Dyed polyethylene yarn and functional fabric containing same

The spun-dyed polyethylene yarn addresses the challenge of uniform dyeing in high-density polyethylene by controlling pigment content and properties, ensuring excellent color uniformity and thermal conductivity for high-quality fabrics.

JP2024543221AActive Publication Date: 2024-11-19KOLON INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024532967
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-08
Filing Date
2022-12-06
Publication Date
2024-11-19
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

High-density polyethylene yarns are difficult to dye uniformly due to their hydrophobic nature and high crystallinity, leading to uneven color distribution and deterioration of physical properties when pigments are added, affecting the quality and performance of the final products.

Method used

A spun-dyed polyethylene yarn is developed with a specific formula for L*, a*, and b* values, ensuring uniform color distribution by controlling pigment content (0.00005 to 1 wt%) and maintaining thermal conductivity, with properties like initial modulus (10 to 300 cN/dtex), strength (1.5 to 20 g/d), and melt index (0.5 to 22 g/10 min).

Benefits of technology

The yarn achieves excellent color uniformity and retains high thermal conductivity, enabling the production of fabrics with superior cooling properties and consistent quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543221000001_ABST
    Figure 2024543221000001_ABST
Patent Text Reader

Abstract

The present invention relates to a dyed polyethylene yarn and a functional fabric containing the same, and more specifically to a dyed polyethylene yarn having excellent color uniformity and a functional fabric containing the same. In the dyed polyethylene yarn containing a pigment according to the present invention, the L*, a*, and b* measured under the following measurement conditions satisfy the following formula. [Measurement conditions] The dyed polyethylene yarn is wound around a flat substrate to form a measurement area, and CCM (Computer Color Matching) measurement is performed on the measurement area. CCM measurement is performed every time the dyed polyethylene yarn is wound around the substrate 70 times, and measurements are performed at least n times (n is a natural number of 50 or more) [Formula] (C max -C min ) / C aver ×100≦15(C max , C min , and C aver (means the maximum, minimum, and average value for any one selected from L*, a*, and b*, respectively.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dyed polyethylene yarn and a functional fabric containing the same, and more particularly to a dyed polyethylene yarn having excellent color uniformity and a functional fabric containing the same. [Background technology]

[0002] High density polyethylene (HDPE) yarn is 0.94g / cm 3 High-density polyethylene yarn refers to a high-strength polyethylene raw yarn having a density of 1000 or more. High-density polyethylene raw yarn is used as a variety of materials that require high strength, such as sports ropes, fishing lines, protective clothing, bulletproof clothing, and stab-proof clothing, and is also used in a variety of composite materials that require ultra-high strength.

[0003] In addition, high-density polyethylene yarn has high thermal conductivity due to lattice vibrations called phonons, and has excellent lightweight properties as its specific gravity is approximately 0.93, making it light enough to float on water.

[0004] Therefore, it is used for a variety of applications, including not only textile products that require high strength, such as the aforementioned sports ropes, fishing lines, protective clothing, bulletproof clothing, and stab-resistant clothing, but also summer clothing, work clothing, and sportswear that require a cool feel.

[0005] However, high density polyethylene yarn is known as a dye-resistant fiber because it is almost impossible to dye it with any dye in a dyeing system due to its hydrophobicity caused by its high crystallinity.

[0006] Currently, there are two methods for dyeing such high density polyethylene yarns: one is a dyeing method in which a pigment is added during spinning, and the other is a polymer blending technique in which other polymers that can be dyed are mixed.

[0007] However, the dyed polyethylene yarn produced by the polymer blending technique has a disadvantage in that it is difficult to maintain the physical properties unique to high-density polyethylene yarn, such as high thermal conductivity and light weight, as polymers having physical properties other than polyethylene are mixed in.

[0008] Therefore, conventionally, dyed polyethylene yarns have been used, which are manufactured through a dyeing method in which a masterbatch chip containing a pigment is melt-spun, as disclosed in Korean Patent Registration No. 10-1992444, 'Method for manufacturing dyed polyethylene multifilament false twisted yarn'.

[0009] However, such conventional dyed polyethylene yarn has a problem that the pigment is difficult to mix uniformly with polyethylene having a relatively high viscosity, and the uneven mixing between the pigment and the polyethylene raw material causes serious color unevenness of the yarn. Therefore, not only does the unevenness of the dyed yarn itself reduce the quality, but the physical properties of the yarn such as strength are also reduced as a large amount of pigment is added to express the desired color. Furthermore, the quality of the final product manufactured from the yarn is also reduced. Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a dyed polyethylene yarn having excellent color uniformity and a functional fabric containing the same. [Means for solving the problem]

[0011] The dyed polyethylene yarn according to the present invention satisfies the following formulas for L*, a*, and b* measured under the following measurement conditions in the dyed polyethylene yarn containing a pigment.

[0012] [Measurement conditions] The dyed polyethylene yarn is wound around a flat substrate to form a measurement area, and a CCM (Computer Color Matching) measurement is performed on the measurement area. The CCM measurement is performed every time the dyed polyethylene yarn is wound around the substrate 70 times, and the measurement is performed at least n times (n is a natural number of 50 or more).

[0013] [formula] (C max -C min ) / C aver ×100≦15

[0014] (C max , C min , and C aver respectively mean the maximum, minimum, and average value of any one selected from L*, a*, and b*.)

[0015] In the dyed polyethylene yarn according to one embodiment of the present invention, the standard deviation of the L* value may be 3 or less when the yarn is measured by CCM.

[0016] In the dyed polyethylene yarn according to one embodiment of the present invention, the pigment may be contained in an amount of 0.00005 to 1 wt % based on the total weight of the dyed polyethylene yarn.

[0017] In the dyed polyethylene yarn according to one embodiment of the present invention, the yarn may have a crystallinity of 60 to 80%.

[0018] In the dyed polyethylene yarn according to one embodiment of the present invention, the yarn may have an initial modulus of 10 to 300 cN / dtex and a strength of 1.5 to 20 g / d, as measured by ASTM D2256.

[0019] In the dyed polyethylene yarn according to one embodiment of the present invention, the yarn may have a melt index (MI, @190°C) of 0.5 to 22 g / 10 min as measured according to ASTM D1238.

[0020] In the dyed polyethylene yarn according to one embodiment of the present invention, the yarn may have a dry heat shrinkage (@100°C) according to ASTM D4974-04 of 2 to 15%.

[0021] The functional fabric according to the present invention is produced from the above-mentioned dyed polyethylene yarn.

[0022] In the functional fabric according to an embodiment of the present invention, the fabric has a cool touch sensation of 0.1 to 0.3 W / cm, measured at 20±2°C and 65±2% RH by contacting a 30±2°C hot plate (T-box) with the fabric at 20±2°C. 2 may be also possible.

[0023] In the functional fabric according to an embodiment of the present invention, the fabric may have a thermal conductivity of 0.05 to 0.25 W / mK in the thickness direction measured at 2.0±2°C and 65±2% RH by contacting a heat source plate (BT-box) of 30±2°C with the fabric of 20±2°C. Effect of the Invention

[0024] The polyethylene yarn according to the present invention has excellent color uniformity and therefore has excellent color development properties compared to the amount of pigment added.

[0025] In addition, the polyethylene yarn according to the present invention can maintain the excellent thermal conductivity inherent to high density polyethylene even though a pigment is added, making it possible to manufacture fabrics having excellent cool sensation properties.

[0026] In addition, the functional fabric according to the present invention contains polyethylene yarn having excellent color uniformity and excellent thermal conductivity, so that it can have excellent color development and color uniformity and at the same time exhibit cool feeling properties. [Brief description of the drawings]

[0027] [Figure 1]FIG. 2 is a schematic diagram showing a process for producing a raw yarn according to one embodiment of the present invention. [Diagram 2] 1 is a photograph of an apparatus for measuring CCM (Computer Color Matching) of a functional fabric according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram illustrating an apparatus for measuring the cool touch sensation of a functional fabric according to one embodiment of the present invention. [Figure 4] FIG. 2 is a schematic diagram illustrating an apparatus for measuring the thermal conductivity in the thickness direction of a functional fabric according to one embodiment of the present invention. [Diagram 5] 1 is a CCM measurement result of a yarn according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Unless otherwise defined, technical and scientific terms used in this specification have the meanings that are commonly understood by those having ordinary knowledge in the technical field to which this invention belongs, and in the following description and attached drawings, descriptions of known functions and configurations that may unnecessarily obscure the gist of the present invention will be omitted.

[0029] Also, as used herein, the singular forms "a," "an," and "the" can be intended to include the plural forms as well, unless the context indicates otherwise.

[0030] Furthermore, units used in this specification, unless otherwise specified, are based on weight. For example, the unit of % or ratio means % by weight or weight ratio, and % by weight means the weight % of any one component in a total composition, unless otherwise defined.

[0031] In addition, the numerical ranges used herein include the lower limit, the upper limit, all values ​​within the range, increments logically derived in the form and width of the range defined, all values ​​limited therein, and all possible combinations of upper and lower limits of numerical ranges limited in different forms. Unless otherwise specified in the specification of the present invention, values ​​outside the numerical range that may occur due to experimental error or rounding of values ​​are also included in the defined numerical range.

[0032] As used herein, the term 'comprising' is an open-ended term having the same meaning as terms such as 'comprising,' 'containing,' 'having,' or 'characterized by,' and does not exclude additional, unrecited elements, materials, or steps.

[0033] Conventional dyed polyethylene yarns have a problem in that the pigment is difficult to mix uniformly with polyethylene having a relatively high viscosity, and the yarn color is seriously non-uniform due to the non-uniform mixing between the pigment and the polyethylene raw material. Therefore, not only does the quality of the dyed yarn itself deteriorate due to the non-uniformity, but the yarn physical properties such as strength deteriorate as a large amount of pigment is added to express the desired color. Furthermore, the quality of the final product manufactured from the yarn also deteriorates.

[0034] Therefore, the applicant conducted extensive research for a long period of time to develop a polyethylene fiber having excellent color uniformity while maintaining the physical properties, and as a result, developed a new dyed polyethylene having excellent color uniformity by increasing the degree of mixing between the pigment and the raw polyethylene yarn materials.

[0035] Specifically, the dyed polyethylene yarn according to the present invention is a dyed polyethylene yarn containing a pigment, and satisfies the following formulas for L*, a*, and b* measured under the following measurement conditions.

[0036] [Measurement conditions] The dyed polyethylene yarn is wound around a flat substrate to form a measurement area, and a CCM (Computer Color Matching) measurement is performed on the measurement area. The CCM measurement is performed every time the dyed polyethylene yarn is wound around the substrate 70 times, and the measurement is performed at least n times (n is a natural number of 50 or more).

[0037] [formula] (C max -C min ) / C aver ×100≦15

[0038] (C max , C min , and C aver respectively mean the maximum, minimum, and average value of any one selected from L*, a*, and b*.)

[0039] Specifically, in the above formula, (C max -C min ) / C aver x 100 may be 10 or less, specifically 0.1 to 8, and more specifically 3 to 7. Such spun-dyed polyethylene raw yarn has excellent color uniformity, and thus has excellent coloring properties compared to the amount of pigment added. In addition, even though a small amount of pigment is added, the excellent coloring properties allow the excellent thermal conductivity inherent to high-density polyethylene to be maintained, and thus fabrics with excellent cooling properties can be manufactured.

[0040] Specifically, a dyed polyethylene yarn is wound around a planar substrate, so that an area covered with the dyed polyethylene, that is, a measurement area, is formed on the substrate.

[0041] In this case, when being wound around the substrate, the dyed polyethylene yarn wound for the n-1th time (n is a natural number of 2 or more) and the dyed polyethylene yarn wound for the nth time may come into contact with each other so as to proceed in either direction around the substrate.

[0042] Such a measurement area is formed by covering the base material with the dyed polyethylene fiber yarn, and thus the dyed polyethylene fiber yarn shows a color similar to that when it is manufactured into a fabric. The measurement area is not limited as long as it is an area that allows CCM measurement. However, the area that the measurement area occupies on the base material can be appropriately adjusted depending on the size of the base material, the thickness of the dyed polyethylene yarn, and the number of times it is wound. As a non-limiting example, the measurement area can be formed by winding a dyed polyethylene yarn having a thickness of 410De 30 times or more, specifically 40 to 100 times, and more specifically 50 to 90 times, on a square plate-shaped base material having a width of 6.5 cm, a length of 6.5 cm, and a height of 0.5 cm.

[0043] After measuring the n-1 (n is a natural number greater than or equal to 2)th CCM through the measurement area formed by the above-mentioned method, when measuring the nth CCM, a measurement area for the nth CCM measurement can be formed on the measurement area formed for the n-1th CCM measurement.

[0044] In the following description, it is assumed that the measurement region formed first is a first measurement region, and the measurement region formed thereafter is a second measurement region.

[0045] After performing a CCM measurement on a first measurement area formed by winding the spun-dyed polyethylene yarn 70 times in one direction around the substrate, a CCM measurement is performed on a second measurement area formed by winding the spun-dyed polyethylene yarn again around the first measurement area. That is, the second measurement area is formed by winding the spun-dyed polyethylene yarn so as to cover the first measurement area while changing the traveling direction to the opposite direction of the substrate.

[0046] Thus, the second measurement area where the nth CCM is measured is the same size as the first measurement area where the n-1th CCM is measured, and the thickness of the measurement area formed on the substrate increases by the thickness of the original dyed polyethylene yarn when the second measurement area is formed on the first measurement area. The positions where the CCM is measured in the first measurement area and the second measurement area may be the same.

[0047] The L*, a*, and b* of the CCM measured through such a measurement area can satisfy the above equations.

[0048] Specifically, the dyed polyethylene yarn may contain, but is not limited to, 0.0001 to 0.5% by weight, more specifically 0.002 to 0.05% by weight, and even more specifically 0.01 to 0.03% by weight of the pigment based on the total weight, but within this range, it is possible to obtain excellent color development and color uniformity compared to the amount added.

[0049] Here, when the raw yarn is measured by CCM, the standard deviation of the L* value is 3 or less, specifically 2 or less, more specifically 1.5 or less, and the yarn may have an excellent color uniformity that is not easily distinguished by the naked eye.

[0050] In the present invention, the pigment is not limited as long as it is a pigment or raw material that is known to be used in the conventional dyeing of polyethylene. As a specific example, when the polyethylene yarn is black, the pigment may be carbon black particles.

[0051] The spun-dyed polyethylene yarn may have an initial modulus measured by ASTM D2256 of 10 to 300 cN / dtex, specifically 50 to 300 cN / dtex, more specifically 70 to 150 cN / dtex. Here, the tenacity measured by ASTM D2256 may be 1.5 to 20 g / d, specifically 4 to 20 g / d, more specifically 10 to 15 g / d, but is not limited thereto. However, within the above range, the yarn may have high thermal conductivity and at the same time an appropriate high twist degree that is advantageous for weaving.

[0052] The dyed polyethylene yarn may have a polydispersity index of 5 to 20, more specifically 7 to 15, and the weight average molecular weight of the dyed polyethylene yarn may be 45,000 to 300,000 g / mol, preferably 100,000 to 200,000 g / mol. Within this range, the flowability of the molten material during melt extrusion of the yarn is good, thermal decomposition is prevented, and yarn breakage does not occur during drawing. This ensures processability, and therefore yarn with uniform physical properties can be produced, and a fabric with excellent durability can be provided.

[0053] The dyed polyethylene yarn may have a melt index (MI, @190°C) of 0.5 to 22 g / 10 min, specifically 1 to 10 g / 10 min, more specifically 2 to 8 g / 10 min, measured at 190°C and 2.16 kg according to ASTM D1238. The dyed polyethylene yarn may have a density of 0.93 to 0.97 g / cm. 3 The crystallinity of the spun polyethylene yarn may be 60-80%, specifically 65-75%, after spinning. The crystallinity of the polyethylene yarn may be determined together with the size of the crystallites during crystallinity analysis using an X-ray diffraction analyzer. As described above, when the melt index, density, and crystallinity are within the above ranges, heat is rapidly diffused and dissipated in the direction of the molecular chains connected through covalent bonds of high density polyethylene (HDPE) through lattices vibrations called 'phonons', and the moisture discharge function of sweat and breath is improved, providing a fabric with excellent cooling sensation.

[0054] The dyed polyethylene yarn has a very low dry heat shrinkage (@100°C) of 2 to 15%, specifically 2.7 to 5%, according to ASTM D4974-04, and therefore has excellent shape stability.

[0055] The original dyed polyethylene yarn of the present invention can be produced through an original dyeing method.

[0056] Specifically, the spun-dyed polyethylene yarn may be produced from a polyethylene resin composition including a color master batch produced by mixing a pigment with polyethylene in chip form, drying the mixture to produce a first master chip, and repeating the steps of melting the first master chip, remixing the pigment, and drying the mixture n times (n is a natural number of 1 or more) to produce an n-th master chip. Here, n may be, but is not limited to, 2 to 5, specifically, 2 to 3. By producing a resin composition by incorporating the color master batch produced from the above steps into a polyethylene resin, the spun-dyed polyethylene yarn may have better color uniformity.

[0057] The pigment content in the color masterbatch can be adjusted in various ways, but may be 0.05 to 10.0 wt %, specifically 0.1 to 5 wt %, based on the total weight of the color masterbatch. In this range, the pigment content is lower than that of conventional color masterbatches, but the color masterbatch can still have excellent color development.

[0058] In addition, the polyethylene resin composition containing such a color masterbatch can be appropriately mixed with the color masterbatch according to the pigment content ratio in the raw yarn described above. Specifically, the polyethylene resin composition can contain 0.1 to 10% by weight of the color masterbatch based on the total weight of the polyethylene resin composition.

[0059] The dyed polyethylene yarn produced by this dyeing method can have excellent color uniformity as described above, making it possible to provide high quality fabrics.

[0060] Hereinafter, a method for producing a spun-dyed polyethylene yarn according to one embodiment of the present invention will be specifically described with reference to FIG.

[0061] First, a pigment is mixed with polyethylene in chip form, and the dried first master chip is melted and mixed again to obtain a second master chip. Then, the second master chip and polyethylene in chip form are put into an extruder 100 and melted to obtain a dyed polyethylene melt.

[0062] Molten polyethylene is transported through a die 200 by a screw (not shown) in the extruder 100 and extruded through a number of holes formed in the die 200. The number of holes in the die 200 can be determined depending on the DPF (Denier Per Filament) and fineness of the raw yarn to be produced. For example, when producing a raw yarn having a total fineness of 75 denier, the die 200 can have 20 to 75 holes, and when producing a raw yarn having a total fineness of 450 denier, the die 200 can have 90 to 450 holes, preferably 100 to 400 holes.

[0063] The melting process in the extruder 100 and the extrusion process through the die 200 can be changed and applied depending on the melting index of the polyethylene chips, but specifically, for example, they are preferably performed at 150 to 315°C, preferably 250 to 315°C, and more preferably 265 to 310°C. That is, it is preferable that the extruder 100 and the die 200 are maintained at 150 to 315°C, preferably 250 to 315°C, and more preferably 265 to 310°C.

[0064] If the spinning temperature is less than 150° C., the polyethylene may not be uniformly melted due to the low spinning temperature, making spinning difficult, whereas if the spinning temperature exceeds 315° C., the polyethylene may be thermally decomposed, making it difficult to achieve the desired strength.

[0065] The ratio L / D of the hole length L to the hole diameter D of the spinneret 200 may be 3 to 40. If L / D is less than 3, a die swell phenomenon occurs during melt extrusion, making it difficult to control the elastic behavior of the polyethylene, resulting in poor spinnability, and if L / D exceeds 40, the molten polyethylene passing through the spinneret 200 may break due to a necking phenomenon, as well as cause uneven extrusion due to a pressure drop.

[0066] As the molten polyethylene is discharged from the holes of the spinneret 200, the polyethylene begins to solidify due to the difference between the spinning temperature and room temperature, forming a semi-solidified filament 11. In this specification, both the semi-solidified filament and the completely solidified filament are collectively referred to as "filament".

[0067] The filaments 11 are completely solidified by being cooled in a cooling section (or "quenching zone") 300. The filaments 11 can be cooled by air cooling.

[0068] In addition, by performing multi-stage cooling in the cooling section, crystallization can be performed more uniformly, which makes it easier to discharge moisture and sweat, and produces a raw yarn with excellent cooling sensation.

[0069] The cooled and fully solidified filaments 11 are then gathered by a concentrator 400 to form a multifilament 10.

[0070] As illustrated in Fig. 1, the polyethylene raw yarn of the present invention can be manufactured through a direct spin-draw (DSD) process. That is, the multifilament 10 is directly transferred to a multi-stage drawing section 500 including a plurality of godet roller sections GR1...GRn, and is multi-stage drawn at a total draw ratio of 2 to 20, preferably 3 to 15, and then wound on a winder 600. In addition, during the multi-stage drawing, a shrinkage drawing (relaxation) of 1 to 5% is imparted in the final drawing section, thereby providing a raw yarn with better durability.

[0071] Alternatively, the polyethylene raw yarn of the present invention can be produced by once winding the multifilament 10 as an undrawn yarn and then drawing the undrawn yarn. That is, the polyethylene raw yarn of the present invention can be produced through a two-stage process in which polyethylene is melt-spun to once produce an undrawn yarn and then the undrawn yarn is drawn.

[0072] The functional fabric according to the present invention contains the above-mentioned dyed polyethylene yarn, and by containing the dyed polyethylene yarn having excellent color uniformity and excellent thermal conductivity, it is possible to have excellent color development and color uniformity while at the same time exhibiting cooling properties.

[0073] The functional fabric according to the present invention may be one that uses the above-described dyed polyethylene yarn alone, or may further include a different type of yarn in order to impart other functionality. However, from the viewpoint of simultaneously having a cool sensation and excellent color uniformity, it is preferable to use the above-described polyethylene yarn alone.

[0074] Specifically, the functional fabric has a cooling sensation of 0.1 to 0.3 W / cm2 when measured at 20±2°C and 65±2% RH by contacting a hot plate (T-box) heated to 30±2°C with the fabric at 20±2°C. 2The thermal conductivity in the thickness direction measured by contacting a heat source plate (BT-box) heated to 30±2°C with a material at 20±2°C is 0.05~0.25W / mK. More specifically, the cool feeling to the touch is 0.15~0.22W / cm 2 The thermal conductivity can be 0.08~0.2W / mK. When the functional fabric having such a cooling sensation is later manufactured or processed into a product and worn by a user, it can provide an appropriate cooling sensation that allows the user to feel comfortable in a high temperature environment.

[0075] Such fabrics can be processed into cooling products that require appropriate cooling sensation. The products can be any conventional textile products, but preferably can be summer clothes, sportswear, masks, and work clothes for imparting cooling sensation to the human body.

[0076] Hereinafter, the present invention will be described in more detail with reference to the following examples. However, the following examples are merely a reference for explaining the present invention in detail, and the present invention is not limited thereto, and may be realized in various forms.

[0077] In addition, unless otherwise defined, all technical and scientific terms have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention belongs. The terms used in the description of this application are merely for the purpose of effectively describing a particular embodiment and are not intended to limit the present invention. In addition, the unit of additives not specifically described in the specification may be weight percent. EXAMPLES

[0078] The physical properties were measured as follows.

[0079] [Measurement of yarn physical properties] <1. CCM (Computer Color Matching) Measurement> As shown in Figure 2, the yarn was wound around a substrate measuring 6.5 cm wide, 6.5 cm long, and 0.5 cm high to form a measurement area, and CCM (Computer Color Matching) measurements were performed on the measurement area. The CCM measurements were performed every 70 times (±10) that the dyed polyethylene yarn was wound around the substrate. The total number of CCM measurements was 135.

[0080] The CCM was measured through a color difference meter (KAE1-063, GNB TECH) to derive the L*, a*, and b* values, as well as the values ​​of the following formulas.

[0081] [formula] (C max -C min ) / C aver ×100

[0082] (C max , C min , and C aver (means the maximum, minimum, and average value for any one selected from L*, a*, and b*, respectively.)

[0083] <2. Weight average molecular weight (Mw) (g / mol) and polydispersity index (PDI)> The polyethylene raw yarn was completely dissolved in the following solvent, and then the weight average molecular weight (Mw) and polydispersity index (Mw / Mn: PDI) of the polyethylene raw yarn were determined using the following gel permeation chromatography (GPC).

[0084] -Analytical equipment: Tosoh HLC-8321 GPC / HT -Column: PLgel guard (7.5 x 50 mm) + 2 x PLgel mixed-B (7.5 x 300 mm) -Column temperature: 160°C -Solvent: Trichlorobenzene (TCB) + 0.04 wt.% dibutylhydroxytoluene (BHT) (after drying with 0.1% CaCl2) -Injector and detector temperature: 160℃ -Detector: RI Detector -Flow rate: 1.0ml / min -Injection volume: 300mL -Sample concentration: 1.5mg / mL -Standard sample: polystyrene

[0085] <3. Strength (g / d), initial modulus (g / d)> The deformation-stress curves of the polyethylene yarns were obtained using a universal tensile tester from Instron Engineering Corp, Canton, Mass., according to the ASTM D2256 method. The sample length was 250 mm, the tensile speed was 300 mm / min, and the initial load was set to 0.05 g / d. The strength (g / d) was calculated from the stress and elongation at the break point, and the initial modulus (g / d) was calculated from the tangent line that gave the maximum slope near the origin of the curve. Five measurements were taken for each yarn, and the average value was calculated.

[0086] <4. Crystallinity> The crystallinity of the polyethylene yarn was measured using an XRD (X-ray Diffractometer) [manufacturer: PANalytical, model name: EMPYREAN]. Specifically, the polyethylene yarn was cut to prepare a sample having a length of 2.5 cm, and the sample was fixed to a sample holder, and then the measurement was performed under the following conditions.

[0087] -Light source (X-ray Source): Cu-K α radiation -Power: 45KV x 25mA - Mode: Continuous scan mode -Scan angle range: 10~40° -Scan speed: 0.1° / sec

[0088] <5. Strength (kgf), elongation at break (%)> The strength at break of the raw yarn samples was measured using an Instron testing machine (Instro Engineering Corp., Canton, Mass.) at a tensile speed of 300 m / min on a 250 mm sample according to ASTM D-885 test method.

[0089] <6. Dry heat shrinkage rate> According to the method of ASTM D4974-04, using a dry heat shrinkage measuring device (manufacturer: TESTRITE, model name: MK-V), the initial length L1 of the sample when a load of 0.2 g / d was applied, and the length L2 of the sample after 2 minutes had elapsed when a load of 0.2 g / d was applied at 100°C were measured, and then the dry heat shrinkage (%) of the raw yarn was calculated according to the following formula 2.

[0090] [Formula 2] Dry heat shrinkage rate (%)=[(L1-L2) / L1]×100

[0091] <7. Melting index> The melt index (MI, @190°C) was measured at 190°C and 2.16 kg according to ASTM D1238.

[0092] [Fabric property measurement] <1. Cool sensation to the touch> The measurements were conducted at the request of the Korea Clothing Testing and Research Institute using a KES-F7 (Thermo Labo II) device in a test environment of 20±2°C and 65±2% RH.

[0093] Specifically, a fabric sample having a size of 20cm x 20cm was prepared and left for 24 hours under conditions of 20±2°C temperature and 65±2% RH. Then, the fabric was measured for its contact coolness (Qmax) using a KES-F7 THERMO LABO II (Kato Tech Co., LTD.) device in a test environment of 20±2°C temperature and 65±2% RH. Specifically, as illustrated in FIG. 3, the fabric sample 23 was placed on a base plate (also called a 'Water-Box') 21 maintained at 20°C±2°C, and a hot plate (T-Box) 22a (contact area: 3cm x 3cm) heated to 30°C±2°C was placed on the fabric sample 23 for only 1 second. That is, the other surface of the fabric sample 23, one surface of which is in contact with the base plate 21, was instantaneously brought into contact with the T-Box 22a. The contact pressure applied to the fabric sample 23 by the T-Box 22a was 6gf / cm. 2 Then, the Qmax value displayed on a monitor (not shown) connected to the device was recorded. This test was repeated 10 times, and the arithmetic mean of the Qmax values ​​was calculated.

[0094] <2. Thermal conductivity> After preparing a fabric sample having a size of 20 cm x 20 cm, it was left for 24 hours under the conditions of a temperature of 20 ± 2 ° C and a RH of 65 ± 2%. Then, in a test environment of a temperature of 20 ± 2 ° C and a RH of 65 ± 2%, the thermal conductivity and heat transfer coefficient of the fabric were measured using a KES-F7 THERMO LABO II (Kato Tech Co., LTD.) device. Specifically, as illustrated in FIG. 4, the fabric sample 23 was placed on a base plate 21 maintained at 20 ° C ± 2 ° C, and a heat source plate (BT-Box) 22b (contact area: 5 cm x 5 cm) at 30 ° C ± 2 ° C was placed on the fabric sample 23 for 1 minute. While the BT-Box 22b was in contact with the fabric sample 23, heat was continuously supplied to the BT-Box 22b so that the temperature was maintained at 30 ° C ± 2 ° C. The amount of heat supplied to maintain the temperature of the BT-Box 22b (i.e., heat flow loss) was displayed on a monitor (not shown) connected to the device. This test was repeated five times, and the arithmetic average of the heat flow loss was calculated. The thermal conductivity and heat transfer coefficient of the fabric were then calculated using the following Equations 3 and 4.

[0095] [Formula 3] K = (W D) / (A ΔT)

[0096] [Formula 4] k=K / D

[0097] Here, K is the thermal conductivity (W / cm °C), D is the thickness (cm) of the fabric sample 23, and A is the contact area of ​​the BT-Box 22b (= 25 cm 2 ), ΔT is the temperature difference between the two sides of the fabric sample 23 (=10°C), W is the heat flow loss (Watt), and k is the heat transfer coefficient (W / cm 2 ·℃).

[0098] [Example 1] <Production of color master batches> After mixing the pigment with polyethylene in the form of chips, the dried primary master chip was melted and mixed again to obtain a secondary master chip, i.e., a color master batch, in which 0.83% by weight of the pigment was mixed with respect to the total weight of the color master chip.

[0099] <Production of polyethylene yarn> A dyed polyethylene yarn having a total fiber size of 410 denier was produced.

[0100] Specifically, polyethylene chips having a weight average molecular weight (Mw) of 154,604 g / mol and the second master chips were put into an extruder and melted to form a melt. At this time, 3% by weight of the second master chips was mixed with respect to the total weight of the melt. The melt was extruded through a die having 200 holes. The ratio of hole length (L) to hole diameter (D) of the die, L / D, was 6. The die temperature was 270°C.

[0101] The filaments formed while being discharged from the nozzle holes of the spinneret were cooled, bundled, and then stretched. The stretched multifilament yarn was then wound on a winder. The winding tension was 0.8 g / d.

[0102] The physical properties of the produced raw yarn were measured and derived (C max -C min ) / C aver The ×100 value was taken as the ΔC value and is shown in Table 1 below.

[0103] <Manufacturing of functional fabrics> The dyed polyethylene yarn thus produced was woven to a surface density of 500 g / m 2 The physical properties of the functional fabric thus produced were measured and are shown in Table 2 below.

[0104] [Example 2] The yarn and fabric were manufactured in the same manner as in Example 1, except that the pigment content in the color masterbatch was changed from 0.83 wt% to 0.40 wt%, and the color masterbatch content in the melt was changed from 3 wt% to 3.3 wt% in Example 1. The physical properties of the yarn and fabric manufactured in the same manner as in Example 1 were measured and are shown in Tables 1 and 2 below, respectively.

[0105] [Example 3] The yarn and fabric were manufactured in the same manner as in Example 1, except that the pigment content in the color masterbatch was changed from 0.83 wt% to 0.40 wt%, and the color masterbatch content in the melt was changed from 3 wt% to 3.8 wt%. The physical properties of the yarn and fabric manufactured in the same manner as in Example 1 were measured and are shown in Tables 1 and 2 below, respectively.

[0106] [Comparative Example 1] In Example 1, a pigment was mixed with polyethylene in chip form having a weight average molecular weight (Mw) of 134,277 g / mol, and then dried to prepare a primary master chip, which was used as a color master batch, and yarn and fabric were manufactured in the same manner as in Example 1, except that the pigment content in the color master batch was changed to 10.0 wt%, and the color master batch content in the melt was changed from 3 wt% to 0.25 wt%. In addition, the physical properties of the yarn and fabric manufactured in the same manner as in Example 1 were measured and are shown in Tables 1 and 2 below, respectively.

[0107] [Table 1]

[0108] [Table 2]

[0109] Referring to Tables 1 and 2 above, it can be seen that the fabrics according to the embodiments have excellent mechanical properties such as strength and elongation, as well as cool feeling properties, and the color uniformity of the raw yarn is very good.

[0110] Fig. 5 shows the results of measuring the time-dependent CCM value through the measurement area of ​​the spun-dyed polyethylene yarn shown in Fig. 2, in which the spun-dyed polyethylene yarn was spun according to the embodiment. Specifically, the CCM values ​​of the spun-dyed polyethylene yarns according to Examples 1 to 3 and the comparative example are shown.

[0111] Referring to FIG. 5, it was confirmed that the dyed polyethylene yarn according to the present invention hardly changes in color even during long-term spinning, making it possible to produce yarn with excellent color uniformity.

[0112] As described above, the present invention has been described using specific details and limited examples and drawings. However, this is merely provided to assist in a more general understanding of the present invention. The present invention is not limited to the above-described examples. Those skilled in the art will appreciate that various modifications and variations can be made from such descriptions.

[0113] Therefore, the concept of the present invention should not be limited to the described embodiments, and all things that are equivalent or have equivalent variations to the scope of the claims, as well as the scope of the claims described below, should be considered to fall within the scope of the concept of the present invention. [Explanation of symbols]

[0114] 10: Multifilament 11: Filament 21: Base plate 23: Fabric 22a:T-box 22b:BT-box 100: Extruder 200: Base 300: Cooling section 400:Focusing part 500: Stretching part 600: Winder

Claims

1. In the pigment-containing dyed polyethylene yarn, A dyed polyethylene yarn, the L*, a*, and b* of which, measured under the following measurement conditions, satisfy the following formulas: [Measurement conditions] The dyed polyethylene yarn is wound around a flat substrate to form a measurement area, and a CCM (Computer Color Matching) measurement is performed on the measurement area. The CCM measurement is performed every time the dyed polyethylene yarn is wound around the substrate 70 times, and the measurement is performed at least n times (n is a natural number of 50 or more). [formula] (C max -C min ) / C aver ×100≦15 (C max , C min , and C aver means the maximum, minimum, and average value for any one selected from L*, a*, and b*, respectively.)

2. 2. The dyed polyethylene yarn according to claim 1, wherein the standard deviation of the L* value is 3 or less when the yarn is measured by CCM.

3. The dyed polyethylene yarn according to claim 1, wherein the pigment is contained in an amount of 0.00005 to 1 wt % based on the total weight of the dyed polyethylene yarn.

4. The dyed polyethylene yarn according to claim 1, wherein the yarn has a crystallinity of 60 to 80%.

5. 2. The method according to claim 1, wherein the yarn has an initial modulus of 10 to 300 cN / dtex and a tenacity of 1.5 to 20 g / d, as measured by ASTM D2256.

6. The method according to claim 1, wherein the yarn has a melt index (MI, @190°C) of 0.5 to 22 g / 10 min, as measured according to ASTM D1238.

7. The dyed polyethylene yarn according to claim 1, wherein the yarn has a dry heat shrinkage (@100°C) according to ASTM D4974-04 of 2 to 15%.

8. A functional fabric produced from the dyed polyethylene yarn of any one of claims 1 to 7.

9. The fabric has a contact cooling sensation of 0.1 to 0.3 W / cm2 when measured at 20±2°C and 65±2% RH by contacting a 30±2°C hot plate (T-box) with the fabric at 20±2°C. 2 The functional fabric according to claim 8.

10. The fabric has a thermal conductivity in the thickness direction measured by contacting a heat source plate (BT-box) at 30±2°C with a fabric at 20±2°C at 20±2°C and 65±2% RH of 0.05 to 0.25 W / mK. The functional fabric according to claim 8.

Citation Information

Patent Citations

  • Comfortable fabric

    JP2015071840A

  • Colored polyethylene fiber and product using the same

    JP2019099954A

  • Spectrally selective fabrics for passive radiative outdoor personal cooling.

    JP2021512228A

  • Improved Anti-squeal shim

    KR102776822B1

  • Cut resistant polyethylene yarn, method for manufacturing same, and protective article produced using same

    WO2020190070A1