Porous flow restrictor and method of manufacture thereof

The dual-density disk design with a high-purity outer tube and porous core addresses insulation and flow control issues in semiconductor manufacturing, ensuring uniform gas flow and preventing contamination.

JP2024542397APending Publication Date: 2024-11-15MOTT CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024526728
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-22
Filing Date
2022-11-21
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing porous flow restrictors in semiconductor manufacturing lack sufficient electrical insulation, dielectric strength, and uniform gas flow control, leading to potential ionization and contamination issues.

Method used

A dual-density disk design comprising a dense outer tube with a porous core, where the outer tube is made of a high-purity metal oxide and the core is less dense, allowing for uniform gas flow and electrical insulation, with machined threads for enhanced performance.

Benefits of technology

The dual-density disk provides effective fluid regulation, maintains electrical insulation, prevents ionization, and ensures high purity, meeting semiconductor manufacturing standards by preventing contamination and ensuring uniform gas flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542397000001_ABST
    Figure 2024542397000001_ABST
Patent Text Reader

Abstract

Disclosed herein is a dual density disk comprising a dense outer tube comprising a metal oxide having a purity greater than 92% and a porous core comprising a metal oxide of a lower density than the density of the dense outer tube, the porous core having a metal oxide purity greater than 99%, and the dense outer tube having an inner tapered surface.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Patent Application No. 63 / 282,011, filed November 22, 2021, which is incorporated by reference herein in its entirety. [Background technology]

[0002] FIELD OF THE DISCLOSURE The present disclosure relates to porous flow restrictors and methods of making same. Summary of the Invention

[0003] Disclosed herein is a dual density disk comprising a dense outer tube comprising a metal oxide having a purity greater than 90% and a porous core comprising a metal oxide of a lower density than the density of the dense outer tube, the porous core having a metal oxide purity greater than 90%, and the dense outer tube having an internal threaded surface.

[0004] Disclosed herein is a method that includes disposing a slurry including a metal oxide powder and a pore former within a densified outer tube, heating the densified outer tube with the slurry disposed therein to a temperature of 300-600°C to activate the pore former, creating a porous core within the densified outer tube, sintering the densified outer tube with the porous core at a temperature of 800-2000°C in one or more steps, and machining threads on an inner surface of the densified outer tube, the threads being parallel to a longitudinal axis of the tube or inclined relative to the longitudinal axis of the tube.

[0005] Also disclosed herein is a method including disposing an alumina powder within a densified outer tube, the alumina powder containing no pore formers; sintering the densified outer tube with the alumina powder disposed therein to a temperature of 800-2000°C; creating a porous core within the densified outer tube, the porous core having a purity of greater than 99%; and machining threads on an inner surface of the densified outer tube, the threads being parallel to a longitudinal axis of the tube or inclined relative to the longitudinal axis of the tube.

[0006] Also disclosed herein is a dual density disk comprising a high density outer tube comprising a first ceramic having a purity greater than 96% and a porous core comprising a second ceramic having a lower density than the density of the high density outer tube, the porous core having a purity greater than 99%, the high density outer tube comprising threads on an inner surface of the high density outer tube, the threads being parallel to the longitudinal axis of the tube or inclined relative to the longitudinal axis of the tube. [Brief description of the drawings]

[0007] [Figure 1A] FIG. 2 is an exemplary schematic diagram of one embodiment of a dense outer tube having a porous metal oxide interior. [Figure 1B] 4 is an exemplary schematic diagram of another embodiment of a dense outer tube having a porous metal oxide interior. FIG. [Figure 1C] 4 is an exemplary schematic diagram of another embodiment of a dense outer tube having a porous metal oxide interior. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Disclosed herein is a porous flow restrictor comprising a ceramic plug having a porous interior. The porous interior regulates fluid flow while maintaining sufficient electrical insulation and dielectric strength and prevents ionization of said fluid when exposed to a high electrical potential over the length of the restrictor. In one embodiment, the porous interior contains grooves or threads along the interface between the porous interior and the solid shell. In another embodiment, the inner porous comprises a taper as illustrated in the accompanying drawings. The taper contains threads on its surface. The ceramic plug is a dual density disk comprising a dense outer tube comprising a metal oxide having a purity of greater than 90%, preferably greater than 92%, preferably greater than 96%, and a porous core comprising a metal oxide of lower density than the density of the dense outer tube, the porous core having a metal oxide purity of greater than 90%, preferably greater than 92%, more preferably greater than 99%. In one embodiment, the metal oxide is alumina. The alumina dense outer tube has a purity of greater than 92%, preferably greater than 96%, while the porous alumina core has a purity of greater than 99%.

[0009] Also disclosed herein is a method comprising disposing a slurry comprising a metal oxide, a powder and a pore former in a densified outer tube, heating the densified outer tube with the slurry disposed therein to a temperature of 100-600°C to activate the pore former, creating a porous core in the densified outer tube, and sintering the densified outer tube with the porous core at a temperature of 800-2000°C in one or more stages. The threads may be machined in the densified outer tube before or after disposing the powder in the densified outer tube. In a preferred embodiment, the threads are machined after the densified outer shell is manufactured and before disposing the powder in the densified outer shell.

[0010] In one embodiment, a method for manufacturing a metal oxide disk includes disposing a metal oxide powder within a dense outer tube. The powder is free of pore formers and / or solvents. The dense outer tube with the metal oxide powder disposed within is subjected to a temperature of 800-2000°C in one or more steps. This creates a porous core within the dense outer tube having a purity of greater than 99%. Both the porous core and the dense outer tube have a purity of greater than 99%.

[0011] Disclosed herein is a dual density disk comprising a dense outer tube comprising a first ceramic having a purity greater than 96% and a porous core comprising a second ceramic having a lower density than the density of the dense outer tube, the porous core having a metal oxide purity greater than 99%. In one embodiment, the first ceramic can be the same as the second ceramic. In another embodiment, the first ceramic can be different from the second ceramic.

[0012] 1A, 1B, and 1C illustrate a ceramic plug 100 including a dense outer tube 102 and a porous central region 104 surrounded by the dense outer tube 102. The outer surface of the porous central region 102 contacts the inner surface of the dense outer tube 102 at its periphery 103. Threads 106 are disposed on the inner surface of the dense outer tube 102. The threads may be parallel to the longitudinal axis AA' of the tube or may be inclined relative to the longitudinal axis of the tube. The threads are located at the inlet, the outlet, or both the inlet and the outlet of the tube.

[0013] FIG. 1A illustrates a ceramic plug 100 having a dense outer tube 102 and a porous central region 104, which contacts an inner surface 106 of the dense outer tube 102. The inner surface 106 (of the dense outer tube 102) has threads machined thereon. The threads may be machined on the entire inner surface for a length L as shown in FIG. 1A, or alternatively, may be machined on only the inner surface for a length L1. The length L1 represents the length of a sleeve 110. The sleeve 110 is integral with the remainder of the ceramic plug 100, offering better alignment, reduced gaps, and improved overall performance. As can be seen, the ceramic plug 100 includes two opposing sleeves 110 at opposite ends of the plug.

[0014] 1B illustrates a tapered sleeve 112 disposed on the opposite side of the ceramic plug 100. The tapered sleeve 112 may or may not contain tapered threads machined on the inner surface 106 of the dense outer tube 102. The dense outer tube 102 in this case also contains a porous central region 104.

[0015] The porous central region may extend along the entire length L of the ceramic plug 100, or alternatively may extend the entire length L-2L1 from the first end of the sleeve 114 to the second end of the sleeve 116. The inlet or outlet diameter is larger than the diameter of the central region of the ceramic plug 100.

[0016] FIG. 1C illustrates a ceramic plug 100 with inlet and outlet ports having diameters smaller than the diameter of the central portion of the ceramic plug. Similar to FIGS. 1A and 1B, a dense outer tube 102 contains a porous central region 104 that contacts an inner surface 106 of the dense outer tube 102. The dense outer tube 102 has an inner diameter d1 that is larger than a diameter d2 at the inlet or outlet of the ceramic plug 100. In one embodiment, there is a step in diameter between the inlet diameter and the central region of the ceramic plug 100. In another embodiment, there is a step in diameter between the outlet diameter and the central region of the ceramic plug 100. The inlet and outlet of the ceramic plug have threads 106 optionally disposed on their respective inner surfaces.

[0017] The dense outer tube has high strength provided by a dense ceramic shell (hereinafter dense shell). The dense shell surrounds a majority of the porous ceramic core (hereinafter porous core), which allows uniform gas flow during manufacturing operations (such as operations for making semiconductor wafers). The dense ceramic shell has a high purity of more than 96%, which prevents contamination of semiconductor components during manufacturing operations to unfold the ceramic disk. The porous core contacts the dense ceramic shell on its inner surface, and the outer tube is in continuous contact with the porous core along the entire circumference of the porous core. In one embodiment, the porous core contains the same chemical composition as the dense shell, except that the core is porous, while the shell is dense. The density of the shell is greater than the density of the porous core.

[0018] In another embodiment, the porous core contains a ceramic having a chemical composition different from that of the dense shell. Disclosed herein is a dual density disk comprising a dense outer tube comprising a first ceramic having a purity greater than 96% and a porous core comprising a second ceramic having a density lower than that of the dense outer tube, the porous core having a metal oxide purity greater than 99%. In one embodiment, the first ceramic can be the same as the second ceramic. In another embodiment, the first ceramic can be different from the second ceramic.

[0019] The ceramics used in the disks include oxides, carbides, oxycarbides, nitrides, oxynitrides, borides, borocarbides, boronitrides, silicides, iodides, bromides, sulfides, selenides, tellurides, fluorides, or borosilicates of metals. Suitable metals are aluminum, titanium, zirconium, silicon, cerium, etc., or combinations thereof.

[0020] In one embodiment, the ceramic is preferably a metal oxide. Preferred metal oxides are titania, silica, alumina, zirconia, ceria, etc., or combinations thereof. The preferred metal oxide for use in the disk is alumina. The article and manufacturing method detailed below are directed to alumina disks, but are equally applicable to any of the ceramics listed above. The temperatures and atmospheres listed below for manufacturing alumina disks work equally well for any of the ceramics listed above, so there is no repeat listing of annealing temperatures, sintering temperatures, or atmospheres and pressures used to manufacture the ceramic disks.

[0021] Also disclosed herein is an alumina disk or rod (hereinafter referred to as a "disk") having a dual density, comprising a dense shell and a porous core (lower density than the shell) used to provide uniform gas flow for semiconductor manufacturing operations. The rod can be sliced ​​into several smaller slices called disks. The disk has high strength provided by the dense shell. The dense shell surrounds the majority of the porous core, which allows uniform gas flow during manufacturing operations (to make semiconductors). In addition, the disk contains alumina with a high purity of more than 96%, which prevents contamination of semiconductor components during manufacturing operations in which the alumina disk is deployed. The porous core contacts a dense outer tube (shell) on its inner surface, which is in continuous contact with the porous core along the entire circumference of the porous core. This core-shell dual density structure provides radial Hermitianity (i.e., prevents leakage from the sides of the porous body) and allows flow only through the longitudinal direction. Note that the outer shell is referred to herein as the "alumina shell," the "alumina tube," the "high density shell," and the "high density outer tube." Each disk has machined threads (as described above) on its opposing ends.

[0022] Also disclosed herein is a method for producing an alumina disk or rod. The method includes filling a dense alumina tube with an alumina slurry. The alumina slurry contains alumina powder (of high purity) and a pore former. The tube with the slurry contained therein is then fired to produce a porous core within the dense alumina tube. The alumina tube with the porous core may then undergo finishing operations such as slicing, lapping, grinding, etc. to produce an alumina disk. The alumina slurry may be in a dry form (without the presence of liquids such as solvents) or in a wet form.

[0023] The porous core is produced by filling the hollow center portion of an alumina tube with a metal oxide slurry or powder (e.g., alumina slurry or powder) and then heating the tube with the slurry or powder contained within to form a metal oxide (e.g., alumina) disk. The slurry contains a metal oxide powder (e.g., alumina powder) having high purity, an optional solvent, and a pore former, which are described in more detail below.

[0024] Porous cores can also be formed without the use of pore formers and solvents. A distribution of particle sizes can produce a porous core when sintered. Adjacent portions of the particles undergo necking as they bond together to form the porous core.

[0025] A metal oxide (e.g., alumina) powder having either a narrow or broad particle size distribution is formed into a slurry with a solvent and a pore former. The alumina powder may have a particle size of 10 nanometers to 500 micrometers, preferably 100 nanometers to 150 micrometers, more preferably 150 nanometers to 100 micrometers. The alumina powder may have a unimodal distribution of particle sizes, or alternatively, may have a bimodal or larger distribution of particle sizes.

[0026] The metal oxide (e.g., alumina) powder also has a purity of greater than 99%, preferably greater than 99.3%. The metal oxide (e.g., alumina) powder may be present in the slurry in an amount of 10-90% by weight, preferably 20-60% by weight, based on the total weight of the slurry.

[0027] The solvent is optional. The solvent used to form the slurry may include polar or non-polar solvents. The solvent may be protic or aprotic. A liquid aprotic polar solvent such as propylene carbonate, ethylene carbonate, butyrolactone, acetonitrile, benzonitrile, nitromethane, nitrobenzene, sulfolane, dimethylformamide, N-methylpyrrolidone, or a combination thereof is generally desirable. Polar protic solvents such as, but not limited to, water, methanol, acetonitrile, nitromethane, ethanol, propanol, isopropanol, butanol, or the like, or a combination thereof may be used. Other non-polar solvents such as benzene, toluene, carbon tetrachloride, hexane, diethyl ether, tetrahydrofuran, or the like, or a combination thereof may also be used. A suitable solvent is water, alcohol, or a combination thereof.

[0028] When present, the solvent may be used in an amount of 5 to 80% by weight, preferably 15 to 60% by weight, based on the total weight of the slurry.

[0029] The pore former is optional. The pore former may or may not be mixed into the slurry to facilitate the formation of a porous core in the metal oxide (e.g., alumina) tube. As mentioned above, the distribution of particle sizes may cause the porosity present in the core (when no solvent or pore former is used in the slurry). The pore former may be a gas, liquid, or solid. In one embodiment, the pore former is organic and may decompose and release gas when heated to high temperatures. Examples of such pore formers include solids such as AIBN (azobisisobutyronitrile), an organic compound with the formula [(CH3)2C(CN)]2N2. It is a white powder and is soluble in alcohol and common organic solvents.

[0030] In another embodiment, the pore former can be an organic polymer. The polymer is generally in powder form and mixed with a metal oxide (e.g., alumina) powder to form a mixture (or slurry, if a solvent is also used) and then placed in a metal oxide (e.g., alumina) tube. When the metal oxide (e.g., alumina) tube is heated to a temperature of 300-600° C., the polymer decomposes and facilitates the formation of pores in the metal oxide (e.g., alumina) powder.

[0031] The organic polymers used in the spaced features and / or surfaces may be selected from a wide variety of thermoplastic polymers, blends of thermoplastic polymers, thermosetting polymers, or blends of thermoplastic polymers with thermosetting polymers. The organic polymer may also be a polymer, copolymer, terpolymer, or blend of a combination comprising at least one of the organic polymers mentioned above. The organic polymer may also be an oligomer, homopolymer, copolymer, block copolymer, alternating block copolymer, random polymer, random copolymer, random block copolymer, graft copolymer, star block copolymer, dendrimer, polyelectrolyte (polymer with some repeating groups containing electrolyte), polyampholyte (polyelectrolyte with both cationic and anionic repeating groups), ionomer, etc., or a combination comprising at least one of the organic polymers mentioned above. The organic polymer has a number average molecular weight of more than 10,000 grams per mole, preferably more than 20,000 g / mole, more preferably more than 50,000 g / mole.

[0032] Exemplary organic polymers include polyacetals, polyacrylic acids, polycarbonates, poly(meth)acrylates, polyalkyds, polystyrenes, polyolefins, polyesters, polyamides, polyaramids, polyamideimides, polyarylates, polyurethanes, epoxies, phenols, silicones, polyarylsulfones, polyethersulfones, polyphenylene sulfides, polysulfones, polyimides, polyetherimides, polytetrafluoroethylenes, polyetherketones, polyetheretherketones, polyetherketoneketones, polybenzoxazoles, polyoxadiazoles, polybenzothiazinophenothiazines, polybenzothiazoles, polypyrazinoquinoxalines, polypyromellitimides, polyquinoxalines, polybenzimidazoles, polyoxazolidine ... Examples of the polysiloxane include sindol, polyoxoisoindoline, polydioxoisoindoline, polytriazine, polypyridazine, polypiperazine, polypyridine, polypiperidine, polytriazole, polypyrazole, polycarborane, polyoxabicyclononane, polydibenzofuran, polyphthalide, polyacetal, polyanhydride, polyvinyl ether, polyvinyl thioether, polyvinyl alcohol, polyvinyl ketone, polyvinyl halide, polyvinyl nitrile, polyvinyl ester, polysulfonate, polysulfide, polythioester, polysulfone, polysulfonamide, polyurea, polyphosphazene, polysilazane, polypropylene, polyethylene, polyethylene terephthalate, polyvinylidene fluoride, polysiloxane, and the like, or a combination thereof.

[0033] In another embodiment, the pore former may be a gas that is soluble in the metal oxide (e.g., alumina) powder or in the solvent used in the slurry. The gas may then phase separate from the slurry (due to binodal decomposition) (in response to pressure and / or temperature changes) to form a porous phase (which is the pores) in the slurry. Examples of such gases include carbon dioxide, argon, hydrogen, nitrogen, or combinations thereof.

[0034] In yet another embodiment, blowing agents such as chlorofluorocarbons, hydrochlorofluorocarbons (HCFCs), and / or hydrofluorocarbons (HFCs) may be used to form the pores. Chlorofluorocarbons (CFCs) are derived from methane and ethane, and these compounds have the formula CCl m F 4-m and C2Cl m F 6-m where m is not zero. Hydrochlorofluorocarbons (HCFCs) are also derived from methane and ethane and have the formula CCl m F n H 4-m-n and C2Cl x F y H 6-x-y where m, n, x, and y are not zero. Hydrofluorocarbons (HFCs) can also be derived from methane, ethane, propane, and butane, which compounds have the formula CF m H 4-m , C2F m H 6-m , C3F m H 8-m , and C4F m H 10-m where m is not zero.

[0035] The pore former may also be used in an amount of 5-50% by weight, preferably 10-25% by weight, based on the total weight of the slurry. Combinations of the above pore formers may also be used.

[0036] The slurry is prepared by mixing a metal oxide powder (e.g., alumina powder), an optional solvent, and a pore former. The slurry is then introduced into the hollow core of the metal oxide tube. The slurry may or may not be compressed.

[0037] The metal oxide (e.g., alumina) tube with the slurry contained therein is subjected to temperatures of 300 and 600° C. for periods of 10 minutes to 12 hours to form pores within the core of the metal oxide tube. This step facilitates activation of the pore former. The high temperature causes the pore former to decompose and release gases that facilitate pore formation within the core of the metal oxide (e.g., alumina) tube.

[0038] The metal oxide (e.g., alumina) tube with the porous metal oxide contained therein is then subjected to one or more sintering steps. In one embodiment, the first sintering step is carried out in air or a controlled atmosphere at a temperature between 800-1600°C. This first sintering step is optional and is carried out to enhance ease of handling (i.e., ensure that the porous core remains intact within the dense metal oxide shell). The first sintering step is carried out in a vacuum, atmospheric pressure, and / or a controlled pressure environment where the pressure is greater than atmospheric pressure, either in vacuum, air, oxygen, argon, nitrogen, natural gas, hydrogen, carbon dioxide, or a combination thereof.

[0039] The metal oxide tube with the porous core is then subjected to a second sintering step carried out at temperatures of 1500° C. and 2000° C. in either vacuum, air, oxygen, argon, nitrogen, natural gas, hydrogen, carbon dioxide, or combinations thereof to produce a metal oxide disk with a porous center that contains open cell pores that allow gas to flow through the metal oxide disk from one end to another.

[0040] In one embodiment, a method for manufacturing a metal oxide disk includes disposing a metal oxide powder within a dense outer tube. The powder is free of pore formers and / or solvents. The dense outer tube with the metal oxide powder disposed therein is sintered in one or more steps to a temperature of 800-2000°C. The two-step sintering process detailed above may also be used here. This creates a porous core within the dense outer tube. This creates a porous core within the dense outer tube with a purity of greater than 99%. Both the porous core and the dense outer tube have a porosity of greater than 99%.

[0041] In both of the sintering methods disclosed above, the porous core has a higher purity than the dense outer tube. This applies to all ceramic discs.

[0042] Here, the sintered metal oxide disk is a dual density part having a first higher density shell and a second lower density core. The part may or may not then be subjected to further finishing operations. The density of the metal oxide shell is greater than the density of the porous metal oxide core. In one embodiment, the finishing operation may involve slicing the disk into several smaller disks. In another embodiment, the metal oxide disk may have features such as edges, steps, or chamfers (or chamfers) that may be machined into the shell prior to the formation of the porosity (interior) or after the formation of the pores. The porous portion in the outer metal oxide shell may be made flush with the shell wall by machining, including milling. The outer diameter may be ground to meet the desired dimensions. The machining may be performed by using a water-soluble coolant to wash away any remaining impurities after machining and ensure high purity of the part.

[0043] Dual density metal oxide disks allow fluids to flow from one side to the other and can be used as flow controllers and filters made with various pore size distributions. High crush strength due to the dense metal oxide shell and high flow rate due to porosity within the shell (formed without compression) are key features of dual density parts. Pore size is greater than 0.5 micrometers and can be controlled for flow control and filtration applications. Strong bonds (via covalent and / or ionic bonds) between the porous metal oxide and the metal oxide tube (shell) are created during the sintering process.

[0044] The dual density metal oxide disks comply with the cleanliness standards set by the semiconductor industry. This is evidenced by low particle shedding under exposure to ultrasonic treatment in deionized water. When tested as detailed below, the crush strength of the dual density metal oxide disks can be greater than 20,000 pounds per square inch, and the crush strength of the porous portion can be greater than 2000 pounds per square inch. The crush strength and flow of gas within the pores depends on the initial particle size distribution of the metal oxide powder used, the amount (i.e., weight percent) of pore former in the blend, and the sintering conditions. In addition, the flow increases with increasing inner diameter and decreasing length of the metal oxide disk. The flow rate, crush strength (of the porous region within the dense shell), and density data of dual density disks obtained using different blend compositions are shown in Table 1 below. Table 1 contains exemplary data from the samples tested. The flow rate was determined at a gauge pressure of 30 pounds per square inch. [Table 1]

[0045] Table 1 shows the composition of the porous core material after sintering. The flow rate through the metal oxide disk can vary over a wide range depending on the application. It is seen that the nitrogen flow rate through the metal oxide disk varies from 5,000 to 30,000 standard cubic centimeters per minute, preferably from 10,000 to 22,000 standard cubic centimeters per minute. Within the metal oxide disk, the porous core has a bulk density of 1.00 to 2.50 g / cc, preferably 1.05 to 1.30 g / cc, preferably 1.08 to 1.27 g / cc, and a crush strength of 1800 to 2500 pounds per square inch. In one embodiment, the porous core has a bulk density of 1.00 to 1.30 g / cc, and a crush strength of more than 2000 pounds per square inch when present within a high density outer tube.

[0046] The porous core has a porosity of more than 30 volume percent, preferably more than 50 volume percent, preferably more than 70 volume percent, preferably more than 80 volume percent, more preferably more than 90 volume percent, based on the total volume of the core. The ceramic disk also exhibits radial Hermitianity, i.e., fluid does not leak out of the sides of the porous body as it is transported through the porous body. Thus, it allows flow only in the longitudinal direction (length L direction (see FIG. 1(A))).

[0047] After production of the porous core (and either before or after a finishing operation), threads may be machined into the opposing ends of the disk (eg, sleeve).

[0048] The disk, having the threads disposed on its inner surface, can then be used in an appropriate instrument.

[0049] Test Method Porous crushing strength test To access the crush strength of the porous core, a method was developed to apply force independently to the porous core alone, rather than to both the porous core and the dense shell. The method involves fixing the part in a device that allows a gauge pin, having a diameter equal to the diameter of the porous core, to rest perpendicular to the surface of the porous core. The opening in the fixture that accommodates the gauge pin is made 0.005 inches wider than the diameter of the gauge pin to minimize frictional forces. The part is fixed in the device such that the shell is pinned to the surface within the device and cannot be displaced, whereas the porous shell can be displaced when subjected to sufficient load.

[0050] To test crush strength, the part is placed in the apparatus and loaded into an MTS or Instron Compressive Strength Tester. The fixture is placed on a flat, fixed bottom plate. A gauge pin is loaded into the top of the fixture. A flat top plate is then set to displace downward at a rate of 0.001 in / sec, loading the gauge pin and then the part. Part failure is recorded by the machine and characterized manually / visually by two failure methods. The first failure method involves the porosity being pushed out of the shell. The second failure mode involves the porous material fracturing. Whatever failure mode occurs first, the load at this failure mode is converted to compressive strength.

[0051] Density Determination Test Shell: The outer diameter and length of the shell are sized through the use of a drop gauge. The inner diameter is measured through imaging and analysis. The mass is recorded through the use of an analytical balance. The density is recorded as the measured mass divided by the calculated volume.

[0052] Porous Core: Mass is measured before and after processing the porous. The difference between the measured mass of the shell only and the measured mass of the finished part (with shell and porous core) is converted to the mass of the porous core. The dimensions of the porous core are measured. A drop gauge measures the length of the porous core and optical imaging obtains the diameter. The density is obtained as the differential mass divided by the calculated volume.

[0053] Shell + Porous: The finished part is sized by drop gauge. Mass is recorded via analytical balance. Bulk part density is calculated as measured mass / calculated volume.

[0054] Although the present disclosure has been described with respect to some embodiments, those skilled in the art will recognize that various changes may be made and equivalents may be substituted for the elements thereof without departing from the scope of the present disclosure. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present disclosure. Therefore, the present disclosure is not limited to the particular embodiment disclosed as the best mode contemplated for carrying out the disclosure, but the present disclosure is intended to include all embodiments falling within the scope of the appended claims.

[0055] While particular embodiments have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are presently unforeseen or that may be unforeseen may occur to applicant or those skilled in the art. Accordingly, the appended claims, as filed and as they may be amended, are intended to embrace all such alternatives, modifications variations, improvements, and substantial equivalents.

[0056] All ranges disclosed herein are inclusive of the endpoints, and the endpoints are combinable independently of each other (e.g., the range "up to 25 wt.%, more specifically, 5 wt.% to 20 wt.%" includes the endpoints and all intermediate values ​​of the range "5 wt.% to 25 wt.%, etc.). "Combination" includes blends, mixtures, alloys, reaction products, and the like. Terms such as "first", "second", and the like do not denote any order, amount, or importance, but rather are used to distinguish one element from another. The terms "a", "an", and "the" do not denote any quantitative limitations and should be construed to cover both the singular and the plural unless otherwise indicated herein or clearly contradicted by context. "Or" means "and / or" unless expressly stated otherwise. References throughout this specification to "some embodiments", "an embodiment", and the like mean that the particular element described in connection with an embodiment is included in at least one embodiment described herein and may or may not be present in other embodiments. In addition, it is to be understood that the described elements may be combined in any suitable manner in the various embodiments. "Combinations thereof" are open-ended and include any combination including at least one of the recited components or features, optionally together with similar or equivalent components or features that are not recited.

[0057] Unless otherwise defined, technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs. All cited patents, patent applications, and other references are incorporated herein by reference in their entirety. However, if a term of this application contradicts or conflicts with a term of an incorporated reference, the term of this application shall take precedence over the conflicting term of the incorporated reference.

[0058] Unless otherwise specified herein, all test standards are the latest standards in effect as of the filing date of this application or, if priority is claimed, the filing date of the earliest priority application in which the test standards are listed.

[0059] Although the disc, assembly, and method of the present disclosure have been described with reference to exemplary embodiments thereof, the present disclosure is not limited to such exemplary embodiments and / or implementations. Rather, the disc, assembly, and method of the present disclosure embrace many embodiments and applications, as will be readily apparent to those skilled in the art from the disclosure herein. The present disclosure expressly encompasses such modifications, enhancements, and / or variations of the disclosed embodiments. Since many changes can be made to the above structures, and many widely different embodiments of the present disclosure can be made without departing from its scope, all matters contained in the drawings and specification should be interpreted as illustrative and not in a limiting sense. Additional modifications, changes, and substitutions are contemplated in the above disclosure. It is therefore appropriate that the appended claims be construed broadly and in a manner consistent with the scope of the present disclosure.

Claims

1. A dual density disc comprising: a dense outer tube comprising a metal oxide having a purity of greater than 92%; a porous core comprising a metal oxide of lower density than a density of the dense outer tube, the porous core having a metal oxide purity of greater than 99%, and the dense outer tube having an inner tapered surface.

2. 10. The dual density disk of claim 1, wherein said porous core has a bulk density of 1.00 to 3.0 g / cc and a crush strength of greater than 2000 pounds per square inch when present within said high density outer tube.

3. 2. The dual density disk of claim 1, wherein said porous core contacts said dense outer tube on its inner surface and said dense outer tube is in continuous contact with said porous core along the entire circumference of said porous core.

4. 10. The dual density disk of claim 1 having radial Hermitianity, which allows flow only in the longitudinal direction without leakage out the sides of the porous body.

5. 2. The dual density disk of claim 1, wherein the high density outer tube has an outer diameter of 1 to 75 millimeters and an inner diameter of 0.8 to 70 millimeters.

6. 2. The dual density disk of claim 1, wherein the high density outer tube has an initial length of 1 to 120 millimeters.

7. 10. The dual density disk of claim 1, wherein the porous core is made from a metal oxide powder having an initial purity of greater than 92%.

8. The dual density disk of claim 1 , wherein the porous core is made from a metal oxide powder having an initial purity of greater than 99%.

9. The dual density disk of claim 1 , wherein the porous core is made from a metal oxide powder having an initial purity of greater than 99.5%.

10. 2. The dual density disk of claim 1, wherein the metal oxide used in the dense outer tube is alumina.

11. 2. The dual density disk of claim 1, wherein the metal oxide used in the porous core is alumina.

12. 2. The dual density disk of claim 1, wherein an internal threaded surface is located at the inlet, the outlet, or both the inlet and the outlet of the tube.

13. 2. The dual density disk of claim 1, wherein the inlet, the outlet, or both the inlet and the outlet of the dual density disk have threads on the tapered surface.

14. 10. The dual density disk of claim 1, wherein the inlet, the outlet, or both the inlet and the outlet of the dual density disk have a diameter greater than a diameter of the porous core.

15. 10. The dual density disk of claim 1, wherein the inlet, the outlet, or both the inlet and the outlet of the dual density disk have a diameter smaller than a diameter of the porous core.

16. 1. A method comprising: In the high density outer tube, disposing a slurry comprising a metal oxide powder and a pore former; heating the dense outer tube with the slurry disposed therein to a temperature of 300-600° C. to activate the pore former; creating a porous core within said dense outer tube; sintering the dense outer tube with the porous core at a temperature of 800-2000° C. in one or more steps; and machining threads on an inner surface of the high density outer tube, the threads being parallel to a longitudinal axis of the tube or inclined relative to the longitudinal axis of the tube.

17. 17. The method of claim 16, wherein the sintering operation is carried out in air, nitrogen, natural gas, argon, hydrogen, or combinations thereof.

18. The method of claim 16 , wherein the pore-forming agent is an organic pore-forming agent.

19. The method of claim 16 , wherein the slurry further comprises a solvent.

20. The method of claim 16, wherein the sintering is preceded by a first sintering step in which the temperature is between 1200 and 1600°C.

21. 17. The method of claim 16, wherein the pore-forming agent is azobisisobutyronitrile.

22. The method of claim 16 , wherein the pore former is a gas that is soluble in the metal oxide slurry.

23. The method of claim 16 , wherein the pore former is a liquid.

24. The method of claim 16 , wherein the pore-forming agent is an organic polymer.

25. The organic polymer may be selected from the group consisting of polyacetal, polyacrylic acid, polycarbonate, poly(meth)acrylate, polyalkyd, polystyrene, polyolefin, polyester, polyamide, polyaramid, polyamideimide, polyarylate, polyurethane, epoxy, phenols, polyarylsulfone, polyethersulfone, polyphenylene sulfide, polyimide, polyetherimide, polytetrafluoroethylene, polyetherketone, polyetheretherketone, polyetherketone, polybenzoxazole, polyoxadiazole, polybenzothiazinophenothiazine, polybenzothiazole, polypyrazinoquinoxaline, polypyromellitimide, polyginoxaline, polybenzimidazole, polyoxadi ...

25. The method of claim 24, wherein the polyisoindoline is a sindol, a polyoxoisoindoline, a polydioxoisoindoline, a polytriazine, a polypyridazine, a polypiperazine, a polypyridine, a polypiperidine, a polytriazole, a polypyrazole, a polycarborane, a polyoxabicyclononane, a polydibenzofuran, a polyphthalide, a polyacetal, a polyanhydride, a polyvinyl ether, a polyvinyl thioether, a polyvinyl alcohol, a polyvinyl ketone, a polyvinyl halide, a polyvinyl nitrile, a polyvinyl ester, a polysulfonate, a polysulfide, a polythioester, a polysulfone, a polysulfonamide, a polyurea, a polyphosphazene, a polysilazan, a polyvinylidene fluoride, a polysiloxane, or a combination thereof.

26. 1. A method comprising: disposing an alumina powder within a dense outer tube, the alumina powder not including a pore former; sintering the dense outer tube with the alumina powder disposed therein at a temperature of 800-2000°C; creating a porous core within the dense outer tube, the porous core having a purity of greater than 99%; and machining threads on an inner surface of the high density outer tube, the threads being parallel to a longitudinal axis of the tube or inclined relative to the longitudinal axis of the tube.

27. 27. The method of claim 26, further comprising heating the densified outer tube with the alumina powder disposed therein to a temperature of 1200-1600°C.

28. A dual density disc comprising: a dense outer tube comprising a first ceramic having a purity greater than 92%; a porous core comprising a second ceramic having a density lower than a density of the dense outer tube, the porous core having a purity greater than 99%; A dual density disk, wherein the high density outer tube comprises threads on an inner surface of the high density outer tube, the threads being parallel to the longitudinal axis of the tube or inclined relative to the longitudinal axis of the tube.

29. 30. The dual density disk of claim 28, wherein the first ceramic is the same as the second ceramic.

30. 30. The dual density disk of claim 28, wherein the first ceramic is different from the second ceramic.

Citation Information

Patent Citations

  • Connecting method, joint assembly, connector and pipe joint

    JP1984001894A

  • The tubular connecting part

    JP1985501172A

  • Ceramic porous sintered compact, component for semiconductor manufacturing apparatus and shower plate, and method of producing porous sintered compact

    JP2011011929A

  • Sintered fiber filter

    JP2013078764A

  • Ceramic discs and rods, methods of manufacture thereof and articles comprising the same

    WO2021108376A1