Conductive polymer particles with excellent corrosion resistance

A multilayered structure of silver oxide, copper, and nickel/silver on polymer particles addresses the challenges of conductivity, corrosion, and bonding strength, providing cost-effective and reliable conductive polymer particles.

JP2024540854AActive Publication Date: 2024-11-06C&C MATERIALS CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2024521342
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-08
Publication Date
2024-11-06
Estimated Expiration
2041-10-08

AI Technical Summary

Technical Problem

Conductive polymer particles face challenges in achieving uniform size, spherical shape, and maintaining electrical conductivity, corrosion resistance, and bonding strength due to the use of expensive palladium catalysts and the inherent properties of metals like copper, nickel, and silver.

Method used

A multilayer structure is formed on the polymer particles, comprising a first layer of silver oxide, a second layer of copper, and optionally a third layer of nickel or silver, which provides excellent electrical conductivity, corrosion resistance, and bonding strength without the need for palladium catalysts.

Benefits of technology

The multilayered conductive polymer particles offer cost-effective, high conductivity, and improved reliability, reducing part weight and ensuring consistent electrical performance across various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540854000001_ABST
    Figure 2024540854000001_ABST
Patent Text Reader

Abstract

The present invention aims to provide conductive polymer particles having a metal layer formed on the surface thereof, which has excellent electrical conductivity, corrosion resistance, and bonding strength with polymer particles. In order to achieve the above-mentioned object, the present invention can provide conductive polymer particles including a first layer containing silver oxide formed on the surface of the polymer particle, a second layer containing copper formed on the first layer, and a third layer containing nickel or silver formed on the second layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to conductive polymer particles having a conductive metal coating layer, and in particular to conductive polymer particles having a multilayer structure and excellent corrosion resistance, in which a copper metal layer is formed on the surface without an expensive palladium catalyst layer, and a nickel or silver coating layer is further formed to protect the copper metal layer, and a method for producing the same. [Background technology]

[0002] Conductive particles are widely used in electronic materials. Among them, metal particles such as copper or nickel have high conductivity and are highly cost competitive, so they are used in a variety of applications that require electrical conductivity, such as films, adhesives, and coating slurries in various electronic components.

[0003] However, it is difficult to produce particles of various sizes during the synthesis process, and it is difficult to maintain uniform particle size and spherical shape between particles, so when producing a conductive film or adhesive, it is difficult to produce a film or adhesive layer of uniform thickness and to maintain uniform contact characteristics. In addition, to compensate for poor contact characteristics, metal particles are added to the film or adhesive in large volume, but the large volume ratio of these metal particles can cause problems such as making the film or adhesive layer heavy and weakening the adhesive force.

[0004] To overcome such problems, anisotropic conductive films, a type of conductive film, use conductive polymer particles in which a conductive metal layer such as copper, nickel, silver, or gold is formed on the surface of polymer particles whose size can be controlled in various ways and whose particle size can be maintained uniformly.

[0005] Anisotropic conductive films provide stable connections between DDI chips and various types of displays to drive displays, and the conductive balls, which are conductive polymer particles used in them, cost 20 to 30 million won per kg, one of the reasons for this is the use of expensive palladium (Pd). This is because the use of palladium is unavoidable to form a catalyst layer for strong bonding between the polymer particles and the metal layer when metal coating is performed to give conductivity to the polymer particles. Therefore, these conductive balls are difficult to use except for expensive anisotropic conductive films.

[0006] Meanwhile, the metal layer coated on the surface of the polymer particles can be made of various metals, but copper has excellent electrical conductivity close to that of silver, but has the problem of being easily oxidized, and nickel has the advantage of being highly corrosion resistant and therefore long-term reliability, but has the problem of low electrical conductivity. Another metal, silver (Ag), has both excellent electrical conductivity and corrosion resistance, but has the problem of being too expensive.

[0007] Thus, it is difficult for the metal layer formed on the surface of the polymer particles to satisfy all of the desired qualities. Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide conductive polymer particles having a metal layer formed on the surface thereof, which metal layer has excellent electrical conductivity, corrosion resistance, and bonding strength with polymer particles.

[0009] Yet another object of the present invention is to provide a method for producing conductive polymer particles, which can inexpensively form a metal layer on the surface of the conductive polymer particles, which metal layer has excellent electrical conductivity, corrosion resistance, and bonding strength with the polymer particles. [Means for solving the problem]

[0010] In order to achieve the above object, the present invention provides conductive polymer particles including a first layer containing silver oxide formed on the surface of the polymer particles, a second layer formed on the first layer and containing copper, and a third layer formed on the second layer and containing nickel or silver.

[0011] In the conductive polymer particles according to the present invention, the polymer particles are one or more selected from the group consisting of acrylic resins, acrylonitrile resins, and styrene resins. When analyzed with a laser scattering particle size analyzer, D 50 may be spherical in the range of 0.1 to 100 μm.

[0012] In the conductive polymer particles according to the present invention, the first layer further contains metallic silver, and the molar ratio of silver element in the silver oxide to silver element in the metallic silver (Ag x+ / Ag 0 (0 < x ≦ 3)) may be in the range of 1 to 20.

[0013] In the conductive polymer particles according to the present invention, the first layer may further contain tin.

[0014] In the conductive polymer particles according to the present invention, it may include a tin layer formed on the surface of the polymer particles and a silver oxide layer formed on the tin layer.

[0015] In the conductive polymer particles according to the present invention, the content of silver contained in the first layer may be 10 to 1,000 ppm of the total weight of the conductive polymer particles.

[0016] In the conductive polymer particles according to the present invention, the first layer may be discontinuous island-like on the surface of the polymer particles.

[0017] In the conductive polymer particles according to the present invention, the content of copper in the second layer may be 90% by weight or more.

[0018] In the conductive polymer particle according to the present invention, the third layer may further contain phosphorus together with the nickel.

[0019] In the conductive polymer particle according to the present invention, the third layer may contain 0.1 to 13.0% by weight of phosphorus together with nickel.

[0020] The present invention can provide a method for producing a conductive polymer, comprising: (a) a hydrophilization step of hydrophilizing the surfaces of polymer particles; (b) a first layer formation step of coating the hydrophilized surfaces of the polymer particles with silver oxide; (c) a second layer formation step of electrolessly plating copper on the first layer; and (d) a third layer formation step of electrolessly plating nickel or silver on the second layer.

[0021] In addition, the present invention can provide a method for producing a conductive polymer, in which tin is coated together with the silver oxide in the step of forming the first layer.

[0022] The method for producing a conductive polymer according to the present invention may further comprise a step of forming a tin layer between steps (a) and (b).

[0023] In addition, the method for producing a conductive polymer according to the present invention may further include, after step (b) and before step (c), a post-treatment step of stirring the polymer particles having the first layer formed thereon in an aqueous solution having a pH of 8 to 14 and a temperature of 20 to 80° C. to adjust the amount of silver oxide. Effect of the Invention

[0024] The conductive polymer particles according to the present invention are inexpensive, have excellent electrical conductivity and corrosion resistance, and can be applied to various electronic components that require electrical conductivity. They also have excellent bonding strength of the surface metal layer, making it possible to achieve weight reduction and improved electrical conductivity and reliability of the components to which they are applied.

[0025] Furthermore, the method for producing conductive polymer particles provided by the present invention enables mass production of conductive polymer particles having excellent conductivity and reliability through an inexpensive process. [Brief description of the drawings]

[0026] [Figure 1] 1 is a scanning electron microscope image of conductive polymer particles according to an embodiment of the present invention and a comparative example. [Diagram 2] FIG. 2 is a diagram showing the analysis results of the conductive polymer particles in one embodiment according to the present invention by X-ray Photoelectron Spectroscopy (XPS).

[0027] Best Mode for Carrying Out the Invention Hereinafter, the configuration and operation of the embodiment of the present invention will be described with reference to the accompanying drawings. In the following, when a specific description of a related known function or configuration is determined to make the gist of the present invention unclear, the detailed description will be omitted. In addition, when a certain part is described as "including" a certain component, this does not mean that other components are excluded, but that other components may be further included, unless otherwise specified.

[0028] Polymer particles can be made into particles of various shapes and sizes. However, due to the nature of the material, the electrical conductivity is either nonexistent or very low, so to overcome this, forming a conductive metal layer on the surface makes it possible to impart electrical conductivity to polymer particles of various shapes and sizes.

[0029] However, since polymers and metals are different materials and their adhesive strength is very low, it is very difficult to form a metal layer on the surface of a polymer. In order to overcome this problem, a method of forming an intermediate layer that facilitates adhesion between a metal layer that provides conductivity and a polymer has been used, and a catalyst layer containing palladium has been formed as the intermediate layer. These palladium catalyst layers have led to the smooth formation of metal layers such as copper, nickel, and silver. However, as is well known, palladium is an expensive precious metal, and in recent years it has been more expensive than gold, so there has been a problem that conductive polymer particles made using it are very expensive.

[0030] In order to solve such problems, the inventors of the present invention have investigated an intermediate layer that is cheaper than palladium and can provide sufficient bonding strength with the surface of a polymer. Since silver oxide is known to be able to smoothly adhere to the surface of a polymer as an oxide and also has excellent bonding strength with metals, they developed a method in which silver oxide is formed as an intermediate layer and then a metal coating layer is formed.

[0031] As a result, it was found that when an intermediate layer of silver oxide alone or a composite of silver oxide and silver metal is formed, the subsequently formed metal layer, the nickel layer, can bond strongly to the polymer particles and can exhibit a bonding strength equal to or greater than that when a conventional layer containing palladium is used.

[0032] On the other hand, the characteristics of the conductive polymer particles are determined by the type of metal layer formed on the surface of the polymer particles. Copper has excellent electrical conductivity, but is easily oxidized, which makes reliability a problem. Nickel, on the other hand, has excellent corrosion resistance, but has a problem of lower electrical conductivity than copper. Silver has both excellent corrosion resistance and electrical conductivity, but is expensive. As such, it is difficult to satisfy all of the characteristics required by industry with only one type of metal.

[0033] In order to overcome such problems, the inventors of the present invention have invented conductive polymer particles having a multi-layered metal layer formed on the surface thereof, in which a copper metal layer is formed first, and then a nickel or silver metal layer is formed on the copper metal layer to protect the copper metal layer.

[0034] As a result, the present invention can provide conductive polymer particles comprising a first layer containing silver oxide formed on the surface of the polymer particle, a second layer containing copper formed on the first layer, and a third layer containing nickel or silver formed on the second layer.

[0035] The polymer particles constituting the core of the conductive polymer particles are one or more selected from the group consisting of acrylic resins, acrylonitrile resins, and styrene resins, and when analyzed with a laser scattering type particle size analyzer, 50 The particles may be spherical with a diameter in the range of 0.1 to 100 μm.

[0036] The conductive polymer particles are advantageous for application to various electronic components, as they have a low density and can be formed into spherical shapes of various particle sizes. For this reason, the polymer particles constituting the core are preferably acrylic resin, acrylonitrile resin, or styrene resin, and spherical products of various particle sizes are commonly used, and by using these, it becomes possible to produce products of various spherical conductive polymer particles. Spherical polymers have the advantage of good filling and flowability, and can maintain the same electrical conductivity in various directions. In addition, acrylic, acrylonitrile, or styrene resins have excellent chemical resistance, do not deform during the process of forming the conductive coating layer, and can be used regardless of the environment of the components to which they are applied.

[0037] In particular, PMMA (Ploy (methyl methacrylate)), an acrylic resin, is spherical and is readily available in a wide variety of particle sizes, and has been verified in a variety of fields, making it possible to commercialize a wide variety of conductive polymer particles. PS (Polystyrene) and PAN (Polyacrylonitrile) also have a wide variety of particle sizes and stable chemical resistance, making it possible to commercialize a wide variety of conductive polymer particles.

[0038] In addition, the polymer particles of the present invention have a particle size of D 50 The standard is 0.1 to 100 μm, where D 50 D means the particle size at which the cumulative percentage of particles reaches 50%. 50 Based on this standard, if the particle size of the polymer particles is less than 0.1 μm, the polymer particles will be excessively agglomerated, making handling difficult, and the increased specific surface area will make it difficult to form a surface metal layer, whereas if it exceeds 100 μm, the specific surface area will decrease, decreasing the content of the metal layer formed on the surface, and the desired electrical conductivity may not be obtained.

[0039] As mentioned above, the surface of the polymer particle is difficult to bond with a metal layer due to the characteristics of the material. In order to modify such surface characteristics, it is necessary to form a catalyst layer. In the present invention, the first layer, which is a catalyst layer containing silver oxide, is formed first, instead of the conventional catalyst layer containing palladium. Silver oxide is excellent not only in bonding with polymers but also with metals, so that the bond between the polymer constituting the core and the metal layer on the surface can be maintained strong.

[0040] In the present invention, the first layer containing silver oxide may further contain tin. Tin is an element used to guide the smooth adhesion of silver oxide to the surface of polymer particles. When performing the coating operation with an aqueous solution, it imparts hydrophilicity to the surface of the polymer particles and helps the adhesion of silver elements to the surface of the polymer particles. These tins can also constitute the first layer together with silver oxide, or may be formed between the first layer containing silver oxide and the surface of the polymer particles.

[0041] The first layer containing silver oxide in the present invention may further contain metallic silver together with silver oxide. When metallic silver is further contained, the bond with copper, which is the metal contained in the second layer, can be further strengthened. Silver oxide strengthens the bond with the polymer, and metallic silver strongly binds to these silver oxides and provides a strong bond with copper, which is the same metal. As a result, the bonding force between the second layer containing copper and the polymer particles is further strengthened.

[0042] At this time, the molar ratio of silver element in silver oxide to silver element in metallic silver in the first layer (Ag x+ / Ag 0 (0 < x ≤ 3)) is preferably in the range of 1 to 20.

[0043] As described above, although containing metallic silver strengthens the bond between the first layer containing silver oxide and the second layer containing copper, if the proportion of silver element in metallic silver is too high compared to the silver element in silver oxide, the bonding force between the first layer and the surface of the polymer particles due to silver oxide decreases accordingly, which is not preferable. Therefore, the molar ratio of silver element in metallic silver to silver element in silver oxide is preferably 1 to 20, more preferably 1 to 10, and even more preferably 2 to 5, so that the proportion of silver element in silver oxide is higher. The measurement of these molar ratios can be performed by X-ray Photoelectron Spectroscopy (XPS).

[0044] Here, the oxidation number of silver in silver oxide can range from +1 to +3, and since the oxidation number does not have to be a constant in the amorphous phase, the oxidation number of silver in silver oxide may be greater than 0 and less than or equal to 3.

[0045] The first layer may further contain palladium, which can further strengthen the bond between the surface of the polymer particle and the silver oxide and the bond between the second layer. In this case, the amount of palladium contained may be even less than that contained in conventional conductive polymer particles without silver oxide. For example, the amount of palladium used in the manufacturing process of conductive polymer particles in the past is generally in the range of 100 to 1,000 ppm based on the conductive polymer particles, but the conductive polymer particles according to the present invention can use an amount of palladium greater than 0 and less than 50 ppm.

[0046] The content of silver in the first layer may be 10 to 1,000 ppm based on the total weight of the conductive polymer particles.

[0047] The metallic silver or silver oxide formed in the first layer can provide a satisfactory bonding strength to the second layer only if it is at a certain content or more, and if it is too much, the process cost increases, which is not preferable. More preferably, it may be 10 to 500 ppm.

[0048] The first layer in the present invention may be in the form of islands discontinuously formed on the surface of the polymer particle. The first layer is a layer that strengthens the bonding force between the polymer particle and the second layer that imparts electrical conductivity, and even if the first layer is in the form of discontinuous islands, it can provide sufficient bonding force to the second layer.

[0049] On the other hand, the first layer may be in the form of a continuous film, but in this case, the first layer must occupy at least 50% of the surface area of ​​the polymer particle, because even if it is in the form of a continuous film, it must occupy at least 50% of the particle surface area in order to provide sufficient binding strength to the second layer.

[0050] A second layer containing copper, a metal with excellent electrical conductivity, is formed on the first layer containing silver oxide. Copper, among metals, has particularly excellent electrical conductivity properties, which allows the conductive polymer particles to have excellent electrical conductivity.

[0051] The copper-containing second layer may be 5 to 40% by weight in the entire conductive polymer particle, but if it is less than 5% by weight, the electrical conductivity may decrease, and if it exceeds 40% by weight, the density of the entire conductive polymer particle increases, which is not preferable, and the risk of the second layer falling off increases. Therefore, the content of the second layer in the conductive polymer particle is preferably 10 to 30% by weight, more preferably 10 to 20% by weight.

[0052] On the other hand, in the present invention, the copper content in the copper-containing second layer is 90% by weight or more. If the copper content is less than 90% by weight, the electrical conductivity of the second layer decreases.

[0053] In the present invention, a third layer containing nickel or silver may be further formed on the second layer containing copper.

[0054] The third layer, containing nickel or silver, prevents the metallic copper formed in the second layer from oxidizing and also has excellent electrical conductivity, ultimately ensuring that the conductive polymer particles have both electrical conductivity and reliability.

[0055] When a metal layer containing highly corrosion-resistant nickel is formed as the third layer, it protects the second layer and, by forming metallic nickel, ensures a certain level of conductivity.

[0056] These third layers may contain not only nickel but also phosphorus, but since the inclusion of phosphorus improves chemical resistance and oxidation resistance, although the electrical conductivity is somewhat reduced, it is preferable for the third layer to contain phosphorus in addition to nickel when used in components where reliability is important. If phosphorus is contained, the phosphorus content in the third layer is preferably 0.1 to 13.0 wt %, but if it is too low, the desired chemical resistance and oxidation resistance will not be improved, and if the phosphorus content exceeds 13 wt %, sufficient electrical conductivity cannot be obtained. More preferably, the phosphorus content is 0.5 to 6 wt %.

[0057] Meanwhile, the third layer may contain metallic silver other than nickel, but silver is ideal in terms of properties as it is a metal with excellent corrosion resistance and electrical conductivity, but it has the disadvantage of being expensive. Therefore, in terms of electrical conductivity, if silver, which has excellent electrical conductivity, is formed as the third layer while protecting the copper on the second layer made of copper, which has the same level of electrical conductivity as silver, it is possible to ensure reliability while minimizing the amount of high silver usage and maximize the conductivity of the conductive polymer particles.

[0058] The present invention can also provide a method for producing a conductive polymer, the method including: (a) a hydrophilization step of hydrophilizing the surfaces of polymer particles; (b) a first layer formation step of coating the hydrophilized surfaces of the polymer particles with silver oxide; (c) a second layer formation step of electrolessly plating copper on the first layer; and (d) a third layer formation step of electrolessly plating nickel or silver on the second layer.

[0059] To produce a conductive polymer, a hydrophilization step is first required to hydrophilize the surface of the polymer particles by introducing chemical functional groups such as -OH, -COOH, -NH2, and NH3. These hydrophilization steps can be carried out in a strong alkaline aqueous solution with a pH of 12 or higher. This is because the strong alkaline solution partially breaks the polymer bonds on the surface of the polymer, which makes it easier for chemical functional groups to attach to the surface of the polymer particles. Therefore, a strong alkaline atmosphere with a pH of 12 or higher is preferred to treat the surface of a stable polymer particle.

[0060] On the other hand, the hydrophilization treatment of polymer particles can be carried out in a strong alkaline aqueous solution as described above, but it is also possible to hydrophilize the polymer particles in a dry manner by modifying the surfaces of the polymer particles through a plasma treatment.

[0061] After the hydrophilization treatment, a first layer containing silver oxide is formed, and tin can be coated together with the silver oxide. Tin can increase the binding force of silver oxide on the surface of the hydrophilized polymer particles.

[0062] For more precise control, a tin layer can be formed first on the hydrophilized polymer surface, followed by the formation of a first layer containing silver oxide.

[0063] The first layer containing silver oxide can be formed using an alkaline aqueous solution having a pH of 8 or higher. This is because silver oxide is well formed in an alkaline atmosphere having a pH of 8 or higher. More preferably, the first layer can be formed using an aqueous solution having a pH in the range of 9 to 11.

[0064] Furthermore, the method for producing a conductive polymer may further include a post-treatment step, after step (b) and before step (c), of stirring the polymer particles having the first layer formed thereon in an aqueous solution having a pH of 8 to 14 and a temperature of 20 to 80° C. to adjust the amount of silver oxide.

[0065] When the first layer is formed in an aqueous solution, silver ions in the aqueous solution may be reduced and attached to the surface of the polymer as metallic silver, not silver oxide. If the proportion of metallic silver is too high, the binding strength between the polymer particles and the first layer may be reduced, which is not preferable. Therefore, in order to increase the content of silver oxide to a desired level, the amount of silver oxide can be adjusted by treating with an alkaline aqueous solution at an appropriate temperature.

[0066] By adjusting the amount of silver oxide in this manner and then forming a second layer containing conductive copper, it becomes possible to provide conductive polymer particles that have excellent bonding strength between the metal coating layer that imparts conductivity and the polymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0067] In order to fully understand the present invention, preferred embodiments of the present invention will now be described with reference to the accompanying drawings.

[0068] The examples of the present invention are provided to more completely explain the present invention to those skilled in the art, and the following examples may be modified in various different forms, and the scope of the present invention is not limited to the following examples. Rather, these examples are provided to make the present disclosure more complete and complete, and to fully convey the concept of the present invention to those skilled in the art.

[0069] [Example 1] 50 g of sodium hydroxide was added to 100 g of deionized water and the temperature was raised to 60°C. 50 10 g of spherical PMMA (manufactured by Sonjin Chemical Co., Ltd.) with a diameter of 20 μm was added and stirred for 10 hours to hydrophilize the surfaces of the PMMA particles. The hydrophilized PMMA particles were then collected, stirred in 100 g of deionized water, washed three times, and then collected.

[0070] The PMMA particles were then added to a solution of 1.5 g of stannous chloride (SnCl2·2H2O) and 6 ml of hydrochloric acid (HCl 35% solution) in 100 g of deionized water, and stirred for 30 minutes to form a tin layer. The temperature of the solution was maintained at 35°C.

[0071] After filtering and collecting the PMMA particles with the tin layer formed, 0.15g of silver nitrate (AgNO3) was dissolved in 100g of deionized water, and the silver nitrate was added to the solution and stirred. At this time, 28% ammonia water was added dropwise to adjust the pH to 9.8.

[0072] The temperature was maintained at 40°C and the mixture was stirred for 1 hour to form a silver oxide layer. After 1 hour, the mixture was filtered and collected, then stirred with 200 g of deionized water, washed three times, and collected. A portion of the powder on which the silver oxide layer was formed was sampled and subjected to surface analysis by X-ray photoelectron spectroscopy (XPS).

[0073] The powder with the silver oxide layer was collected, and a copper coating layer was formed by electroless plating. A copper sulfate complex solution was prepared by adding 40g of EDTA (Ethylene-diamine-tetraacetic acid), 30g of NaOH, and 20g of copper sulfate to 300g of deionized water, and the polymer particles with the silver oxide layer were added. While stirring, a formaldehyde solution was dripped as a reducing agent to form a copper-containing coating layer.

[0074] A nickel coating layer was further formed on the polymer particles with the copper coating layer formed. For this purpose, the powder with the copper coating layer formed was added to a nickel plating solution prepared by adding 20g of nickel chloride (NiCl2·6H2O), 10g of sodium acetate, 5g of maleic acid, 30g of sodium hypophosphite as a reducing agent, and 3ml of lead acetate to 300g of deionized water, and the powder was then stirred and maintained at 70~90℃ for 2 hours to perform electroless plating.

[0075] [Example 2] The copper coating layer was formed in the same manner as in Example 1, and then a silver-containing coating layer was formed by electroless plating. For this purpose, a silver coating solution was prepared by mixing 2g of EDTA (Ethylene-diamine-tetraacetic acid), 2.5ml of 28% ammonia water, and 3g of silver nitrate (AgNO3) in 300g of deionized water, and then the polymer particles formed up to the copper coating layer were added thereto and stirred, while a reducing solution of 10g of glucose and 2g of sodium hydroxide dissolved in 50g of deionized water was dripped for 1 hour to form a third layer containing silver.

[0076] [Example 3] As in Example 1, after the first layer containing silver oxide was formed on the surface of the PMMA particles, post-treatment was performed with an alkaline aqueous solution. For the post-treatment, 28% ammonia water was added to 100 g of deionized water and kept at 60° C., and then the PMMA particles with the first layer were added and stirred. The pH of the aqueous solution before the PMMA particles were added was 9.5.

[0077] Thereafter, the second layer containing copper and the third layer containing nickel were formed in the same manner as in Example 1.

[0078] [Comparative Example 1] As in Example 1, a hydrophilic treatment and a tin layer were formed. Then, without forming a silver oxide layer, electroless plating was immediately performed to successively form a second layer containing copper and a third layer containing nickel. The electroless plating of copper and nickel was performed in the same manner as in Example 1.

[0079] [Comparative Example 2] As in Example 1, a first layer containing silver oxide was formed on the surface of the PMMA particles. Then, ascorbic acid was added to the aqueous solution to convert part of the silver oxide on the surface into metallic silver, and then electroless plating was performed to sequentially form a second layer containing copper and a third layer containing nickel. The electroless plating of copper and nickel was performed in the same manner as in Example 1.

[0080] [Comparative Example 3] As in Example 1, the copper coating layer was formed, but no subsequent steps were carried out.

[0081] After forming the first layer on the conductive polymer particles thus prepared, the ratio of silver element between silver oxide and metallic silver, the content of silver element, nickel content, and phosphorus content were analyzed, and the coating state was observed using a Scanning Electron Microscope (SEM). The ratio of silver element was analyzed by XPS by taking a sample after forming the first layer. The content of silver element, nickel content, and phosphorus content were analyzed using an Inductively Coupled Plasma Mass Spectrometer (ICP).

[0082] The reliability was evaluated by a reflow test in which the conductive polymers prepared in Examples 1 to 3 and Comparative Examples 1 and 2 were mixed with a certain amount of acrylic binder, coated on a polyimide film, dried, and then held on molten lead for 30 seconds, and the conductivity was measured.

[0083] The results are shown in Table 1 below. Here, the Cu content indicates the weight percentage of copper element based on the entire conductive polymer.

[0084] [Table 1]

[0085] 1 shows scanning electron microscope images of conductive polymer particles according to the examples. FIG. 1(a) is a scanning electron microscope image of a sample according to Example 1, FIG. 1(b) is a scanning electron microscope image of a sample according to Example 2, and FIG. 1(c) is a scanning electron microscope image of a sample according to Comparative Example 2.

[0086] Both samples from Examples 1 and 2 show that a dense coating layer was formed, but in Comparative Example 2, in which the first layer had a high content of metallic silver, the coating layer was not dense and the bonding was not strong.

[0087] FIG. 2 shows the results of measuring the ratio of silver element between silver oxide and metallic silver in the first layer of the sample according to Example 1. As a result of XPS, it is possible to measure it from the peak ratio of the ratio of silver in the reduced state and the ratio of silver in the oxidized state. x+ / Ag 0 ) was 3.80.

[0088] On the other hand, as shown in Table 1, the corrosion resistance was evaluated by a reflow test. In Examples 1 to 3, even after the reflow test, the resistance of the film using the conductive polymer particles was good, at 100 mΩ or less. However, in Comparative Example 2, in which the formation of the coating layer was unstable, the resistance increased significantly, and in the sample of Comparative Example 3, in which the third protective layer was not formed, the resistance was too high to be measured.

Claims

1. a first layer comprising silver oxide formed on the surface of a polymer particle; a second layer formed on the first layer and comprising copper; a third layer formed on the second layer and comprising nickel or silver; Including, Conductive polymer particles.

2. The polymer particles are at least one selected from the group consisting of acrylic resins, acrylonitrile resins, and styrene resins, and have a particle size distribution of D 50 is spherical in the range of 0.1 to 100 μm; The conductive polymer particle according to claim 1 .

3. The first layer further contains metallic silver, and the molar ratio of silver element in the silver oxide to silver element in the metallic silver (Ag x+ / Ag 0 (0<x≦3)) is in the range of 1 to 20; The conductive polymer particle according to claim 1 .

4. The first layer further comprises tin. The conductive polymer particle according to claim 1 .

5. The content of silver in the first layer is 10 to 1,000 ppm based on the total weight of the conductive polymer particles. The conductive polymer particle according to claim 1 .

6. The third layer further contains phosphorus together with the nickel. The conductive polymer particle according to claim 1 .

7. The third layer contains 0.1 to 13.0 wt. % phosphorus; The conductive polymer particle according to claim 6 .

8. (a) a hydrophilization step of hydrophilizing the surface of polymer particles; (b) forming a first layer by coating silver oxide on the polymer particles whose surfaces have been hydrophilized; (c) forming a second layer by electrolessly plating copper on the first layer; (d) forming a third layer by electrolessly plating nickel or silver on the second layer; Including, A method for producing conductive polymer particles.

9. The method further includes a step of forming a tin layer between steps (a) and (b). A method for producing the conductive polymer particles according to claim 8.

10. After the step (b) and before the step (c), a post-treatment step is further included in which the polymer particles on which the first layer is formed are stirred in an aqueous solution having a pH of 8 to 14 and a temperature of 20 to 80° C. to adjust the amount of the silver oxide. A method for producing the conductive polymer particles according to claim 8.

Citation Information

Patent Citations

  • Method for making conductive silicone rubber

    JP1978145882A

  • The external storage medium

    JP1985116699U

  • Production of silver-tin series solder alloy powder

    JP1999293307A

  • Electroconductive fine particles, anisotropic electroconductive material and connecting structure

    JP2010103080A

  • Conductive particulate

    JP2013073919A