Biodegradable polyester resin and its manufacturing method
A copolymer of furandicarboxylic acid, aliphatic diol, and lactone compounds in polyester resin production addresses thermal discoloration issues, ensuring biodegradability and maintaining color stability.
Patent Information
- Application Number
- JP2024532357
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-07
- Filing Date
- 2022-11-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The production of polyester resins using furandicarboxylic acid leads to thermal discoloration issues such as yellowing and browning due to its low thermal stability, and existing methods to address this are inadequate.
A polyester resin is formulated as a copolymer of furandicarboxylic acid, an aliphatic diol compound, and a lactone compound, with controlled reaction steps and the use of titanium-based catalysts to minimize thermal discoloration during manufacturing.
The resulting polyester resin exhibits excellent biodegradability while effectively suppressing thermal discoloration, maintaining desirable physical properties and color characteristics.
Smart Images

Figure 2024541605000001 
Figure 2024541605000002 
Figure 2024541605000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a biodegradable polyester resin and a method for producing the same. [Background technology]
[0002] Polyester resin is a polymer resin that has ester (RO-C(=O)-R') functional groups in its main chain, and is used in a variety of industrial applications, including packaging, displays, and insulating materials.
[0003] A representative example is polyethylene terephthalate (PET) resin, which is produced by the reaction of terephthalic acid (TPA) and ethylene glycol (EG).
[0004] However, the main raw material for terephthalic acid is paraxylene, which is produced by refining crude oil. Therefore, the production and use of terephthalic acid leads to the depletion of crude oil resources. In addition, when terephthalic acid is decomposed, carbon dioxide emissions increase, which leads to environmental pollution and may cause climate change such as global warming.
[0005] In relation to this, attempts are being made to replace terephthalic acid with 2,5-furandicarboxylic acid (FDCA) during the production of polyester resins. Here, furandicarboxylic acid is a biomass-derived material that can prevent the depletion of crude oil resources and minimize environmental pollution and climate change due to its biodegradability.
[0006] However, furandicarboxylic acid is a compound with low thermal stability, and the process of esterifying this compound with a diol component induces thermal discoloration such as yellowing and browning.
[0007] Such problems cannot be solved by simply mixing furandicarboxylic acid with an aliphatic dicarboxylic acid and reacting it with the diol component. Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a polyester resin which exhibits excellent biodegradability and is suppressed from discoloring due to heat during the production process. [Means for solving the problem]
[0009] The present invention provides a polyester resin comprising a copolymer of a monomer mixture containing a furandicarboxylic acid compound, an aliphatic diol compound, and a lactone compound. Effect of the Invention
[0010] According to the present invention, it is possible to provide a polyester resin which exhibits excellent biodegradability and is suppressed from discoloring due to heat during the production process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] (Definition of terms) Throughout this specification, when a part is said to "comprise" a certain element, this means that it can further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.
[0012] To the extent used throughout this specification, the terms "step of" or "step of" do not mean "step for."
[0013] As used herein, the term "residue" refers to a certain portion or unit derived from a specific compound that is included in the product of a chemical reaction when the specific compound participates in the reaction.
[0014] For example, in the polyester resin, the "residue" derived from the furandicarboxylic acid compound means a portion derived from a furandicarboxylic acid compound.
[0015] The term "alkyl" as used herein, unless otherwise specified, refers to a saturated monovalent aliphatic hydrocarbon group, including straight and branched chains, having the specified number of carbon atoms. An alkyl group typically contains 1 to 20 carbon atoms ("C1-20 alkyl"), preferably 1 to 12 carbon atoms ("C1-12 alkyl"), more preferably 1 to 8 carbon atoms ("C1-8 alkyl"), or 1 to 6 carbon atoms ("C1-6 alkyl"), or 1 to 4 carbon atoms ("C1-4 alkyl"). Examples of alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, iso-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, and the like. An alkyl group may be substituted or unsubstituted. Unless otherwise specified, an alkyl group may be substituted with one or more halogens, up to the total number of hydrogen atoms present on the alkyl residue. Thus, alkyl having 1 to 4 carbon atoms includes halogenated alkyl groups, for example, fluorinated alkyl groups having 1 to 4 carbon atoms, such as trifluoromethyl (-CF3) or difluoroethyl (-CH2CHF2).
[0016] An alkyl group described herein as optionally substituted may be substituted with one or more substituents, which are independently selected unless otherwise specified. The total number of substituents is equal to the total number of hydrogen atoms on the alkyl residue to the extent that such substitution makes chemical sense. An optionally substituted alkyl group can typically contain 1-6 optional substituents, sometimes 1-5 optional substituents, preferably 1-4 optional substituents, and more preferably 1-3 optional substituents.
[0017] Suitable optional substituents for the alkyl group include, but are not limited to, alkyl of 1 to 8 carbon atoms, alkenyl of 2 to 8 carbon atoms, alkynyl of 2 to 8 carbon atoms, cycloalkyl of 3 to 8 carbon atoms, 3 to 12 membered heterocyclyl, aryl of 6 to 12 carbon atoms, and 5 to 12 membered heteroaryl, halo, =O (oxo), =S (thiono), =N-CN, =N-OR. x , =NR x , -CN, -C(O)R x , -CO2R x , -C(O)NR x R y , -SR x , -SOR x , -SO2R x , -SO2NR x R y , -NO2, -NR x R y , -NR x C(O)R y , -NR x C(O)NR x R y , -NR x C(O)OR x , -NR x SO2R y , -NR x SO2NR x R y , -OR x , -OC(O)R x and -OC(O)NR x R y Including each R x and R y are independently hydrogen (H), alkyl having 1 to 8 carbon atoms, acyl having 1 to 8 carbon atoms, alkenyl having 2 to 8 carbon atoms, alkynyl having 2 to 8 carbon atoms, cycloalkyl having 3 to 8 carbon atoms, 3 to 12 membered heterocyclyl, aryl having 6 to 12 carbon atoms, or 5 to 12 membered heteroaryl, or R x and R y can be taken together with the N atom to which they are attached to form a 3- to 12-membered heterocyclyl or a 5- to 12-membered heteroaryl ring, each of which is optionally selected from O, N, and S(O) q(wherein q is 0 to 2); each R x and R y is optionally substituted with 1 to 3 substituents independently selected from the group consisting of halo, =O, =S, =N-CN, =N-OR', =NR', -CN, -C(O)R', -COR', -C(O)NR'2, -SOR', -SOR', -SONR', -SONR'2, -NO2, -NR'2, -NR'C(O)R', -NR'C(O)NR'2, -NR'C(O)OR', -NR'SOR', -NR'SONR'2, -OR', -OC(O)R' and -OC(O)NR'2, wherein each R' is independently selected from hydrogen (H), and each of said alkyl having 1 to 8 carbon atoms, alkenyl having 2 to 8 carbon atoms, alkynyl having 2 to 8 carbon atoms, cycloalkyl having 3 to 8 carbon atoms, 3 to 12 membered heterocyclyl, aryl having 6 to 12 carbon atoms, or heteroaryl having 5 to 12 carbon atoms may be optionally substituted as further defined herein.
[0018] The term "alkoxy" as used herein, unless otherwise specified, refers to a monovalent -O-alkyl group in which the alkyl portion has the specified number of carbon atoms. An alkoxy group typically has 1 to 8 carbon atoms ("C1-8 alkoxy"), or 1 to 6 carbon atoms ("C1-6 alkoxy"), or 1 to 4 carbon atoms ("C1-4 alkoxy"). For example, an alkoxy having 1 to 4 carbon atoms includes methoxy (-OCH3), ethoxy (-OCH2CH3), isopropoxy (-OCH(CH3)2), tert-butyloxy (-OC(CH3)3), and the like. The alkoxy groups are as applicable to the alkyl, and may be substituted or unsubstituted on the alkyl portion with the same groups described herein. In particular, an alkoxy group may be optionally substituted with one or more halo atoms, in particular one or more fluoro atoms, up to the total number of hydrogen atoms present on the alkyl portion. Such groups have a specified number of carbon atoms and are substituted with one or more halo substituents, e.g., when fluorinated, are more specifically referred to as "fluoroalkoxy" groups; typically such groups contain 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms, sometimes 1 or 2 carbon atoms, and 1, 2 or 3 halo atoms (i.e., a "C1-6 haloalkoxy," a "C1-4 haloalkoxy," or a "C1-2 haloalkoxy"). More specifically, a fluorinated alkyl group can be specifically referred to as a fluoroalkoxy group, typically substituted with 1, 2 or 3 fluoro atoms, e.g., a C1-6, C1-4, or C1-2 fluoroalkoxy group. Thus, fluoroalkoxy of 1 to 4 carbon atoms includes trifluoromethyloxy (-OCF3), difluoromethyloxy (-OCF2H), fluoromethyloxy (-OCFH2), difluoroethyloxy (-OCH2CF2H), and the like.
[0019] The term "divalent aliphatic hydrocarbon (i.e., alkylene)" as used herein, unless otherwise specified, refers to a divalent hydrocarbyl group having a specified number of carbon atoms that can link two other groups together. Sometimes, alkylene is -(CH2) n- (where n is 1 to 8, preferably n is 1 to 4). In certain cases, alkylene can also be substituted with other groups and can contain at least one degree of unsubstitution (i.e., alkenylene or alkynylene residue) or ring. The open valences of an alkylene need not be at opposite ends of the chain. Thus, branched alkylene groups, such as -CH(Me)-, -CH2CH(Me)-, and -C(Me)2-, are also included within the scope of the term "alkylene", as are cyclic groups, such as cyclopropane-1,1-diyl, and unsaturated groups, such as ethylene (-CH=CH-) or propylene (-CH2-CH=CH-). The alkylene group can be substituted or unsubstituted with the same groups as described herein for alkyl.
[0020] As used herein, the terms "optionally substituted" and "substituted or unsubstituted" are used interchangeably to indicate that the particular group being described may have no non-hydrogen substituents (i.e., unsubstituted) or that the group may have one or more non-hydrogen substituents (i.e., substituted). Unless otherwise specified, the total number of substituents that may be present is equal to the number of H atoms present in the unsubstituted form of the group being described. When any substituent is attached through a double bond (e.g., an oxo (=O) substituent), the group occupies an available valence and the total number of other substituents included is reduced by two. When any substituent is independently selected from a list of substituents, the selected groups may be the same or different. It will be understood that throughout this specification, the number and nature of any substituent is limited to the extent that such substitution satisfies chemical significance.
[0021] In this specification, the CIE1976 L*a*b* color system corresponds to a color space defined by the CIE (International Commission on Illumination) and currently standardized worldwide.
[0022] In this CIE 1976 L*a*b* color space, the L* value represents lightness in CIE and ranges from 0 to 100, with 0 representing perfect black and 100 representing perfect white. a* represents the leaning towards either red or green, and if this value is positive, i.e., "+", it is red; if it is negative, i.e., "-", it is green. b* represents the leaning towards either yellow or blue, and if this value is positive, i.e., "+", it is yellow; if it is negative, i.e., "-", it is blue.
[0023] Based on the above definitions, the embodiments of the present invention will be described in detail. However, these are merely presented as examples and do not limit the present invention, and the present invention is defined only by the scope of the claims below.
[0024] (polyester resin) In one embodiment of the present invention, there is provided a polyester resin comprising a copolymer of a monomer mixture containing a furandicarboxylic acid compound, an aliphatic diol compound, and a lactone compound.
[0025] The furandicarboxylic acid-based compound itself has excellent biodegradability, and the lactone-based compound is converted into a compound having excellent biodegradability by a ring-opening polymerization reaction, so that polyester resins produced using these as raw materials have remarkably excellent biodegradability.
[0026] Alternatively, the first oligomer may be prepared in the presence of a titanium (Ti)-based catalyst containing a thermal stabilizer during the preparation of the polyester resin, thereby minimizing thermal discoloration during the preparation process (particularly polycondensation) of each type of polyester resin.
[0027] The polyester resin will be described in detail below.
[0028] Furandicarboxylic acid compounds The polyester resin contains residues derived from furandicarboxylic acid compounds (hereinafter, "residues derived from furandicarboxylic acid compounds") and exhibits excellent biodegradability due to the furandicarboxylic acid compounds.
[0029] The furandicarboxylic acid compound is represented by the following Chemical Formula 1:
[0030] [ka]
[0031] In the above chemical formula 1, L1 and L2 each independently represent a single bond, or a substituted or unsubstituted alkylene having 1 to 10 carbon atoms.
[0032] For example, the furandicarboxylic acid compound is 2,5-furandicarboxylic acid, and in this case, L1 and L2 in Formula 1 may all be single bonds.
[0033] The residue derived from the furandicarboxylic acid compound is represented by the following formula 1-1:
[0034] [ka]
[0035] In the above chemical formula 1-1, L1 and L2 each independently represent a single bond or a substituted or unsubstituted alkylene having 1 to 10 carbon atoms; * indicates the bonding position.
[0036] For example, when the furandicarboxylic acid compound is 2,5-furandicarboxylic acid, L1 and L2 in Formula 1-1 may all be single bonds.
[0037] Aliphatic diol compounds The polyester resin contains a residue derived from an aliphatic diol compound (hereinafter, "residue derived from an aliphatic diol compound"), and exhibits excellent compatibility and elongation properties due to the residue derived from the aliphatic diol compound.
[0038] The aliphatic diol compound is represented by the following Chemical Formula 2:
[0039] [ka]
[0040] In the above chemical formula 2, L3 and L4 each independently represent a substituted or unsubstituted alkylene having 1 to 10 carbon atoms.
[0041] For example, the aliphatic diol compound may be ethylene glycol or 1,4-butanediol. In this case, L3 in the above formula 2 may be a C1 alkylene (i.e., methylene), and R4 may be a C1 alkylene (i.e., methylene) or a C3 alkylene (i.e., propylene).
[0042] The residue derived from an aliphatic diol compound is represented by the following chemical formula 2-1:
[0043] [ka]
[0044] In the above chemical formula 2-1, R3 and R4 each independently represent a substituted or unsubstituted alkylene having 1 to 10 carbon atoms; * indicates a bonding position.
[0045] For example, when the aliphatic diol compound is ethylene glycol or 1,4-butanediol, R3 in the formula 2-1 can be a C1 alkylene (i.e., methylene), and R4 can be a C1 alkylene (i.e., methylene) or a C3 alkylene (i.e., propylene).
[0046] Lactone Compounds The polyester resin contains a residue derived from the lactone compound (hereinafter, "residue derived from a lactone compound"), and exhibits excellent biodegradability due to the residue derived from the lactone compound.
[0047] The lactone compound is represented by the following formula 3:
[0048] [ka]
[0049] In the above Chemical Formula 3, L5 is a substituted or unsubstituted alkylene having 1 to 10 carbon atoms.
[0050] For example, the lactone compound may be caprolactone, in which case L5 in Formula 3 may be a C5 alkylene (i.e., pentylene).
[0051] The lactone compound-derived residue is represented by the following chemical formula 3-1:
[0052] [ka]
[0053] In the above chemical formula 3-1, L5 is a substituted or unsubstituted alkylene having 1 to 10 carbon atoms; * indicates the bonding position.
[0054] For example, when the lactone compound is caprolactone, L5 in Formula 3-1 can be a C5 alkylene (ie, pentylene).
[0055] Copolymer structure The copolymer constituting the polyester resin may be a random copolymer or a block copolymer.
[0056] Specifically, the polyester resin may be the following first type polyester resin, second type polyester resin, or third type polyester resin.
[0057] 1) First type polyester resin: A block copolymer of a first oligomer and a second oligomer, the first oligomer being a polymer of a furandicarboxylic acid compound and a first aliphatic diol compound, and the second oligomer being a polymer of a lactone compound and a second aliphatic diol compound.
[0058] 2) Second type polyester resin: a block copolymer of a first oligomer and a monomer, the first oligomer being a polymer of a furandicarboxylic acid compound and a first aliphatic diol compound, and the monomer being a lactone compound.
[0059] 3) Third type polyester resin: A random copolymer of a furandicarboxylic acid compound, an aliphatic diol compound, and a lactone compound, in which the aliphatic diol compound includes a first aliphatic diol compound and a second aliphatic diol compound different from the first aliphatic diol compound.
[0060] Although more detailed descriptions will be given later, the polyester resin of the first type can be produced by subjecting an esterification reaction product (first oligomer) of the furandicarboxylic acid compound and the first aliphatic diol compound, and an esterification reaction product (second oligomer) of the lactone compound and the second aliphatic diol compound to an esterification reaction, a prepolymerization reaction, and a polycondensation reaction.
[0061] In addition, the second type polyester resin can be prepared by subjecting the esterification reaction product (first oligomer) of the furandicarboxylic acid compound and the first aliphatic diol compound, and the lactone compound to an esterification reaction, a prepolymerization reaction, and a polycondensation reaction.
[0062] In addition, the polyester resin of the third embodiment can be prepared by subjecting a furandicarboxylic acid-based compound, a first aliphatic diol-based compound, a second aliphatic diol-based compound, and a lactone-based compound to an esterification reaction, a prepolymerization reaction, and a polycondensation reaction.
[0063] The polyester resin of the first type and the polyester resin of the second type are advantageous in that the molecular weight can be easily adjusted and the structure can be easily designed, as compared with the polyester resin of the third type, and that the physical properties and color characteristics can be easily controlled.
[0064] For example, the polyester resin of the first type is represented by the following formula 4-1, and the polyester resin of the second type is represented by the following formula 4-2:
[0065] [ka]
[0066] [ka]
[0067] In the above chemical formulas 4-1 and 4-2, L1 and L2 each independently represent a single bond or a substituted or unsubstituted alkylene having 1 to 10 carbon atoms; L3 and L 31 , L 32 , L4, L 41 and L 42 each independently represents a substituted or unsubstituted alkylene having 1 to 10 carbon atoms; L5 is a substituted or unsubstituted alkylene having 1 to 10 carbon atoms; m and n each independently represent an integer of 1 to 100, and m:n is 1:10 to 10:1; * indicates a bonding position.
[0068] The m:n ratio may be 10:1 to 1:10, 8:1 to 1:8, 6:1 to 1:6, or 4:1 to 1:4.
[0069] Molar ratio In the polyester resins of the first and second embodiments, the first oligomer may be produced by controlling the molar ratio of the furandicarboxylic acid compound and the first aliphatic diol compound to 5:1 to 1:10, 3:1 to 1:7, 1:1 to 1:3, or 1:2 to 1:2.5.
[0070] If the first aliphatic diol compound is used in an amount of more than 10 molar parts based on 1 molar part of the furan dicarboxylic acid compound, the esterification reaction rate may be slowed down, or the physical properties and productivity of the final polyester resin may be reduced.
[0071] On the other hand, if the aliphatic diol compound is used in an amount less than 1 / 5 molar part based on 1 molar part of the furandicarboxylic acid compound, the unreacted components of the furandicarboxylic acid compound remain in excess, making it impossible to accurately confirm the end point of the esterification reaction, which may result in a prolonged esterification reaction, which may induce thermal discoloration of the final polyester resin or reduce the physical properties and brightness of the final polyester resin.
[0072] In the polyester resin of the first embodiment, the second oligomer may be produced by controlling the molar ratio of the lactone compound and the second aliphatic diol compound to 5:1 to 1:10, 3:1 to 1:7, 1:1 to 1:3, or 1:2 to 1:2.5.
[0073] If the second aliphatic diol compound is used in an amount of more than 10 molar parts based on 1 molar part of the lactone compound, the esterification reaction rate may be slowed down, or the physical properties and productivity of the final polyester resin may be reduced.
[0074] On the other hand, if the aliphatic diol compound is used in an amount less than 1 / 5 molar part based on 1 molar part of the lactone compound, the unreacted components of the lactone compound remain in excess, making it impossible to accurately confirm the end point of the esterification reaction, which may result in a prolonged esterification reaction, which may induce thermal discoloration of the final polyester resin or reduce the physical properties and brightness of the final polyester resin.
[0075] The polyester resin of the first type may be produced by controlling the molar ratio of the first oligomer and the second oligomer to 10:1 to 1:10, 8:1 to 1:8, 6:1 to 1:6, or 4:1 to 1:4.
[0076] In addition, the polyester resin of the second type may be produced by controlling the molar ratio of the first oligomer and the monomer (lactone compound) to 10:1 to 1:10, 8:1 to 1:8, 6:1 to 1:6, or 4:1 to 1:4.
[0077] If the second oligomer or the monomer (lactone compound) is used in an amount of more than 10 molar parts based on 1 molar part of the first oligomer, the esterification reaction rate may be slowed, or the physical properties and productivity of the final polyester resin may be reduced.
[0078] On the other hand, if the second oligomer or the monomer (lactone compound) is used in an amount less than 1 / 10 part by mole based on 1 part by mole of the first oligomer, the unreacted components of the first oligomer remain in an excessive amount, making it impossible to accurately confirm the end point of the esterification reaction, which may result in a prolonged esterification reaction, which may induce thermal discoloration of the final polyester resin or may reduce the physical properties and brightness of the final polyester resin.
[0079] Number average molecular weight (Mn) and molecular weight distribution (MWD) of polyester resin The polyester resin may have a number average molecular weight (Mn) of 50,000 to 200,000 g / mol, 60,000 to 180,000 g / mol, 70,000 to 150,000 g / mol, 80,000 to 130,000 g / mol, 90,000 to 110,000 g / mol, or 99,000 to 101,000 g / mol.
[0080] If the number average molecular weight of the polyester resin is less than 50,000 g / mol, it is difficult to process the polyester resin into a film for use as a packaging material, and the desired modulus cannot be achieved. Conversely, if the number average molecular weight is more than 200,000 g / mol, the viscosity becomes high, leading to low productivity and yield.
[0081] The polyester resin may have a ratio of weight average molecular weight (Mw) / number average molecular weight (Mn), i.e., a molecular weight distribution (MWD) of 1.0 to 3.0, specifically 1.1 to 2.5, more specifically 1.3 to 2.0, for example, 1.6 to 1.9.
[0082] If the molecular weight distribution of the polyester resin is less than 1.0, process control becomes difficult, resulting in a high defect rate and high process costs. On the other hand, if the molecular weight distribution of the polyester resin of the embodiment exceeds 3.0, the non-uniform molecular weight distribution may cause defects during product manufacturing.
[0083] Color properties of polyester resin The polyester resin may have an L* value of 93 or more, an a* value of 0 to 2, and a b* value of 7 or less according to the CIE1976 L*a*b* color system.
[0084] For example, the measurement method of the polyester resin color difference meter is as follows: 2 g of a polyester resin sample is dissolved in 20 ml of hexafluoroisopropanol (HFIP) (0.1 g / ml in HFIP). The color difference meter of the sample solution is measured in a Tuartz cell dedicated to solution color difference meter measurement using a CM-3700A product manufactured by Konica Minolta.
[0085] The higher the L* value, the closer the color to white the color can be expressed. However, depending on the use and purpose of the product to which the polyester resin of the embodiment is applied, the L* value can be controlled within a range of 93 or more, 94 or more, or 95 or more, and 100 or less, 99 or less, or 98 or less.
[0086] Specifically, the L* value of the polyester resin of the first embodiment may be smaller than that of the polyester resin of the second embodiment, which may be due to the fact that the polyester resin of the first embodiment is prepared by further including the second aliphatic diol compound.
[0087] In the case of the a* value, the smaller the value, the lighter the red and the darker the green, but depending on the use and purpose of the product to which the polyester resin of the embodiment is applied, the a* value may be controlled within a range of 0 or more, 0.1 or more, 0.3 or more, 0.5 or more, or 0.7 or more, and 2 or less, 1.8 or less, 1.7 or less, 1.5 or less, or 1.4 or less.
[0088] Specifically, the a* value of the polyester resin of the first embodiment may be larger than that of the polyester resin of the first embodiment, which may be due to the fact that the polyester resin is prepared by further including the second aliphatic diol compound.
[0089] In the case of the b* value, the smaller the value is within the range of 7 or less, the lighter the yellow color and the darker the blue color. In particular, according to the test examples described below, while all the comparative examples have b* values exceeding 7, all the examples have b* values of 7 or less, and it can be seen that thermal discoloration such as yellowing and browning during the manufacturing process was suppressed.
[0090] However, depending on the use or purpose of the product to which the polyester resin is applied, the b* value can be controlled to be 7 or less, 6.8 or less, 6.6 or less, or 6.4 or less, and the degree of yellow and blue can be controlled within a range of 0 or more, 1 or more, 2 or more, 3 or more, or 4 or more.
[0091] Specifically, the b* value of the polyester resin of the first embodiment may be larger than that of the polyester resin of the second embodiment, which may be due to the fact that the polyester resin of the first embodiment is prepared by further including the second aliphatic diol compound.
[0092] The color properties of the polyester resin of the embodiment can be adjusted by the reaction order of the monomers in the production process, the amount of the monomers used, and the like.
[0093] Physical Properties of Polyester The polyester resin is characterized by the change in intrinsic viscosity (ΔIV 12 ) may be 0.80 to 1.0, specifically 0.82 to 0.98 dl / g, more specifically 0.85 to 0.95 dl / g, for example, 0.87 to 0.92 dl / g:
[0094] [Formula 1] △IV 12 =IV1-IV2
[0095] In the above formula 1, IV1 is the intrinsic viscosity at 25°C, and IV2 is the intrinsic viscosity at 35°C.
[0096] The change in intrinsic viscosity according to the above formula (ΔIV 12If the modulus is less than the lower limit, it is difficult to process the film for use as a packaging material, and the desired modulus cannot be achieved. In contrast, if the modulus is more than the upper limit, the viscosity becomes high, leading to low productivity and low yield.
[0097] The polyester resin may have an intrinsic viscosity at 25° C. of 1.0 to 2.5 dl / g, specifically 1.3 to 2.3 dl / g, more specifically 1.5 to 2.0 dl / g, for example, 1.8 to 2.0 dl / g.
[0098] The polyester resin may have an intrinsic viscosity at 35° C. of 0.5 to 1.5 dl / g, specifically 0.7 to 1.3 dl / g, more specifically 0.9 to 1.1 dl / g, for example, 1.0 to 1.1 dl / g.
[0099] If the intrinsic viscosity measured at each of the temperatures is below the lower limit, it is difficult to process the film for use as a packaging material, and the desired modulus cannot be achieved.In contrast, if the intrinsic viscosity is above the upper limit, the viscosity becomes high, resulting in low productivity and yield.
[0100] The polyester resin may have a glass transition temperature (Tg) of -60 to 10°C, specifically -55 to 5°C, for example, 50 to 1°C.
[0101] If the glass transition temperature is less than -60°C, the polyester resin cannot have physical properties or thermal stability at room temperature, and there is a limit to the film processing process of the polyester resin for use as a packaging material.In contrast, in order to have a glass transition temperature exceeding 10°C, the density of the molecular structure must be high, and in this case, the crystallinity of the polyester resin also increases, resulting in a decrease in transparency.
[0102] (Method of producing polyester resin) In another embodiment of the present invention, there is provided a method for producing a polyester resin, the method including copolymerizing a monomer mixture including a furandicarboxylic acid compound, an aliphatic diol compound, and a lactone compound.
[0103] This makes it possible to obtain a polyester resin having the above-mentioned excellent properties.
[0104] raw material In preparing the polyester resin, the furan dicarboxylic acid compound, the first aliphatic diol compound, the second aliphatic diol compound and the lactone compound are used as raw materials. The structure of each raw material is as described above.
[0105] Reaction sequence The polyester resin of the third type may be prepared by subjecting a furandicarboxylic acid-based compound, a first aliphatic diol-based compound, a second aliphatic diol-based compound, and a lactone-based compound to an esterification reaction, a prepolymerization reaction, and a polycondensation reaction.
[0106] As described above, when a furan dicarboxylic acid compound is used alone as a diacid component, it is inevitable that a yellowed or browned polyester resin is obtained. In addition, even if an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid are mixed together with a diol component and reacted, there is a limit to the suppression of thermal discoloration, and there is also a problem that physical properties such as intrinsic viscosity are reduced.
[0107] The above problem can be solved by controlling the reaction sequence.
[0108] Specifically, the method includes the steps of: preparing a first oligomer by esterifying a furandicarboxylic acid compound and an aliphatic diol compound; preparing a second oligomer by esterifying a lactone compound and a second aliphatic diol compound; and subjecting the first oligomer and the second oligomer to an esterification reaction, a prepolymerization reaction, and a polycondensation reaction, thereby preparing the first type of polyester resin.
[0109] Separately, the second type of polyester resin may be produced by the steps of: preparing a first oligomer by esterifying a furandicarboxylic acid-based compound and an aliphatic diol-based compound; and esterifying, prepolymerizing, and polycondensing the first oligomer and a lactone-based compound monomer.
[0110] More specifically, in the process of preparing the first oligomer, the size and molecular weight of the oligomer can be controlled to a level that avoids thermal discoloration.
[0111] In this manner, when the first oligomer is reacted with the second oligomer or the lactone compound in sequence (i.e., esterification, prepolymerization, and polycondensation) while the size and molecular weight of the oligomer are controlled, not only is thermal discoloration suppressed, but the intrinsic viscosity also increases rapidly.
[0112] In short, by first esterifying the furan dicarboxylic acid compound and the first aliphatic diol compound, and then further reacting the lactone compound monomer or the esterification reaction product thereof with the second aliphatic diol compound, it is possible to obtain a polyester resin having improved physical properties such as intrinsic viscosity as well as suppressing yellowing or browning during the manufacturing process.
[0113] Furthermore, when preparing the polyester resin of each type, the first oligomer may be prepared in the presence of a titanium (Ti)-based catalyst containing a thermal stabilizer, thereby minimizing thermal discoloration during the preparation process (especially polycondensation) of the polyester resin of each type.
[0114] Preparation of the first oligomer In preparing the polyester resin of each of the above types, the furandicarboxylic acid-based compound is first reacted with the aliphatic diol-based compound to prepare a first oligomer having a low degree of polymerization.
[0115] Considering the amount of the furan dicarboxylic acid compound and the first aliphatic diol compound that is lost or remains unreacted during the esterification reaction, the aliphatic diol compound may be used in excess of the amount of the desired copolymer composition.
[0116] Specifically, in the esterification reaction step of the furandicarboxylic acid compound and the first aliphatic diol compound, 1 / 5 to 10 molar parts, 1 / 3 to 7 molar parts, 1 to 3 molar parts, or 2 to 2.5 molar parts of the first aliphatic diol compound may be reacted with 1 molar part of the furandicarboxylic acid compound.
[0117] If the first aliphatic diol compound is used in an amount of more than 10 parts by mole based on 1 part by mole of the furan dicarboxylic acid compound, the esterification reaction rate may be slowed down, or the physical properties and productivity of the final polyester resin may be reduced.
[0118] On the other hand, if the first aliphatic diol compound is used in an amount less than 1 / 5 molar part based on 1 molar part of the furandicarboxylic acid compound, the unreacted components of the furandicarboxylic acid compound remain in an excessive amount, making it impossible to accurately confirm the end point of the esterification reaction, which may result in a prolonged esterification reaction, which may induce thermal discoloration of the final polyester resin or may reduce the physical properties and brightness of the final polyester resin.
[0119] A first oligomer including a residue derived from a furandicarboxylic acid compound and a residue derived from a first aliphatic diol compound can be produced by the esterification reaction of the furandicarboxylic acid compound and the first aliphatic diol compound.
[0120] In this process, the size and molecular weight of the first oligomer can be controlled to a level that avoids thermal discoloration. For example, when a first oligomer having a number average molecular weight of 1500 to 4000 g / mol is formed, the size and molecular weight prevent thermal damage to the molecule at high temperatures, and thermal discoloration in subsequent steps can be avoided.
[0121] The esterification reaction of the furandicarboxylic acid compound and the first aliphatic diol compound can be carried out in a nitrogen (N2) atmosphere.
[0122] In addition, the esterification reaction of the furandicarboxylic acid compound and the first aliphatic diol compound can be carried out at a temperature range of 160°C or more, 170°C or more, or 180°C or more, and 260°C or less, 240°C or less, or 220°C or less.
[0123] In addition, the esterification reaction of the furandicarboxylic acid compound and the first aliphatic diol compound can be carried out for 1 hour or more, 1.5 hours or more, or 2 hours or more, and 8 hours or less, 7 hours or less, or 6 hours or less.
[0124] If the esterification reaction temperature, reaction time, etc. of the furan dicarboxylic acid compound and the first aliphatic diol compound are below the respective ranges, the reaction yield is low or the reaction does not occur sufficiently, and the physical properties of the final polyester are deteriorated. In contrast, if the esterification reaction temperature, reaction time, etc. of the furan dicarboxylic acid compound and the first aliphatic diol compound are above the respective ranges, a depolymerization reaction occurs, and the polyester resin is not synthesized, or the appearance of the synthesized polyester is likely to be yellow.
[0125] The esterification reaction of the furan dicarboxylic acid compound and the first aliphatic diol compound (i.e., the preparation of the first oligomer) can be carried out in the presence of a titanium (Ti) catalyst containing a thermal stabilizer, thereby minimizing thermal discoloration during the preparation process (particularly polycondensation) of each type of polyester resin.
[0126] Preparation of the second oligomer In the production of the polyester resin of the first embodiment, a second oligomer is produced separately from the first oligomer. Specifically, a lactone compound and a second aliphatic diol compound are reacted to produce a second oligomer having a low degree of polymerization.
[0127] Taking into consideration the amount of the lactone compound and the second aliphatic diol compound lost or unreacted during the esterification reaction, the aliphatic diol compound may be used in excess of the desired copolymer composition.
[0128] Specifically, in the esterification reaction step of the lactone compound and the second aliphatic diol compound, the first aliphatic diol compound may be reacted in an amount of 1 / 5 to 10 molar parts, 1 / 3 to 7 molar parts, 1 to 3 molar parts, or 2 to 2.5 molar parts based on 1 molar part of the lactone compound.
[0129] If the second aliphatic diol compound is used in an amount of more than 10 molar parts based on 1 molar part of the lactone compound, the molecular weight of these oligomers becomes low, and discoloration occurs during the polycondensation process carried out at high temperatures, and the physical properties and hue of the final polyester resin are deteriorated.
[0130] On the other hand, if the second aliphatic diol compound is used in an amount less than 1 / 5 molar part based on 1 molar part of the lactone compound, the unreacted components of the lactone compound remain in an excessive amount, making it impossible to accurately confirm the end point of the esterification reaction, which may result in a prolonged esterification reaction, which may induce thermal discoloration of the final polyester resin or may reduce the physical properties and brightness of the final polyester resin.
[0131] In the esterification reaction process of the lactone compound and the second aliphatic diol compound, a ring-opening polymerization reaction of the lactone compound can occur, thereby producing a second oligomer containing a residue derived from the lactone compound and a residue derived from the second aliphatic diol compound.
[0132] In this process, the size and molecular weight of the second oligomer can be controlled to a level that avoids thermal discoloration. For example, when a second oligomer having a number average molecular weight of 1500 to 4000 g / mol is formed, the size and molecular weight prevent thermal damage to the molecule at high temperatures, and thermal discoloration in subsequent steps can be avoided.
[0133] The esterification reaction of the lactone compound and the second aliphatic diol compound can be carried out in a nitrogen (N2) atmosphere.
[0134] In addition, the esterification reaction of the lactone compound and the second aliphatic diol compound can be carried out at a temperature range of 160°C or more, 170°C or more, or 180°C or more, and 260°C or less, 240°C or less, or 220°C or less.
[0135] The esterification reaction of the lactone compound and the second aliphatic diol compound can be carried out for 1 hour or more, 1.5 hours or more, or 2 hours or more, and can be carried out for 8 hours or less, 7 hours or less, or 6 hours or less.
[0136] If the esterification reaction temperature, reaction time, etc. of the lactone compound and the second aliphatic diol compound are below the respective ranges, the reaction yield is low or the reaction does not occur sufficiently, and the physical properties of the final polyester are deteriorated. In contrast, if the esterification reaction temperature, reaction time, etc. of the lactone compound and the second aliphatic diol compound are above the respective ranges, a depolymerization reaction occurs, and the polyester resin is not synthesized, or the appearance of the synthesized polyester is likely to be yellow.
[0137] The esterification reaction of the lactone compound and the second aliphatic diol compound (i.e., the preparation of the second oligomer) can be carried out in the presence of an antimony (Sb)-based catalyst, thereby minimizing thermal discoloration during the preparation process of the second oligomer (particularly, polycondensation).
[0138] Reaction of the first oligomer with the second oligomer or lactone compound; In preparing the polyester resin of the first type, the first oligomer and the second oligomer are reacted in sequence (that is, esterification reaction, prepolymerization, and polycondensation reaction).
[0139] Meanwhile, when preparing the polyester resin of the second type, the first oligomer and the lactone compound are reacted in sequence (that is, esterification reaction, prepolymerization, and polycondensation reaction).
[0140] In this case, 1 / 10 to 10 molar parts, 1 / 8 to 8 molar parts, 1 / 6 to 6 molar parts, or 1 / 4 to 4 molar parts of the second oligomer or the lactone compound can be reacted with 1 molar part of the first oligomer.
[0141] If the second oligomer or the lactone compound is used in an amount of more than 10 parts by mole based on 1 part by mole of the first oligomer, the esterification reaction rate may be slowed down, or the physical properties and productivity of the final polyester resin may be reduced.
[0142] On the other hand, if the second oligomer or the lactone compound is used in an amount less than 1 / 10 part by mole based on 1 part by mole of the first oligomer, the unreacted components of the first oligomer remain in an excessive amount, making it impossible to accurately confirm the end point of the esterification reaction, which may result in a prolonged esterification reaction, which may induce thermal discoloration of the final polyester resin or may reduce the physical properties and brightness of the final polyester resin.
[0143] When the polyester resin of the first type is produced, the residue derived from the aliphatic diol compound in the first oligomer and the residue derived from the lactone compound in the second oligomer are bonded together.
[0144] When preparing the polyester resin of the second type, a ring-opening polymerization reaction of the lactone compound may occur, whereby the residue derived from the aliphatic diol compound in the first oligomer and the residue derived from the lactone compound are bonded to each other.
[0145] The reaction of the second oligomer or the lactone compound with the first oligomer may produce a third oligomer having a larger size and molecular weight than the first oligomer and the second oligomer. The third oligomer may have a number average molecular weight of 2,000 to 8,000 g / mol.
[0146] The esterification reaction of the second oligomer or the lactone compound with the first oligomer may be carried out in a nitrogen (N2) atmosphere.
[0147] In addition, the esterification reaction of the second oligomer or the lactone compound with the first oligomer may be carried out at a temperature range of 160°C or more, 170°C or more, or 180°C or more, and 260°C or less, 240°C or less, or 220°C or less.
[0148] In addition, the esterification reaction of the second oligomer or the lactone compound with the first oligomer may be carried out for 1 hour or more, 1.5 hours or more, or 2 hours or more, and may be carried out for 8 hours or less, 7 hours or less, or 6 hours or less.
[0149] If the esterification reaction temperature, reaction time, etc. of the second oligomer or lactone compound and the first oligomer are below the respective ranges, the reaction yield is low or the reaction does not occur sufficiently, resulting in poor physical properties of the final polyester. In contrast, if the esterification reaction temperature, reaction time, etc. of the second oligomer or lactone compound and the first oligomer are above the respective ranges, a depolymerization reaction occurs, resulting in no synthesis of a polyester resin, or the appearance of the synthesized polyester is likely to turn yellow.
[0150] Meanwhile, the esterification reaction of the second oligomer or the lactone compound with the first oligomer may be carried out in the presence of an esterification catalyst containing a titanium (Ti) compound. In particular, the esterification catalyst is added to the esterification reaction of the second oligomer or the lactone compound with the first oligomer, thereby improving the reaction rate from the initial stage of the reaction and shortening the time that the polyester resin is exposed to heat.
[0151] The titanium (Ti)-based compound may be, for example, titanium oxide, titanium butoxide, titanium alkoxide, titanium chelate, or a mixture thereof.
[0152] The esterification catalyst can be used in an amount of 1 ppm to 100 ppm based on the central metal atom of the polyester to be synthesized. If the content of the esterification catalyst is too low, it becomes difficult to significantly improve the efficiency of the esterification reaction, and the amount of reactants that do not participate in the reaction can increase significantly. If the content of the esterification catalyst is too high, the appearance properties of the polyester produced will decrease. If the content of the esterification catalyst is too high, the polyester produced will yellow and the appearance properties will decrease.
[0153] In preparing the polyester resin of each type, the second oligomer or the lactone compound and the first oligomer are esterified, and then a polymer having a higher degree of polymerization is prepared by prepolymerization.
[0154] A heat stabilizer may be used in the prepolymerization step, and the use of such a stabilizer can minimize thermal discoloration during the prepolymerization step as well as the subsequent polycondensation reaction.
[0155] Specifically, the thermal stabilizer includes at least one selected from the group of phosphorus-based thermal stabilizers including trimethyl phosphonoacetate, triethyl phosphonoacetate, phosphoric acid, phosphorous acid, polyphosphoric acid, trimethyl phosphate (TMP), triethyl phosphate, trimethyl phosphine, and triphenyl phosphine;
[0156] For example, the heat stabilizer can be added in an amount about twice that of the esterification catalyst. When the heat stabilizer is used in the above range, thermal discoloration during the prepolymerization and polycondensation reactions can be minimized.
[0157] The pre-polymerization can be carried out under temperature controlled conditions (thermal pre-condensation).
[0158] Specifically, the prepolymerization can be performed including: a step of increasing the temperature until the temperature reaches a range of 220 to 260° C.; and a step of maintaining the reached temperature and prepolymerizing the second esterification reaction product.
[0159] In addition, after the pressure is reduced until the pressure during the temperature increase reaches 0 to 0.3 atm, the ultimate pressure can be maintained while the ultimate temperature is maintained.
[0160] The prepolymerization step is a step of changing the pressure from normal pressure to vacuum before carrying out the polycondensation reaction (vacuum) described below, and is a step of gradually changing the pressure from normal pressure (1 atm) to vacuum (0 atm). If the prepolymerization step is omitted, the secondary esterification reaction product volatilizes during the sudden change to a vacuum state, inducing the Dolby phenomenon, reducing the yield of the final polyester resin, and potentially adversely affecting its physical properties.
[0161] In preparing each of the above polyester resins, the second oligomer or lactone compound and the first oligomer are subjected to an esterification reaction and a prepolymerization reaction, and then the prepolymerized polymer is subjected to a polycondensation reaction.
[0162] The poly-condensation step can be carried out in a vacuum atmosphere at a temperature of 220 to 300° C. and a pressure of 0.8 to 0.4 torr or less for 2 to 6 hours.
[0163] The polycondensation reaction step can be carried out under a vacuum slightly higher than 0 atm. The degree of vacuum is measured with a vacuum gauge, and polymerization is usually carried out in the range of 0.8 to 0.4 torr.
[0164] In the polycondensation, a polycondensation reaction catalyst can be used.
[0165] The polycondensation catalyst may be added to the product of the esterification reaction before the start of the polycondensation reaction, may be added to a mixture containing the diol component and the dicarboxylic acid component before the esterification reaction, or may be added during the esterification reaction step.
[0166] The polycondensation catalyst may be a titanium-based compound, a germanium-based compound, an antimony-based compound, an aluminum-based compound, a tin-based compound, or a mixture thereof.
[0167] Examples of the titanium-based compound include tetraethyl titanate, acetyl tripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, polybutyl titanate, 2-ethylhexyl titanate, octylene glycol titanate, titanium lactate, triethanolamine titanate, acetylacetonate titanate, ethyl acetoacetic ester titanate, isostearyl titanate, titanium dioxide, titanium dioxide / silicon dioxide copolymer, and titanium dioxide / zirconium dioxide copolymer.
[0168] Examples of the germanium-based compound include germanium dioxide (GeO2), germanium tetrachloride (GeCl4), germanium ethyleneglycoxide, germanium acetate, copolymers using these, and mixtures thereof.
[0169] [Mode for carrying out the invention] The present invention will now be described with reference to examples. However, the following examples are merely illustrative of the present invention, and the scope of the present invention is not limited to these examples.
[0170] [Examples 1-1 to 1-5: Polyester resin of the first type] Example 1-1 1 mol of 2,5-furandicarboxylic acid (FDCA) and 2 to 2.5 mol of 1,4-butanediol (1,4-BDO) were added to the hopper of a 10 L first autoclave reactor. Then, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate (product name: Plenact-55, manufacturer: AJINOMOTO FINE TECHNO), a type of titanium (Ti)-based catalyst containing a thermal stabilizer, was added in an amount of 50 ppm based on Ti, and the esterification reaction of the FDCA and 1,4-BDO was carried out at a temperature of 190°C in a nitrogen atmosphere for 2 to 3 hours. This reaction produced a first oligomer consisting of FDCA-derived and 1,4-BDO-derived residues.
[0171] Separately, 1 mol of caprolactone (CL) and ethylene glycol (EG) were added to the hopper of a 10 L second Autoclave reactor. Then, antimony acetate, a type of antimony (Sb)-based catalyst, was added in an amount of 50 ppm based on Sb, and the esterification reaction of the CL and EG was carried out at a temperature of 190°C in a nitrogen atmosphere for 2 to 3 hours. As a result of this reaction, a second oligomer consisting of CL-derived residues and EG-derived residues was produced.
[0172] When the reaction for producing the first oligomer and the second oligomer was completed, the second oligomer was introduced into the hopper of a 10 L third Autoclave reactor, in the amount of the second oligomer introduced according to Table 1 below.
[0173] The esterification reaction of the first oligomer and the second oligomer was carried out at a temperature of 190° C. in a nitrogen atmosphere for 1 hour.
[0174] The reaction is terminated when the outflow water generated by the esterification reaction of the first oligomer and the second oligomer is no longer discharged. After the reaction is completed, titanium tert-butoxide, which is a type of Tin Alkoxide catalyst, is added as a polycondensation catalyst in an amount of 100 ppm based on Tin, and triethyl phosphonoacetate, a thermal stabilizer, is added in an amount of 200 ppm, which is twice the amount of the polycondensation catalyst. After adding the polycondensation catalyst and the thermal stabilizer, the mixture is stirred for 30 minutes, and the internal temperature of the reactor is raised for 1 hour to reach a temperature range of 220 to 240°C, and then the pressure is gradually reduced for 1 hour using a vacuum pump to allow the internal pressure of the reactor to reach 1 atm to 0 atm, thereby carrying out prepolymerization.
[0175] Then, the reaction was carried out for 2 to 6 hours at a temperature range of 220 to 240°C under high vacuum of 0.8 torr or less, and when the load transmitted to the torque meter of the autoclave reached a desired load, the load was drained to obtain the polyester resin of Example 1-1.
[0176] Examples 1-2 to 1-5 Each of the polyester resins of Examples 1-2 to 1-5 was produced in the same manner as in Example 1-1, except that the amounts of the first oligomer and the second oligomer added were changed according to Table 1 below.
[0177] [Table 1]
[0178] [Examples 2-1 to 2-5: Polyester resin of the second form] Example 2-1 Each of the polyester resins of Examples 2-1 to 2-5 was produced in the same manner as in Example 1-1, except that the second oligomer was changed to caprolactone (CL), in which the amount of caprolactone added is shown in Table 2 below.
[0179] [Table 2]
[0180] Example 3-1 (FDCA+1,4-BDO+CL+EG) Into the hopper of a 2L first autoclave reactor, 4.03 mol of 2,5-furandicarboxylic acid (FDCA), 10.08 mol of 1,4-butanediol (1,4-BDO), 1.34 mol of caprolactone (CL) and 0.175 mol of ethylene glycol (EG) were added. Then, dibutyltin oxide, a type of Tin catalyst, was added in an amount of 50 ppm based on Tin, and the esterification reaction of the FDCA, 1,4-BDO, caprolactone and EG was carried out at a temperature of 190°C in a nitrogen atmosphere for 2 to 3 hours. As a result of this reaction, oligomers consisting of FDCA-derived residues, 1,4-BDO-derived residues, CL-derived residues and EG-derived residues were produced.
[0181] After the esterification reaction was completed, titanium tert-butoxide, a type of Tin Alkoxide catalyst, was added as a polycondensation catalyst in an amount of 100 ppm based on Tin, and triethyl phosphonoacetate, a thermal stabilizer, was added in an amount of 200 ppm, which is twice the amount of the polycondensation catalyst. After adding the polycondensation catalyst and the thermal stabilizer, the mixture was stirred for 30 minutes, and the temperature inside the reactor was raised for 1 hour to reach a temperature range of 220 to 240°C, and then the pressure was gradually reduced using a vacuum pump for 1 hour to allow the pressure inside the reactor to reach 1 atm to 0 atm, thereby allowing prepolymerization to proceed.
[0182] Then, the reaction was carried out for 2 to 6 hours at a temperature range of 220 to 240°C under high vacuum of 0.8 torr or less, and when the load transmitted to the torque meter of the autoclave reached a desired load, the load was drained to obtain the polyester resin of Example 3-1.
[0183] Example 3-2 (FDCA+1,4-BDO+CL+EG) A polyester resin was obtained in the same manner as in Example 3-1, except that the amounts of raw materials charged were changed to the compositions shown in Table 3 below.
[0184] Example 3-3 (FDCA+1,4-BDO+CL+EG) A polyester resin was obtained in the same manner as in Example 3-1, except that the amounts of raw materials charged were changed to the compositions shown in Table 3 below.
[0185] Example 3-4 (FDCA+1,4-BDO+CL+EG) A polyester resin was obtained in the same manner as in Example 3-1, except that the amounts of raw materials charged were changed to the compositions shown in Table 3 below.
[0186] Example 3-5 (FDCA+1,4-BDO+CL+EG) A polyester resin was obtained in the same manner as in Example 3-1, except that the amounts of raw materials charged were changed to the compositions shown in Table 3 below.
[0187] [Table 3]
[0188] [Comparative Example] Comparative example 1-1 (FDCA+1,4-BDO) 4.75 mol of 2,5-furandicarboxylic acid (FDCA) and 11.89 mol of 1,4-butanediol (1,4-BDO) were added to the hopper of a 10 L first autoclave reactor. Then, dibutyltin oxide, a type of Tin catalyst, was added in an amount of 50 ppm based on Tin, and the esterification reaction of the FDCA and 1,4-BDO was carried out at a temperature of 190°C in a nitrogen atmosphere for 2 to 3 hours. This reaction produced oligomers consisting of FDCA-derived residues and 1,4-BDO-derived residues.
[0189] After the esterification reaction was completed, titanium tert-butoxide, a type of Tin Alkoxide catalyst, was added as a polycondensation catalyst in an amount of 100 ppm based on Tin, and triethyl phosphonoacetate, a thermal stabilizer, was added in an amount of 200 ppm, which is twice the amount of the polycondensation catalyst. After adding the polycondensation catalyst and the thermal stabilizer, the mixture was stirred for 30 minutes, and the internal temperature of the reactor was raised for 1 hour to reach a temperature range of 220 to 240°C, and then the pressure was gradually reduced using a vacuum pump for 1 hour to allow the internal pressure of the reactor to reach 1 atm to 0 atm, thereby allowing prepolymerization to proceed.
[0190] Then, the reaction was carried out for 2 to 6 hours at a temperature range of 220 to 240°C under high vacuum of 0.8 torr or less, and when the load transmitted to the torque meter of the autoclave reached a desired load, the load was drained to obtain a polyester resin of Comparative Example 1.
[0191] Comparative example 1-2 (CL+EG) 8.76 mol of caprolactone (CL) and 0.175 mol of ethylene glycol (EG) were added to the hopper of a 2L first autoclave reactor. Then, dibutyltin oxide, a type of Tin catalyst, was added in an amount of 50 ppm based on Tin, and the esterification reaction of the FDCA and 1,4-BDO was carried out at a temperature of 190°C in a nitrogen atmosphere for 2 to 3 hours. This reaction produced oligomers consisting of CL-derived residues and EG-derived residues.
[0192] After the esterification reaction was completed, titanium tert-butoxide, a type of Tin Alkoxide catalyst, was added as a polycondensation catalyst in an amount of 100 ppm based on Tin, and triethyl phosphonoacetate, a thermal stabilizer, was added in an amount of 200 ppm, which is twice the amount of the polycondensation catalyst. After adding the polycondensation catalyst and the thermal stabilizer, the mixture was stirred for 30 minutes, and the internal temperature of the reactor was raised for 1 hour to reach a temperature range of 220 to 240°C, and then the pressure was gradually reduced using a vacuum pump for 1 hour to allow the internal pressure of the reactor to reach 1 atm to 0 atm, thereby allowing prepolymerization to proceed.
[0193] Then, the reaction was carried out for 2 to 6 hours at a temperature range of 220 to 240°C under high vacuum of 0.8 torr or less, and when the load transmitted to the torque meter of the autoclave reached a desired load, the load was drained to obtain a polyester resin of Comparative Example 2.
[0194] [Table 4]
[0195] Test Example 1: Weight, Color, and Physical Properties of Polyester Resins The weight, color, and physical properties of each of the polyester resin samples were evaluated by the following methods, and the evaluation results are shown in Tables 5 to 7 below.
[0196] 1) Number average molecular weight (Mn) and molecular weight distribution (MWD) of polyester resin: The molecular weight distribution ("Mw / Mn") was determined by measuring Mw and Mn using gel permeation chromatography (GPC).
[0197] Specifically, the analysis was performed using a TSKgel guardcolumn SuperAW-H + 2x TSKgel SuperAWM-H (6.0 x 150 mm) column and a Tosoh HLC-8420 GPC apparatus. The evaluation temperature was 40°C, HFIP + 0.01N NaTFA was used as the developing solvent, and the flow rate was 0.3 mL / min.
[0198] Samples, including polyester resin samples, were prepared to a concentration of 3 mg / 10 mL and then delivered in 10 μL volumes. Calibration curves generated using PMMA standards were used to derive Mw and Mn values and determine the molecular weight distribution ("Mw / Mn").
[0199] 2) Color characteristics: L*, a* and b* values were measured under the following conditions using a Chip color difference meter manufactured by Nippon Denshoku (sa-4000).
[0200] Specifically, 2 g of a polyester resin sample was dissolved in 20 ml of hexafluoroisopropanol (HFIP) (0.1 g / ml in HFIP). The color of the sample solution was measured using a Tuartz cell dedicated to solution colorimeter measurement using a Konica Minolta CM-3700A product.
[0201] 3) Intrinsic viscosity (IV): 0.5 g of a polyester resin sample was dissolved in 10 ml of a 1:1 (v:v) phenol:tetrachloroethane solution, and the IV was measured at 25°C and 35°C using an Ostwald viscometer.
[0202] 4) Glass transition temperature (Tg): Measured using a DSC manufactured by TA Instruments under conditions of N2, 20 psi, and a rate of 20°C / min from room temperature to 300°C.
[0203] [Table 5]
[0204] According to Table 5 above, the polyester resins of the examples have Mn of 99,000 to 101,000 g / mol and MWD of 1.6 to 1.9.
[0205] On the other hand, it was found that the polyester resins of Examples 1-1 to 1-5 and 2-1 to 2-5 had similar levels of Mn but reduced MWD compared to Examples 3-1 to 3-5 in which all raw materials (FDCA, 1,4-BDO, CL and EG) were reacted together.
[0206] The polyester resin of such an embodiment can have its Mn and MWD controlled by adjusting the types and amounts of raw materials used during production.
[0207] [Table 6]
[0208] According to Table 6 above, the polyester resins of the examples have an L* value of 95.1 to 97.8, an a* value of 0.79 to 1.3, and a b* value of 4.3 to 6.4 according to the CIE1976 L*a*b* color system.
[0209] In particular, the b* values of the polyester resins of Examples 1-1 to 1-5 and 2-1 to 2-5, as measured by the CIE 1976 L*a*b* color system, are lower than those of Comparative Examples 1-1 and 1-2, due to the control of the types of residues (monomers) in the final resin.
[0210] Furthermore, the polyester resins of Examples 1-1 to 1-5 and 2-1 to 2-5 have lower b* values in the CIE1976 L*a*b* color system than those of Examples 3-1 to 3-5, which is due to the formation of a block copolymer.
[0211] The polyester resin of such an embodiment can control the L* value, a* value and b* value according to the CIE1976 L*a*b* color system by adjusting the types and amounts of raw materials used during production.
[0212] Meanwhile, the L* value of the polyester resin of the first embodiment (Examples 1-1 to 1-5) may be smaller and the a* and b* values may be larger than those of the polyester resin of the second embodiment (Examples 2-1 to 2-5). This may be due to the fact that the polyester resin of the first embodiment (Examples 1-1 to 1-5) is prepared by further including the second aliphatic diol compound.
[0213] [Table 7]
[0214] According to Table 7, the polyester resin of the embodiment has a change in intrinsic viscosity (ΔIV 12 =IV1-IV2) is 0.87 to 0.92, the intrinsic viscosity is 1.88 to 1.95 dl / g at 25°C, and 1.01 to 1.03 dl / g at 35°C. The polyester resin of the example has a glass transition temperature of -46.1 to 0.5°C.
[0215] The intrinsic viscosity and glass transition temperature of the polyester resin of this embodiment can be controlled at each temperature by adjusting the types and amounts of raw materials used during production.
[0216] Test Example 2: Physical properties of films containing polyester resin For each of the polyester resin samples, the physical properties after film production were evaluated by the following methods, and the evaluation results are shown in Table 8 below.
[0217] 1) Transmittance: Each of the polyester resin samples was used to produce a biaxially stretched film. Specifically, the polyester resin sample was melted at a temperature of 180 to 260° C. in an extruder.
[0218] The melt was extruded through a die to form a sheet and quenched. The sheet thus obtained was stretched 3.0 times in the machine direction (MD) and then 3.7 times in the transverse direction (TD). In order to impart dimensional stability to the stretched film, the film was heat-set at 120 to 160°C under tension to obtain a biaxially stretched film.
[0219] The polyester film thus produced was cut into a size of 10 cm x 10 cm (longitudinal length x horizontal length) to prepare a test piece. The parallel transmittance and diffuse transmittance of the test piece were measured by the ASTM D1003-97 measurement method using a Minolta CM-3600A measuring device. The transmittance is defined as the combined value of the parallel transmittance and diffuse transmittance. Therefore, the transmittance was calculated from the parallel transmittance and diffuse transmittance of the test piece.
[0220] 2) Modulus, tensile strength and elongation: For polyester resin samples, a Microcompounder extruder was used to prepare ASTM D638-V Type test specimens at an extrusion temperature of 120~160℃ and a screw speed of 100~120rpm.
[0221] The polyester resin test specimen thus prepared was mounted in the LD direction using a vice grip in a universal testing machine UTM 5566A (Instron). The strength at the point where the sample broke while stretching at a rate of 5 mm / min at room temperature until breakage occurred was defined as the tensile strength, the stretched length was defined as the elongation rate, and the slope of the load against the initial deformation was defined as the tensile modulus.
[0222] [Table 8]
[0223] According to Table 8, the films produced using the polyester resins of the examples had transmittance of 88.12-89.25%, tensile modulus of 110-159 MPa, tensile strength of 16.1-60 MPa, and elongation of 361-830%. The polyester resins of the examples can be controlled in transmittance, tensile modulus, tensile strength, and elongation by adjusting the types and amounts of raw materials used during production.
[0224] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited thereto, and can be embodied in various modified forms within the scope of the claims, the detailed description of the invention, and the attached drawings, which of course also fall within the scope of the present invention.
Claims
1. A polyester resin comprising a copolymer of a monomer mixture containing a furandicarboxylic acid compound, an aliphatic diol compound and a lactone compound.
2. The polyester resin according to claim 1, wherein the furan dicarboxylic acid compound is represented by the following chemical formula 1: [Case 1] In the above Chemical Formula 1, L 1 and L 2 each independently represents a single bond or a substituted or unsubstituted alkylene having 1 to 10 carbon atoms.
3. The polyester resin according to claim 1, wherein the aliphatic diol compound is represented by the following chemical formula 2: [chemical 2] In the above Chemical Formula 2, L 3 and L 4 each independently represents a substituted or unsubstituted alkylene having 1 to 10 carbon atoms.
4. The lactone compound is represented by the following chemical formula 3: [C3] In the above Chemical Formula 3, L 5 is a substituted or unsubstituted alkylene having 1 to 10 carbon atoms.
5. The polyester resin according to claim 1, wherein the polyester resin has a number average molecular weight (Mn) of 50,000 to 200,000 g / mol.
6. The polyester resin according to claim 1, wherein the polyester resin has a molecular weight distribution (MWD) of 1.0 to 3.
0.
7. The polyester resin according to claim 1, wherein the polyester resin has an L* value of 93 or more, an a* value of 0 to 2, and a b* value of 7 or less according to the CIE 1976 L*a*b* color system.
8. The polyester resin has a change in intrinsic viscosity (ΔIV) according to the following formula 1: 12 2. The polyester resin according to claim 1, wherein the β- [Formula 1] △IV 12 = IV 1 -IV 2 In the above formula 1, IV 1 is the intrinsic viscosity at 25°C, and IV 2 is the intrinsic viscosity at 35°C.
9. The polyester resin according to claim 1, wherein the polyester resin has a glass transition temperature (Tg) of -60 to 10°C.
10. The polyester resin according to claim 1 , wherein the copolymer is a random copolymer or a block copolymer.
11. the block copolymer is a block copolymer of a first oligomer and a second oligomer; the first oligomer is a polymer of a furandicarboxylic acid compound and a first aliphatic diol compound; The polyester resin according to claim 10 , wherein the second oligomer comprises a polymer of a lactone compound and a second aliphatic diol compound.
12. the block copolymer is a block copolymer of a first oligomer and a monomer; the first oligomer is a polymer of a furandicarboxylic acid compound and a first aliphatic diol compound; The polyester resin according to claim 10, wherein the monomer is a lactone compound.
13. The polyester resin according to claim 11 or 12, wherein the molar ratio of the furandicarboxylic acid compound and the first aliphatic diol compound in the first oligomer is 5:1 to 1:
10.
14. The polyester resin according to claim 11, wherein the molar ratio of the lactone compound and the polymer of the second aliphatic diol compound in the second oligomer is 5:1 to 1:
10.
15. 12. The polyester resin of claim 11, wherein the molar ratio of the first oligomer to the second oligomer is from 10:1 to 1:
10.
16. The polyester resin according to claim 12, wherein the molar ratio of the first oligomer to the monomer is from 10:1 to 1:
10.
17. A method for producing a polyester resin, comprising copolymerizing a monomer mixture containing a furandicarboxylic acid compound, an aliphatic diol compound, and a lactone compound.
18. The step of copolymerizing the monomer mixture comprises: preparing a first oligomer by esterifying a furan dicarboxylic acid compound and a first aliphatic diol compound; preparing a second oligomer by esterifying the lactone compound and the second aliphatic diol compound; and subjecting the first oligomer and the second oligomer to an esterification reaction, a prepolymerization reaction, and a polycondensation reaction.
19. The step of copolymerizing the monomer mixture comprises: preparing a first oligomer by esterifying a furan dicarboxylic acid compound and an aliphatic diol compound; and subjecting the first oligomer and the lactone compound monomer to an esterification reaction, a prepolymerization reaction, and a polycondensation reaction.
20. The method for producing a polyester resin according to claim 18 or 19, wherein the production of the first oligomer is carried out in the presence of a titanium (Ti)-based catalyst containing a heat stabilizer.
21. The method for producing a polyester resin according to claim 18, wherein the second oligomer is produced in the presence of an antimony (Sb)-based catalyst.