solvents.

[0043] Specifically, the organic solvent may include a cyclic carbonate organic solvent, a linear carbonate organic solvent, or a mixture thereof.

[0044] The cyclic carbonate organic solvent is a high-viscosity organic solvent that has a high dielectric constant and therefore easily dissociates the lithium salt in the electrolyte. Specific examples of the cyclic carbonate organic solvent include at least one organic solvent selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and among these, ethylene carbonate may be included.

[0045] The linear carbonate organic solvent is an organic solvent having low viscosity and low dielectric constant, and a representative example thereof may be at least one organic solvent selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and specifically may include ethyl methyl carbonate (EMC).

[0046] In addition, in order to produce an electrolyte having high ionic conductivity, the organic solvent may further contain at least one or more ester-based organic solvents selected from the group consisting of linear ester-based organic solvents and cyclic ester-based organic solvents in addition to the at least one or more carbonate-based organic solvents selected from the group consisting of cyclic carbonate-based organic solvents and linear carbonate-based organic solvents.

[0047] Specific examples of such linear ester-based organic solvents include at least one organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.

[0048] The cyclic ester organic solvent may be at least one organic solvent selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.

[0049] Meanwhile, the organic solvent may be any organic solvent commonly used in non-aqueous electrolytes without limitation, if necessary, and may further include at least one of an ether-based organic solvent, a glyme-based solvent, and a nitrile-based organic solvent.

[0050] The ether solvent may be any one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, 1,3-dioxolane (DOL), and 2,2-bis(trifluoromethyl)-1,3-dioxolane (TFDOL), or a mixture of two or more of these, but is not limited thereto.

[0051] The glyme-based solvent has a higher dielectric constant and lower surface tension than linear carbonate-based organic solvents and is less reactive with metals, and may include at least one selected from the group consisting of dimethoxyethane (glyme, DME), diethoxyethane, diglyme, triglyme, and tetraglyme (TEGDME), but is not limited thereto.

[0052] The nitrile-based solvent may be one or more selected from the group consisting of acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile, but is not limited thereto.

[0053] The non-aqueous electrolyte of the present invention may further contain fluoroethylene carbonate (FEC) in order to improve the life characteristics at high voltage. The fluoroethylene carbonate (FEC) may be contained in an amount of 1 to 30 parts by weight, preferably 5 to 15 parts by weight, per 100 parts by weight of the non-aqueous electrolyte.

[0054] In addition, the nonaqueous electrolyte of the present invention may contain the compound of Formula 1 and fluoroethylene carbonate in a weight ratio of 1:1 to 1:30, preferably 1:2 to 1:25, and more preferably 1:3 to 1:15. When the compound of Formula 1 and fluoroethylene carbonate are contained in the above relative ratio, the effect of improving the life at high voltage and the effect of improving storage characteristics can be maximized.

[0055] In addition to the fluoroethylene carbonate, the non-aqueous electrolyte of the present invention may further contain a known electrolyte additive, as necessary, in order to prevent the non-aqueous electrolyte from being decomposed in a high-output environment, which would cause the collapse of the negative electrode, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and the effect of suppressing battery expansion at high temperatures.

[0056] Representative examples of such other electrolyte additives may include at least one SEI film-forming additive selected from the group consisting of cyclic carbonate-based compounds, sultone-based compounds, sulfate-based compounds, phosphate-based compounds, borate-based compounds, nitrile-based compounds, benzene-based compounds, amine-based compounds, silane-based compounds, and lithium salt-based compounds.

[0057] Examples of the cyclic carbonate compounds include vinylene carbonate (VC) and vinyl ethylene carbonate.

[0058] The sultone compound includes at least one compound selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone, ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.

[0059] Examples of the sulfate-based compounds include ethylene sulfate (Esa), trimethylene sulfate (TMS), and methyl trimethylene sulfate (MTMS).

[0060] The phosphate-based compound may be one or more compounds selected from the group consisting of lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tetramethyltrimethylsilylphosphate, trimethylsilylphosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite.

[0061] The borate-based compounds include tetraphenylborate, lithium oxalyl difluoroborate (LiODFB), lithium bis(oxalate) borate (LiB(C 2 O 4 ) 2 , LiBOB).

[0062] The nitrile compound may be at least one compound selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile.

[0063] The benzene-based compound may be fluorobenzene, the amine-based compound may be triethanolamine or ethylenediamine, and the silane-based compound may be tetravinylsilane.

[0064] The lithium salt-based compound is a compound different from the lithium salt contained in the non-aqueous electrolyte, and may be lithium difluorophosphate (LiDFP), LiPO 2 F 2 , or LiBF 4 etc.

[0065] Among these other electrolyte additives, a combination of vinylene carbonate (VC), 1,3-propane sultone (PS), and ethylene sulfate (Esa) can form a stronger SEI film on the surface of the negative electrode during the initial activation process of the secondary battery, suppress the generation of gas that may be generated by decomposition of the electrolyte at high temperatures, and improve the high-temperature stability of the secondary battery.

[0066] On the other hand, the other electrolyte additives may be used in combination of two or more kinds, and may be included in an amount of 0.1 to 10 wt%, specifically 0.2 to 8 wt%, and preferably 0.5 to 8 wt%, based on the total weight of the non-aqueous electrolyte. When the content of the other electrolyte additives satisfies the above range, better ion conductivity and cycle characteristic improvement effects can be obtained.

[0067] Lithium secondary battery The present invention also provides a lithium secondary battery containing the non-aqueous electrolyte.

[0068] Specifically, the lithium secondary battery includes a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, a separator interposed between the positive electrode and the negative electrode, and the nonaqueous electrolyte described above.

[0069] In this regard, the lithium secondary battery of the present invention may be manufactured by a conventional method known in the art, for example, by forming an electrode assembly in which a positive electrode, a negative electrode, and a separator are sequentially stacked between the positive electrode and the negative electrode, and then inserting the electrode assembly into a battery case and injecting the non-aqueous electrolyte according to the present invention into the battery case.

[0070] The lithium secondary battery of the present invention has a driving voltage of 4.47 V or more and can be driven at a high voltage.

[0071] (1) Positive electrode The positive electrode can be manufactured by coating a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive material, a solvent, etc. on a positive electrode current collector.

[0072] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel, aluminum, nickel, titanium, fired carbon, or a material obtained by surface treatment with carbon, nickel, titanium, silver, etc. on the surface of aluminum or stainless steel may be used.

[0073] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically, may include a lithium metal oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum and lithium. More specifically, the lithium metal oxide is a lithium-manganese-based oxide (e.g., LiMnO 2 、LiMn 2 O 4 etc.), lithium-cobalt-based oxide (e.g., LiCoO 2 etc.), lithium-nickel-based oxide (e.g., LiNiO 2 etc.), lithium-nickel-manganese-based oxide (e.g., LiNi 1-Y Mn Y O 2 (where 0 < Y < 1), LiMn 2-Z Ni Z O 4 (where 0 < Z < 2), etc.), lithium-nickel-cobalt-based oxide (e.g., LiNi 1-Y1 Co Y1 O 2 (where 0 < Y1 < 1), etc.), lithium-manganese-cobalt-based oxide (e.g., LiCo 1-Y2 Mn Y2 O 2 (where 0 < Y2 < 1), LiMn2-Z1 Co Z1 O 4 (where 0 < Z1 < 2, etc.), lithium-nickel-manganese-cobalt-based oxides (e.g., Li(Ni p Co q Mn r )O 2 (where 0 < p < 1, 0 < q < 1, 0 < r < 1, p + q + r = 1) or Li(Ni p1 Co q1 Mn r1 )O 4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r1 < 2, p1 + q1 + r1 = 2, etc.), or lithium-nickel-cobalt-transition metal (M) oxides (e.g., Li(Ni p2 Co q2 Mn r2 M s2 )O 2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r2, and s2 are the atomic fractions of the respective independent elements, 0 < p2 < 1, 0 < q2 < 1, 0 < r2 < 1, 0 < s2 < 1, and p2 + q2 + r2 + s2 = 1, etc.) and the like, and any one or two or more of these compounds may be included.

[0074] Among them, from the viewpoint of being able to enhance the capacity characteristics and stability of the battery, the lithium metal oxide is LiCoO 2 , LiMnO 2 , LiNiO 2 , lithium nickel manganese cobalt oxide (e.g., Li(Ni 1 / 3 Mn 1 / 3 Co 1 / 3 )O 2 , Li(Ni 0.6 Mn 0.2 Co 0.2 )O 2 , Li(Ni 0.5 Mn 0.3 Co 0.2 )O 2 , Li(Ni 0.7 Mn 0.15 Co 0.15 )O 2 , and Li(Ni 0.8Mn 0.1 Co 0.1 )O 2 ), lithium nickel cobalt aluminum oxide (e.g., Li(Ni 0.8 Co 0.15 Al 0.05 )O 2 ), or lithium nickel manganese cobalt aluminum oxide (e.g., Li(Ni 0.86 Co 0.05 Mn 0.07 Al 0.02 )O 2 ) and the like, and any one or a mixture of two or more of these may be used.

[0075] Among others, the positive electrode active material may be a lithium-cobalt-based oxide represented by the following chemical formula 2.

[0076] [Chemical formula 2] Li a1 Co 1-x1 M 1 x1 O 2+β

[0077] In the above Chemical Formula 2, M 1 contains one or more selected from the group consisting of Al, B, Ba, Ca, Zr, Ti, Mg, Ta, Nb, Sr, W, and Mo, and <a1≦1.1、0≦x1≦0.2、0≦β≦0.02であってよい。

[0078] The positive electrode active material may be contained in an amount of 60 to 99 wt %, preferably 70 to 99 wt %, and more preferably 80 to 98 wt %, based on the total weight of solid matter excluding the solvent in the positive electrode mixture slurry.

[0079] The binder is a component that assists in binding the active material and conductive material and the like to the current collector.

[0080] Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, various copolymers, and the like.

[0081] Generally, the binder may be contained in an amount of 1 to 20% by weight, preferably 1 to 15% by weight, and more preferably 1 to 10% by weight, based on the total weight of solids in the positive electrode mixture slurry excluding the solvent.

[0082] The conductive material is a component for further improving the conductivity of the positive electrode active material, and may be added in an amount of 1 to 20% by weight based on the total weight of the solid content in the negative electrode mixture slurry. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and may be, for example, carbon powder such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive fibers such as carbon fibers and metal fibers; carbon fluoride powder; conductive powder such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives.

[0083] Generally, the conductive material may be contained in an amount of 1 to 20% by weight, preferably 1 to 15% by weight, and more preferably 1 to 10% by weight, based on the total weight of solids excluding the solvent in the positive electrode mixture slurry.

[0084] The solvent may contain an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a suitable viscosity when the positive electrode active material, and optionally a binder and a conductive material, etc. are contained. For example, the solvent may be contained so that the concentration of the solid content including the positive electrode active material, and optionally a binder and a conductive material, is 50 to 95% by weight, preferably 70 to 95% by weight, and more preferably 70 to 90% by weight.

[0085] (2) Negative electrode The negative electrode can be prepared by coating a negative electrode mixture slurry containing a negative electrode active material, a binder, a conductive material, and a solvent on a negative electrode current collector, or a graphite electrode made of carbon (C) or a metal itself can be used as the negative electrode.

[0086] For example, when the negative electrode is manufactured by coating the negative electrode mixture slurry on the negative electrode current collector, the negative electrode current collector generally has a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and for example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. may be used. In addition, as with the positive electrode current collector, the binding force of the negative electrode active material may be strengthened by forming fine irregularities on the surface, and it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric body, etc.

[0087] In addition, the negative electrode active material may include at least one selected from the group consisting of lithium metal, a carbon material capable of reversibly intercalating / deintercalating lithium ions, a metal or an alloy of these metals and lithium, a metal composite oxide, a material capable of doping and dedoping lithium, and a transition metal oxide.

[0088] The carbonaceous material capable of reversibly intercalating / deintercalating lithium ions may be any carbonaceous negative electrode active material commonly used in lithium ion secondary batteries, and representative examples thereof include crystalline carbon, amorphous carbon, or both. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, and calcined coke.

[0089] The metal or the alloy of these metals and lithium may be a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of these metals and lithium.

[0090] The metal composite oxides include PbO, PbO 2 , Pb 2 O 3 , Pb 3 O 4 , Sb 2 O 3 , Sb 2 O 4 , Sb 2 O 5 , GeO, GeO 2 , Bi 2 O 3 , Bi 2 O 4 , Bi 2 O 5 , Li x Fe 2 O 3 (0≦x≦1), Li x WO 2 (0≦x≦1), and Sn x Me 1-x Me' y O z(Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, elements of Group 1, Group 2, Group 3 of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8) can be selected from the group consisting of.

[0091] As the substance capable of doping and undoping lithium, Si, SiO x (0 < x ≦ 2), Si-Y alloy (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO 2 , Sn-Y (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), etc. can be mentioned, and at least one of these and SiO 2 may be mixed and used. The element Y may be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0092] Examples of the transition metal oxide include lithium-containing titanium composite oxide (LTO), vanadium oxide, lithium vanadium oxide, etc.

[0093] Among them, the negative electrode of the present invention may contain any one or more selected from the group consisting of Si, Si-C, and SiO x (0 < x ≦ 2) as the negative electrode active material. Preferably, the negative electrode active material may be a mixture of graphite and SiO x (0 < x ≦ 2). From the viewpoint of increasing the capacity of the lithium secondary battery, the graphite and SiO x (0 < x ≦ 2) may be contained in a weight ratio of 97:3 to 70:30.

[0094] The negative electrode active material may be contained in an amount of 60 to 99% by weight, preferably 70 to 99% by weight, and more preferably 80 to 98% by weight, based on the total weight of the solid content in the negative electrode mixture slurry.

[0095] The binder is a component that assists in binding between the conductive material, the active material, and the current collector. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0096] Generally, the binder may be contained in an amount of 1 to 20% by weight, preferably 1 to 15% by weight, and more preferably 1 to 10% by weight, based on the total weight of solids excluding the solvent in the negative electrode mixture slurry.

[0097] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 1 to 20% by weight based on the total weight of the solid content in the negative electrode mixture slurry. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and may be, for example, carbon powder such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc.

[0098] The conductive material may be contained in an amount of 1 to 20% by weight, preferably 1 to 15% by weight, and more preferably 1 to 10% by weight, based on the total weight of solids excluding the solvent in the negative electrode mixture slurry.

[0099] The solvent may include water or an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a suitable viscosity when the negative electrode active material, and optionally a binder and a conductive material, etc. are included. For example, the solvent may be included so that the concentration of the solid content including the negative electrode active material, and optionally a binder and a conductive material, is 50% by weight to 95% by weight, preferably 70% by weight to 90% by weight.

[0100] When a metal is used as the negative electrode, the negative electrode can be manufactured by physically bonding, rolling, or depositing a metal on a metal thin film or the negative electrode current collector. The deposition method can be an electrical deposition or chemical vapor deposition method.

[0101] For example, the metal thin film itself or the metal bonded / rolled / deposited onto the negative electrode current collector may include one metal or an alloy of two metals selected from the group consisting of lithium (Li), nickel (Ni), tin (Sn), copper (Cu), and indium (In).

[0102] (3) Separator As the separator, a conventional porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, may be used alone or in a laminated state, or a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, etc., may be used, but is not limited thereto. In addition, in order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be selectively used as a single layer or a multilayer structure.

[0103] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0104] The present invention will be described in more detail below with reference to specific examples. However, the following examples are merely illustrative for understanding the present invention and are not intended to limit the scope of the present invention. It is obvious to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present description, and it goes without saying that such changes and modifications belong to the scope of the attached claims.

[0105] Working Example Example 1 (Production of non-aqueous electrolyte) In an organic solvent (ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 30:70 volume ratio), LiPF 6 A non-aqueous solvent was prepared by dissolving the compound represented by the following formula 1a in an amount of 1M, and 10 g of fluoroethylene carbonate (FEC) was added to 89 g of the non-aqueous solvent to prepare a non-aqueous electrolyte.

[0106] [ka]

[0107] (manufacturing lithium secondary batteries) Cathode active material (LiCoO 2 ), conductive material (carbon black), and binder (polyvinylidene fluoride) were added to the solvent N-methyl-2-pyrrolidone (NMP) in a weight ratio of 97.5:1.3:1.2 to prepare a positive electrode slurry (solid content 74 wt%). The positive electrode slurry was applied to one side of a positive electrode current collector (aluminum thin film) with a thickness of 130 μm, and dried and roll pressed to prepare a positive electrode.

[0108] Anode active material (graphite:SiO = 92:8 weight ratio), conductive material (carbon black), and binder (polyvinylidene fluoride) were added to a solvent, N-methyl-2-pyrrolidone (NMP), in a weight ratio of 96.8:0.2:3.0 to prepare anode slurry (solid content 60 wt%). The anode slurry was applied to one side of anode current collector (Cu thin film) with a thickness of 128 μm, and dried and roll pressed to prepare anode.

[0109] In a dry room, a porous polymer separator made of a polyolefin polymer was interposed between the positive electrode and the negative electrode, and the non-aqueous electrolyte was then injected to manufacture a secondary battery.

[0110] Example 2 A secondary battery was manufactured in the same manner as in Example 1, except that a non-aqueous electrolyte was prepared by adding 1 g of a compound represented by the following formula 1b and 10 g of fluoroethylene carbonate (FEC) to 89 g of the non-aqueous solvent prepared in Example 1.

[0111] [ka]

[0112] Example 3 A secondary battery was manufactured in the same manner as in Example 1, except that 1 g of a compound represented by the following formula 1c and 10 g of fluoroethylene carbonate (FEC) were added to 89 g of the nonaqueous solvent prepared in Example 1 to prepare a nonaqueous electrolyte.

[0113] [ka]

[0114] Example 4 A secondary battery was manufactured in the same manner as in Example 1, except that 0.5 g of the compound of Formula 1a and 10 g of fluoroethylene carbonate (FEC) were added to 89.5 g of the nonaqueous solvent prepared in Example 1 to prepare a nonaqueous electrolyte.

[0115] Example 5 A secondary battery was manufactured in the same manner as in Example 1, except that 2 g of the compound of Formula 1a and 10 g of fluoroethylene carbonate (FEC) were added to 88 g of the nonaqueous solvent prepared in Example 1 to prepare a nonaqueous electrolyte.

[0116] Comparative Example 1 A secondary battery was manufactured in the same manner as in Example 1, except that a non-aqueous electrolyte was prepared using 100 g of the non-aqueous solvent prepared in Example 1.

[0117] Experimental Example 1: Evaluation of high temperature cycle characteristics For each of the secondary batteries produced in Examples 1 to 5 and Comparative Example 1, the cycle characteristics were evaluated.

[0118] Specifically, each of the batteries manufactured in Examples 1 to 5 and Comparative Example 1 was charged at 45° C. with a constant current of 1 C to 4.47 V and discharged at a constant current of 0.5 C to 3.11 V as one cycle, and then the capacity retention rate relative to the initial capacity after one cycle was measured after 600 charge-discharge cycles. The results are shown in Table 1 below.

[0119] [Table 1]

[0120] As shown in Table 1, Examples 1 to 5, in which the additive for non-aqueous electrolytes of the present invention was used, had higher capacity retention rates and better life characteristics than Comparative Example 1, in which the additive was not used.

[0121] Experimental Example 2: Evaluation of high temperature storage characteristics For each of the secondary batteries produced in Examples 1 to 5 and Comparative Example 1, high-temperature storage characteristics were evaluated.

[0122] Specifically, each of the secondary batteries of Examples 1 to 5 and Comparative Example 1 was fully charged to 4.47 V and then stored at 60° C. for 6 weeks.

[0123] Before storage, the capacity of the fully charged secondary battery was measured and set as the initial capacity of the secondary battery.

[0124] After 6 weeks, the capacity of the secondary battery was measured and the capacity loss during the 6-week storage period was calculated. The percentage of the lost capacity relative to the initial capacity of the secondary battery was calculated to obtain the capacity retention rate after 6 weeks. The results are shown in Table 2 below.

[0125] [Table 2]

[0126] As shown in Table 2, the secondary batteries of Examples 1 to 5 had higher capacity retention rates after 6 weeks than the secondary battery of Comparative Example 1, and were confirmed to have stable performance at high temperatures.

Claims

1. A lithium salt; An organic solvent; A non-aqueous electrolyte comprising a compound represented by the following formula 1 as an additive: 【Chemistry 1】 (In the above Chemical Formula 1, R 1 is any one selected from the group consisting of an alkyl group having 1 to 5 carbon atoms, a hydrogen atom of which may be substituted with a fluorine atom, an aryl group having 6 to 8 carbon atoms, a hydrogen atom of which may be substituted with a fluorine atom, and a nitrile group; R 2 ~R 4 are each independently an alkyl group having 1 to 5 carbon atoms.

2. R of Formula 1 1 is CF 3 The non-aqueous electrolyte according to claim 1 .

3. R of Formula 1 1 The non-aqueous electrolyte according to claim 1 , wherein is a nitrile group.

4. The non-aqueous electrolyte according to claim 1, wherein the compound of Chemical Formula 1 is a compound of Chemical Formula 1-1 below: 【Chemistry 2】 (In the above Chemical Formula 1-1, R 2 ~R 4 are each independently an alkyl group having 1 to 5 carbon atoms, R 6 ~R 10 are each independently H or F.

5. The non-aqueous electrolyte according to claim 1, wherein the compound of the formula 1 is any one selected from the group consisting of the following formulas 1a to 1c: 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】

6. The non-aqueous electrolyte of claim 1, wherein the additive is contained in an amount of 0.1 to 4 parts by weight based on 100 parts by weight of the non-aqueous electrolyte.

7. 10. The non-aqueous electrolyte of claim 1 further comprising fluoroethylene carbonate (FEC).

8. The non-aqueous electrolyte of claim 7, wherein the fluoroethylene carbonate (FEC) is contained in an amount of 1 to 30 parts by weight based on 100 parts by weight of the non-aqueous electrolyte.

9. 8. The non-aqueous electrolyte of claim 7, wherein the compound of Formula 1 and fluoroethylene carbonate are contained in a weight ratio of 1:1 to 1:

30.

10. The lithium salts are LiCl, LiBr, LiI, and LiBF. 4 , LiClO 4 , LiB 10 C 10 , LiAlCl 4 , LiAlO 2 , LiPF 6 , LiCF 3 SO 3 , LiCH 3 CO 2 , LiCF 3 CO 2 , LiAsF 6 , LiSbF 6 , LiCH 3 SO 3 , LiN(SO 2 F) 2 , LiN(SO 2 CF 2 CF 3 ) 2 , and LiN(SO 2 CF 3 ) 2 The non-aqueous electrolyte according to claim 1 , wherein the non-aqueous electrolyte is one or more selected from the group consisting of:

11. The non-aqueous electrolyte according to claim 1 , wherein the lithium salt is contained at a concentration of 0.5M to 3M.

12. A positive electrode and A negative electrode; A lithium secondary battery comprising the nonaqueous electrolyte according to any one of claims 1 to 11, A lithium secondary battery having a driving voltage of 4.47 V or more.

13. 13. The lithium secondary battery according to claim 12, wherein the positive electrode comprises a lithium cobalt-based oxide as a positive electrode active material.

14. The negative electrode contains, as a negative electrode active material, Si, Si-C, and SiO x The lithium secondary battery according to claim 12, comprising at least one selected from the group consisting of (0<x≦2).

Citation Information

Patent Citations

  • Lithium ion battery electrolyte and lithium ion battery prepared therefrom

    CN108306048A

  • Electrolyte and secondary battery using same

    CN113130990A

  • Electrolyte additive, secondary battery electrolyte, secondary battery and terminal

    CN113540561A

  • Lithium ion secondary battery having extended cycle life in charge / Discharge

    JP2000223152A

  • Cathode material for lithium secondary batteries, cathode and lithium secondary battery containing the same

    JP2022508147A