Insulating composition for secondary battery electrodes in which different binders are blended, its manufacturing method, and secondary battery electrodes containing the insulating composition

A blended insulating composition for secondary battery electrodes, using aqueous and non-aqueous binders with inorganic particles, addresses issues of reduced adhesion and gelation, ensuring safety and uniform coating by enhancing wet adhesion and insulation.

JP2024543666AActive Publication Date: 2024-11-21LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024534753
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-07-27
Filing Date
2023-07-20
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing insulating layers for secondary battery electrodes face issues with reduced wet adhesive strength when impregnated with electrolyte and gelation due to the use of non-aqueous and water-based binders, which can compromise safety and coating processes.

Method used

An insulating composition is developed by blending an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder, along with inorganic particles, to enhance wet adhesion and prevent gelation, using a solvent substitution method and heat treatment to replace aqueous solvent with non-aqueous solvent.

Benefits of technology

The insulating composition achieves excellent wet adhesion, prevents gelation, and forms a uniform layer, improving safety and processability of secondary battery electrodes by enhancing insulation properties and adhesion to the active material layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543666000001_ABST
    Figure 2024543666000001_ABST
Patent Text Reader

Abstract

The present invention relates to an insulating composition comprising a blend of an aqueous binder dispersed in a non-aqueous solvent and a non-aqueous binder. When applied as an electrode insulating layer, the insulating composition has excellent wet adhesion and can prevent gelation with an active material slurry, and is therefore effectively applicable to a process of simultaneously coating an active material slurry and the insulating composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0093079 dated July 27, 2022, and all contents disclosed in the documents of said Korean patent application are incorporated herein by reference.

[0002] The present invention relates to an insulating composition in which different binders are blended, a method for producing the same, and an electrode for a secondary battery including the insulating composition. [Background technology]

[0003] 2. Description of the Related Art As technological development and demand for mobile devices increases, the demand for secondary batteries as an energy source is rapidly increasing. Accordingly, much research is being conducted into batteries that can meet various needs.

[0004] One of the main research topics of such secondary batteries is to improve their safety. The main cause of safety-related accidents in batteries is the abnormal high temperature caused by a short circuit between the positive and negative electrodes. That is, under normal circumstances, a separator between the positive and negative electrodes maintains electrical insulation, but under abnormal circumstances such as overcharging or overdischarging the battery, internal short circuit caused by dendritic growth of the electrode material or foreign matter, penetration of the battery by a sharp object such as a nail or screw, or excessive deformation of the battery due to external force, the existing separator shows its limitations. Various methods have been tried to reduce the possibility of short circuiting of electrodes under such external impact or high temperature conditions. For example, in order to solve the internal short circuit of a battery, a method has been proposed in which an insulating layer is formed by attaching insulating tape to the uncoated part of the electrode and a part of the active material layer or coating an insulating liquid thereon.

[0005] Conventionally, a non-aqueous binder (e.g., PVDF) was used as the insulating layer for the electrode to be coated. However, the insulating layer formed with a non-aqueous binder has a low adhesive strength (hereinafter, wet adhesive strength) when soaked in an electrolyte, and cannot prevent the migration of lithium ions to the overlay region of the electrode, resulting in a problem of capacity development.

[0006] Therefore, research has been conducted into using water-based binders such as styrene-butadiene rubber (SBR) as the insulating layer of the electrode. To form an insulating layer with a water-based binder, water is used as a solvent in the process of manufacturing the coating liquid. However, in the case of electrodes, especially positive electrodes, there is a limitation in that the active material components are very vulnerable to moisture. Therefore, using water as a solvent can cause damage to the positive electrode active material layer.

[0007] Furthermore, if the insulating composition for forming the insulating layer contains an aqueous binder, there is a limitation in that gelation occurs when the aqueous binder comes into contact with the non-aqueous binder contained in the active material slurry.

[0008] Therefore, there is a need to develop a new insulating composition that has excellent wet adhesion and does not cause gelation with the binder contained in the active material slurry. Summary of the Invention [Problem to be solved by the invention]

[0009] Therefore, an object of the present invention is to provide an insulating composition that can be used as an insulating layer for an electrode and has excellent processability, a method for producing the insulating composition, and an electrode including the insulating composition. [Means for solving the problem]

[0010] In order to solve the above-mentioned problems, an insulating composition for a secondary battery electrode according to an embodiment of the present invention is a composition in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended.

[0011] In one embodiment, the insulating composition for a secondary battery electrode includes a binder matrix in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended, and inorganic particles dispersed in the binder matrix.

[0012] In a specific embodiment, the insulating composition for a secondary battery electrode includes 5 to 50 parts by weight of an aqueous binder substituted with a non-aqueous solvent, 5 to 50 parts by weight of a non-aqueous binder, and 30 to 90 parts by weight of inorganic particles.

[0013] In a specific embodiment, the insulating composition for a secondary battery electrode according to the present invention further includes a non-aqueous organic solvent, for example, the non-aqueous organic solvent includes at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethylmethyl carbonate (EMC), dimethylcarbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol.

[0014] For example, the non-aqueous solvent is N-methyl-pyrrolidone (NMP), the aqueous binder is styrene-butadiene rubber (SBR), and the non-aqueous binder is polyvinylidene fluoride (PVDF).

[0015] In another example, the inorganic particles are one or more of boehmite (AlOOH) and alumina (Al2O3).

[0016] In one embodiment, the insulating composition has a viscosity in the range of 50 cP to 50,000 cP at 25°C.

[0017] The present invention also provides a method for producing the insulating composition for a secondary battery electrode described above. In one embodiment, the method for producing the insulating composition for a secondary battery electrode according to the present invention includes the steps of evaporating the aqueous solvent from a mixture of an aqueous binder dispersed in an aqueous solvent and a non-aqueous solvent to produce an aqueous binder substituted with a non-aqueous solvent, and mixing the aqueous binder substituted with the non-aqueous solvent with the non-aqueous binder to produce a blended binder.

[0018] In one embodiment, the step of preparing the blended binder includes mixing inorganic particles.

[0019] In another embodiment, the step of preparing the aqueous binder substituted with the non-aqueous solvent is performed by heat-treating a mixture of the aqueous binder dispersed in the aqueous solvent and the non-aqueous solvent to evaporate the aqueous solvent.

[0020] For example, the heat treatment is carried out at a temperature in the range of 80 to 150°C.

[0021] The present invention also provides a secondary battery electrode including an insulating layer formed using the insulating composition for a secondary battery electrode described above. In one embodiment, the secondary battery electrode according to the present invention includes an electrode current collector, an active material layer formed on one or both sides of the electrode current collector, and an insulating layer formed on one or both sides of the electrode current collector and located in an edge region of the active material layer. The insulating layer has a composition in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended.

[0022] In a specific embodiment, the insulating layer has a composition in which inorganic particles are dispersed in a binder matrix in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended.

[0023] For example, the insulating layer has an average thickness (D ave ) is in the range of 1 to 50 μm.

[0024] For example, the secondary battery electrode is a positive electrode. Effect of the Invention

[0025] The insulating composition according to the present invention, when applied as an electrode insulating layer, has excellent wet adhesion and can prevent gelation caused by the application of different binders between the active material slurry and the insulating composition, and can be effectively applied to a process of simultaneously coating the active material slurry and the insulating composition. [Brief description of the drawings]

[0026] [Figure 1] 1 is a photograph showing the manufacturing process of a metal specimen according to Example 1. [Diagram 2] 1 is a graph illustrating a thickness change profile for a positive electrode specimen having an insulating layer formed thereon. [Diagram 3] 1 is a graph illustrating a thickness change profile for a positive electrode specimen having an insulating layer formed thereon. [Figure 4] 1 is a graph illustrating a thickness change profile for a positive electrode specimen having an insulating layer formed thereon. [Diagram 5] 1 is a graph showing the results of evaluating capacity development for a half cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Since the present invention can be modified in various ways and can have various embodiments, a specific embodiment will be described in detail.

[0028] However, this is not intended to limit the invention to the particular embodiments, but should be understood to include all modifications, equivalents, or alternatives falling within the spirit and scope of the invention.

[0029] In the present invention, terms such as "comprise" and "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, but should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0030] In addition, in the present invention, when a layer, film, region, plate, or other portion is described as being "on" another portion, this includes not only the case where it is "directly on" the other portion, but also the case where there is another portion in between. Conversely, when a layer, film, region, plate, or other portion is described as being "under" the other portion, this includes not only the case where it is "directly under" the other portion, but also the case where there is another portion in between. In addition, in the present application, being "on" can include not only the case where it is located at the top, but also the case where it is located at the bottom.

[0031] In the present invention, the term "insulating coating layer" refers to an insulating member formed by coating and drying from at least a portion of the uncoated portion of the electrode current collector to at least a portion of the electrode active material layer.

[0032] In the present invention, the term "wet adhesion" refers to the adhesion of an insulating coating layer measured in a state where the insulating coating layer is immersed in an electrolyte. More specifically, the wet adhesion can be measured by immersing a metal specimen having an insulating coating layer formed thereon in an electrolyte, applying ultrasonic waves, and then checking whether or not the insulating coating layer is swelled or detached.

[0033] The present invention will now be described in more detail.

[0034] The present invention relates to an insulating composition, which can be used as an insulating composition for a secondary battery electrode. Specifically, the present invention provides an insulating composition that can be used to form an insulating layer located in an edge region of an electrode active material layer during a process for manufacturing a secondary battery electrode.

[0035] Conventionally, a non-aqueous binder has been used as the positive electrode insulating layer. However, the insulating layer using the non-aqueous binder has a limitation in that the wet adhesion strength decreases when the layer is impregnated with an electrolyte. Meanwhile, the use of an aqueous binder as the positive electrode insulating layer has a problem in that water is used as a solvent. The positive electrode contains a large amount of lithium component, and if it comes into contact with water, its safety is rapidly reduced and in the worst case, a fire may be caused. In addition, a problem occurs in that the slurry for the insulating layer using a non-aqueous binder and the slurry for the positive electrode active material layer cannot be coated at the same time. Specifically, gelation occurs due to the application of different binders between the slurry for the insulating layer and the slurry for the positive electrode active material layer.

[0036] The present invention can solve these problems at the same time by providing an insulating composition having a composition in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended.

[0037] Specifically, the present invention provides an aqueous binder that does not contain "water" through solvent replacement. This can eliminate factors that hinder safety when applied to a positive electrode. In addition, the use of an aqueous binder prevents a decrease in wet adhesion when impregnated with an electrolyte. In addition, the present invention does not induce gelation with the binder component contained in the slurry for the positive electrode active material layer by blending with a non-aqueous binder.

[0038] In a specific embodiment, the insulating composition according to the present invention includes a binder matrix in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended, and inorganic particles dispersed in the binder matrix. The insulating composition contains inorganic particles, which enhances the insulating properties and enables the formation of a more uniform insulating layer.

[0039] In one embodiment, the insulating composition according to the present invention may contain the aqueous binder substituted with a non-aqueous solvent and the non-aqueous binder in a ratio of 5-95:5-95 parts by weight. Specifically, the ratio of the aqueous binder substituted with a non-aqueous solvent and the non-aqueous binder may be in the range of 10-90:10-90, 30-80:20-70, 40-60:40-60, 35-55:45-65, or 45-65:35-55, based on parts by weight.

[0040] The insulating composition according to the present invention may further include inorganic particles. In this case, for example, the insulating composition includes 5 to 50 parts by weight of an aqueous binder substituted with a non-aqueous solvent, 5 to 50 parts by weight of a non-aqueous binder, and 30 to 90 parts by weight of inorganic particles. Alternatively, the insulating composition includes 20 to 55 parts by weight of an aqueous binder substituted with a non-aqueous solvent, 20 to 55 parts by weight of a non-aqueous binder, and 10 to 80 parts by weight of inorganic particles. Alternatively, the insulating composition includes 25 to 50 parts by weight of an aqueous binder substituted with a non-aqueous solvent, 25 to 50 parts by weight of a non-aqueous binder, and 20 to 50 parts by weight of inorganic particles.

[0041] In one embodiment, the water-based binder can be one or more selected from the group consisting of styrene-butadiene rubber, acrylate styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, acrylic rubber, butyl rubber, fluororubber, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene copolymer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, hydroxypropylmethylcellulose, hydroxypropylcellulose and diacetylcellulose.For example, the water-based binder can be styrene-butadiene rubber.

[0042] In the present invention, when the aqueous binder is applied, a pretreatment is performed using a solvent replacement method. For example, the aqueous binder is applied in a state where the "water" of the aqueous binder is replaced with an organic solvent. The solvent replacement method can be performed by mixing the aqueous binder dispersed in the aqueous solvent with a non-aqueous solvent, and then volatilizing and removing the aqueous solvent by heat treatment.

[0043] In the present invention, the wet adhesion of the insulating layer can be increased by applying a "solvent-substituted" water-based binder without inducing gelation between the binders.

[0044] In one embodiment, the non-aqueous binder may include one or more resins selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As one example, the non-aqueous binder may include polyvinylidene fluoride (PVDF).

[0045] In the present invention, by using a non-aqueous binder together, the adhesive strength with the active material layer, particularly with the positive electrode active material layer to which a PVDF binder is applied, can be increased and the occurrence of gelling between the binders can be suppressed.

[0046] In addition, the inorganic particles may be, for example, one or more selected from the group consisting of AlOOH, Al2O3, γ-AlOOH, Al(OH)3, Mg(OH)2, Ti(OH)4, MgO, CaO, Cr2O3, MnO2, Fe2O3, Co3O4, NiO, ZrO2, BaTiO3, SnO2, CeO2, Y2O3, SiO2, silicon carbide (SiC) and boron nitride (BN). In a specific example, the inorganic particles may be one or more selected from the group consisting of AlOOH, Al2O3, γ-AlOOH and Al(OH)3. For example, the inorganic particles may be one or more of boehmite (AlOOH) and alumina (Al2O3), or AlOOH.

[0047] The average particle size of the inorganic particles may be 0.1 μm to 100 μm, 0.5 μm to 80 μm, 1 μm to 50 μm, 2 μm to 30 μm, 3 μm to 20 μm, or 5 μm to 10 μm.

[0048] In the present invention, by providing an insulating composition containing inorganic particles, it is possible to improve the insulating properties and form a more uniform insulating layer.

[0049] In another embodiment, the insulating composition according to the present invention further includes a non-aqueous organic solvent. For example, the non-aqueous organic solvent included in the insulating composition may be one or more selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol.

[0050] In a specific example, the non-aqueous organic solvent may be one or more selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc) and dimethylsulfoxide (DMSO), and may be one or more selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF) and dimethylacetamide (DMAc).

[0051] For example, the non-aqueous organic solvent may be an amide-based organic solvent, and the same solvent as that used in preparing the positive electrode slurry may be used, and the non-aqueous organic solvent may be N-methyl-pyrrolidone (NMP).

[0052] In another aspect, the insulating composition may use the same non-aqueous organic solvent as the positive electrode active material layer slurry. When the positive electrode active material layer slurry and the insulating composition use the same solvent, the occurrence of cracks due to the difference in boiling points during drying can be suppressed.

[0053] As an example, in the insulating composition according to the present invention, the non-aqueous solvent may be N-methyl-pyrrolidone (NMP), the aqueous binder may be styrene-butadiene rubber (SBR), and the non-aqueous binder may be polyvinylidene fluoride (PVDF).

[0054] In another embodiment, the insulating composition has a viscosity in the range of 50 cP to 50,000 cP at 25° C. Specifically, the insulating composition may have a viscosity at 25° C. of 50 cP to 50,000 cP, 100 cP to 45,000 cP, 1,000 cP to 40,000 cP, 2,000 cP to 35,000 cP, 3,000 cP to 30,000 cP, 4,000 cP to 20,000 cP, or 5,000 cP to 10,000 cP. When the viscosity is in the above range, the adhesive strength with the electrode active material layer can be improved, and coating properties, processability, and the like can be improved.

[0055] The present invention also provides a method for producing the insulating composition described above. In one embodiment, the method for producing the insulating composition according to the present invention includes the steps of evaporating the aqueous solvent from a mixture of the aqueous binder dispersed in the aqueous solvent and the non-aqueous solvent to produce an aqueous binder substituted with the non-aqueous solvent, and mixing the aqueous binder substituted with the non-aqueous solvent and the non-aqueous binder to produce a blended binder.

[0056] In the present invention, the aqueous solvent, e.g., water, used for dispersing the aqueous binder is removed through the "solvent replacement" method. In addition, the aqueous binder is replaced with a non-aqueous solvent, thereby enhancing the blending effect with the non-aqueous binder.

[0057] In one embodiment, the step of preparing the blended binder may include a process of mixing inorganic particles. By mixing inorganic particles, the insulating properties can be improved and a more uniform insulating layer can be formed.

[0058] In another embodiment, in the step of preparing the aqueous binder substituted with the non-aqueous solvent, a mixture of the aqueous binder and the non-aqueous binder dispersed in the aqueous solvent is heat-treated to evaporate the aqueous solvent. This results in the aqueous solvent being substituted with the non-aqueous solvent. In addition, a process of applying ultrasonic waves may be applied together with the heat treatment.

[0059] In a specific example, the heat treatment may be performed at a temperature in the range of 80° C. to 150° C. For example, the heat treatment may be performed at a temperature in the range of 80° C. to 130° C., in the range of 90° C. to 120° C., or in the range of 100° C. to 120° C. For example, when the aqueous solvent is "water", the heat treatment temperature can be around 100° C., but it is possible to lower the heat treatment temperature by applying pressure or the like.

[0060] The present invention also provides a secondary battery electrode using the insulating composition described above. Specifically, the insulating composition can be used as an insulating layer that insulates a boundary region between an uncoated portion and a coated portion during the manufacture of the secondary battery electrode.

[0061] In one embodiment, a secondary battery electrode according to the present invention includes an electrode current collector, an active material layer formed on one or both sides of the electrode current collector, and an insulating layer formed on one or both sides of the electrode current collector and positioned in an edge region of the active material layer, the insulating layer having a composition in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended.

[0062] In one embodiment, the insulating layer has a composition in which inorganic particles are dispersed in a binder matrix in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended, where the aqueous binder substituted with a non-aqueous solvent, the non-aqueous binder, and the inorganic particles are the same as those described above.

[0063] In another embodiment, the insulating layer has an average thickness (D ave For example, the average thickness (Dave ) is in the range of 3 μm to 20 μm, in the range of 5 μm to 20 μm, or in the range of 5 μm to 15 μm.

[0064] In addition, the positive electrode of the secondary battery according to the present invention has a structure in which an insulating layer is formed so as to cover a part of the slurry for the positive electrode active material layer applied to the current collector from a part of the uncoated part of the current collector. For example, the insulating layer has a thickness of about 100% or more than the average thickness (D ave Here, the boundary region between the insulating layer and the active material layer does not include a region where the thickness of the insulating layer is 30% or less of the average thickness (D ave ) before reaching the coating region of the active material.

[0065] For example, the secondary battery electrode does not exclude the negative electrode, but specifically means the positive electrode of the secondary battery.

[0066] Specifically, the positive electrode can be manufactured by applying a slurry for a positive electrode active material layer to one or both sides of a current collector. In this case, the current collector can be a current collector for a positive electrode for a lithium secondary battery according to the present invention, and can be one having high conductivity without inducing a chemical change in the battery. For example, one or more of stainless steel, aluminum, nickel, titanium, and calcined carbon can be used, and in the case of aluminum or stainless steel, one that has been surface-treated with one or more of carbon, nickel, titanium, and silver can also be used. For example, the current collector can be aluminum.

[0067] In addition, in the slurry for the positive electrode active material, any positive electrode active material that is commonly used in a positive electrode can be used as the positive electrode active material, and lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or a lithium composite oxide that is a combination of these can be used, but is not limited thereto.

[0068] The non-aqueous binder contained in the positive electrode active material slurry may include one or more resins selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As one example, the binder may include polyvinylidene fluoride.

[0069] In this case, the conductive material may be used to improve the performance of the positive electrode, such as the electrical conductivity, and may be one or more selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber. For example, the conductive material may include acetylene black.

[0070] The positive electrode of the secondary battery according to the present invention includes a structure in which an insulating composition is applied to cover a portion of a slurry for a positive electrode active material layer applied to a current collector from a portion of an uncoated portion of the current collector. In this case, the slurry for a positive electrode active material layer may be in an undried state. Here, the term "undried" may refer to a slurry that has not been subjected to a separate drying process in a drying device or equipment.

[0071] As described above, the slurry for the insulating coating layer and the slurry for the positive electrode active material layer can be simultaneously coated onto the current collector.

[0072] In addition, the secondary battery electrode can be manufactured by drying the slurry for the positive electrode active material layer and the insulating composition applied to the current collector. In a specific example, the process of drying the slurry for the positive electrode active material layer and the insulating composition applied to the current collector can be performed at an average temperature range of 50°C to 300°C.

[0073] The process of drying the slurry for the positive active material layer and the insulating composition may be performed by a drying method commonly known in the art to completely dry the slurry for the positive active material layer and the slurry for the insulating coating layer to remove the solvent. In a specific example, the drying may be performed at a temperature at which the solvent is completely evaporated, and may be performed by changing a hot air method, a direct heating method, an induction heating method, or the like, but is not limited thereto.

[0074] At this time, the drying temperature may be in the range of 50° C. to 300° C., and may be 60° C. to 200° C. or 70° C. to 150° C. The method may further include a rolling process after the process of coating and drying the positive electrode active material slurry and the insulating composition on the current collector.

[0075] The present invention will now be described in more detail with reference to examples and experimental examples.

[0076] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.

[0077] <Example 1> 100g of styrene-butadiene rubber (hereinafter referred to as SBR, Zeon's BM451B product) binder dispersed in water as a solvent at a ratio of 60:40 (parts by weight) was added to 500g of N-methyl-2-pyrrolidone (NMP) solvent and stirred. The stirred mixture was then heated at 100°C to 120°C for 2 hours to evaporate the water contained therein, producing an SBR binder substituted with NMP. Next, the NMP-substituted SBR binder and PVDF binder were mixed and stirred in a weight ratio of 50:50 to produce an insulating composition. The viscosity of the insulating composition produced was 5,000 cP.

[0078] <Example 2> Inorganic particles, such as boehmite (AlOOH), were added and stirred to the insulating composition prepared in Example 1. The mixing ratio of the SBR binder substituted with NMP, the PVDF binder, and the inorganic particles was adjusted to a weight ratio of 20:20:60.

[0079] <Examples 3 to 5> An insulating composition was obtained in the same manner as in Example 2, except that the type and content of the binder, the content of the inorganic particles, etc., when preparing the insulating composition were changed as shown in Table 1.

[0080] <Comparative Example 1> A commercially available PVDF binder was used as the insulating composition, which was controlled to a viscosity of 5,000 cP using NMP solvent.

[0081] <Comparative Example 2> A commercially available PVDF binder and boehmite (AlOOH), which is an inorganic particle, were mixed in a ratio of 50:50 parts by weight, and the viscosity was controlled to 5,000 cP using NMP solvent to obtain an insulating composition.

[0082] <Comparative Example 3> A commercially available SBR binder and boehmite (AlOOH), which is an inorganic particle, were mixed in a ratio of 50:50 by weight, and the viscosity was controlled to 5,000 cP using a water solvent to obtain an insulating composition.

[0083] <Comparative Example 4> A separate NMP solvent replacement process was not applied to the SBR binder. It was confirmed that serious gelation occurred during the mixing process of the SBR binder and the PVDF binder, and a composition that could be coated could not be produced.

[0084] The specific compositions of Examples 1 to 5 and Comparative Examples 1 to 4 are shown in Table 1 below.

[0085] [Table 1]

[0086] <Experimental Example 1. Wet Adhesion Strength Measurement of Insulation Coating Layer> In order to evaluate the adhesive strength of the insulating coating layer according to the present invention, the following experiment was carried out.

[0087] <Metal specimen with insulating coating layer> The insulating compositions prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were coated on aluminum metal foil and dried to prepare metal specimens having an insulating layer with an average thickness of about 10 μm. The metal specimens having the insulating layer were punched into a size of 2 cm x 2 cm using a punching machine for measuring adhesive strength. FIG. 1 is a photograph of the manufacturing process of the metal specimen according to Example 1.

[0088] <Ultrasonic application> 200 g of electrolyte EC / EMC=3 / 7 (vol.%) was placed in a 250 ml beaker, and the metal specimen with the insulating layer formed thereon was impregnated with the electrolyte. The metal specimen was fixed with a jig to control its movement.

[0089] Ultrasonic waves were applied to the electrolyte in which the metal specimens were immersed using an ultrasonic disperser (BANDELIN, 4200). The ultrasonic wave application conditions were as follows:

[0090] -Frequency: 20kHz -Tip diameter: 13mm (TS-113) -Amplitude: 100% (Peak-to-peak 132μm when using 13mm tip)

[0091] The results are shown in Table 2 below.

[0092] [Table 2]

[0093] As seen in Table 2, no swelling or detachment occurred in the insulating coating layer of the metal specimen in Example 1. However, the boiling point of EMC is 107.5°C, and the temperature rise of the electrolyte due to the application of ultrasonic waves causes the solvent to evaporate, changing the measurement environment, so the measurement was stopped when the temperature reached 109°C.

[0094] In addition, no swelling or detachment occurred in the insulating coating layer of the metal specimens of Examples 2 to 4, as in Example 1. However, since the boiling point of EMC is 107.5°C and the solvent evaporates, changing the measurement environment, the measurement was stopped when the temperature reached 109°C.

[0095] In addition, swelling occurred in the metal specimens of Comparative Examples 1 and 2 within 5 minutes of applying ultrasonic waves to the electrolyte. In particular, in the metal specimen of Comparative Example 2, a detachment phenomenon was observed along with swelling.

[0096] This confirmed that the insulating layers of Examples 1 to 4 were superior to the insulating layers of Comparative Examples 1 and 2 in wet adhesion strength.

[0097] <Experimental Example 3. Evaluation of coating process of insulating composition> LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.1 96 parts by weight of O2, 2 parts by weight of PVDF as a binder, and 2 parts by weight of carbon black as a conductive material were weighed and mixed in N-methylpyrrolidone (NMP) solvent to prepare a slurry for a positive electrode active material layer. The slurry for the active material layer was applied to an aluminum foil, dried, and then rolled to prepare a positive electrode having a positive electrode active material layer (average thickness: 130 μm).

[0098] An insulating composition was coated on the edge portion of the positive electrode active material layer to a thickness of about 10 μm, and then dried in a convection oven (130° C.) to prepare a positive electrode.

[0099] The thickness of the insulating layer of the prepared positive electrode specimen was measured. The measurement results are shown in Figures 2 to 4. In Figures 2 to 4, the x-axis relatively represents the distance where the insulating layer is formed, and the x-axis value of 0.8 and above is the region where the active material layer is formed. The y-axis also represents the thickness (μm).

[0100] Figure 2 shows the change in thickness of an electrode specimen in which an insulating layer is formed on an electrode using the insulating composition (PVDF) according to Comparative Example 1. Referring to Figure 2, it can be seen that the insulating layer of the insulating composition according to Comparative Example 1 spreads during the coating and drying process, and the maximum thickness does not exceed 5 μm. Values ​​on the x-axis beyond 0.8 reflect the thickness of the active material layer.

[0101] FIG. 3 shows the change in thickness of an electrode specimen in which an insulating layer is formed on an electrode using an insulating composition (SBR+AlCOOH) according to Comparative Example 3. Referring to FIG. 3, it was shown that the insulating composition according to Comparative Example 3 has an average thickness of about 8 μm in the range of 0.3 to 0.8 (boundary region) based on the x-axis. However, at the point of 0.8 based on the x-axis, the thickness of the insulating layer suddenly decreases, and a point of about 2 μm level appears. This means that when the insulating layer is formed, the coating uniformity suddenly decreases at the boundary region with the active material layer.

[0102] FIG. 4 shows the thickness change of an electrode specimen in which an insulating layer is formed on an electrode using the insulating composition according to Example 2 (SBR+PVDF+AlCOOH substituted with NMP). Referring to FIG. 4, it is shown that the insulating composition according to Example 2 has an average thickness of about 8 μm in the range of 0.3 to 0.8 (boundary region) based on the x-axis. In addition, compared with FIG. 3, it was confirmed that the phenomenon of the insulating layer thickness suddenly decreasing at the point of 0.8 based on the x-axis does not occur. This means that the coating uniformity is excellent in the boundary region with the active material layer when the insulating layer is formed.

[0103] <Experimental Example 4. Capacity development evaluation of battery cells> The performance of the battery was evaluated after applying a positive electrode active material layer using the insulating composition according to the present invention. Specifically, in order to evaluate the performance of the positive electrode, a half cell was produced and then the capacity development was evaluated.

[0104] <Half-cell manufacturing> LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.196 parts by weight of O2, 2 parts by weight of PVDF as a binder, and 2 parts by weight of carbon black as a conductive material were weighed and mixed in N-methylpyrrolidone (NMP) solvent to prepare a slurry for a positive electrode active material layer. The slurry for the active material layer was applied to an aluminum foil, dried, and then rolled to prepare a positive electrode having a positive electrode active material layer (average thickness: 130 μm).

[0105] The surface of the positive electrode was coated with an insulating composition to a thickness of about 10 μm, and then dried in a convection oven (130°C) to prepare a positive electrode. A coin-type half cell was prepared using lithium foil as the negative electrode and an electrolyte containing 1M LiPF6 in a solvent of EC:DMC:DEC=1:2:1.

[0106] <Capacity development evaluation> Each cell was charged and discharged at 45° C. and 0.1 C to evaluate whether capacity development occurred.

[0107] The results of the capacity development evaluation are shown in Fig. 5. In Fig. 5, Example 1 is a case where the positive electrode surface is coated with the insulating composition according to Example 1 (SBR+PVDF substituted with NMP). Comparative Example 1 is a case where the positive electrode surface is coated with the insulating composition (PVDF) according to Comparative Example 1. Comparative Example 4 is a case where the positive electrode surface is not coated with the insulating composition.

[0108] The capacity achieved in Comparative Example 4 was taken as 100%, and it was shown that the cell capacity in Comparative Example 1 was at a level of about 40%.

[0109] In contrast, Example 1 showed a cell capacity of less than 1%, which means that when coated with the insulating composition of Example 1, there was almost no migration of lithium ions.

[0110] These results suggest that the insulating coating layer has excellent wet adhesion in the electrolyte, prevents the migration of lithium ions in the overlay region of the electrode, and suppresses the development of capacity during discharge.

Claims

1. An insulating composition for a secondary battery electrode, comprising a blend of an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder.

2. a binder matrix in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended; The insulating composition for a secondary battery electrode according to claim 1 , further comprising inorganic particles dispersed in the binder matrix.

3. 5 parts by weight to 50 parts by weight of an aqueous binder substituted with a non-aqueous solvent; 5 parts by weight to 50 parts by weight of a non-aqueous binder; 30 parts by weight to 90 parts by weight of inorganic particles; The insulating composition for a secondary battery electrode according to claim 2 .

4. The insulating composition for a secondary battery electrode further contains a non-aqueous organic solvent, 2. The insulating composition for a secondary battery electrode according to claim 1, wherein the non-aqueous organic solvent includes at least one selected from the group consisting of N-methyl-pyrrolidone, dimethylformamide, dimethylacetamide, dimethylsulfoxide, ethylene carbonate, diethyl carbonate, ethyl methyl carbonate, dimethyl carbonate, propylene carbonate, dipropyl carbonate, butylene carbonate, methyl propyl carbonate, ethyl propyl carbonate, acetonitrile, dimethoxyethane, tetrahydrofuran, gamma butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol.

5. The non-aqueous solvent is N-methyl-pyrrolidone, the water-based binder is a styrene-butadiene rubber; 2. The insulating composition for a secondary battery electrode according to claim 1, wherein the non-aqueous binder is polyvinylidene fluoride.

6. The inorganic particles are boehmite (AlOOH) and alumina (Al 2 O 3 3. The insulating composition for a secondary battery electrode according to claim 2, wherein the insulating composition is one or more of the following:

7. 2. The insulating composition for a secondary battery electrode according to claim 1, wherein the insulating composition has a viscosity in the range of 50 cP to 50,000 cP at 25°C.

8. preparing an aqueous binder substituted with a non-aqueous solvent by evaporating the aqueous solvent from a mixture of the aqueous binder dispersed in the aqueous solvent and the non-aqueous solvent; and mixing the aqueous binder substituted with the non-aqueous solvent with the non-aqueous binder to prepare a blended binder.

9. The step of preparing the blended binder comprises: The method for producing the insulating composition for a secondary battery electrode according to claim 8, further comprising a step of mixing inorganic particles.

10. In the step of preparing an aqueous binder substituted with a non-aqueous solvent, The method for producing an insulating composition for a secondary battery electrode according to claim 8, wherein the mixture of the aqueous binder dispersed in the aqueous solvent and the non-aqueous solvent is heat-treated to evaporate the aqueous solvent.

11. The method for producing an insulating composition for a secondary battery electrode according to claim 10, wherein the heat treatment is carried out in a range of 80 to 150°C.

12. An electrode current collector; an active material layer formed on one or both sides of an electrode current collector; an insulating layer formed on one or both sides of an electrode current collector and located in an edge region of the active material layer; The insulating layer has a composition in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended.

13. The secondary battery electrode according to claim 12 , wherein the insulating layer has a composition in which inorganic particles are dispersed in a binder matrix in which an aqueous binder substituted with a non-aqueous solvent and a non-aqueous binder are blended.

14. The insulating layer has an average thickness (D ave 13. The secondary battery electrode according to claim 12, wherein the thickness of the first electrode is in the range of 1 to 50 μm.

15. The secondary battery electrode of claim 12 , wherein the secondary battery electrode is a positive electrode.

Citation Information

Patent Citations

  • Electrochemical device and electronic device

    CN114156433A

  • Nonaqueous electrolyte secondary battery and manufacturing method of electrode

    JP2009054455A

  • Organic / inorganic composite separation membrane coated with a porous active layer and electrochemical element equipped therewith

    JP2010517811A

  • Method for manufacturing slurry for lithium ion secondary battery heat-resistant layer and method for manufacturing electrode for lithium ion secondary battery

    JP2014165096A

  • Method for manufacturing slurry for lithium ion secondary battery heat-resistant layer and method for manufacturing electrode for lithium ion secondary battery

    JP2014165097A