Polypropylene composite material having a melting point gradient structure, its preparation method and system and use thereof

A polypropylene composite with a melting point gradient structure addresses the limitations of existing materials by enhancing mechanical properties and delamination strength, achieving efficient production with reduced energy consumption and improved processing efficiency.

JP2024542407APending Publication Date: 2024-11-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024527163
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-08
Filing Date
2022-11-07
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing polypropylene composite materials face challenges in achieving a wider processing temperature range, stronger mechanical properties, and higher delamination strength simultaneously, with existing methods often resulting in reduced mechanical strength and inadequate delamination resistance.

Method used

A polypropylene composite material with a melting point gradient structure is designed, comprising a core layer and outer layers with varying melting points, allowing for a laminated structure that improves mechanical properties and delamination strength through a controlled melting point gradient.

Benefits of technology

The composite material exhibits enhanced tensile strength, impact resistance, and delamination strength while reducing energy consumption and operation time, with improved processing efficiency and lower hot press temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542407000004
    Figure 2024542407000004
  • Figure 2024542407000001
    Figure 2024542407000001
  • Figure 2024542407000002
    Figure 2024542407000002
Patent Text Reader

Abstract

The present invention relates to a polypropylene composite material having a melting point gradient structure, its preparation method, and its system and use. The composite material comprises a plurality of polypropylene sheet layer units that are laminated in sequence; each polypropylene sheet layer unit group comprises at least one identical or different polypropylene sheet layer unit, and the structure of each polypropylene sheet layer unit is B i A i B' i and the structure of the polypropylene composite material is ... group i, ... group 2, group 1, group 2, ... group i, ...; polypropylene composition A i The melting point of polypropylene composition B i and B' i the average melting point of all the outer layers in the i-th group is higher than the average melting point of all the outer layers in the (i-1)-th group. The polypropylene composite material having a melting point gradient structure of the present invention has very good tensile properties and very good impact resistance, and also has good interlayer peel strength at a relatively low heat press temperature.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polypropylene composite material, more particularly to a polypropylene composite material having a melting point gradient structure and a method for preparing the same, as well as a system and use thereof. [Background technology]

[0002] In recent years, easy-to-recycle, lightweight, high-strength, high-impact polymer composite materials, especially self-reinforced polymer composite materials, have become one of the research hot spots.

[0003] The reinforcement phase and matrix of self-reinforced polymer composites consist of the same type of polymer but with different morphology, and the reinforcement phase is usually highly oriented fibers or flat ribbons. Most self-reinforced polymer composites are prepared by heat pressing. When the reinforcement phase is heat pressed at a certain pressure and temperature, the fiber surfaces of the reinforcement phase melt into the matrix melt. The surfaces of the matrix melt and the reinforcement phase co-crystallize during melting, thus providing sufficient interfacial bond strength.

[0004] For example, in US8021592B2, melt-spun oriented polyolefin fibers with a weight average molecular weight of less than 250,000 are woven, then heat-pressed, and the surface layer of the polyolefin fabric is partially melt-bonded using a specific high temperature, high pressure, and cooling time to prepare a polyolefin sheet. This preparation method is sensitive to the heat-pressing temperature, and the required heat-pressing temperature is high. The oriented fibers in the composite polyolefin fibers prepared after heat-pressing cause relatively large orientation defects, resulting in a significant decrease in mechanical strength, and the self-reinforcement effect needs to be further improved.

[0005] In order to widen the window of heat pressing and reduce the heat pressing pressure, in US8133537B2, three layers of polyolefin fibers with different melting points are heat pressed to obtain a polyolefin composite, in which the melting points of the first and second layers of polyolefin are lower than that of the core layer, and it is noted that the viscosity of the second polymer is about 10% or less of the viscosity of the first polymer when measured at 170°C. However, the impact strength and interlayer peel strength of the heat pressed composite produced in this way are small, and it is impossible to obtain a heat pressed composite with both good mechanical properties and higher interlayer peel strength. Summary of the Invention

[0006] The purpose of the present invention is to overcome the technical problem that existing polypropylene composite materials have difficulty in simultaneously having a wider processing temperature, stronger mechanical properties and higher interlayer peel strength. The present invention provides a polypropylene composite material with a melting point gradient structure and its preparation method, as well as its system and use, through the design of the melting point gradient structure of laminated polypropylene. This preparation method can improve production efficiency and reduce production energy consumption while shortening the heat press operation time. The polypropylene composite material obtained by this method has excellent mechanical properties and good interlayer peel strength at the same time.

[0007] The first object of the present invention is to provide a polypropylene composite material, the material comprising a plurality of polypropylene sheet layer units laminated in sequence; each polypropylene sheet layer unit group comprises at least one identical or different polypropylene sheet layer unit, each polypropylene sheet layer unit comprising a core layer A; i , and core layer A i Outer layer B located on both sides of i and B' i Including B i A i B' iThe polypropylene composite material has a structure in which, from bottom to top, the nth group, ... the ith group, ... the 2nd group, the 1st group, the 2nd group, ... the ith group, ... the nth group, and the total number of the lamination groups of the polypropylene sheet layer unit group is 2n-1, where i and n are both integers of 2 or more, and i≦n; where, in the polypropylene sheet layer unit, the core layer A i Polypropylene composition A i and outer layer B i is the outer layer B' i Same or different, outer layer B i Polypropylene composition B i and an outer layer B' i Polypropylene composition B' i Polypropylene composition A i The melting point of polypropylene composition B i and polypropylene composition B' i the average melting point of all the outer layers of the i-th group is higher than the average melting point of all the outer layers of the i-1th group.

[0008] According to the present invention, in the structure of the polypropylene composite material, the upper group i can be the same as or different from the lower group i-1.

[0009] In a preferred embodiment of the present invention, the melting point of the polypropylene composition A is i and the melting point of polypropylene composition B i The difference between the melting point of polypropylene composition A and the melting point of polypropylene composition B is i and the melting point of polypropylene composition B' i The difference between these is 5°C or more, preferably 10°C or more, more preferably 20°C or more; more preferably 20 to 60°C.

[0010] According to the present invention, the core layers in each polypropylene sheet layer unit may be made of the same material or different materials, and the present invention is not particularly limited thereto. Polypropylene Composition A i The melting point of polypropylene composition B i , Polypropylene Composition B' iIf the melting point of the polyimide is higher than that of the polyimide, better technical effects can be obtained.

[0011] In a preferred embodiment of the present invention, the difference between the average melting point of all the outer layers of the i-th group and the average melting point of all the outer layers of the i-1-th group, whether the difference is the same or different, is 1 to 40° C., preferably 1 to 10° C., and more preferably 1 to 5° C. According to the present invention, the total number of laminations of the polypropylene sheet layer unit group is 2n-1, and the selection range of the total number of laminations of the polypropylene sheet layer unit group is wide. In a preferred embodiment of the present invention, it is preferably 2≦n≦100, more preferably 2≦n≦50, and further preferably 2≦n≦30.

[0012] According to the present invention, the number of polypropylene sheet layer units in each polypropylene sheet layer unit group can be selected from a wide range. In a preferred embodiment of the present invention, each polypropylene sheet layer unit group independently contains 1 to 10, preferably 1 to 5, more preferably 1 to 3 identical or different polypropylene sheet layer units, more preferably one polypropylene sheet layer unit. Preferably, the number of polypropylene sheet layer units in each polypropylene sheet layer unit group is the same.

[0013] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, and more preferably within ±1°C of the average melting point of all the outer layers in that group.

[0014] In an embodiment in which each polypropylene sheet layer unit group includes only one polypropylene sheet layer unit, for example, the structure of the polypropylene composite material is B from bottom to top. n A n B' n ......B i A i B' i ......B2A2B'2, B1A1B'1, B2A2B'2......B i A iB' i ......B n A n B' n The total number of lamination units of the polypropylene sheet layer unit is 2n-1, where i and n are both integers of 2 or more, and i≦n.

[0015] In an embodiment in which each polypropylene sheet layer unit group includes two or more polypropylene sheet layer units, for example from bottom to top, the structure of the polypropylene sheet layer unit group i is B i1 A i1 B' i1 , B i2 A i2 B' i2 ......B ip A ip B' ip , the structure of the polypropylene composite material is (B n1 A n1 B' n1 , B n2 A n2 B' n2 ......B nq A nq B' nq ).....(B i1 A i1 B' i1 , B ip A ip B' ip )......(B 21 A 21 B' 21 , B 22 A 22 B' 22 ......B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A 12 B' 12 ......B 1j A 1j B' 1j )(B 21 A 21 B' 21 , B 22 A 22 B' 22......B 2k A 2k B' 2k )......(B i1 A i1 B' i1 , B i2 A i2 B' i2 ......B ip A ip B' ip )......(B n1 A n1 B' n1 , B n2 A n2 B' n2 ......B nq A nq B' nq ), and the total number of lamination units of the polypropylene sheet layer unit is j+2k+......2p+......2q; j, k, p, and q are each independently an integer of 2 or more, preferably an integer of 2 to 10, more preferably an integer of 2 to 5, and even more preferably an integer of 2 to 3.

[0016] In a preferred embodiment of the present invention, the polypropylene sheet layer unit comprises an intermediate layer C i and C' i The polypropylene sheet layer unit structure is B i C i A i C' i B' i and the middle layer C i is the middle layer C' i Same or different from middle layer C i Polypropylene composition C i and an intermediate layer C' i Polypropylene composition C' i Polypropylene composition A i The melting point of polypropylene composition C i and polypropylene composition C' i higher than the melting point of

[0017] According to the present invention, the core layer A in each polypropylene sheet layer unit iThe thickness ratio of the core layer A in each polypropylene sheet layer unit can be selected within a wide range. i The thickness of the core layer A is 51% to 89%, preferably 71% to 89%, and more preferably 71% to 80% of the total thickness of each polypropylene sheet layer unit. i Outer layer B located on both sides of i and B' i The thicknesses of the core layer A and the core layer B may be the same or different, and are preferably the same. i The middle layer C located on both sides of i and C' i The thicknesses of may be the same or different, and are preferably the same.

[0018] The thickness of each polypropylene sheet layer unit can be selected within a wide range. In a preferred embodiment of the present invention, the thickness of each polypropylene sheet layer unit is 10 to 1000 μm, preferably 30 to 500 μm, and more preferably 50 to 300 μm.

[0019] According to the present invention, the core layer A i , outer layer B i , B' i , middle layer C i , C' i The thickness can be controlled by the melt pump of the extruder during processing.

[0020] According to the present invention, polypropylene composition A i Polypropylene Composition B includes, but is not limited to, one or more of polypropylene homopolymer, polypropylene random copolymer, and polypropylene impact copolymer; i , B' i are each one or more of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer, and optionally a thermal adhesion improver y i Polypropylene composition C, including, but not limited to i , C' iare each one or more of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer, and optionally a thermal adhesion improver z i Including, but not limited to:

[0021] According to the present invention, polypropylene composition A i can be selected within a wide range. In a preferred embodiment of the present invention, polypropylene composition A i includes one or more of polypropylene homopolymer, polypropylene random copolymer, and polypropylene impact copolymer.

[0022] According to the present invention, polypropylene composition B i and B' i each of which comprises one or more of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; preferably polypropylene composition B i and / or polypropylene composition B' i is a thermal adhesion improver y i Also contains

[0023] According to the present invention, polypropylene composition C i and C' i each of which comprises one or more of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; preferably polypropylene composition C i and / or polypropylene composition C' i is a thermal adhesion improver i Also contains

[0024] In a more preferred embodiment of the present invention, the polypropylene composition Ai comprises a polypropylene homopolymer a i , and polypropylene impact copolymer b i In an even more preferred embodiment of the present invention, the polypropylene composition A i Based on the total weight of polypropylene composition Ai is 50 to 99% by weight of polypropylene homopolymer a i , 1 to 50% by weight of polypropylene impact copolymer b i More preferably, the polypropylene composition A comprises i is 70-90% by weight of polypropylene homopolymer a i , 10 to 30% by weight of polypropylene impact copolymer b i Includes.

[0025] In a more preferred embodiment of the present invention, polypropylene composition B i , Polypropylene Composition B' i are polypropylene random copolymer x i , and thermal adhesion improver y i Preferably, polypropylene composition B i , Polypropylene Composition B' i Polypropylene composition B based on the total weight of each of i , Polypropylene Composition B' i are 70 to 99% by weight of polypropylene random copolymer x i , 1 to 30% by weight of a thermal adhesion improver y i Preferably, polypropylene composition B i is 80-90% by weight of polypropylene random copolymer x i , 10 to 20% by weight of a thermal adhesion improver y i Includes.

[0026] In a more preferred embodiment of the present invention, polypropylene composition C i , Polypropylene composition C' i are polypropylene random copolymer β i and polypropylene homopolymer gamma i and thermal adhesion improver z i Preferably, the polypropylene composition C i , Polypropylene composition C' i Based on the total weight of each of the polypropylene composition C i , Polypropylene composition C'i are 30 to 60% by weight of thermal adhesion improver z i , 35 to 55% by weight of polypropylene random copolymer β i and 5 to 15% by weight of polypropylene homopolymer γ i More preferably, the polypropylene composition C i , Polypropylene composition C' i are 35 to 55% by weight of thermal adhesion improver z i , 40 to 55% by weight of polypropylene random copolymer β i and 5 to 10% by weight of polypropylene homopolymer γ i Includes.

[0027] According to the present invention, polypropylene homopolymer a i can be selected within a wide range. In a preferred embodiment of the present invention, the polypropylene homopolymer a i has a melting point of 150 to 170° C., preferably 160 to 170° C.; and / or an isotacticity (mm) of 96% or less, preferably 97% or less, more preferably 98% or less.

[0028] According to the present invention, polypropylene homopolymer a i The melt flow rate of the polypropylene homopolymer a can be selected within a wide range, and is preferably i has a melt flow rate at 230° C. under a load of 2.16 kg of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, and more preferably 2.5 to 18 g / 10 min.

[0029] According to the present invention, "and / or" refers to either a single condition or to a combination of two conditions.

[0030] According to the present invention, polypropylene impact copolymer b i can be selected within a wide range. In a preferred embodiment of the present invention, the polypropylene impact copolymer b ihas a melting point of 150-170°C, the monomer copolymerized with propylene in the polypropylene impact copolymer is ethylene or butene, preferably butene; and / or the polypropylene impact copolymer has a melting point of 20 KJ / m 2 (23°C) or higher Izod impact strength.

[0031] According to the present invention, polypropylene impact copolymer b i The melt flow rate of the polypropylene impact copolymer b can be selected within a wide range, and is preferably i has a melt flow rate at 230° C. under a load of 2.16 kg of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, and more preferably 2.5 to 18 g / 10 min.

[0032] Through research conducted by the present inventors, polypropylene composition A i When the melt mass flow rate and polymer composition ratio of the raw materials used in are within the preferred range, the polypropylene impact copolymer b in the composition i It was found that the sheet has good impact performance because it can better absorb impact energy and meet the requirements for impact performance. At the same time, polypropylene homopolymer a i Since the polymer segments are relatively regular, crystallization occurs during preparation of the sheets, and the sheets also have good tensile properties.

[0033] In a preferred embodiment of the present invention, polypropylene composition A i also includes a β-nucleating agent; preferably the β-nucleating agent is selected from at least one of polycyclic aromatic hydrocarbons, Group IIA binary complexes, aromatic diamides, rare earth compounds, and cyclic dicarboxylate nucleating agents.

[0034] According to the invention, the amount of β-nucleating agent can be chosen within wide limits, preferably polypropylene composition A i The content of the β-nucleating agent in the polypropylene composition A is iThe content of the β-nucleating agent is 0.01 to 0.5 parts by weight based on 100 parts by weight of the total amount. Specifically, for example, the content of the β-nucleating agent can be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5 parts by weight.

[0035] In a preferred embodiment of the present invention, the polypropylene random copolymer x i has a melting point of 110 to 150°C, preferably 120 to 140°C, preferably the average melting point of all polypropylene random copolymers in group i is higher than the average melting point of all polypropylene random copolymers in group i-1, preferably the difference in melting point therebetween is 1 to 40°C, more preferably 1 to 10°C, most preferably 1 to 5°C; preferably polypropylene random copolymer x i are copolymers of propylene with ethylene and / or butene, preferably ethylene-propylene-butene terpolymers and / or propylene-ethylene bipolymers.

[0036] According to the present invention, polypropylene random copolymer x i The melt flow rate of the polypropylene random copolymer x can be selected from a wide range, and the melt flow rate at 230° C. and a load of 2.16 kg is preferably 0.5 to 50 g / 10 min, more preferably 1 to 20 g / 10 min, and more preferably 3 to 18 g / 10 min. i has a molecular weight distribution Mw / Mn of 5-12, preferably 7-10.

[0037] In a preferred embodiment of the present invention, the thermal adhesion improver y i has a melting point or viscous flow temperature of 70 to 110°C. And / or, the thermal adhesion improver y i is selected from one or more of polyolefin elastomer, ethylene-propylene-diene-terpolymer rubber, SEBS, SBS, EVA, and petroleum resin, and is preferably a thermal adhesion improver y i is a polyolefin elastomer and / or a petroleum resin.

[0038] In a preferred embodiment of the present invention, the polyolefin elastomer is preferably an elastomer of ethylene copolymerized with propylene and / or an α-olefin, the α-olefin being preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin having a softening point of 100-150°C; preferably a cyclopentadiene type resin.

[0039] According to the present invention, the thermal adhesion improver y i The melt flow rate of the thermal adhesion improver y can be selected within a wide range. i has a melt flow rate at 190° C. under a load of 2.16 kg of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 1 to 18 g / 10 min, and further preferably 3 to 18 g / 10 min.

[0040] Through research conducted by the present inventors, polypropylene composition B i and polypropylene composition B' i When the composition ratio of each of the polymers is within the above preferred range, the low melting point polypropylene random copolymer x in the composition i and thermal adhesion improver y i It has been found that the heat pressing temperature can be significantly reduced and the heat pressing temperature window can be widened. In addition, the heat adhesion improver y i provides good adhesion to the sheets and further improves the interlayer peel strength.

[0041] Through research conducted by the present inventors, polypropylene composition A i and polypropylene composition B i and polypropylene composition B' i The polymer composition ratios of each of the polymer compositions A and B, and polymer composition A iIt has been found that when the thickness distribution is within the above preferred range, the sheet preparation process can be made even smoother, and the sheet uniformity, tensile strength, impact properties, and interlayer peel strength can be made even better.

[0042] According to the present invention, the polypropylene sheet layer unit is B i C i A i C' i B' i In the case of the sheet structure, the thickness ratio of each layer can be selected within a wide range. i The thickness of the intermediate layer C is 51% to 89%, preferably 71% to 89%, of the total thickness of the polypropylene sheet layer unit. i , C' i The thickness of the outer layer B is 6% to 20%, preferably 6% to 15% of the total thickness. i , B' i The thickness of the second insulating layer occupies 5% to 30%, preferably 5% to 15%, of the total thickness.

[0043] According to the present invention, the polypropylene random copolymer β i can be selected within a wide range. In a preferred embodiment of the present invention, the polypropylene random copolymer β i has a melting point of 110 to 150°C, preferably 120 to 140°C; and / or polypropylene random copolymer β i has a melt flow rate of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 3 to 18 g / 10 min at 230° C. and a load of 2.16 kg; and / or polypropylene random copolymer β i has a molecular weight distribution Mw / Mn of 5 to 12, preferably 7 to 10. Preferably, the polypropylene random copolymer β i are copolymers of propylene with ethylene and / or butene, preferably ethylene-propylene-butene terpolymers and / or propylene-ethylene bipolymers.

[0044] According to the present invention, polypropylene homopolymer γ i can be selected within a wide range. In a preferred embodiment of the present invention, the polypropylene homopolymer γ i has a melting point of 150 to 170°C, preferably 160 to 170°C; and / or polypropylene homopolymer γ i has a melt flow rate of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 2.5 to 18 g / 10 min at 230° C. under a load of 2.16 kg; and / or polypropylene homopolymer γ i has an isotacticity (mm) of 96% or more.

[0045] In a preferred embodiment of the present invention, the thermal adhesion improver z i has a melting point or viscous flow temperature of 70 to 110°C. And / or, a thermal adhesion improver z i is selected from one or more of polyolefin elastomer, ethylene-propylene-diene-terpolymer rubber, SEBS, SBS, EVA, and petroleum resin. i is a polyolefin elastomer and / or a petroleum resin.

[0046] In a preferred embodiment of the present invention, the polyolefin elastomer is preferably an elastomer of ethylene copolymerized with propylene and / or an α-olefin, the α-olefin being preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin having a softening point of 100-150°C; preferably a cyclopentadiene type resin.

[0047] According to the present invention, the thermal adhesion improver z i The melt flow rate of the thermal adhesion improver z can be selected within a wide range. ihas a melt flow rate at 190° C. under a load of 2.16 kg of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, preferably 1 to 18 g / 10 min, and more preferably 3 to 18 g / 10 min.

[0048] In a preferred embodiment of the present invention, the polypropylene random copolymer x i , and polypropylene random copolymer β i have a difference in melting point of less than 10°C, preferably less than 5°C, more preferably less than 3°C; and / or a difference in melt flow rate at 230°C, 2.16 kg load of less than 10 g / 10 min, preferably less than 5 g / 10 min, more preferably less than 3 g / 10 min; and / or a difference in molecular weight distribution of less than 3, preferably less than 2, more preferably less than 1. More preferably, the polypropylene random copolymer x i and polypropylene random copolymer β i is the same as

[0049] In a preferred embodiment of the present invention, polypropylene homopolymer a i , and polypropylene homopolymer γ i and / or a difference in melting point of less than 10° C., preferably less than 5° C., more preferably less than 3° C.; and / or a difference in melt flow rate at 230° C., 2.16 kg load of less than 10 g / 10 min, preferably less than 5 g / 10 min, more preferably less than 3 g / 10 min; and / or a difference in isotacticity (mm) of less than 3%, preferably less than 2%, more preferably less than 1%; and more preferably a difference in isotacticity (mm) of less than 3%, preferably less than 2%, more preferably less than 1%; i and polypropylene homopolymer γ i is the same as

[0050] In a preferred embodiment of the present invention, the thermal adhesion improver y i , and thermal adhesion improver z ihas a difference in melting point or viscous flow temperature of less than 10° C., preferably less than 5° C., more preferably less than 3° C.; and / or a difference in melt flow rate at 190° C. and 2.16 kg load of less than 10 g / 10 min, preferably less than 5 g / 10 min, more preferably less than 3 g / 10 min. More preferably, the thermal adhesion improver y i and thermal adhesion improver i is the same as

[0051] Through research conducted by the present inventors, polypropylene composition C i , C' i and polypropylene composition B i , B' i It has been found that when the melt mass flow rate and polymer composition ratio of the low melting point polypropylene random copolymer and the thermal adhesion improver in the composition are within the above preferred ranges, the heat press temperature can be significantly reduced and the heat press temperature window can be widened, and the thermal adhesion improver can provide good adhesion to the sheet and further improve the interlayer peel strength.

[0052] In a preferred embodiment of the present invention, polypropylene composition A i The melting point of polypropylene composition C i , C' i and polypropylene composition B i , B' i and the temperature difference between the respective melting points is preferably 5° C. or more, more preferably 10° C. or more, and more preferably 20° C. or more. i Polypropylene homopolymer a in the component i The melting point of polypropylene composition C i , C' i Polypropylene random copolymer β i Melting point of polypropylene composition B i , B' i Polypropylene random copolymer x i The melting point of each is higher than that of the other, and the temperature difference between their melting points is 10°C or more.

[0053] According to the present invention, the polypropylene compositions Ci and C' of the present invention i and polypropylene compositions Bi and B' i The difference in melting point between the two is not particularly limited.

[0054] Through research conducted by the present inventors, polypropylene composition A i , Polypropylene Composition C i , C' i , and composition B i , B' i It has been found that when the melt mass flow rate, the melting point difference, the polymer composition ratio, and the thickness distribution of the polymer composition are within the above preferred ranges, the sheet preparation process can be made even smoother, and the sheet uniformity, tensile strength, impact properties, and interlayer peel strength can be made even better.

[0055] According to the present invention, the polypropylene sheet layer unit B i C i A i C' i B' i The sheet structure is made of polypropylene composition A. i , Polypropylene Composition C i , C' i , and polypropylene composition B i , B' i The composition can be obtained by co-extrusion of the components comprising:

[0056] According to the present invention, the polypropylene sheet can be a film and can have a certain thickness. In the present invention, the polypropylene film is one form of the polypropylene sheet.

[0057] According to the present invention, the polypropylene sheet layer unit is a polypropylene sheet and / or a polypropylene fabric; the polypropylene sheet layer unit may be a polypropylene sheet or may be a polypropylene fabric. In a preferred embodiment of the present invention, the polypropylene sheet layer unit is a polypropylene sheet or a polypropylene fabric.

[0058] In a preferred embodiment of the present invention, the polypropylene sheet is made of polypropylene composition A. i , Polypropylene Composition B i , Polypropylene Composition B' i , optionally polypropylene composition C i , optionally polypropylene composition C' i The composition is prepared by co-extruding components comprising:

[0059] In a preferred embodiment of the present invention, a polypropylene fabric is prepared by the following method: i , Polypropylene Composition B i , Polypropylene Composition B' i , optionally polypropylene composition C i , optionally polypropylene composition C' i The components comprising are co-extruded to obtain a polypropylene sheet, and then the polypropylene sheet is woven to obtain a polypropylene fabric; preferably, the polypropylene fabric has a plain weave, twill weave and / or satin weave configuration.

[0060] According to the invention, preferably the various polypropylene sheet layer units are connected by heat press bonding.

[0061] In a preferred embodiment of the present invention, the polypropylene composite has at least one of the following characteristics: A tensile strength in the machine direction of 160 MPa or more, preferably 180 MPa or more; an interlayer peel strength of 1.3 N / mm or more, preferably 1.5 N / mm or more.

[0062] The tensile strength in the machine direction is measured according to the method specified in GB / T1040.1-2018, and the delamination strength is measured according to the method specified in GB / T2358-98. The samples corresponding to the above two tests are the standard samples required by the above test standards.

[0063] When the polypropylene composite material is obtained by hot pressing and fusing five polypropylene sheet layer units, and the thickness of the polypropylene composite material is about 390 μm, it has a drop impact strength of 42 J or more, preferably 45 J or more.

[0064] The drop impact strength is measured according to the method specified in GB / T14153-1993, and the thickness of the sample is the thickness of the prepared product.

[0065] A second object of the present invention is to provide a method for preparing the above-mentioned polypropylene composite material, comprising the steps of laminating 2n-1 polypropylene sheet layer unit groups in the order of nth group, ... ith group, ... 2nd group, 1st group, 2nd group, ... ith group, ... nth group, and then performing heat pressing and fusion bonding.

[0066] In an embodiment in which each polypropylene sheet layer unit group includes only one polypropylene sheet layer unit, the preparation method includes the following steps: i A i B' i The 2n-1 polypropylene sheet layer units having the structure n A n B' n ......B i A i B' i ......B2A2B'2, B1A1B'1, B2A2B'2......B i A i B' i ......B n A n B' n The process then involves laminating the layers in the order listed above, followed by heat pressing and fusion bonding.

[0067] In an embodiment in which each polypropylene sheet layer unit group comprises two or more polypropylene sheet layer units, the preparation method includes the following steps: sequentially laminating the polypropylene sheet layer units of each polypropylene sheet layer unit group, then sequentially laminating 2n-1 polypropylene sheet layer unit groups in the order of nth group, ... ith group, ... 2nd group, 1st group, 2nd group, ... ith group, ... nth group, and then performing heat pressing and fusion.

[0068] In a preferred embodiment of the present invention, the preparation method comprises the steps of: (1) Polypropylene Composition A i , Polypropylene Composition B i and polypropylene composition B' i , optionally polypropylene composition C i , optionally polypropylene composition C' i A, B i A i B' i Structure or B i C i A i C' i B' i co-extrusion, casting or calendering according to the structure and stretching to obtain a polypropylene sheet; (2) Optionally, the polypropylene sheet is divided and cut, and then woven into B i A i B' i Structure or B i C i A i C' i B' i obtaining a structural polypropylene fabric; (3) Polypropylene sheets and / or polypropylene fabrics are sequentially laminated, heat pressed and fused, then cooled and molded to form a polypropylene composite material.

[0069] In a preferred embodiment of the present invention, in step (1), polypropylene composition Ai The preparation of polypropylene composition A includes melt blending ingredients such as components including at least one of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer. i The melt blending conditions and the apparatus are all the same as those of the polyolefin melt blending conditions and the apparatus of the prior art. Preferably, the melt temperature is 190-240° C., and the apparatus is preferably a twin-screw extruder.

[0070] In a preferred embodiment of the present invention, in step (1), polypropylene composition B i , B' i The preparation of polypropylene composition B includes melt blending ingredients such as components including at least one of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; i , B' i The melt blending conditions and the apparatus are all the same as those of the polyolefin melt blending conditions and the apparatus of the prior art. Preferably, the melt temperature is 190-240° C., and the apparatus is preferably a twin-screw extruder.

[0071] In a preferred embodiment of the present invention, in step (1), polypropylene composition C i , C' i The preparation of polypropylene composition C includes melt blending ingredients such as components including at least one of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; i , C' i The melt blending conditions and the apparatus are all the same as those of the polyolefin melt blending conditions and the apparatus of the prior art. Preferably, the melt temperature is 190-240° C., and the apparatus is preferably a twin-screw extruder.

[0072] In a preferred embodiment of the present invention, in step (1), the temperature of co-extrusion and casting is independently selected from 200 to 240°C; and / or the temperature of the calender roller is 50 to 70°C.

[0073] In a preferred embodiment of the present invention, the stretching conditions include: a stretching temperature of 90-165°C, preferably 90-140°C, more preferably 90-119°C; and / or a stretching ratio of 1-15, preferably 2-9.

[0074] In a preferred embodiment of the present invention, the polypropylene sheet obtained in step (1) has a width of 2 to 5 mm.

[0075] In a preferred embodiment of the present invention, in step (3), the heat pressing conditions include the following: a heat pressing temperature of 115-170°C, preferably 115-159°C, more preferably 140-159°C, a heat pressing pressure of 2-10 MPa, a preheating time of 5-600 s, and a heat pressing time of 1-600 s, preferably 10-500 s.

[0076] In a preferred embodiment of the present invention, the pressure for cooling and molding is 2 to 8 MPa, and the cooling time is 30 to 700 s.

[0077] In a preferred embodiment of the invention, the laminated adjacent polypropylene fabrics are oriented at an angle of 0 to 90 degrees relative to each other along their respective warp directions; and / or the laminated adjacent polypropylene sheets are oriented at an angle of 0 to 90 degrees relative to each other along their respective machine directions, the machine direction being the stretch direction (MD).

[0078] In a more preferred embodiment of the present invention, the method for preparing a polypropylene composite material comprises the following steps: Step a: Polypropylene composition A i , Polypropylene Composition B i , Polypropylene Composition B' i , optionally polypropylene composition C i , optionally polypropylene composition C' i A, B i A i B' i Structure or B i Ci A i C' i B' i Co-extrusion molding according to the structure, and casting or calendaring to obtain a co-extruded polypropylene sheet; preferably, the temperature of co-extrusion molding, casting or calendaring is 200-230°C, and the temperature of the calendar roller is 50-70°C; Step b: The coextruded polypropylene sheet is solid-phase stretched at a certain temperature to obtain a stretched polypropylene film or a stretched polypropylene sheet; the stretching temperature is preferably 90 to 165°C, more preferably 90 to 140°C, and more preferably 90 to 119°C, and the stretching ratio is 1 to 15; Step c: preparing polypropylene ribbons by splitting and cutting the stretched polypropylene film or stretched polypropylene sheet, and weaving the ribbons to obtain polypropylene fabric; preferably, the width of the polypropylene ribbon is 2-5mm, and the structure of the polypropylene fabric includes, but is not limited to, plain weave, twill weave, satin weave and / or other three-dimensional polypropylene fabrics; Step d: The stretched polypropylene film, sheet or fabric is laminated from bottom to top in the order of nth group...ith group...2nd group, 1st group, 2nd group...ith group...nth group, and the total number of laminated groups is 2n-1, where n is 2 or more. The polypropylene sheet or fabric is heat pressed and fused, and then cooled and molded to make a polypropylene composite; the heat press temperature is preferably 110-180°C, more preferably 115-170°C, and even more preferably 130-160°C, the heat press pressure is 2-10MPa, the preheat time is 5-600s, the heat press time is 1-600s, preferably 10-500s, the cooling pressure is 2-8MPa, and the cooling time is 30s-700s; preferably, the polypropylene sheets in the polypropylene composite are arranged at an angle of 0-90 degrees relative to each other along their respective machine directions, and the polypropylene fabrics in the polypropylene composite are arranged at an angle of 0-90 degrees relative to each other along their respective warp directions.

[0079] The third object of the present invention is to provide a continuous hot press molding system for polypropylene composite material of the present invention, which includes a preheater 1, a crawler type continuous flat heat press 2, a crawler type continuous flat cooling press 3, a sheet cutting machine 4 and a sheet laminating machine 5, which are sequentially arranged as shown in FIG. 1; Preferably, the crawler type continuous plate hot press 3 includes a preheating unit 6 , an independent heating and pressing unit 7 , an air-cooling unit 8 , and a lifting mechanism 9 .

[0080] According to the present invention, in a preferred specific embodiment, during the heat pressing and cooling process, the pressure is preferably maintained continuously and not decreased, and the heat pressing process is carried out continuously, preferably using a continuous heat pressing composite molding device consisting of a preheater 1, a crawler type continuous flat heat press 2, a crawler type continuous flat cooling press 3, a sheet cutting machine 4 and a sheet laminating machine 5, as shown in FIG. 1; preferably, the crawler type continuous flat heat press 2 has a preheating unit 6, an independent heating and pressing unit 7, an air cooling unit 8 and a lifting mechanism 9. In the preparation, the stretched polypropylene film, sheet or (and) fabric is sequentially laminated, then preheated by the preheater 1, the preheated sample is sequentially heat pressed and fused by the crawler type continuous flat heat press 2, and then cooled and molded by the crawler type continuous flat cooling press 3 to make a polypropylene composite material, i.e., a laminated heat pressing product. After that, the heat pressing product is cut by the sheet cutting machine 4 as necessary, and then laminated and arranged by the sheet laminating machine 5. Here, in the crawler-type continuous flat hot press 2, the hot press temperature is controlled by a preheating unit 6, an independent heating and pressing unit 7, and an air-cooling unit 8, and the hot press pressure is controlled by a lifting mechanism 9.

[0081] Through the research conducted by the present inventors, it has been found that when the preparation process parameters are within the above preferred ranges, more preferably when the present preparation apparatus is employed to prepare the polypropylene composite material, the polypropylene composite material has better tensile strength, impact properties and interlayer peel strength.

[0082] The fourth object of the present invention is to provide the use of the polypropylene composite material as described above and the polypropylene composite material prepared by the above-mentioned preparation method in the applications of consumer goods, automobile manufacturing, sports protection and military materials.

[0083] According to a specific embodiment of the present invention, the material fields include luggage and transportation industry, shoe industry, automobile manufacturing industry, sports equipment manufacturing industry, audio equipment manufacturing industry and military field.

[0084] The fifth object of the present invention is to provide a polypropylene sheet having a structure of BAB', which comprises a layer A and layers B and B' located on both sides of the layer A, which is preferably used as a polypropylene sheet layer unit in the above-mentioned polypropylene composite material, i.e., as a polypropylene sheet layer unit in a self-reinforced polymer composite material; wherein the layer A contains a polypropylene composition A, the layer B is the same as or different from the layer B', the layer B contains a polypropylene composition B, the layer B' contains a polypropylene composition B', and the melting point of the polypropylene composition A is higher than the melting points of the polypropylene composition B and the polypropylene composition B'; wherein the polypropylene composition A contains a polypropylene homopolymer a and a polypropylene impact copolymer b; the polypropylene composition B and the polypropylene composition B' contain a polypropylene random copolymer x and a thermal adhesion improver y, respectively; preferably, the polypropylene random copolymer x has a molecular weight distribution Mw / Mn of 5 to 12, preferably 7 to 10.

[0085] In a preferred embodiment of the present invention, the polypropylene sheet further comprises layers C and C' in a structure of BCAC'B'; layer C is the same as or different from layer C', layer C contains polypropylene composition C, and layer C' contains polypropylene composition C'; the melting point of polypropylene composition A is higher than the melting points of polypropylene composition C and polypropylene composition C'; wherein polypropylene composition C and polypropylene composition C' respectively comprise polypropylene random copolymer β, polypropylene homopolymer γ, and thermal adhesion improver z; preferably, polypropylene random copolymer β has a molecular weight distribution Mw / Mn of 5-12, preferably 7-10.

[0086] All the features described above for the polypropylene sheet layer unit apply to the polypropylene sheet. Layer A of the polypropylene sheet layer unit i , layer B i , layer B i ', layer C i and layer C i The features described for ' apply to layers A, B, B', C and C' of the polypropylene sheet, respectively; polypropylene composition A of the polypropylene sheet layer unit i , B i , B i ', C i and C i The features described for ' apply to the polypropylene compositions A, B, B', C and C' of the polypropylene sheet, respectively; the polypropylene homopolymer a of the polypropylene sheet layer unit i , polypropylene impact copolymer b i , polypropylene random copolymer x i , Thermal adhesion improver y i , polypropylene random copolymer β i , polypropylene homopolymer γ i , and thermal adhesion improver z iThe features described above apply to the polypropylene homopolymer a, the polypropylene impact copolymer b, the polypropylene random copolymer x, the thermal adhesion improver y, the polypropylene random copolymer β, the polypropylene homopolymer γ, and the thermal adhesion improver z of the polypropylene sheet, respectively.

[0087] In a preferred embodiment of the present invention, the melting point of polypropylene composition A is higher than that of polypropylene compositions B, B'; preferably, the melting point of polypropylene homopolymer a in polypropylene composition A is higher than that of polypropylene random copolymer x in polypropylene compositions B, B', and preferably the temperature difference between the respective melting points is 10°C or more. In this preferred specific embodiment, the inventors of the present invention have surprisingly found that by heat pressing the obtained polypropylene sheet, a polypropylene composite material having better mechanical properties is obtained, and at the same time, even if the heat pressing temperature is low or the heat pressing temperature range is wide, the interlayer peel strength of the obtained polypropylene composite material is higher, and a polypropylene composite material having better interlayer peel strength is obtained.

[0088] Through research conducted by the present inventors, it has been found that when the melt mass flow rate, the polymer composition ratio of polypropylene composition A to polypropylene compositions B and B', and the thickness distribution of film layer A are within preferred ranges, the sheet preparation process can be carried out more smoothly, and the sheet can have better uniformity, tensile strength, impact properties, and interlayer peel strength.

[0089] The BAB' sheet structure of the polypropylene sheet can be prepared by various methods. In a preferred embodiment of the present invention, the BAB' sheet structure of the polypropylene sheet is obtained by co-extruding the components comprising the polypropylene composition A and the polypropylene compositions B, B'.

[0090] In a preferred embodiment of the present invention, the melting point of polypropylene composition A is higher than the melting points of polypropylene compositions B, B' and polypropylene compositions C, C', and preferably the temperature difference between the respective melting points is 5° C. or more, preferably 10° C. or more, more preferably 20° C. or more. Preferably, the melting point of polypropylene homopolymer a in the component of polypropylene composition A is higher than the melting point of polypropylene random copolymer β in polypropylene compositions B, B' and the melting point of polypropylene random copolymer x in polypropylene compositions C, C', and the temperature difference between the respective melting points is 10° C. or more.

[0091] According to the present invention, the difference in melting point between the polypropylene compositions B, B' and the polypropylene compositions C, C' in the present invention is not particularly limited.

[0092] Through research conducted by the present inventors, it has been found that when the melt mass flow rates, melting point difference, polymer composition ratio and polymer composition thickness distribution of polypropylene composition A, polypropylene compositions B, B' and compositions C, C' are within the above-mentioned preferred ranges, the sheet preparation process can be carried out more smoothly, and the sheet uniformity, tensile strength, impact properties and interlayer peel strength can be made better.

[0093] According to the present invention, the BCAC'B' sheet structure of the polypropylene composite sheet is obtained by co-extruding the components comprising polypropylene composition A, polypropylene compositions B, B' and polypropylene compositions C, C'.

[0094] A sixth object of the present invention is to provide a process for preparing the above polypropylene sheet which comprises co-extruding, casting or calendaring polypropylene composition A, polypropylene composition B, polypropylene composition B', optionally polypropylene composition C, optionally polypropylene composition C' according to BAB' structure or BCAC'B' structure and stretching to obtain a polypropylene sheet.

[0095] In a preferred embodiment of the present invention, the preparation of polypropylene composition A comprises melt blending components comprising polypropylene homopolymer a and polypropylene impact copolymer b; and / or the preparation of polypropylene compositions B, B' comprises melt blending components comprising polypropylene random copolymer x and thermal adhesion improver y; and / or the preparation of polypropylene compositions C, C' comprises melt blending components comprising thermal adhesion improver z, polypropylene random copolymer β and polypropylene homopolymer γ; and / or the coextrusion and casting temperatures are independently selected from 200 to 240°C; and / or the temperature of the calendar rollers is 50 to 70°C; and / or the stretching conditions comprise a stretching temperature of 90 to 165°C, preferably 90 to 140°C, more preferably 90 to 119°C; and a stretching ratio of 1 to 15, preferably 2 to 9.

[0096] According to some embodiments of the present invention, polypropylene composition A, polypropylene composition B, polypropylene composition B', optionally polypropylene composition C, optionally polypropylene composition C' are co-extruded, cast or calendered according to BAB' structure or BCAC'B' structure to obtain a co-extruded polypropylene sheet. The process of extrusion-calendering can include passing the co-extruded polypropylene sheet through a calender roller and a take-up roller in sequence, and then subjecting it to solid-state stretching, edge cutting and rolling to prepare a sheet. Here, the temperature of extrusion and casting is 200-230°C, and the temperature of the calender roller is 50-70°C. The specific process of film preparation by extrusion-calendering is a common choice in the art, and further detailed description is omitted.

[0097] All the features described above with respect to the method for preparing the polypropylene sheet layer unit also apply to the method for preparing the polypropylene sheet.

[0098] A seventh object of the present invention is to provide a three-dimensional polypropylene fabric obtained by weaving the polypropylene sheet as described above, preferably having a three-dimensional structure of plain weave, twill weave and / or satin weave.

[0099] To facilitate weaving, it is preferable to cut the polypropylene sheet into pieces having a width of 2 to 5 mm, and then weave the pieces to obtain a polypropylene fabric.

[0100] In a more preferred embodiment of the present invention, the polypropylene fabric is a plain weave, twill weave, satin weave or 3D polypropylene fabric obtained by weaving a three-layer coextrusion oriented polypropylene ribbon, the three-layer coextrusion oriented polypropylene ribbon comprises a layer A formed from a high melting point polypropylene composition A, and layers B, B' formed from low melting point polypropylene compositions B, B', where the polypropylene composition A comprises a polypropylene homopolymer a, a polypropylene impact copolymer b; the polypropylene compositions B, B' comprise a polypropylene random copolymer x, and a thermal adhesion enhancer y, and the three-layer polypropylene fabric has a structure of BAB' from bottom to top.

[0101] In a more preferred embodiment of the present invention, the polypropylene fabric is a plain weave, twill weave, satin weave and / or 3D polypropylene fabric obtained by weaving a 5-layer coextrusion stretched polypropylene ribbon, the coextrusion stretched polypropylene ribbon includes a layer A formed from a high melting point polypropylene composition A, an intermediate layer C, C' formed from a polypropylene composition C and a layer B, B' formed from a low melting point polypropylene composition B, the polypropylene composition A includes a polypropylene homopolymer a, a polypropylene impact copolymer b, the polypropylene compositions C, C' include a thermal adhesion improver z, a polypropylene random copolymer β, and a polypropylene homopolymer γ, the polypropylene compositions B, B' include a polypropylene random copolymer x, and a thermal adhesion improver y, and the 5-layer polypropylene fabric has a structure of BCAC'B' from bottom to top.

[0102] All of the features described above with respect to the polypropylene sheet layer unit and the polypropylene sheet apply to the polypropylene fabric.

[0103] The eighth object of the present invention is to provide a polypropylene composite material, prepared by heat pressing and fusing multiple layers of polypropylene sheets as described above and / or polypropylene fabrics as described above; preferably, the polypropylene fabrics are arranged and stacked at an angle of 0-90 degrees to each other along their respective warp directions from top to bottom, and the number of layers is preferably 2 or more, more preferably 2-200 layers; and most preferably 4-100 layers. The polypropylene sheets are arranged and stacked at an angle of 0-90 degrees to each other along their respective machine directions from top to bottom, and the number of layers is preferably 2 or more, more preferably 2-200 layers, and most preferably 4-100 layers.

[0104] In a preferred embodiment of the present invention, the polypropylene composition A contained in each layer of the laminated polypropylene fabric can be the same or different, and the polypropylene composition A contained in each layer can be independently selected, and preferably, the polypropylene composition A of each layer is the same.

[0105] In a preferred embodiment of the present invention, the polypropylene composite has at least one of the following characteristics: a tensile strength in the machine direction of 150 MPa or more, preferably 170 MPa or more; The interlayer peel strength is 1 N / mm or more, and preferably 1.2 N / mm or more.

[0106] The tensile strength is measured according to the method specified in GB / T1040.1-2018, and the delamination strength is measured according to the method specified in GB / T2358-98. The samples corresponding to the above two tests are the standard samples required by the above test standards.

[0107] The polypropylene composite material is obtained by heat pressing and fusing 24 layers of polypropylene fabric, and has a drop impact strength of 228J or more, preferably 240J or more, when its thickness is about 1.6mm.

[0108] The drop impact strength is measured according to the method specified in GB / T14153-1993, and the thickness of the sample is the thickness of the prepared product.

[0109] According to the present invention, when the polypropylene composite sheet has a sheet structure of BCAC'B', the polypropylene composite has at least one of the following characteristics: The tensile strength in the machine direction (MD) is 150 MPa or more, preferably 170 MPa or more; the interlayer peel strength is 1.1 N / mm or more, preferably 1.3 N / mm or more. When a composite is obtained by heat pressing and fusing 24 layers of polypropylene fabric and has a thickness of about 1.8 mm, it has a drop impact strength of 240 J or more, preferably 250 J or more.

[0110] A ninth object of the present invention is to provide a process for the preparation of polypropylene composite as above which comprises laminating, heat pressing and fusing polypropylene sheets and / or polypropylene fabrics and then cooling and molding them to form a polypropylene composite.

[0111] In a preferred embodiment of the present invention, the temperature for heat pressing and fusion is 115 to 170°C, preferably 115 to 159°C, and more preferably 140 to 159°C.

[0112] In a preferred embodiment of the present invention, the pressure for heat pressing and fusion is 2 to 10 MPa.

[0113] In a preferred embodiment of the present invention, the preheating time for heat pressing and fixing is 5 to 600 s, and the heat pressing time is 1 to 600 s, preferably 10 to 500 s.

[0114] In a preferred embodiment of the present invention, the pressure for cooling and molding is 2 to 8 MPa, and the cooling and molding time is 30 to 700 s.

[0115] In a preferred embodiment of the present invention, the number of layers of the polypropylene sheet and / or polypropylene fabric is 2 or more, preferably 2 to 200 layers, and more preferably 4 to 100 layers.

[0116] In a preferred embodiment of the present invention, adjacent layers in a laminate of polypropylene sheets are oriented at angles of 0 to 90 degrees relative to each other along their respective machine directions (MD).

[0117] In a preferred embodiment of the invention, adjacent layers in a polypropylene fabric stack are oriented at angles of 0 to 90 degrees relative to each other along their respective warp directions.

[0118] In a more preferred embodiment of the present invention, a method for preparing a high strength, high impact polypropylene composite material comprises the following steps: Step a: polypropylene composition A, polypropylene composition B, B' are co-extruded, cast or calendered according to the BAB' structure to obtain a co-extruded polypropylene sheet; preferably, the temperature of extrusion, casting or calendering is 200-240°C, and the temperature of the calender roller is 50-70°C; Step b: Stretching the coextruded polypropylene sheet at a certain temperature to obtain a stretched polypropylene sheet; preferably, the stretching temperature is 90-165°C, preferably 90-140°C, more preferably 90-119°C, and the stretching ratio is 1-15, preferably 2-9. Step c: Dividing and cutting the stretched polypropylene sheet to prepare polypropylene ribbons, and weaving the ribbons to obtain polypropylene fabric; preferably, the width of the polypropylene ribbon is 2-5mm, and the polypropylene fabric includes plain weave, twill weave, satin weave or other three-dimensional polypropylene fabric; Step d: polypropylene fabrics are sequentially laminated, heat pressed and fused, and then cooled and molded to prepare a polypropylene composite material; preferably in step d, the heat pressing conditions are a heat pressing temperature of 115-170°C, preferably 115-159°C, more preferably 140-159°C; a heat pressing pressure of 2-10 MPa, a preheating time of 5-600 s, a heat pressing time of 1-600 s, preferably 10-500 s, a cooling pressure of 2-8 MPa, and a cooling time of 30 s-700 s; preferably, adjacent polypropylene fabrics in the polypropylene composite material can be arranged at an angle of 0-90 degrees to each other along their respective warp directions.

[0119] According to some embodiments of the present invention, in step c, cutting is performed using a multi-blade high-speed dividing cutter to obtain oriented polypropylene ribbons with a width of 2-5 mm. The oriented ribbons are woven using a commercially available weaving machine according to a designed fabric structure to obtain plain weave, twill weave, satin weave and / or other three-dimensional polypropylene fabrics.

[0120] In a more preferred embodiment of the present invention, the method for preparing a polypropylene composite material comprises the following steps: Step a: Co-extrusion, casting or calendaring the polypropylene composition A, the polypropylene compositions C, C', and the polypropylene compositions B, B' according to the BCAC'B' structure to obtain a co-extruded polypropylene sheet; preferably, the temperature of the extrusion, casting or calendaring is 200-230°C, and the temperature of the calendar roller is 50-70°C; Step b: Stretching the coextruded polypropylene sheet at a certain temperature to obtain a stretched polypropylene sheet; the stretching temperature is preferably 90 to 165°C, more preferably 90 to 140°C, and more preferably 90 to 119°C, and the stretching ratio is 1 to 15; Step c: Dividing and cutting the polypropylene stretched sheet to prepare polypropylene ribbons, and weaving the ribbons to obtain polypropylene fabrics; preferably, the width of the polypropylene ribbon is 2-5 mm, and the polypropylene fabrics include plain weave, twill weave, satin weave or other three-dimensional polypropylene fabrics; Step d: polypropylene sheets or fabrics are sequentially laminated, heat pressed and fused, then cooled and molded to make a polypropylene composite; preferably, the heat pressing conditions are a heat pressing temperature of 115-170°C, preferably 115-159°C, more preferably 140-159°C; a heat pressing pressure of 2-10 MPa, a pre-heating time of 5-300 s, a heat pressing time of 1-300 s, preferably 1-9 s or 61-100 s, a cooling pressure of 2-8 MPa, and a cooling time of 30 s-700 s; in the polypropylene composite, the polypropylene fabrics can be arranged at an angle of 0-90 degrees relative to each other along their respective warp directions; and / or the polypropylene composite sheets are arranged at an angle of 0-90 degrees relative to each other along their respective machine directions.

[0121] According to the present invention, in a preferred specific embodiment, during the heat pressing and cooling process, the pressure is preferably maintained continuously and does not decrease, and the heat pressing process is carried out continuously.Preferably, a continuous heat pressing composite molding device is used, which is composed of a preheater, a crawler type continuous flat heat press, a crawler type continuous flat cooling press, a sheet cutting machine, and a sheet laminating machine, which are arranged in sequence;preferably, the crawler type continuous flat heat press has a preheating unit, an independent heating and pressing unit, an air cooling unit, and a lifting mechanism.

[0122] In the preparation, polypropylene sheets and / or polypropylene fabrics are laminated in sequence, then preheated by a preheating machine, the preheated samples are heat pressed and fused in sequence by a crawler-type flat heat press, and then cooled and molded by a crawler-type continuous flat cooling press to produce a polypropylene composite material, i.e., a laminated heat-pressed product. After that, the heat-pressed product is cut by a sheet cutting machine as required, and laminated and arranged by a sheet laminating machine. The crawler-type continuous flat heat press has a preheating unit, an independent heating and pressing unit, an air-cooling unit to control the heat-pressing temperature, and a lifting mechanism to control the heat-pressing pressure. Through the research conducted by the present inventors, it has been found that when the preparation process parameters are within the preferred range, preferably, the preparation device is adopted to prepare the polypropylene composite material, and the polypropylene composite material has better tensile strength, impact properties, and interlayer peel strength.

[0123] A tenth object of the present invention is to provide the use of the polypropylene sheet as described above, the polypropylene fabric as described above, the polypropylene composite material as described above, and the polypropylene composite material prepared by the preparation method as described above in the applications of sports protection, automobile manufacturing, consumer goods, and military materials.

[0124] According to a specific embodiment of the present invention, the material fields include luggage and transportation industry, shoe industry, automobile manufacturing industry, sports equipment manufacturing industry, audio equipment manufacturing industry, and military field.

[0125] Compared with the prior art, the present invention has the following beneficial effects: (1) The polypropylene composite material of the present invention has a melting point gradient structure. Due to this specific structure, the inventors of the present invention have surprisingly found that the resulting polypropylene composite material simultaneously has good tensile strength, impact properties, and interlayer peel strength.

[0126] In particular, when the polypropylene composite sheet has a BAB' sheet structure, the polypropylene composite has the following characteristics: tensile strength in machine direction (MD) of 150 MPa or more, preferably 170 MPa or more; interlayer peel strength of 1 N / mm or more, preferably 1.2 N / mm or more; drop impact strength of 228 J or more, preferably 240 J or more, when the composite is obtained by hot pressing and fusing 24 layers of polypropylene fabric and has a thickness of about 1.6 mm.

[0127] In particular, when the polypropylene composite sheet has a BCAC'B' sheet structure, the polypropylene composite has the following characteristics: tensile strength in machine direction (MD) of 150 MPa or more, preferably 170 MPa or more; peel strength between layers of 1.1 N / mm or more, preferably 1.3 N / mm or more. When the thickness of the composite obtained by heat pressing and fusing 24 layers of polypropylene fabric is about 1.8 mm, its drop impact strength is 240 J or more, preferably 250 J or more.

[0128] (2) The polypropylene composite of the present invention can be adapted to be prepared at a lower heat press temperature and a wider heat press temperature range, which can effectively reduce the energy consumption of the equipment and the damage of the composite under high temperature operation. At the same time, even when prepared at a lower heat press temperature, the composite has good interlayer peel strength.

[0129] (3) This preparation method can shorten the operation time of the heat press, improve the production efficiency, and reduce the production energy consumption.

[0130] (4) The present invention adopts a melting point gradient structure design, which reduces and expands the hot pressing temperature, and the hot pressing temperature range can reach 70°C; effectively reducing the energy consumption of the equipment and the damage of composite materials under high temperature operation.

[0131] The present invention also relates to the following embodiments: 1. A plurality of polypropylene sheet layer units are laminated in sequence, each of the polypropylene sheet layer units being a core layer A i and Core Layer A i Outer layer B located on both sides of i and B' i Including B i A i B' i The polypropylene composite structure is B from bottom to top. n A n B' n ......B i A i B' i ......B2A2B'2, B1A1B'1, B2A2B'2......B i A i B' i ......B n A n B' n the total number of laminations of the polypropylene sheet layer units is 2n-1; i and n are both integers of 2 or more, and i≦n; Here, the core layer A in the polypropylene sheet layer unit i Polypropylene composition A i and outer layer B i However, the outer layer B' i Same or different, outer layer B i However, polypropylene composition B i and an outer layer B' i Polypropylene composition B' i Contains Polypropylene composition A i The melting point of polypropylene composition B i , Polypropylene Composition B' i higher than the melting point of polypropylene composition B i , Polypropylene Composition B' i The melting points of the adjacent polypropylene compositions B' are i-1 , Polypropylene Composition B i-1 polypropylene composite material, which has a melting point higher than that of

[0132] 2. Polypropylene Composition Ai Melting point of polypropylene composition B i and polypropylene composition A i and polypropylene composition B' i and / or Polypropylene composition B i , Polypropylene Composition B' i and the melting points of adjacent polypropylene compositions B' i-1 , Polypropylene Composition B i-1 and the melting point difference between them, whether they are the same or different, is 1 to 40°C, preferably 1 to 10°C, and more preferably 1 to 5°C.

[0133] 3. The polypropylene composite according to embodiment 1, characterized in that 2≦n≦100, preferably 2≦n≦50.

[0134] 4. Core layer A of each polypropylene sheet layer unit i The polypropylene composite material according to embodiment 1, characterized in that the thickness of each polypropylene sheet layer unit accounts for 51% to 89%, preferably 71% to 89%, and more preferably 71% to 80% of the total thickness of each polypropylene sheet layer unit.

[0135] 5. Polypropylene Composition A i comprises one or more of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; and / or Polypropylene composition B i and B' i Each of the polypropylene compositions B and C comprises one or more of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer, and preferably comprises polypropylene composition B. i and / or polypropylene composition B' i However, the thermal adhesion improver y i2. The polypropylene composite of embodiment 1, further comprising:

[0136] 6. Polypropylene Composition A i However, polypropylene homopolymer a i , and polypropylene impact copolymer b i Includes; Preferably, based on the total weight of polypropylene composition A, polypropylene composition A i However, 50 to 99% by weight of polypropylene homopolymer a i , 1 to 50% by weight of polypropylene impact copolymer b i More preferably, the polypropylene composition A comprises i However, 70 to 90% by weight of polypropylene homopolymer a i , 10 to 30% by weight of polypropylene impact copolymer b i and / or Polypropylene composition B i , Polypropylene Composition B' i are polypropylene random copolymer x i , and thermal adhesion improver y i Includes; Preferably, polypropylene composition B i , Polypropylene Composition B' i Polypropylene composition B based on the total weight of each of i , Polypropylene Composition B' i Each of them is 70 to 99% by weight of polypropylene random copolymer x i , 1 to 30% by weight of a thermal adhesion improver y i Preferably, polypropylene composition B i However, 80-90% by weight of polypropylene random copolymer x i , 10 to 20% by weight of a thermal adhesion improver y i 6. The polypropylene composite material of embodiment 5, comprising:

[0137] 7. Polypropylene homopolymer a ihas a melting point of 150-170°C; and / or Polypropylene homopolymer a i has an isotacticity (mm) of 96% or less; and / or Polypropylene Impact Copolymer B i has a melting point of 150-170°C; and / or the monomer copolymerized with propylene in the polypropylene impact copolymer is ethylene or butene, preferably butene; and / or Polypropylene impact copolymer: 20KJ / m 2 7. The polypropylene composite material of embodiment 6, having an Izod impact strength of at least

[0138] 8. Polypropylene random copolymer x i has a melting point of 110 to 150°C, and x i The melting point of x i-1 and / or Polypropylene Random Copolymer x i 7. The polypropylene composite according to embodiment 6, wherein said polypropylene composite is a copolymer of propylene with ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene bipolymer.

[0139] 9. Thermal adhesion improver i has a melting point or viscous flow temperature of 70 to 110°C; and / or Thermal adhesion improver i is selected from one or more of polyolefin elastomers, ethylene-propylene-diene-terpolymer rubbers, SEBS, SBS, EVA, and petroleum resins; Preferably, the thermal adhesion improver y i 7. The polypropylene composite material according to embodiment 6, wherein said polyolefin elastomer and / or petroleum resin are polyolefin elastomers and / or petroleum resins.

[0140] 10. The polyolefin elastomer is an elastomer of ethylene copolymerized with propylene and / or an α-olefin, the α-olefin being preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or 10. The polypropylene composite material according to embodiment 9, wherein the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin having a softening point of 100-150°C, preferably a cyclopentadiene type resin.

[0141] 11. Polypropylene Composition A i but also includes a β-nucleating agent; preferably the β-nucleating agent is selected from at least one of polycyclic aromatic hydrocarbons, Group IIA binary complexes, aromatic diamides, rare earth compounds, and cyclic dicarboxylate nucleating agents; and / or Polypropylene composition A i The content of the β-nucleating agent in the polypropylene composition A is i The polypropylene composite material according to embodiment 5, wherein the content is 0.01 to 0.5 parts by weight based on 100 parts by weight of the total amount.

[0142] 12. The polypropylene sheet layer unit is a polypropylene sheet and / or a polypropylene fabric; preferably, the polypropylene sheet layer unit is a polypropylene sheet or a polypropylene fabric; more preferably, The polypropylene sheet is made of polypropylene composition A. i , Polypropylene Composition B i and polypropylene composition B' i and / or The polypropylene fabric is prepared by the following method: i , Polypropylene Composition B i , Polypropylene Composition B' i12. The polypropylene composite material according to any one of embodiments 1 to 11, characterized in that the polypropylene composite material is prepared by a process comprising co-extruding a component comprising the components to obtain a polypropylene sheet and then weaving the polypropylene sheet to obtain a polypropylene fabric; preferably, the polypropylene fabric has a plain weave, twill weave and / or satin weave configuration.

[0143] 13. The polypropylene composite material according to embodiment 12, characterized in that the various polypropylene sheet layer units are connected by heat press bonding.

[0144] 14.B i A i B' i The 2n-1 polypropylene sheet layer units having the structure n A n B' n ......B i A i B' i ......B2A2B'2, B1A1B'1, B2A2B'2......B i A i B' i ......B n A n B' n 14. A method for preparing a polypropylene composite material according to any one of embodiments 1 to 13, comprising the steps of: sequentially laminating the above-mentioned components in the order of:

[0145] 15. The process according to embodiment 14, comprising the following steps: (1) Polypropylene Composition A i , Polypropylene Composition B i and polypropylene composition B' i A, B i A i B' i co-extrusion, casting or calendering according to the structure and stretching to obtain a polypropylene sheet; (2) Optionally, the polypropylene sheet is split and cut, then woven into B iA i B' i obtaining a structural polypropylene fabric; (3) sequentially laminating and heat pressing polypropylene sheets and / or polypropylene fabrics, then cooling and molding to form a polypropylene composite material.

[0146] 16. Polypropylene composition A in step (1) i comprising melt blending components comprising at least one of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; and / or Polypropylene composition B in step (1) i comprising melt blending components comprising at least one of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; and / or The temperatures of co-extrusion and casting in step (1) are each independently selected from 200 to 240° C.; and / or The temperature of the calendar roller in step (1) is 50 to 70° C.; and / or The stretching temperature in step (1) is 90 to 165°C, preferably 90 to 140°C, more preferably 90 to 119°C; and / or 16. The process according to embodiment 15, wherein the stretching ratio in step (1) is 1-15.

[0147] 17. In step (3): The heat pressing conditions are as follows: a heat pressing temperature of 115 to 170° C., preferably 115 to 159° C., more preferably 140 to 159° C., a heat pressing pressure of 2 to 10 MPa, a preheating time of 5 to 600 s, and a heat pressing time of 1 to 600 s, preferably 10 to 500 s; and / or a pressure for cooling and forming of 2 to 8 MPa, and a cooling time of 30 s to 700 s; and / or The laminated adjacent polypropylene fabrics are oriented at an angle of 0 to 90 degrees relative to each other along their respective warp directions; and / or 16. The method of claim 15, wherein the laminated adjacent polypropylene sheets are oriented at an angle of 0 to 90 degrees relative to each other along their respective machine directions.

[0148] 18. Including a preheating machine, a crawler type continuous flat heat press, a crawler type continuous flat cooling press, a sheet cutting machine and a sheet laminating machine arranged in sequence; Preferably, the continuous hot press molding system for polypropylene composite materials according to any one of embodiments 1 to 13, characterized in that the crawler-type continuous flat hot press includes a preheating unit, an independent heating and pressing unit, an air-cooling unit and a lifting mechanism.

[0149] 19. Use of the polypropylene composite material according to any one of embodiments 1 to 13 and the polypropylene composite material prepared by the preparation method according to any one of embodiments 14 to 17 in the applications of consumer goods, automobile manufacturing, sports protection, and military materials. [Brief description of the drawings]

[0150] [Figure 1] This is a schematic diagram of the layout of the processing equipment used in a preferred embodiment of the present invention. 1 is a preheating machine, 2 is a crawler type continuous flat heat press, 3 is a crawler type continuous flat cooling press, 4 is a sheet cutting machine, and 5 is a sheet laminating machine. The crawler type continuous flat heat press 2 is equipped with a preheating unit 6, an independent heating unit and pressing unit 7, an air cooling unit 8, and a lifting mechanism 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0151] The present invention will be described in detail below with reference to the accompanying drawings and examples. Hereinafter, it should be pointed out that the following examples are for further illustrating the present invention, and should not be understood as limiting the protection scope of the present invention, and that non-essential modifications and adjustments of the present invention made by those skilled in the art still fall within the protection scope of the present disclosure.

[0152] The properties of the polypropylene compositions and sheets were tested according to the following methods and the product test results are shown in Table 1: (1) Melt mass flow rate (MFR): Measured according to the method specified in GB / T 3682-2000. For polypropylene (including polypropylene homopolymer, polypropylene impact copolymer, and polypropylene random copolymer), the test temperature is 230°C and the load is 2.16 kg. For thermal adhesion improvers, the test temperature is 190°C and the load is 2.16 kg. (2) Molecular weight distribution (Mw / Mn): measured according to the method specified in GB / T 36214.1-2018, where Mw is the weight average molecular weight in g / mol and Mn is the number average molecular weight in g / mol. (3) Melting point of material: Measure according to the method specified in GB / T 28724-2012. Sample mass 5 mg, heating from 50°C to 230°C at a heating rate of 10°C / min, holding at 230°C for 3 minutes to remove thermal history, cooling from 230°C to 50°C at a heating rate of 10°C / min, holding at 50°C for 1 minute, and finally heating from 50°C to 230°C at a heating rate of 10°C / min, taking the final heating curve to determine the melting point or melting range of the material. (4) Sheet tensile strength: Measured in accordance with the method specified in GB / T1040.1-2018. (5) Drop impact strength: Measured in accordance with the method specified in GB / T14153-1993. (6) Interlaminar peel strength: Measured according to the method specified in GB / T2358-98.

[0153] In the following examples, the β-nucleating agent of grade VP101B is from Beijing Chemical Research Institute, Sinopec Corporation. The sources of some raw materials are listed in the examples, and the remaining raw materials are commercially available unless otherwise specified.

[0154] Example A1 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0155] (1) Preparation of polypropylene composition A: Component a is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 160°C, a melt flow rate (melt mass flow rate) of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer prepared by SINOPEC Beijing Chemical Research Institute, with an ethylene content of 11wt%, a melting point of 155°C, and an Izod impact strength of 23KJ / m 2 (23°C) and a melt flow rate of 2.0g / 10min. The components prepared above are weighed and mixed in a ratio of 80 parts by weight of component a (Wa) and 20 parts by weight of component b (Wb).

[0156] 0.05 parts by weight of β-nucleating agent of grade VP101B is added. The mixture is then added to a high speed agitator to mix uniformly, and the mixture is added to the feeder of a W&P twin screw extruder, from where it is fed into the twin screw. During processing, the temperature of the screw is maintained at 200-230°C, and the material is melt mixed uniformly through the screw, extruded, pelletized, and dried to obtain pellets of polypropylene composition A, the melting point of which is tested to be 157°C.

[0157] (2) Polypropylene Composition B i Preparation of: Component x1 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 8.9, a melt flow rate of 8.1g / 10min, and a melting point of 130°C; Component x2 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 7.6, a melt flow rate of 8.1g / 10min, and a melting point of 130°C. component x3 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution (Mw / Mn) of 7.3, a melt flow rate of 6.6g / 10min, and a melting point of 140°C; component y is a polyolefin elastomer of grade 6102 purchased from ExxonMobil, which is an ethylene-propylene copolymer.

[0158] The above prepared components are mixed with component x i Mass fraction Wx i and the mass fraction Wy of component y was 15 parts by weight. The other steps were the same as in step (1), and finally polypropylene composition B i pellets (i.e., x i +y=B i , i = 1, 2, 3). When tested, the melting points of B1, B2, and B3 are 127°C, 132°C, and 138°C, respectively.

[0159] (3) Preparation of three-layer coextruded polypropylene sheets: Pellets of polypropylene composition A and polypropylene composition B prepared in the above steps (1) and (2) i After drying the pellets, polypropylene composition A was added to the core layer extruder of a multi-layer extrusion calendar machine, and polypropylene composition B was added to the core layer extruder of a multi-layer extrusion calendar machine. iare added to the upper and lower surface layer extruders of a multi-layer extrusion calendar machine. The pellets are co-extruded and compounded, and then discharged from the die of the extruder, passed through a calendar roller and a take-up roller in sequence, and then subjected to solid-state drawing, edge cutting and rolling to prepare sheets B1AB1, B2AB2 and B3AB3, respectively. Here, the extrusion and casting temperatures are 230°C, and the calendar roller temperature is 58°C. The temperature during solid-state drawing is 140°C, the drawing speed is 2m / min, and the drawing ratio is 7 times.

[0160] The composite film (polypropylene sheet) prepared after stretching and rolling is the top layer (outer layer film B i ), core layer (film A), bottom layer (outer layer film B i The thickness of the composite film is 80 μm, with the thickness of film layer A accounting for 80% of the total thickness of the sheet.

[0161] (4) Preparation of polypropylene fabric: The three-layer coextruded polypropylene sheet prepared in step (3) above is divided and cut into oriented polypropylene ribbons with a width of 3 mm using a multi-blade high-speed dividing and cutting machine. The oriented ribbons are woven using a commercially available weaving machine according to the designed fabric structure to obtain plain woven polypropylene fabrics B1AB1, B2AB2, and B3AB3.

[0162] (5) Preparation of polypropylene composites: The polypropylene fabrics prepared in the above step (4) are laminated in the order of B3A3B3, B2A2B2, B1A1B1, B2A2B2, and B3A3B3 from bottom to top, with a total of 5 laminates, and the laminated polypropylene fabrics are heat pressed and fused, cooled and molded to form a polypropylene composite material. The polypropylene fabrics are arranged at a 90 degree angle to each other along their respective warp directions. The heat pressing conditions adopted are a temperature of 145°C, a heat pressing pressure of 5MPa, a preheating time of 90s, a heat pressing time of 90s, and a cooling time of 300s. The thickness of the prepared polypropylene composite material is 391μm.

[0163] Example A2 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0164] (1) Preparation of polypropylene composition A: Component a is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer prepared by SINOPEC Beijing Chemical Research Institute, with an ethylene content of 8wt%, a melting point of 155°C, a melt flow rate of 3.2g / 10min, and an Izod impact strength of 25KJ / m 2 (23°C). The components prepared above were mixed in a mixture of 70 parts by weight of component a (Wa) and 70 parts by weight of component b (Wb n The materials are weighed and mixed in a ratio of 30 parts by weight. 0.05 parts by weight of β-nucleating agent of grade VP101B is added. The mixture is then added to a high-speed agitator to mix uniformly, and the mixture is added to the feeder of a twin-screw extruder manufactured by W&P, from where it is fed into the twin screws. During processing, the temperature of the screws is maintained at 200-230°C, and the materials are melt-mixed uniformly through the screws, extruded, pelletized and dried, resulting in a pellet of polypropylene composition A, which has a melting point of 161°C according to tests.

[0165] (2) Polypropylene composition B i Preparation of: Component x1 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 8.4, a melting point of 128°C, and a melt flow rate of 7.8g / 10min; Component x2 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 7.6, a melting point of 134°C, and a melt flow rate of 6.9g / 10min; Component x3 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution (Mw / Mn) of 7.1, a melting point of 142°C, and a melt flow rate of 5.2g / 10min; component y is a grade of polyolefin elastomer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene copolymer with an ethylene content of 15wt%, a melting point of 105°C, and a melt flow rate of 9g / 10min under a load of 2.16kg, all of which are prepared by SINOPEC Beijing Chemical Research Institute.

[0166] The above prepared components are mixed with component x i Mass fraction Wx i and the mass fraction Wy of component y was 20 parts by weight. The other steps were the same as in step (1), and finally polypropylene composition B i pellets (i.e., x i +y=B i , i = 1, 2, 3). When tested, the melting points of B1, B2, and B3 are 126°C, 133°C, and 140°C, respectively.

[0167] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0168] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0169] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example A1.

[0170] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0171] Example A3 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0172] (1) Preparation of polypropylene composition A: Same as Example A1, with the mass fraction Wa of component a being 90 parts by weight and the mass fraction Wb of component b being 10 parts by weight. 0.05 parts by weight of β-nucleating agent of grade VP101B is added. Pellets of polypropylene composition A are obtained. When tested, the melting point of the pellets of polypropylene composition A is 158°C.

[0173] (2) Polypropylene composition B i Preparation of: The same as Example A1, with the corresponding component x i Mass fraction Wx i is 90 parts by weight, the mass fraction Wy of component y is 10 parts by weight, and polypropylene composition B i pellets (i.e., x i +y=B i , i = 1, 2, 3) are finally obtained. When tested, the melting points of B1, B2, and B3 are 128°C, 134°C, and 139°C, respectively.

[0174] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0175] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0176] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example A1.

[0177] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0178] Example A4 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0179] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0180] (2) Preparation of Polypropylene Composition B i : The preparation process is the same as step (2) of Example A1.

[0181] (3) Preparation of three-layer coextruded polypropylene sheets: The main steps are the same as in Example A1. The polypropylene sheet has a thickness of 80 μm, and the thickness of the film layer A accounts for 90% of the total thickness of the sheet.

[0182] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0183] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example A1.

[0184] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0185] Example A5 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0186] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0187] (2) Polypropylene composition B i Preparation of: The preparation process is the same as step (2) of Example A1.

[0188] (3) Preparation of three-layer coextruded polypropylene sheets: The main steps are the same as those in Example A1. The polypropylene sheet has a thickness of 80 μm, and the thickness of the film layer A accounts for 70% of the total thickness of the sheet.

[0189] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0190] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example A1.

[0191] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0192] Example A6 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0193] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0194] (2) Polypropylene composition B iPreparation of: The preparation process is the same as step (2) of Example A1.

[0195] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0196] (4) Preparation of polypropylene fabric: The main steps are the same as step (4) of Example A1. The oriented ribbon is woven according to the designed fabric structure using a commercial loom to obtain a satin-woven polypropylene fabric.

[0197] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example A1.

[0198] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0199] Example A7 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0200] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0201] (2) Polypropylene Composition B i Preparation of: The preparation process is the same as step (2) of Example A1.

[0202] (3) Preparation of three-layer coextruded polypropylene sheets: The main preparation process is the same as step (3) of Example A1, where the sheet stretch ratio is 10.

[0203] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0204] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example A1.

[0205] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0206] Example A8 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0207] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0208] (2) Polypropylene Composition B i Preparation of: The preparation process is the same as step (2) of Example A1.

[0209] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0210] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0211] (5) Preparation of polypropylene composites: The main preparation process is the same as step (5) of Example A1, where the polypropylene fabrics are arranged at a 45 degree angle to each other along their respective warp directions.

[0212] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0213] Example A9 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0214] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0215] (2) Polypropylene composition B i Preparation of: The preparation process is the same as step (2) of Example A1.

[0216] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0217] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0218] (5) Preparation of polypropylene composites: The main preparation process is the same as step (5) of Example A1, where the polypropylene fabrics are arranged at a 0 degree angle to each other along their respective warp directions.

[0219] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0220] Example A10 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0221] (1) Preparation of polypropylene composition A: Same as Example A1, except no β-nucleating agent was added to component A.

[0222] (2) Preparation of polypropylene composition Bi: Same as Example A1.

[0223] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0224] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0225] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example A1.

[0226] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0227] Example A11 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0228] (1) Preparation of polypropylene composition A: Component a is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 160°C, a melt flow rate (melt mass flow rate) of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer prepared by SINOPEC Beijing Chemical Research Institute, with an ethylene content of 11wt%, a melting point of 155°C, and an Izod impact strength of 23KJ / m 2 (23°C) and a melt flow rate of 2.0g / 10min. The components prepared above are weighed and mixed in a ratio of 80 parts by weight of component a (Wa) and 20 parts by weight of component b (Wb).

[0229] 0.05 parts by weight of β-nucleating agent of grade VP101B is added. The mixture is then added to a high speed agitator to mix uniformly, and the mixture is added to the feeder of a W&P twin screw extruder, from where it is fed into the twin screw. During processing, the temperature of the screw is maintained at 200-230°C, and the material is melt mixed uniformly through the screw, extruded, pelletized, and dried to obtain pellets of polypropylene composition A, the melting point of which is tested to be 157°C.

[0230] (2) Preparation of polypropylene composition B: Component α is a polyolefin elastomer of grade 6102 purchased from ExxonMobil, an ethylene-propylene copolymer with an ethylene content of 16 wt% (melt flow rate at 190°C, 1.4g / 10min under 2.16kg load); component β1 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, an ethylene-propylene-butene terpolymer with a molecular weight distribution (Mw / Mn) of 8.9, a melt flow rate of 8.1g / 10min, and a melting point of 130°C; component β2 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute. Component β3 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 7.3, a melting point of 6.6g / 10min, and a melting point of 140°C; component γ is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, which is a melting point of 160°C, and an isotacticity of 97%.

[0231] The components prepared above are mixed at a mass fraction of component α W α 45 parts by weight, mass fraction of component β W β 45 parts by weight, W γThe other steps were the same as in step (1), and polypropylene composition B was finally obtained. i pellets (i.e., α + β i +γ=B i , i = 1, 2, 3). When tested, the melting points of B1, B2, and B3 are 129°C, 136°C, and 141°C, respectively.

[0232] (3) Preparation of polypropylene composition C: Component x1 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 8.9, a melt flow rate of 8.1g / 10min, and a melting point of 130°C; Component x2 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 7.6, a melt flow rate of 8.1g / 10min, and a melting point of 130°C. component x3 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 7.3, a melt flow rate of 6.6g / 10min, and a melting point of 140°C; component y is a polyolefin elastomer of grade 6102 purchased from ExxonMobil, which is an ethylene-propylene copolymer.

[0233] The above prepared components are mixed with component x i Mass fraction Wx i and the mass fraction Wy of component y was 15 parts by weight. The other steps were the same as in step (1), and polypropylene composition C was finally obtained. i pellets (i.e., x i +y=C i , i = 1, 2, 3). When tested, the melting points of C1, C2, and C3 are 127°C, 132°C, and 138°C, respectively.

[0234] After drying the pellets of polypropylene composition A, polypropylene composition B and polymer C prepared in the above steps (1), (2) and (3), polypropylene composition A is added to the core layer extruder of a multi-layer extrusion calendar, polypropylene composition B is added to the middle layer extruder of a multi-layer extrusion calendar, and polypropylene composition C is added to the upper and lower surface layer extruders of a multi-layer extrusion calendar. The pellets are co-extruded and compounded, and then discharged from the die of the extruder, and then passed through a calendar roller and a take-up roller in sequence, and then subjected to solid-state stretching, edge cutting and rolling to prepare a sheet. Here, the extrusion and casting temperatures are 230°C, and the calendar roller temperature is 60°C. The temperature during solid-state stretching is 138°C, the stretching speed is 2m / min, and the stretch ratio is 7 times.

[0235] The polypropylene composite sheet (composite film) prepared after stretching and rolling had a top layer (film layer C i ), middle layer (film layer B i ), core layer (film layer A i ), middle layer (film layer B i ), bottom layer (film layer C i The polypropylene composite sheet is 80 μm thick, and the film layer A is i The thickness of film layer B accounts for 80% of the total thickness of the sheet. i The thickness of the film layer C accounts for 10% of the total thickness of the sheet. i The thickness of this layer accounts for 10% of the total thickness of the sheet.

[0236] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example A1.

[0237] (6) Preparation of polypropylene composites: The preparation process is the same as step (6) of Example A1.

[0238] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0239] Example A12 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0240] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0241] (2) Preparation of polypropylene composition B: The main preparation process is the same as step (2) of Example A1. However, component B i Materials and x i selects: Component x1 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 110°C; Component x2 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 115°C; Component x3 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 120°C; Component x4 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 125°C; Component x5 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 130°C. Component x6 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer and has a melting point of 135°C; Component x7 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer and has a melting point of 140°C; Component x8 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer and has a melting point of 145°C; Component x9 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer and has a melting point of 150°C; Wherein, the molecular weight distributions Mw / Mn of components x1 to x9 are all between 7 to 10, and the melt flow rates of components x1 to x9 are all between 1 to 20g / 10min.

[0242] Polypropylene composition B i pellets (i.e., x i +y=B i, i=1, 2, 3, 4, 5, 6, 7, 8, 9) are finally obtained. When tested, the melting points of B1 are 110°C, B2 are 113°C, B3 are 117°C, B4 are 123°C, B5 are 127°C, B6 are 133°C, B7 are 137°C, B8 are 142°C, and B9 are 148°C.

[0243] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0244] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0245] (5) Preparation of polypropylene composites: The polypropylene fabrics prepared in step (4) above are laminated in the order of B9A9B9...B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3, ...B9A9B9 from bottom to top, with a total number of laminates being 17. The laminated polypropylene fabrics are heat pressed and fused, cooled and molded to form a polypropylene composite material. The polypropylene fabrics are arranged at a 90 degree angle to each other along their respective warp directions. The heat pressing conditions are: temperature 150°C, heat pressing pressure 5MPa, preheating time 300s, heat pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.24mm.

[0246] Example A13 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0247] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0248] (2) Preparation of polypropylene composition B: The main preparation process is the same as step (2) of Example A1. However, component B i Materials and x i selects: Components x1-x3 are polypropylene random copolymers prepared by SINOPEC Beijing Chemical Research Institute, which are ethylene-propylene-butene terpolymers, with a melting point of 110°C; components x4-x6 are polypropylene random copolymers prepared by SINOPEC Beijing Chemical Research Institute, which are ethylene-propylene-butene terpolymers, with a melting point of 130°C; components x7-x9 are polypropylene random copolymers prepared by SINOPEC Beijing Chemical Research Institute, which are ethylene-propylene-butene terpolymers, with a melting point of 150°C; where, the molecular weight distributions Mw / Mn of components x1-x9 are all between 7-10, and the melt flow rates of components x1-x9 are all between 1-20g / 10min.

[0249] Polypropylene composition B i pellets (i.e., x i +y=B i , i=1, 2, 3, 4, 5, 6, 7, 8, 9...27) are finally obtained. When tested, the melting points of B1 to B3 are 110°C, those of B4 to B6 are 127°C, and those of B7 to B9 are 148°C.

[0250] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0251] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0252] (5) Preparation of polypropylene composites: The polypropylene fabrics prepared in the above step (4) are sequentially laminated in the order of B9A9B9...B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3, ...B9A9B9 from bottom to top, with a total number of laminates being 17. The laminated polypropylene fabrics are heat pressed and fused, cooled and molded to form a polypropylene composite material. The polypropylene fabrics are arranged at a 90 degree angle to each other along their respective warp directions. The heat pressing conditions are: temperature 150°C, heat pressing pressure 5MPa, preheating time 300s, heat pressing time 180s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.24mm.

[0253] Example A14 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0254] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0255] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example A1.

[0256] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0257] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0258] (5) Preparation of polypropylene composites: The main steps are the same as those in Example A1. However, the heat pressing conditions are changed to a temperature of 150°C, a heat pressing pressure of 8MPa, a preheating time of 180s, a heat pressing time of 180s, and a cooling time of 700s. The thickness of the prepared polypropylene composite material is 387μm.

[0259] Example A15 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0260] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0261] (2) Preparation of polypropylene composition B: The main preparation process is the same as step (2) of Example A1, except that component B i Materials and x i selects: Component x1 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 110°C; component x2 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 130°C; component x3 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 150°C; where, the molecular weight distributions Mw / Mn of components x1 to x3 are all between 7 to 10, and the melt flow rates of components x1 to x3 are all between 1 to 20g / 10min.

[0262] Polypropylene composition B i pellets (i.e., x i +y=B i , i = 1, 2, 3) are finally obtained. When tested, the melting points of B1, B2, and B3 are 110°C, 128°C, and 147°C, respectively.

[0263] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0264] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0265] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example A1.

[0266] The thickness of the prepared polypropylene composite material is the same as in Example A1.

[0267] Example A16 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0268] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0269] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example A1.

[0270] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0271] (4) Preparation of polypropylene composites: Instead of preparing a polypropylene fabric, the three-layer coextruded polypropylene sheet obtained in step (3) (replacing the polypropylene fabric obtained in step (4) of Example A1) is subjected to sequential lamination and heat pressing according to step (5) of Example A1.

[0272] The thickness of the resulting polypropylene composite material is similar to that of Example A1.

[0273] Example A17 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0274] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example A1.

[0275] (2) Preparation of polypropylene composition B: The main preparation process is the same as step (2) of Example A1. However, component B i Materials and x i selects: Components x1-x3 are polypropylene random copolymers prepared by SINOPEC Beijing Chemical Research Institute, which are ethylene-propylene-butene terpolymers, with a melting point of 110°C; components x4-x6 are polypropylene random copolymers prepared by SINOPEC Beijing Chemical Research Institute, which are ethylene-propylene-butene terpolymers, with a melting point of 115°C; components x7-x9 are polypropylene random copolymers prepared by SINOPEC Beijing Chemical Research Institute, which are ethylene-propylene-butene terpolymers, with a melting point of 120°C; components x 10 ~x 12 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a melting point of 125°C; component x 13 ~x 15 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a melting point of 130°C; component x 16 ~x 18is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a melting point of 135°C; component x 19 ~x 21 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a melting point of 140°C; component x 22 ~x 24 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a melting point of 145°C; component x 25 ~x 27 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a melting point of 150°C; where the components x1-x 27 The molecular weight distribution Mw / Mn of each is between 7 and 10, and the components x1 to x 27 The melt flow rates of all are between 1 and 20 g / 10 min.

[0276] Polypropylene composition B i pellets (i.e., x i +y=B i , i=1, 2, 3, 4, 5, 6, 7, 8, 9...27) are finally obtained. When tested, the melting points of B1 to B3 were 110°C, B4 to B6 were 113°C, B7 to B9 were 117°C, and B 10 ~B 12 The melting point of is 123℃, B 13 ~B 15 The melting point of is 127℃, B 16 ~B 18 The melting point of is 133℃, B 19 ~B 21 The melting point of is 137℃, B 22 ~B 24 The melting point of is 142℃, B 25 ~B 27 The melting point of is 148°C.

[0277] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example A1.

[0278] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example A1.

[0279] (5) Preparation of polypropylene composites: The polypropylene fabric prepared in the above step (4) is placed on the bottom and top of the 27 A 27 B 27 ...B9A9B9...B3A3B3, B2A2B2, B1A1B1, B2A2B2, B3A3B3, ...B9A9B9...B 27 A 27 B 27 The polypropylene fabrics are laminated in the order of 150°C, with a total of 53 laminates. The laminated polypropylene fabrics are heat pressed and fused, then cooled and molded to form a polypropylene composite. The polypropylene fabrics are arranged at a 90° angle to each other along their respective warp directions. The heat pressing conditions are: temperature 150°C, heat pressing pressure 5MPa, preheating time 500s, heat pressing time 360s, and cooling time 800s. The thickness of the prepared polypropylene composite is 3.92mm.

[0280] Example A18 A coextruded polypropylene sheet is prepared according to the method of Example A1, except that the material of component Bi is selected as follows: component x1 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 4.2 and a melting point of 142°C; component x2 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 4.7 and a melting point of 138°C; component x3 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 5.4 and a melting point of 133°C; the melt flow rates of components x1-x3 are all 2-10g / 10min.

[0281] Polypropylene composition B i pellets (i.e., x i +y=B i , i = 1, 2, 3) are finally obtained. When tested, the melting points of B1, B2, and B3 are 139°C, 134°C, and 129°C, respectively.

[0282] Comparative Example A1 A coextruded polypropylene sheet is prepared according to the method of Example A1, except that the materials of component Bi are selected as follows: component x1 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 140°C; component x2 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 135°C; component x3 is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, and has a melting point of 130°C; the molecular weight distribution Mw / Mn of components x1-x3 are all 7-10, and the melt flow rate of components x1-x3 are all 2-10g / 10min.

[0283] Polypropylene composition B i pellets (i.e., x i +y=B i , i = 1, 2, 3) are finally obtained. When tested, the melting points of B1, B2, and B3 are 138°C, 132°C, and 127°C, respectively.

[0284] Comparative example A2 Polypropylene composition B i A three-layer coextruded polypropylene sheet is prepared according to the method of Example A1, except that contains only component y.

[0285] Polypropylene fabrics and polypropylene composites are prepared according to the method of Example A1.

[0286] Comparative example A3 A three-layer coextruded polypropylene sheet is prepared according to the method of Example A1, except that the thickness of film layer A accounts for 95% of the total thickness of the sheet. Polypropylene fabrics and polypropylene composites are prepared according to the method of Example A1.

[0287] Comparative example A4 A three-layer coextruded polypropylene sheet is prepared according to the method of Example A1, except that the thickness of film layer A accounts for 50% of the total thickness of the sheet. Polypropylene fabrics and polypropylene composites are prepared according to the method of Example A1.

[0288] Comparative Example A5 Component B i A coextruded polypropylene sheet (17 layers) is prepared according to the method of Example A12, except that the materials are selected as follows: components x1 to x9 are all polypropylene random copolymers prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 110°C; the molecular weight distributions Mw / Mn of components x1 to x9 are all between 7 and 10, and the melt flow rates of components x1 to x9 are all between 2 and 10g / 10min.

[0289] Finally, polypropylene composition B i The pellets obtained were B i The melting point of is 110°C.

[0290] The adopted heat pressing conditions are temperature 150 °C, heat pressing pressure 5 MPa, preheating time 300 s, heat pressing time 180 s, and cooling time 600 s. The thickness of the prepared polypropylene composite material is 1.24 mm.

[0291] Comparative example A6 A coextruded polypropylene sheet (17 layers) is prepared according to the method of Example A12, except that the materials of component Bi are selected as follows: components x1 to x9 are all polypropylene random copolymers prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 130°C; the molecular weight distributions Mw / Mn of components x1 to x9 are all between 7 and 10, and the melt flow rates of components x1 to x9 are all between 2 and 10 g / 10 min.

[0292] Finally, polypropylene composition B i The pellets obtained were B i The melting point of is 127°C.

[0293] The adopted heat pressing conditions are temperature 150 °C, heat pressing pressure 5 MPa, preheating time 300 s, heat pressing time 180 s, and cooling time 600 s. The thickness of the prepared polypropylene composite material is 1.24 mm.

[0294] Comparative example A7 A coextruded polypropylene sheet (17 layers) is prepared according to the method of Example A12, except that the materials of component Bi are selected as follows: components x1 to x9 are all polypropylene random copolymers prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 150°C; the molecular weight distributions Mw / Mn of components x1 to x9 are all between 7 and 10, and the melt flow rates of components x1 to x9 are all between 2 and 10 g / 10 min.

[0295] Finally, polypropylene composition B i The pellets obtained were B i The melting point of is 148°C.

[0296] The adopted heat pressing conditions are temperature 150 °C, heat pressing pressure 5 MPa, preheating time 300 s, heat pressing time 180 s, and cooling time 600 s. The thickness of the prepared polypropylene composite material is 1.24 mm.

[0297] Experimental Example The polypropylene composite materials obtained in the above examples and comparative examples were tested according to the following methods, and the results are shown in Table 1: (1) Sheet tensile strength: measured according to the method specified in GB / T1040.1-2018; (2) Drop impact strength: measured according to the method specified in GB / T14153-1993; (3) Interlaminar peel strength: Measured according to the method specified in GB / T2358-98. The thicknesses of the polypropylene composite materials obtained in Examples A1-9, 12, and 13 and Comparative Examples A1-4 were all close to about 390 μm, and in the range of 390 μm±10 μm.

[0298] [Table 1]

[0299] As can be seen from the results of the examples in Table 1, the polypropylene composite material having a melting point gradient structure prepared according to the present invention has good tensile properties and impact properties, and at the same time, has good interlayer peel strength even at lower heat press temperatures.

[0300] The polypropylene composite material with melting point gradient structure described in the present invention has a machine direction (MD) tensile strength of 160 MPa or more, an interlayer peel strength of 1.3 N / mm or more, and a drop impact strength of 42 J or more when the composite material is obtained by hot pressing and fusing only five layers of polypropylene fabric and has a thickness of only about 390 μm.

[0301] As can be seen from the preferred examples A1 to A3, the polypropylene composite material with melting point gradient structure prepared in the present invention has a tensile strength in the machine direction (MD) of 180 MPa or more, an interlayer peel strength of 1.5 N / mm or more, and a drop impact strength of 45 J or more when the composite material obtained by hot pressing and fusing only five layers of polypropylene fabric has a thickness of only about 390 μm.

[0302] As can be seen from Comparative Examples A1-8, polypropylene composites prepared by schemes outside the scope of the present invention result in poor performance of the laminated polypropylene sheets or fabrics, resulting in significant reductions in the tensile strength, impact properties or interlayer delamination strength of the resulting polypropylene composites.

[0303] Specifically, as can be seen from the comparison of Comparative Examples A5 to 7 and Example A12, the tensile strength, impact properties and interlayer peel strength of the polypropylene composite material having the melting point gradient structure of the present invention are higher than those of the conventional polypropylene composite material not having a melting point gradient structure. The polypropylene composite material having the melting point gradient structure of the present invention requires a shorter heat press time or a lower heat press temperature for processing compared to the conventional polypropylene composite material not having a melting point gradient structure. The reduction in heat press time or heat press temperature can reduce damage to mechanical properties caused by the disorder of molecular chain orientation, and it is believed that the reduction in heat press time or heat press temperature can achieve the beneficial effects of reducing costs and improving efficiency.

[0304] Example B1 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0305] (1) Preparation of polypropylene composition A: Component a is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 160°C, a melt flow rate (melt mass flow rate) of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer prepared by SINOPEC Beijing Chemical Research Institute (test conditions: 23°C, Izod impact strength: 23KJ / m 2 ), the ethylene content is 11% by weight, the melt flow rate is 2.0 g / 10 min, and the melting point is 155°C.

[0306] The components prepared above are weighed and mixed in a ratio of 80 parts by weight of the mass fraction Wa of component a and 20 parts by weight of the mass fraction Wb of component b. 0.05 parts by weight of β-nucleating agent of grade VP101B is added. Then, the mixture is added to a high-speed agitator to mix uniformly, and the mixture is added to the feeder of a twin-screw extruder manufactured by W&P, from which it is fed into the twin-screw. During the process, the temperature of the screw is maintained at 200-230°C, and the material is uniformly melt mixed through the screw, extruded, pelletized, and dried to obtain a polypropylene composition pellet, and the melt mass flow rate is 4.6g / 10min according to the test; the melting point of polypropylene composition A is 157°C.

[0307] (2) Preparation of polypropylene composition B: Component x is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution (Mw / Mn) of 7.3, a melting point of 140°C, and a melt flow rate of 6.6g / 10min; component y is a polyolefin elastomer of grade 6102 purchased from ExxonMobil, which is an ethylene-propylene copolymer with an ethylene content of 16 wt%, a melt flow rate of 1.4g / 10min at 190°C and a load of 2.16kg; The components prepared above were weighed and mixed in a ratio of 85 parts by weight of component x (Wx) and 15 parts by weight of component y (Wy), and the other steps were the same as in step (1). Finally, pellets of polypropylene composition B were obtained, and the melt mass flow rate of the pellets was 5.2 g / 10 min, and the melting point was 138°C according to a test.

[0308] (3) Preparation of three-layer coextruded polypropylene sheets: After drying the pellets of polypropylene composition A and polypropylene composition B prepared in the above steps (1) and (2), polypropylene composition A is added to a core layer extruder of a multi-layer extrusion calendar machine, and polypropylene composition B is added to the upper and lower surface layer extruders of the multi-layer extrusion calendar machine.

[0309] The pellets are coextruded and compounded, and after exiting the extruder die, are passed sequentially through calendar rollers, take-up rollers, and then subjected to solid state drawing, edge cutting and rolling to prepare a sheet.

[0310] Here, the extrusion and casting temperature is 230° C., and the calendar roller temperature is 55° C. The polypropylene sheet (composite film) prepared after stretching and rolling is composed of an upper layer (film layer B), a core layer (film layer A), and a lower layer (film layer B).

[0311] The polypropylene sheet (composite film) had a thickness of 80 μm, with the thickness of film layer A accounting for 80% of the total thickness of the sheet.

[0312] (4) Preparation of polypropylene fabric: The three-layer coextruded polypropylene sheet prepared in (3) above is divided and cut into oriented polypropylene ribbons with a width of 3 mm using a multi-blade high-speed dividing and cutting machine. The oriented ribbons are woven according to the designed fabric structure using a commercially available weaving machine to obtain a plain woven polypropylene fabric.

[0313] (5) Preparation of polypropylene composites: The polypropylene fabrics prepared in step (4) above are sequentially laminated and heat pressed to prepare a laminated polypropylene sheet. The laminated polypropylene sheet includes 24 layers of polypropylene fabric, which are arranged at a 90 degree angle to each other along their respective warp directions. The heat press conditions are: temperature 150°C, heat press pressure 5MPa, preheat time 180s, heat press time 180s, and cooling time 600s. The thickness of the prepared polypropylene composite material is 1.67mm.

[0314] Example B2 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0315] (1) Preparation of polypropylene composition A: Component a is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 165℃, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer prepared by SINOPEC Beijing Chemical Research Institute under test conditions of 23℃, with an Izod impact strength of 25KJ / m 2 The ethylene content is 8% by weight, the melt flow rate is 3.2 g / 10 min, and the melting point is 155°C.

[0316] The components prepared above are weighed and mixed in a ratio of 70 parts by weight of the mass fraction Wa of component a and 30 parts by weight of the mass fraction Wb of component b. 0.05 parts by weight of β-nucleating agent of grade VP101B is added. The mixture is then added to a high-speed agitator to mix uniformly, and the mixture is added to the feeder of a twin-screw extruder manufactured by W&P, from which it is fed into the twin-screw. During the process, the temperature of the screw is maintained at 200-230°C, and the material is uniformly melt mixed through the screw, extruded, pelletized, and dried to obtain a polypropylene composition pellet, the melt mass flow rate is 7.3g / 10min according to the test, and the melting point of polypropylene composition A is 161°C.

[0317] (2) Preparation of polypropylene composition B: Component x is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a melting point of 134°C, a molecular weight distribution (Mw / Mn) of 7.6, and a melt flow rate of 5.2g / 10min; component y is a grade of polyolefin elastomer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene copolymer with an ethylene content of 15% by weight, a melting point of 105°C, 190°C, and a melt flow rate of 9g / 10min at a load of 2.16kg according to tests; The components prepared above are weighed and mixed in a ratio of 80 parts by weight of component x (Wx) and 20 parts by weight of component y (Wy), and the other steps are weight-mixed in the same ratio as in step (1). Finally, pellets of polypropylene composition B are obtained, and the melt mass flow rate is 9.6 g / 10 min according to the test. The melting point of polypropylene composition B is 130°C.

[0318] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example B1.

[0319] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0320] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example B1.

[0321] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0322] Example B3 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0323] (1) Preparation of polypropylene composition A: The mass fraction Wa of component a is 90 parts by weight, and the mass fraction Wb of component b is 10 parts by weight. 0.05 parts by weight of β-nucleating agent of grade VP101B is added. Pellets of polypropylene composition A are obtained, and the melt mass flow rate is 6.8 g / 10 min according to the test, and the melting point of polypropylene composition A is 158 ° C.

[0324] (2) Preparation of polypropylene composition B: The mass fraction Wx of component x was 90 parts by weight, and the mass fraction Wy of component y was 10 parts by weight, which is the same as in Example B1. Finally, pellets of polypropylene composition B were obtained, and the melt mass flow rate was tested to be 8.7 g / 10 min, and the melting point of polypropylene composition B was 139°C.

[0325] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example B1.

[0326] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0327] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example B1.

[0328] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0329] Example B4 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0330] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0331] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0332] (3) Preparation of three-layer coextruded polypropylene sheets: The main steps are the same as those in Example B1. The thickness of the polypropylene sheet is 80 μm, and the thickness of the film layer A accounts for 90% of the total thickness of the sheet.

[0333] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0334] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example B1.

[0335] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0336] Example B5 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0337] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0338] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0339] (3) Preparation of three-layer coextruded polypropylene sheets: The main steps are the same as those in Example B1. The thickness of the polypropylene sheet is 80 μm, and the thickness of the film layer A accounts for 70% of the total thickness of the sheet.

[0340] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0341] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example B1.

[0342] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0343] Example B6 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0344] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0345] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0346] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example B1.

[0347] (4) Preparation of polypropylene fabric: The main steps are the same as step (4) of Example B1. The oriented ribbon is woven according to the designed fabric structure using a commercial loom to obtain a satin-woven polypropylene fabric.

[0348] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example B1.

[0349] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0350] Example B7 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0351] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0352] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0353] (3) Preparation of three-layer coextruded polypropylene sheets: The main preparation process is the same as step (3) of Example B1, where the stretching ratio of the sheet is 10.

[0354] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0355] (5) Preparation of polypropylene composites: The preparation process is the same as step (5) of Example B1.

[0356] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0357] Example B8 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0358] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0359] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0360] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example B1.

[0361] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0362] (5) Preparation of polypropylene composites: The main preparation process is the same as step (5) of Example B1, where the polypropylene fabrics are arranged at a 45 degree angle to each other along their respective warp directions.

[0363] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0364] Example B9 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0365] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0366] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0367] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example B1.

[0368] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0369] (5) Preparation of polypropylene composites: The main preparation process is the same as step (5) of Example B1, where the polypropylene fabrics are arranged at a 0 degree angle to each other along their respective warp directions.

[0370] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0371] Example B10 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0372] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0373] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0374] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example B1.

[0375] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0376] (5) Preparation of polypropylene composites: The main process is the same as in Example B1. The laminated polypropylene sheet contains two layers of polypropylene fabric. The heat press conditions adopted are: temperature 140°C, heat press pressure 2MPa, preheat time 120s, heat press time 10s, and cooling time 300s. The thickness of the prepared polypropylene composite material is 128μm.

[0377] Example B11 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0378] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0379] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0380] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example B1.

[0381] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0382] (5) Preparation of polypropylene composites: The main process is the same as in Example B1. The laminated polypropylene sheet contains 100 layers of polypropylene fabric. The heat press conditions adopted are 159°C, heat press pressure 10MPa, preheat time 300s, heat press time 300s, and cooling time 700s. The thickness of the prepared polypropylene composite material is 7.23mm.

[0383] Example B12 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0384] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0385] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0386] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example B1.

[0387] (4) Preparation of polypropylene fabric: The preparation process is the same as step (4) of Example B1.

[0388] (5) Preparation of polypropylene composites: The main steps are the same as those in Example B1: temperature 155°C, heat press pressure 8MPa, preheat time 300s, heat press time 300s, cooling time 700s. The thickness of the prepared polypropylene composite material is 1.58mm.

[0389] Example B13 This example is used to illustrate the preparation of the polypropylene composition, three-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0390] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B1.

[0391] (2) Preparation of polypropylene composition B: The preparation process is the same as step (2) of Example B1.

[0392] (3) Preparation of three-layer coextruded polypropylene sheets: The preparation process is the same as step (3) of Example B1.

[0393] (4) Preparation of polypropylene composites: Instead of preparing polypropylene fabric, the three-layer coextruded polypropylene sheet obtained in step (3) (instead of the polypropylene fabric obtained in step (4) of Example B1) was subjected to sequential lamination and heat pressing according to step (5) of Example B1. The thickness of the prepared polypropylene composite material is 1.51 mm.

[0394] Example B14 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0395] (1) Preparation of polypropylene composition A: Component a is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 160°C, a melt flow rate (melt mass flow rate) of 3.2g / 10min, a melting point of 160°C, and an isotacticity of 97%; component b is a polypropylene impact copolymer prepared by SINOPEC Beijing Chemical Research Institute (test conditions: 23°C, Izod impact strength: 23KJ / m 2 ), the ethylene content is 11% by weight, the melt flow rate is 2.0 g / 10 min, and the melting point is 155°C.

[0396] The components prepared above are mixed at a mass fraction of component a, W a 80 parts by weight, mass fraction of component b W bThe mixture is weighed and mixed in a ratio of 20 parts by weight. 0.05 parts by weight of β-nucleating agent of grade VP101B is added. The mixture is then added to a high-speed agitator to mix uniformly, and the mixture is added to the feeder of a twin-screw extruder manufactured by W&P, from which it is fed into the twin screws. During processing, the temperature of the screw is maintained at 200-230°C, and the material is uniformly melt mixed through the screw, extruded, pelletized, and dried to obtain a polypropylene composition pellet, the melt mass flow rate of which is 4.6g / 10min according to the test; the melting point of polypropylene composition A is 157°C.

[0397] (2) Preparation of polypropylene composition C: Component α is a grade 6102 polyolefin elastomer purchased from ExxonMobil, which is an ethylene-propylene copolymer with an ethylene content of 16 wt% (melt flow rate of 1.4 g / 10 min at 190°C and 2.16 kg load); component β is a grade polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution (Mw / Mn) of 7.3, a melting point of 140°C, and a melt flow rate of 6.6 g / 10 min; component γ is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, which has a melt flow rate of 3.2 g / 10 min, a melting point of 160°C, and an isotacticity of 97%. Here, the mass fraction W of component α is α is 45 parts by weight, and the mass fraction of component β W β is 45 parts by weight, W γ is 10 parts by weight, and then the mixture is added to a high-speed agitator to mix uniformly, and the mixture is added to the feeder of a twin-screw extruder manufactured by W&P, from which it is fed into the twin-screw. During processing, the temperature of the screw is maintained at 200-230°C, and the material is uniformly melt mixed through the screw, extruded, pelletized, and dried to obtain polypropylene composition pellet C, the melt mass flow rate of which is tested to be 6.9g / 10min, and the melting point of polypropylene composition C is 145°C.

[0398] (3) Preparation of polypropylene composition B: Component x is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution (Mw / Mn) of 7.3, a melting point of 140°C, and a melt flow rate of 6.6g / 10min; component y is a polyolefin elastomer of grade 6102 purchased from ExxonMobil, which is an ethylene-propylene copolymer with an ethylene content of 16 wt% (melt flow rate of 1.4g / 10min at 190°C and a load of 2.16 kg).

[0399] The components prepared above are mixed at mass fraction W of component x. x 85 parts by weight, mass fraction of component y W y The other steps are the same as those in step (1). Finally, pellets of polypropylene composition B are obtained, and the melt mass flow rate is 5.2 g / 10 min according to the test; the melting point of polypropylene composition B is 138 ° C.

[0400] (4) Preparation of 5-layer coextruded polypropylene composite sheets: After drying the pellets of polypropylene composition A, polypropylene composition C and polymer B prepared in (1) and (2) above, polypropylene composition A is added to the core layer extruder of a multi-layer extrusion calendar, polypropylene composition C is added to the middle layer extruder of a multi-layer extrusion calendar, and polypropylene composition B is added to the upper and lower surface layer extruders of a multi-layer extrusion calendar. The pellets are co-extruded and compounded, and then discharged from the die of the extruder, and passed through a calendar roller and a take-up roller in sequence, and then subjected to solid-state stretching, edge cutting and rolling to prepare the sheet described above. Here, the extrusion and casting temperatures are 230°C, and the calendar roller temperature is 60°C. The temperature during solid-state stretching is 138°C, the stretching speed is 2m / min, and the stretch ratio is 7 times.

[0401] The polypropylene composite sheet (composite film) prepared after stretching and rolling is composed of an upper layer (film layer B), an intermediate layer (film layer C), a core layer (film layer A), an intermediate layer (film layer C), and a lower layer (film layer B). The thickness of the polypropylene composite sheet is 80 μm, with the thickness of film layer A accounting for 80% of the total thickness of the sheet, the thickness of film layer C accounting for 10% of the total thickness of the sheet, and the thickness of film layer B accounting for 10% of the total thickness of the sheet.

[0402] (5) Preparation of polypropylene fabric: The five-layer coextruded polypropylene composite sheet prepared in (4) above is divided into oriented polypropylene ribbons with a width of 3 mm using a multi-blade high-speed dividing cutter. The oriented ribbons are woven according to the designed fabric structure using a commercial weaving machine to obtain a plain woven polypropylene fabric.

[0403] (6) Preparation of polypropylene composites: The polypropylene fabrics prepared in step (5) above are sequentially laminated and heat pressed to prepare a laminated polypropylene composite sheet. The laminated polypropylene composite sheet is composed of 24 layers of polypropylene fabric, and the polypropylene fabrics are arranged at a 90 degree angle to each other along their respective warp directions. The heat pressing conditions are: temperature 153°C, heat pressing pressure 5MPa, preheating time 300s, heat pressing time 180s, and cooling time 600s.

[0404] The thickness of the prepared polypropylene composite is 1.82 mm.

[0405] Example B15 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0406] (1) Preparation of polypropylene composition A: Component a is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 165℃, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer prepared by SINOPEC Beijing Chemical Research Institute under test conditions of 23℃, with an Izod impact strength of 25KJ / m 2 The ethylene content is 8% by weight, the melt flow rate is 3.2 g / 10 min, and the melting point is 155°C. The components prepared above are mixed with each other at a mass fraction of component a of W a 70 parts by weight, mass fraction of component b W b The materials are weighed and mixed in a ratio of 30 parts by weight. 0.05 parts by weight of β-nucleating agent of grade VP101B is added. The mixture is then added to a high-speed agitator to mix uniformly, and the mixture is added to the feeder of a twin-screw extruder manufactured by W&P, from which it is fed into the twin screws. During processing, the temperature of the screw is maintained at 200-230°C, and the materials are uniformly melt mixed through the screw, extruded, pelletized, and dried to obtain a polypropylene composition pellet, with a melt mass flow rate of 7.3 g / 10 min according to testing. The melting point of polypropylene composition A is 161°C.

[0407] (2) Preparation of polypropylene composition C: Component α is a grade polyolefin elastomer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene copolymer with an ethylene content of 15 wt%, a melting point of 105°C, (melt flow rate at 190°C, 2.16 kg load 9g / 10min); component β is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution (Mw / Mn) of 7.6, a melting point of 134°C, and a melt flow rate of 5.2g / 10min; component γ is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, which has a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%. Here, the mass fraction W of component α is α is 55 parts by weight, and the mass fraction of component β W β is 40 parts by weight, Wγ is 5 parts by weight, and then the mixture is added to a high-speed agitator to mix uniformly, and the mixture is added to the feeder of a twin-screw extruder manufactured by W&P, from which it is fed into the twin-screw. During processing, the temperature of the screw is maintained at 200-230°C, and the material is uniformly melt mixed through the screw, extruded, pelletized, and dried to obtain polypropylene composition pellet C, the melt mass flow rate of which is tested to be 7.8g / 10min, and the melting point of polypropylene composition C is 156°C.

[0408] (3) Preparation of polypropylene composition B: Component x is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution (Mw / Mn) of 7.6, a melting point of 134°C, and a melt flow rate of 5.2g / 10min; component y of component α is a grade of polyolefin elastomer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene copolymer with an ethylene content of 15 wt%, a melting point of 105°C, (melt flow rate of 9g / 10min at 190°C and a load of 2.16 kg). The components prepared above are divided into 1000 and 15000 parts by mass fraction W of component x. x 80 parts by weight, mass fraction of component y W y The other steps are the same as those in step (1). Finally, pellets of polypropylene composition B are obtained. The melt mass flow rate of the pellets is 9.6 g / 10 min according to a test, and the melting point of polypropylene composition B is 130°C.

[0409] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The preparation process is the same as step (4) of Example B14.

[0410] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0411] (6) Preparation of polypropylene composites: The preparation process is the same as step (6) of Example B14.

[0412] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0413] Example B16 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0414] (1) Preparation of polypropylene composition A: Same as in Example B1, but with the mass fraction Wa of component a being 90 parts by weight and the mass fraction Wb of component b being 10 parts by weight. 0.05 parts by weight of β-nucleating agent of grade VP101B are added. Pellets of polypropylene composition A are obtained. Its melt mass flow rate, as tested, is 6.8 g / 10 min. The melting point of polypropylene composition A is 158 ° C.

[0415] (2) Preparation of polypropylene composition C: The same as in Example B1, but with the mass fraction W of component α α 35 parts by weight, mass fraction of component β W β 55 parts by weight, W γ Finally, pellets of polypropylene composition C are obtained, and the melt mass flow rate is 7.3 g / 10 min according to the test, and the melting point of polypropylene composition C is 142°C.

[0416] (3) Preparation of polypropylene composition B: The same as Example B1, except that the mass fraction Wx of component x is 90 parts by weight, and the mass fraction Wy of component y is 10 parts by weight. Finally, pellets of polypropylene composition B are obtained, and the melt mass flow rate is 8.7 g / 10 min according to the test, and the melting point of polypropylene composition B is 139 ° C.

[0417] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The preparation process is the same as step (4) of Example B14.

[0418] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0419] (6) Preparation of polypropylene composites: The preparation process is the same as step (6) of Example B14.

[0420] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0421] Example B17 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0422] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0423] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0424] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0425] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The main steps are the same as in Example B14, with the thickness of film layer A accounting for 90% of the total thickness of the sheet, the thickness of film C accounting for 5% of the total thickness of the sheet, and the thickness of film B accounting for 5% of the total thickness of the sheet.

[0426] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0427] (6) Preparation of polypropylene composites: The preparation process is the same as step (6) of Example B14.

[0428] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0429] Example B18 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0430] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0431] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0432] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0433] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The main steps are the same as in Example B14. The thickness of the polypropylene composite sheet is 80 μm, the thickness of film layer A accounts for 70% of the total thickness of the sheet, the thickness of film C accounts for 15% of the total thickness of the sheet, and the thickness of film B accounts for 15% of the total thickness of the sheet.

[0434] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0435] (6) Preparation of polypropylene composites: The preparation process is the same as step (6) of Example B14.

[0436] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0437] Example B19 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0438] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0439] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0440] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0441] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The preparation process is the same as step (4) of Example B14.

[0442] (5) Preparation of polypropylene fabric: The main steps are the same as step (5) of Example B14. The oriented ribbon is woven according to the designed fabric structure using a commercial loom to obtain a satin-woven polypropylene fabric.

[0443] (6) Preparation of polypropylene composites: The preparation process is the same as step (6) of Example B14.

[0444] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0445] Example B20 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0446] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0447] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0448] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0449] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The main preparation process is the same as step (4) of Example B14, where the stretching ratio of the sheet is 10.

[0450] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0451] (6) Preparation of polypropylene composites: The preparation process is the same as step (6) of Example B14.

[0452] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0453] Example B21 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0454] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0455] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0456] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0457] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The preparation process is the same as step (4) of Example B14.

[0458] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0459] (6) Preparation of polypropylene composites: The main preparation process is the same as step (6) of Example B14, where the polypropylene fabrics are arranged at a 45 degree angle to each other along their respective warp directions.

[0460] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0461] Example B22 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0462] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0463] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0464] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0465] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The preparation process is the same as step (4) of Example B14.

[0466] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0467] (6) Preparation of polypropylene composites: The main preparation process is the same as step (6) of Example B14, where the polypropylene fabrics are arranged at a 0 degree angle to each other along their respective warp directions.

[0468] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0469] Example B23 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0470] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0471] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0472] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0473] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The preparation process is the same as step (4) of Example B14.

[0474] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0475] (6) Preparation of polypropylene composites: The main preparation process is the same as step (6) of Example B14. The laminated polypropylene composite sheet contains two layers of polypropylene fabric. The heat press conditions adopted are temperature 145°C, heat press pressure 2MPa, preheat time 150s, heat press time 60s, and cooling time 300s. The thickness of the prepared polypropylene composite is 136μm.

[0476] Example B24 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0477] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0478] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0479] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0480] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The preparation process is the same as step (4) of Example B14.

[0481] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0482] (6) Preparation of polypropylene composites: The main preparation process is the same as step (6) of Example B14. The laminated polypropylene composite sheet contains 100 layers of polypropylene fabric. The heat press conditions adopted are 159°C, heat press pressure 10MPa, preheat time 420s, heat press time 300s, and cooling time 700s. The thickness of the prepared polypropylene composite is 7.45mm.

[0483] Example B25 This example is used to illustrate the preparation of the polypropylene composition, five-layer coextruded polypropylene composite sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0484] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0485] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0486] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0487] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The preparation process is the same as step (4) of Example B14.

[0488] (5) Preparation of polypropylene fabric: The preparation process is the same as step (5) of Example B14.

[0489] (6) Preparation of polypropylene composites: The main preparation process is the same as step (6) of Example B14. Temperature 155°C, heat press pressure 8MPa, preheating time 300s, heat press time 300s, cooling time 700s. The thickness of the prepared polypropylene composite material is 1.61mm.

[0490] Example B26 This example is used to illustrate the preparation of the polypropylene composition, 5-layer coextruded polypropylene sheet, polypropylene fabric and polypropylene composite provided in the present invention.

[0491] (1) Preparation of polypropylene composition A: The preparation process is the same as step (1) of Example B14.

[0492] (2) Preparation of polypropylene composition C: The preparation process is the same as step (2) of Example B14.

[0493] (3) Preparation of polypropylene composition B: The preparation process is the same as step (3) of Example B14.

[0494] (4) Preparation of 5-layer coextruded polypropylene composite sheets: The preparation process is the same as step (4) of Example B14.

[0495] (5) Preparation of polypropylene composites: The main preparation process is the same as step (6) of Example B14, except that instead of preparing polypropylene fabric, the 5-layer coextruded polypropylene sheet obtained in step (4) above is sequentially laminated and hot-pressed (instead of the polypropylene fabric of Example B14).

[0496] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0497] Example B27 A five-layer coextruded polypropylene sheet is prepared according to the method of Example B14, except that the material of component A is selected as follows: component a is a polypropylene homopolymer prepared by SINOPEC Beijing Chemical Research Institute, with a melting point of 155°C, a melt flow rate of 14.3g / 10min, and an isotacticity of 96%.

[0498] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0499] Example B28 According to the method of Example B14, a five-layer coextruded polypropylene sheet is prepared, except that the material of component B is selected as follows: component x is a polypropylene random copolymer prepared by SINOPEC Beijing Chemical Research Institute, which is an ethylene-propylene-butene terpolymer, with a molecular weight distribution (Mw / Mn) of 10.5, a melting point of 130°C, and a melt flow rate of 9.2g / 10min; The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0500] Comparative Example B1 A three-layer coextruded polypropylene sheet is prepared according to the method of Example B1, except that polypropylene composition A is extruded and cast alone to prepare a monolayer film having a thickness of 80 μm. A polypropylene fabric and a polypropylene composite are prepared according to the method of Example B1.

[0501] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0502] Comparative example B2 A three-layer coextruded polypropylene sheet is prepared according to the method of Example B1, except that polypropylene composition B is extruded and cast alone to prepare a monolayer film having a thickness of 80 μm. A polypropylene fabric and a polypropylene composite are prepared according to the method of Example B1.

[0503] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0504] Comparative Example B3 A three-layer coextruded polypropylene sheet is prepared according to the method of Example B1, except that polypropylene composition A contains only component b.

[0505] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0506] Comparative example B4 A three-layer coextruded polypropylene sheet is prepared according to the method of Example B1, except that polypropylene composition B contains only component y.

[0507] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0508] Comparative Example B5 A three-layer coextruded polypropylene sheet is prepared according to the method of Example B1, except that the thickness of film layer A accounts for 95% of the total thickness of the sheet. Polypropylene fabrics and polypropylene composites are prepared according to the method of Example B1.

[0509] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0510] Comparative example B6 A three-layer coextruded polypropylene sheet is prepared according to the method of Example B1, except that the thickness of film layer A accounts for 50% of the total thickness of the sheet. Polypropylene fabrics and polypropylene composites are prepared according to the method of Example B1.

[0511] The thickness of the prepared polypropylene composite material is the same as in Example B1.

[0512] Comparative Example B7 A 5-layer coextruded polypropylene composite sheet is prepared according to the method of Example B14, except that polypropylene composition A is extruded and cast alone to prepare a monolayer film having a thickness of 80 μm. A polypropylene fabric and a polypropylene composite are prepared according to the method of Example B1.

[0513] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0514] Comparative example B8 A 5-layer coextruded polypropylene composite sheet is prepared according to the method of Example B14, except that polypropylene composition C is extruded and cast alone to prepare a monolayer film having a thickness of 80 μm. A polypropylene fabric and a polypropylene composite are prepared according to the method of Example B1.

[0515] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0516] Comparative Example B9 A 5-layer coextruded polypropylene composite sheet is prepared according to the method of Example B14, except that polypropylene composition B is extruded and cast alone to prepare a monolayer film having a thickness of 80 μm. A polypropylene fabric and a polypropylene composite are prepared according to the method of Example B1.

[0517] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0518] Comparative Example B10 A five-layer coextruded polypropylene composite sheet is prepared according to the method of Example B14, except that polypropylene composition A contains only component b.

[0519] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0520] Comparative Example B11 A five-layer coextruded polypropylene composite sheet is prepared according to the method of Example B14, except that polypropylene composition B contains only component y.

[0521] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0522] Comparative example B12 A five-layer coextruded polypropylene composite sheet is prepared according to the method of Example B14, except that the thickness of film layer A is 95% of the total thickness of the sheet, the thickness of film C is 2.5% of the total thickness of the sheet, and the thickness of film B is 2.5% of the total thickness of the sheet. The polypropylene fabric and polypropylene composite were prepared according to the method of Example B1.

[0523] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0524] Comparative Example B13 A five-layer coextruded polypropylene composite sheet is prepared according to the method of Example B14, except that the thickness of film layer A is 50% of the total thickness of the sheet, the thickness of film C is 25% of the total thickness of the sheet, and the thickness of film B is 25% of the total thickness of the sheet. The polypropylene fabric and polypropylene composite are prepared according to the method of Example B1.

[0525] The thickness of the prepared polypropylene composite material is the same as in Example B14.

[0526] Experimental Example The polypropylene composite materials obtained in the above examples and comparative examples were tested according to the following methods, and the results are shown in Tables 2 and 3: (1) Tensile strength: Prepared and measured according to the method specified in GB / T1040.1-2018; (2) Interlaminar peel strength: Prepare and measure according to the method specified in GB / T2358-98.

[0527] (3) Drop impact strength: Measured according to the method specified in GB / T14153-1993. The thicknesses of the polypropylene composite materials obtained in Examples B1-9 and Comparative Examples B1-6 are all close to about 1.6 mm, within the range of 1.6 mm ± 1 mm. The thicknesses of the polypropylene composite materials obtained in Examples B14-22, B26 and Comparative Examples B7-13 are all close to about 1.8 mm, within the range of 1.8 mm ± 1 mm.

[0528] [Table 2]

[0529] As can be seen from the results of the examples in Table 3, the polypropylene composite prepared according to the present invention has good tensile and impact properties, and at the same time has good interlayer peel strength even at lower heat press temperatures. The polypropylene composite sheet according to the present invention has a machine direction (MD) tensile strength of 150 MPa or more, an interlayer peel strength of 1 N / mm or more, and a drop impact strength of 228 J or more when the polypropylene composite is obtained by heat pressing and fusing 24 layers of polypropylene fabric and has a thickness of about 1.6 mm.

[0530] As can be seen from the preferred examples B1-3, the polypropylene composite material prepared in the present invention has a tensile strength in the machine direction (MD) of 170 MPa or more, and an interlayer peel strength of 1.2 N / mm or more. The polypropylene composite material is obtained by heat pressing and fusing 24 layers of polypropylene fabric, and has a drop impact strength of 240 J or more when it has a thickness of about 1.6 mm.

[0531] As can be seen from Comparative Examples B1-6, simply adopting a single-layer sheet structure or adopting an interlayer ratio outside the range of the inventive examples reduces the performance of the laminated polypropylene sheet or fabric, resulting in a significant decrease in the tensile strength, impact properties or interlayer peel strength of the resulting polypropylene composite material.

[0532] [Table 3]

[0533] As can be seen from the results of the examples in Table 3, the polypropylene composite prepared according to the present invention has good tensile and impact properties, and at the same time has good interlayer peel strength even at lower heat press temperatures. When the polypropylene composite sheet has a BCACB sheet structure, the polypropylene composite according to the present invention has a machine direction (MD) tensile strength of 150 MPa or more, an interlayer peel strength of 1.1 N / mm or more, and when the polypropylene composite is obtained by heat pressing and fusing 24 layers of polypropylene fabric and has a thickness of about 1.8 mm, it has a drop impact strength of 240 J or more.

[0534] As can be seen from the preferred examples B14-16, the polypropylene composite material prepared in the present invention has a tensile strength in the machine direction (MD) of 170 MPa or more and a peel strength of 1.3 N / mm or more. The polypropylene composite material obtained by hot pressing and fusing 24 layers of polypropylene fabric has a drop impact strength of ≧250 J when the thickness is about 1.8 mm. As can be seen from the comparative examples B7-13, simply adopting a single layer film structure or adopting a film layer ratio outside the range of the present invention examples reduces the performance of the laminated polypropylene sheet or fabric, and the tensile strength, impact properties, and peel strength of the resulting polypropylene composite material are significantly reduced.

[0535] While various embodiments of the present invention have been described above, the foregoing description is illustrative, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0536] It is understood that the range endpoints and values ​​disclosed herein are not limited to such exact ranges or values, and that these ranges or values ​​include values ​​approaching these ranges or values. For numerical ranges, one or more new numerical ranges can be obtained by combining the endpoints of each range with each other, the endpoints of each range with individual point values, and the individual point values ​​with each other, and these value ranges should be considered as specifically disclosed herein.

Claims

1. A polypropylene composite material comprising a plurality of polypropylene sheet layer units laminated in sequence; each polypropylene sheet layer unit group comprises at least one identical or different polypropylene sheet layer unit, and each polypropylene sheet layer unit comprises a core layer A. i , and the core layer A i Outer layer B located on both sides of i and B' i Including B i A i B' i the polypropylene composite material has a structure in which, from bottom to top, the layers are n-th group, ... i-th group, ... 2nd group, 1st group, 2nd group, ... i-th group, ... n-th group, and the total number of lamination groups of the polypropylene sheet layer unit groups is 2n-1; i and n are both integers of 2 or more, and i≦n; Here, in the polypropylene sheet layer unit, the core layer A i Polypropylene composition A i The outer layer B i The outer layer B' i The outer layer B may be the same or different from the outer layer B. i Polypropylene composition B i and the outer layer B' i is the polypropylene composition B' i Contains The polypropylene composition A i The melting point of the polypropylene composition B i and the polypropylene composition B' i the average melting point of all the outer layers of group i is higher than the average melting point of all the outer layers of group i-1.

2. The polypropylene composition A i and the melting point of the polypropylene composition B i and the melting point difference between said polypropylene composition A and said polypropylene composition B. i and the melting point of the polypropylene composition B' i and / or The polypropylene composite material according to claim 1, characterized in that the difference between the average melting point of all outer layers of the i-th group and the average melting point of all outer layers of the i-1-th group, whether the difference is the same or different, is 1 to 40°C, preferably 1 to 10°C, and more preferably 1 to 5°C.

3. 2≦n≦100, preferably 2≦n≦50; and / or The polypropylene composite material according to claim 1 or 2, characterized in that each of the polypropylene sheet layer unit groups independently comprises 1 to 10, preferably 1 to 5, identical or different polypropylene sheet layer units.

4. The polypropylene sheet layer unit is an intermediate layer C i and C' i The polypropylene sheet layer unit has a structure of B i C i A i C' i B' i and the intermediate layer C i The intermediate layer C' i the intermediate layer C i Polypropylene composition C i and the intermediate layer C' i Polypropylene composition C' i The polypropylene composition A comprises i The melting point of the polypropylene composition C i and the polypropylene composition C' i The polypropylene composite material according to any one of claims 1 to 3, characterized in that the melting point of the polypropylene composite material is higher than that of the polypropylene composite material.

5. Core layer A of each polypropylene sheet layer unit i The polypropylene composite material according to any one of claims 1 to 4, characterized in that the thickness of each polypropylene sheet layer unit accounts for 51% to 89%, preferably 71% to 89%, and more preferably 71% to 80% of the total thickness, based on the total thickness of each polypropylene sheet layer unit.

6. The polypropylene composition A i comprises one or more of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; and / or Polypropylene Composition B i and B' i each of which comprises one or more of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; preferably, said polypropylene composition B i and / or said polypropylene composition B' i Further, a thermal adhesion improver y i The polypropylene composite material according to any one of claims 1 to 5, characterized in that it contains

7. The polypropylene composition C i and C' i each of which comprises one or more of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer, and preferably said polypropylene composition C i and / or polypropylene composition C' i However, the thermal adhesion improver z i 5. The polypropylene composite material according to claim 4, further comprising:

8. The polypropylene composition A i Polypropylene homopolymer a i , and polypropylene impact copolymer b i Including; Preferably, the polypropylene composition A i Based on the total weight of the polypropylene composition A i 50 to 99% by weight of polypropylene homopolymer a i , 1 to 50% by weight of polypropylene impact copolymer b i More preferably, said polypropylene composition A i 70 to 90% by weight of polypropylene homopolymer a i , 10 to 30% by weight of polypropylene impact copolymer b i and / or Polypropylene Composition B i , Polypropylene Composition B' i Each of them is a polypropylene random copolymer x i and thermal adhesion improver y i Including; Preferably, said polypropylene composition B i , the polypropylene composition B' i Based on the total weight of each of the polypropylene compositions B i , the polypropylene composition B' i Each of them is 70 to 99% by weight of polypropylene random copolymer x i , 1 to 30% by weight of a thermal adhesion improver y i More preferably, said polypropylene composition B i , the polypropylene composition B' i Each of them is 80 to 90% by weight of polypropylene ram copolymer x i , 10 to 20% by weight of a thermal adhesion improver y i The polypropylene composite material according to any one of claims 1 to 7, characterized in that it comprises

9. The polypropylene composition C i , the polypropylene composition C' i are polypropylene random copolymer β i and polypropylene homopolymer gamma i and thermal adhesion improver z i Including; Preferably, said polypropylene composition C i , the polypropylene composition C' i Based on the total weight of each of the polypropylene compositions C i , the polypropylene composition C' i Each of them is 30 to 60% by weight of the thermal adhesion improver z i , 35 to 55% by weight of polypropylene random copolymer β i and 5 to 15% by weight of polypropylene homopolymer gamma i More preferably, said polypropylene composition C i , the polypropylene composition C' i Each of them is 35 to 55% by weight of the thermal adhesion improver z i , 40 to 55% by weight of polypropylene random copolymer β i and 5 to 10% by weight of polypropylene homopolymer gamma i The polypropylene composite material according to claim 4, characterized in that it comprises

10. The polypropylene homopolymer a i but: and / or a melting point of 150 to 170° C., preferably 160 to 170° C.; A melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 2.5 to 18 g / 10 min; and / or 9. The polypropylene composite material according to claim 8, characterized in that it has an isotacticity (mm) of 96% or more.

11. The polypropylene homopolymer gamma i but: and / or a melting point of 150 to 170° C., preferably 160 to 170° C.; A melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 2.5 to 18 g / 10 min; and / or Has an isotacticity (mm) of 96% or more; Preferably, the polypropylene homopolymer a i and the polypropylene homopolymer γ i but: a difference in melting points of less than 10° C., preferably less than 5° C., more preferably less than 3° C.; and / or a difference in melt flow rate at 230° C. and 2.16 kg load of less than 10 g / 10 min, preferably less than 5 g / 10 min, more preferably less than 3 g / 10 min; and / or having a difference in isotacticity (mm) of less than 3%, preferably less than 2%, more preferably less than 1%; More preferably, polypropylene homopolymer a i and polypropylene homopolymer γ i The polypropylene composite material according to claim 9, characterized in that

12. The polypropylene impact copolymer b i has a melting point of 150-170°C; and / or The polypropylene impact copolymer b i the monomer copolymerized with propylene in is ethylene or butene, preferably butene; and / or The polypropylene impact copolymer b i has a melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 2.5 to 18 g / 10 min; and / or The polypropylene impact copolymer b i But 20KJ / m 2 The polypropylene composite material according to claim 8, characterized in that it has an Izod impact strength of or greater.

13. The polypropylene random copolymer x i but: a melting point of 110 to 150°C, preferably 120 to 140°C; and / or A melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 3 to 18 g / 10 min; and / or and / or has a molecular weight distribution Mw / Mn of from 5 to 12, preferably from 7 to 10; and / or The polypropylene random copolymer x i 9. The polypropylene composite according to claim 8, characterized in that is a copolymer of propylene with ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene bipolymer.

14. The polypropylene random copolymer β i but: a melting point of 110 to 150°C, preferably 120 to 140°C; and / or A melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 3 to 18 g / 10 min; and / or and / or has a molecular weight distribution Mw / Mn of from 5 to 12, preferably from 7 to 10; and / or The polypropylene random copolymer β i is a copolymer of propylene with ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene bipolymer; Preferably, the polypropylene random copolymer x i and the polypropylene random copolymer β i but: a difference in melting points of less than 10° C., preferably less than 5° C., more preferably less than 3° C.; and / or a difference in melt flow rate at 230° C. and 2.16 kg load of less than 10 g / 10 min, preferably less than 5 g / 10 min, more preferably less than 3 g / 10 min; and / or having a molecular weight distribution difference of less than 3, preferably less than 2, more preferably less than 1; More preferably, the polypropylene random copolymer x i and the polypropylene random copolymer β i The polypropylene composite material according to claim 9, characterized in that

15. The thermal adhesion improver y i but: A melting point or viscous flow temperature of 70-110° C.; and / or and / or having a melt flow rate at 190° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 1 to 18 g / 10 min; and / or The thermal adhesion improver y i is selected from one or more of polyolefin elastomer, ethylene-propylene-diene-terpolymer rubber, SEBS, SBS, EVA, petroleum resin, preferably polyolefin elastomer and / or petroleum resin.

16. The thermal adhesion enhancing agent z i but: A melting point or viscous flow temperature of 70-110° C.; and / or and / or having a melt flow rate at 190° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 1 to 18 g / 10 min; and / or The thermal adhesion improver z i is selected from one or more of polyolefin elastomer, ethylene-propylene-diene-terpolymer rubber, SEBS, SBS, EVA, and petroleum resin, preferably polyolefin elastomer and / or petroleum resin; Preferably, the thermal adhesion improver y i and the thermal adhesion improver z i but: a difference in melting point or viscous flow temperature of less than 10° C., preferably less than 5° C., more preferably less than 3° C.; and / or have a difference in melt flow rate at 190°C and 2.16 kg load of less than 10 g / 10 min, preferably less than 5 g / 10 min, more preferably less than 3 g / 10 min; More preferably, the thermal adhesion improver y i and the thermal adhesion improver z i The polypropylene composite material according to claim 9, characterized in that

17. the polyolefin elastomer is an elastomer of ethylene copolymerized with propylene and / or an α-olefin, the α-olefin being preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or The polypropylene composite material according to claim 15 or 16, characterized in that the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin with a softening point of 100-150°C, preferably a cyclopentadiene type resin.

18. The polypropylene composition A i but also includes β-nucleating agents; preferably the β-nucleating agent is selected from at least one of polycyclic aromatic hydrocarbons, Group IIA binary complexes, aromatic diamides, rare earth compounds, and cyclic dicarboxylate nucleating agents; and / or The polypropylene composition A i The content of the β-nucleating agent in the polypropylene composition A is i The polypropylene composite material according to claim 6, characterized in that the content is 0.01 to 0.5 parts by weight based on a total amount of 100 parts by weight.

19. The polypropylene sheet layer unit is a polypropylene sheet and / or a polypropylene fabric; preferably, the polypropylene sheet layer unit is a polypropylene sheet or a polypropylene fabric; more preferably, The polypropylene sheet is made of polypropylene composition A i , Polypropylene Composition B i , Polypropylene Composition B' i , optionally polypropylene composition C i , optionally a polypropylene composition C' i and / or The polypropylene fabric may be prepared by the following method: i , Polypropylene Composition B i , Polypropylene Composition B' i , optionally polypropylene composition C i , optionally a polypropylene composition C' i and then weaving the polypropylene sheet to obtain the polypropylene fabric; preferably, the polypropylene fabric has a plain weave, twill weave and / or satin weave configuration. A polypropylene composite material according to any one of claims 1 to 18, characterized in that

20. 20. The polypropylene composite material according to claim 19, characterized in that the various polypropylene sheet layer units are connected by heat press bonding.

21. 21. A method for preparing a polypropylene composite material according to any one of claims 1 to 20, comprising the steps of sequentially laminating 2n-1 polypropylene sheet layer unit groups in the order of nth group, ... ith group, ... 2nd group, 1st group, 2nd group, ... ith group, ... nth group, and then performing heat pressing and fusion bonding.

22. 22. The process according to claim 21, characterized in that it comprises the following steps: (1) Polypropylene Composition A i , Polypropylene Composition B i , Polypropylene Composition B' i , optionally polypropylene composition C i , optionally a polypropylene composition C' i A, B i A i B' i Structure or B i C i A i C' i B' i co-extrusion, casting or calendaring according to the structure and stretching to obtain a polypropylene sheet; (2) Optionally, the polypropylene sheet is divided and cut, and then woven to form B i A i B' i Structure or B i C i A i C' i B' i obtaining a structural polypropylene fabric; (3) The polypropylene sheets and / or the polypropylene fabric are sequentially laminated, heat pressed and fused, then cooled and molded to form a polypropylene composite material.

23. The polypropylene composition A in the step (1) i comprising melt blending components comprising at least one of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; and / or The polypropylene composition B in the step (1) i , the polypropylene composition B' i comprising melt blending components comprising at least one of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; and / or The polypropylene composition C in the step (1) i , the polypropylene composition C' i comprising melt blending components comprising at least one of a polypropylene homopolymer, a polypropylene random copolymer, and a polypropylene impact copolymer; and / or The temperatures of the co-extrusion and casting in step (1) are each independently selected from 190 to 240° C.; and / or The temperature of the calendar roller in step (1) is 50 to 70° C.; and / or The stretching temperature in the step (1) is 90 to 165°C, preferably 90 to 140°C, more preferably 90 to 119°C; and / or The preparation method according to claim 22, characterized in that the stretching ratio in step (1) is 1-15.

24. In step (3): The heat pressing conditions are as follows: a heat pressing temperature of 115 to 170° C., preferably 115 to 159° C., more preferably 140 to 159° C., a heat pressing pressure of 2 to 10 MPa, a preheating time of 5 to 600 s, a heat pressing time of 1 to 600 s, preferably 10 to 500 s; and / or and / or a pressure for cooling and forming of 2 to 8 MPa and a cooling time of 30 s to 700 s; the laminated adjacent polypropylene fabrics are oriented at an angle of 0 to 90 degrees relative to each other along their respective warp directions; and / or 23. The method of claim 22, wherein the laminated adjacent polypropylene sheets are oriented at an angle of 0 to 90 degrees relative to each other along their respective machine directions.

25. The machine includes a preheater, a crawler type continuous flat heat press, a crawler type continuous flat cooling press, a sheet cutter and a sheet laminator, which are arranged in sequence; Preferably, the crawler type continuous flat heat press comprises a preheating unit, an independent heating and pressing unit, an air-cooling unit, and a lifting mechanism.

26. Use of the polypropylene composite material according to any one of claims 1 to 20 and the polypropylene composite material prepared by the preparation method according to any one of claims 21 to 24 in the applications of consumer goods, automobile manufacturing, sports protection and military materials.

27. A polypropylene sheet preferably used as a polypropylene sheet layer unit in the polypropylene composite material according to claim 1, comprising a layer A and a layer B and a layer B' located on both sides of the layer A, and having a structure of BAB'; wherein layer A contains polypropylene composition A, layer B is the same as or different from layer B', layer B contains polypropylene composition B, layer B' contains polypropylene composition B', and the melting point of said polypropylene composition A is higher than the melting points of said polypropylene composition B and said polypropylene composition B'; A polypropylene sheet, wherein the polypropylene composition A comprises a polypropylene homopolymer a and a polypropylene impact copolymer b; and the polypropylene composition B and the polypropylene composition B' each comprise a polypropylene random copolymer x and a thermal adhesion improver y.

28. the polypropylene sheet further comprises layers C and C' in a structure of BCAC'B'; layer C is the same as or different from layer C', layer C contains polypropylene composition C, and layer C' contains polypropylene composition C'; the melting point of the polypropylene composition A is higher than the melting points of polypropylene composition C and polypropylene composition C'; The polypropylene sheet according to claim 27, wherein the polypropylene composition C and the polypropylene composition C' each contain a polypropylene random copolymer β and a polypropylene homopolymer γ, and a thermal adhesion improver z.

29. Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50 to 99 wt. % of polypropylene homopolymer a, 1 to 50 wt. % of polypropylene impact copolymer b; preferably, the polypropylene composition A comprises 70 to 90 wt. % of polypropylene homopolymer a, 10 to 30 wt. % of polypropylene impact copolymer b; and / or The polypropylene sheet according to claim 27, characterized in that, based on the total weight of each of the polypropylene composition B and the polypropylene composition B', the polypropylene composition B and the polypropylene composition B' each contain 70 to 99 wt% of the polypropylene random copolymer x and 1 to 30 wt% of the thermal adhesion improver y; preferably, the polypropylene composition B and the polypropylene composition B' each contain 80 to 90 wt% of the polypropylene random copolymer x and 10 to 20 wt% of the thermal adhesion improver y.

30. The thickness of the film layer A is 51% to 89%, preferably 71% to 89%, more preferably 71% to 80% of the total thickness of the polypropylene sheet.

31. The polypropylene composition C and the polypropylene composition C' each contain 30 to 60% by weight of a thermal adhesion improver z, 35 to 55% by weight of a polypropylene random copolymer β, and 5 to 15% by weight of a polypropylene homopolymer γ, based on the total weight of each of the polypropylene composition C and the polypropylene composition C'; preferably, the polypropylene composition C and the polypropylene composition C' each contain 35 to 55% by weight of a thermal adhesion improver z, 40 to 55% by weight of a polypropylene random copolymer β, and 5 to 10% by weight of a polypropylene homopolymer γ. The polypropylene sheet according to claim 28,

32. 29. The polypropylene sheet according to claim 28, characterized in that, based on the total thickness of each polypropylene sheet, the thickness of layer A accounts for 51% to 89%, preferably 71% to 89%, of the total thickness; the thickness of layers C, C' accounts for 6% to 20%, preferably 6% to 15%, of the total thickness; and the thickness of layers B, B' accounts for 5% to 30%, preferably 5% to 15%, of the total thickness.

33. The polypropylene homopolymer a is: and / or a melting point of 150 to 170° C., preferably 160 to 170° C.; A melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 2.5 to 18 g / 10 min; and / or 28. Polypropylene sheet according to claim 27, characterized in that it has an isotacticity (mm) of 96% or more.

34. The polypropylene homopolymer γ is and / or a melting point of 150 to 170° C., preferably 160 to 170° C.; A melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 2.5 to 18 g / 10 min; and / or Has an isotacticity (mm) of 96% or more; Preferably, the polypropylene homopolymer a and the polypropylene homopolymer γ are: a difference in melting points of less than 10° C., preferably less than 5° C., more preferably less than 3° C.; and / or a difference in melt flow rate at 230° C. and 2.16 kg load of less than 10 g / 10 min, preferably less than 5 g / 10 min, more preferably less than 3 g / 10 min; and / or having a difference in isotacticity (mm) of less than 3%, preferably less than 2%, more preferably less than 1%; More preferably, the polypropylene homopolymer a and the polypropylene homopolymer γ are identical to each other.

35. said polypropylene impact copolymer b having a melting point of 150-170°C; and / or The monomer copolymerized with propylene in said polypropylene impact copolymer b is ethylene or butene, preferably butene; and / or The polypropylene impact copolymer b has a melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 2.5 to 18 g / 10 min; and / or The polypropylene impact copolymer b has an Izod impact strength of 20 KJ / m 2 The polypropylene sheet according to claim 27, characterized in that

36. The polypropylene random copolymer x is: a melting point of 110 to 150°C, preferably 120 to 140°C; and / or A melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 3 to 18 g / 10 min; and / or and / or has a molecular weight distribution Mw / Mn of from 5 to 12, preferably from 7 to 10; and / or 28. Polypropylene sheet according to claim 27, characterized in that the polypropylene random copolymer x is a copolymer of propylene with ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene bipolymer.

37. The polypropylene random copolymer β is: a melting point of 110 to 150°C, preferably 120 to 140°C; and / or A melt flow rate at 230° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 3 to 18 g / 10 min; and / or and / or has a molecular weight distribution Mw / Mn of from 5 to 12, preferably from 7 to 10; and / or The polypropylene random copolymer β is a copolymer of propylene with ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene bipolymer; Preferably, the polypropylene random copolymer x and the polypropylene random copolymer β are: a difference in melting points of less than 10° C., preferably less than 5° C., more preferably less than 3° C.; and / or a difference in melt flow rate at 230° C. and 2.16 kg load of less than 10 g / 10 min, preferably less than 5 g / 10 min, more preferably less than 3 g / 10 min; and / or having a molecular weight distribution difference of less than 3, preferably less than 2, more preferably less than 1; More preferably, the polypropylene random copolymer x and the polypropylene random copolymer β are identical, according to claim 28.

38. The thermal adhesion improver y is: A melting point or viscous flow temperature of 70-110° C.; and / or and / or having a melt flow rate at 190° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 1 to 18 g / 10 min; and / or The polypropylene sheet according to claim 27, characterized in that the thermal adhesion improver y is selected from one or more of polyolefin elastomer, ethylene-propylene-diene-terpolymer rubber, SEBS, SBS, EVA, and petroleum resin, preferably polyolefin elastomer and / or petroleum resin.

39. The thermal adhesion improver z is A melting point or viscous flow temperature of 70-110° C.; and / or and / or having a melt flow rate at 190° C. and 2.16 kg load of 0.5 to 50 g / 10 min, preferably 1 to 20 g / 10 min, more preferably 1 to 18 g / 10 min; and / or The thermal adhesion improver z is selected from one or more of polyolefin elastomer, ethylene-propylene-diene-terpolymer rubber, SEBS, SBS, EVA, and petroleum resin, and is preferably polyolefin elastomer and / or petroleum resin; Preferably, the thermal adhesion improver y and the thermal adhesion improver z are: a difference in melting point or viscous flow temperature of less than 10° C., preferably less than 5° C., more preferably less than 3° C.; and / or have a difference in melt flow rate at 190°C and 2.16 kg load of less than 10 g / 10 min, preferably less than 5 g / 10 min, more preferably less than 3 g / 10 min; More preferably, the polypropylene sheet according to claim 28, characterized in that the thermal adhesion improver y and the thermal adhesion improver z are identical.

40. the polyolefin elastomer is an elastomer of ethylene copolymerized with propylene and / or an α-olefin, the α-olefin being preferably a C4-C12 α-olefin, more preferably 1-butene and / or 1-octene; and / or 40. The polypropylene sheet according to claim 38 or 39, characterized in that the petroleum resin is a C5 and / or C9 hydrogenated petroleum resin having a softening point of 100 to 150 ° C, preferably a cyclopentadiene type resin.

41. The polypropylene composition A also comprises a β-nucleating agent; preferably the β-nucleating agent is selected from at least one of polycyclic aromatic hydrocarbons, Group IIA binary complexes, aromatic diamides, rare earth compounds, and cyclic dicarboxylate nucleating agents; and / or The content of the β-nucleating agent in the polypropylene composition A is 0.01 to 0.5 parts by weight based on 100 parts by weight of a total amount of the polypropylene composition A. The polypropylene sheet according to any one of claims 27 to 40,

42. The melting point of the polypropylene homopolymer a in the polypropylene composition A is higher than the melting point of the polypropylene random copolymer x in the polypropylene compositions B and B', and preferably the temperature difference between the respective melting points is 10°C or more; and / or 28. Polypropylene sheet according to claim 27, characterized in that the BAB' sheet structure of the polypropylene sheet is obtained by co-extruding components comprising the polypropylene composition A and the polypropylene compositions B, B'.

43. Preferably, the melting point of the polypropylene homopolymer a in the polypropylene composition A is higher than the melting point of the polypropylene random copolymer x in the polypropylene compositions B and B' and the melting point of the polypropylene random copolymer β in the polypropylene compositions C and C', and the temperature difference between the respective melting points is 10°C or more; and / or 29. The polypropylene sheet according to claim 28, characterized in that the BCAC'B' sheet structure of the polypropylene composite sheet is obtained by co-extruding components comprising the polypropylene composition A, the polypropylene compositions B, B' and the polypropylene compositions C, C'.

44. 44. A method for preparing a polypropylene sheet according to any one of claims 27 to 43, comprising co-extruding, casting or calendaring said polypropylene composition A, said polypropylene composition B, said polypropylene composition B', optionally said polypropylene composition C, optionally said polypropylene composition C' according to a BAB' structure or a BCAC'B' structure and stretching to obtain said polypropylene sheet.

45. preparing the polypropylene composition A comprises melt blending components comprising the polypropylene homopolymer a and the polypropylene impact copolymer b; and / or The preparation of the polypropylene compositions B, B' comprises melt blending components comprising the polypropylene random copolymer x and a thermal adhesion promoter y; and / or The preparation of the polypropylene compositions C, C' comprises melt blending components comprising the thermal adhesion improver z, the polypropylene random copolymer β and the polypropylene homopolymer γ; and / or the co-extrusion and casting temperatures are each independently selected from 200 to 240° C.; and / or the temperature of the calender rollers is between 50 and 70° C.; and / or 45. The method of claim 44, characterized in that the stretching conditions comprise: a stretching temperature of 90-165°C, preferably 90-140°C, more preferably 90-119°C; a stretching ratio of 1-15.

46. A polypropylene fabric, comprising a three-dimensional polypropylene fabric obtained by weaving the polypropylene sheet according to any one of claims 27 to 43, Preferably, the polypropylene fabric is obtained by splitting and cutting the polypropylene sheet and weaving, and / or the polypropylene fabric has a plain weave, twill weave and / or satin weave configuration.

47. A polypropylene composite material prepared by multi-layering the polypropylene sheet according to any one of claims 27 to 43 and / or the polypropylene fabric according to claim 46 via heat pressing and fusing, preferably The polypropylene composite is prepared with multiple layers of polypropylene sheets or fabrics by heat pressing and fusing; and / or The layers of polypropylene sheet are arranged and laminated from top to bottom along their respective machine directions at angles of 0 to 90 degrees relative to each other; and / or The multiple layers of polypropylene fabric are arranged and stacked from top to bottom along their respective warp directions at angles of 0 to 90 degrees relative to each other; and / or A polypropylene composite material, wherein the number of layers of said polypropylene sheet and / or said polypropylene fabric is 2 or more, more preferably 2-200 layers, and most preferably 4-100 layers.

48. 48. A method of preparing a polypropylene composite material according to claim 47, comprising laminating, heat pressing and fusing said polypropylene sheets and / or said polypropylene fabrics, and then cooling and molding to form a polypropylene composite material.

49. The temperature of said heat pressing and fusing is 115-170°C, preferably 115-159°C, more preferably 140-159°C; and / or The pressure of the heat pressing and fusing is 2-10 MPa; and / or The pre-heating time for the heat pressing and fusing is 5-600 s, and the heat pressing time is 1-600 s, preferably 10-500 s; and / or The pressure of the cooling and molding is 2-8 MPa, and the time of the cooling and molding is 30 s-700 s; and / or The number of layers of the polypropylene sheet and / or the polypropylene fabric is 2 or more, preferably 2 to 200 layers; more preferably 4 to 100 layers; and / or and / or wherein adjacent layers of the polypropylene fabric are arranged at angles of 0 to 90 degrees relative to each other along their respective warp directions; and / or 49. The method of claim 48, wherein adjacent layers of the laminated polypropylene sheet are oriented at an angle of 0 to 90 degrees relative to each other along their respective machine directions.

50. Use of the polypropylene sheet according to any one of claims 27 to 43, the polypropylene fabric according to claim 46, the polypropylene composite according to claim 47 and the polypropylene composite prepared by the preparation method according to claims 48 or 49 in the applications of sports protection, automotive manufacturing, military materials and consumer goods.

Citation Information

Patent Citations

  • Self-reinforced polypropylene composite material and preparation method thereof

    CN103112224A

  • Polypropylene self-reinforced composite and preparation method thereof

    CN105563976A

  • Polypropylene self-reinforced composite and preparation method thereof

    CN105566744A

  • polyolefin film, tape or yarn

    JP2004534681A

  • Methods of forming thermoplastic composites

    JP2009516603A