Positive electrode active material and method for producing same

A multi-step water washing process with boron-containing coatings on nickel-based positive electrode materials addresses residual lithium and structural issues, resulting in improved electrochemical and thermal stability for lithium batteries.

JP2024540563AActive Publication Date: 2024-10-31LG CHEM LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024529674
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-03
Filing Date
2022-12-02
Publication Date
2024-10-31
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

Nickel-based positive electrode active materials with high nickel content face issues such as residual lithium causing performance degradation, gelation during manufacturing, and structural cracks due to lithium movement, leading to reduced long-term battery performance and stability.

Method used

A method involving multiple water washing steps with specific ratios of water washing solutions and the addition of boron-containing raw materials to form a uniform Li-B-O solid solution coating on the surface of the lithium transition metal oxide, minimizing surface deterioration and controlling residual lithium.

Benefits of technology

The method results in a positive electrode active material with improved electrochemical performance, thermal stability, and reduced gas generation, enhancing the long-term performance of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540563000001
    Figure 2024540563000001
  • Figure 2024540563000002
    Figure 2024540563000002
  • Figure 2024540563000003
    Figure 2024540563000003
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a positive electrode active material, which can minimize surface deterioration of the positive electrode active material occurring during a washing process, effectively control residual lithium, and form a uniform coating layer on the surface of the positive electrode active material, and to a positive electrode active material manufactured by the same, and the method includes the steps of: (A) preparing a lithium transition metal oxide; (B) mixing the lithium transition metal oxide with a first washing solution to wash the lithium transition metal oxide with water for a first time, and then performing a first filtration; and (C) washing and filtering the lithium transition metal oxide that has undergone step (B). (D) performing a second washing and a second filtration simultaneously with a second washing solution using a filtration device capable of simultaneous filtration; and (C) drying the lithium transition metal oxide that has been subjected to steps (C) and then mixing a coating element-containing raw material with the dried lithium transition metal oxide and heat treating the mixture to form a coating layer, wherein the coating element-containing raw material contains a boron-containing raw material and one or more lithium-containing raw materials selected from LiOH, Li2CO3, and Li2O.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0171783 filed on December 3, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a positive electrode active material and a method for producing the same. [Background technology]

[0003] Nickel-based positive electrode active materials are manufactured by mixing a nickel-based positive electrode active material precursor with a lithium-containing raw material and then calcining the mixture. During this process, however, there is a problem that unreacted lithium-containing raw material and by-products such as LiOH and Li2CO3 remain on the surface of the positive electrode active material.

[0004] In particular, nickel-based positive electrode active materials containing a high content of nickel have the problem of a large amount of residual lithium. Such by-products can react with the electrolyte to cause problems with the long-term performance of the battery (e.g., reduced long-term life, increased resistance, etc.) and stability problems (e.g., gas generation, etc.). In addition, gelation can occur during the manufacturing process of the electrode slurry.

[0005] To prevent this, in the conventional manufacturing process of a positive electrode active material, a positive electrode active material precursor and a lithium-containing raw material are mixed and baked to manufacture a positive electrode active material, and then the positive electrode active material is washed with a washing solution (e.g., deionized water, distilled water, etc.) to control the residual lithium. Meanwhile, in order to effectively control the residual lithium, there is a method of using a large amount of washing solution in the washing process, but the use of a large amount of washing solution can cause process problems and can cause problems such as a decrease in battery performance due to deterioration of the surface of the positive electrode active material.

[0006] In addition, in the case of nickel-based positive electrode active materials that contain a high content of nickel, as the charge-discharge cycle of a battery containing such materials progresses, the movement of lithium within the positive electrode active material causes repeated contraction and expansion, which leads to the generation of cracks. Such cracks have a negative effect on the long-term performance of the battery.

[0007] Therefore, there is a need for a positive electrode active material and a manufacturing method thereof that can effectively control residual lithium, suppress deterioration of the positive electrode active material, and improve the long-term performance of the battery when applied to the battery. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made to solve the above problems, and aims to provide a positive electrode active material and a manufacturing method thereof, which can minimize surface deterioration of a positive electrode active material that may occur during a water washing process during the manufacture of the positive electrode active material, effectively control residual lithium, and form a uniform coating layer on the surface of the positive electrode active material, thereby minimizing deterioration in battery performance. [Means for solving the problem]

[0009] The present invention provides a method for producing a positive electrode active material, a positive electrode active material, and a positive electrode.

[0010] (1) The present invention provides a method for producing a positive electrode active material, the method comprising the steps of: (A) preparing a lithium transition metal oxide; (B) mixing the lithium transition metal oxide with a first washing solution to perform a first water wash on the lithium transition metal oxide, and then performing a first filtration; (C) simultaneously performing a second water wash and a second filtration on the lithium transition metal oxide that has undergone step (B) with a second washing solution using a filtration device capable of simultaneously performing water washing and filtration; and (D) drying the lithium transition metal oxide that has undergone step (C), and then mixing a coating element-containing raw material with the dried lithium transition metal oxide and heat-treating it to form a coating layer, the coating element-containing raw material including a boron-containing raw material and one or more lithium-containing raw materials selected from LiOH, Li2CO3, and Li2O.

[0011] (2) The present invention provides the method for producing a positive electrode active material according to (1) above, wherein the lithium transition metal oxide contains nickel in an amount of 70 mol % or more of all metals other than lithium.

[0012] (3) The present invention provides the method for producing a positive electrode active material according to (1) or (2) above, wherein the content of the second washing solution is 10 parts by weight to 50 parts by weight with respect to 100 parts by weight of the first washing solution.

[0013] (4) The present invention provides the method for producing a positive electrode active material according to any one of (1) to (3), wherein the content of the first washing solution is 50 parts by weight to 150 parts by weight based on 100 parts by weight of the lithium transition metal oxide.

[0014] (5) The present invention provides the method for producing a positive electrode active material according to any one of (1) to (4), wherein the content of the second washing solution is 5 parts by weight to 50 parts by weight based on 100 parts by weight of the lithium transition metal oxide.

[0015] (6) The present invention provides the method for producing a positive electrode active material according to any one of (1) to (5), wherein a sum of a content of the first washing solution and a content of the second washing solution is 55 parts by weight to 150 parts by weight per 100 parts by weight of the lithium transition metal oxide.

[0016] (7) The present invention provides the method for producing a positive electrode active material according to any one of (1) to (6), wherein the one or more lithium-containing raw materials selected from LiOH, Li2CO3, and Li2O are added in an amount of 160 ppm to 500 ppm by weight based on the dried lithium transition metal oxide.

[0017] (8) The present invention provides a positive electrode active material comprising: a lithium transition metal oxide; and a coating layer formed on the lithium transition metal oxide, the coating layer comprising a Li-BO solid solution, the Li-BO solid solution comprising 50 wt % to 60 wt % of BO, 2 wt % to 7 wt % of LiB2O3, and 1 wt % to 5 wt % of Li2B3O6.

[0018] (9) The present invention provides a positive electrode active material according to the above (8), wherein the lithium transition metal oxide contains nickel in an amount of 70 mol % or more of all metals other than lithium.

[0019] (10) The present invention provides the positive electrode active material according to (8) or (9), wherein a ratio of the LiB2O3 content to the BO2 content is 0.05 to 0.20.

[0020] (11) The present invention provides the positive electrode active material according to any one of the above (8) to (10), wherein a ratio of the content of Li2B3O6 to the content of BO2 is 0.01 to 0.10.

[0021] (12) The present invention provides a positive electrode comprising the positive electrode active material according to any one of (8) to (11) above. Effect of the Invention

[0022] In the present invention, the surface is controlled by the water washing process in step (C), and a coating layer is formed on the surface-controlled cathode active material in step (D) using a boron-containing raw material and at least one lithium-containing raw material selected from LiOH, Li2CO3, and Li2O, thereby minimizing surface deterioration of the cathode active material that occurs during the water washing process, effectively controlling residual lithium, and forming a uniform coating layer on the surface of the cathode active material. Therefore, a battery using the cathode active material manufactured by the method of the present invention can have excellent performance, particularly excellent electrochemical performance and thermal stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0024] In this specification, the terms "comprise", "include", "comprise", "have" and the like are intended to specify the presence of embodied features, numerals, steps, components, or combinations thereof, and are not intended to preclude the presence or additional possibility of one or more different features, numerals, steps, components, or combinations thereof.

[0025] The present invention will now be described in further detail.

[0026] Method for producing positive electrode active material The present inventors have discovered that it is possible to minimize surface deterioration of a positive electrode active material that occurs during a water washing process in a manufacturing process of the positive electrode active material, to effectively control residual lithium, and to form a uniform coating layer on the surface of the positive electrode active material, thereby completing the present invention.

[0027] The method for producing a positive electrode active material according to the present invention includes the steps of (A) preparing a lithium transition metal oxide, (B) mixing the lithium transition metal oxide with a first washing solution to first wash the lithium transition metal oxide, and then first filtering the lithium transition metal oxide, (C) simultaneously performing a second washing and a second filtering on the lithium transition metal oxide after step (B) with a second washing solution using a filtering device capable of simultaneously washing and filtering, and (D) drying the lithium transition metal oxide after step (C), mixing a coating element-containing raw material with the dried lithium transition metal oxide, and heat-treating the mixture to form a coating layer, where the coating element-containing raw material includes a boron-containing raw material and at least one lithium-containing raw material selected from LiOH, Li2CO3, and Li2O.

[0028] Each step of the method for producing the positive electrode active material will be specifically described below.

[0029] (A) Step A method for producing a positive electrode active material according to the present invention includes the step of providing a lithium transition metal oxide.

[0030] The step of preparing the lithium transition metal oxide may include mixing a positive electrode active material precursor with a lithium-containing raw material, and calcining the mixture to produce the lithium transition metal oxide.

[0031] The positive electrode active material precursor may have a composition represented by, for example, chemical formula A or chemical formula B below.

[0032] [Chemical formula A] [Ni x Co y M1 z M2 w ](OH)2

[0033] [Chemical formula B] [Ni x Co y M1 z M2 w ]O·OH

[0034] In Chemical Formula A and Chemical Formula B, M1 can be one or more selected from Mn and Al, and M2 can be one or more selected from Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and Y.

[0035] The x means the atomic fraction of nickel among the metal elements in the precursor, and may be 0.7≦x<1, 0.7≦x≦0.98, or 0.7≦x≦0.95.

[0036] The y represents the atomic fraction of cobalt among the metal elements in the precursor, and is 0 <y≦0.3または0.01≦y≦0.3であることができる。

[0037] The z represents the element fraction of the M1 element among the metal elements in the precursor, and is 0 <z≦0.3または0.01≦z≦0.3であることができる。

[0038] The w means the element fraction of the M2 element among the metal elements in the precursor, and may be 0≦w≦0.2, 0≦w≦0.1, 0≦w≦0.05, or 0≦w≦0.02.

[0039] The lithium-containing raw material may be, for example, at least one selected from the group consisting of lithium carbonate (Li2CO3), lithium hydroxide (LiOH), LiNO3, CH3COOLi, and Li2(COO)2, and may be preferably lithium carbonate (Li2CO3), lithium hydroxide (LiOH), or a combination thereof.

[0040] When preparing the positive electrode active material, the positive electrode active material precursor and the lithium-containing raw material may be mixed in a molar ratio of 1:1 to 1:1.625 or 1:1 to 1:1.15. If the lithium-containing raw material is mixed in an amount less than this range, the capacity of the positive electrode active material may be reduced, and if the lithium-containing raw material is mixed in an amount exceeding this range, unreacted Li may remain as a by-product, resulting in a reduction in capacity and separation of the positive electrode active material particles after firing (inducing an agglomeration phenomenon of the positive electrode active material).

[0041] The calcination can be carried out at a temperature of 700°C to 1000°C. If the calcination temperature is less than 700°C, the raw materials may remain in the particles due to insufficient reaction, which may reduce the high temperature stability of the battery, and the volume density and crystallinity may decrease, resulting in reduced structural stability. On the other hand, if the calcination temperature exceeds 1000°C, uneven growth of the particles may occur, and the particles may be difficult to disintegrate, resulting in reduced capacity. On the other hand, in consideration of the control of the particle size, capacity, stability, and reduction of lithium-containing by-products of the produced positive electrode active material, the calcination temperature may more preferably be 700°C to 980°C.

[0042] The calcination can be carried out for 5 to 35 hours. If the calcination time is less than 5 hours, the reaction time may be too short, making it difficult to obtain a highly crystalline positive electrode active material, whereas if the calcination time exceeds 35 hours, the particle size may become too large, resulting in reduced production efficiency.

[0043] According to the present invention, the lithium transition metal oxide may contain 70 mol % or more of nickel among all metals other than lithium. Specifically, the lithium transition metal oxide may have a composition represented by the following Chemical Formula 1.

[0044] [Chemical formula 1] Li 1+a Ni x1 Co y1 M1 z1 M2 w1 O2

[0045] In the formula (1), 0 ≦ a ≦ 0.3, 0.7 ≦ x1 < 1.0, 0 < y1 ≦ 0.3, 0 < z1 ≦ 0.3, 0 ≦ w1 ≦ 0.2, and x1 + y1 + z1 + w1 = 1. M1 is one or more selected from Mn and Al, and M2 can be one or more selected from Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and Y.

[0046] Said x1 represents the atomic fraction of nickel among the metal elements other than lithium in the lithium transition metal oxide, and can be 0.7 ≦ x1 < 1, 0.7 ≦ x1 ≦ 0.98, or 0.7 ≦ x1 ≦ 0.95.

[0047] Said y1 represents the atomic fraction of cobalt among the metal elements other than lithium in the lithium transition metal oxide, and can be 0 < y1 ≦ 0.3 or 0.01 ≦ y1 ≦ 0.3.

[0048] Said z1 represents the elemental fraction of the M1 element among the metal elements other than lithium in the lithium transition metal oxide, and can be 0 < z1 ≦ 0.3 or 0.01 ≦ z1 ≦ 0.3.

[0049] Said w1 represents the elemental fraction of the M2 element among the metal elements other than lithium in the lithium transition metal oxide, and can be 0 ≦ w1 ≦ 0.2, 0 ≦ w1 ≦ 0.1, 0 ≦ w1 ≦ 0.05, or 0 ≦ w1 ≦ 0.02.

[0050] (B) step and (C) step The method for producing a positive electrode active material according to the present invention includes a step of mixing the lithium transition metal oxide and a first washing solution to perform first washing on the lithium transition metal oxide and then performing first filtration (step (B)), and a step of simultaneously performing second washing and second filtration on the lithium transition metal oxide that has undergone step (B) with a second washing solution using a filtration device capable of simultaneously performing washing and filtration (step (C)).

[0051] When the lithium transition metal oxide that has been subjected to step (B) is subjected to a second washing and a second filtration simultaneously with a second washing solution using a filtration device capable of simultaneous washing and filtration, the ions remaining on the surface of the positive electrode active material are easily removed, which is advantageous in terms of preventing surface deterioration of the positive electrode active material and reducing residual lithium, compared to the case of mixing the lithium transition metal oxide with the washing solution, washing with water, and then filtering twice as in step (B).

[0052] In addition, when steps (B) and (C) are performed in this order, unnecessary ions on the surface of the positive electrode active material can be removed more quickly than when step (C) is performed first and then step (B).

[0053] The filtering device capable of simultaneously performing washing and filtering may be, but is not limited to, a funnel filter, a filter press, or the like.

[0054] Here, the content of the second washing solution may be 10 parts by weight to 50 parts by weight based on 100 parts by weight of the first washing solution. When the content of the second washing solution satisfies this range, surface deterioration of the positive electrode active material occurring during the washing process can be minimized, and residual ions on the surface of the positive electrode active material can be effectively controlled. Therefore, a battery using the positive electrode active material manufactured by the method according to the present invention can have excellent performance, particularly excellent electrochemical performance and thermal stability.

[0055] The present invention includes steps (B) and (C) as the water washing process, which not only reduces the amount of water used, but also minimizes surface deterioration of the positive electrode active material that occurs during the water washing process and effectively controls residual lithium, so that a battery using the positive electrode active material manufactured by the method of the present invention can have excellent performance.

[0056] According to the present invention, even when using a lithium transition metal oxide having a high nickel content as represented by Chemical Formula 1, by performing a water washing process as in the present invention, it is possible to minimize surface deterioration of the cathode active material occurring during the water washing process and effectively control residual lithium, thereby providing a cathode active material having excellent performance.

[0057] According to the present invention, the content of the first washing solution may be 50 parts by weight to 150 parts by weight, specifically 50 parts by weight to 100 parts by weight, based on 100 parts by weight of the lithium transition metal oxide. When the content of the first washing solution is within the above range, unnecessary ions on the surface of the positive electrode active material can be sufficiently removed, and lithium inside the positive electrode active material can be prevented from being released.

[0058] According to the present invention, the content of the second washing solution may be 5 parts by weight to 50 parts by weight, specifically 10 parts by weight to 30 parts by weight, based on 100 parts by weight of the lithium transition metal oxide. In addition, the sum of the content of the first washing solution and the content of the second washing solution may be 55 parts by weight to 150 parts by weight, specifically 60 parts by weight to 130 parts by weight, and more specifically 60 parts by weight to 125 parts by weight, based on 100 parts by weight of the lithium transition metal oxide. In this case, residual ions on the surface of the positive electrode active material can be effectively removed, and surface deterioration of the positive electrode active material occurring during the water washing process can be minimized.

[0059] The solvents of the first washing solution and the second washing solution may each independently be one or more selected from deionized water, distilled water, ethanol, and industrial water. Specifically, the solvents of the first washing solution and the second washing solution may be deionized water and / or distilled water. In this case, lithium is easily dissolved, which may be advantageous for removing residual lithium present on the surface.

[0060] The first water washing may be performed for 5 to 30 minutes, specifically 5 to 20 minutes, and more specifically 5 to 15 minutes. When the first water washing time is within the above range, only the remaining lithium on the surface can be removed, and dissolution of the lithium inserted inside can be suppressed to the maximum.

[0061] The first water washing can be carried out at a temperature of 5° C. to 30° C., specifically 5° C. to 25° C. When the first water washing is carried out at a temperature within the above range, there is an advantage that it is advantageous for controlling lithium carbonate, which is easily dissolved in the washing solution at a low temperature.

[0062] The second water washing may be performed for 1 minute to 30 minutes, specifically 1 minute to 20 minutes, and more specifically 1 minute to 15 minutes. The second water washing may be performed at a temperature of 5° C. to 30° C., specifically 5° C. to 25° C. When the time and temperature of the second water washing process are within the above ranges, it is advantageous in controlling ions present on the surface of the positive electrode active material.

[0063] (D) Step The method for producing a positive electrode active material according to the present invention includes a step of drying the lithium transition metal oxide after step (C), mixing a coating element-containing raw material with the dried lithium transition metal oxide, and heat-treating the mixture to form a coating layer. The coating element-containing raw material includes a boron-containing raw material and at least one lithium-containing raw material selected from LiOH, Li2CO3, and Li2O. This allows the production of a positive electrode active material having a coating layer containing a Li-BO solid solution formed on the surface of the lithium transition metal oxide. Here, the Li-BO solid solution may include 50% to 60% by weight of BO2, 2% to 7% by weight of LiB2O3, and 1% to 5% by weight of Li2B3O6.

[0064] The drying step is a step for removing moisture from the positive electrode active material that contains moisture after the water washing step, and can be performed under temperature conditions of 100° C. to 150° C. for 12 hours or more.

[0065] The boron-containing source material may be an acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide or oxyhydroxide containing B, for example, boric acid (H3BO3).

[0066] The boron-containing raw material may be added in an amount of 200 ppm to 2000 ppm by weight based on the dried lithium transition metal oxide. When the content of the boron-containing raw material is within the above range, the capacity of the battery may be improved, and the resulting coating layer may suppress a direct reaction between the electrolyte and the lithium transition metal oxide, thereby improving the long-term performance characteristics of the battery.

[0067] According to the present invention, the one or more lithium-containing raw materials selected from LiOH, Li2CO3, and Li2O may be added to the dried lithium transition metal oxide in a weight amount of 160 ppm to 500 ppm, specifically 160 ppm to 400 ppm, and more specifically 160 ppm to 300 ppm. When the content of the one or more lithium-containing raw materials selected from LiOH, Li2CO3, and Li2O is within the above range, the boron-containing raw materials may all participate in the reaction (i.e., the lithium-containing raw materials and the boron-containing raw materials all react), so that no reactants remain, and a coating layer including a Li-BO solid solution may be more easily formed.

[0068] The coating element-containing source material may further include acetates, nitrates, sulfates, halides, sulfides, hydroxides, oxides, or oxyhydroxides of Zr, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, Y, or combinations thereof, as required.

[0069] The heat treatment can be performed at a temperature of 200°C to 400°C. When the heat treatment temperature is within the above range, a coating layer can be formed while maintaining the structural stability of the transition metal oxide. The heat treatment can be performed for 1 hour to 10 hours. When the heat treatment time is within the above range, an appropriate coating layer can be formed and production efficiency can be improved.

[0070] positive electrode active material The present invention also provides a positive electrode active material produced by the above-mentioned method.

[0071] Specifically, the positive electrode active material according to the present invention includes a lithium transition metal oxide and a coating layer formed on the lithium transition metal oxide, the coating layer including a Li-BO solid solution, the Li-BO solid solution including 50% to 60% by weight of BO2, 2% to 7% by weight of LiB2O3, and 1% to 5% by weight of Li2B3O6. In this case, the coating layer is stable, and the electrochemical performance and thermal stability of a battery including the positive electrode active material are excellent.

[0072] The Li-BO solid solution may further contain LiBO3, LiB2O4, B3O5, etc., in addition to BO2, LiB2O3, and Li2B3O6. Here, LiBO3, LiB2O4, and B3O5 may be contained in the Li-BO solid solution in amounts of 2% by weight to 3% by weight, 30% by weight to 35% by weight, and 2% by weight to 7% by weight, respectively.

[0073] According to the present invention, the lithium transition metal oxide may contain 70 mol % or more of nickel among all metals other than lithium. Specifically, the lithium transition metal oxide may have a composition represented by Chemical Formula 1, as described above in the method for manufacturing a positive electrode active material.

[0074] According to the present invention, the ratio of the LiB2O3 content to the BO2 content may be 0.05 to 0.20. When the ratio of the LiB2O3 content to the BO2 content is within the above range, the coating layer of the battery including the positive electrode active material according to the present invention is stable, and the battery including the positive electrode active material has excellent electrochemical performance and thermal stability. The ratio of the LiB2O3 content to the BO2 content may be specifically 0.07 to 0.12 in order to further improve the rate characteristics, life characteristics, and gas generation of the battery.

[0075] According to the present invention, the ratio of the Li2B3O6 content to the BO2 content may be 0.01 to 0.10. When the ratio of the Li2B3O6 content to the BO2 content is within the above range, the coating layer is stable, and the electrochemical performance and thermal stability of the battery including the positive electrode active material are excellent. The ratio of the Li2B3O6 content to the BO2 content may be specifically 0.02 to 0.05 in order to further improve the rate characteristics, life characteristics, and gas generation of the battery.

[0076] The coating layer may have a thickness of 5 nm to 10 nm. In this case, since the coating layer has a thin and uniform surface, the rate characteristic or life characteristic of the battery including the positive electrode active material according to the present invention can be improved.

[0077] positive electrode The present invention can also provide a positive electrode for a lithium secondary battery, which contains the above-mentioned positive electrode active material.

[0078] Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector and including the above-mentioned positive electrode active material.

[0079] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the current collector to increase the adhesive force of the positive electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0080] The positive electrode active material layer may contain a conductive material and a binder in addition to the positive electrode active material.

[0081] Here, the positive electrode active material may be included in an amount of 80% by weight to 99% by weight, more specifically, 85% by weight to 98% by weight, based on the total weight of the positive electrode active material layer. When included in the above content range, excellent capacity characteristics can be exhibited.

[0082] In this case, the conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery to be constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and one or more of these can be used alone or in combination. The conductive material can be included in an amount of 1% by weight to 30% by weight based on the total weight of the positive electrode active material layer.

[0083] The binder serves to improve the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 wt% to 30 wt% based on the total weight of the positive electrode active material layer.

[0084] The positive electrode can be manufactured by a normal positive electrode manufacturing method, except for using the positive electrode active material. Specifically, the positive electrode can be manufactured by applying a positive electrode mixture manufactured by mixing or dispersing the positive electrode active material and, optionally, a binder and a conductive material in a solvent onto a positive electrode current collector, followed by drying and rolling. Here, the types and contents of the positive electrode active material, binder, and conductive material are as described above. In addition, as another method, the positive electrode can also be manufactured by casting the positive electrode mixture onto another support, peeling it off from the support, and laminating the film obtained on the positive electrode current collector.

[0085] The solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and one or more of these may be used alone or in combination. The amount of the solvent used may be sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to provide a viscosity that allows excellent thickness uniformity during subsequent coating for the manufacture of a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.

[0086] Lithium secondary battery In addition, the present invention can provide an electrochemical device including the positive electrode. The electrochemical device can be, for example, a battery or a capacitor, and more specifically, a lithium secondary battery.

[0087] The lithium secondary battery specifically includes a positive electrode, a negative electrode facing the positive electrode, and a separator and an electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.

[0088] Also, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0089] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0090] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of usually 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0091] The negative electrode active material layer includes a negative electrode active material, and optionally a binder and a conductive material.

[0092] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β(0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a thin film of metallic lithium may be used as the negative electrode active material. In addition, the carbon material may be either low-crystalline carbon or high-crystalline carbon. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.

[0093] The negative electrode active material may be included in an amount of 80% by weight to 99% by weight based on the total weight of the negative electrode active material layer.

[0094] The binder is a component that helps bind the conductive material, active material, and current collector, and can be added in an amount of 0.1% by weight to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0095] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0096] The negative electrode active material layer can be manufactured by coating a negative electrode mixture, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent, on a negative electrode current collector and drying the coating. Alternatively, the negative electrode mixture can be cast on a separate support, and then peeled off from the support to obtain a film, which can be laminated on the negative electrode current collector.

[0097] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte solution is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, etc., can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used as a single layer or a multilayer structure.

[0098] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0099] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0100] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethanol and isopropyl alcohol, nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of the battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, so that the electrolyte can exhibit excellent performance.

[0101] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0102] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, in order to improve the life characteristics of the battery, suppress the decrease in the capacity of the battery, and improve the discharge capacity of the battery. In this case, the additives may be contained in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.

[0103] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0104] Therefore, according to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0105] The battery module or battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0106] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0107] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but also preferably as a unit battery in a medium- to large-sized battery module including a large number of battery cells.

[0108] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0109] Manufacturing Example Ni 0.86 Co 0.05 Mn 0.07 Al 0.02 A precursor having a composition represented by (OH)2 was mixed with LiOH in a molar ratio of 1:1.05, and then calcined at 780°C for 10 hours in an oxygen atmosphere to obtain Li[Ni 0.86 Co 0.05 Mn 0.07 Al 0.02 ]O2 was prepared.

[0110] Examples and Comparative Examples Example 1 100 parts by weight of the lithium transition metal oxide prepared in the preparation example was mixed with 100 parts by weight of deionized water (first washing solution), and the mixture was washed with water for 5 minutes at 25°C, and then filtered with a filter press for 5 minutes. Then, 25 parts by weight of deionized water (second washing solution) was passed through 100 parts by weight of the lithium transition metal oxide for 2 minutes at 25°C using a filter press, and the mixture was dried in a vacuum oven at 130°C for 12 hours or more. H3BO3 and LiOH were mixed with the dried lithium transition metal oxide at 1000 ppm and 160 ppm by weight, respectively, and then heat-treated at 300°C for 5 hours in an air atmosphere to produce a positive electrode active material in which a coating layer containing Li-BO solid solution was formed on the lithium transition metal oxide.

[0111] Example 2 A positive electrode active material was prepared in the same manner as in Example 1, except that H3BO3 and LiOH were mixed with the dried lithium transition metal oxide in amounts of 1000 ppm and 224 ppm by weight, respectively, based on the dried lithium transition metal oxide.

[0112] Example 3 A positive electrode active material was prepared in the same manner as in Example 1, except that H3BO3 and LiOH were mixed with the dried lithium transition metal oxide in amounts of 1000 ppm and 288 ppm by weight, respectively, based on the dried lithium transition metal oxide.

[0113] Comparative Example 1 100 parts by weight of the lithium transition metal oxide prepared in Preparation Example was mixed with 100 parts by weight of deionized water, washed for 5 minutes at 25°C, filtered for 5 minutes using a filter press, and dried for 12 hours or more in a vacuum oven at 130°C. H3BO3 was mixed with the dried lithium transition metal oxide in an amount of 1000 ppm by weight based on the dried lithium transition metal oxide, and then heat-treated at 300°C for 5 hours in an air atmosphere to prepare a positive electrode active material in which a coating layer containing a Li-BO solid solution was formed on the lithium transition metal oxide.

[0114] Comparative Example 2 100 parts by weight of the lithium transition metal oxide prepared in Preparation Example was mixed with 100 parts by weight of deionized water, washed for 5 minutes at 25°C, filtered for 5 minutes using a filter press, and dried for 12 hours or more in a vacuum oven at 130°C. H3BO3 and LiOH were mixed with the dried lithium transition metal oxide at 1000 ppm and 224 ppm by weight, respectively, and then heat-treated at 300°C for 5 hours in an air atmosphere to prepare a positive electrode active material in which a coating layer containing Li-BO solid solution was formed on the lithium transition metal oxide.

[0115] Comparative Example 3 A positive electrode active material was produced in the same manner as in Example 1, except that only H3BO3 was mixed with the dried lithium transition metal oxide in an amount of 1000 ppm by weight based on the dried lithium transition metal oxide.

[0116] Comparative Example 4 100 parts by weight of the lithium transition metal oxide prepared in the preparation example was mixed with 100 parts by weight of deionized water (first washing solution), washed with first water at 25°C for 5 minutes, and then filtered with a filter press for 5 minutes. Then, 25 parts by weight of deionized water (second washing solution) was mixed with 100 parts by weight of the lithium transition metal oxide, washed with second water at 25°C for 5 minutes, and then filtered with a filter press for 5 minutes. Then, the mixture was dried in a vacuum oven at 130°C for 12 hours or more. H3BO3 and LiOH were mixed with the dried lithium transition metal oxide at 1000 ppm and 160 ppm by weight, respectively, and then heat-treated at 300°C for 5 hours in an air atmosphere to prepare a positive electrode active material in which a coating layer containing Li-BO solid solution was formed on the lithium transition metal oxide.

[0117] [Table 1]

[0118] Experimental Example Experimental Example 1: Confirmation of the type and content of Li-BO solid solution The surface analysis of the positive electrode active materials produced in the examples and comparative examples was carried out to confirm the type and content of the Li-BO solid solution contained in the coating layer, which are shown in the following Table 2. Specifically, the surface analysis of the positive electrode active materials was carried out by secondary ion mass spectrometry (SIMS), using a TOF-SIMS5 manufactured by IonTOF (Germany), under the following conditions.

[0119] Negative mode: 1) Primary Ion: Bi3 + 30keV 2)Field of View: 100μm×100μm 3) Raster size: 256μm×256μm 4) Cycle time: 100μs 5) Scan: 15 times

[0120] [Table 2] Experimental example 2: Half-cell characterization Lithium secondary batteries were produced using the positive electrode active materials produced in the Examples and Comparative Examples, and the charge / discharge capacity, capacity retention rate at high temperature, and resistance increase rate of each lithium secondary battery were evaluated.

[0121] Specifically, the positive electrode active materials prepared in the examples and comparative examples were mixed with carbon black conductive material and PVdF binder in a weight ratio of 97.5:1.0:1.5 in NMP solvent to prepare positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector, dried at 130°C, and rolled to prepare a positive electrode. Meanwhile, a Li metal disk was used as the negative electrode active material. An electrode assembly was prepared by interposing a separator between the positive electrode and negative electrode prepared as above, and the electrode assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a lithium secondary battery. Here, an electrolyte obtained by dissolving 1M LiPF6 in an organic solvent of EC / EMC / DMC (3 / 3 / 4, vol%) was injected to prepare a lithium secondary battery.

[0122] The lithium secondary battery prepared as above was charged at a constant current of 0.1C at 25°C until the voltage reached 4.3V, and then discharged at a constant current of 0.1C until the voltage reached 3.0V. The charge capacity and discharge capacity are shown in Table 3 below. In order to confirm the rate characteristics, the lithium secondary battery prepared as above was charged and discharged at a constant current of 0.1C, a constant current of 2.0C, and a constant current of 0.33C in the range of 25°C and 3.0 to 4.3V to obtain the discharge capacity value at each C-rate, and the percentage of the discharge capacity value at the constant current of 2.0C to the discharge capacity value at the constant current of 0.1C and the percentage of the discharge capacity value at the constant current of 0.33C to the discharge capacity value at the constant current of 0.1C are shown in Table 3 below.

[0123] The capacity of the lithium secondary battery was measured by repeating 30 charge-discharge cycles, in which the battery was charged at a constant current of 0.33 C at 45° C. in the range of 3.0 to 4.3 V until the voltage reached 4.3 V, and then discharged at a constant current of 0.33 C until the voltage reached 3.0 V. In particular, the ratio of the 30th cycle capacity to the 1st cycle capacity was taken as the capacity retention rate, which is shown in Table 3 below. In addition, the voltage drop for 60 seconds after the start of discharge in each cycle was measured, and this was divided by the applied current value to measure the resistance at high temperature. In particular, the increase rate of the 30th cycle resistance value to the 1st cycle resistance value is shown in Table 3 below.

[0124] [Table 3]

[0125] It can be confirmed that the batteries including the positive electrode active materials of Examples 1 to 3 manufactured by the manufacturing method according to the present invention have both superior rate characteristics and capacity retention rate, and a lower resistance increase rate, compared to the batteries including the positive electrode active materials of Comparative Examples 1 to 4. In particular, it can be confirmed that the battery including the positive electrode active material of Example 2 has superior rate characteristics and capacity retention rate, and a lower resistance increase rate.

[0126] Experimental Example 3: Evaluation of high temperature storage of monocell and evaluation of volume change Monocells were manufactured using the positive electrode active materials manufactured in the examples and comparative examples, and high-temperature storage evaluation and volume change evaluation were performed for each.

[0127] Specifically, the positive electrode active materials prepared in the examples and comparative examples were mixed with carbon black conductive material and PVdF binder in a weight ratio of 97.5:1.0:1.5 in NMP solvent to prepare positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector, dried at 130°C, and rolled to prepare a positive electrode. A negative electrode active material, which was a mixture of natural graphite and artificial graphite in a ratio of 9:1, conductive material, additives, and binders, was mixed in an NMP solvent in a weight ratio of 95.6:1.0:2.3:1.1 to prepare a negative electrode slurry, which was applied to one side of a copper current collector, dried, and rolled to prepare a negative electrode. An electrode assembly was prepared by interposing a separator between the positive and negative electrodes prepared as above, and the electrodes were laminated at 80°C to properly bond them, and aluminum and nickel tabs were welded, and the assembly was placed in an aluminum pouch and electrolyte was injected to prepare a monocell. Here, the electrolyte used was prepared by dissolving 0.7M LiPF6 in an organic solvent of EC / EMC (3 / 7, vol%).

[0128] -High temperature storage rating (Initial HPPC (Hybrid Pulse Power Characterization)) The mono cell manufactured as described above was charged at 25°C for 3 hours at a current of 0.1C, one side of the pouch was opened, vacuum degassed, and resealed. Then, charge and discharge were repeated three times at a current of 0.33C, and then charging was performed at a current of 0.33C. After discharging to SOC 50, a current of 2.5C was applied for 10 seconds while measuring the voltage, and the resistance was calculated from the measured value. The capacity value of Initial HPPC in Table 4 below indicates the discharge capacity value of the third cycle.

[0129] (High temperature storage RPT) After the HPPC evaluation was completed, the mono cell was charged to SOC 100 and then stored in a 60°C oven for one week. After one week, it was charged and discharged three times at a current of 0.33C in a room temperature chamber, and the capacity and resistance were measured from the discharge data of the third cycle. After the measurement, the cell was stored in a 60°C oven again, and then taken out every week and evaluated in the same way as the first week.

[0130] The results of the high temperature storage evaluation are shown in Table 4 below.

[0131] In Table 4 below, the retention rate indicates the ratio of the capacity maintained to the capacity at 0 weeks, and the increase rate indicates the ratio of the resistance increased to the resistance at 0 weeks.

[0132] [Table 4]

[0133] -Evaluation of volume changes The mono cell prepared as above was charged at 25°C for 3 hours at a current of 0.1C, and then one side of the pouch was opened, vacuum degassed, and resealed. Then, charge and discharge were repeated three times at a current of 0.33C, and then charging was performed at a current of 0.33C. The charged mono cell was opened, the negative electrode was separated, and the positive electrode and the separator were alternately stacked three by three, then placed in an aluminum pouch, and electrolyte was injected to prepare a cell for volume measurement. Here, an electrolyte prepared by dissolving 0.7M LiPF6 in an organic solvent of EC / EMC (3 / 7, vol%) was used as the electrolyte. The prepared cells were stored in an oven at 60°C, and then taken out at weekly intervals to measure the volume change rate at room temperature for 12 weeks. The volume change rate of each cell relative to the initial volume is shown in Table 5.

[0134] [Table 5]

[0135] It can be confirmed that the monocells including the positive electrode active materials of Examples 1 to 3 produced by the production method according to the present invention have superior high-temperature storage characteristics and small monocell volume change, and thus have a low amount of gas generation, compared to the monocells including the positive electrode active materials of Comparative Examples 1 to 4. In particular, it can be confirmed that the monocell including the positive electrode active material of Example 2 has a significantly low amount of gas generation.

[0136] In other words, according to the method for producing a positive electrode active material of the present invention, by controlling the surface by the water washing process in step (C) and forming a coating layer on the surface-controlled positive electrode active material in step (D) using a boron-containing raw material and at least one lithium-containing raw material selected from LiOH and Li2CO3, it is possible to minimize surface deterioration of the positive electrode active material that occurs during the water washing process, effectively control residual lithium, and form a uniform coating layer on the surface of the positive electrode active material. As a result, it is found that a battery using the positive electrode active material produced by the method of the present invention has excellent performance, particularly electrochemical performance and thermal stability.

Claims

1. (A) providing a lithium transition metal oxide; (B) mixing the lithium transition metal oxide with a first washing solution to first wash the lithium transition metal oxide, and then performing a first filtration; (C) performing a second washing and a second filtration simultaneously on the lithium transition metal oxide that has been subjected to step (B) with a second washing solution using a filtration device capable of simultaneously washing with water and filtering; (D) drying the lithium transition metal oxide obtained by step (C), and then mixing the dried lithium transition metal oxide with a coating element-containing raw material and heat-treating the mixture to form a coating layer; The coating element-containing source material is a boron-containing source material, LiOH, Li 2 CO 3 and Li 2 1. A method for producing a positive electrode active material comprising:

2. The method for producing a positive electrode active material according to claim 1 , wherein the lithium transition metal oxide contains nickel in an amount of 70 mol % or more of all metals other than lithium.

3. 2. The method for producing a positive electrode active material according to claim 1, wherein a content of the second washing solution is 10 parts by weight to 50 parts by weight with respect to 100 parts by weight of the first washing solution.

4. 2. The method for producing a positive electrode active material according to claim 1, wherein the content of the first washing solution is 50 parts by weight to 150 parts by weight based on 100 parts by weight of the lithium transition metal oxide.

5. 2. The method for producing a positive electrode active material according to claim 1, wherein the content of the second washing solution is 5 parts by weight to 50 parts by weight based on 100 parts by weight of the lithium transition metal oxide.

6. 2. The method for producing a positive electrode active material according to claim 1, wherein a sum of a content of the first washing solution and a content of the second washing solution is 55 parts by weight to 150 parts by weight based on 100 parts by weight of the lithium transition metal oxide.

7. The LiOH, Li 2 CO 3 and Li 2 2. The method for producing a positive electrode active material according to claim 1, wherein the one or more lithium-containing raw materials selected from O are added in an amount of 160 ppm to 500 ppm by weight to the dried lithium transition metal oxide.

8. a lithium transition metal oxide; a coating layer formed on the lithium transition metal oxide; The coating layer includes a Li-B-O solid solution, and the Li-B-O solid solution is B 2 50% by weight to 60% by weight of LiB 2 O 3 2% by weight to 7% by weight, Li 2 B 3 O 6 A positive electrode active material comprising 1% by weight to 5% by weight of the above.

9. The positive electrode active material according to claim 8 , wherein the lithium transition metal oxide contains nickel in an amount of 70 mol % or more of all metals other than lithium.

10. The BO 2 LiB content 2 O 3 The positive electrode active material according to claim 8, wherein the ratio of the contents of is 0.05 to 0.

20.

11. The BO 2 Li relative to the content 2 B 3 O 6 The positive electrode active material according to claim 8, wherein the ratio of the contents of is 0.01 to 0.

10.

12. A positive electrode comprising the positive electrode active material according to any one of claims 8 to 11.

Citation Information

Patent Citations

  • Positive electrode active material for lithium secondary battery, method for producing the same, and lithium secondary battery including the same

    JP2021508658A

  • Positive active material for rechargeable lithium battery, method of preparing the same, and rechargeable lithium battery including the same