Method and system for converting copper cyanide to copper oxide
The method of converting copper cyanide to copper oxide through acidic and alkaline reactions with separation steps addresses inefficiencies in existing processes, facilitating efficient copper oxide production and on-site processing with reduced costs and environmental impact.
Patent Information
- Application Number
- JP2024533225
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-03
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-08
AI Technical Summary
Existing methods for converting copper cyanide to copper oxide are inefficient and costly, particularly in slurry systems, and pose challenges due to the need for capital-intensive solid/liquid separation equipment and low copper concentrations in effluents, leading to increased operating costs and environmental risks.
A method involving contacting copper cyanide solution with an acidic solution to produce a copper cyanide slurry, followed by separation and then reacting the solid copper cyanide with sodium hydroxide to form copper oxide, utilizing a system with separation devices to manage solids and liquids effectively.
The process allows for the efficient conversion of copper cyanide to copper oxide, enabling easy transportation and on-site processing into copper cathodes, reducing environmental risks and operational costs while minimizing equipment requirements.
Smart Images

Figure 2024541682000001_ABST
Abstract
Description
[Technical Field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Application No. 63 / 285,532 (filed December 3, 2021), which is incorporated herein by reference.
[0002] Technical field of the invention The present disclosure relates to improved methods and systems for converting copper cyanide to copper oxide. [Background technology]
[0003] Leaching gold ore with cyanide is a well-established, robust, and cost-effective process. The presence of other minerals in gold ore complicates the process for the mine and makes leaching gold with cyanide less cost-effective. Most copper minerals have good solubility in cyanide solutions (Leaver & Woolf, 1931). When copper minerals are present in gold ore, they co-leach with the gold. This creates gold recovery problems and increases cyanide consumption. Copper cyanide can load activated carbon, which affects gold recovery. To address this issue, most operations simply increase the cyanide levels, resulting in increased operating costs.
[0004] Several studies have been conducted with the aim of developing cost-effective methods to minimize the impact of copper on gold recovery (Dai, Simon & Breuer, 2012). Several methods have explored recovering both copper and cyanide to improve economics. SART (sulfurization-acidification-recycle-enrichment) and AVR (acidification-volatilization-reneutralization) are two well-known and industrially applied processes (Botz & Acar, 2007 and Lopez-Pacheco, 2016). Using these processes, copper is recovered by precipitation, while cyanide is recovered by capturing hydrogen cyanide (HCN) gas during the acidification of copper-containing cyanide solutions.
[0005] The SART and AVR processes are effective for clear solutions. However, they are challenging for slurry systems such as carbon-in-leach (CIL) or carbon-in-pulp (CIP) because of the need for capital-intensive solid / liquid separation equipment. Furthermore, in most commercial operations, copper concentrations in the effluent are typically low, making the recovery process uneconomical.
[0006] Cyanide gold leaching is typically performed at pH 10.5-11. At these pH levels, the copper that co-elutes with gold is mostly present as a copper tricyanide complex, which has low adsorption efficiency on activated carbon. This low adsorption rate means that copper continues to build up in the circuit as the process water is recycled.
[0007] Many studies have addressed this issue, including Sceresini (1991), who patented a process utilizing low-cyanide pre-CIL to selectively recover copper on activated carbon prior to precious metal recovery. The copper-loaded carbon was then cold-stripped to produce a high-grade copper cyanide solution, which was subsequently acidified to produce a copper cyanide precipitate and HCN gas. The HCN gas was recovered and neutralized, while the copper cyanide was boiled with sulfuric acid to produce copper sulfate.
[0008] More recently, Dixon (2017) proposed a process to address the same problem by selectively removing copper from the circuit using continuous leaching of activated carbon. The copper-containing leachate is then sent to a Merrill Crowe circuit for precious metal recovery, after which copper is precipitated as copper cyanide (CuCN).
[0009] However, there is a need in the art for a more efficient and cost-effective process for converting copper cyanide to copper oxide. Summary of the Invention
[0010] The present invention provides a method for converting copper cyanide to copper oxide, comprising: contacting the copper cyanide solution with an acidic solution in a precipitation tank under reaction conditions sufficient to produce a copper cyanide slurry; removing the copper cyanide slurry from the settling tank; Optionally, removing gaseous effluent produced in said settling tank; separating solid copper cyanide from the copper cyanide slurry in a first separation device; removing the solid copper cyanide from the first separation device; Optionally, removing a liquid effluent in said first separation device; contacting the solid copper cyanide with a sodium hydroxide solution in a production tank under reaction conditions sufficient to produce a copper oxide slurry; removing the copper oxide slurry from the production tank; separating solid copper oxide from the copper oxide slurry in a second separation device; Optionally, removing the solid copper oxide from the second separation device; and and optionally removing from the second separation device any residual sodium hydroxide that did not react during the process of contacting the solid copper cyanide with the sodium hydroxide solution in the production tank.
[0011] The present invention also provides a system for converting copper cyanide to copper oxide, comprising: 1. A settling tank for contacting a copper cyanide solution with an acidic solution to produce a copper cyanide slurry, comprising: Optionally, the settling tank has a first output port for discharging the copper cyanide slurry; a settling tank, optionally having a second output port for discharging gaseous effluent generated within the settling tank; a first separation device for receiving the copper cyanide slurry and separating solid copper cyanide from the copper cyanide slurry, the first separation device comprising: Optionally, the first separation device has a third output port for discharging the solid copper cyanide; a first separation device, optionally having a fourth output port for discharging liquid effluent generated within the first separation device; a production tank for receiving the solid copper cyanide and contacting the solid copper cyanide with a sodium hydroxide solution to produce a copper oxide slurry; a production tank, optionally having a fifth output port for discharging the copper oxide slurry; a second separation device for receiving the copper oxide slurry and separating solid copper oxide from the copper oxide slurry, Optionally, the second separation device has a sixth output port for discharging the solid copper oxide; and optionally, the second separation device having a seventh output port for releasing any residual sodium hydroxide that did not react during the process of converting the solid copper cyanide to the copper oxide slurry in the production tank.
[0012] The present invention allows for increased handling options as the recovered copper oxide can be a) easily transported to a smelter with minimal constraints (compared to transporting copper cyanide) and b) processed on-site to produce copper cathode. The process of the present invention can be easily adapted to most brownfield operations with minimal new equipment and reagents required.
[0013] Additionally, the present invention minimizes the risks associated with transporting copper cyanide, reduces environmental impact, and increases manufacturing efficiency by allowing copper cathode to be produced in the same plant where the extraction process is carried out. [Brief explanation of the drawings]
[0014] [Figure 1] 1 illustrates an exemplary system for carrying out the method for converting copper cyanide to copper oxide of the present invention. [Figure 2] The effect of the initial NaOH:CuCN ratio on the copper grade in the product is shown. [Figure 3] The effect of the initial NaOH:CuCN ratio on NaOH consumption is shown. [Figure 4] 1 shows the relationship between residual NaOH in the solid product and copper grade. [Figure 5] 1 shows the relationship between residual NaOH in the filtrate and copper grade. [Figure 6] The copper grade in the product is shown relative to the NaOH consumption rate. DETAILED DESCRIPTION OF THE INVENTION
[0015] The present invention provides a method for converting copper cyanide to copper oxide, comprising: contacting the copper cyanide solution with an acidic solution in a precipitation tank under reaction conditions sufficient to produce a copper cyanide slurry; removing the copper cyanide slurry from the settling tank; Optionally, removing gaseous effluent produced in said settling tank; separating solid copper cyanide from the copper cyanide slurry in a first separation device; removing the solid copper cyanide from the first separation device; Optionally, removing a liquid effluent in said first separation device; contacting the solid copper cyanide with a sodium hydroxide solution in a production tank under reaction conditions sufficient to produce a copper oxide slurry; removing the copper oxide slurry from the production tank; separating solid copper oxide from the copper oxide slurry in a second separation device; Optionally, removing the solid copper oxide from the second separation device; and and optionally removing from the second separation device any residual sodium hydroxide that did not react during the process of contacting the solid copper cyanide with the sodium hydroxide solution in the production tank.
[0016] The acidic solution may be selected from the group consisting of sulfuric acid, nitric acid, and hydrochloric acid.
[0017] The method of the present invention further includes receiving the copper cyanide solution in the precipitation tank from the elution vessel. The copper-containing activated carbon can be contacted with a solution of sodium hydroxide and sodium cyanide in the elution vessel to produce an eluate containing the copper cyanide solution. The copper-containing activated carbon can further contain gold and / or silver. The sodium hydroxide and sodium cyanide can have a pH in the range of about 11-12 and a temperature in the range of about 0-60°C. The sodium hydroxide and sodium cyanide solution in the elution vessel can be received from a recycle solution tank.
[0018] The method of the present invention may further include receiving the gaseous effluent produced in the settling tank in a gas scrubber. The gaseous effluent may be hydrogen cyanide gas. The hydrogen cyanide gas may be contacted with a sodium hydroxide solution in the gas scrubber to produce a sodium cyanide solution. The sodium cyanide solution may be removed from the gas scrubber.
[0019] The method of the present invention further optionally includes contacting the solid copper cyanide with water in a production tank. The solid copper cyanide can be contacted with sodium hydroxide solution in the production tank at ambient temperature, and optionally, air sparging can be performed in the production tank. The molar ratio of NaOH:CuCN in the production tank can range from 2 to 0.1 (e.g., 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2), preferably 0.84 or greater. The percent solids as CuCN can range from 5% to 50% (e.g., 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%). The dosage rate of NaOH in the production tank can be at least 0.265 kg (eg, at least 0.295 kg) NaOH per kg of copper.
[0020] The copper oxide slurry can contain copper(I) oxide and / or copper(II) oxide, and can recover 70% or more (e.g., 75%, 80%, 85%, 90%) of the copper in the copper oxide.
[0021] Any residual sodium hydroxide present in the second separation device can be recycled back to the recycle solution tank, gas scrubber, production tank, or any combination thereof.
[0022] The present invention also relates to systems for carrying out the methods of the present invention. For example, the present invention relates to a system for converting copper cyanide to copper oxide, comprising: 1. A settling tank for contacting a copper cyanide solution with an acidic solution to produce a copper cyanide slurry, comprising: Optionally, the settling tank has a first output port for discharging the copper cyanide slurry; a settling tank, optionally having a second output port for discharging gaseous effluent generated within the settling tank; a first separation device for receiving the copper cyanide slurry and separating solid copper cyanide from the copper cyanide slurry, the first separation device comprising: Optionally, the first separation device has a third output port for discharging the solid copper cyanide; a first separation device, optionally having a fourth output port for discharging liquid effluent generated within the first separation device; a production tank for receiving the solid copper cyanide and contacting the solid copper cyanide with a sodium hydroxide solution to produce a copper oxide slurry; a production tank, optionally having a fifth output port for discharging the copper oxide slurry; a second separation device for receiving the copper oxide slurry and separating solid copper oxide from the copper oxide slurry, Optionally, the second separation device has a sixth output port for discharging the solid copper oxide; and optionally, the second separation device having a seventh output port for releasing any residual sodium hydroxide that did not react during the process of converting the solid copper cyanide to the copper oxide slurry in the production tank.
[0023] The acidic solution may be selected from the group consisting of sulfuric acid, nitric acid, and hydrochloric acid.
[0024] The precipitation tank can include a first input port for receiving a copper cyanide solution and a second input port for receiving an acidic solution. The first input port for receiving the copper cyanide solution can be connected to an elution vessel. The elution vessel can include a solid input port for receiving the copper-containing activated carbon and a liquid input port for receiving a sodium hydroxide and sodium cyanide solution. The copper-containing activated carbon can further include gold and / or silver. The copper-containing activated carbon can be contacted with a sodium hydroxide and sodium cyanide solution to produce an eluate comprising a copper cyanide solution. The sodium hydroxide and sodium cyanide solution can have a pH in the range of about 11-12 and a temperature in the range of about 0-60°C.
[0025] As used herein, the term "port" means any opening for the introduction or release of solids and / or fluids.
[0026] The liquid input port for receiving the sodium hydroxide and sodium cyanide solution may be connected to a recycle solution tank containing the sodium hydroxide and sodium cyanide solution.
[0027] The second output port of the settling tank can be connected to a gas scrubber for receiving the gaseous effluent produced in the settling tank. The gaseous effluent can be hydrogen cyanide gas. The hydrogen cyanide gas can be contacted with a sodium hydroxide solution in the gas scrubber to produce a sodium cyanide solution. The gas scrubber can include a liquid input port for receiving the sodium hydroxide solution and a liquid output port for removing the sodium cyanide solution.
[0028] The production tank for receiving the solid copper cyanide can include a first liquid input port for receiving sodium hydroxide solution and, optionally, a second liquid input port for receiving water. The solid copper cyanide can be contacted with the sodium hydroxide solution in the production tank at ambient temperature, and optionally, air sparged in the production tank. The molar ratio of NaOH:CuCN in the production tank ranges from 2 to 0.1 (e.g., 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2), preferably 0.84 or greater. The percent solids as CuCN ranges from 5% to 50% (e.g., 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%). The dosage of NaOH in the production tank is at least 0.265 kg (e.g., at least 0.295 kg) NaOH per kg of copper.
[0029] The copper oxide slurry can contain copper(I) oxide and / or copper(II) oxide, and can recover 70% or more (e.g., 75%, 80%, 85%, 90%) of the copper in the copper oxide.
[0030] Any residual sodium hydroxide present in the second separation device can be recycled back to the recycle solution tank, gas scrubber, production tank, or any combination thereof.
[0031] Figure 1 is a schematic diagram of an exemplary system for carrying out a method for extracting CuO solids from CuCN produced during the leaching of gold from gold- and copper-loaded activated carbon. The activated carbon may contain other metals (e.g., silver) and materials other than or in addition to gold. Additionally, process equipment not central to the discussion has been omitted. Thus, one skilled in the art will understand that pumps, heat exchangers, and tanks not shown in Figure 1 may be required.
[0032] System 600 includes a recycle solution tank 601 , an elution vessel 603 , a CuCN precipitation tank 605 , a gas scrubber 607 , a first solid / liquid separation vessel 609 , a CuO production tank 611 , and a second solid / liquid separation vessel 613 .
[0033] Gold- and copper-bearing activated carbon produced from a conventional carbon adsorption process is loaded into elution vessel 603. Although not shown in FIG. 1 , as explained above, the activated carbon may contain other metals (e.g., silver) and / or materials other than or in addition to gold. A recycle tank 601 is connected to elution vessel 603. A sodium hydroxide and sodium cyanide solution (NaOH+NaCN) is injected into the bottom of elution vessel 603, and the NaOH+NaCN solution passes through the activated carbon present in elution vessel 603.
[0034] The NaOH+NaCN solution present in the elution vessel 603 may have a high pH (e.g., about 11-12) and may be heated before and / or after being introduced into the elution vessel. When the NaOH+NaCN solution contacts the activated carbon in the elution vessel, a copper cyanide solution is produced, especially at low temperatures (e.g., 0-60°C). The copper cyanide solution may be a copper cyanide complex solution. The copper cyanide complex solution may include, for example, dicyanide, tricyanide, and tetracyanide complexes, or combinations thereof.
[0035] The elution solution produced in elution vessel 603 containing the copper cyanide solution is added to CuCN precipitation tank 605. The elution solution can be added directly to CuCN precipitation tank 605, or the elution solution can be provided to a storage tank (not shown) and dynamically added to CuCN precipitation tank 605 from the storage tank.
[0036] In an exemplary embodiment, gold can be extracted from the elution solution before it is fed to the CuCN precipitation tank 605. That is, gold, in addition to copper cyanide complexes, can be contained in the elution solution from the elution vessel 603, particularly if the solution is in the temperature range of 100-120° C. or less. If gold is contained in the eluate stream fed from the elution vessel 103, a separate process can be implemented to divert the stream to capture the gold before the solution is added to the CuCN precipitation tank 605.
[0037] For example, although not shown, a switch can be provided between the outlet of the elution vessel 103 and the CuCN precipitation tank 605, and the switch can be associated with whether gold is extracted or separated from the stream output from the elution vessel 103.
[0038] In the CuCN precipitation tank 605, an acidic solution is added to the elution solution and the mixed solution is stirred using a stirrer or mixer 606. The acidic solution can be any acid (e.g., sulfuric acid, nitric acid, or hydrochloric acid) that has the desired pH level. In an exemplary embodiment, the pH of the acidic solution is between 2 and 3 to achieve maximum CuCN precipitation without using too much acidic solution.
[0039] The CuCN precipitation tank 605 may include a gas extraction system for extracting hydrogen cyanide (HCN) gas produced in the CuCN precipitation tank 605 to a gas scrubber 607. That is, the eluate solution enters the CuCN precipitation tank 605 at a high pH, and an acidic solution is added to lower the pH. As the pH drops in the CuCN precipitation tank 605, HCN gas is produced.
[0040] After the HCN gas is extracted into the gas scrubber 607, a NaOH solution can be added to the extracted HCN gas in the gas scrubber 607 to create a NaCN solution. This NaCN solution can be reused or recycled in various processes.
[0041] The solution remaining in CuCN precipitation tank 605 after the HCN gas has been extracted is a slurry. This slurry is then output from CuCN precipitation tank 605 to first solid / liquid separation tank 609. For example, first solid / liquid separation tank 609 can be a filter that filters CuCN solids from the remaining solution. The solids can be input to CuO production tank 611, and the remaining solution, which has a lower pH, can be removed from first solid / liquid separation tank 609 and recycled throughout the process. This solution can have a lower pH and can be returned to CuCN precipitation tank 605. The amount of solution used in CuCN precipitation tank 605 can be less than the main process solution, allowing the acidic solution to be easily neutralized and recycled back into the process.
[0042] After the CuCN solids are introduced into CuO production tank 611, water and NaOH are added to CuO production tank 611. That is, the CuO can be repulped with water and the solution can be agitated using an agitator or mixer 612. NaOH is then added to CuO production tank 611 and the resulting solution is agitated for about 1 hour.
[0043] The solution output from CuO production tank 611 is then input to a second solid / liquid separation tank 613 to filter out the CuO solids from the solution. The filtered solution can be recycled to recycle solution tank 601, gas scrubber 607, CuO production tank 611, or any other process using a similar solution to reuse the solution. [Example]
[0044] Example
[0045] The conversion of cuprous cyanide (CuCN) to copper oxide was investigated by varying the percent solids as CuCN and the molar ratio of sodium hydroxide (NaOH):CuCN at ambient temperature. Analytical grade copper cyanide and sodium hydroxide were used, and a reaction time of 1 hour was used. The temperature, pH, and oxidation-reduction potential (ORP) of the slurry after the addition of NaOH were monitored. A total of 11 tests were conducted at ambient temperature. The slurry from each test was filtered at the end of the reaction. The filtrate was assayed for copper, total cyanide, weak acid dissociable (WAD) cyanide, alkalinity (as grams of sodium hydroxide per liter), and pH. The filtered solid was assayed for copper. The parameters investigated are summarized in Table 1. [Table 1]
[0046] The focus of the work was to define the optimum and highest percent solids and concentration of copper in solution. CuCN was converted to various copper oxides based on: [ka]
[0047] Results and Discussion
[0048] Table 2 compares the copper recovery and copper grade in the converted products. The converted products ranged in color from black to brownish black to greenish yellow, indicating the presence of various copper compounds. The copper grade in the products ranged from 78 to 89%, confirming the presence of several copper compounds. The theoretical grade of copper contained in cupric oxide (CuO) is 79.9%, and the theoretical grade of copper contained in cuprous oxide (Cu2O) is 88.8%. [Table 2]
[0049] The highest copper grade of 89.4% was achieved at 20% solids and an initial NaOH:CuCN molar ratio of 0.84. The corresponding copper recovery in the product was 76%. This indicates that the initial CuCN is converted to CuO at molar ratios of 0.84 and above. The highest recovery of 81% was achieved at 30% solids. A molar ratio of 0.75 yielded a much higher copper grade in the product than a ratio of 0.56. The only drawback observed at 30% solids and a molar ratio of 0.75 was that the slurry was too viscous, resulting in insufficient stirring.
[0050] Figure 2 shows the effect of the initial NaOH:CuCN molar ratio on the copper grade in the product. Molar ratios below 0.84 yielded an average copper grade of approximately 80%, while molar ratios above 0.84 yielded copper grades approaching 88%. This implies that lower molar ratios produce CuO, while higher molar ratios produce CuO.
[0051] As shown in Figure 3, the initial NaOH:CuCN molar ratio also affected the amount of NaOH consumed. Higher molar ratios consumed less NaOH. At molar ratios greater than 0.84, less than 50% of the NaOH was consumed. The molar ratios that produced the highest copper grades also consumed less NaOH during the process. Any remaining NaOH not consumed during the reaction can be recycled back into the CuCN conversion circuit or leaching circuit.
[0052] To confirm the back-calculation assay with the solution assay, the filtered solids were subjected to XRD. See Table 3. XRD showed that Run 4, which had the highest Cu grade, also had the highest CuO at 76%. The highest CuO was achieved with the heating and air sparging conditions, with a CuO grade of 78%. However, heating and air sparging only improved conversion by 2%. This 2% increase may not be economically beneficial compared to the no-heat option. [Table 3]
[0053] To further understand the residual NaOH and copper grade in grams per liter (gpl) in the solids, a 20% solids condition was used. Figure 4 shows the variation in grams per liter residual NaOH and solid copper grade. 20 gpl of residual NaOH is required for the production of CuO. As shown in Figure 5, the percent copper in the filtrate was found to be independent of residual NaOH. Approximately 25% of the copper in the feed was recovered in the filtrate in all test conditions.
[0054] Figure 6 shows the relationship between NaOH consumption (kg NaOH per kg copper in the feed) and copper grade in the product. A copper product of over 88% Cu (cuprous oxide) can be produced by consuming 0.295 kilograms of sodium hydroxide per kilogram of copper in the feed. This corresponds to 21 grams per liter (gpl) of NaOH at 10% solids.
[0055] The lower the % solids, the lower the NaOH consumption at molar ratios of NaOH:CuCN above 0.6. Therefore, a trade-off must be made between capital and operating costs. A higher % solids optimizes capital costs, while a lower % solids optimizes operating costs. Consuming 0.265 kg of NaOH per kg of copper in the feed results in a product (cupric oxide) containing approximately 80% copper. Lower grade copper oxide can be produced to optimize both recovery and operating costs.
[0056] conclusion
[0057] The conversion of CuCN to CuO can be achieved with NaOH at ambient temperature. The following conclusions were drawn: • The highest copper grade in the solid product was achieved at NaOH:CuCN molar ratios above 0.84. Approximately 25% of the copper in the feed was recovered in the filtrate. • The highest level of copper recovery was obtained at 30% solids, but the slurry was too viscous. The minimum required consumption rate was 0.265 kg NaOH per kg copper to produce cupric oxide. Cuprous oxide required a higher NaOH dosage rate of 0.295 kg NaOH per kg copper in the feed. • Lower percent solids optimizes operational costs due to less NaOH consumption, while higher percent solids optimizes capital costs. The higher the NaOH:CuCN molar ratio, the lower the NaOH consumption rate, which means that the filtrate can be recycled back to either the CuCN conversion circuit or the elution circuit.
[0058] The process of converting copper cyanide to cupric oxide provides more viable options for shipping and disposal, making the process advantageous from an economic and environmental standpoint.
[0059] Illustrative Embodiments
[0060] E1. A method for converting copper cyanide to copper oxide, comprising: contacting the copper cyanide solution with an acidic solution in a precipitation tank under reaction conditions sufficient to produce a copper cyanide slurry; removing the copper cyanide slurry from the settling tank; Optionally, removing gaseous effluent produced in said settling tank; separating solid copper cyanide from the copper cyanide slurry in a first separation device; removing the solid copper cyanide from the first separation device; Optionally, removing a liquid effluent in said first separation device; contacting the solid copper cyanide with a sodium hydroxide solution in a production tank under reaction conditions sufficient to produce a copper oxide slurry; removing the copper oxide slurry from the production tank; separating solid copper oxide from the copper oxide slurry in a second separation device; Optionally, removing the solid copper oxide from the second separation device; and and optionally removing from the second separation device any residual sodium hydroxide that did not react during the process of contacting the solid copper cyanide with the sodium hydroxide solution in the production tank.
[0061] E2. The method of E1, wherein said acidic solution is selected from the group consisting of sulfuric acid, nitric acid, and hydrochloric acid.
[0062] E3. The method of E1 or E2, further comprising receiving the copper cyanide solution in the precipitation tank from an elution vessel.
[0063] E4. The method of E3, further comprising contacting the copper-containing activated carbon with a solution of sodium hydroxide and sodium cyanide in said elution vessel to produce an eluate comprising said copper cyanide solution.
[0064] E5. The method of E4, wherein the copper-containing activated carbon further contains gold and / or silver.
[0065] E6. The method of E5, wherein the solution of sodium hydroxide and sodium cyanide has a pH in the range of about 11-12 and a temperature in the range of about 0-60°C.
[0066] E7. The method of any one of E3-E6, further comprising receiving the solution of sodium hydroxide and sodium cyanide in the elution vessel from a recycle solution tank.
[0067] E8. The method of any one of E1-E7, further comprising receiving the gaseous effluent produced in the settling tank in a gas scrubber.
[0068] E9. The method of E8, wherein the gaseous effluent is hydrogen cyanide gas.
[0069] E10. The method of E9, further comprising contacting the hydrogen cyanide gas with a sodium hydroxide solution in the gas scrubber to produce a sodium cyanide solution.
[0070] E11. The method of E10, further comprising removing the sodium cyanide solution from the gas scrubber.
[0071] E12. The method of any one of E1-E11, optionally further comprising contacting the solid copper cyanide with water in the production tank.
[0072] E13. The method of any one of E1-E12, wherein the solid copper cyanide is contacted with the sodium hydroxide solution in the production tank at ambient temperature.
[0073] E14. The method of any one of E1-E13, further comprising air sparging in the production tank.
[0074] E15. The method of any one of E1 to E14, wherein the molar ratio of NaOH:CuCN in the production tank is in the range of 2 to 0.1 (e.g., 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2), preferably 0.84 or greater.
[0075] E16. The method of any one of E1-E15, wherein the percent solids as CuCN is in the range of 5% to 50% (e.g., 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%).
[0076] E17. The method of any one of E1-E16, wherein the dosage rate of NaOH in the production tank is at least 0.295 kg NaOH per kg copper.
[0077] E18. The method of any one of E1-E17, wherein the dosage rate of NaOH in the production tank is at least 0.265 kg NaOH per kg copper.
[0078] E19. The method of any one of E1-E18, wherein the copper oxide slurry comprises copper(I) oxide and / or copper(II) oxide.
[0079] E20. The method of E19, wherein 70% or more (eg, 75%, 80%, 85%, 90%) of the copper is recovered in the copper oxide.
[0080] E21. The method of any one of E8-E20, further comprising recycling any residual sodium hydroxide present in the second separation device back to the recycle solution tank, the gas scrubber, the production tank, or any combination thereof.
[0081] E22. A system for converting copper cyanide to copper oxide, comprising: 1. A settling tank for contacting a copper cyanide solution with an acidic solution to produce a copper cyanide slurry, comprising: Optionally, the settling tank has a first output port for discharging the copper cyanide slurry; Optionally, the settling tank has a second output port for discharging gaseous effluent generated within the settling tank; a first separation device for receiving the copper cyanide slurry and separating solid copper cyanide from the copper cyanide slurry, the first separation device comprising: Optionally, the first separation device has a third output port for discharging the solid copper cyanide; a first separation device, optionally having a fourth output port for discharging liquid effluent generated within the first separation device; a production tank for receiving the solid copper cyanide and contacting the solid copper cyanide with a sodium hydroxide solution to produce a copper oxide slurry; Optionally, the production tank has a fifth output port for discharging the copper oxide slurry; and a second separation device for receiving the copper oxide slurry and separating solid copper oxide from the copper oxide slurry, Optionally, the second separation device has a sixth output port for discharging the solid copper oxide; and optionally, the second separation device having a seventh output port for discharging any residual sodium hydroxide that did not react during the process of converting the solid copper cyanide to the copper oxide slurry in the production tank.
[0082] E23. The system of E22, wherein the settling tank has a first input port for receiving the copper cyanide solution and a second input port for receiving the acid solution.
[0083] E24. The system of E22 or E23, wherein the acidic solution is selected from the group consisting of sulfuric acid, nitric acid, and hydrochloric acid.
[0084] E25. The system of any one of E22-E24, wherein the first input port for receiving the copper cyanide solution is connected to an elution vessel.
[0085] E26. The system of E25, wherein the elution vessel has a solids input port for receiving activated carbon containing copper and a liquid input port for receiving a solution of sodium hydroxide and sodium cyanide.
[0086] E27. The system of E26, wherein the copper-containing activated carbon further comprises gold and / or silver.
[0087] E28. The system of E27, wherein the copper-containing activated carbon is contacted with the sodium hydroxide and sodium cyanide solution to produce an effluent comprising the copper cyanide solution.
[0088] E29. The system of E28, wherein the sodium hydroxide and sodium cyanide solution has a pH in the range of about 11-12 and a temperature in the range of about 0-60°C.
[0089] E30. The system of any one of E22 to E29, wherein the liquid input port for receiving the sodium hydroxide and sodium cyanide solution is connected to a recycle solution tank containing the sodium hydroxide and sodium cyanide solution.
[0090] E31. The system of any one of E22 to E30, wherein the second output port of the settling tank is connected to a gas scrubber for receiving the gaseous effluent generated within the settling tank.
[0091] E32. The system of E31, wherein said gaseous effluent is hydrogen cyanide gas.
[0092] E33. The system of E32, wherein the hydrogen cyanide gas is contacted with sodium hydroxide solution in the gas scrubber to produce a sodium cyanide solution.
[0093] E34. The system of E33, wherein the gas scrubber has a liquid input port for receiving the sodium hydroxide solution and a liquid output port for removing the sodium cyanide solution.
[0094] E35. The system of any one of E22 to E34, wherein the production tank for receiving the solid copper cyanide has a first liquid input port for receiving the sodium hydroxide solution and, optionally, a second liquid input port for receiving water.
[0095] E36. The system of any one of E22 to E35, wherein the solid copper cyanide is contacted with the sodium hydroxide solution in the production tank at ambient temperature.
[0096] E37. The system of any one of E22 to E35, wherein the solid copper cyanide is contacted with the sodium hydroxide solution in the production tank at about 40-50°C.
[0097] E38. The system of any one of E22 to E37, further comprising air sparging in the production tank.
[0098] E39. The system of any one of E22 to E38, wherein the molar ratio of NaOH:CuCN in the production tank is in the range of 2 to 0.1 (e.g., 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2), preferably 0.84 or greater.
[0099] E40. The system of any one of E22 to E39, wherein the percent solids as CuCN is in the range of 5% to 50% (e.g., 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%).
[0100] E41. The system of any one of E22 to E40, wherein the dosage rate of NaOH in the production tank is at least 0.295 kg of NaOH per kg of copper.
[0101] E42. The system of any one of E22 to E40, wherein the dosage rate of NaOH in the production tank is at least 0.265 kg NaOH per kg copper.
[0102] E43. The system of any one of E22 to E42, wherein the copper oxide slurry comprises copper(I) oxide and / or copper(II) oxide.
[0103] E44. The system of E22-E43, wherein 70% or more (e.g., 75%, 80%, 85%, 90%) of the copper is recovered in the copper oxide.
[0104] E45. The system of any one of E31-E44, wherein any residual sodium hydroxide present in the second separation device is recycled back to the recycle solution tank, the gas scrubber, the production tank, or any combination thereof. References 1.Botz, M and Acar, S (2007), “Copper precipitation and cyanide recovery pilot testing for the Newmont Yanacocha project”. SME Annual Meeting, Denver, Colorado. 2.Dai, X, Simons, A and Breuer, P (2012), “A review of copper cyanide recovery techniques for the cyanidation of copper containing gold ores”. Minerals Engineering, Vol. 25, Issue 1, pp. 1-13 3.Dixon, S(2017), “Copper Prestrip to copper cyanide”, CIM Journal, Vol 1, No. 1, pp. 19-24. 4.Leaver, ES, & Woolf, JA (1931). Copper and zinc in cyanidation sulphide-acid precipitation (Tech. Rep. No. 494). Washington, DC: USBM Technical Paper 494. 5.Lopez-Pancheco, A(2016), “Yanacocha's copper rush. SART plant optimization unlocks the future for the Newmont mine.” CIM Magazine, Vol.11, No.1, pp.34-35. 6.Sceresini,B(1991),“Development and application of a process for the recovery of copper and complexed cyanide from cyanidation slurries” in Proceedings of Randol Gold Forum,Cairns,Australia.
Claims
1. 1. A method for converting copper cyanide to copper oxide, comprising the steps of: contacting the copper cyanide solution with an acidic solution in a precipitation tank under reactive conditions sufficient to produce a copper cyanide slurry; removing the copper cyanide slurry from the settling tank; Optionally, removing gaseous effluent produced in said settling tank; separating solid copper cyanide from the copper cyanide slurry in a first separation device; removing the solid copper cyanide from the first separation device; Optionally, removing a liquid effluent in said first separation device; contacting the solid copper cyanide with a sodium hydroxide solution in a production tank under reaction conditions sufficient to produce a copper oxide slurry; removing the copper oxide slurry from the production tank; separating solid copper oxide from the copper oxide slurry in a second separation device; Optionally, removing the solid copper oxide from the second separation device; and and optionally removing from said second separation device any residual sodium hydroxide that did not react during said process of contacting said solid copper cyanide with said sodium hydroxide solution in said production tank.
2. 2. The method of claim 1, wherein the acid solution is selected from the group consisting of sulfuric acid, nitric acid, and hydrochloric acid.
3. 10. The method of claim 1, further comprising receiving the copper cyanide solution in the precipitation tank from a leaching vessel.
4. 4. The method of claim 3, further comprising contacting copper-containing activated carbon in said elution vessel with a solution of sodium hydroxide and sodium cyanide to produce an eluate comprising said copper cyanide solution.
5. The method of claim 4, wherein the copper-containing activated carbon further comprises gold and / or silver.
6. 6. The method of claim 5, wherein the sodium hydroxide and sodium cyanide solution has a pH in the range of about 11-12 and a temperature in the range of about 0-60°C.
7. 4. The method of claim 3, further comprising receiving the solution of sodium hydroxide and sodium cyanide in the elution vessel from a recycle solution tank.
8. 10. The method of claim 1, further comprising receiving the gaseous effluent produced in the settling tank in a gas scrubber.
9. 9. The method of claim 8, wherein the gaseous effluent is hydrogen cyanide gas.
10. 10. The method of claim 9, further comprising contacting the hydrogen cyanide gas in the gas scrubber with a sodium hydroxide solution to produce a sodium cyanide solution.
11. 11. The method of claim 10, further comprising removing the sodium cyanide solution from the gas scrubber.
12. 10. The method of claim 1, further comprising optionally contacting the solid copper cyanide with water in the production tank.
13. 2. The method of claim 1, wherein the solid copper cyanide is contacted with the sodium hydroxide solution in the production tank at ambient temperature.
14. 10. The method of claim 1, further comprising air sparging in the production tank.
15. 2. The method of claim 1, wherein the molar ratio of NaOH:CuCN in the production tank ranges from 2 to 0.
1.
16. 2. The method of claim 1, wherein the percent solids as CuCN ranges from 5% to 50%.
17. 2. The method of claim 1, wherein the dosage rate of NaOH in the production tank is at least 0.295 kg NaOH per kg copper.
18. 2. The method of claim 1, wherein the dosage rate of NaOH in the production tank is at least 0.265 kg NaOH per kg copper.
19. 2. The method of claim 1, wherein the copper oxide slurry comprises copper(I) oxide and / or copper(II) oxide.
20. 20. The method of claim 19, wherein 70% or more of the copper is recovered in the copper oxide.
21. 9. The method of claim 8, further comprising recycling any residual sodium hydroxide present in the second separation device back to the recycle solution tank, the gas scrubber, the production tank, or any combination thereof.
22. 1. A system for converting copper cyanide to copper oxide, comprising:
1. A settling tank for contacting a copper cyanide solution with an acidic solution to produce a copper cyanide slurry, comprising: Optionally, the settling tank has a first output port for discharging the copper cyanide slurry; Optionally, the settling tank has a second output port for discharging gaseous effluent generated within the settling tank; a first separation device for receiving the copper cyanide slurry and separating solid copper cyanide from the copper cyanide slurry, Optionally, the first separation device has a third output port for discharging the solid copper cyanide; Optionally, the first separation device has a fourth output port for discharging liquid effluent generated within the first separation device; a production tank for receiving the solid copper cyanide and contacting the solid copper cyanide with a sodium hydroxide solution to produce a copper oxide slurry; Optionally, the production tank has a fifth output port for discharging the copper oxide slurry; and a second separation device for receiving the copper oxide slurry and separating solid copper oxide from the copper oxide slurry, Optionally, the second separation device has a sixth output port for discharging the solid copper oxide; and optionally, said second separation device having a seventh output port for discharging any residual sodium hydroxide that did not react during the process of converting said solid copper cyanide to said copper oxide slurry in said production tank.
23. 23. The system of claim 22, wherein the settling tank has a first input port for receiving the copper cyanide solution and a second input port for receiving the acid solution.
24. 23. The system of claim 22, wherein the acid solution is selected from the group consisting of sulfuric acid, nitric acid, and hydrochloric acid.
25. 23. The system of claim 22, wherein the first input port for receiving the copper cyanide solution is connected to an elution vessel.
26. 26. The system of claim 25, wherein the elution vessel has a solids input port for receiving activated carbon containing copper and a liquid input port for receiving a solution of sodium hydroxide and sodium cyanide.
27. 27. The system of claim 26, wherein the copper-containing activated carbon further comprises gold and / or silver.
28. 28. The system of claim 27, wherein the copper-containing activated carbon is contacted with the sodium hydroxide and sodium cyanide solution to produce an eluate comprising the copper cyanide solution.
29. 30. The system of claim 28, wherein the sodium hydroxide and sodium cyanide solution has a pH in the range of about 11-12 and a temperature in the range of about 0-60°C.
30. 23. The system of claim 22, wherein the liquid input port for receiving the sodium hydroxide and sodium cyanide solution is connected to a recycle solution tank containing the sodium hydroxide and sodium cyanide solution.
31. 23. The system of claim 22, wherein the second output port of the settling tank is connected to a gas scrubber for receiving the gaseous effluent generated within the settling tank.
32. 32. The system of claim 31 , wherein the gaseous effluent is hydrogen cyanide gas.
33. 33. The system of claim 32, wherein the hydrogen cyanide gas is contacted with a sodium hydroxide solution in the gas scrubber to produce a sodium cyanide solution.
34. 34. The system of claim 33, wherein the gas scrubber has a liquid input port for receiving the sodium hydroxide solution and a liquid output port for removing the sodium cyanide solution.
35. 23. The system of claim 22, wherein the production tank for receiving the solid copper cyanide has a first liquid input port for receiving the sodium hydroxide solution and, optionally, a second liquid input port for receiving water.
36. 23. The system of claim 22, wherein the solid copper cyanide is contacted with the sodium hydroxide solution in the production tank at ambient temperature.
37. 23. The system of claim 22, further comprising air sparging in the production tank.
38. 23. The system of claim 22, wherein the molar ratio of NaOH:CuCN in the production tank is between 2 and 0.
1.
39. 23. The system of claim 22, wherein the percent solids as CuCN ranges from 5% to 50%.
40. 23. The system of claim 22, wherein the dosage rate of NaOH in the production tank is at least 0.295 kg NaOH per kg copper.
41. 23. The system of claim 22, wherein the dosage rate of NaOH in the production tank is at least 0.265 kg NaOH per kg copper.
42. 23. The system of claim 22, wherein the copper oxide slurry comprises copper(I) oxide and / or copper(II) oxide.
43. 23. The system of claim 22, wherein at least 70% of the copper is recovered in the copper oxide.
44. 32. The system of claim 31 , wherein any residual sodium hydroxide present in the second separation device is recycled back to the recycle solution tank, the gas scrubber, the production tank, or any combination thereof.