High-rate, long-cycle, high-safety positive electrode plate for lithium batteries, and its manufacturing method and use
A surface-coated positive electrode plate with specific components improves lithium ion transport and stabilizes the CEI, addressing the challenges of increased density in lithium batteries, enhancing rate and cycle stability while ensuring safety and scalability.
Patent Information
- Application Number
- JP2024532330
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-01-30
- Filing Date
- 2023-01-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-01-28
AI Technical Summary
Existing methods fail to simultaneously improve the rate characteristics, cycle stability, and safety of lithium batteries as the loading and compaction density of the positive electrode plate increases, leading to reduced lithium ion transport and safety concerns.
A positive electrode plate with a functional layer containing specific components like Li1-x1Ti1-x1OPO4 and Li1+x2Alx2M2(PO4)3, which are mixed and coated on the surface of the positive electrode, forming a porous structure to enhance lithium ion conduction and stabilize the solid electrolyte interface (CEI), preventing short circuits and electrolyte decomposition.
The solution significantly improves the rate characteristics, cycle stability, and safety of lithium batteries by enhancing lithium ion conduction and stabilizing the CEI, while being compatible with existing manufacturing processes and suitable for large-scale applications.
Smart Images

Figure 2024542667000001_ABST
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of Chinese patent application No. 202210113785.8, filed on January 30, 2022, the contents of which are incorporated herein by reference. [Technical field]
[0002] The present invention relates to the technical field of lithium batteries, and in particular to a high-rate, long-cycle, high-safety positive electrode plate for lithium batteries, and its manufacturing method and use. [Background technology]
[0003] Lithium-ion batteries have the advantages of high energy density, good cycle characteristics, long service life, low self-discharge, and no memory effect. Their application in energy storage, power batteries, 3C electronics and other fields is gradually expanding, and their future applications are promising.
[0004] Lithium batteries have an increasing energy density, providing better range for power electronics products such as electric vehicles and digital products. Increasing the loading and compression density of the electrode plate, especially the positive electrode plate, is an effective way to increase the energy density of the battery. However, as the loading and compression density of the positive electrode plate increase, the positive electrode active material layer becomes thicker and the porosity decreases, making it difficult to transport lithium ions in the positive electrode plate, resulting in serious polarization of the battery, which reduces the discharge specific capacity and rate characteristics of the battery, and also reduces cycle stability. In addition, as the energy density of the battery increases, it tends to become more difficult to ensure the safety of the battery. There has been no technology to solve these problems simultaneously.
[0005] Existing methods for improving the rate performance of batteries are as follows:
[0006] Cathode surface doping: The invention application with publication number CN113224287A describes a strontium-doped ternary lithium-ion battery cathode material (Li 1-x Sr x[Ni 1-y-z Co y M z O₂, where M is one of the metals Mn and Al, 0 < x ≤ 0.1, 0 < y ≤ 1, 0 < z ≤ 1), its manufacturing method, and its use are disclosed. By doping strontium metal ions to replace lithium sites, the degree of cation mixing is reduced, the lithium ion channel is expanded, the layered structure is stabilized, and the rate performance of the lithium battery is effectively improved. However, this method often brings the problem of accelerating the capacity decay of the material while improving the rate performance.
[0007] Existing methods for improving the safety of the battery are as follows.
[0008] Positive electrode coating: The invention application with publication number CN113809280A discloses a positive electrode material, its manufacturing, and its use, which manufactures a positive electrode material having a substantially planar coating effect by changing sintering technical means and utilizing the interaction of coating agents. The positive electrode material manufactured by this method has a wide coating range of the surface coating layer, greatly reduces the degree of erosion of material particles by the electrolyte, effectively reduces the occurrence probability of side reactions, and improves the safety of the material. However, there are disadvantages that the process of the method is complex and it affects the rate performance of the battery.
[0009] Use of electrolyte additives: The invention application with publication number CN113690490A discloses a phosphite-based lithium ion battery electrolyte additive that can effectively prevent the combustion and explosion of organic solvents, enhance the thermal stability of the electrolyte itself, enhance the stability of the positive electrode, and improve the cycle stability and safety of the battery. There are disadvantages that it impairs the electrical properties of the battery such as cycle characteristics and rate characteristics.
[0010] Applying adhesive to separator: The invention application with publication number CN108963153B discloses a lithium ion battery separator and its manufacturing method, which is formed by coating at least one surface of a base film layer with an aqueous ceramic slurry coating, and then coating a composite adhesive layer made of polyethylene glycol and polymethyl methacrylate on the aqueous ceramic slurry coating and / or the surface of the base film layer, so that the resulting lithium ion battery separator has good adhesion, can prevent short circuit caused by the misalignment of the electrode plates, improve the battery hardness, and greatly improve the safety of the battery. However, it has the disadvantage of impairing the rate characteristics of the battery.
[0011] Existing methods for improving both the electrical properties and safety of batteries are:
[0012] CN108365260B discloses a quasi-solid electrolyte comprising a polymer, a ceramic electrolyte, a lithium salt and an ionic liquid as a raw material composition. The ceramic electrolyte comprises a lithium titanium aluminum phosphate as a main phase and a heterophase TiP2O7 / TiO2. Preferably, the content of the heterophase in the ceramic electrolyte is 2-7%, and the mass ratio of TiP2O7 to TiO2 is 1.5-2.5:1. The overall properties of the quasi-solid electrolyte manufactured using the ceramic electrolyte with the above content of the heterophase are optimal. The heterophase with the special composition and content has lithium absorption properties, can improve the transportability of lithium ions, and can reduce the contact between the lithium titanium aluminum phosphate as a main phase and metallic lithium, and can improve the interface stability with metallic lithium. However, this patent does not improve the electrical properties and safety of the positive electrode, and the method is not compatible with the mainstream manufacturing process of existing lithium ion battery positive plate, and is not suitable for large-scale application.
[0013] CN113707880A relates to a positive electrode plate containing a solid electrolyte, its manufacturing method and its use, for the purpose of improving the rate characteristics of a battery and improving the cycle characteristics and safety. The solid electrolyte contained in the positive electrode slurry facilitates the permeation and infiltration of the electrolyte in the transverse and longitudinal directions of the plate, and facilitates the storage and infiltration of the electrolyte, thereby alleviating the expansion of the plate during the cycle of the cell, reducing the amount of electrolyte extruded under pressure during the expansion of the plate, so that the plate contains abundant electrolyte even after the cell has been cycled for a long time, ensuring normal transport of lithium ions, and improving the cycle characteristics. However, from the data of the examples, it was found that the battery capacity and safety were only slightly increased, and the effect on the rate characteristics was not supported by data, and the addition of the conventional solid electrolyte could not achieve the purpose of comprehensively improving the electrical characteristics and safety of the battery.
[0014] Therefore, there is a need to find a method that can improve the electrical properties and safety of batteries while also having simple steps and low costs. Summary of the Invention
[0015] In view of the limitations of the prior art, the present invention provides a high-rate, long-cycle, high-safety positive electrode plate for lithium batteries, its manufacturing method and use. The positive electrode plate of the present invention includes a positive electrode material layer and a functional layer located directly on the positive electrode material layer.
[0016] The functional layer material includes component 1, and component 1 includes Li 1-x1 Ti 1-x1 A x1 OPO4, Li 1-x1 Ti 1-x1 A x1 PO5, Li 2-y1 Ti 1-y1 A y1 OM1O4, Li 2-y1 Ti 1-y1 A y1 M1O5, where 0≦x1≦0.7, 0≦y1≦1, A is at least one selected from Nb, Ta, and Sb, and M1 is at least one selected from Si and Ge; Component 1 is preferably at least one of LiTiOPO4, Li 0.9 Nb 0.1 Ti 0.9 OPO4, Li 0.9 Ta 0.1 Ti 0.9 OPO4, Li2TiOSiO4, LiTaOGeO4.
[0017] The functional layer material contains Component 2, and Component 2 is at least one or a combination of a plurality of selected from LiM22(PO4)3, Li 1+x2 Al x2 M2 2-x2 (PO4)3, M2O2, Li 16-4y2 M2 y2 O8, M2P2O7, M3PO4, M32SiO5, M43(PO4)2, M42SiO4, where M2 is one selected from Ti, Ge, Zr, and Hf, where 0 < x2 < 0.6, and M3 and M4 are one of Al, Ga, Sc, Y, Ca, Sr, Zn, Si, In, Lu, La, Fe, Cr, Ge, where 3 < y2 < 4. Component 2 is preferably one of InPO4, LATP, AlPO4, LAGP, LATP + AlPO4, LAGP + Al2SiO5, InPO4 + LATP, Al2SiO5, TiO2 + LiTi2(PO4)3, TiP2O7 + LiGe2(PO4)3.
[0018] In the functional layer, the form of the mixed component composed of Component 1 and Component 2 is such that the particles of Component 1 and the particles of Component 2 are uniformly mixed with each other, or each primary particle contains the crystal form of Component 1 and the crystal form of Component 2.
[0019] The functional layer has a porous structure with a porosity of p (20% ≤ p ≤ 80%) and a thickness of h (0 μm < h ≤ 10 μm).
[0020] The particle size of Component 1 is 10 nm to 10 μm. Preferably, it is 50 nm to 1 μm.
[0021] The particle size of the component 2 is from 10 nm to 10 μm, and preferably from 50 nm to 1 μm.
[0022] Preferably, the positive electrode active material particles are at least one selected from the group consisting of lithium cobalt oxide positive electrodes and modified materials thereof, NCM ternary positive electrodes and modified materials thereof, NCA ternary positive electrodes and modified materials thereof, nickel lithium manganate positive electrodes and modified materials thereof, lithium rich positive electrodes and modified materials thereof, and lithium iron phosphate positive electrodes and modified materials thereof; the conductive agent is at least one selected from Super-P, KS-6, carbon black, nano carbon fiber, carbon nanotube, acetylene black, and graphene; The binder is selected from polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polytetrafluoroethylene, homopolymers, copolymers, modified compounds of the above polymers, or mixtures of the above polymers with other polymers or small molecules.
[0023] The second object of the present invention is to provide a method for producing a positive electrode plate for a lithium battery according to the first object of the present invention, in which the component 1 or the mixture of components 1 and 2 is coated on the surface of the positive electrode to form a functional layer on the surface of the positive electrode material layer. The surface coating of the positive electrode plate includes a slurry of component 1 or the mixture of components 1 and 2, and since the electrode plate has a porous structure, when the component 1 or the mixture of components 1 and 2 is coated on the surface of the positive electrode by the coating process, in addition to forming a coating on the surface of the positive electrode, some particles penetrate and disperse between the positive electrode active material particles.
[0024] Preferably, the method comprises the steps of: Step 1 of producing a positive electrode active layer; Step 2: uniformly mixing component 1 or a mixture of component 1 and component 2 with a solvent and pulverizing the mixture to form a slurry of 10 nm to 10 um; Step 3 of adding a binder to the slurry obtained in step 2 and uniformly mixing to produce a coating slurry; and step 4 of applying the slurry obtained in step 3 onto a positive electrode active layer and drying it to obtain a positive electrode plate.
[0025] Preferably, In step 2, the solvent in the slurry is at least one of deionized water, ethanol, NMP, alcohol, isopropanol, and acetone; The mass ratio of the solvent to the positive electrode material is (2000-10:100).
[0026] In step 4, The air drying is carried out at a temperature of 80 to 180° C. for 10 minutes to 9 hours, and the vacuum drying is carried out at a temperature of 80 to 180° C. for 3 to 100 hours.
[0027] A third object of the present invention is to provide the use of the positive plate according to the first object of the present invention in a lithium battery.
[0028] The lithium battery is a liquid battery or a solid battery.
[0029] In the present invention, the rate characteristics, cycle characteristics, and safety of a battery can be improved by coating the surface of a positive electrode plate with a functional layer containing component 1 or a mixture of components 1 and 2 having a particle diameter D50 of 0.01 to 10 μm by surface coating. In the prior art, component 1 is a heterophase that occurs during the sintering process of a solid electrolyte, and the presence of such a heterophase reduces the ionic conductivity of the solid electrolyte, so it must be removed when producing the solid electrolyte. In other words, it is generally believed that such a component cannot be used in a solid electrolyte due to its extremely low ionic conductivity. However, the present inventors have found through a large amount of testing that the ionic conductivity of such a component is relatively low, and is 10 times lower than the ionic conductivity of a general solid electrolyte. -4 S / cm, which is much smaller than the ionic conductivity of the electrolyte, 10 -2S / cm, and it was found that although component 1 cannot directly contribute to the ion conductivity after mixing with the electrolyte, it can significantly improve the rate characteristics, cycle characteristics and safety of the positive electrode when added to the positive electrode. It is believed that component 1 can change the composition of the CEI to make it more stable, avoid the rupture of the CEI and the resulting battery polarization and thermal runaway, and further improve the rate characteristics, cycle characteristics and safety of the positive electrode plate in the actual operation of the battery, because its specific chemical composition can participate in the formation of the CEI on the surface of the positive electrode material. In addition, component 2 can suppress the decomposition of the electrolyte and the generation of insulating components on the surface of the positive electrode material, so the simultaneous use of component 2 and component 1 can exert a synergistic effect, and an excellent CEI can be constructed, and the electrical properties and safety of the battery can be improved simultaneously and comprehensively. In particular, when component 1 or a mixture of components 1 and 2 forms a coating on the surface of the electrode plate, the coating not only separates the positive electrode and the negative electrode to prevent short circuits inside the battery, but also improves the CEI of the positive electrode surface layer, thereby improving the lithium ion conduction in the direction parallel to the positive electrode surface and reducing the decomposition of the electrolyte on the positive electrode surface. Since the positive electrode surface is the most sufficient area for contact with the electrolyte, the positive electrode surface can be protected, thereby improving the battery characteristics overall and most effectively. The introduction of additives into the positive electrode by the surface coating helps to exert the rate characteristics of the battery without changing the current mainstream manufacturing process of the positive electrode plate, separator, and battery, and has the advantages of high stability and low cost, making it suitable for large-scale application.
[0030] Compared with the prior art, the present invention has the following advantages and significant effects.
[0031] The component 1 or the mixed component particles of component 1 and component 2 in the surface functional layer of the lithium battery positive electrode of the present invention have high chemical stability and can be added to the positive electrode by surface coating after the production of the positive electrode plate, without changing the mainstream manufacturing process of the conventional positive electrode plate, separator and battery, and is compatible with the mainstream manufacturing process of the existing lithium ion battery positive electrode plate, does not affect the manufacturing process of the positive electrode and cell, has the advantages of high stability and low cost, and is suitable for large-scale application. On the other hand, the methods of doping the positive electrode material and coating the positive electrode surface both require changes to the manufacturing technology of the existing positive electrode material, and are difficult to improve the discharge specific capacity and rate characteristics. The component 1 added to the positive electrode plate for lithium batteries of the present invention has low lithium ion conductivity, unlike conventional solid electrolytes. In the prior art, it was common to select an additive component with high lithium ion conductivity in order to improve the electrical properties of the battery. However, it was discovered that by creatively adding particles with low lithium ion conductivity such as component 1 to the positive electrode, the rate characteristics, cycle characteristics and safety of the battery can be significantly improved by improving the surface CEI of the positive electrode particles, thereby overcoming existing technical prejudices.
[0032] The mixed particle of component 1 and component 2 added simultaneously to the positive electrode plate for lithium batteries of the present invention can improve the stability of the CEI on the surface of the positive electrode particle, inhibit the release of oxygen from the positive electrode during thermal runaway and the reaction with the electrolyte, inhibit the decomposition of the electrolyte, and improve the electrical characteristics and safety of the battery. Experiments have demonstrated that the synergistic effect is better when component 1 and component 2 are used simultaneously.
[0033] Component 1 or a mixture of components 1 and 2 forms a safety coating on the surface of the positive plate, which can separate the positive and negative electrodes and improve the safety of the battery. It has been experimentally proven that a battery with a safety coating will not ignite or explode in a hot box test, because the safety coating can separate the positive and negative electrodes to prevent short circuits. The safety coating not only separates the positive and negative electrodes to prevent short circuits inside the battery, but also improves the CEI of the positive plate surface layer, thereby improving lithium ion conduction in the direction parallel to the positive plate surface and reducing the decomposition of the electrolyte on the positive plate surface. This is because the positive plate surface is the area that has the most sufficient contact with the electrolyte, and therefore protecting the positive plate surface can most effectively improve the battery characteristics.
[0034] The porosity of the functional layer of the positive electrode plate for lithium batteries of the present invention is specially designed, if the porosity is less than 20%, it is disadvantageous to the rate characteristics of the battery, if the porosity is more than 80%, it is disadvantageous to the cycle characteristics of the battery. The thickness of the functional layer is specially designed, if the coating thickness is greater than 10 μm, it is disadvantageous to the rate characteristics of the battery.
[0035] The positive electrode exhibits excellent rate characteristics, cycle characteristics and safety. [Brief description of the drawings]
[0036] [Figure 1] FIG. 2 is a structural schematic diagram of a positive electrode plate for a lithium battery in Example 1. [Diagram 2] FIG. 4 is a structural schematic diagram of a positive electrode plate for a lithium battery in Example 2. [Diagram 3] FIG. 2 is a schematic diagram of a heavy-duty impact test according to the present invention. [Figure 4] FIG. 13 is a structural schematic diagram of a positive electrode plate for a lithium battery in Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0037] The present invention will be specifically described below with reference to certain figures and examples. It should be noted that the following examples are only used to further explain the present invention and are not to be understood as limiting the scope of protection of the present invention. Non-essential improvements and adjustments of the present invention made by those skilled in the art based on the content of the present invention also belong to the scope of protection of the present invention. Example 1
[0038] Step 1: An NCM positive electrode active layer was prepared, with the mass of active material being 100 g. Step 2: Component 1 LiTiOPO4 and component 2 Li 1.4 Al 0.4 Ti 1.6 25 kg of the mixed component composed of (PO4)3 and 500 kg of NMP were mixed uniformly and ground to a slurry with D50:300 nm. The ratio of component 1 to component 2 was 1:4. Step 3: 1 kg of PVDF was added to the slurry obtained in step 2 and stirred uniformly to produce a coating slurry with a viscosity value of 200 mPa·S. Step 4: The slurry obtained in step 3 was applied onto the NCM90 positive electrode active layer and baked to obtain a positive electrode plate with a coating thickness of 1 μm and a porosity of 40%. The positive electrode plate for lithium batteries manufactured by the above method includes a current collector 5, a positive electrode material layer located on the current collector 5, and a functional layer 3 located directly on the positive electrode material layer, as shown in the structural schematic diagram of FIG. 1, the positive electrode material layer includes a positive electrode active material 4, a conductive agent, and a binder, and the functional layer 3 includes a particle 1 of component 1 and a particle 2 of component 2, where the particles of component 1 and the particles of component 2 in the functional layer 3 are uniformly distributed, and some of the particles of component 1 and the particles of component 2 are diffused in the positive electrode material layer and distributed between the particles of the positive electrode active material 4. The positive electrode plate and the SiOC650 negative electrode were combined to assemble a soft-pack lithium battery, and the lithium battery manufactured as above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were performed, respectively. Specific test results of electrochemical properties are shown in Table 1, and safety test results are shown in Table 2. The test method for the electrochemical properties of the lithium battery used in this application is as follows. 1. Cycling characteristic test a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Discharge the battery at a constant current of 1C until the end-of-discharge voltage is reached, then stop discharging and record the discharge capacity, completing one cycle. c) Repeat steps a and b until the discharge capacity falls below 80% of the first cycle discharge capacity, at which point record the total number of cycles the battery has undergone. 2. Rate Test a) At 23℃±2℃, charge the battery at rates of 0.1C, 0.2C, 0.33C, 1C, 2C, and 3C to the charge end voltage, then discharge at the same rate current to the discharge end voltage, and repeat 4 cycles at the same rate. b) Record the discharge capacity at each rate. c) The ratio of the 2C or 3C discharge capacity to the 0.33C discharge capacity is calculated, expressed as 2C / 0.33C or 3C / 0.33C, and the rate characteristics are evaluated. 3. High temperature cycle a) At 45°C, charge at a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging, and stop charging when the charging current rate drops to 0.05C. b) Leave the battery at 45°C for 5 hours. c) Under high temperature conditions of 45°C, the battery is discharged at a constant current of 1C until the discharge end voltage is reached, then the discharge is stopped and the discharge capacity is recorded, which completes one cycle. d) Repeat steps a through c until the discharge capacity falls below 80% of the first cycle discharge capacity, at which point record the battery's discharge capacity and the total number of cycles. The safety test method for lithium-ion batteries is as follows: 1. Overcharging a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Continue charging the battery at a constant current of 1C until the battery begins to experience thermal runaway, and record the battery voltage when thermal runaway begins. 2. Hotbox a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Place the battery in the test box. Heat the test box at a rate of 5℃ / min. After the temperature inside the box reaches 160℃±2℃, keep the temperature constant for 1 hour. If the battery does not emit smoke, fire or explode, it passes; if not, it fails. 3. Falling a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Free fall from a height of 1 m onto a concrete slab. The soft-pack battery is dropped once on each side for a total of six tests. After six tests, if the battery does not emit smoke, catch fire or explode, it is considered to have passed the test; otherwise, it has failed the test. 4. Heavy object impact a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) A battery 8 is placed on the surface of the platform, and a metal rod 9 with a diameter of 15.8 mm±0.2 mm is placed horizontally on the upper surface of the geometric center of the battery. A weight of 9.1 kg±0.1 kg is allowed to fall freely from a height of 610 mm±25 mm onto the surface of the battery on which the metal rod is placed, and the battery is observed for 6 hours. A schematic diagram of the heavy-weight impact test is shown in Figure 3, where 5 is a towing rope, 6 is a guide pipe, and 7 is a steel impact box (hinged door is not shown). Only the large surfaces of the soft-pack batteries are impact tested, ensuring that only one impact test is performed per sample. If the battery does not emit smoke, fire or explode, it passes; if not, it fails. 5. Stab a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Using a φ8 mm high-temperature resistant steel needle (the cone angle of the needle tip is 45°, the surface of the needle is shiny and free of rust, oxide layers and oil stains), pierce the battery at the geometric center of the piercing surface from a direction perpendicular to the battery plate at a speed of 25 mm / s, and leave the steel needle inside the battery. c) Observe for 1 hour. If the battery does not emit smoke, fire or explode, it passes; if not, it fails. Example 2
[0039] The mixed component 25 kg consisting of component 1 and component 2 was changed to one containing only 25 kg of component 1 and not containing component 2, the positive electrode active material was changed to NCM83, and the battery structure was changed to NCM83||SiOC650, with the other parameters being the same as in Example 1. The manufactured positive electrode plate for lithium batteries includes a current collector 5, a positive electrode material layer located on the current collector 5, and a functional layer 3 located directly on the positive electrode material layer, as shown in the structural schematic diagram of FIG. 2, the positive electrode material layer includes a positive electrode active material 4, a conductive agent, and a binder, and the functional layer 3 includes particles 1 of component 1, where the particles of component 1 in the functional layer 3 are uniformly distributed, and some of the particles of component 1 are diffused in the positive electrode material layer and distributed between the particles of the positive electrode active material 4. The lithium batteries manufactured as described above were subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the lithium battery manufactured using this positive electrode plate are shown in Table 1, and the safety test results are shown in Table 2. Example 3
[0040] The other parameters were the same as in Example 1, except that component 2 was changed to AlPO4, the positive electrode active material was changed to NCM83, the negative electrode was changed to SiOC450, and the battery structure was changed to NCM83||SiOC450. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 4
[0041] Component 2 is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in components 1 and 2 1.4 Al 0.4 Ti 1.6 The mass ratio of (PO4)3 and AlPO4 was 1:8:1, the positive electrode active material was changed to LCO, the negative electrode was changed to SiOC450, and the battery structure was changed to LCO||SiOC450, and the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 5
[0042] The 25 kg mixed component consisting of components 1 and 2 was changed to one containing only component 1 LiTaOSiO4 25 kg and not containing component 2, the positive electrode active material was changed to LFP, the negative electrode was changed to graphite, and the battery structure was changed to LFP||graphite, with the other parameters being the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. Table 1 shows the specific test results of the electrochemical properties of the manufactured lithium battery, and Table 2 shows the results of the safety tests. Example 6
[0043] Component 1 was changed to LiTaOGeO4 and component 2 was changed to Li 1.4 Al0.4 Ge 1.6 The other parameters were the same as in Example 1, except that the active material of the positive electrode was changed to (PO4)3, the active material of the positive electrode was changed to NCM83, the active material of the negative electrode was changed to graphite, and the battery structure was changed to NCM83||graphite. The lithium batteries manufactured as described above were subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium batteries are shown in Table 1, and the results of the safety tests are shown in Table 2. Example 7
[0044] Component 2 is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in components 1 and 2 1.4 Al 0.4 Ti 1.6 The mass ratio of (PO4)3 and AlPO4 was 1:8:1, and the porosity was changed to 80%, with the other parameters being the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 8
[0045] Component 2 is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in components 1 and 2 1.4 Al 0.4 Ti 1.6 The mass ratio of (PO4)3 and AlPO4 was 1:8:1, and the porosity was changed to 20%, with the other parameters being the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 9
[0046] Component 2 is Li1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in components 1 and 2 1.4 Al 0.4 Ti 1.6 The mass ratio of (PO4)3 and AlPO4 was changed to 1:8:1, and the coating thickness was changed to 500 nm. Each primary particle of the mixed component contained component 1 crystal type and component 2 crystal type particles, and the particle diameter D50 of the primary particle of the mixed component was 300 nm, and the morphology of the mixed component of component 1 and component 2 was shown in FIG. 4, where 1 is the mixed component of component 1 and component 2 in one particle, 2 is the coating, 3 is the active material, and 4 is the current collector. Other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were performed. Specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 10
[0047] Component 2 is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in components 1 and 2 1.4 Al 0.4 Ti 1.6 The mass ratio of (PO4)3 and AlPO4 was 1:8:1, and the coating thickness was changed to 10 μm, with the other parameters being the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 11
[0048] Component 2 is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in components 1 and 2 1.4 Al 0.4 Ti 1.6The mass ratio of (PO4)3 and AlPO4 was 1:8:1, the porosity was changed to 20%, and the D50 of the mixed component consisting of component 1 and component 2 was 50 nm, except that the remaining parameters were the same as in Example 9. After the above-mentioned lithium battery was subjected to processes such as injection, formation, and capacity grading, electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the lithium battery manufactured are shown in Table 1, and the safety test results are shown in Table 2. Example 12
[0049] Component 2 is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in components 1 and 2 1.4 Al 0.4 Ti 1.6 The mass ratio of (PO4)3 and AlPO4 was 1:8:1, and the D50 of the mixed component consisting of component 1 and component 2 was changed to 1 μm, and the remaining parameters were the same as in Example 9. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 13
[0050] Component 2 is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in components 1 and 2 1.4 Al 0.4 Ti 1.6 The mass ratio of (PO4)3 and AlPO4 was 1:8:1, the D50 of the mixed component consisting of component 1 and component 2 was changed to 50 nm, the coating thickness was changed to 10 nm, and the remaining parameters were the same as in Example 9. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 1
[0051] Except for not including components 1 and 2, the other parameters were the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 2
[0052] Other than the absence of components 1 and 2, the positive electrode active material was changed to NCM83, and the battery structure was changed to NCM83||SiOC650, the other parameters were the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 3
[0053] Other than the absence of components 1 and 2, the positive electrode active material was changed to NCM83, the negative electrode was changed to SiOC450, and the battery structure was changed to NCM83||SiOC450, the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 4
[0054] Other than the absence of component 1 and component 2, the positive electrode active material was changed to LCO, the negative electrode was made to SiOC450, and the battery structure was made to LCO||SiOC450, the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 5
[0055] Other than not containing components 1 and 2, changing the positive electrode active material to LFP, changing the negative electrode to graphite, and changing the battery structure to LFP||graphite, the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were carried out. Specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 6
[0056] Other than the absence of components 1 and 2, the positive electrode active material was changed to NCM83, the negative electrode was graphite, and the battery structure was NCM83||graphite, the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 7
[0057] The other parameters were the same as in Example 1, except that the 25 kg of the mixed component consisting of components 1 and 2 was changed to 25 kg of Al2O3. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 8
[0058] The 25 kg mixed component consisting of component 1 and component 2 was changed to 25 kg ZnO, the positive electrode active material was changed to NCM83, and the battery structure was changed to NCM83||SiOC650, with the other parameters being the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. Table 1 shows the specific test results of the electrochemical properties of the manufactured lithium battery, and Table 2 shows the results of the safety tests. Comparative Example 9
[0059] 25 kg of a mixture consisting of components 1 and 2 is placed in Li 1.4 Al 0.4 Ti 1.6 The other parameters were the same as in Example 1, except that the weight of the battery was changed to 325 kg (PO4), the positive electrode active material was changed to NCM83, the negative electrode was changed to SiOC450, and the battery structure was changed to NCM83||SiOC450. The lithium batteries manufactured as described above were subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. Table 1 shows the specific test results of the electrochemical properties of the manufactured lithium batteries, and Table 2 shows the results of the safety tests. Comparative Example 10
[0060] The 25 kg of the mixed component consisting of component 1 and component 2 was changed to 25 kg of AlPO4, the positive electrode active material was changed to LCO, the negative electrode was changed to SiOC450, and the battery structure was changed to LCO||SiOC450, and the other parameters were the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 11
[0061] 25 kg of the mixture consisting of components 1 and 2 is 0.5 La 0.5 The other parameters were the same as in Example 1, except that the TiO3 was changed to 25 kg, the positive electrode active material was changed to LFP, the negative electrode was changed to graphite, and the battery structure was changed to LFP||graphite. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 12
[0062] 25 kg of a mixture consisting of components 1 and 2 is added to Li7La3Zr2O 12The weight of the battery was changed to 25 kg, the positive electrode active material was changed to NCM83, the negative electrode was changed to graphite, and the battery structure was changed to NCM83||graphite, with the other parameters being the same as in Example 1. The lithium batteries manufactured as described above were subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium batteries are shown in Table 1, and the safety test results are shown in Table 2. Table 1 shows the electrochemical property data of the examples.
[0063] [Table 1] Table 2 shows safety data for the examples.
[0064] [Table 2]
[0065] From the data in Tables 1 and 2, it can be seen that the rate characteristics, cycle characteristics and safety of a battery can be significantly improved by coating the positive electrode surface with a functional layer containing component 1 or a mixture of components 1 and 2. Comparing Example 5 with Comparative Example 11, it was found that constructing a highly efficient CEI is the key to improving the electrical characteristics and safety of liquid batteries and solid batteries, so coating the positive electrode with component 1 has a much stronger effect of improving the battery rate characteristics, cycle characteristics and safety than coating a solid electrolyte with high lithium ion conductivity. From the comparison of Example 1 with Examples 7 and 8, it was found that there is an optimal design for the porosity of the functional layer on the positive electrode plate of the lithium battery of the present invention, and if the porosity is too small, it is disadvantageous to the rate characteristics of the battery, and if the porosity is too large, it is disadvantageous to the cycle characteristics of the battery. From the comparison of Example 1 with Examples 9, 10 and 13, it was found that there is an optimal thickness for the functional layer, and if the thickness is too small, it is disadvantageous to the safety, and if the thickness is too large, it is disadvantageous to the rate characteristics. Comparing Example 1 with Examples 11 and 12, it is found that there is an optimal particle size for components 1 and 2, and optimizing the particle size can improve the electrical properties and safety of the battery. If the particle size is too small, the additive particles are prone to agglomeration, which affects the rate characteristics. If the particle size is too large, the additive particles cannot make sufficient contact with the surface of the active material particles, which particularly affects the rate characteristics and safety. If the particle size is too small or too large, it is disadvantageous to construct a stable CEI.
[0066] It should be understood that the above embodiments are merely exemplary embodiments adopted to explain the principles of the present invention, but the present invention is not limited thereto. Those skilled in the art can make various modifications and improvements without departing from the spirit and essence of the present invention, and these modifications and improvements are considered to be within the protection scope of the present invention.
Claims
1. A positive electrode plate for a lithium battery comprising a positive electrode material layer and a functional layer located directly on the positive electrode material layer, The functional layer material includes component 1, and component 1 includes Li 1-x1 Ti 1-x1 A x1 O.P.O. 4 , Li 1-x1 Ti 1-x1 A x1 P.O. 5 , Li 2-y1 Ti 1-y1 A y1 OM1O 4 , Li 2-y1 Ti 1-y1 A y1 M1O 5 wherein 0≦x1≦0.7, 0≦y1≦1, A is at least one selected from Nb, Ta, and Sb, and M1 is at least one selected from Si and Ge; The component 1 is preferably LiTiOPO 4 , Li 0.9 Nb 0.1 Ti 0.9 O.P.O. 4 , Li 0.9 T 0.1 Ti 0.9 O.P.O. 4 , Li 2 TiOSiO 4 , LiTaOGeO 4 13. A positive electrode for a lithium battery, comprising at least one of the following:
2. The functional layer material further includes component 2, which is LiM2 2 (P.O. 4 ) 3 , Li 1+x2 A x2 M2 2-x2 (P.O. 4 ) 3 , M2O 2 , Li 16-4y2 M2 y2 O 8 , M2P 2 O 7 , M3PO 4 , M3 2 SiO 5 , M4 3 (P.O. 4 ) 2 , M4 2 SiO 4 wherein M2 is one selected from Ti, Ge, Zr, and Hf, where 0<x2<0.6; M3 and M4 are independently any one selected from Al, Ga, Sc, Y, Ca, Sr, Zn, Si, In, Lu, La, Fe, Cr, and Ge, where 3<y2<4; The component 2 is preferably InPO 4 , LATP, AlPO 4 , LAGP, LATP+AlPO 4 , LAGP+Al 2 SiO 5 , InPO 4 + LATP, Al 2 SiO 5 , TiO 2 +LiTi 2 (P.O. 4 ) 3 , TiP 2 O 7 + LiGe 2 (P.O. 4 ) 3 2. The positive electrode plate for a lithium battery according to claim 1, wherein the positive electrode plate is one of the following:
3. The positive electrode plate for a lithium battery according to claim 1, characterized in that in the functional layer material, the form of the mixed component composed of component 1 and component 2 is a form in which particles of component 1 and particles of component 2 are uniformly mixed with each other, or each primary particle contains a crystal form of component 1 and a crystal form of component 2.
4. The positive electrode plate for a lithium battery according to claim 1, characterized in that the functional layer has a three-dimensional porous structure having a porosity p (20%≦p≦80%) and a thickness h (0 μm<h≦10 μm).
5. The positive electrode plate for a lithium battery according to claim 1, characterized in that the particle size of component 1 in the functional layer is 10 nm to 10 μm, preferably 50 nm to 1 μm.
6. The positive electrode plate for a lithium battery according to claim 2, characterized in that the particle size of component 2 in the functional layer is 10 nm to 10 μm, preferably 50 nm to 1 μm.
7. 2. The positive electrode plate for lithium batteries according to claim 1, wherein the positive electrode active material comprises at least one of a lithium cobalt oxide positive electrode and a modified material thereof, an NCM ternary positive electrode and a modified material thereof, an NCA ternary positive electrode and a modified material thereof, a lithium nickel manganate positive electrode and a modified material thereof, a lithium rich positive electrode and a modified material thereof, and a lithium iron phosphate positive electrode and a modified material thereof.
8. Step 1 of producing a positive electrode active layer; Step 2: uniformly mixing component 1 or a mixture of component 1 and component 2 with a solvent and pulverizing the mixture to form a slurry having a size of 10 nm to 10 μm; Step 3 of adding a binder to the slurry obtained in step 2 and uniformly mixing to produce a coating slurry; and step 4 of applying the slurry obtained in step 3 onto a positive electrode active layer and drying to obtain a positive electrode plate. The method for producing a positive electrode plate for a lithium battery according to any one of claims 1 to 6.
9. The method according to claim 7, wherein the solvent comprises at least one of deionized water, ethanol, NMP, alcohol, isopropanol, and acetone.
10. A lithium battery cell comprising a positive electrode plate, a negative electrode plate, a separator, an electrolyte, and a case, the positive electrode plate being the positive electrode plate according to any one of claims 1 to 7.
11. 10. The lithium battery cell according to claim 9, wherein the lithium battery is a liquid battery or a solid-state battery.
Citation Information
Patent Citations
All solid battery
JP2011150817A
Composite compound with mixed crystalline structure
US20090220860A1