Primer for battery electrodes

A copolymer primer enhances adhesion between electroactive materials and current collectors, ensuring strong bonding without compromising electrode performance.

JP2024543660APending Publication Date: 2024-11-21SOLVAY SPECIALTY POLYMERS ITALY SPA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024534619
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-20
Filing Date
2022-12-15
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing methods fail to achieve excellent adhesion between electroactive materials and current collectors without adversely affecting the electrochemical performance of electrodes.

Method used

A copolymer is used as a primer to enhance adhesion between electroactive materials and current collectors, comprising a surface-modified metal substrate with a first layer of the copolymer, a composition containing electrode active material and binder, and a second layer adhered to the first layer.

Benefits of technology

The copolymer primer achieves excellent adhesion while maintaining the electrochemical performance of the electrodes, improving uniformity and adhesion strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543660000001
    Figure 2024543660000001
  • Figure 2024543660000002
    Figure 2024543660000002
  • Figure 2024543660000003
    Figure 2024543660000003
Patent Text Reader

Abstract

The present invention relates to primers and electrodes containing the primers that improve adhesion between electroactive materials and current collectors.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to European Patent Application No. 21306846.3, filed December 20, 2021, the entire contents of which are incorporated herein by reference for all purposes.

[0002] The present invention relates to a primer that improves adhesion between a composition containing an electroactive material and a current collector, and an electrode containing the primer. [Background technology]

[0003] Electrochemical cells (also called "batteries") typically comprise a cathode and an anode, collectively referred to as electrodes. To manufacture such electrodes, an electroactive material is deposited on a conductive support, which acts as the electrode's current collector. For an electrochemical cell to function, efficient electrical contact must be maintained between the electroactive material and the conductive support.

[0004] Such electrical contact can be provided, for example, by the use of at least one primer deposited between the electroactive material and the conductive support. Suitable primers for the manufacture of electrodes are disclosed, for example, in WO 2009 / 054987 (Sion Power Corporation).

[0005] EP 2639863 (Zeon Corporation) discloses a positive electrode for a secondary battery including a current collector made of aluminum or an aluminum alloy and a positive electrode active material layer, the positive electrode active material layer including a positive electrode active material, an aqueous binder, an organic phosphonic acid compound, and a polyvalent metal compound. Summary of the Invention

[0006] Applicant has recognized that, despite various attempts made in the art, a need remains to provide an electrode in which excellent adhesion is achieved between the electroactive material and the current collector without adversely affecting the electrochemical performance of the final electrode.

[0007] Faced with such technical challenges, the Applicant has surprisingly found that a copolymer obtained by radical polymerization of at least one phosphorus-containing unsaturated monomer with acrylic acid and / or methacrylic acid [copolymer (A)] can advantageously be used as a primer providing excellent adhesion between the electroactive material of the cathode and the current collector.

[0008] The Applicant has surprisingly found that such good adhesion can be achieved by using small amounts of said copolymer (A) so as not to adversely affect the electrochemical performance of the final electrode.

[0009] Thus, in a first embodiment, the present invention provides a method for producing a cellular membrane comprising: - a surface-modified metal substrate having at least one surface that is at least partially chemically modified; - a first layer attached to said at least one surface of said metal substrate, said first layer comprising at least one copolymer (A) as defined above; - a composition comprising at least one type of electrode active material [compound (AM)] and at least one type of binder [binder (B)] [composition (C EA a second layer attached to the first layer, the second layer including at least The present invention relates to an electrode [electrode (E)] comprising:

[0010] The electrode (E) can be either a cathode (positive electrode) or an anode (negative electrode).

[0011] Preferably, the electrode (E) is a cathode (positive electrode).

[0012] In a second embodiment, the present invention relates to a method for producing an electrode (E) as defined above, said method comprising the steps of: (1) providing a metal substrate having at least one surface; a step (1b) of surface treatment of said at least one surface of said metal substrate to provide a surface-modified metal substrate having at least one surface that is at least partially chemically modified; (2) contacting the at least one surface of the metal substrate with at least one copolymer (A) to provide a first layer; (3) contacting the first layer with an electrode-forming composition [composition (CE)] comprising at least one electrode active material [compound (AM)], at least one binder [binder (B)], and at least one solvent [solvent (S)]; The present invention relates to a method comprising the steps of:

[0013] In another embodiment, the present invention relates to an electrochemical device, preferably a secondary battery, comprising a positive electrode and a negative electrode, at least one of said positive electrode and said negative electrode being an electrode (E) as defined above.

[0014] In a further embodiment, the present invention relates to the use of said copolymer (A) as a primer in a current collector of an electrochemical device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] For purposes of this invention and in the following claims: - the term "electroactive material (AM)" is intended to mean a compound capable of incorporating or inserting into its structure and subsequently releasing therefrom alkali or alkaline earth metal ions during the charging and discharging phases of an electrochemical device. The compound (AM) is preferably capable of incorporating or inserting and releasing lithium ions; - the term "secondary battery" is intended to denote a rechargeable battery; - the terms "cathode" and "positive electrode" are used synonymously; - The terms "anode" and "negative electrode" are used synonymously.

[0016] In the present invention, the nature of the metal substrate depends on whether it provides a positive or negative final electrode.

[0017] Advantageously, when the electrode of the invention is a cathode (positive electrode), the metal substrate comprises, and preferably consists of, at least one metal selected from the group consisting of aluminum (Al), nickel (Ni), titanium (Ti) and alloys thereof, with aluminum being preferred.

[0018] Advantageously, when the electrode of the invention is an anode (negative electrode), the metal substrate comprises, and preferably consists of, silicon (Si) or at least one metal selected from the group consisting of lithium (Li), sodium (Na), zinc (Zn), magnesium (Mg), copper (Cu) and their alloys, with copper being preferred.

[0019] Preferably, the copolymer (A) is at least one phosphorus-containing unsaturated monomer of formula (a) or (b) represented as follows: [ka] (wherein n is 1 or 2), (b) H2C=CH-P(=O)-(OH)2 It is obtained by radical polymerization of acrylic acid and / or methacrylic acid.

[0020] Preferably, the copolymer (A) has a molecular weight of at least 7,500 Da, more preferably from 10 kDa to 1500 kDa, even more preferably from 10 kDa to 150 kDa, especially from 10 kDa to 100 kDa.

[0021] According to a preferred embodiment, said copolymer (A) is obtained by radical copolymerization of the phosphorus-containing unsaturated monomer of said formula (b) with acrylic acid.

[0022] According to this embodiment, the phosphorus-containing unsaturated monomer of formula (b) and acrylic acid are in a molar ratio of from 40:60 to 20:80, preferably from 35:65 to 25:75, and even more preferably 30:70.

[0023] Preferably, according to this first embodiment, the copolymer (A) has a molecular weight of between 25 kDa and 85 kDa.

[0024] According to a second preferred embodiment, said copolymer (A) is obtained by radical copolymerization of a mixture of 2-hydroxyethyl methacrylate phosphates according to said formula (a) (wherein n is 1 and 2) with acrylic acid and methacrylic acid.

[0025] More preferably, said copolymer (A) is obtained by radical copolymerization of a mixture having the following molar ratios, based on the total amount of acrylic acid, methacrylic acid and 2-hydroxyethyl methacrylate phosphate of formula (a): - acrylic acid: 65 to 90%, preferably 80 to 90%, more preferably 83 to 85%, - methacrylic acid: 5 to 30%, preferably 5 to 15%, more preferably 11 to 13%, - 2-hydroxyethyl methacrylate phosphate: 2 to 12%, preferably 2 to 10%, more preferably 2 to 6%, and even more preferably about 4%.

[0026] Preferably, according to this second embodiment, the copolymer (A) has a molecular weight of between 15 kDa and 35 kDa.

[0027] The average molecular weight (typically the weight average molecular weight) is measured by size exclusion chromatography (SEC).

[0028] Advantageously, the first layer containing the compound (A) has a thickness of less than 1 μm.

[0029] Composition (C EA ) The properties of the compound (AM) in depend on whether the composition is used for the production of a positive electrode [electrode (Ep)] or a negative electrode [electrode (En)].

[0030] When forming a positive electrode (Ep) for a lithium-ion secondary battery, the compound (AM) may include a complex metal chalcogenide of the chemical formula LiMQ2 (where M is at least one metal selected from transition metals such as Co, Ni, Fe, Mn, Cr, and V or metals such as Al, and mixtures thereof, and Q is a chalcogen such as O or S). Among these, it is preferable to use a lithium-based complex metal oxide of the chemical formula LiMO2 (where M is the same as defined above). Preferred examples thereof include LiCoO2, LiNiO2, LiNixCo1-xO2 (0 < x < 1), LiNiaCobAlcO2 (a + b + c = 1), and spinel-structured LiMn2O4.

[0031] As an alternative, when continuing to form a positive electrode (Ep) for a lithium-ion secondary battery, the compound (AM) has the chemical formula M1M2(JO4)fE1-f (where M1 is lithium and may be partially substituted by another alkali metal corresponding to less than 20% of the M1 metal, M2 is a transition metal of +2 oxidation level selected from Fe, Mn, Ni, or mixtures thereof, and may be partially substituted by one or more additional metals of +1 to +5 oxidation levels corresponding to less than 35% of the M2 metal including 0, JO4 is any oxyanion, J is any of P, S, V, Si, Nb, Mo, or combinations thereof, E is a fluoride, hydroxide, or chloride anion, and f is the mole fraction of the JO4 oxyanion usually included in the range of 0.75 to 1) and may include a lithiated or partially lithiated transition metal oxyanion-based electroactive material.

[0032] The M1M2(JO4)fE1-f electroactive material as defined above is preferably phosphate-based and may have a regular or modified olivine structure.

[0033] More preferably, the compound (AM) when forming the positive electrode (Ep) has the formula Li3-xM'yM''2-y(JO4)3, where 0≦x≦3, 0≦y≦2, M' and M'' are the same or different metals, at least one of which is a transition metal, and JO4 is preferably PO4, which may be partially substituted with another oxyanion, where J is any of S, V, Si, Nb, Mo, or combinations thereof. Even more preferably, the compound (AM) is a phosphate-based electrode active material of the formula Li(FexMn1-x)PO4, where 0≦x≦1, x is preferably 1 (i.e., lithium iron phosphate of the formula LiFePO4).

[0034] When forming a composite negative electrode (En) for a lithium ion secondary battery, the compound (AM) is preferably - graphitic carbon capable of intercalating lithium, typically present in the form of lithium-hosting powders, flakes, fibers, or spheres (e.g., mesocarbon microbeads); - lithium metal, Lithium alloy compositions, including in particular those described in U.S. Pat. No. 6,203,944 (3M INNOVATIVE PROPERTIES) and / or WO 00 / 03444 (MINNESOTA MINING AND MANUFACTURING CO.); - Generally, the chemical formula is Li4Ti5O 12 These compounds are lithium titanates having a mobile ion, i.e., Li + Lithium titanate, which is generally considered a "zero strain" insertion material, having a low level of physical expansion when receiving - Lithium-silicon alloys, commonly known as lithium silicides with high Li / Si ratios, specifically those with the formula Li 4.4 Si lithium silicide, - Chemical formula Li 4.4 Lithium-germanium alloys containing a crystalline phase of Ge; - Lithium-tin and lithium-antimony alloys may include.

[0035] In some embodiments, the carbon-based material can be, for example, graphite, such as natural or artificial graphite, graphene, carbon black, or a mixture thereof.

[0036] The carbon-based material is preferably graphite.

[0037] The silicon-based compound may be one or more selected from the group consisting of chlorosilane, alkoxysilane, aminosilane, fluoroalkylsilane, silicon, silicon chloride, silicon carbide, and silicon oxide. More specifically, the silicon-based compound may be silicon oxide or silicon carbide.

[0038] When present in compound (AM), at least one silicon-based compound is contained in compound (AM) in an amount ranging from 1 to 30% by weight, preferably from 5 to 20% by weight, based on the total weight of compound (AM).

[0039] Preferably, when the electrode (E) is an anode, said binder (B) is selected from an aqueous solution of polyacrylic acid (PAA), carboxymethyl cellulose and styrene butadiene (CMC-SBR).

[0040] Preferably, when the electrode (E) is a cathode, said binder (B) is selected from semi-crystalline polymers or elastomers, more preferably semi-crystalline polymers.

[0041] As used herein, the term "semicrystalline" refers to a fluoropolymer that has at least one crystalline melting point in addition to the glass transition temperature Tg in DSC analysis.For the purposes of the present invention, semicrystalline fluoropolymer is intended herein to mean a fluoropolymer that has a heat of fusion of advantageously at least 0.4 J / g, preferably at least 0.5 J / g, more preferably at least 1 J / g, as determined according to ASTM D3418.

[0042] For purposes of the present invention, the term "elastomer" is intended to denote true elastomers or polymer resins that serve as building blocks to obtain true elastomers.

[0043] True elastomers are defined by ASTM, Special Technical Bulletin, Standard No. 184, as materials which can be stretched to twice their inherent length at room temperature and which, when released after being held under tension for 5 minutes, simultaneously return to within 10% of their original length.

[0044] Preferably, the intrinsic viscosity of the copolymer (A), measured in dimethylformamide at 25° C., is comprised between 0.05 l / g and 0.60 l / g, more preferably between 0.15 l / g and 0.50 l / g, even more preferably between 0.20 l / g and 0.45 l / g.

[0045] The copolymers (A) of the invention usually have a melting temperature (Tm) comprised between 120°C and 200°C.

[0046] The melting temperature can be determined from a DSC curve obtained by differential scanning calorimetry (hereinafter also referred to as DSC). When the DSC curve shows multiple melting peaks (endothermic peaks), the melting temperature (Tm) is determined based on the peak with the largest peak area.

[0047] Preferably, said binder (B) is chosen from VDF-based polymers, more preferably from VDF homopolymers or copolymers of VDF and at least one (per)fluorinated monomer different from VDF and / or at least one (meth)acrylic monomer.

[0048] Non-limiting examples of suitable (per)fluorinated monomers other than VDF include, inter alia: (a) C2-C8 partially or fully fluorinated olefins, such as tetrafluoroethylene (TFE), hexafluoropropylene (HFP), pentafluoropropylene, and hexafluoroisobutylene; (b) Vinyl fluoride (VF), trifluoroethylene (TrFE), chemical formula CH2=CH-R f (In the formula, R f C2-C8 hydrogenated olefins different from VDF, such as perfluoroalkylethylenes in which C1-C6 perfluoroalkyl groups are used; (c) C2-C8 chloro- and / or bromo- and / or iodo-fluoroolefins such as chlorotrifluoroethylene (CTFE); (d) Chemical formula CF2=CFOR f (In the formula, R f is a (per)fluoroalkyl vinyl ether (PAVE) having a C1-C6 (per)fluoroalkyl group, for example, CF3, C2F5, C3F7.

[0049] Preferably, the at least one (meth)acrylic monomer is according to the following formula: [ka] During the ceremony, R1, R2, and R3 are equal to or different from each other and independently represent a hydrogen atom or a C1-C3 hydrocarbon group; R OH is a hydrogen atom or a C1-C5 hydrocarbon moiety containing at least one hydroxyl group.

[0050] More preferably, said binder (B) is selected from the group consisting of VDF homopolymers and copolymers of VDF and at least one (meth)acrylic monomer as defined above.

[0051] Suitable binders (B) are commercially available, for example, from Solvay Specialty Polymers under the trade name Solef® PVDF.

[0052] Good results have been obtained by carrying out, after step (1) and before step (2), a step (1b) of surface treatment of said at least one surface of said metal substrate.

[0053] As will be apparent to a person skilled in the art, the above step (1b) of surface treatment includes any surface treatment applied at least partially to the surface, the surface treatment being selected from the group consisting of chemical modification, chemical etching, electrochemical etching, electrodeposition, chemical oxidation treatment, coating, corona discharge.

[0054] For example, chemical etching can effectively roughen the surface of the current collector, which is favorable for improving the adhesion and interfacial conductivity between the electrode and the current collector. Chemical modification can be obtained appropriately by treating with chemicals such as acids. Coating is another effective method to modify the surface of the metal substrate to achieve better performance in terms of enhanced electronic conductivity, adhesion to the electrode, and reduced corrosion. Reduced corrosion is expected to improve the general performance of the battery by improving the electronic conductivity and thus the good contact with the electrode paste.

[0055] Good results have been obtained by carrying out step (1b) via chemical etching, more preferably by contacting said at least one surface of said metal substrate with an acid solution, preferably a nitric acid solution.

[0056] Preferably, said contacting step is carried out by immersing said at least one surface in said acid solution.

[0057] Alternatively, if circumstances require, the contacting step may be performed by applying the acid solution to at least a portion of the at least one surface of the metal substrate. As will be appreciated by those skilled in the art, the area of ​​the at least one surface of the metal substrate that is to be etched may include the entire surface or at least a portion of the surface.

[0058] Preferably, after step (1b) and before step (2), at least one step of cleaning and / or rinsing said at least one surface of said metal substrate is performed.

[0059] Preferably, if performed, the washing step is carried out using an organic solvent, more preferably acetone is used.

[0060] Preferably, if performed, the rinsing step is performed using water.

[0061] Preferably, step (2) above is carried out by techniques known in the art, such as dip coating, spray coating, or the like.

[0062] Preferably, after step (2) and before step (3) above, at least one rinsing step is performed.

[0063] Preferably, step (3) is carried out by contacting an electrode-forming composition [composition (CE)] with the first layer.

[0064] Advantageously, said composition (CE) comprises at least one electroactive substance [compound (AM)] as defined above, at least one binder (B) as defined above and at least one solvent [solvent (S)].

[0065] The solvent (S) may preferably be an organic polar solvent, examples of which include N-methyl-2-pyrrolidone (NPM), N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, hexamethylphosphamide, dioxane, tetrahydrofuran, tetramethylurea, triethyl phosphate, trimethyl phosphate, and mixtures thereof, as well as isobutylnitrile, isobutylbutyrate, dibutyl ether, methyl isobutyl ketone, dibutyl carbonate, tert-butyl acetoacetate.

[0066] Preferably, step (3) above is followed by at least one step of drying.

[0067] Preferably, the drying step is carried out at a temperature of 50° C. to 150° C. and / or for a time of 30 seconds to 30 minutes. Such conditions can be appropriately selected by those skilled in the art depending on the solvent to be evaporated. Preferably, the solvent to be evaporated is water.

[0068] Advantageously, after the drying step, the final dry electrode loading is between 5 and 40 mg / cm 2 The variation is ±2mg / cm 2 It was.

[0069] More preferably, when the electrode is a cathode, the final dry electrode load is 15 to 40 mg / cm 2 The variation is ±2mg / cm 2 It is.

[0070] More preferably, when the electrode is an anode, the final dry electrode load is 5 to 20 mg / cm 2 The variation is ±2mg / cm 2 It is.

[0071] If necessary, the drying step can be followed by a step of compaction, for example by calendaring, this additional step helping to achieve the target porosity and density of the final electrode (E) of the invention.

[0072] For example, the compressing step may be preferably carried out by hot pressing at a temperature of 25°C to 130°C.

[0073] The composition directly adhered to the first layer (composition (C EA ) corresponds to the electrode-forming composition (also referred to as composition (CE)), and it is clear that the solvent is at least partially removed during the manufacturing process of the electrode, e.g. during the drying step and / or the subsequent pressing step as disclosed herein above.

[0074] The secondary battery of the present invention is preferably an alkali metal secondary battery or an alkaline earth metal secondary battery.

[0075] The secondary battery of the present invention is more preferably a lithium ion secondary battery.

[0076] The electrochemical device according to the present invention, which is preferably a secondary battery, comprises a positive electrode, a negative electrode, and a separator inserted between the positive electrode and the negative electrode, and at least one of the positive electrode and the negative electrode is the electrode (E) of the present invention.

[0077] Electrochemical devices according to the present invention can be prepared by standard methods known to those skilled in the art.

[0078] To the extent that the disclosures of the patents, patent applications, and publications incorporated herein by reference conflict with the statements of this application to the extent that a term may be unclear, the statements of this application will control.

[0079] The present invention will now be described with reference to the following examples, the purposes of which are illustrative only and are not intended to limit the scope of the invention.

[0080] Experimental section Sample preparation A conventional current collector made of aluminum was used.

[0081] The LCO-based cathode slurry was prepared as follows: Solef® 5130 was dissolved in NMP at 6 wt%. After dissolution was complete, LCO as active material and carbon additive SC65 (both in powder form) were added to the polymer solution. The relative amounts of the components [LCO:binder:SC65], in wt%, were 97:1:2. The total solids of the slurry was set at 75%. Planetary mixing was then performed in a closed vessel for 10 minutes to homogenize the mixture. The slurry was dispersed by a disperser at 2000 rpm for 50 minutes using a toothed impeller under constant N2 flux. The resulting slurry was cast onto an Al current collector by doctor blade method to achieve a target load of 30 mg / cm2 for the final dried electrode. 2 In this case, ±2mg / cm 2 Variation in was allowed. The dyeing step was performed in a vacuum oven at 90° C. for 50 minutes, with the first 25 minutes under dynamic vacuum and the last 25 minutes under static vacuum.

[0082] Criteria (not according to the present invention) To obtain a baseline system for peel adhesion measurements, 16 aluminum current collectors were used as standards. An appropriate amount of LCO-based cathode slurry was poured onto each of the current collectors and then allowed to dry. Peel tests were performed as disclosed below. The average results are reported in Table 1.

[0083] Comparison (not according to the invention) 25 aluminum current collectors were used as comparison. Each of the Al current collectors was etched with 5 wt% HNO3 aqueous solution at 40°C for 4 minutes. An appropriate amount of LCO-based cathode slurry was poured onto each of the current collectors and then dried. A peel test was performed as disclosed below. The average results are reported in Table 1.

[0084] Current collector A and current collector B according to the present invention Aluminum current collectors 6 and 9 were prepared according to the present invention. Each of the Al current collectors was etched with a 5 wt % HNO3 aqueous solution at 40° C. for 4 minutes. Each was then dip-coated with a solution of copolymer (A) as follows: - Copolymer (A)-1: a random copolymer obtained by copolymerizing a 70:30 molar ratio mixture of acrylic acid and vinyl phosphoric acid. Copolymer (A)-1 had a weight average molecular weight (Mw) ranging from about 30 to 80 kDa, as measured by GPC using the following conditions: The SEC was equipped with a multi-angle laser light scattering (MALLS) Mini Dawn TREOS detector and an Agilent concentration detector (RI detector). The SEC-MALLS system was operated with three Varian Aquagel OH mixed H, 8 μm, 3*30 cm columns, a flow rate of 1 mL / min, and the following mobile phase: 100% water, 100 mM NaCl, 25 mM NaH2PO4, 25 mM Na2HPO4 buffer solution (pH=7). The polymer samples were diluted in the mobile phase for at least 4 hours to 0.5 wt% actives, then filtered through a Millipore filter 0.45 μm and 100 microliters were injected into the mobile phase flow. Absolute molar mass was obtained using dn / dC of poly(acrylic acid) equal to 0.1875 mL / g. The detectors used were RI (Agilent concentration detector) + MALLS (multi-angle laser light scattering) Mini Dawn TREOS. - Copolymer (A)-2: a random copolymer obtained from the copolymerization of a mixture of acrylic acid, methacrylic acid, and 2-hydroxyethyl methacrylate phosphate of formula (a) in a molar ratio of about 83:13:4. Copolymer (A)-2 had a Mw in the range of about 20 to 30 kDa as determined by SEC chromatography using the following conditions: The SEC was equipped with a multi-angle laser light scattering (MALLS) Mini Dawn TREOS detector and an Agilent concentration detector (RI detector). The SEC-MALLS system was operated with three Varian Aquagel OH mixed H, 8 μm, 3*30 cm columns, a flow rate of 1 mL / min, and the following mobile phases: 85% water, 100 mM NaCl, 25 mM NaH2PO4, 25 mM NaH2PO4-15% methanol. The polymer samples were diluted in the mobile phase for at least 4 hours to 0.5 wt% actives, then filtered through a Millipore filter 0.45 μm, and 100 microliters were injected into the mobile phase flow. Absolute molar mass was obtained using dn / dC of poly(acrylic acid) equal to 0.1875 mL / g.

[0085] Immersion was performed for 2 minutes at 45° C., followed by rinsing and drying for 5 minutes starting at room temperature and up to 100° C. An appropriate amount of standard LCO-based cathode slurry was poured onto each of the treated Al current collectors and then dried.

[0086] The copolymer (A)-1 defined above was used to obtain the current collector (A), and the copolymer (A)-2 was used to obtain the current collector (B).

[0087] Peel testing was performed as disclosed below, and the average results are reported in Table 1.

[0088] Example 1 Adhesion Test Peel tests were performed using an Instron 5943 instrument with a speed of 300 mm / min and maximum cell load of 10 N according to the following procedure.

[0089] In the 180° peel test, a constant angle of 180° was maintained while peeling the two bonded parts. The average load required to separate the two parts over the length of the specimen was recorded and expressed in N / m.

[0090] The coefficient of variation was also calculated as the ratio between the mean load and the standard deviation.

[0091] [Table 1]

[0092] The results reported in Table 1 show that current collector B according to the present invention exhibited about a 15% increase in adhesion between the aluminum substrate and the electroactive material while maintaining an acceptable coefficient of variation.

[0093] From the results reported in Table 1, the current collector A according to the present invention is * ) while improving the average load compared to the current collector shown as * ) which indicates that the use of the primer allows for greater uniformity in terms of the average loading measured on the electrode.

Claims

1. An electrode [electrode (E)], a surface-modified metal substrate having at least one surface which is at least partially chemically modified; a first layer adhered to said at least one surface of said metal substrate, said first layer comprising at least one copolymer [copolymer (A)] obtained by radical polymerization of at least one phosphorus-containing unsaturated monomer with acrylic acid and / or methacrylic acid; At least one composition [composition (C)] comprising at least one electrode active material [compound (AM)] and at least one binder [binder (B)] EA a second layer adhered to the first layer, the second layer comprising An electrode [electrode (E)] comprising:

2. The copolymer (A) is At least one phosphorus-containing unsaturated monomer of formula (a) or (b): [Formula 1] (wherein n is 1 or 2); (b) H 2 C=CH-P(=O)-(OH) 2 Electrode (E) according to claim 1, obtained by radical polymerization of a tert-butyl ether copolymer with acrylic acid and / or methacrylic acid.

3. The copolymer (A) is represented by the formula (b)H 2 C=CH-OP(=O)-(OH) 2 Electrode (E) according to claim 2, obtained by radical copolymerization of a phosphorus-containing unsaturated monomer of formula (I) with acrylic acid.

4. 4. The electrode (E) of claim 3, wherein the phosphorus-containing unsaturated monomer of formula (b) and acrylic acid are in a molar ratio of 40:60 to 20:

80.

5. The copolymer (A) is 2-hydroxyethyl methacrylate phosphate according to formula (a) according to claim 2, where n=1; 2-hydroxyethyl methacrylate phosphate according to formula (a) according to claim 2, where n=2; - Acrylic acid and methacrylic acid Electrode (E) according to claim 2, obtained by radical copolymerization of

6. The copolymer (A) is composed of acrylic acid, methacrylic acid, and 2-hydroxyethyl methacrylate phosphate of the formula (a) in the following molar ratios based on the total amount of the acrylic acid, methacrylic acid, and 2-hydroxyethyl methacrylate phosphate of the formula (a): acrylic acid: 65 to 90%, preferably 80 to 90%, more preferably 83 to 85%, methacrylic acid: from 5 to 30%, preferably from 5 to 15%, more preferably from 11 to 13%, 2-hydroxyethyl methacrylate phosphate: 2 to 12%, preferably 2 to 10%, more preferably 2 to 6%, and even more preferably about 4%. Electrode (E) according to claim 5, obtained by radical copolymerization of a mixture having

7. The electrode is a positive electrode, The metal substrate comprises at least one metal selected from the group consisting of aluminum (Al), nickel (Ni), titanium (Ti), and alloys thereof; The compound (AM) is (I) Complex metal chalcogenides of formula LiMQ2, where M is at least one metal selected from transition metals such as Co, Ni, Fe, Mn, Cr, and V, or metals such as Al, and mixtures thereof, and Q is a chalcogen such as O or S; or (II) Lithiated or partially lithiated transition metal oxyanion-based electroactive materials of formula M1M2(JO4)fE1-f, where M1 is lithium, optionally partially replaced by another alkali metal representing less than 20% of the M1 metal, M2 is a transition metal with an oxidation level of +2 selected from Fe, Mn, Ni, or mixtures thereof, optionally partially replaced by one or more further metals with an oxidation level of +1 to +5 representing less than 35% (including 0) of the M2 metal, JO4 is any oxyanion where J is any of P, S, V, Si, Nb, Mo, or combinations thereof, E is an anion of fluoride, hydroxide, or chloride, and f is the mole fraction of the JO4 oxyanion, typically comprised between 0.75 and 1. and / or Electrode (E) according to any one of claims 1 to 6, wherein the binder (B) is selected from semi-crystalline polymers or elastomers.

8. 8. The electrode (E) according to claim 7, wherein the binder (B) is selected from VDF-based polymers, preferably from the group comprising VDF homopolymers and copolymers of VDF with at least one (per)fluorinated monomer different from VDF and / or with at least one (meth)acrylic monomer.

9. An electrode (E), The electrode is a negative electrode, The metal substrate contains at least one metal selected from the group consisting of silicon (Si), lithium (Li), sodium (Na), zinc (Zn), magnesium (Mg), copper (Cu), and alloys thereof; The compound (AM) is - graphitic carbon capable of intercalating lithium; - lithium metal, - lithium alloy compositions, - lithium titanate, - lithium-silicon alloys, - lithium-germanium alloys, - Lithium-tin and lithium-antimony alloys and / or 7. The electrode (E) according to any one of claims 1 to 6, wherein the binder (B) is selected from aqueous solutions of polyacrylic acid, carboxymethylcellulose and styrene butadiene.

10. A method for producing an electrode [electrode (E)] according to any one of claims 1 to 9, said method comprising the steps of: (1) providing a metal substrate having at least one surface; a step (1b) of surface treatment of said at least one surface of said metal substrate to provide a surface-modified metal substrate having at least one surface that is at least partially chemically modified; (2) contacting said at least one surface of said metal substrate with at least one copolymer [copolymer (A)] obtained by radical polymerization of at least one phosphorus-containing unsaturated monomer with acrylic acid and / or methacrylic acid to provide a first layer; (3) contacting the first layer with an electrode-forming composition [composition (CE)] comprising at least one electrode active material [compound (AM)], at least one binder [binder (B)], and at least one solvent [solvent (S)]; A method comprising:

11. 1. A method comprising: said step (1b) of surface treatment is carried out via chemical etching, and / or - after said step (1b) and before said step (2), at least one step of cleaning and / or rinsing said at least one surface of said metal substrate is carried out; and / or - after said step (2) and before said step (3), at least one rinsing step is carried out; and / or The method according to claim 10, wherein step (3) is followed by at least one step of drying and / or pressing.

12. 11. The method according to claim 10, wherein the solvent (S) is an organic polar solvent, preferably selected from the group consisting of N-methyl-2-pyrrolidone (NPM), N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, hexamethylphosphamide, dioxane, tetrahydrofuran, tetramethylurea, triethyl phosphate, trimethyl phosphate, and mixtures thereof, as well as isobutylnitrile, isobutylbutyrate, dibutyl ether, methyl isobutyl ketone, dibutyl carbonate, tert-butyl acetoacetate.

13. An electrochemical device, which is preferably a secondary battery, comprising a positive electrode and a negative electrode, at least one of the positive electrode and the negative electrode being the electrode (E) according to any one of claims 1 to 9.

14. Use of at least one copolymer [copolymer (A)] obtainable by radical polymerization of at least one phosphorus-containing unsaturated monomer with acrylic acid and / or methacrylic acid as a primer in a current collector of an electrochemical device.

Citation Information

Patent Citations

  • Conductive primer composition for non-aqueous electrolyte electrical energy storage devices

    JP2017504672A

  • Insulating paste for lithium ion secondary battery current collector and insulator layer

    JP2021176147A

  • Electrode for electrochemical elements, and electrochemical element

    WO2015115201A1