Negative electrode and secondary battery including the same
The use of primary artificial graphite particles with an amorphous carbon coating and secondary uncoated particles in the negative electrode structure addresses the limitations of conventional graphite-based electrodes, enhancing energy density and rapid charging performance.
Patent Information
- Application Number
- JP2024527824
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-08
- Filing Date
- 2022-12-07
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-12-07
AI Technical Summary
Conventional negative electrode active materials in secondary batteries face issues with low energy density, irreversible reactions, and poor rapid charging performance due to the use of natural or artificial graphite, which limits the battery's capacity and charging efficiency.
A negative electrode design incorporating primary artificial graphite particles with an amorphous carbon coating and secondary uncoated artificial graphite particles, where the average particle size ratio is optimized to improve packing and reduce resistance, enhancing energy density and rapid charging performance.
The optimized particle structure improves energy density and rapid charging performance by allowing better packing and reducing resistance, resulting in superior output characteristics for secondary batteries.
Smart Images

Figure 2024543463000001 
Figure 2024543463000002 
Figure 2024543463000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0174644 filed on December 8, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a negative electrode and a secondary battery including the same. [Background technology]
[0003] With the rapid increase in the use of fossil fuels, there is an increasing need for the use of alternative and clean energy, and as part of this, the field in which research is being most actively conducted is the field of power generation and storage using electrochemical reactions.
[0004] Currently, a representative example of an electrochemical element that uses electrochemical energy is a secondary battery, and the range of its use is gradually expanding. Recently, with the development of technology and increasing demand for portable devices such as mobile computers, mobile phones, and cameras, the demand for secondary batteries as energy sources is rapidly increasing. In addition, in order to improve the convenience of using secondary batteries, there is a demand for shortening the charging time, and therefore, there is a demand for excellent rapid charging performance.
[0005] In general, a secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode contains a negative electrode active material that inserts and extracts lithium ions released from the positive electrode.
[0006] As the negative electrode active material, graphite-based active materials such as natural graphite or artificial graphite are generally used. However, conventionally used natural graphite is advantageous in that it is inexpensive and has high cost performance, but has a problem that it causes a large irreversible reaction due to electrolyte penetration and decomposition reaction when applied to a battery due to its irregular structure, and conventionally used artificial graphite is advantageous in that it has excellent initial charge / discharge efficiency, but has a problem that it exhibits a lower discharge capacity than natural graphite, resulting in a decrease in battery capacity and energy density.
[0007] In order to solve this problem, conventionally, negative electrode active materials have been used that are a mixture of normal natural graphite and artificial graphite, or negative electrode active materials in which an amorphous carbon coating layer is formed on normal natural graphite or artificial graphite, etc. However, in such cases, the electrode is not sufficiently rolled, so that the thickness of the electrode and the cell cannot be reduced, resulting in a problem of reduced energy density.
[0008] JP 2019-179687 A discloses an artificial graphite-based negative electrode material and a negative electrode for a non-aqueous secondary battery containing the same, but fails to provide an alternative to the above-mentioned problems. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2019-179687 A Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a negative electrode having high energy density and excellent rapid charging performance and output performance.
[0011] Another object of the present invention is to provide a secondary battery including the above-mentioned negative electrode. [Means for solving the problem]
[0012] The present invention relates to a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including a first negative electrode active material and a second negative electrode active material, the first negative electrode active material being coated artificial graphite particles including primary artificial graphite particles and an amorphous carbon coating layer disposed on the primary artificial graphite particles, the second negative electrode active material being uncoated artificial graphite particles in a secondary particle form in which two or more primary artificial graphite particles are granulated, and the average particle diameter (D 50 ) to the average particle size (D 50 ) is 1.2 to 4.7.
[0013] The present invention also provides a secondary battery including the above-mentioned negative electrode, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. Effect of the Invention
[0014] The negative electrode of the present invention includes a first negative electrode active material, which is a coated artificial graphite particle including a primary artificial graphite particle and an amorphous carbon coating layer, and a second negative electrode active material, which is a non-coated artificial graphite particle in the form of a secondary particle formed by granulating the primary artificial graphite particle, and the average particle diameter (D 50 In the anode of the present invention, the first anode active material can be arranged and packed in the empty space between the second anode active material, the relatively soft second anode active material can improve the rollability and the energy density of the anode can be improved, and the first anode active material in the form of primary artificial graphite particles with an amorphous carbon coating layer formed thereon can be arranged between the second anode active material, which can contribute to reducing the resistance of the anode and improving the fast charging performance, thereby realizing an anode and a secondary battery having high energy density and excellent output characteristics and fast charging performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] In the following, the present invention will be described in more detail in order to facilitate understanding of the present invention.
[0016] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his / her invention.
[0017] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless it has a clearly different meaning in the context.
[0018] It should be understood that in this specification, terms such as "comprises," "comprises," or "having" specify the presence of embodied features, numbers, steps, components, or combinations thereof, but do not preclude the presence or additional possibility of one or more different features, numbers, steps, components, or combinations thereof.
[0019] In this specification, D 50 can be defined as the particle size that corresponds to 50% of the cumulative volume in the particle size distribution curve (graph curve of particle size distribution degree). 50 can be measured by using, for example, a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to several mm, and can provide results with high reproducibility and high resolution.
[0020] <Negative electrode> The present invention relates to a negative electrode, specifically to a negative electrode for a lithium secondary battery.
[0021] The negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, the negative electrode active material layer including a negative electrode active material, the negative electrode active material including a first negative electrode active material and a second negative electrode active material, the first negative electrode active material being coated artificial graphite particles including primary artificial graphite particles and an amorphous carbon coating layer disposed on the primary artificial graphite particles, the second negative electrode active material being uncoated artificial graphite particles in a secondary particle form in which two or more primary artificial graphite particles are granulated, and the average particle diameter (D 50 ) to the average particle size (D 50 ) is characterized in that the ratio is 1.2 to 4.7.
[0022] The negative electrode of the present invention includes a first negative electrode active material, which is a coated artificial graphite particle including a primary artificial graphite particle and an amorphous carbon coating layer, and a second negative electrode active material, which is a non-coated artificial graphite particle in the form of a secondary particle formed by granulating the primary artificial graphite particle, and the average particle diameter (D 50 In the anode of the present invention, the first anode active material can be arranged and packed in the empty space between the second anode active material, the relatively soft second anode active material can improve the rollability and the energy density of the anode can be improved, and the first anode active material in the form of primary artificial graphite particles with an amorphous carbon coating layer formed thereon can be arranged between the second anode active material, which can contribute to reducing the resistance of the anode and improving the fast charging performance, thereby realizing an anode and a secondary battery having high energy density and excellent output characteristics and fast charging performance.
[0023] The negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector.
[0024] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, the negative electrode current collector may be made of copper, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. Specifically, a transition metal that easily adsorbs carbon, such as copper or nickel, may be used as the negative electrode current collector. The thickness of the negative electrode current collector may be 6 μm to 20 μm, but the thickness of the current collector is not limited thereto.
[0025] The negative electrode active material layer may be disposed on at least one surface of the negative electrode current collector. Specifically, the negative electrode active material layer may be disposed on one or both surfaces of the negative electrode current collector.
[0026] The negative electrode active material layer includes a negative electrode active material. The negative electrode active material includes a first negative electrode active material and a second negative electrode active material. Here, the average particle size (D 50 ) to the average particle size (D 50 ) ratio is 1.2 to 4.7.
[0027] According to the present invention, the first negative electrode active material is a coated artificial graphite particle in which an amorphous carbon coating layer is formed on a primary artificial graphite particle, and the second negative electrode active material is a non-coated artificial graphite particle in the form of a secondary particle. The first negative electrode active material and the second negative electrode active material have an appropriate average particle size (D 50 The second negative active material is contained in the negative active material layer at a ratio of 0.01 to 0.01 mm. Since the second negative active material has a secondary particle form, it can exhibit excellent fast charging performance and excellent rolling performance. In addition, the first negative active material has an average particle size (D 50), when the first negative electrode active material is disposed between the second negative electrode active material, the packing of the negative electrode active material layer can be improved. In addition, the first negative electrode active material includes an amorphous carbon coating layer disposed on a surface thereof, and ... negative electrode according to the present invention can improve energy density, rapid charging performance, and output performance due to excellent rolling properties.
[0028] For example, the average particle size (D 50 ) to the average particle size (D 50 When the ratio of the average particle diameter (D) of the first negative electrode active material is less than 1.2, the first negative electrode active material layer cannot be packed between the second negative electrode active material layers at a desired level, which may result in a decrease in energy density, and the small particle diameter of the first negative electrode active material may clog the voids, which may result in a decrease in fast charging performance and output performance. 50 ) to the average particle size (D 50 If the ratio exceeds 4.7, rapid charging performance and output performance may be reduced due to differentiation caused by particle cracking during rolling.
[0029] Specifically, the average particle size (D 50 ) to the average particle size (D 50 ) may be 2.0 to 3.5, in which case the above-mentioned energy density, rapid charging performance, and output performance can be further improved.
[0030] The first negative electrode active material is a coated-artificial graphite particle including primary artificial graphite particles and an amorphous carbon coating layer disposed on the primary artificial graphite particles.
[0031] The primary artificial graphite particles may refer to artificial graphite particles in the form of a single particle, and are used as a term to distinguish them from "secondary artificial graphite particles", which are aggregates of two or more primary artificial graphite particles aggregated by an intentional granulation or bonding process.
[0032] The first negative electrode active material (coated artificial graphite particles) according to the present invention includes an amorphous carbon coating layer that is harder than graphite, and therefore when the first negative electrode active material is disposed between the second negative electrode active material, the shape of the first negative electrode active material can be maintained even by rolling, which can contribute to improving the overall charge mobility of the negative electrode, reducing resistance, and improving fast charging performance. In addition, the first negative electrode active material has a smaller average particle size (D) than the second negative electrode active material. 50 ), the packing of the negative electrode active material layer is improved, and the energy density of the negative electrode can be improved. If the first negative electrode active material does not contain an amorphous carbon coating layer, the electrical conductivity is reduced, which may affect the void structure after rolling, resulting in reduced fast charging performance and output performance.
[0033] The amorphous carbon coating layer may be included in the first negative electrode active material in an amount of 1 wt % to 10 wt %, specifically, 3 wt % to 5 wt %.
[0034] The amorphous carbon coating layer may be formed by providing a carbon precursor to the primary artificial graphite particles and then heat-treating the carbon precursor. The carbon precursor may be, but is not limited to, polymer resins such as sucrose, phenol resin, naphthalene resin, polyvinyl alcohol resin, furfuryl alcohol resin, polyacrylonitrile resin, polyamide resin, furan resin, cellulose resin, styrene resin, polyimide resin, epoxy resin, vinyl chloride resin, polyvinyl chloride, etc.; pitches such as coal-based pitch, petroleum-based pitch, mesophase pitch, etc. The heat treatment temperature may be 1,000°C to 1,800°C.
[0035] The average particle size (D 50 ) may be 4 μm to 13 μm, specifically 7 μm to 10 μm. When it is in this range, the specific surface area of the first negative electrode active material can be reduced to a preferable level, which not only contributes to improving the capacity of the negative electrode but also allows empty spaces formed between the second negative electrode active material described later to be densely filled, thereby enabling improvement in rolling performance.
[0036] The first negative electrode active material has a BET specific surface area of 0.1 m 2 / g~3.0m 2 / g, specifically 0.5m 2 / g~2.0m 2 / g, and when it is in this range, it is preferable in that side reactions of the electrolyte are minimized and high-temperature output performance is improved. The BET specific surface area can be measured using a BEL Sorption instrument (manufactured by BEL Japan).
[0037] The second negative electrode active material is uncoated artificial graphite particles in a secondary particle form obtained by granulating two or more primary artificial graphite particles. As the second negative electrode active material is an artificial graphite particle in a secondary particle form, the second negative electrode active material may have excellent fast charging performance as well as excellent rolling performance due to voids formed between the primary artificial graphite particles present therein.
[0038] The uncoated artificial graphite particles may refer to uncoated artificial graphite particles in which the artificial graphite is entirely exposed on the surface. More specifically, the uncoated artificial graphite particles may be uncoated artificial graphite particles or may not include a separate coating layer (such as an amorphous carbon coating layer). For example, when secondary artificial graphite particles having an amorphous carbon coating layer are used as the second negative electrode active material, the negative electrode active material layer is not well pressed even by rolling, energy density is not ensured, and cracks are generated in the particles, which increases the specific surface area, aggravates side reactions of the electrolyte, and clogs the voids, resulting in problems of reduced fast charging performance and output performance.
[0039] The uncoated artificial graphite particles can be produced by mixing coke and binder pitch, subjecting the mixture to high-temperature heat treatment to produce primary artificial graphite particles, mixing the primary artificial graphite particles with binder pitch, and then subjecting the mixture to high-temperature heat treatment, specifically, heat treatment at a temperature of 2,500°C to 3,200°C. The binder pitch is graphitized by the high-temperature heat treatment, making it possible to produce uncoated artificial graphite particles free of coating materials such as amorphous carbon. In order to ensure sufficient graphitization, the total heat treatment time (time considering all of the temperature rise, heat treatment temperature maintenance, and temperature drop) of the high-temperature heat treatment is preferably 1 week to 3 weeks, and the heat treatment temperature maintenance time is preferably 48 hours to 70 hours. The coke may be needle coke and / or isotropic coke, the coke and the binder pitch may be mixed in a weight ratio of 80:20 to 95:5, and the primary particles and the binder pitch may be mixed in a weight ratio of 80:20 to 95:5.
[0040] The uncoated artificial graphite particles have an average particle size (D 50 When the average particle size of the primary artificial graphite particles contained in the non-coated artificial graphite particles is within the above range, the capacity is adjusted to a preferred level, and the average particle size (D 50 More specifically, in the uncoated artificial graphite particles, the average particle diameter (D 50 ) can be specifically 8 μm to 9 μm. When the average particle size of the primary artificial graphite particles is within the above range, the developed capacity can be sufficiently maintained while the charging characteristics such as rapid charging can also be maintained at a high level.
[0041] The average particle size (D 50 ) may be 15 μm to 25 μm, specifically 17 μm to 22 μm. When it is in this range, a decrease in quick charging performance due to an excessive particle size is prevented, and the specific surface area of the active material is adjusted to a preferable level, which is favorable for improving high temperature performance.
[0042] The BET specific surface area of the second negative electrode active material is 0.1 m 2 / g~3.0m 2 / g, specifically 0.5m 2 / g~2.0m 2 / g, and when it is in this range, it is preferable in that side reactions of the electrolyte are minimized and high-temperature output performance is improved. The BET specific surface area can be measured using a BEL Sorption instrument (manufactured by BEL Japan).
[0043] The first negative electrode active material and the second negative electrode active material may have at least one shape selected from the group consisting of a plate shape, a needle shape, and a polygonal shape, independently of each other. In this case, the negative electrode active materials can be densely arranged in the negative electrode, improving the packing property and acting advantageously in improving the energy density of the negative electrode.
[0044] The first negative electrode active material and the second negative electrode active material may be included in the negative electrode active material layer in a weight ratio of 10:90 to 80:20, specifically, a weight ratio of 25:75 to 50:50. When the weight ratio is within the above range, it is preferable in that a void structure can be well maintained even in a high energy density electrode.
[0045] The tap density of the negative electrode active material may be 1.00 g / cc to 1.20 g / cc, specifically, 1.03 g / cc to 1.05 g / cc. When the tap density of the negative electrode active material is within the above range, the tap density is sufficiently high, and the electrode can be coated with a thin thickness.
[0046] The tap density is the mass per volume of a powder made of particles, and means the density when the voids between the particles are filled by constant tapping or vibration. Factors that affect the tap density include particle size distribution, moisture content, particle shape, and cohesiveness. The tap density can predict the fluidity and compressibility of a material. The tap density can be measured according to ASTM D4781, and can be calculated using the formula TD=W / V (TD: tap density, W: weight of sample (g), V: volume of sample after tapping).
[0047] The BET specific surface area of the negative electrode active material is 0.1 m 2 / g~3.0m 2 / g, specifically 0.5m 2 / g~2.0m 2 / g, more specifically 1.3m 2 / g~1.5m 2 / g, and when it is in this range, it is preferable in that side reactions of the electrolyte are minimized and high-temperature output performance is improved. The BET specific surface area can be measured using a BEL Sorption instrument (manufactured by BEL Japan).
[0048] The average particle size (D 50 ) can be 12 μm to 20 μm, specifically 14 μm to 18 μm.
[0049] In X-ray diffraction (XRD) analysis of the negative active material, the crystal size La(100) in the a-axis direction may be 200 nm to 300 nm, and the crystal size Lc(002) in the c-axis direction may be 50 nm to 100 nm. When the crystal size is within the above range, the crystallinity of the particles is sufficiently controlled, which is preferable in terms of capacity expression and improvement of fast charging performance.
[0050] In this specification, the La(100) means the width of a crystallite in the a-axis direction calculated based on the diffraction line of the (100) crystal plane during XRD analysis of the particle, and means the crystal size on the (100) plane in the a-axis direction, and the Lc(002) means the width of a crystallite in the c-axis direction calculated based on the diffraction line of the (002) crystal plane during XRD analysis of the particle, and means the crystal size on the (002) plane in the c-axis direction of an uncoated artificial graphite particle.
[0051] In X-ray Diffraction analysis of the negative active material, the crystal size La(100) in the a-axis direction may be 210 nm to 290 nm, more specifically 230 nm to 270 nm, and in X-ray Diffraction analysis of the coated artificial graphite particles, the crystal size Lc(002) in the c-axis direction may be 60 nm to 90 nm, more specifically 65 nm to 85 nm.
[0052] In this specification, La(100) and Lc(002) can be measured by XRD analysis. Specifically, XRD analysis can be performed using a Bruker AXS D4 Endeavor XRD (voltage: 40 kV, current: 40 mA) under the condition of Cu Ka radiation (wavelength: 1.54 Å), with a scanning speed of 87.5 seconds per 0.02° from 2-Theta 10° to 90°. Among the measurement results, the full width at half maximum (FWHM) of the (002) crystal peak shown at 2θ in the vicinity of 20° to 30° and the full width at half maximum of the (100) crystal peak shown at 2θ in the vicinity of 38° to 50° can be measured, and the Lc(002) value and La(100) value can be calculated by the Scherrer formula.
[0053] The negative electrode active material layer may contain 80% by weight to 99% by weight, preferably 88% by weight to 98% by weight, of the negative electrode active material.
[0054] The negative electrode active material layer may further contain a binder, a conductive material, and / or a thickener in addition to the above-mentioned negative electrode active material.
[0055] The binder, as a component that facilitates bonding between the active material and / or the current collector, can usually be contained in the negative electrode active material layer in an amount of 1 wt % to 30 wt %, preferably 1 wt % to 10 wt %.
[0056] The binder can include at least one selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, and fluororubber, preferably at least one selected from polyvinylidene fluoride and styrene-butadiene rubber.
[0057] As the thickener, any thickener that has been used in conventional lithium secondary batteries can be used, and an example thereof is carboxymethyl cellulose (CMC).
[0058] The conductive material can be contained in the negative electrode active material layer in an amount of 1 to 30% by weight, preferably 1 to 10% by weight, as a component for further improving the conductivity of the negative electrode active material.
[0059] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. Specific examples of commercially available conductive materials include acetylene black-based products (Chevron Chemical Company products and Denka Black (manufactured by Denka Singapore Private Limited)), Gulf Oil Company products, Ketjenblack, EC-based products (manufactured by Armak Company), Vulcan XC-72 (manufactured by Cabot Company), and Super P (manufactured by Timcal).
[0060] The thickness of the negative electrode active material layer may be, but is not limited to, 10 μm to 150 μm, specifically 50 μm to 100 μm.
[0061] The rolling density of the negative electrode may be 1.5 g / cc to 2.0 g / cc, specifically 1.6 g / cc to 1.8 g / cc. According to the present invention, the two types of artificial graphite particles have preferred average particle diameters (D 50 ) in the negative electrode in accordance with the ratio thereof, it is possible to realize a negative electrode having excellent energy density, and in particular, improved rapid charging performance even at the above rolling density.
[0062] The negative electrode active material layer may be manufactured by mixing the above-mentioned negative electrode active material and at least one selected from a binder, a conductive material, and a thickener in a solvent to prepare a negative electrode slurry, and applying the negative electrode slurry to the negative electrode current collector, rolling, and drying the negative electrode slurry.
[0063] The solvent may include water or an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the negative electrode active material and, optionally, a binder and a conductive material are included. For example, the solvent may be included so that the concentration of solids including the negative electrode active material and, optionally, at least one selected from a binder, a thickener, and a conductive material is 50% by weight to 95% by weight, preferably 70% by weight to 90% by weight.
[0064] <Secondary battery> The present invention also provides a secondary battery, more specifically a lithium secondary battery, including the above-mentioned negative electrode.
[0065] The secondary battery may include the above-mentioned negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte.
[0066] The positive electrode can face the negative electrode.
[0067] The positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector.
[0068] The positive electrode current collector can be any negative electrode current collector commonly used in the art, and is not particularly limited as long as it does not cause chemical changes in the secondary battery and has high conductivity.For example, the positive electrode current collector can include at least one selected from copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and aluminum-cadmium alloy, and preferably aluminum.
[0069] The positive electrode current collector may have fine irregularities on its surface to strengthen the binding force of the positive electrode active material, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0070] The positive electrode current collector can generally have a thickness of 3 μm to 500 μm.
[0071] The positive electrode active material layer can contain a positive electrode active material.
[0072] The positive electrode active material can be a compound capable of reversible intercalation and deintercalation of lithium. Specifically, it can include a lithium composite metal oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum and lithium. More specifically, the lithium composite metal oxide includes lithium-manganese-based oxides (e.g., LiMnO2, LiMn2O4, etc.), lithium-cobalt-based oxides (e.g., LiCoO2, etc.), lithium-nickel-based oxides (e.g., LiNiO2, etc.), lithium-nickel-manganese-based oxides (e.g., LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < Z < 2), etc.), lithium-nickel-cobalt-based oxides (e.g., LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1), etc.), lithium-manganese-cobalt-based oxides (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-z1 Co z1 O4 (where 0 < Z1 < 2), etc.), lithium-nickel-manganese-cobalt-based oxides (e.g., Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2), etc.), or lithium-nickel-cobalt-transition metal (M) oxides (e.g., Li(Ni p2 Co q2 Mn r3 M S2)O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are, as atomic fractions of independent elements, 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1), etc.), and one or more of these compounds can be included. Among them, in terms of being able to enhance the capacity characteristics and stability of the battery, the lithium composite metal oxide is LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (for example, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), or lithium nickel cobalt aluminum oxide (for example, Li(Ni 0.8 Mn 0.15 Co 0.05 )O2, etc.), and considering the remarkable improvement effect by controlling the types and content ratios of the constituent elements forming the lithium composite metal oxide, the lithium composite metal oxide can be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc., and one or more mixtures of these can be used.
[0073] The positive electrode active material can be contained in the positive electrode active material layer at 80% to 99% by weight.
[0074] The positive electrode active material layer may further contain, in addition to the positive electrode active material, at least one selected from the group consisting of a binder and a conductive material.
[0075] The binder is a component that facilitates binding between the active material and the conductive material and between the current collector, and is usually added in an amount of 1 to 30% by weight based on the total weight of the positive electrode mixture. Examples of such binders include at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber.
[0076] The binder may be included in the positive electrode active material layer in an amount of 1% by weight to 30% by weight.
[0077] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material include graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fibers and metal fibers, metal powders such as carbon fluoride, aluminum, and nickel powder, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and conductive materials such as polyphenylene derivatives. Specific examples of commercially available conductive materials include acetylene black (Chevron Chemical Company products and Denka Black (manufactured by Denka Singapore Private Limited)), Gulf Oil Company products, Ketjenblack, EC (manufactured by Armak Company), Vulcan XC-72 (manufactured by Cabot Company), and Super P (manufactured by Timcal).
[0078] The conductive material may be added in an amount of 1% by weight to 30% by weight in the positive electrode active material layer.
[0079] The separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, etc. can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single layer or multilayer structure.
[0080] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.
[0081] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0082] The organic solvent can be any organic solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, examples of the organic solvent include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether and tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2 to C20 linear, branched, or cyclic hydrocarbon group that may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes. Among them, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant capable of enhancing the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, and the electrolyte solution can exhibit excellent performance.
[0083] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as the lithium salt. The concentration of the lithium salt is preferably within the range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0084] As described above, the lithium secondary battery according to the present invention exhibits excellent discharge capacity, rapid charging characteristics and stable capacity retention, and is therefore useful in portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs), and is particularly suitable for use as a constituent battery of medium- to large-sized battery modules. Accordingly, the present invention also provides a medium- to large-sized battery module including the above-mentioned secondary battery as a unit cell.
[0085] Such a medium- to large-sized battery module can be preferably used as a power source that requires high output and large capacity, such as electric vehicles, hybrid electric vehicles, and power storage devices.
[0086] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may be embodied in various different forms and should not be construed as limited to the embodiments set forth herein.
[0087] Examples and Comparative Examples Example 1: Preparation of negative electrode 1. Preparation of the first negative electrode active material Primary artificial graphite particles in single particle form (average particle size (D 50 The primary artificial graphite particles and pitch were mixed, and then heat-treated at 1,300°C for 12 hours to produce coated artificial graphite particles in which an amorphous carbon coating layer was located on the primary artificial graphite particles.
[0088] The amorphous carbon coating layer was formed on the coated synthetic graphite particles at 4% by weight.
[0089] The average particle size of the coated artificial graphite particles (D 50 ) was 8 μm.
[0090] 2. Preparation of second negative electrode active material Multiple primary artificial graphite particles (average particle size (D 50 Uncoated artificial graphite particles (average particle size (D): 8 μm) in the form of secondary particles agglomerated 50 ):20 μm) was prepared.
[0091] Specifically, the uncoated artificial graphite particles are made by pulverizing the coke raw material to an average particle size (D 50 The coke was then pulverized into coke with an average particle diameter (D) of 8 μm, and the pulverized coke was mixed with pitch to produce an intermediate granulated in the form of secondary particles. The temperature was gradually increased to 3,000°C, maintained at 3,000°C for 60 hours, and gradually decreased to room temperature for heat treatment to graphitize and produce secondary particles. The average particle diameter (D) of the secondary particles was then measured. 50 The total heat treatment time of the intermediate was 2 weeks.
[0092] The first and second negative active materials prepared as described above were mixed in a weight ratio of 30:70 to prepare a negative active material of Example 1.
[0093] The average particle size (D 50 ) is 17 μm, and the BET specific surface area is 1.4 m 2 / g and the tap density was 1.04 g / cc.
[0094] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 242.5 nm, and the crystal size in the c-axis direction, Lc(002), was 72.5 nm.
[0095] Example 2: Preparation of negative electrode active material Average particle size (D 50 The coated artificial graphite particles were prepared in the same manner as in Example 1, except that primary artificial graphite particles having a single particle shape of 12 μm were used. The average particle size (D 50 ) was 12 μm.
[0096] A negative electrode active material of Example 2 was prepared in the same manner as in Example 1, except that the coated artificial graphite particles prepared as described above were used as the first negative electrode active material.
[0097] The average particle size (D 50 ) is 18 μm, and the BET specific surface area is 1.2 m 2 / g and the tap density was 1.07 g / cc.
[0098] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 241.5 nm, and the crystal size in the c-axis direction, Lc(002), was 71.8 nm.
[0099] Example 3: Preparation of negative electrode active material Average particle size (D 50 The coated artificial graphite particles were prepared in the same manner as in Example 1, except that primary artificial graphite particles having a single particle shape of 5 μm in diameter were used. 50 ) was 5 μm.
[0100] A negative electrode active material of Example 3 was prepared in the same manner as in Example 1, except that the coated artificial graphite particles prepared as described above were used as the first negative electrode active material.
[0101] The average particle size (D 50 ) is 15 μm, and the BET specific surface area is 1.6 m2 / g and the tap density was 1.06 g / cc.
[0102] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 240.5 nm, and the crystal size in the c-axis direction, Lc(002), was 71.5 nm.
[0103] Example 4: Preparation of negative electrode active material The same first and second negative electrode active materials as those prepared in Example 1 were prepared, and the first and second negative electrode active materials were mixed in a weight ratio of 70:30 to prepare a negative electrode active material of Example 4.
[0104] The average particle size (D 50 ) is 13 μm, and the BET specific surface area is 1.8 m 2 / g and the tap density was 1.11 g / cc.
[0105] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 242.1 nm, and the crystal size in the c-axis direction, Lc(002), was 71.4 nm.
[0106] Example 5: Preparation of negative electrode active material The same first and second negative electrode active materials as those prepared in Example 1 were prepared, and the first and second negative electrode active materials were mixed in a weight ratio of 15:85 to prepare a negative electrode active material of Example 5.
[0107] The average particle size (D 50 ) is 19 μm, and the BET specific surface area is 1.0 m 2 / g and the tap density was 1.01 g / cc.
[0108] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 243.0 nm, and the crystal size in the c-axis direction, Lc(002), was 71.9 nm.
[0109] Comparative Example 1: Production of negative electrode active material Primary artificial graphite particles in single particle form (average particle size (D 50 ):8 μm) was used as a first negative active material. No amorphous carbon coating layer was formed on the first negative active material.
[0110] A negative electrode active material of Comparative Example 1 was prepared in the same manner as in Example 1, except that the first negative electrode active material was used.
[0111] The average particle size (D 50 ) is 17 μm, and the BET specific surface area is 1.8 m 2 / g and the tap density was 0.99 g / cc.
[0112] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 241.3 nm, and the crystal size in the c-axis direction, Lc(002), was 71.3 nm.
[0113] Comparative Example 2: Production of negative electrode active material 1. Preparation of the first negative electrode active material Primary artificial graphite particles in single particle form (average particle size (D 50 ):6 μm) was used as a first negative electrode active material. No amorphous carbon coating layer was formed on the first negative electrode active material.
[0114] 2. Preparation of second negative electrode active material Average diameter of secondary particles (D 50 A second negative electrode active material was prepared in the same manner as in Example 1, except that the diameter of the nanoparticles was adjusted to 22 μm instead of 20 μm.
[0115] The first and second negative active materials prepared as described above were mixed in a weight ratio of 30:70 to prepare a negative active material of Comparative Example 2.
[0116] The average particle size (D 50 ) is 15 μm, and the BET specific surface area is 2.1 m 2 / g and the tap density was 1.01 g / cc.
[0117] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 242.5 nm, and the crystal size in the c-axis direction, Lc(002), was 71.6 nm.
[0118] Comparative Example 3: Production of negative electrode active material Only the second negative electrode active material of Example 1 was replaced with the negative electrode active material of Comparative Example 3.
[0119] The average particle size (D 50 ) is 20 μm, and the BET specific surface area is 1.2 m 2 / g and the tap density was 0.97 g / cc.
[0120] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 242.2 nm, and the crystal size in the c-axis direction, Lc(002), was 71.5 nm.
[0121] Comparative Example 4: Production of negative electrode active material The uncoated artificial graphite particles used in Example 1 were prepared. The uncoated artificial graphite particles were mixed with pitch and then heat-treated at 1,300° C. for 12 hours to form an amorphous carbon coating layer on the uncoated artificial graphite particles, which was used as the negative electrode active material of Comparative Example 4.
[0122] The amorphous carbon coating layer was formed in an amount of 3 wt % based on the total weight of the amorphous carbon coating layer and the uncoated artificial graphite particles.
[0123] The average particle size (D 50 ) is 20 μm, and the BET specific surface area is 1.1 m 2 / g and the tap density was 0.98 g / cc.
[0124] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 242.6 nm, and the crystal size in the c-axis direction, Lc(002), was 71.1 nm.
[0125] Comparative Example 5: Production of negative electrode active material Only the first negative electrode active material of Example 1 was used as the negative electrode active material of Comparative Example 5.
[0126] The average particle size (D 50 ) is 8 μm, and the BET specific surface area is 2.0 m 2 / g and the tap density was 1.07 g / cc.
[0127] Furthermore, the crystal size in the a-axis direction, La(100), measured by X-ray diffraction analysis of the negative electrode active material, was 242.7 nm, and the crystal size in the c-axis direction, Lc(002), was 71.8 nm.
[0128] Comparative Example 6: Production of negative electrode active material 1. Preparation of the first negative electrode active material Primary artificial graphite particles in single particle form (average particle size (D 50 ):8 μm) was used as a first negative active material. No amorphous carbon coating layer was formed on the first negative active material.
[0129] 2. Preparation of second negative electrode active material The uncoated artificial graphite particles used in Example 1 were prepared. The uncoated artificial graphite particles were mixed with pitch and then heat-treated at 1,300° C. for 12 hours to form an amorphous carbon coating layer on the uncoated artificial graphite particles. This was used as a second negative electrode active material of Comparative Example 6.
[0130] The amorphous carbon coating layer was formed in an amount of 3 wt % based on the total weight of the amorphous carbon coating layer and the uncoated artificial graphite particles.
[0131] The average particle size (D 50 ) was 20 μm.
[0132] The first and second negative active materials prepared as described above were mixed in a weight ratio of 30:70 to prepare a negative active material of Comparative Example 6.
[0133] The average particle size (D 50 ) is 18 μm, and the BET specific surface area is 1.1 m 2 / g and the tap density was 1.02 g / cc.
[0134] Furthermore, the crystal size in the a-axis direction, La(100), measured by X-ray diffraction analysis of the negative electrode active material, was 241.6 nm, and the crystal size in the c-axis direction, Lc(002), was 71.6 nm.
[0135] Comparative Example 7: Production of negative electrode active material A negative electrode active material of Comparative Example 7 was prepared in the same manner as in Example 1, except that the second negative electrode active material prepared in Comparative Example 6 was used instead of the second negative electrode active material of Example 1.
[0136] The average particle size (D 50 ) is 19 μm, and the BET specific surface area is 1.0 m 2 / g and the tap density was 1.06 g / cc.
[0137] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 242.3 nm, and the crystal size in the c-axis direction, Lc(002), was 71.4 nm.
[0138] Comparative Example 8: Production of negative electrode active material Average particle size (D 50 ) Coated artificial graphite particles were produced in the same manner as in Example 1, except that primary artificial graphite particles having a single particle shape of 18 μm were used.
[0139] The average particle size of the coated artificial graphite particles (D 50 ) was 18 μm.
[0140] A negative active material of Comparative Example 8 was prepared in the same manner as in Example 1, except that the coated artificial graphite particles prepared as described above were used as the first negative active material.
[0141] The average particle size (D 50 ) is 21 μm, and the BET specific surface area is 1.1 m 2 / g and the tap density was 1.01 g / cc.
[0142] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 242.6 nm, and the crystal size in the c-axis direction, Lc(002), was 71.9 nm.
[0143] Comparative Example 9: Production of negative electrode active material 1. Preparation of the first negative electrode active material Average particle size (D 50 The coated artificial graphite particles were prepared in the same manner as in Example 1, except that primary artificial graphite particles having a single particle shape of 5 μm in diameter were used. 50 ) was 5 μm.
[0144] 2. Preparation of second negative electrode active material Average diameter of secondary particles (D 50 A second negative electrode active material was prepared in the same manner as in Example 1, except that the diameter of the nanoparticles was adjusted to 27 μm instead of 20 μm.
[0145] The first and second negative active materials prepared as described above were mixed in a weight ratio of 30:70 to prepare a negative active material of Comparative Example 9.
[0146] The average particle size (D 50 ) is 24 μm, and the BET specific surface area is 1.1 m 2 / g and the tap density was 1.08 g / cc.
[0147] Furthermore, the negative electrode active material was measured by X-ray diffraction analysis, and the crystal size in the a-axis direction, La(100), was 242.8 nm, and the crystal size in the c-axis direction, Lc(002), was 71.3 nm.
[0148] [Table 1]
[0149] [Table 2]
[0150] [Table 3]
[0151] Experimental Example <Production of negative electrodes> 1. Manufacturing of negative electrode The negative electrode active material prepared in Example 1, styrene-butadiene rubber as a binder, carbon black as a conductive material, and carboxymethyl cellulose (CMC) as a thickener were added to water as a solvent in a weight ratio of 94:3:1:2 to prepare a negative electrode slurry. The negative electrode slurry was applied to a copper foil (negative electrode current collector) having a thickness of 8 μm at a thickness of 14 mg / cm. 2 The negative electrode slurry was applied at a loading amount of 15.2 cm and then dried, where the temperature of the circulating air was 130° C. The current collector to which the negative electrode slurry was applied was then roll pressed and dried in a vacuum oven at 30° C. for 1 hour. 2 The negative electrode of Example 1 (rolling density: 1.78 g / cc) including a negative electrode active material layer was produced by punching out the negative electrode into a rectangular shape.
[0152] The negative electrodes of Examples 2 to 5 and Comparative Examples 1 to 9 were produced in the same manner as the negative electrode production method of Example 1, except that the negative electrode active material of Example 1 was replaced with the negative electrode active materials of Examples 2 to 5 and Comparative Examples 1 to 9, respectively.
[0153] Experimental example 1: Evaluation of output performance <Manufacturing full-cell secondary batteries> A positive electrode active material LCO, a carbon black conductive material, and a binder PVDF powder were mixed in a weight ratio of 92:2:6 in a solvent N-methyl-2-pyrrolidone to prepare a positive electrode slurry.
[0154] The prepared positive electrode slurry was applied to a positive electrode current collector with a thickness of 15 μm (mg / cm 2 ) was applied to a unit area of 23 mg, dried in a vacuum oven at 130°C for 1 hour, and then rolled at a pressure of 15 MPa between rolls heated to 80°C to prepare a positive electrode with a final rolled density of 3.8 g / cc.
[0155] A porous polyethylene separator was placed between each of the negative and positive electrodes prepared in Examples 1 to 5 and Comparative Examples 1 to 9, and then an electrode assembly was prepared by stacking. The electrode assembly was then placed in an aluminum pouch-type battery case, and an electrolyte (ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 1:4 (volume ratio), lithium hexafluorophosphate (LiPF 61 mol), vinylene carbonate (VC) content 0.5 wt % based on the weight of the electrolyte) was injected to prepare a full-cell secondary battery.
[0156] <Evaluation of output performance> The full-cell secondary batteries of Examples 1 to 5 and Comparative Examples 1 to 9 prepared as described above were charged to 4.4 V at 0.33 C, and then discharged for 10 seconds at a 2.5 C pulse while controlling the SOC to 50%, and the resistance increase rate (%) was measured as a voltage drop / applied current. The results are shown in Table 4 below.
[0157] Experimental example 2: Evaluation of quick charging performance The full-cell secondary batteries of Examples 1 to 5 and Comparative Examples 1 to 9 produced in Experimental Example 1 were cycle-charged and discharged at 45° C. to measure the capacity retention rate after 100 cycles, and the rapid charge performance was evaluated.
[0158] Specifically, the full-cell secondary batteries of Examples 1 to 5 and Comparative Examples 1 to 9 were charged and discharged up to the 100th cycle under the conditions of charge (CC / CV mode, 1C charge, cut-off at 0.005V and 0.005C) and discharge (CC mode, 0.5C discharge, cut-off at 1.5V).
[0159] The capacity retention rate was evaluated by the following formula, and the results are shown in Table 4.
[0160] Capacity retention rate (%) = {(discharge capacity at 100th cycle) / (discharge capacity at first cycle)} x 100
[0161] [Table 4]
[0162] Referring to Table 4, it can be seen that the negative electrodes of Examples 1 to 5 according to the present invention exhibit significantly superior effects in output performance and rapid charging performance compared to the negative electrodes of Comparative Examples 1 to 9.
Claims
1. A negative electrode current collector; a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, The negative electrode active material layer contains a negative electrode active material, the negative electrode active material includes a first negative electrode active material and a second negative electrode active material, the first negative electrode active material is a coated-artificial graphite particle including a primary artificial graphite particle and an amorphous carbon coating layer disposed on the primary artificial graphite particle; The second negative electrode active material is a non-coated artificial graphite particle in the form of a secondary particle obtained by granulating two or more primary artificial graphite particles, The average particle size (D 50 ) to the average particle size (D 50 ) is 1.2 to 4.
7.
2. The average particle size (D 50 ) to the average particle size (D 50 2. The negative electrode according to claim 1, wherein the ratio of
3. The average particle size (D 50 2. The negative electrode according to claim 1, wherein the thickness of the first electrode is 4 μm to 13 μm.
4. The negative electrode of claim 1 , wherein the amorphous carbon coating layer is included in the first negative electrode active material in an amount of 1 wt % to 10 wt %.
5. 2. The negative electrode of claim 1, wherein the second negative electrode active material comprises the uncoated synthetic graphite particles.
6. The average particle size (D 50 2. The negative electrode according to claim 1, wherein the thickness of the first electrode is 15 μm to 25 μm.
7. The uncoated artificial graphite particles have an average particle size (D 50 2. The negative electrode according to claim 1, wherein the negative electrode is formed by granulating two or more primary artificial graphite particles having a particle size of 7 μm to 10 μm.
8. 2. The negative electrode of claim 1, wherein the first negative electrode active material and the second negative electrode active material are contained in the negative electrode active material layer in a weight ratio of 10:90 to 80:
20.
9. The average particle size (D 50 2. The negative electrode according to claim 1, wherein the thickness of the first electrode is 12 μm to 20 μm.
10. The BET specific surface area of the negative electrode active material is 0.1 m 2 / g to 3.0 m 2 / g.
11. 2. The negative electrode according to claim 1, wherein the negative electrode active material has a crystal size La(100) in the a-axis direction of 200 nm to 300 nm and a crystal size Lc(002) in the c-axis direction of 50 nm to 100 nm, as determined by XRD analysis.
12. 2. The negative electrode of claim 1, wherein the tap density of the negative electrode active material is 1.00 g / cc to 1.20 g / cc.
13. 2. The negative electrode according to claim 1, wherein the negative electrode has a rolling density of 1.5 g / cc to 2.0 g / cc.
14. The negative electrode according to any one of claims 1 to 13, A positive electrode facing the negative electrode; a separator interposed between the negative electrode and the positive electrode; and an electrolyte.
Citation Information
Patent Citations
Lithium ion secondary battery
JP2016048668A
Negative electrode active material for lithium secondary battery, method of preparing the same, and negative electrode for lithium secondary battery and lithium secondary battery including the same
US20210126248A1
Artificial graphite-based negative electrode material, negative electrode for nonaqueous secondary battery, and nonaqueous secondary battery
JP2019179687A