Polypropylene resin composition for insulating layer of electrode cable having excellent whitening resistance and molded product using the same
A polypropylene resin composition with a propylene block copolymer and additives addresses flexibility and electrical property issues in power cables, providing improved whitening resistance and recyclability.
Patent Information
- Application Number
- JP2024529299
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-22
- Filing Date
- 2022-09-27
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-09-27
AI Technical Summary
Existing polypropylene insulation layers for power cables suffer from low flexibility and inadequate electrical properties, leading to installation difficulties and a whitening phenomenon due to heterogeneous material characteristics, while cross-linked polyethylene is environmentally unfriendly and non-recyclable.
A polypropylene resin composition comprising 70 to 90 parts by weight of a propylene block copolymer with ethylene-propylene rubber dispersed in a propylene-ethylene random copolymer, 5 to 20 parts by weight of high molecular weight atactic polypropylene, and 5 to 20 parts by weight of a polyolefin elastomer, enhancing flexibility and electrical properties with improved whitening resistance.
The resin composition achieves excellent flexibility, electrical properties, and whitening resistance, making it suitable for power cables with recyclability and reduced environmental impact.
Smart Images

Figure 2024540467000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an environmentally friendly resin composition for an insulating layer of a power cable, and more particularly to a recyclable, environmentally friendly resin composition for an insulating layer of a power cable which has excellent flexibility and electrical properties.
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2021-0161553, filed on November 22, 2021, the entire text of which is incorporated herein by reference. [Background technology]
[0003] Cross-linked materials such as polyethylene (PE), polyvinyl chloride (PVC), and ethylene-propylene rubber (EPR) are mainly used as insulating materials for power cables. Among them, cross-linked polyethylene (XLPE) is made by converting the linear molecular structure of polyethylene into a three-dimensional network structure through a cross-linking process, and while it retains the excellent mechanical properties and chemical resistance of conventional polyethylene, it has improved heat resistance and has been used as an insulating layer for high-voltage power cables. However, since cross-linked polyethylene is a cross-linked polymer, it cannot be recycled and must be incinerated to be disposed of, which makes it somewhat unenvironmentally friendly.
[0004] Recently, there has been development of an insulating layer resin that can be used in power distribution lines (22.9kv or more) that uses polypropylene (PP), a material that is easily recyclable and has high heat resistance. Compared to XLPE insulating layers, polypropylene insulating layers are easier to manufacture and are environmentally friendly due to their non-crosslinked form, and are known to have excellent performance and usability, including heat resistance. The manufacturing process of polypropylene insulating layers does not generate toxic substances such as methane gas or various by-products, and greenhouse gases such as CO2 generated during the manufacturing process can be reduced by about 30% compared to XLPE. Another advantage of polypropylene insulating layers is that they are recyclable and heat resistant, which can increase transmission capacity.
[0005] However, power cables containing polypropylene insulation layers have problems with poor cable installation due to low flexibility caused by the high rigidity inherent to polypropylene, and electrical properties are somewhat insufficient compared to XLPE. Therefore, there is a need to develop an insulation layer composition that is environmentally friendly while improving on the high rigidity and electrical properties of polypropylene.
[0006] Recently, attempts have been made to improve flexibility and electrical properties by using olefin rubber with polypropylene materials. However, polypropylene materials and olefin rubber have heterogeneous properties and cannot be mixed with each other, resulting in the formation of a boundary between the matrix and domain. When tension is applied to this boundary during the installation of power lines, microcrazes occur at the interface, causing whitening.
[0007] International Publication No. WO2013 / 148028 discloses a polypropylene mixture for thermoplastic insulation, which is a mixture of polypropylene with ethylene, α-olefin, EPDM, etc., and discloses changes in AC breakdown voltage strength depending on the cooling rate. However, it does not mention improvements in heat resistance and flexibility of the composition, and problems such as breakage during installation may occur due to inferior flexibility.
[0008] Korean Patent Publication No. 2014-0040082 discloses a thermoplastic polymer material that ensures flexibility by mixing an α-olefin comonomer rubber phase with a propylene copolymer. However, if the rubber phase content is low, the flexibility decreases when used as an insulating material, making installation and construction difficult, while if the rubber phase content is high, the advantages of polypropylene that determine mechanical properties are lost, and there is a problem that the dielectric breakdown strength decreases due to the whitening phenomenon that can occur as a resin composition with heterogeneous properties. Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention provides a recyclable resin composition for the insulating layer of a power cable, which has excellent flexibility and electrical properties while also having excellent whitening resistance, and a molded product using the same. [Means for solving the problem]
[0010] In order to solve the above problems, the present invention provides a polypropylene resin composition for an insulating layer of a power cable, comprising 70 to 90 parts by weight of a propylene block copolymer in which ethylene-propylene rubber (EPR) is dispersed in a propylene-ethylene random copolymer, 5 to 20 parts by weight of a polyolefin elastomer (POE), and 5 to 20 parts by weight of a high molecular weight atactic polypropylene (Atatic PP) having a weight average molecular weight of 100,000 g / mol or more.
[0011] The present invention also provides a polypropylene resin composition for an insulating layer of a power cable, characterized in that the ethylene-derived repeating units of the propylene block copolymer are contained in an amount of 0.1 to 5 weight % of the propylene-ethylene random copolymer, 30 to 60 weight % of the ethylene-propylene rubber (EPR), and 5 to 25 weight % of the propylene block copolymer.
[0012] The present invention also provides a polypropylene resin composition for an insulating layer of a power cable, characterized in that the propylene block copolymer has a melting point of 150 to 170°C, a melting enthalpy of 65 to 85 J / g, a melt index (MI, 230°C, 2.16 kg load) of 0.1 to 10 g / 10 min, and a xylene soluble content of 15 to 50 wt% of the propylene block copolymer.
[0013] The propylene block copolymer is obtained by reacting propylene and ethylene in a loop reactor to polymerize a propylene-ethylene random copolymer, and then continuously polymerizing propylene and ethylene in a gas phase reactor in the presence of the propylene-ethylene random copolymer to disperse ethylene-propylene rubber (EPR) in the propylene-ethylene random copolymer.
[0014] The polyolefin elastomer contains two or more repeating units selected from the group consisting of ethylene-derived repeating units, propylene-derived repeating units, and (C4-C12) α-olefin-derived repeating units, and the polypropylene resin composition for use in an insulating layer of a power cable contains the ethylene-derived repeating units or the propylene-derived repeating units.
[0015] The present invention also provides a polypropylene resin composition for an insulating layer of a power cable, characterized in that the resin composition has a white index of 40 or less as measured by the following method.
[0016] [How to measure whiteness] The resin composition was formed into a sheet having a thickness of 2 mm at 230°C using a press molding machine, and then cooled at 10°C for 5 minutes to prepare a sample (60 x 45 x 2 mm). A bending test was performed by applying a force of 10 N, and the whiteness of the test piece subjected to the bending test was measured using a spectrophotometer (7000A_IQPC, manufactured by Ecolorplus) according to the ASTM E313 standard.
[0017] The resin composition for insulating a power cable is characterized in that the resin composition has a flexural modulus of 300 to 550 MPa, an AC dielectric breakdown strength of 50 kV / mm or more, and an impulse dielectric breakdown strength of 90 kV / mm or more, as measured by the following method.
[0018] [Method for measuring flexural modulus] According to the ASTM D790 standard, the test piece (127 x 12.7 x 6.4 mm) is fixed at a support interval (Span) of 100 mm, and a bending load is applied at a speed of 28 mm / min to measure the bending modulus.
[0019] [Method of measuring dielectric breakdown strength] The resin composition was formed into a sheet having a thickness of 1 mm using a press molding machine, and then cooled at 10° C. for 5 minutes. According to the ASTM D149 standard, a voltage of 30 kV was applied for 5 minutes, and then the voltage was increased by 10 kV and maintained for 5 minutes. This process was continued until dielectric breakdown occurred. If dielectric breakdown occurred, the voltage at that time was defined as the AC dielectric breakdown strength. An impulse voltage of 80 kV was applied to the sheet 10 times each in positive and negative polarities, and then an impulse voltage was applied 3 times by increasing the voltage by 10 kV. This process was continued until breakdown occurred. If dielectric breakdown occurred, the voltage at that time was defined as the impulse dielectric breakdown strength.
[0020] In order to achieve the above-mentioned other object, the present invention provides a power cable including the above-mentioned resin composition as an insulating layer. Effect of the Invention
[0021] The present invention uses a propylene block copolymer in which ethylene-propylene rubber (EPR) is dispersed in a propylene-ethylene random copolymer, and a high molecular weight atactic polypropylene for a polyolefin elastomer, and can provide a resin composition for the insulating layer of a recyclable power cable that has excellent flexibility and electrical properties while also having excellent whitening resistance, and a power cable using the same. [Brief description of the drawings]
[0022] [Figure 1] FIG. 2 is a schematic diagram showing a cross section of a power cable produced from a resin composition according to the present invention. [Diagram 2] 1 is a photograph showing the results of observing a cross section of a test piece subjected to bending evaluation in an experimental example using an optical microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The present invention will be described in detail below through preferred embodiments. Prior to this, the terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as having meanings and concepts that correspond to the technical ideas of the present invention, based on the principle that the inventor can appropriately define the concepts of terms to best describe his / her invention. Therefore, it should be understood that the configuration of the embodiment described in this specification is only one of the most preferred embodiments of the present invention, and does not fully represent the technical ideas of the present invention, and therefore, at the time of this application, there may be various equivalents and modifications that can replace them.
[0024] The present invention discloses a polypropylene resin composition for an insulating layer of a power cable, comprising 70 to 90 parts by weight of a propylene block copolymer in which ethylene-propylene rubber (EPR) is dispersed in a propylene-ethylene random copolymer, 5 to 20 parts by weight of a polyolefin elastomer (POE), and 5 to 20 parts by weight of a high molecular weight atactic polypropylene (Atatic PP) having a weight average molecular weight of 100,000 g / mol or more.
[0025] Each of the components of the resin composition for the insulating layer of a power cable according to the present invention will be described in detail below.
[0026] Polypropylene can be classified into homopolypropylene (H-PP), propylene random copolymer (R-PP), and propylene block copolymer (B-PP). Among these, propylene random copolymer and propylene block copolymer have higher flexibility and bending property than homopolypropylene, and are more suitable for power cables. Here, propylene block copolymer has an advantage of being superior in flexibility and bending property than propylene random copolymer, so propylene block copolymer is used in the present invention.
[0027] In the present invention, the propylene block copolymer is a type of RTPO (Reactor-made Thermoplastic Polyolefin elastomers), and refers to a polymer containing a large number of polymers exhibiting rubber properties in a polymer containing units derived from a propylene monomer.
[0028] In the present invention, the propylene block copolymer is obtained by reacting propylene and ethylene in a loop reactor to polymerize a propylene-ethylene random copolymer, and then copolymerizing propylene and ethylene gases in a gas phase reactor in the presence of the propylene-ethylene random copolymer in a continuous polymerization, thereby dispersing the ethylene-propylene rubber (EPR) in the propylene-ethylene random copolymer. By producing the propylene block copolymer by the continuous polymerization as described above, the ethylene-propylene rubber (EPR) can be uniformly dispersed in the polypropylene matrix as small domains.
[0029] Here, in the present invention, the domain size and dispersion degree of the ethylene-propylene rubber (EPR) are not limited, but considering the flexibility and electrical properties of the final resin composition, the average size of the domain may be 0.1 to 5 μm, preferably 0.5 to 2 μm, and the domain dispersion degree may be 0.1 to 0.7, preferably 0.2 to 0.6. The domain size and dispersion degree may be measured by cutting a specimen prepared by compression molding (at 220° C. for 4 minutes) of the resin composition into a width of 1 mm and a length of 10 cm, immersing it in xylene at 60° C. to dissolve the ethylene-propylene rubber, and analyzing the voids present on the surface of the specimen with a scanning electron microscope (SEM).
[0030] In the present invention, the propylene block copolymer may contain 50 to 85% by weight of propylene-ethylene random copolymer and 15 to 50% by weight of ethylene-propylene rubber, and preferably 60 to 75% by weight of propylene-ethylene random copolymer and 25 to 40% by weight of ethylene-propylene rubber. The propylene block copolymer is in a form in which ethylene-propylene rubber particles are dispersed in a matrix of propylene-ethylene random copolymer. In particular, the propylene block copolymer may be a block copolymer in which ethylene-propylene rubber is polymerized stepwise in a reactor to a propylene-ethylene random copolymer. The propylene block copolymer has ethylene-propylene rubber dispersed in a specific content range and has a lower flexural modulus than a propylene homopolymer or a propylene-ethylene random copolymer, so that it can maximize the improvement of flexibility when applied to an insulating layer of a power cable, and can have excellent elasticity and improve strength.
[0031] In this specification, the propylene block copolymer is produced by producing a large amount of ethylene-propylene rubber (EPR) using a high content of ethylene in a polymerization reactor, and has the advantages of having high strength and excellent flexibility since it contains a repeating unit derived from ethylene-propylene rubber (EPR) with a high content compared to conventional propylene block copolymers.
[0032] Without being limited by theory, the propylene block copolymer produced in the reactor generally has a repeating unit content of ethylene of 5 to 25% by weight, preferably 10 to 20% by weight, of the entire block copolymer due to technical difficulties. The repeating unit content of ethylene may be 0.1 to 5% by weight, preferably 0.1 to 3% by weight, more preferably 0.5 to 2% by weight, of the propylene-ethylene random copolymer, and may be 30 to 60% by weight, preferably 40 to 50% by weight, of the ethylene-propylene rubber (EPR). Within the range of the repeating unit content of ethylene, the flexibility, bending properties, and electrical properties may be maximized. In addition, if the repeating unit content of ethylene exceeds 5% by weight of the propylene-ethylene random copolymer, the melting point of the block copolymer may decrease, and the heat resistance stability may decrease.
[0033] The propylene block copolymer may have a melting point of 150 to 170° C., preferably 160 to 170° C., and a melting enthalpy of 65 to 85 J / g, preferably 75 to 85 J / g. If the melting point and melting enthalpy of the propylene block copolymer are within the above ranges, the flexibility and electrical properties to be realized in the present invention can be satisfied when the propylene block copolymer is used as an insulating layer of a power cable.
[0034] In addition, the propylene block copolymer may have a melt index (MI, 230°C, 2.16 kg load) of 0.1 to 10 g / 10 min, preferably 0.3 to 5 g / 10 min, and more preferably 0.5 to 2 g / 10 min. If the melt index is less than 0.1 g / 10 min, a load may be applied to the extruder during the cable extrusion process, and if it exceeds 10 g / 10 min, eccentricity of the insulation layer of the cable molded product may occur.
[0035] In addition, the propylene block copolymer may have a xylene soluble content (XS) of 15 to 50 wt %, preferably 25 to 40 wt %, of the propylene block copolymer. The xylene soluble content depends on the content of ethylene-propylene rubber (EPR) contained in the propylene block copolymer, and within this content range, flexibility, bending properties, and electrical properties may be maximized.
[0036] In the present invention, the propylene block copolymer is included in an amount of 70 to 90 parts by weight, preferably 75 to 85 parts by weight. If the amount of the propylene block copolymer is less than 70 parts by weight, the electrical properties may be deteriorated and whitening may occur, and if the amount of the propylene block copolymer is more than 90 parts by weight, the flexibility may be reduced.
[0037] The present invention includes a polyolefin elastomer (POE) as a modifier to improve the flexibility and flex properties of the final resin composition.
[0038] The polyolefin elastomer includes two or more selected from the group consisting of repeating units derived from ethylene, repeating units derived from propylene, and repeating units derived from an α-olefin (C4-C12), and may include the repeating units derived from ethylene or the repeating units derived from propylene. For example, it may be a copolymer of ethylene and propylene, or a random or block copolymer elastomer of an α-olefin of one of ethylene and propylene and 1-butene, 1-pentene, 1-hexene, 1-octene, or the like, or a combination of these elastomers. More preferably, propylene-ethylene rubber (PER) or ethylene-1-octene rubber (EOR) may be used, and most preferably, propylene-ethylene rubber (PER) may be used.
[0039] The polyethylene elastomer (POE) may be included in an amount of 5 to 20 parts by weight, preferably 4 to 15 parts by weight. If the amount of POE is less than 5 parts by weight, the flexibility of the final resin composition may decrease, and if it exceeds 20 parts by weight, the electrical properties may decrease.
[0040] The atactic polypropylene effectively fills the interface when voids occur at the interface between the propylene block copolymer and the polyolefin elastomer (POE). In the present invention, a high molecular weight atactic polypropylene (Atactic PP) having a weight average molecular weight (Mw) of 100,000 g / mol or more, preferably 120,000 g / mol or more, more preferably 120,000 to 1,000,000 g / mol may be used.
[0041] If the molecular weight of the atactic polypropylene is low, it may cause a deterioration in dielectric breakdown strength under high voltage, and the effect of improving the whitening phenomenon when a high tension force is applied is not significant.
[0042] The atactic polypropylene (Atactic PP) may be included in an amount of 5 to 20 parts by weight, preferably 5 to 15 parts by weight. If the amount of atactic polypropylene (Atactic PP) is less than 5 parts by weight, the effect of improving the whitening phenomenon of the resin composition is insignificant, and if the amount of atactic polypropylene (Atactic PP) is more than 20 parts by weight, the dielectric breakdown strength is reduced.
[0043] In the present invention, atactic polypropylene (Atactic PP) has soft crystal spherulites and serves to reduce the flexural modulus of the final resin composition. When mixed with a propylene block copolymer including the propylene-ethylene random copolymer, it can show a significant effect in improving the whitening phenomenon and improving the dielectric breakdown strength compared to when mixed with a propylene block copolymer including a propylene homocopolymer.
[0044] Such atactic polypropylene (Atactic PP) is a non-crystalline polypropylene having an isotacticity (Pentad II, mmmm) of 5 to 20%, preferably 5 to 15%, and may be produced by a method known in the art, for example, by referring to Patent Application No. 2011-0033626 submitted by the applicant, which is incorporated herein by reference.
[0045] In addition to the above components, the resin composition according to the present invention may further contain one or more additives that are commonly used when applied to the insulation layer of a cable, and preferably may further contain an antioxidant, a neutralizing agent, or a water tree inhibitor.
[0046] The antioxidant may be added to inhibit yellowing of the resin composition and provide color stability and transparency. Any antioxidant capable of preventing oxidation of the resin composition for the insulating layer of the power cable may be used without limitation. Preferred antioxidants include hindered phenol-based antioxidants, such as 4,4'-thiobis(2-t-butyl-5-methylphenol), 2,2'-thio-diethyl-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 4,4'-thiobis(2-methyl-6-t-butylphenol), 2.2'-thiobis(6-t-butyl- One or more antioxidants selected from the group consisting of 2,2'-thiobis(6-t-butyl-4-methylphenol), octadecyl[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], and thiodiethylene-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] may be used.
[0047] The neutralizing agent is used to effectively remove catalyst residue remaining after polymerization and prevent decomposition of the resin composition, and any neutralizing agent that can prevent decomposition of the resin composition for the insulating layer of the power cable may be used without limitation.
[0048] The water tree inhibitor is added for the purpose of preventing water treeing, which is a type of micro-breakdown that occurs and gradually grows due to the combined action of moisture and voltage at a voltage below the breakdown voltage. The water tree phenomenon reduces the electrical insulation properties of the insulating layer, causing a reduction in the life of the insulating layer. The water tree inhibitor may be any material that can reduce the combined action of moisture and voltage.
[0049] The polypropylene resin composition for the insulating layer of a power cable according to the present invention may be prepared by mixing and extruding the above-mentioned components according to a conventional method known in the art. For example, the above-mentioned components may be put into a twin-screw extruder and melt-kneaded to prepare a resin composition.
[0050] The resin composition for an insulating layer of a power cable according to the present invention as described above has excellent whitening resistance while satisfying excellent flexibility and electrical properties, and is environmentally friendly and therefore recyclable. More specifically, the whiteness measured by the method described below can be 40 or less, preferably 35 or less, the flexural modulus can be 300 to 550 MPa, preferably 350 to 500 MPa, the AC dielectric breakdown strength can be 50 kV / mm or more, preferably 55 kV / mm or more, and the impulse dielectric breakdown strength can be 90 kV / mm or more, preferably 95 kV / mm or more.
[0051] [How to measure whiteness] The resin composition was formed into a sheet having a thickness of 2 mm at 230°C using a press molding machine, and then cooled at 10°C for 5 minutes to prepare a sample (60 x 45 x 2 mm). A bending test was performed by applying a force of 10 N, and the whiteness of the test piece subjected to the bending test was measured using a spectrophotometer (7000A_IQPC, manufactured by Ecolorplus) according to the ASTM E313 standard.
[0052] [Method for measuring flexural modulus] According to the ASTM D790 standard, the test piece (127 x 12.7 x 6.4 mm) is supported at a fixed interval of 100 mm, and a bending load is applied at a speed of 28 mm / min. The measured value is the bending modulus.
[0053] [Method of measuring dielectric breakdown strength] The resin composition was formed into a sheet having a thickness of 1 mm using a press molding machine, and then cooled at 10° C. for 5 minutes. According to the ASTM D149 standard, a voltage of 30 kV was applied for 5 minutes, and then the voltage was increased by 10 kV and maintained for 5 minutes. This process was continued until dielectric breakdown occurred. If dielectric breakdown occurred, the voltage at that time was defined as the AC dielectric breakdown strength. An impulse voltage of 80 kV was applied to the sheet 10 times each in positive and negative polarities, and then an impulse voltage was applied 3 times by increasing the voltage by 10 kV. This process was continued until breakdown occurred. If dielectric breakdown occurred, the voltage at that time was defined as the impulse dielectric breakdown strength.
[0054] A power cable can be manufactured using the polypropylene resin composition for the insulating layer of a power cable according to the present invention. Fig. 1 is a schematic diagram showing a cross section of a power cable manufactured using the resin composition according to the present invention.
[0055] 1, a power cable manufactured using the resin composition for an insulating layer of a power cable according to the present invention includes a conductor 1, an inner semiconductive layer 2 surrounding the conductor 1, an insulating layer 3 surrounding the inner semiconductive layer 2, an outer semiconductive layer 4 surrounding the insulating layer 3, and a sheath layer 5 surrounding the outer semiconductive layer 4, and the insulating layer 3 may include the resin composition according to the present invention. Since details of each layer constituting the power cable, except for the insulating layer, are generally known to those skilled in the art, detailed description thereof will be omitted in the present invention. EXAMPLES
[0056] The present invention will be described below with reference to specific production examples, examples, and comparative examples.
[0057] <Production Example 1: Production of Propylene Block Copolymer (Resin 1)> Propylene and ethylene were reacted in a loop reactor to obtain a propylene-ethylene random copolymer, and the propylene-ethylene random copolymer polymerized in the loop reactor, ethylene, and propylene were fed into a gas phase reactor to carry out a copolymerization reaction of ethylene-propylene in a continuous process to produce a propylene block copolymer. The propylene block copolymer produced had 1% by weight of ethylene-derived repeat units in the propylene-ethylene random copolymer, 43% in the ethylene-propylene rubber (EPR), and 15% by weight in the total copolymer, a xylene soluble content of 29% by weight, a melt index of 1g / 10min, a melting point of 150.7℃, and a melting enthalpy of 67.4J / g. The melt index, xylene soluble content, melting point, and melting enthalpy of the propylene block copolymer were measured by the following methods, respectively. Melt Index (MI): Measured according to ASTM D1238 standard at a temperature of 230° C. and a load of 2.16 kg. -Xylene solubles (XS): According to ASTM D5492 standard, propylene block copolymer was dissolved in boiling xylene, cooled at room temperature and separated into a part dissolved in xylene and an insoluble part, the part dissolved in xylene was collected separately, the xylene was evaporated on a hot plate, and the weight percentage of the remaining part was measured. Melting point and melting enthalpy: Using a differential scanning calorimeter (DSC), the sample was heated to 200°C at a rate of 10°C / min, and then cooled to -30°C twice. The data measured the second time were used.
[0058] <Comparative Production Example 1: Production of Propylene Block Copolymer (Resin 2)> A propylene block copolymer was prepared in the same manner as in Preparation Example 1 of Resin 1, except that a propylene homopolymer was obtained by reacting propylene in a loop reactor in Preparation Example 1. The propylene block copolymer prepared had 42% ethylene-derived repeat units in the ethylene-propylene rubber (EPR) and 14 wt% in the total copolymer, a xylene soluble content of 29 wt%, a melt index of 1g / 10min, a melting point of 163.7°C, and a melting enthalpy of 77.4 J / g.
[0059] <Polyolefin elastomer (POE) (resin 3)> Polyolefin elastomers include propylene-ethylene rubber (PER) (Vistamaxx TM 3020FL (manufactured by Exxonmobil Chemical, melting point 60.2°C, specific gravity 0.874) was prepared.
[0060] <Production Example 2: Production of Atactic Polypropylene (Resin 4)> Patent Application No. 2011-0033626 was referred to. The inside of a high-pressure reactor (internal volume: 2 L, stainless steel) was replaced with nitrogen at room temperature, and about 4.0 mL of methylaluminoxane toluene solution (10 wt% solution of methylaluminoxane in toluene, 6 mmol based on Al, manufactured by Albemarle) was added to the reactor, followed by adding 500 g of propylene and heating to 70°C. Next, a solution (1.5 mL, 3.0 μmol of Ti) in which a transition metal compound represented by the following chemical formula 1 was dissolved in toluene was injected into the reactor to carry out polymerization. After the polymerization reaction, the temperature was lowered to room temperature, excess propylene was removed, and the polymer was recovered. The obtained polymer was dried for more than 4 hours while heating at 80°C in a vacuum oven to produce atactic polypropylene (xylene soluble content 98 wt%, MI (230°C, 2.16 kg load) 2g / 10min, Mw (measured by GPC analysis, PL-GPC220, Agilent) 320,000g / mol, Tg (glass transition temperature) -5°C, II (%, mmmm)2).
[0061] <Production Example 3: Production of Atactic Polypropylene (Resin 5)> In Preparation Example 2, by adjusting the amount of propylene, the amount of catalyst, the reaction time, etc., an atactic polypropylene with a xylene soluble content of 98 wt%, MI (230°C, 2.16 kg load) of 50 g / 10 min, Mw (measured by GPC analysis, PL-GPC220, Agilent) of 120,000 g / mol, Tg (glass transition temperature) of -5°C, and II (%, mmmm) of 1.5 was produced.
[0062] <Comparative Production Example 2: Production of Atactic Polypropylene (Resin 6)> In Preparation Example 2, by adjusting the amount of propylene, the amount of catalyst, the reaction time, etc., an atactic polypropylene with a xylene soluble content of 98 wt%, MI (230°C, 2.16 kg load) of 100 g / 10 min, Mw (measured by GPC analysis, PL-GPC220, Agilent) of 40,000 g / mol, Tg (glass transition temperature) of -5°C, and II (%, mmmm) of 1.9 was produced.
[0063] <Examples and Comparative Examples> A mixture consisting of the components shown in Table 1 below was mixed in a mixer for 5 minutes, and then extruded in a twin-screw extruder at 190 to 230° C. to produce a pellet-shaped resin composition.
[0064] <Test Example> The pellet-shaped resin composition thus prepared was used to measure the flexural properties, electrical properties, and whiteness according to the following methods, and the results are shown in Table 1 below.
[0065] [Measurement method] (1) Flexural modulus According to the ASTM D790 standard, the test piece (127 x 12.7 x 6.4 mm) was supported at a fixed interval of 100 mm, and a bending load was applied at a speed of 28 mm / min. The measured value was taken as the flexural modulus. If the flexural modulus was 550 MPa or less, the flexibility and flexural properties were judged to be good, and if it was 500 MPa or less, it was judged to be excellent.
[0066] (2) Dielectric breakdown strength The resin composition was prepared into a sheet having a thickness of 1 mm using a press molding machine, and then cooled at 10° C. for 5 minutes. According to ASTM D149, 30 kV was applied for 5 minutes, then increased by 10 kV and maintained for 5 minutes until breakdown occurred. The voltage at which breakdown occurred was defined as the AC breakdown strength. An impulse voltage of 80 kV was applied to the sheet 10 times each in positive and negative polarities, then increased by 10 kV and applied 3 times in impulse voltages until breakdown occurred. The voltage at which breakdown occurred was defined as the impulse breakdown strength. If the AC breakdown strength is 50 kV / mm or more and the impulse breakdown strength is 90 kV / mm or more, the electrical properties are deemed to be excellent.
[0067] (3) Whiteness (whitening phenomenon) The resin composition was prepared into a sheet having a thickness of 2 mm at 230°C using a press molding machine, and then cooled at 10°C for 5 minutes to prepare a sample (60×45×2 mm), which was subjected to bending evaluation by applying a force of 10 N. The whiteness of the specimen subjected to bending evaluation was measured using a spectrophotometry device (7000A_IQPC, manufactured by Ecolorplus) according to the ASTM E313 standard. In addition, the cross section of the specimen subjected to bending evaluation was observed under an optical microscope (observation temperature 134°C, magnification ×100, 2 min), and the results are shown in FIG. 2.
[0068] [Table 1]
[0069] Referring to Table 1 and FIG. 2, it can be seen that the resin compositions for the insulating layer of power cables (Examples 1 to 3) using the propylene block copolymer in which ethylene-propylene rubber (PER) is dispersed in the propylene-ethylene random copolymer and the high molecular weight atactic polypropylene as the polyolefin elastomer according to the present invention are recyclable resin compositions and have excellent flexibility and electrical properties while also exhibiting excellent whitening resistance.
[0070] In contrast, when atactic polypropylene was not used (Comparative Example 1), the flexibility, electrical properties, and whitening resistance were all inferior; when atactic polypropylene was used but the molecular weight did not reach a specific level (Comparative Example 5), the whitening resistance was not satisfied; when atactic polypropylene with a specific level of high molecular weight was used but its content was too low (Comparative Example 2), the electrical properties and whitening resistance were poor; when its content was excessive (Comparative Example 3), the bending properties were reduced; and when the matrix component of the propylene block copolymer was a propylene homocopolymer (Comparative Example 4), the electrical properties were not satisfied and the bending properties and whitening resistance were significantly reduced.
[0071] The preferred embodiments of the present invention have been described in detail above. The description of the present invention is for illustrative purposes only, and those skilled in the art will understand that the present invention can be easily modified into other specific forms without changing the technical concept or essential features of the present invention.
[0072] Therefore, the scope of the present invention is indicated by the claims set forth below rather than the above detailed description, and all modifications and variations derived from the meaning, scope, and equivalent concepts of the claims should be interpreted as being included in the scope of the present invention.
Claims
1. 70 to 90 parts by weight of a propylene block copolymer in which ethylene-propylene rubber (EPR) is dispersed in a propylene-ethylene random copolymer; 5 to 20 parts by weight of polyolefin elastomer (POE); 5 to 20 parts by weight of high molecular weight atactic polypropylene (Atactic PP) having a weight average molecular weight of 100,000 g / mol or more; 1. A polypropylene resin composition for an insulating layer of a power cable comprising:
2. The ethylene-derived repeating unit of the propylene block copolymer is The propylene-ethylene random copolymer contains 0.1 to 5% by weight of the propylene-ethylene random copolymer, The ethylene-propylene rubber (EPR) contains 30 to 60% by weight of the ethylene-propylene rubber, 2. The polypropylene resin composition for an insulating layer of a power cable according to claim 1, wherein the polypropylene resin composition is contained in an amount of 5 to 25% by weight of the propylene block copolymer.
3. 2. The polypropylene resin composition for an insulating layer of a power cable according to claim 1, wherein the propylene block copolymer has a melting point of 150 to 170° C., a melting enthalpy of 65 to 85 J / g, a melt index (MI, 230° C., 2.16 kg load) of 0.1 to 10 g / 10 min, and a xylene soluble content of 15 to 50 wt % of the propylene block copolymer.
4. 2. The polypropylene resin composition for a power cable insulating layer according to claim 1, wherein the propylene block copolymer is obtained by reacting propylene and ethylene in a loop reactor to polymerize a propylene-ethylene random copolymer, and then continuously polymerizing propylene and ethylene in a gas phase reactor in the presence of the propylene-ethylene random copolymer to disperse ethylene-propylene rubber (EPR) in the propylene-ethylene random copolymer.
5. The polyolefin elastomer contains two or more repeating units selected from the group consisting of repeating units derived from ethylene, repeating units derived from propylene, and repeating units derived from (C4-C12) α-olefins, and contains the repeating units derived from ethylene or the repeating units derived from propylene. The polypropylene resin composition for use in an insulating layer of a power cable according to claim 1,
6. The polypropylene resin composition for an insulating layer of a power cable according to claim 1, characterized in that the resin composition has a whiteness index of 40 or less as measured by the following method: [Method of measuring whiteness] The resin composition was prepared into a sheet having a thickness of 2 mm at 230° C. using a press molding machine, and then cooled at 10° C. for 5 minutes to prepare a sample (60×45×2 mm). A bending test was performed by applying a force of 10 N to the sample. The whiteness of the sample subjected to the bending test was measured using a spectrophotometer (Ecolorplus, 7000A_IQPC) according to the ASTM E313 standard.
7. The resin composition for insulating a power cable according to claim 1, characterized in that the resin composition has a flexural modulus of 300 to 550 MPa, an AC dielectric breakdown strength of 50 kV / mm or more, and an impulse dielectric breakdown strength of 90 kV / mm or more, as measured by the following method: [Method for measuring flexural modulus] According to the ASTM D790 standard, the support interval (Span) of a test piece (127×12.7×6.4 mm) is fixed at 100 mm, and a bending load is applied at a speed of 28 mm / min to measure the bending modulus. [Method of measuring dielectric breakdown strength] The resin composition was formed into a sheet having a thickness of 1 mm using a press molding machine, and then cooled at 10° C. for 5 minutes. According to ASTM D149 standard, a voltage of 30 kV was applied for 5 minutes, and then the voltage was increased by 10 kV and maintained for 5 minutes until a dielectric breakdown occurred. If a dielectric breakdown occurred, the voltage was defined as the AC dielectric breakdown strength. An impulse voltage of 80 kV was applied to the sheet 10 times each in positive and negative polarities, and then an impulse voltage was applied 3 times by increasing the voltage by 10 kV. This process was continued until a breakdown occurred. If a dielectric breakdown occurred, the voltage was defined as the impulse dielectric breakdown strength.
8. A power cable comprising the resin composition according to claim 1 as an insulating layer.
Citation Information
Patent Citations
Polypropylene resin for power cable and power cable comprising the same in insulation layer
EP3342816A1
Polypropylene resin for insulator of power cable
JP2019073678A
Cleansing Composition
KR1020210158608A
Non-conductive adhesive for distribution panel and manufacturing method thereof
KR102022949B1
Modified resins and uses thereof
US20200056018A1