Lithium metal electrode, its manufacturing method and lithium secondary battery including the same

A lithium metal electrode with a protective layer of amorphous carbon and ceramic particles addresses dendrite formation and low efficiency issues, enhancing battery performance and lifespan.

JP2024540630AActive Publication Date: 2024-10-31RES INST OF IND SCI & TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024530433
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-02
Filing Date
2022-10-20
Publication Date
2024-10-31
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

Existing lithium metal electrodes in secondary batteries face issues such as lithium dendrite formation, reduced lifespan due to electronically conductive materials, and low initial Coulombic efficiency caused by amorphous carbon in the non-negative electrode coating layer, which hinder their use in electric vehicles.

Method used

A lithium metal electrode with a protective layer containing amorphous carbon and lithium ion conduction-enhancing ceramic particles is developed, which controls dendrite formation and improves charging and discharging characteristics.

Benefits of technology

The protective layer enhances lithium ion conduction, reduces dendrite formation, and increases the initial coulombic efficiency, leading to improved charge/discharge performance and extended battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540630000001_ABST
    Figure 2024540630000001_ABST
Patent Text Reader

Abstract

The present invention relates to a lithium metal electrode, a manufacturing method thereof, and a lithium secondary battery including the same. According to one embodiment, a lithium metal electrode may be provided that includes a current collector and a metal layer including a lithium component, the metal layer being located on at least one surface of the current collector, and a protective layer including amorphous carbon and lithium ion conduction promoting ceramic particles is formed on the metal side surface.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present embodiment relates to a lithium metal electrode, a method for producing the same, and a lithium secondary battery including the same. [Background technology]

[0002] 2. Description of the Related Art In recent years, with the explosive demand for electric vehicles and the demand for increased driving distances, secondary batteries having high capacity and high energy density have been actively developed worldwide in order to meet this demand.

[0003] In order to reduce the cost and improve the energy density of secondary batteries, it has been proposed to use a lithium metal electrode as the negative electrode of a lithium secondary battery.

[0004] In order to form such a lithium metal anode, a method of rolling a lithium foil onto a current collector is generally used, but when rolling, it is difficult to realize a lithium metal anode having a thickness of 20 μm or less.

[0005] On the other hand, in order to realize a secondary battery having a high energy density by substantially using a lithium metal negative electrode, a thin-film lithium metal negative electrode having a thickness of 10 to 20 μmm is required.

[0006] However, when lithium metal is used as the negative electrode in an all-solid-state battery, a highly resistive phase is generated due to the reaction between lithium and the all-solid-state electrolyte, and lithium dendrites are continuously generated due to local non-uniformity in current density during charging and discharging, or highly resistive lithium by-products are generated, resulting in failure due to short circuit or overvoltage during charging and discharging, or a decrease in capacity.

[0007] To solve these problems, various methods have been proposed, such as forming a protective coating layer or a lithium alloy layer on the lithium metal to prevent reactions with solid-state batteries and the precipitation and growth of lithium dendrites. However, sufficient life characteristics have yet to be achieved for use in electric vehicles (EVs).

[0008] To meet these needs, recent Korean Patent Application No. 10-2018-0136041 (Patent Document 1), Korean Patent Application No. 10-2019-0134804 (Patent Document 2), Korean Patent Application No. 10-2020-7006820 (Patent Document 3), Nature Energy 5, 299 (2020) (Non-Patent Document 1), etc. have attempted to solve the above problem by precipitating lithium during charging and discharging using a non-anode coating layer that is a mixture of amorphous carbon and silver (Ag) nanoparticles. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Korean Patent Application No. 10-2018-0136041 [Patent Document 2] Korean Patent Application No. 10-2019-0134804 [Patent Document 3] Korean Patent Application No. 10-2020-7006820 [Non-patent literature]

[0010] [Non-Patent Document 1] Nature Energy 5, 299(2020)

[0011] However, there is a problem that materials with electronic conductivity, such as lithium-based alloys or lithium-containing compounds, are generated within the anode coating layer or at the interface during charging and discharging, which induces current concentration and lithium dendrites, shortening the lifespan.

[0012] In addition, the initial coulombic efficiency is low due to the irreversible reaction caused by amorphous carbon, which is the main material of the anode coating layer.

[0013] To solve these problems, a sacrificial positive electrode is used, and a large amount of precious metal nanoparticles is also used, which significantly reduces price competitiveness and makes commercialization difficult.

[0014] Therefore, there is a need to develop a technology that can manufacture electrodes that have excellent initial efficiency and excellent charge / discharge characteristics. Summary of the Invention [Problem to be solved by the invention]

[0015] As described above, this embodiment aims to solve the problems of lithium dendrite formation and reduced lifespan due to electronic conductive materials in the anode layer, the problem of reduced initial Coulombic efficiency due to initial irreversibility caused by amorphous carbon in the anode coating layer and the problem of having to use a sacrificial cathode to compensate for this, and the problem of having to use a large amount of precious metal nanoparticles such as silver (Ag) to form an alloy with lithium during charging.

[0016] Another object of the present invention is to provide a lithium metal electrode having excellent charge / discharge characteristics by preventing dendrite formation through a protective layer contained in the electrode layer, a method for producing the same, and a lithium secondary battery including the same. [Means for solving the problem]

[0017] According to an embodiment, the lithium metal electrode includes a current collector, a metal layer including a lithium alloy disposed on at least one surface of the current collector, and a protective layer disposed on the metal layer, the protective layer including amorphous carbon and lithium ion conduction promoting ceramic particles. Effect of the Invention

[0018] According to this embodiment, a lithium ion conduction promoting protective layer is formed on a lithium metal electrode, and the formation of lithium dendrites during the charge and discharge process of a lithium secondary battery to which this is applied can be controlled, thereby mitigating the decrease in the life span of the lithium secondary battery.

[0019] In addition, the decrease in the initial coulombic efficiency of the lithium secondary battery can be controlled, and the charge / discharge characteristics can be significantly improved. [Brief description of the drawings]

[0020] [Figure 1] 1 is a schematic diagram illustrating a lithium metal electrode manufactured according to an embodiment. [Diagram 2] FIG. 13 is a schematic diagram of a lithium metal electrode according to another embodiment. [Diagram 3] 1A to 1C are diagrams illustrating a process for manufacturing a lithium metal electrode according to an embodiment; [Figure 4] 4 is a SEM photograph showing a cross section of a current collector on which an alloy material coating layer is formed in the process of producing a lithium metal electrode according to Example 1. [Diagram 5] 3 is a SEM photograph showing a cross section of a current collector on which an alloy material coating layer and a lithium ion conduction promoting protective layer are formed in the process of producing a lithium metal electrode according to Example 1. [Figure 6a] 1 is a SEM photograph showing a cross section of a lithium metal electrode produced in Example 1. [Figure 6b] 2 is a SEM photograph showing a cross section of the lithium metal electrode produced in Comparative Example 1. [Figure 6c] 4 is a SEM photograph showing a cross section of a lithium metal electrode produced in Comparative Example 2. [Figure 6d] 1 is a SEM photograph showing a cross section of a lithium metal electrode produced in Comparative Example 3. [Figure 7a] 1 is a photograph showing the surface microstructure of the lithium metal electrode prepared in Example 1. [Figure 7b] 3 is a photograph showing the results of a component analysis of the lithium metal electrode produced in Example 1. [Figure 8a] 3 is a photograph showing the surface microstructure of the lithium metal electrode prepared according to Comparative Example 1. [Figure 8b] 3 is a photograph showing the results of a component analysis of the lithium metal electrode produced in Comparative Example 1. [Figure 9a]4 is a photograph showing the surface microstructure of the lithium metal electrode prepared according to Comparative Example 2. [Figure 9b] 4 is a photograph showing the results of a component analysis of the lithium metal electrode produced in Comparative Example 2. [Figure 10a] 4 is a photograph showing the surface microstructure of the lithium metal electrode prepared according to Comparative Example 3. [Figure 10b] 4 is a photograph showing the results of a component analysis of the lithium metal electrode produced in Comparative Example 3. [Figure 11] 1 is a diagram showing the results of evaluating the initial effects of secondary batteries manufactured according to Example 1 and Comparative Examples 1 to 3. [Figure 12] 1 is a diagram showing the results of evaluating the charge-discharge life of secondary batteries produced in Example 1 and Comparative Examples 1 to 3. [Figure 13] 1 is a diagram showing the results of evaluating the charge-discharge life of secondary batteries produced in Examples 1 to 4 and Comparative Example 2. [Figure 14] FIG. 1 is a schematic diagram of a secondary battery to which a lithium metal electrode manufactured according to the present invention is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, a first part, component, region, layer or section described below can be referred to as a second part, component, region, layer or section without departing from the scope of the present invention.

[0022] The terminology used herein is merely for the purpose of referring to specific embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. As used herein, the meaning of "comprises" is intended to embody certain properties, regions, integers, steps, operations, elements and / or components, and does not exclude the presence or addition of other properties, regions, integers, steps, operations, elements and / or components.

[0023] When an element is described as being "on" or "above" another element, it may be exactly on or above the other element, or it may have other elements between them. In contrast, when an element is referred to as being "directly on" another element, there are no other elements between them.

[0024] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted as having a meaning consistent with the relevant technical literature and the presently disclosed content, and are not interpreted in an ideal or very formal sense unless defined.

[0025] Hereinafter, the present invention will be described in detail with reference to examples, which are presented by way of example only and are not intended to limit the present invention, which is defined only by the scope of the claims that follow.

[0026] FIG. 1 is a diagram illustrating a lithium metal electrode manufactured according to one embodiment, FIG. 2 is a diagram illustrating a lithium metal electrode according to another embodiment, and FIG. 3 is a diagram illustrating a method of manufacturing a lithium metal electrode for a secondary battery according to one embodiment.

[0027] Referring to FIG. 1, a lithium metal electrode 100 according to one embodiment includes a current collector 11 and a metal layer 12 located on at least one side of the current collector 11, and a protective layer 30 located on the other side of the metal layer 12 facing the current collector 11.

[0028] The current collector 11 is for electrical connection within the lithium secondary battery.

[0029] The current collector 11 may have the form of a thin film (foil), but is not limited thereto. For example, the current collector 11 may have the form of a mesh, a foam, a rod, a wire, or a sheet made of woven wire or fiber.

[0030] The material of the current collector 11 may be any material that is electrically conductive and has limited reaction with lithium, such as copper, nickel, titanium, stainless steel, gold, platinum, silver, tantalum, ruthenium, and alloys thereof, carbon, conductive polymers, and composite fibers in which a conductive layer is coated on a non-conductive polymer, or a combination thereof.

[0031] If the thickness of the current collector 11 is large, the battery weight increases and the energy density of the battery decreases, and if the thickness of the current collector 11 is small, there is a risk of overheating during high current operation and the current collector 11 may be damaged by tension during the battery manufacturing process. Therefore, the thickness of the current collector 11 can be in the range of 1 μm to 50 μm.

[0032] The metal layer 12 includes a lithium alloy layer 21 located on the current collector 11 and containing a lithium alloy, and a lithium metal layer 41 located on the lithium alloy layer 21. Here, the lithium alloy layer 21 may be a layer containing a lithium alloy in which a parent lithium component contained in the coating layer of the current collector 11 and lithium deposited from the lithium source are alloyed by applying a current between the current collector 11 and a lithium source. When a high current is applied to perform an electrodeposition process in order to increase the electrodeposition speed during the formation of the metal layer, there is a problem that the performance of the lithium secondary battery is reduced. However, when the metal layer 12 is formed in a structure including a lithium alloy layer 21 containing a lithium component, even if a high current is applied to perform the electrodeposition process, it is possible to prevent excessive generation of fine lithium particles and destruction of the film, which is a surface protective layer of the lithium metal layer already formed in the electrodeposition process.

[0033] More specifically, since the metal layer 12 of the present embodiment includes a lithium alloy layer containing a lithium component, when a lithium metal layer is formed on the lithium alloy layer by applying a high current in an electrodeposition process, the initially generated lithium particles are induced to grow well to form particles with a coarse structure, and at the same time, the lithium metal layer, and consequently the metal layer 12, can have a uniform surface.

[0034] Therefore, the performance of the secondary battery using the lithium metal electrode of this embodiment, specifically the charge and discharge characteristics, can be significantly improved. Also, even when a high current is applied to perform a high-speed electrodeposition process, a high-performance lithium metal electrode for secondary batteries can be manufactured, so the productivity of the lithium metal electrode for secondary batteries can be significantly improved.

[0035] The lithium alloy layer 21 may be an alloy of lithium and a parent lithium metal, and the parent lithium metal may be one or more selected from the group consisting of In, Ag, Sn, Zn, Si, Al, and Bi, but is not limited thereto.

[0036] In this embodiment, the lithium alloy layer includes a lithium-phile metal. When the lithium alloy layer includes such a lithium-phile metal, since the lithium-phile metal has high electronic conductivity, electrons are smoothly supplied from the current collector, and lithium ions are reduced, so that the electrodeposition of the lithium metal layer is easily performed.

[0037] Meanwhile, the metal layer serves to facilitate more efficient deposition of lithium beneath the protective layer during charging of the battery.

[0038] The thickness of the metal layer 12 can be in the range of 1 μm to 100 μm, more specifically, 5 μm to 30 μm.

[0039] If the thickness of the metal layer 12 is too thick, when the lithium metal electrode of this embodiment is applied to a secondary battery, there is a problem that the weight and volume of the battery increase and the energy density decreases. In addition, when forming the metal layer 12, the time and cost of the electrodeposition process increase in proportion to the thickness, so the thickness of the metal layer 12 is preferably 100 μm or less.

[0040] In addition, if the thickness of the metal layer 12 is too thin, when the lithium metal electrode of this embodiment is applied to a secondary battery, there is a problem that the charge and discharge life of the battery is reduced. Specifically, during charging and discharging of the battery, lithium in the battery is gradually consumed due to a side reaction between the lithium contained in the negative electrode active material layer, i.e., the metal layer of the present invention, and the electrolyte, and the battery capacity is reduced. However, if the thickness of the metal layer 12 is thin, the amount of lithium available to replenish the lithium consumed during charging and discharging is reduced, thereby reducing the charge and discharge life of the battery. Therefore, it is preferable that the thickness of the metal layer 12 is 1 μm or more.

[0041] The protective layer 30 is located on the metal layer 12 and includes amorphous carbon and ceramic particles that promote lithium ion conductivity.

[0042] When lithium metal is used as the negative electrode in an all-solid-state battery, high resistance is generated due to the reaction between the all-solid-state electrolyte and lithium, and lithium dendrites are continuously generated due to localized non-uniformity in current density during charging and discharging, or highly resistive lithium by-products are generated, which can cause failure due to short circuit or overvoltage during charging and discharging, or reduce the battery capacity.

[0043] However, as in this embodiment, the protective layer containing amorphous carbon and lithium ion conductivity promoting ceramic particles can improve not only the output characteristics and life characteristics of the lithium metal electrode, but also the structural safety.

[0044] More specifically, the lithium metal electrode of the present embodiment includes a protective layer 30 including amorphous carbon and lithium ion conductivity promoting ceramic particles, which can promote the movement of lithium ions on the electrode surface during charging and discharging, and can suppress the generation of electronically conductive materials at the interface. Also, the protective layer 30 can play a role in reducing electronic conductivity inside the electrode.

[0045] Therefore, the performance of the secondary battery to which the lithium metal electrode according to this embodiment is applied, specifically, the output characteristics and life characteristics of the battery, can be significantly improved.

[0046] The amorphous carbon may be at least one selected from the group consisting of acetylene black, super P black, carbon black, denka black, activated carbon, graphite, hard carbon, and soft carbon, but is not limited thereto.

[0047] Representative examples of the lithium ion conductivity promoting ceramic particles include Li2TiO3, LiNbO3, LiTaO3, LiZrO3, and Li4Ti5O 12The lithium ion conductive ceramic particles may be one or more selected from the group consisting of particles that promote lithium ion conduction and inhibit electron conduction, such as, but not limited to, Li2CO3, Li3BO3, SrTiO3, etc. The lithium ion conductive ceramic particles promote lithium ion conduction and inhibit electron conduction in and at the interface of the protective layer during the charging process of a battery using a lithium negative electrode, thereby allowing lithium to easily move to the lower part of the protective layer.

[0048] In this embodiment, the average particle size D(50) of the lithium ion conduction promoting ceramic particles may be in the range of 100 nm to 1,000 nm. If the average particle size D(50) of the lithium ion conduction promoting ceramic particles is less than 100 nm, the distribution of the ceramic particles in the coating layer may be uneven due to aggregation between primary particles, and if it is more than 1,000 nm, the large particles may act as a resistance layer, resulting in a decrease in lithium ion conductivity.

[0049] In particular, such a material does not react well with the sulfide-based electrolyte material of the all-solid-state battery and has excellent chemical stability, which is advantageous for improving the interface stability and charge / discharge life of the all-solid-state battery. The ion conduction promoting protective layer may be formed by preparing the composite in a slurry form and applying the same. In order to prepare the slurry, a binder may be further included.

[0050] The lithium ion conduction promoting protective layer may include amorphous carbon and lithium ion conduction promoting ceramic particles in a weight ratio of 99.5:0.5 to 40:60, specifically, 98.5:1.5 to 50:50, and more specifically, 97:3 to 70:30.

[0051] If the amount of the lithium ion conduction promoting ceramic particles is too small, the effect of promoting lithium ion conduction by mixing the lithium ion conduction promoting ceramic particles cannot be sufficiently obtained, and if the amount of the lithium ion conduction promoting ceramic particles is too large, the connection between the ceramic particles at room temperature is poor, so the density of the protective layer decreases, which may actually hinder lithium ion conduction.In addition, if an excessive amount of ceramic particles, which have a relatively high density compared to amorphous carbon, is included, there is a problem that a decrease in battery energy density is caused.

[0052] On the other hand, the protective layer of this embodiment may contain a binder.

[0053] In this case, the binder may be an aqueous binder, and the aqueous binder may be at least one selected from the group consisting of a rubber-based binder selected from the group consisting of acrylonitrile butadiene rubber, styrene butadiene rubber (SBR), and acrylic rubber, and a polymer resin such as hydroxyethyl cellulose, carboxymethyl cellulose, and polyvinylidene fluoride, but is not limited thereto.

[0054] Here, the binder may be added in an amount of 1 to 15 parts by weight, more specifically 3 to 10 parts by weight, based on the weight of the slurry formed by mixing the lithium ion conductivity promoting ceramic particles, amorphous carbon and water.

[0055] When the amount of binder added satisfies the above range, the particles constituting the protective layer are efficiently bound to form a protective layer with excellent performance without inducing a decrease in battery energy density due to an increase in weight and volume, and the life characteristics of the secondary battery can be further improved. If the amount of binder added is too small, there is a problem that the bonding force between the particles is reduced when forming the protective layer, and if the amount of binder added is too large, there is a problem that not only does it cause a decrease in energy density, but also the resistance of the protective layer is greatly increased, hindering lithium ion conduction.

[0056] The thickness of the protective layer including the amorphous carbon, the lithium ion conduction promoting ceramic particles, and the binder may be in the range of 0.01 μm to 50 μm, more specifically, 1 μm to 20 μm. When the thickness of the protective layer satisfies the above range, the effect obtained by including the amorphous carbon and the lithium ion conduction promoting ceramic particles prevents lithium dendrites from being formed on the surface of the protective layer, and allows lithium ions to penetrate well through the inside of the protective layer, so that lithium can be precipitated from the lower surface of the protective layer. On the other hand, if the thickness of the protective layer including the amorphous carbon and the lithium ion conduction promoting ceramic particles is too thin, it is disadvantageous in that it cannot function as a protective layer. On the other hand, if the thickness of the protective layer is too thick, the resistance of the protective layer becomes too large, which may cause an increase in overvoltage during the operation of the secondary battery, and also causes a decrease in the battery energy density due to an increase in weight and volume. However, the thickness of the protective layer can be variably adjusted according to the design of the secondary battery structure.

[0057] Meanwhile, although not shown, the metal layer 12 of this embodiment may further include a coating layer (SEI, Solid-Electrolyte Interphase) located on the surface of the metal layer 12 .

[0058] The coating layer is formed by a reaction between the lithium metal of the electrodeposited lithium supply source and a plating solution during the manufacturing process of the metal layer 12, and the thickness, composition, characteristics, etc. of the coating can be controlled by adjusting the composition of the plating solution used and the conditions of the electrodeposition process.

[0059] The thickness of the coating layer can be, for example, in the range of 2 nm to 2 μm, and more specifically, 10 nm to 500 nm.

[0060] If the thickness of the coating layer located on the surface of the metal layer 12 is too thick, the lithium ion conductivity may decrease, the interface resistance may increase, and the charge / discharge characteristics may decrease when applied to a battery. Also, if the thickness of the coating layer is too thin, the coating layer may easily be washed away during application of the lithium metal electrode according to the embodiment to a battery.

[0061] Therefore, it is preferable that the coating layer be formed uniformly and densely over the entire surface of the metal layer 12 with a small thickness that satisfies the above-mentioned thickness range.

[0062] In this case, the coating layer may include one or more materials selected from the group consisting of Li-NCHO-based ionic compounds, Li-PCHO-based ionic compounds, LiF, and Li3N.

[0063] FIG. 2 is a schematic diagram of a lithium metal electrode according to another embodiment.

[0064] 2, a lithium metal electrode 100 for a secondary battery according to another embodiment includes a current collector 11 and a metal layer 12 formed by mixing lithium and a lithium alloy and located on at least one surface of the current collector 11. Here, the lithium alloy may be formed by applying a current between the current collector 11 and a lithium supply source to alloy a lithium parent component contained in a coating layer formed on the current collector 11 with lithium deposited from the lithium supply source.

[0065] In this case, the metal layer 12 may contain a lithium-loving metal, which may be, for example, one or more selected from the group consisting of In, Ag, Sn, Zn, Si, Al, and Bi, but is not limited thereto.

[0066] In this embodiment, the metal layer 12 contains a lithium-phile metal. When the metal layer 12 containing a lithium-phile metal is formed in this manner, the nucleation free energy can be lowered at the initial stage of nucleation of lithium particles in the electrodeposition process, so that a lithium metal layer having a coarse particle structure can be formed even under high current and overvoltage conditions.

[0067] In this embodiment, the thickness of the metal layer 12 may be in the range of 1 μm to 100 μm, more specifically, 5 μm to 30 μm. In this embodiment, when the metal layer 12 satisfies the above thickness range, it is possible to maximize the energy density of the battery while improving the charge and discharge life of the battery, as well as to minimize the time and cost of the electrodeposition process when forming the metal layer 12. If the thickness of the metal layer is too thin, the initial coulombic efficiency decreases due to initial irreversibility, and the charge and discharge performance decreases due to a lack of surplus lithium. On the other hand, if the thickness of the metal layer is too thick, there is a problem that not only the energy density of the battery decreases, but also the process time and the amount of metal raw material used when forming the metal layer increase.

[0068] Meanwhile, although not shown in FIG. 2, the metal layer of this embodiment may further include a coating layer located on the surface of the metal layer.

[0069] Such a coating layer is the same as that described in the lithium metal electrode for a secondary battery according to the above embodiment, and therefore a description thereof will be omitted here.

[0070] A method for manufacturing a lithium metal electrode according to an embodiment includes the steps of: forming a coating layer on at least one surface of a current collector using a coating composition including a lithium parent component; forming a protective layer on a surface of the coating layer using a slurry including amorphous carbon and lithium ion conduction promoting particles; positioning the current collector having the coating layer and protective layer formed thereon in a plating solution, and then positioning a lithium supply source at a predetermined distance from the protective layer; and applying a current between the current collector and the lithium supply source to form a metal layer including a lithium alloy in which the lithium parent component included in the coating layer and lithium deposited from the lithium supply source are alloyed.

[0071] In the step of forming a protective layer on the surface of the coating layer using the slurry including the amorphous carbon and the lithium ion conduction promoting ceramic particles, the lithium ion conduction promoting protective layer may include amorphous carbon and lithium ion conduction promoting ceramic particles in a weight ratio of 99.5:0.5 to 40:60, specifically, 98.5:1.5 to 50:50, and more specifically, 97:3 to 70:30.

[0072] First, a coating composition containing a lithium-prone metal is used to form an alloy material coating layer on at least one surface of a current collector.

[0073] In this case, the lithium-parent metal may be, for example, one or more selected from the group consisting of In, Ag, Sn, Zn, Si, Al, and Bi, but is not limited thereto.

[0074] The alloy material coating layer may be formed by at least one of electrolytic and electroless plating, sputtering, electron beam and thermal vapor deposition.

[0075] Meanwhile, in the step of forming the alloy material coating layer, the thickness of the alloy material coating layer formed on at least one surface of the current collector may be in the range of 0.001 μm to 10 μm, specifically, 0.01 μm to 1 μm, more specifically, 100 nm to 500 nm.

[0076] If the thickness of the alloy material coating layer is too thin, it is insufficient to perform the role of forming a lithium alloy with lithium, and if the thickness is too thick, a large amount of cost and time is consumed in forming the alloy material coating layer, resulting in a decrease in production efficiency and economic efficiency, an increase in the weight of the battery, and a decrease in energy density.

[0077] After the alloy material coating layer forming step, a protective layer is applied to the surface of the alloy material coating layer formed.

[0078] In this case, the protective layer is a lithium ion conduction promoting protective layer and may include amorphous carbon and lithium ion conduction promoting ceramic particles.

[0079] In this case, the amorphous carbon may be at least one selected from the group consisting of acetylene black, super-P black, carbon black, denka black, activated carbon, graphite, hard carbon and soft carbon, but is not limited thereto.

[0080] The lithium ion conductivity promoting ceramic particles are Li2TiO3, LiNbO3, LiTaO3, LiZrO3, Li4Ti5O 12 The lithium ion conductivity may be one or more selected from the group consisting of particles having low electronic conductivity and high lithium ion conductivity, such as Li2CO3, Li3BO3, SrTiO3, etc., but is not limited thereto.

[0081] Meanwhile, in this case, the lithium ion conduction promoting protective layer may contain a binder.

[0082] The binder may be an aqueous binder, and the aqueous binder may be at least one selected from the group consisting of a rubber-based binder selected from the group consisting of acrylonitrile-butadiene rubber, styrene-butadiene rubber (SBR), and acrylic rubber, and a polymer resin such as hydroxyethyl cellulose, carboxymethyl cellulose, and polyvinylidene fluoride, but is not limited thereto.

[0083] The lithium ion conduction promoting protective layer may be formed by applying a slurry prepared by mixing the amorphous carbon, the lithium ion conduction promoting ceramic particles, and a binder in water using at least one of a doctor blade method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, and a brush coating method.

[0084] Here, the lithium ion conduction promoting protective layer may include amorphous carbon and lithium ion conduction promoting ceramic particles in a weight ratio of 99.5:0.5, specifically, 98.5:1.5 to 50:50, and more specifically, 97:3 to 70:30.

[0085] The binder may be added in an amount of 0.5 to 10 parts by weight, more specifically 1 to 3 parts by weight, based on the weight of the lithium ion conductivity promoting ceramic particles, amorphous carbon and water mixed together.

[0086] Meanwhile, in the step of forming the lithium ion conduction promoting protective layer, the thickness of the lithium ion conduction promoting protective layer formed on the surface of the alloy material coating layer may be in the range of 0.01 μm to 50 μm, more specifically, 1 μm to 20 μm.

[0087] When the thicknesses of the alloy material coating layer and the lithium ion conduction promoting protective layer satisfy the above ranges, the lithium metal electrode for a secondary battery according to one embodiment can be manufactured to have a lithium metal electrode structure as shown in FIG. 1 or FIG. 2.

[0088] After the lithium ion conduction promoting protective layer forming step, the steps of positioning the current collector on which the alloy material coating layer and the lithium ion conduction promoting protective layer are sequentially formed in a plating solution, positioning a lithium supply source at a predetermined distance from the current collector, and applying a current between the current collector and the lithium supply source to form a metal layer are performed.

[0089] With reference to FIG. 3, the step of forming the metal layer will be described in more detail.

[0090] First, the current collector 11 having the alloy material coating layer 20 and the lithium ion conduction promoting protective layer 30 formed thereon is placed in the plating solution 50, and then the lithium supply source 40 is placed at a predetermined distance from the lithium ion conduction promoting protective layer 30.

[0091] The lithium supply source 40 may be, for example, lithium metal, a lithium alloy, a foil of the lithium metal or lithium alloy pressed onto a current collector, or a plating solution in which a lithium salt is dissolved.

[0092] The current collector 11 is the same as that described above, and a description thereof will be omitted here.

[0093] The plating solution 50 can be prepared by dissolving a lithium salt in a non-aqueous solvent.

[0094] More specifically, the lithium salt may be LiCl, LiBr, LiI, LiCO3, LiNO3, LiFSI, LiTFSI, LiBF4, LiPF6, LiAsF6, LiClO4, LiN(SO2CF3)2, LiBOB, or a combination thereof. The concentration of the lithium salt may be 0.1 to 3.0 M based on the total electrolyte.

[0095] More specifically, in this embodiment, the plating solution contains a nitrogen-based compound in at least one of the lithium salt and the non-aqueous solvent.

[0096] The nitrogen-based compound may include, for example, one or more selected from the group consisting of lithium nitrate, lithium bis fluorosulfonyl imide, lithium bis trifluoromethane sulfonimide, e-caprolactam, N-methyl-e-caprolactam, triethylamine, and tributylamine.

[0097] Among the nitrogen-based compounds, at least one of lithium nitrate, lithium bis fluorosulfonyl imide, and lithium bis trifluoromethane sulfonimide can be used as the lithium salt.

[0098] Among the nitrogen-based compounds, at least one of e-caprolactam, N-methyl-e-caprolactam, triethylamine, and tributylamine can be used as the non-aqueous solvent.

[0099] Meanwhile, the plating solution may contain a general non-aqueous solvent as a solvent, taking into consideration the viscosity of the plating solution, etc. If the viscosity of the plating solution is too high, the mobility of lithium ions decreases, and the ionic conductivity of the plating solution decreases, which increases the time required for the electrodeposition process and reduces productivity.

[0100] The solvent can include, for example, one or more selected from the group consisting of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, and 1,3,5-trioxane.

[0101] The current density of the current applied in the step of applying a current to form a lithium metal layer on at least one surface of the current collector is 0.1 mA / cm 2 ~100mA / cm 2 in the range of 0.2mA / cm 2 ~50mA / cm 2 range, 5mA / cm 2 ~30mA / cm 2 or 7mA / cm 2 ~25mA / cm 2 may be in the range.

[0102] The duration of application of the current may be in the range of 0.05 hours to 50 hours, more specifically, in the range of 0.25 hours to 25 hours.

[0103] In this way, in this embodiment, even under high current conditions, the excessive generation of fine lithium particles is prevented, and the lithium particles generated in the early stage are induced to grow well, so that a lithium metal electrode having a metal layer including a lithium metal layer having a coarse particle structure can be manufactured. In addition, the metal layer manufactured in this way has excellent surface uniformity. Therefore, as shown in FIG. 1, the lithium alloy layer 21 containing a lithium component and the lithium metal layer 41 located on the lithium alloy layer 21 can be manufactured to have a lithium metal electrode structure having a metal layer 12 or a lithium metal electrode structure having a metal layer 12 formed by mixing lithium and a lithium alloy as shown in FIG. 2. The thickness of the metal layer 12 can be in the range of 1 μm to 100 μm, more specifically, 5 μm to 30 μm.

[0104] When the lithium metal electrode manufactured according to the present embodiment is applied, the charge and discharge characteristics of the secondary battery can be significantly improved.

[0105] A secondary battery according to one embodiment includes a positive electrode, a negative electrode, and an electrolyte located between the positive electrode and the negative electrode, where the negative electrode may be a lithium metal electrode according to the present invention.

[0106] FIG. 14 is a diagram illustrating a schematic structure of a secondary battery according to an embodiment.

[0107] Referring to FIG. 14, the secondary battery 200 of this embodiment may include an electrode assembly including a positive electrode 70 , a negative electrode 100 , and a separator 90 disposed between the positive electrode 70 and the negative electrode 100 .

[0108] Such an electrode assembly is wound or folded and housed in a battery case 95.

[0109] Then, the electrolyte 80 is injected into the battery case 95 and sealed to complete the secondary battery 200. At this time, the battery case 95 may have a cylindrical, square, pouch, coin, or other shape.

[0110] For convenience, FIG. 14 illustrates the negative electrode 100 according to one embodiment. However, any of the lithium metal electrodes for secondary batteries according to the above-described embodiments may be used as the negative electrode.

[0111] The positive electrode 70 may include a positive electrode active material layer and a positive electrode current collector.

[0112] The positive electrode active material layer may contain, for example, at least one metal selected from Ni, Co, Mn, Al, Cr, Fe, Mg, Sr, V, La, and Ce, and a Li compound containing at least one nonmetallic element selected from the group consisting of O, F, S, P, and combinations thereof. The positive electrode active material layer may contain active material particles having an average particle size of about 0.01 μm to 200 μm, which may be appropriately selected depending on the required characteristics of the battery.

[0113] In some cases, a conductive agent may be added to the positive electrode active material layer.

[0114] The conductive agent may be, for example, carbon black and ultrafine graphite particles, fine carbon such as acetylene black, nano metal particle paste, etc., but is not limited thereto.

[0115] The positive electrode current collector serves to support the positive electrode active material layer, and may be, for example, an aluminum foil, a nickel foil, or a combination thereof, but is not limited thereto.

[0116] The electrolyte 80 filled in the lithium secondary battery 200 may be a non-aqueous electrolyte or a solid electrolyte.

[0117] The non-aqueous electrolyte may contain, for example, a lithium salt such as lithium hexafluorophosphate or lithium perchlorate, and a solvent such as ethylene carbonate, propylene carbonate, or butylene carbonate. The solid electrolyte may be, for example, a gel polymer electrolyte in which a polymer electrolyte such as polyethylene oxide or polyacrylonitrile is impregnated with an electrolyte, or an inorganic solid electrolyte such as LiI or Li3N.

[0118] The separator 90 separates the positive and negative electrodes and provides a passage for lithium ions to move, and any material commonly used in lithium secondary batteries may be used. That is, a material having low resistance to the movement of electrolyte ions and excellent electrolyte impregnation ability may be used. Here, the separator may be made of, for example, glass fiber, polyester, polyethylene, polypropylene, polytetrafluoroethylene, or a combination thereof, and may be in the form of a nonwoven fabric or a woven fabric. Meanwhile, when a solid electrolyte is used as the electrolyte 80, the solid electrolyte may also serve as the separator 90. EXAMPLES

[0119] Hereinafter, the present invention will be described in detail with reference to the following examples, which are presented by way of example only and are not intended to limit the present invention, which is defined only by the scope of the claims set forth below.

[0120] [Example 1] A lithium metal electrode for a secondary battery according to Example 1 was manufactured by the same process as that shown in FIG.

[0121] First, a coating layer 20 containing silver (Ag) was formed to a thickness of about 300 nm on one surface of a copper current collector 11 using an electroless plating method (see FIG. 4).

[0122] Thereafter, a protective layer 30 was formed to a thickness of about 5 μm on the surface of the coating layer 20 by slurry coating using a comma coater, specifically, a lithium ion conduction promoting protective layer was formed (see FIG. 5).

[0123] Here, the protective layer 30 is made by mixing amorphous carbon using acetylene black and lithium ion conduction promoting ceramic particles using lithium titanium oxide (Li2TiO3) in a weight ratio of 7:3 with a solvent using water. At this time, carboxymethyl cellulose and styrene-butadiene rubber binders were added at 1.5 wt% each based on the weight of the mixture composed of acetylene black, lithium titanium oxide (Li2TiO3) and water to prepare a slurry.

[0124] The current collector 11 having the coating layer 20 and the protective layer 30 formed thereon is placed in the plating solution 50, and then the lithium supply source 40 is placed at a predetermined distance from the protective layer 30.

[0125] The plating solution 50 was prepared by adding nitrogen-based compounds, lithium bis(fluorosulfonyl)imide and lithium nitrate, in an amount of 40 wt % and 10 wt % based on 100 wt % of the plating solution, respectively, to a 1,2-dimethoxyethane solvent, and adding a fluorine-based compound, fluoroethylene carbonate, in an amount of 10 wt % based on 100 wt % of the plating solution.

[0126] As the lithium supply source 40, a lithium metal plate having a purity of 99.9% or more and a thickness of 500 μm was used by pressing it onto a copper current collector (Cu plate).

[0127] The lithium supply source 40 and the current collector 11 were laminated in an electrically insulated state in the plating solution 50, and then a power supply device was used to apply a current to the current collector 11 and the lithium ion conduction promoting protective layer 30 using the lithium supply source 40 and the current collector 11 as (+) and (-) electrodes, respectively, to deposit lithium between the current collector 11 and the lithium ion conduction promoting protective layer 30, thereby forming a metal layer.

[0128] At this time, the average current density of the process is 4mA / cm 2 The process time was about 15 minutes, and a lithium metal electrode, i.e., a negative electrode, on which a metal layer of about 5 μm in thickness was formed was produced.

[0129] [Examples 2, 3, 4 and Reference Example 1] A negative electrode was prepared in the same manner as in Example 1, except that the weight ratio of the amorphous carbon and the lithium ion conduction promoting ceramic particles was adjusted as shown in Table 3 below when preparing the protective layer.

[0130] [Comparative Example 1] A negative electrode was prepared in the same manner as in Example 1, except that a coating layer was not formed on one side of the current collector, a protective layer was formed using 100% amorphous carbon, and no metal layer was formed between the current collector and the protective layer.

[0131] [Comparative Example 2] A negative electrode was prepared in the same manner as in Example 1, except that the protective layer was formed using 100% amorphous carbon.

[0132] [Comparative Example 3] A negative electrode was prepared in the same manner as in Example 1, except that no coating layer was formed on one side of the current collector, and no metal layer was formed between the current collector and the protective layer.

[0133] (Experimental Example 1) The cross-sectional structures of the negative electrodes prepared in Example 1 and Comparative Examples 1, 2, and 3 were analyzed and are shown in FIGS. 6a, 6b, 6c, and 6d, respectively.

[0134] That is, FIGS. 6a, 6b, 6c, and 6d are photographs showing cross sections of the negative electrodes prepared in Example 1 and Comparative Examples 1, 2, and 3 analyzed using a scanning electron microscope (SEM).

[0135] 6b and 6d, it can be seen that in the negative electrodes prepared in Example 1 and Comparative Example 2, a metal layer was uniformly formed between the protective layer and the current collector.

[0136] (Experimental Example 2) The surface microstructures of the negative electrodes prepared according to Example 1 and Comparative Examples 1, 2, and 3 are shown in Figures 7a, 8a, 9a, and 10a, respectively, and the surface components of the negative electrodes prepared according to Example 1 and Comparative Examples 1, 2, and 3 were analyzed and are shown in Figures 7b, 8b, 9b, and 10b.

[0137] The microstructure of the negative electrode surface was analyzed using a scanning electron microscope (SEM), and the components of the negative electrode surface were analyzed by energy dispersive X-ray spectroscopy.

[0138] 7a, 7b, 10a, and 10b are compared with 8a, 8b, 9a, and 9b, and it can be seen that titanium (Ti) elements are observed on the surface of the negative electrodes manufactured according to Example 1 and Comparative Example 3, which contain the lithium ion conduction promoting ceramic particles. This is believed to be due to the use of lithium titanium oxide (Li2TiO3) as the lithium ion conduction promoting ceramic particles. Meanwhile, fluorine (F) and sulfur (S) are additionally observed on the surface of the negative electrodes manufactured according to Example 1 and Comparative Example 2, which use the electrodeposition plating process. This is believed to be due to the surface insulating layer (SEI) formed by the decomposition reaction of the plating solution in the electrodeposition process. From this, it can be seen that the surface of the negative electrode contains a coating layer containing a Li-NCHO-based ionic compound and an ion conductive material such as LiF formed by the fluorine-based compound contained in the plating solution.

[0139] (Experimental Example 3) Using the negative electrodes, i.e., lithium metal electrodes, prepared in Example 1 and Comparative Examples 1, 2, and 3, solid-state batteries were manufactured as shown in FIG. 14, and the initial coulombic efficiency was evaluated.

[0140] To evaluate the initial coulombic efficiency of the all-solid-state battery cell, a pressurized dedicated evaluation cell capable of maintaining an inert atmosphere was used.

[0141] Specifically, the solid electrolyte used was sulfide-based ajirodite (Li6PS5Cl). The solid electrolyte was made into a pellet shape with a thickness of about 0.7 mm, and the density was improved by compressing it at a pressure of 370 MPa.

[0142] Lithium having a thickness of 0.5 mm was placed on one side of the solid electrolyte, and the negative electrodes prepared in Example 1 and Comparative Examples 1, 2, and 3 were placed on the other side. A pressure of 50 MPa was applied to attach the positive electrode and the negative electrode according to the present invention to the solid electrolyte.

[0143] During the initial coulombic efficiency evaluation, the dedicated evaluation cell was pressurized at a pressure of 16 MPa.

[0144] Here, the initial coulombic efficiency is 1mA / cm during the first charging process. 2 Charge for 3 hours at a constant current of 3mAh / cm 2 After charging, 1mA / cm 2 The battery was discharged at a constant current of 1 V, and when the discharge voltage exceeded 1 V, the discharge was stopped and the discharge capacity was measured and calculated.

[0145] The results of evaluating the initial coulombic efficiency of the secondary batteries are shown in FIG.

[0146] [Table 1]

[0147] 8a, 8b, 10a, 10b and Table 1, the solid-state batteries using the negative electrodes manufactured according to Comparative Example 1 and Comparative Example 3, in which no metal layer was formed between the current collector and the protective layer, showed low initial Coulombic efficiencies of 81.3% and 92.3%, respectively. This indicates that a significant amount of lithium is consumed in an initial irreversible reaction during the charging process, which is believed to be mainly due to the irreversible reaction caused by the amorphous carbon in the protective layer.

[0148] Meanwhile, the secondary batteries using the negative electrodes manufactured according to Example 1 and Comparative Example 2, in which a metal layer was formed between the current collector and the protective layer through an electrodeposition process, exhibited high initial Coulombic efficiency of 131.0% and 138.2%, respectively. This is believed to be because the initial discharge capacity was larger than the charge capacity due to the lithium contained in the metal layer and the surplus lithium in the lithium alloy.

[0149] Therefore, it can be confirmed that when a negative electrode having a metal layer formed thereon is manufactured by the same method as in this example, the problem of reduction in discharge capacity due to initial irreversibility does not occur.

[0150] (Experimental Example 4) (Experimental Example 4-1) Using the negative electrodes, i.e., lithium metal electrodes, prepared in Example 1 and Comparative Examples 1, 2, and 3, solid-state batteries were prepared as shown in FIG. 14, and their charge / discharge characteristics were evaluated.

[0151] The all-solid-state battery cell used in the charge / discharge evaluation was the pressurized dedicated evaluation cell used in Experimental Example 3.

[0152] The charge / discharge performance was evaluated as follows.

[0153] 1mA / cm 2 Charge for 1 hour at a constant current of 1mA / cm 2 One cycle was defined as one hour of discharge at a constant current.

[0154] In addition, the charge / discharge life was defined as the end of the life when a short circuit occurs between the positive electrode and the negative electrode manufactured according to the present invention during charging / discharging or when the voltage between the two electrodes exceeds 2V.

[0155] The results of evaluating the charge / discharge performance are shown in FIG.

[0156] [Table 2]

[0157] 12 and Table 2, the charge / discharge life of the all-solid-state battery using the anode manufactured according to Comparative Example 1 and Comparative Example 3, in which no metal layer is formed between the current collector and the protective layer, is 68 and 220 times, respectively, and the charge / discharge life of the all-solid-state battery using the anode manufactured according to Comparative Example 2 and Example 1, in which a metal layer is formed between the current collector and the protective layer, is 292 and 921 times, respectively. That is, it can be confirmed that the charge / discharge life of the all-solid-state battery using the anode in which a metal layer is formed between the current collector and the protective layer is significantly superior to that of the all-solid-state battery using the anode in which no metal layer is formed between the current collector and the protective layer.

[0158] Therefore, it can be confirmed that the charge and discharge life of a secondary battery is significantly improved when a negative electrode having a metal layer formed between a current collector and a protective layer is used.

[0159] In addition, when comparing Comparative Example 2 in which a metal layer is formed between the current collector and the protective layer with Example 1, it was found that the charge / discharge life of the all-solid-state battery employing the anode produced according to Example 1, which contains ceramic particles in the protective layer, was 921 cycles, which was significantly superior to the charge / discharge life of 292 cycles of the all-solid-state battery employing the anode produced according to Comparative Example 2, which does not contain ceramic particles in the protective layer.

[0160] Similarly, when comparing Comparative Example 1 and Comparative Example 3 in which no metal layer was formed between the current collector and the protective layer, the charge / discharge life of the all-solid-state battery employing the anode produced according to Comparative Example 3 in which the protective layer contained ceramic particles was 220 cycles, which was significantly superior to the charge / discharge life of the all-solid-state battery employing the anode produced according to Comparative Example 1 in which the protective layer did not contain ceramic particles, which was 68 cycles.

[0161] Therefore, it can be confirmed that the charge and discharge life of a secondary battery containing ceramic particles in a protective layer is significantly improved.

[0162] In particular, the charge / discharge life of the all-solid-state battery using the anode produced according to Example 1, in which a metal layer was formed between the current collector and the protective layer and the protective layer contained ceramic particles, was 921 cycles, which was found to be significantly superior to the charge / discharge life of the all-solid-state batteries using the anodes produced according to Comparative Examples 1, 2, and 3.

[0163] Therefore, it can be seen that when the negative electrode according to the present invention in which a metal layer is formed between a protective layer containing ceramic particles and a current collector is applied, the charge and discharge life of the secondary battery can be significantly improved.

[0164] (Experimental Example 4-2) The charge and discharge characteristics of the all-solid-state batteries using the negative electrodes prepared in Examples 2, 3, and 4 and Reference Example 1, in which the weight ratio of the amorphous carbon and the lithium ion conduction promoting ceramic particles was changed when preparing the lithium ion conduction promoting protective layer, were evaluated. The results are shown in FIG. 13 and Table 3 below.

[0165] [Table 3]

[0166] Referring to FIG. 13 and Table 3, as the amount of the lithium ion conduction promoting ceramic particles in the lithium ion conduction promoting protective layer increases, the charge / discharge life of the solid-state battery increases and then decreases again.

[0167] When the weight ratio of lithium ion conduction-promoting ceramic particles and amorphous carbon contained in the lithium ion conduction-promoting protective layer was 70:30, it was found that the charge / discharge life was shorter than that of an all-solid-state battery containing a protective layer made of 100% amorphous carbon.

[0168] The present invention is not limited to the above-mentioned embodiment, and can be manufactured in various different forms, and a person having ordinary skill in the art to which the present invention belongs can understand that the present invention can be embodied in other specific forms without changing the technical idea or essential characteristics of the present invention. Therefore, the above-mentioned embodiment should be understood to be illustrative in all respects and not restrictive.

Claims

1. Current collector; a metal layer comprising a lithium alloy and located on at least one surface of the current collector; and a protective layer overlying the metal layer; The lithium metal electrode, wherein the protective layer comprises amorphous carbon and ceramic particles that facilitate lithium ion conduction.

2. The lithium ion conductivity promoting ceramic particles are Li 2 TiO 3 , LiNbO 3 , LiTaO 3 , LiZrO 3 , Li 4 Ti 5 O 12 , Li 2 CO 3 , Li 3 B.O. 3 , SrTiO 3 The lithium metal electrode of claim 1, comprising one or more of the following:

3. 2. The lithium metal electrode of claim 1, wherein the protective layer comprises amorphous carbon and lithium ion conductivity enhancing ceramic particles in a weight ratio of 99.5:0.5 to 40:

60.

4. The metal layer containing a lithium alloy is 10. The lithium metal electrode of claim 1 comprising a lithium alloy layer disposed on the current collector and a lithium metal layer disposed on the lithium alloy layer.

5. 2. The lithium metal electrode of claim 1, wherein the metal layer comprising a lithium alloy is a composite layer comprising lithium and a lithium alloy.

6. 2. The lithium metal electrode of claim 1, wherein the metal layer containing a lithium alloy is a composite layer containing one or more of In, Ag, Sn, Zn, Si, Al, and Bi.

7. 2. The lithium metal electrode of claim 1, wherein the average thickness of the metal layer is from 1 μm to 100 μm.

8. 2. The lithium metal electrode of claim 1, wherein the protective layer has an average thickness of 1 μm to 20 μm.

9. The protective layer is Further comprising a coating layer located on the surface of the protective layer; The coating layer is made of an ionic compound based on Li-N-C-H-O, an ionic compound based on Li-P-C-H-O, LiF, and Li 3 2. The lithium metal electrode of claim 1, comprising one or more materials selected from the group consisting of N.

10. forming a coating layer on at least one surface of a current collector using a coating composition containing a lithium-philic component; forming a protective layer on the surface of the coating layer using a slurry containing amorphous carbon and lithium ion conductivity-promoting ceramic particles; placing the current collector having the coating layer and the protective layer formed thereon in a plating solution, and then placing a lithium supply source at a predetermined distance from the protective layer; applying an electric current between the current collector and the lithium source to form a metal layer including a lithium alloy in which the lithium parent component contained in the coating layer is alloyed with lithium deposited from the lithium source.

11. In the step of forming the coating layer, The method for manufacturing a lithium metal electrode according to claim 10, wherein the coating layer formed on at least one surface of the current collector has a thickness ranging from 0.001 μm to 10 μm.

12. forming a protective layer on the surface of the coating layer using a slurry including amorphous carbon and lithium ion conductivity enhancing ceramic particles; 11. The method of claim 10, wherein the weight ratio of the amorphous carbon to the lithium ion conductivity enhancing ceramic particles is 99.5:0.5 to 40:

60.

13. In the step of forming the metal layer, The metal layer is a lithium alloy layer comprising the lithium alloy; The method for producing a lithium metal electrode according to claim 10, wherein the lithium metal electrode is formed in a multi-layer structure including a lithium metal layer formed on the lithium alloy layer.

14. In the step of forming the metal layer, The metal layer is The method for producing a lithium metal electrode according to claim 10, wherein the lithium metal electrode is formed in a single layer structure containing the lithium alloy and the lithium metal deposited from the lithium source.

15. forming a metal layer containing a lithium alloy, The method for producing a lithium metal electrode according to claim 10, wherein the thickness of the metal layer is 1 μm to 100 μm.

16. Negative electrode; a positive electrode; and Contains electrolytes, A lithium secondary battery, wherein the negative electrode is the lithium metal electrode according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for plating a metal negative electrode under a protective coating.

    JP2002504741A

  • Negative electrode protective agent for lithium ion secondary battery, and negative electrode for lithium ion secondary battery including the same

    JP2010067508A

  • Lithium metal negative electrode, its manufacturing method and lithium secondary battery including the same

    JP2020502761A

  • Plating metal negative electrodes under protective coatings

    US20010041294A1

  • Lithium metal anode, fabrication method thererof, and lithium secondary battery comprising same anode

    US20190348668A1