High coercivity Nd-Fe-B sintered magnets and their manufacturing method and applications

The two-alloy method with controlled Mn, Cu, and Al addition, along with jet milling and sintering, addresses the limitations of existing methods by enhancing coercive force and maintaining magnetic performance in Nd-Fe-B sintered magnets.

JP2024541030AActive Publication Date: 2024-11-06YANTAI ZHENGHAI MAGNETIC MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024525290
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-07-06
Filing Date
2023-06-07
Publication Date
2024-11-06
Estimated Expiration
2043-06-07

AI Technical Summary

Technical Problem

Existing methods for improving the coercive force of Nd-Fe-B sintered magnets face limitations, particularly in maintaining magnetic performance when adjusting grain boundary structures with metals like Al and Cu, as excessive addition leads to deterioration, and there is a need for new techniques to enhance coercivity in harsh working environments.

Method used

A two-alloy method involving Mn-free and Mn-containing auxiliary alloy flakes, with controlled addition of Mn, Cu, and Al, combined with jet milling and specific sintering and tempering processes, to create a high coercivity Nd-Fe-B sintered magnet.

Benefits of technology

The method enhances coercive force by forming a uniform grain boundary phase, reducing the intrusion of Cu and Al into the main phase, and maintaining magnetic performance, resulting in a sintered magnet with improved coercivity and residual magnetism.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541030000001_ABST
    Figure 2024541030000001_ABST
Patent Text Reader

Abstract

The present invention discloses a high coercive force Nd-Fe-B sintered magnet and its manufacturing method and application, the sintered magnet is 100% by mass and contains the following components: R 26-37 wt%, where R is at least one rare earth element including Nd, Mn 0.07-0.23 wt%, B 0.8-1 wt%, M 0.5-4 wt%, where M contains Cu and / or Al, and further contains at least one selected from Co, Ti, Ni, Zr, Ga, and the balance is Fe. The present invention manufactures a Nd-Fe-B sintered magnet by mixing a Mn-containing auxiliary alloy powder with a Mn-free NdFeB main alloy powder, and the Mn-containing auxiliary alloy powder must contain at least one of metallic Cu and Al in addition to Mn element within the scope of the present invention, and Mn replaces part of Fe in the main phase, thereby reducing the amount of beneficial elements dissolved in the main phase at the grain boundary and improving the coercive force.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a prior application, bearing patent application number 202210800345X and entitled "High coercivity Nd-Fe-B sintered magnet, its manufacturing method and application," filed with the State Intellectual Property Office of the People's Republic of China on July 6, 2022. The above prior application is incorporated herein by reference in its entirety.

[0002] The present invention relates to the field of rare earth permanent magnets, and more particularly to a high coercive force Nd-Fe-B based sintered magnet and its manufacturing method and applications. [Background technology]

[0003] Permanent magnet materials are widely used in clean energy fields such as the new energy vehicle industry and wind power generation, and the clean energy field is obviously an important direction for future development. The rapid development of the clean energy field has increased the requirements for the magnetic performance of sintered magnets, and the increasingly harsh working environments require that the coercivity of sintered magnets be further improved.

[0004] Optimizing the coercive force of permanent magnet materials has traditionally been a technical difficulty that needs to be overcome. Although the powder particle size can be reduced by process measures, the grain size can be refined, and the coercive force can be improved, the refinement of the grain size increases the powder surface energy, which makes the sintered grains more likely to grow abnormally. With the continuous progress of NdFeB processing, the performance leap by process measures is becoming weaker and weaker, and other technologies should be actively pursued.

[0005] In addition to process means, it is possible to improve the coercivity by adjusting the grain boundary structure, and it has been demonstrated that metals such as Al and Cu can effectively improve the wettability between the main phase and the grain boundary phase, thereby improving the coercivity. Taking Al as an example, the solid solution of Al in the main phase causes a decrease in the Curie temperature and a decrease in remanence. Taking Cu as an example, when Cu is distributed at the interface between the main phase and the grain boundary phase, it can effectively increase the coercivity, but when Cu penetrates into the main phase, it causes a decrease in magnetic performance. The method of improving the coercivity by adjusting the grain boundary structure through the addition of such metals depends on the amount of metal added, and when the amount of metal added is below a certain limit, the magnetic performance is hardly improved, and when the amount of metal added exceeds a certain limit, the magnetic performance is decreased. Therefore, in order to achieve a higher coercivity index, it is necessary to introduce a new technology for adjusting the grain boundary structure based on the existing technology.

[0006] Regarding the above technical problems, the document CN101657863B discloses that the coercivity can be improved by adding Al to a rare earth-iron-boron sintered magnet, and that the coercivity can be improved while minimizing the decrease in magnetic performance by replacing the iron component with Mn. The document CN102067249B discloses that the amount of Cu added can be increased and the coercivity can be improved by adding a certain amount of Mn to a rare earth-transition metal-boron sintered magnet. Both of the above documents propose to add Mn to a rare earth-iron-boron sintered magnet to improve the coercivity, and prove that the addition of Mn can improve the coercivity of the sintered magnet, but the range of the Mn content is different between the two documents. In Table 4 of the embodiment of document CN101657863B, the highest coercivity occurs when the Mn atomic amount is 0.05%, and when the Mn atomic amount exceeds 0.05%, the effect of improving the coercivity is not significant. When the Mn atomic amount is 0.4%, the coercivity level is lower than when the Mn atomic amount is 0.01%, and the Mn content is far from the "Mn: 0.02 atomic % or more, less than 0.5 atomic %" described in the document.

[0007] Document CN101689416B discloses that adding Pr and Mn to a sintered magnet in a specified range can improve the room temperature coercivity, and mentions that if the amount of Pr added is less than the specified amount, no technical effect can be obtained, but does not develop a specific theory. Summary of the Invention

[0008] In order to improve the above technical problems, the technical proposal of the present invention is as follows:

[0009] A high coercive force Nd-Fe-B based sintered magnet, the mass ratio of which is 100%, the sintered magnet comprising the following components: 26-37 wt% R, where R is at least one rare earth element including Nd; Mn 0.07-0.23 wt%, B 0.8-1 wt%, M 0.5 to 4 wt%, the M containing Cu and / or Al and further containing at least one selected from Co, Ti, Ni, Zr, and Ga; The balance is Fe.

[0010] According to an embodiment of the present invention, the R is 28 to 36 wt %, and the R contains Nd and further contains at least one selected from Pr, Dy, Ho, and Tb.

[0011] According to an embodiment of the present invention, the Mn is 0.07 wt%, 0.08 wt%, 0.1 wt%, 0.12 wt%, 0.14 wt%, 0.15 wt%, 0.16 wt%, 0.17 wt%, 0.18 wt%, 0.19 wt%, 0.2 wt%, 0.21 wt%, 0.22 wt% or 0.23 wt%.

[0012] According to an embodiment of the present invention, the B is 0.8 wt%, 0.82 wt%, 0.84 wt%, 0.86 wt%, 0.88 wt%, 0.9 wt%, 0.92 wt%, 0.94 wt%, 0.95 wt%, 0.98 wt%, or 1 wt%.

[0013] According to an embodiment of the present invention, the M is preferably 0.8 to 3 wt %, and the M contains Cu and / or Al, and further contains at least one selected from Co, Ti, Ni, Zr, and Ga.

[0014] According to an embodiment of the present invention, the crystal grain size of the high coercive force Nd-Fe-B sintered magnet is 3 to 6 μm, and preferably 3.9 to 4.8 μm.

[0015] The present invention further provides a method for producing the above-mentioned high coercivity Nd—Fe—B based sintered magnet, the method comprising the following steps: (S1) First, Mn-free NdFeB main alloy flakes and Mn-containing auxiliary alloy flakes are produced, The Mn-free neodymium-iron-boron main alloy flakes contain 29-36 wt% R, 0.9-1 wt% B, 0.1-3.5 wt% M, and the balance is Fe; The Mn-containing auxiliary alloy flakes contain 12 to 37 wt% R, 1 to 10 wt% Mn, 0 to 1 wt% B, 0.5 to 30 wt% M, and the balance is Fe; Preferably, in step (S1), M in the main alloy flake does not contain Cu and / or Al, M in the auxiliary alloy flake necessarily contains Cu and / or Al, the Cu content in the auxiliary alloy flake is 0-9 wt%, the Al content is 0-8 wt%, and the Cu and Al contents are not 0 at the same time; (S2) The Mn-free neodymium-iron-boron main alloy flakes and Mn-containing auxiliary alloy flakes from step (S1) are subjected to hydro-crushing and jet milling to obtain a mixed alloy powder, which is then subjected to pressing, sintering and tempering to produce the above-mentioned high coercivity Nd-Fe-B sintered magnet.

[0016] According to an embodiment of the present invention, in the step (S1), in the Mn-containing auxiliary alloy flakes, the R contains at least 12 to 30 wt % of Nd.

[0017] According to an embodiment of the present invention, in step (S2), the Mn-free NdFeB main alloy flakes account for 87-98 wt% of the total amount of the Mn-free NdFeB main alloy flakes and the Mn-containing auxiliary alloy flakes, for example, 87 wt%, 87.6 wt%, 89 wt%, 91 wt%, 92 wt%, 93 wt%, 95 wt%, 96.3 wt%, 97 wt%, 97.6 wt%, 97.8 wt%, 98 wt%.

[0018] According to an embodiment of the present invention, in step (S2), the mixed alloy powder includes Mn-free NdFeB main alloy powder and Mn-containing auxiliary alloy powder.

[0019] According to an embodiment of the present invention, in step (S2), the mixed alloy powder is oriented and compacted in a magnetized magnetic field, and after compaction, it can be subjected to cold isostatic pressing and then pressed to form a green compact.

[0020] According to an embodiment of the present invention, in step (S2), the sintering temperature is 800-1200°C, and the temperature maintenance time is 3-20 h. Preferably, a secondary sintering is used, the first sintering temperature is 900-1200°C, preferably 900-1080°C, and the temperature maintenance time is 3-8 h, preferably 6-8 h, and the second sintering temperature is 800-1100°C, and the temperature maintenance time is 3-7 h.

[0021] Preferably, when the Mn content in the sintered magnet is 0.15 to 0.23 wt % and the alloy powder grain size is 3.0 to 3.8 μm, the first sintering temperature is 900 to 1050° C. and the temperature maintenance time is 6 to 8 hours.

[0022] According to an embodiment of the present invention, in step (S2), the tempering treatment is a secondary tempering treatment, for example, the secondary tempering treatment is performed in a vacuum tempering furnace, the primary tempering temperature is 700-950°C, and the temperature maintenance time is 4-8 h, and the secondary tempering temperature is 450-600°C, and the temperature maintenance time is 4-8 h.

[0023] According to an embodiment of the present invention, step (S2) may comprise: (S2a) subjecting the Mn-free Nd-Fe-B main alloy flakes and the Mn-containing auxiliary alloy flakes in step (S1) to hydro-crushing and jet milling, respectively, to obtain Mn-free Nd-Fe-B main alloy powder and Mn-containing auxiliary alloy powder, respectively; and uniformly mixing the Mn-free Nd-Fe-B main alloy powder and the Mn-containing auxiliary alloy powder to obtain a mixed alloy powder, which is then subjected to pressing, sintering and tempering to produce the above-mentioned high coercivity Nd-Fe-B sintered magnet.

[0024] According to the present invention, in step (S2a), the average particle size of the Mn-free NdFeB main alloy powder is 3.0 to 3.8 μm, for example, 3 μm, 3.1 μm, 3.2 μm, 3.3 μm, 3.4 μm, 3.5 μm, 3.6 μm, 3.7 μm or 3.8 μm.

[0025] Preferably, the average particle size of the Mn-containing auxiliary alloy powder is 3 to 4 μm, for example, 3 μm, 3.1 μm, 3.2 μm, 3.3 μm, 3.4 μm, 3.5 μm, 3.6 μm, 3.7 μm, 3.8 μm, 3.9 μm or 4 μm.

[0026] According to an embodiment of the present invention, step (S2) may be (S2b) mixing the Mn-free Nd-Fe-B main alloy flakes of step (S1) and the Mn-containing auxiliary alloy flakes, followed by hydro-crushing and jet milling to obtain a mixed alloy powder, which is then subjected to pressing, sintering and tempering to produce the above-mentioned high coercivity Nd-Fe-B sintered magnet.

[0027] According to the present invention, in step (S2b), the average particle size of the mixed alloy powder is 3.0 to 3.8 μm, for example, 3.0 μm, 3.1 μm, 3.2 μm, 3.3 μm, 3.4 μm, 3.5 μm, 3.6 μm, 3.7 μm or 3.8 μm.

[0028] As an exemplary embodiment of the present invention, the method for producing the high coercive force Nd—Fe—B based sintered magnet specifically includes the following steps: (1) Produce Mn-free NdFeB main alloy flakes and Mn-containing auxiliary alloy flakes, (2) mixing the Mn-free NdFeB main alloy flakes and the Mn-containing auxiliary alloy flakes in a certain ratio, and then subjecting them to hydrogen crushing-jet milling to obtain a mixed alloy powder containing the Mn-free NdFeB main alloy powder and the Mn-containing auxiliary alloy powder; or the Mn-free NdFeB main alloy flakes and the Mn-containing auxiliary alloy flakes are respectively subjected to hydrogen crushing-jet milling to obtain Mn-free NdFeB main alloy powders and Mn-containing auxiliary alloy powders, respectively; and mixing the main alloy powders and auxiliary alloy powders, in which the Mn-free NdFeB main alloy powder has a particle size of 3.0-3.8 μm and the Mn-containing auxiliary alloy powder has a particle size of 3.0-4.0 μm; Among them, the Mn-free NdFeB main alloy flakes account for 87-98 wt% of the total amount of the Mn-free NdFeB main alloy flakes and the Mn-containing auxiliary alloy flakes; (3) The uniformly mixed alloy powder in step (2) is oriented and molded in a magnetizing magnetic field, and then molded through a cold isostatic press to form a powder compact. The powder compact is sintered in a vacuum sintering furnace, the first sintering temperature is 900-1200°C, and the temperature is maintained for 3-8 hours. The second sintering is performed at a temperature of 800-1100°C, and the temperature is maintained for 3-7 hours to produce a body; When the Mn content in the sintered magnet is 0.15-0.23 wt% and the alloy powder grain size is 3.0-3.8 μm, the first sintering temperature is 900-1050° C. and the temperature maintenance time is 6-8 h; (4) The matrix from step (3) is subjected to a second tempering in a vacuum tempering furnace, the first tempering temperature being 700-950°C and the temperature maintenance time being 4-8 h, and the second tempering temperature being 450-600°C and the temperature maintenance time being 4-8 h, thereby producing the above-mentioned high coercive force Nd-Fe-B sintered magnet.

[0029] The present invention further provides applications for the above-mentioned high coercivity Nd-Fe-B sintered magnets in the fields of new energy vehicle industry and wind power generation. Beneficial Effects of the Invention: The present invention manufactures Nd-Fe-B sintered magnets by mixing Mn-containing auxiliary alloy powder with Mn-free NdFeB main alloy powder, and the Mn-containing auxiliary alloy powder must contain at least one of metals Cu and Al in addition to Mn element within the scope of the present invention, and Mn replaces part of Fe in the main phase, which can reduce the amount of beneficial elements dissolved in the main phase at the grain boundary and improve the coercivity. The present invention also replaces part of Nd with Pr, but in addition to ensuring that Nd is the main element in the main phase, the amount of Pr added is not related to the amount of Mn added, and there is a possibility that Pr will not react after being added to the main phase.

[0030] In the prior art, it is common to improve the coercivity by improving the grain boundary structure using low melting point metals, Cu and Al. Al has a high solubility in the main phase and may impair the magnetic performance if it penetrates into the main phase, while Cu improves the wettability of the grain boundary phase at the grain boundary and promotes the formation of a thin grain boundary phase, so the amounts of Al and Cu added should be controlled within an appropriate range. In the present invention, Mn is added in the form of auxiliary alloy powder, and when Fe is replaced with Mn, a coating layer of Mn is formed, which reduces the penetration of Cu and Al into the main phase and improves the grain boundary structure. Therefore, compared to the alloy melting method of the prior art, the two-alloy method of the present invention can improve the coercivity of the sintered magnet and overcome the problem of the large decrease in remanence caused by the prior art.

[0031] In the present invention, the main alloy flakes and the auxiliary alloy flakes are crushed to 3.0-3.8 μm and 3-4 μm by jet milling, respectively, or the main alloy flakes and the auxiliary alloy flakes are mixed and then crushed to 3.0-3.8 μm, so that finer crystal grains can be obtained, and at the same time, grain boundary elements such as Mn, Cu, and Al added to the auxiliary alloy can surround the main phase crystal grains more sufficiently and uniformly, and strengthen the grain boundaries. Furthermore, when the grain size of the mixed alloy powder becomes small, the surface energy increases rapidly, and a sintered magnet with higher coercivity can be manufactured by controlling the sintering temperature and sintering time under the premise of ensuring sufficient sintered body density. The present invention further found that when the proportion of Mn in the sintered magnet is 0.15-0.23 wt% and the alloy powder grain size is 3.0-3.8 μm, a higher coercivity can be obtained by extending the appropriate sintering time at a sintering temperature of 900-1050°C and using the same tempering process.

[0032] The present invention provides a method for producing a high coercivity Nd-Fe-B sintered magnet by using a two-alloy method, in which a main alloy powder is mixed with an auxiliary alloy powder containing Mn, Cu and / or Al, and the sintering temperature is adjusted to obtain a uniform and continuous grain boundary phase, thereby improving the coercivity, and enabling the production of a sintered magnet with higher coercivity when the crystal grain size is small. [Brief description of the drawings]

[0033] [Figure 1] 1 is a graph showing the change in Hcj depending on the amount of Mn added for the sintered magnets of Examples 3, and 8 to 16, and Comparative Examples 9 to 13. [Diagram 2] 1 is a graph showing the changes in the average particle size of the mixed alloy powders of Examples 17 to 21 and Comparative Examples 14 to 18, and the crystal grain size and coercive force of the sintered magnets. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] The device of the present invention will be described in more detail below in accordance with specific examples. It should be understood that the following examples are merely illustrative and interpretive of the present invention and should not be interpreted as limiting the scope of the claims of the present invention. Any technology realized based on the above content of the present invention is included in the scope of the claims of the present invention.

[0035] Unless otherwise stated, all components used in the following examples are commercially available or can be manufactured by known methods. [Examples 1 to 6, Comparative Examples 1 to 6] It was produced in the following manner.

[0036] (1) The raw materials (all units are wt%) were weighed according to the compounding ratio of each main alloy flake in Table 1, and the arranged raw materials were melted in an argon gas atmosphere and cast into a quench roll to produce Mn-free NdFeB main alloy flakes (i.e., the main alloy in Table 1). Similarly, the auxiliary alloy raw materials were melted in an argon gas atmosphere to cast Mn-containing auxiliary alloy flakes (i.e., the auxiliary alloy in Table 1). The main alloy flakes and the auxiliary alloy flakes were mixed in the appropriate ratio, and then subjected to hydrogen crushing and jet milling crushing to obtain a mixed alloy powder with a uniform particle size. The particle size of the mixed alloy powder is as shown in Table 2.

[0037] (2) The mixed alloy powder in step (1) was oriented and compacted in a magnetized magnetic field, and then subjected to cold isostatic pressing to form a green compact. The green compact was subjected to a secondary sintering heat treatment at the sintering temperature and for the sintering time shown in Table 2.

[0038] (3) The above-mentioned raw material was subjected to a second tempering in a vacuum tempering furnace. The first tempering temperature was 800°C and the temperature was maintained for 5 hours. The second tempering temperature was 500°C and the temperature was maintained for 5 hours, thereby producing a sintered magnet. Example 7 Example 7 differs from Examples 1 to 6 in the following respects.

[0039] (1) The compounding ratio of each element in Example 7 is as shown in Table 1. The raw materials (units are all wt%) were weighed according to the compounding ratio of each main alloy flake in Table 1, and the arranged raw materials were melted in an argon gas atmosphere and cast into a quenching roll to prepare Mn-free NdFeB main alloy flakes (i.e., the main alloy in Table 1). Similarly, the auxiliary alloy raw materials were melted in an argon gas atmosphere to cast Mn-containing auxiliary alloy flakes (i.e., the auxiliary alloy in Table 1). The main alloy flakes and auxiliary alloy flakes produced were subjected to hydrogen crushing and jet milling crushing, respectively, to obtain main alloy powders and auxiliary alloy powders with uniform particle sizes, respectively. The main alloy powders had an average particle size of 3.4 μm, and the auxiliary alloy powders had an average particle size of 3.4 μm. The main alloy powders and auxiliary alloy powders were uniformly mixed to obtain mixed alloy powders.

[0040] (2) The mixed alloy powder in step (1) was oriented and compacted in a magnetized magnetic field, and then subjected to cold isostatic pressing to form a green compact. The green compact was subjected to a secondary sintering heat treatment at the sintering temperature and for the sintering time shown in Table 2.

[0041] (3) The above-mentioned raw material was subjected to a second tempering in a vacuum tempering furnace. The first tempering temperature was 800°C and the temperature was maintained for 5 hours. The second tempering temperature was 500°C and the temperature was maintained for 5 hours, thereby producing a sintered magnet. [Comparative Examples 7 to 8] (1) The raw materials (all units are wt%) were weighed out according to the alloy component ratios in Table 1. The raw materials were melted in an argon gas atmosphere and cast into a quenching roll to produce flakes. The flakes were then subjected to hydrogen crushing and jet milling to obtain a neodymium-iron-boron alloy powder with a uniform particle size.

[0042] (2) The neodymium-iron-boron alloy powder in step (1) was oriented and compacted in a magnetized magnetic field, and then subjected to cold isostatic pressing to form a green compact. The green compact was subjected to secondary sintering heat treatment at the sintering temperature and for the sintering time shown in Table 2.

[0043] (3) The above-mentioned raw material was subjected to a second tempering in a vacuum tempering furnace. The first tempering temperature was 800°C and the temperature was maintained for 5 hours. The second tempering temperature was 500°C and the temperature was maintained for 5 hours, thereby producing a sintered magnet.

[0044] [Table 1]

[0045] [Table 2]

[0046] [Table 3]

[0047] [Table 4]

[0048] Comparing the data for Example 1 and Comparative Example 1, Comparative Example 1 does not contain Mn element, but the evaluation results of the magnetic performance of both show that since the present invention contains Mn element, the produced sintered magnets have higher Hcj and the reduction in Br is very small.

[0049] Comparing Example 1 with Comparative Example 7, the Hcj of the sintered magnet produced by the dual alloy production process of the present invention is significantly improved, and similarly, comparing Example 6 with Comparative Example 8, the Hcj of the sintered magnet produced by the dual alloy production process is significantly improved. It can be seen that the Mn of the present invention, which is added to the sintered magnet as an auxiliary alloy, has a higher coercive force.

[0050] Comparing Example 2 with Comparative Examples 2 and 3, Example 2 added Al, Cu, and Mn to the auxiliary alloy, while Comparative Example 2 added only Mn to the auxiliary alloy, without adding Al or Cu to the alloy, and Comparative Example 3 added Al and Cu to the auxiliary alloy and Mn to the main alloy. From the magnetic performance results in Table 3, it can be seen that in Comparative Examples 2 and 3, despite the addition of Mn, Al and Cu were not added to the auxiliary alloy, resulting in insufficient Hcj of the sintered magnet, and even though Mn was added as the main alloy, the Hcj of the sintered magnet was insufficient. Similarly, comparing Example 5 and Comparative Example 6, Example 5 added Al, Cu, and Mn to the auxiliary alloy, while Comparative Example 6 added Mn only to the auxiliary alloy, and from the magnetic performance results in Table 3, Comparative Example 6 had a lower Hcj.

[0051] It can be seen that the present invention can produce a sintered magnet with excellent coercivity by adding Al and / or Cu to the auxiliary alloy and simultaneously adding Mn. From the above, it can be seen that the Mn element of the present invention can be added to the auxiliary alloy to act on the grain boundaries, reducing the intrusion of Cu and Al into the main phase after forming an enveloping layer at the grain boundaries, thereby effectively improving the coercivity.

[0052] Comparing Example 6 and Example 7, in Example 6, the main alloy flakes and the auxiliary alloy flakes are mixed before hydrogen crushing and then further crushed by jet milling, whereas in Example 7, the main alloy flakes and the auxiliary alloy flakes are respectively hydrogen crushed and jet milled to obtain the main alloy powder and the auxiliary alloy powder, respectively, and then the main alloy powder and the auxiliary alloy powder are mixed together. As can be seen from Table 3, the impact of the two mixing methods on the magnetic performance is not significant.

[0053] Comparing Example 3 with Comparative Example 4, Example 3 contains 0.12 wt% Mn while Comparative Example 4 contains 0.3 wt% Mn. Comparing Example 4 with Comparative Example 5, Example 4 contains 0.14 wt% Mn while Comparative Example 5 contains 0.25 wt% Mn. The magnetic performance results in Table 3 show that the performance of the sintered magnet produced according to the present invention is superior, and that when the amount of Mn added exceeds a certain limit, the magnetic performance of the sintered magnet decreases. [Examples 8 to 16, Comparative Examples 9 to 13] (1) In Examples 8 to 16 and Comparative Examples 9 to 13, only the total Mn content was changed based on Example 3. The total Mn content in Examples 8 to 16 was 0.07 wt%, 0.08 wt%, 0.1 wt%, 0.14 wt%, 0.16 wt%, 0.18 wt%, 0.2 wt%, 0.22 wt%, and 0.23 wt%, and the Mn content in Comparative Examples 9 to 12 was 0.00 wt%, 0.24 wt%, 0.26 wt%, 0.28 wt%, and 0.3 wt%. The raw materials (units are all wt%) were weighed according to the compounding ratio of each main alloy flake, and the arranged raw materials were melted in an argon gas atmosphere and cast into a quenching roll to produce Mn-free neodymium iron boron main alloy flakes. Similarly, the auxiliary alloy raw material is melted in an argon gas atmosphere to cast Mn-containing auxiliary alloy flakes, and the main alloy flakes and the auxiliary alloy flakes are mixed in a certain ratio. After that, the mixture is crushed by hydrogen and then crushed by jet milling to obtain a mixed alloy powder with a uniform particle size. The average particle size of the mixed alloy powder is 3.7 μm.

[0054] (2) The mixed alloy powder in step (1) was oriented in a magnetized magnetic field, and then compacted by cold isostatic pressing. The compact was sintered for the first time at 1060°C for 5.4 h, and then sintered for the second time at 1080°C for 5.5 h.

[0055] (3) The above-mentioned raw material was subjected to a second tempering in a vacuum tempering furnace. The first tempering temperature was 800°C and the temperature was maintained for 5 hours. The second tempering temperature was 500°C and the temperature was maintained for 5 hours, thereby producing a sintered magnet.

[0056] FIG. 1 shows the tendency of the coercive force to change with the amount of Mn added in Example 3, Examples 8 to 16, and Comparative Examples 9 to 13. As can be seen from FIG. 1, when only the amount of Mn added was changed and the other factors were not changed, the coercive force was highest when the Mn content was 0.17 to 0.23%.

[0057] For these reasons, the range of Mn content in the auxiliary alloy is preferably 0.17 to 0.23%. [Examples 17 to 21, Comparative Examples 14 to 18] (1) The raw materials (units are all wt%) were weighed according to the compounding ratio in Table 4, the arranged raw materials were melted in an argon gas atmosphere, and cast into a quench roll to produce Mn-free neodymium-iron-boron main alloy flakes, and similarly, the auxiliary alloy raw materials were melted in an argon gas atmosphere to cast Mn-containing auxiliary alloy flakes. After the main alloy flakes and auxiliary alloy flakes were mixed in the appropriate ratio, they were crushed by hydrogen and jet milling, and the particle size of the mixed alloy powder with a uniform particle size was as shown in Table 5, among which the same raw materials were used in Examples 17 to 21 and Comparative Examples 14 to 18.

[0058] (2) The mixed alloy powder in step (1) was oriented and compacted in a magnetized magnetic field, and then subjected to cold isostatic pressing to form a green compact. The green compact was subjected to a secondary sintering heat treatment at the sintering temperature and for the sintering time shown in Table 5.

[0059] (3) The above-mentioned raw material was subjected to a second tempering in a vacuum tempering furnace. The first tempering temperature was 800°C and the temperature was maintained for 5 hours. The second tempering temperature was 500°C and the temperature was maintained for 5 hours, thereby producing a sintered magnet.

[0060] [Table 5]

[0061] [Table 6]

[0062] As can be seen from Table 5, making the crystal grains of a sintered magnet finer can effectively improve the coercive force.

[0063] FIG. 2 is a graph showing the average particle size, grain size, and coercive force of the mixed alloy powders of Examples 17-21 and Comparative Examples 14-18. By adjusting the average particle size of the mixed powder, the growth of magnet grains can be controlled in a specific temperature range, and the preferred grain size is 3.9-4.8 μm. Table 5 and FIG. 2 together show that the coercive force is the best when the average grain size of the mixed alloy powder is between 3.0-3.8 μm. If the grain size of the mixed alloy powder is <3.0 μm, over-sintering is likely to occur due to sintering, and the coercive force drops sharply. If the grain size of the mixed alloy powder is >3.8 μm, the uniformity of the grain size of the product cannot be effectively controlled, and the grain size of the product is >4.8 μm.

[0064] The above describes the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modifications, equivalent replacements, improvements, etc. made within the scope of the spirit and principles of the present invention are included within the scope of the claims of the present invention.

Claims

1. A high coercive force Nd-Fe-B based sintered magnet, the mass ratio of which is 100%, and the sintered magnet contains the following components: 26-37 wt% R, where R is at least one rare earth element including Nd; Mn 0.07 to 0.23 wt%, B 0.8-1 wt%, M 0.5 to 4 wt%, the M containing Cu and / or Al and further containing at least one selected from Co, Ti, Ni, Zr, and Ga; A sintered magnet, the remainder of which is Fe.

2. 2. The sintered magnet according to claim 1, wherein the high coercive force Nd—Fe—B sintered magnet has a crystal grain size of 3 to 6 μm.

3. 3. A method for producing a sintered magnet according to claim 1 or 2, comprising the steps of: (S1) First, prepare Mn-free NdFeB main alloy flakes and Mn-containing auxiliary alloy flakes, The Mn-free neodymium-iron-boron main alloy flakes contain 29-36 wt% R, 0.9-1 wt% B, 0.1-3.5 wt% M, and the balance is Fe; The Mn-containing auxiliary alloy flakes contain 12-37 wt% R, 1-10 wt% Mn, 0-1 wt% B, 0.5-30 wt% M, and the balance is Fe; (S2) subjecting the Mn-free Nd-Fe-B main alloy flakes and Mn-containing auxiliary alloy flakes of step (S1) to hydro-crushing and jet milling to obtain mixed alloy powder, which is then subjected to pressing, sintering and tempering to produce the high coercivity Nd-Fe-B sintered magnet.

4. 4. The method for producing a sintered magnet as claimed in claim 3, characterized in that, in step (S1), M in the main alloy flakes does not contain Cu and / or Al, M in the auxiliary alloy flakes necessarily contains Cu and / or Al, the Cu content in the auxiliary alloy flakes is 0-9 wt%, the Al content is 0-8 wt%, and the Cu and Al contents are not simultaneously 0.

5. 4. The method for producing a sintered magnet according to claim 3, wherein in step (S1), in the Mn-containing auxiliary alloy flakes, the R contains at least 12 to 30 wt % Nd.

6. In step (S2), the Mn-free NdFeB main alloy flakes account for 87-98 wt% of the total amount of the Mn-free NdFeB main alloy flakes and the Mn-containing auxiliary alloy flakes; And / or, in step (S2), the mixed alloy powder comprises a Mn-free NdFeB main alloy powder and a Mn-containing auxiliary alloy powder; And / or, in step (S2), the sintering temperature is 800-1200°C and the temperature maintenance time is 3-20 h; and / or using secondary sintering, the first sintering temperature is 900-1200°C, the temperature holding time is 3-8 h, the second sintering temperature is 800-1100°C, the temperature holding time is 3-7 h; and / or the method for producing a sintered magnet according to claim 3, characterized in that when the ratio of Mn in the sintered magnet is 0.15-0.23 wt% and the grain size of the alloy powder is 3.0-3.8 μm, the first sintering temperature is 900-1050°C and the temperature maintenance time is 6-8 h.

7. 4. The method for producing a sintered magnet as claimed in claim 3, wherein in step (S2), the tempering treatment is a secondary tempering, the primary tempering temperature is 700-950°C and the temperature maintenance time is 4-8 h, and the secondary tempering temperature is 450-600°C and the temperature maintenance time is 4-8 h.

8. Step (S2) is (S2a) respectively subjecting the Mn-free Nd-Fe-B main alloy flakes and the Mn-containing auxiliary alloy flakes in step (S1) to hydro-crushing and jet milling to obtain Mn-free Nd-Fe-B main alloy powder and Mn-containing auxiliary alloy powder, respectively, and uniformly mixing the Mn-free Nd-Fe-B main alloy powder and the Mn-containing auxiliary alloy powder to obtain a mixed alloy powder, which is then subjected to pressing, sintering and tempering to produce the high coercive force Nd-Fe-B sintered magnet; and / or in step (S2a), the Mn-free NdFeB main alloy powder has an average particle size of 3.0-3.8 μm; and / or the Mn-containing auxiliary alloy powder has an average particle size of 3 to 4 μm.

9. Step (S2) may also be (S2b) mixing the Mn-free Nd-Fe-B main alloy flakes of step (S1) with the Mn-containing auxiliary alloy flakes, followed by hydro-crushing and jet milling to obtain a mixed alloy powder, which is then subjected to pressing, sintering and tempering to produce the high coercivity Nd-Fe-B sintered magnet; And / or, in step (S2b), the mixed alloy powder has an average particle size of 3.0 to 3.8 μm.

10. Application of the sintered magnet according to claim 1 or 2 in the fields of new energy vehicle industry and wind power generation.

Citation Information

Patent Citations

  • Method for preparing rare earth magnet, and rare earth magnet

    JP2011014668A

  • R-t-b based sintered magnet

    JP2017073465A

  • R-t-b based sintered magnet

    JP2020161788A

  • R-t-b sintered magnet

    WO2008139556A1

  • R-t-cu-mn-b type sintered magnet

    WO2009150843A1