Method for increasing the interlacing strength of interlaced multifilaments

A novel nozzle design with opposing airflow vortices and controlled pressures enhances interlaced multifilament entanglement strength, improving weaving quality by stabilizing knots and reducing loosening.

JP2024543672AActive Publication Date: 2024-11-21JIANGSU HENGLI CHEM FIBER
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2024535227
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-30
Filing Date
2022-11-02
Publication Date
2024-11-21
Estimated Expiration
2042-11-02

AI Technical Summary

Technical Problem

Existing interlace processing technologies face challenges in maintaining the entanglement strength of interlaced multifilaments, leading to loosening during weaving due to uniform airflow directions and pressures, which affect weaving quality.

Method used

A novel nozzle design with two injection ports creating vortices in opposite directions within the yarn guide tube, combined with controlled airflow pressures, to enhance entanglement stability and strength.

Benefits of technology

The method results in interlaced yarns with high entanglement strength, reducing loosening during weaving and eliminating the need for additional processes like twisting or sizing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543672000001_ABST
    Figure 2024543672000001_ABST
Patent Text Reader

Abstract

The objective of the present invention is to provide a method for increasing the interlace strength of interlace multifilaments. The method for increasing the interlace strength of interlace multifilaments is as follows: by DTY technology, multifilaments are sequentially subjected to initial tension by a tension adjuster, sandwiched by a feed roller and introduced into a yarn guide tube, sandwiched by a guide roller and drawn out, and taken up by a take-up roller to become an interlace yarn; in which, a line passing through the pinching point of the feed roller and the pinching point of the guide roller overlaps with the central axis of the yarn guide tube, and the speed of the feed roller and the guide roller is the same; when the multifilaments pass through the yarn guide tube of the nozzle, compressed air is intermittently injected into the yarn guide tube A and the yarn guide tube B by the nozzle I and the nozzle II, respectively, and the input air pressure of the nozzle I is greater than the input air pressure of the nozzle II. The interlace yarn of the present invention has a high interlace strength and is not easily loosened, so that the weaving process is simplified so that twisting and sizing processes are not required.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of spinning technology, and in particular to a method for increasing the entanglement strength of interlaced multifilaments. [Background technology]

[0002] Interlacing is a widely applied and mature technology in chemical fiber manufacturing, with high practicality and potential. Interlacing is a method to efficiently increase the bundling of filaments without the need for twisting or sizing processes, and can simplify the weaving process of filaments. In the current interlacing technology, a high-pressure airflow is blown onto the filaments introduced into the interlacer through a nozzle, and the high-pressure airflow forms a vortex inside the yarn guide tube, entangling the single filament yarns and forming a knot. The factors that affect the interlacing strength of filaments are usually the pressure of compressed air and the processing speed. Although the interlacing strength can be improved by optimizing the pressure of compressed air and the processing speed, the interlacing strength obtained in this way is still likely to loosen when it comes into contact with the friction between the heddle and reed of the loom, resulting in a deterioration in weaving quality. Summary of the Invention [Problem to be solved by the invention]

[0003] In response to the shortcomings of the prior art, the present invention provides a method for increasing the interlacing strength of interlaced multifilaments, namely, using a novel nozzle. In the novel nozzle, airflows injected from two nozzles form vortices in different directions in the yarn duct, and the filament single yarns are intertwined in different directions. As a result, the knots of the yarn are stable, the interlacing strength is increased, and the interlacing loosening is reduced, improving the weaving quality of the yarn. [Means for solving the problem]

[0004] In order to achieve the above object, the present invention proposes the following. 1. A method for increasing the entanglement strength of an interlaced multifilament yarn using a DTY spinning process, comprising: The non-interlaced multifilament, the pretension of which is adjusted by a tensor, is gripped by a feed roller and a feed roll and passed through a yarn path of a nozzle, and is gripped by a pull-out roller and a pull-out roll and pulled out, and the interlaced multifilament is wound up by a winding roller to form a yarn. The nozzle is formed by processing a cubic structure (made of a metal material), and in the cubic structure, faces a and a', faces b and b', and faces c and c' are parallel to each other, respectively; The processing involves forming grooves w, v, and u on face c, which penetrate face b and face b'. a through hole is formed which communicates the surface a with the surface a', passes through the grooves w, v, and u, and serves as a yarn path for the nozzle; The yarn path between the grooves w and v is designated as yarn path A. The yarn path between the grooves v and u is designated as yarn path B. a hole x is formed on a surface b, the hole x being in communication with the yarn path A and having a connecting surface with the yarn path A that completely fits into a side wall of the yarn path A; a hole y is formed on the surface b', the hole y being in communication with the yarn path B and having a connection surface with the yarn path B that completely fits into a side wall of the yarn path B; a central axis of the hole x and a central axis of the hole y are both perpendicular to a central axis of the yarn path on different planes, the central axes of the hole x and the hole y are parallel to each other as projection lines onto a transverse cross section of the yarn path and are symmetrical with respect to a center point of the transverse cross section, the hole x is an nozzle I of the yarn path A, and the hole y is an nozzle II of the yarn path B, a line connecting a gripping point between the feed roller and the feed roll and a gripping point between the pull-out roller and the pull-out roll overlaps with a central axis of the yarn path; the feed roller and the pull-out roller have the same linear speed; When the multifilament passes through the yarn path of the nozzle, compressed airflows are intermittently blown out from nozzle I and nozzle II to yarn path A and yarn path B, respectively (i.e., in yarn path A, the multifilament is subjected to the interlacing action of the airflow blown out from nozzle I, and then in yarn path B, the multifilament is subjected to the interlacing action of the airflow blown out from nozzle II). The time at which the airflow is blown out from nozzle I to yarn path A is t1, and after Δt has elapsed, the airflow is blown out from nozzle II to yarn path B, and the blowing time is t2, t1 and t2 are the same, Δt=d / v, d is the horizontal distance between the central axis of nozzle I and the central axis of nozzle II, v is the linear velocity of the pull-out roller, A method is provided in which the pressure of the airflow ejected from nozzle I to yarn path A is greater than the pressure of the airflow ejected from nozzle II to yarn path B.

[0005] The principle is that when interlaced yarn is subjected to the impact force of the nozzle airflow, the original parallel monofilaments are separated into multiple bulky open sections, and the sections between them are entangled with each other by the vortex current to form knots, i.e. entangled sections. There are usually two indices to evaluate interlaced yarn. The first is the entanglement number N, which indicates the number of entangled sections per unit length (m), and the second is the entanglement strength S, defined as Nr / N, where Nr is the residual entanglement number after applying a load of 132mN / tex to a unit length of yarn for 3 minutes. The evaluation method is performed according to the Chinese industrial standard FZ / T 50001-2005 "Method for measuring the entanglement number of synthetic fibers."

[0006] The principle of the present invention is as follows.

[0007] The biggest factor in creating interlaced yarn is the entanglement of the multifilament single yarns caused by the air flow in the yarn duct, so the direction of yarn movement is along the swirling direction of the air. In the case of interlaced yarns in the prior art, the entanglement direction of the single yarns is almost the same, so the entanglement strength of the yarns is low and there is slack in the entanglement during weaving.

[0008] In the present invention, first, the line passing through the pinch point of the feed roller and the pinch point of the guide roller overlaps with the central axis of the yarn guide tube, and the linear speed of the feed roller and the guide roller are the same to prevent overcharging between the feed roller and the guide roller and ensure that the multifilament is located on the central axis of the yarn guide tube. Secondly, two nozzles are provided on both sides of the nozzle, and both nozzles are located at the twisting position of the central axis of the yarn guide tube, so that the air swirl mainly blows the outer single yarn of the multifilament to make the single yarn wind around the fiber axis. More specifically, the nozzle I is located above the central axis of the yarn guide tube A and the nozzle II is located below the central axis of the yarn guide tube B, so that the swirl in the yarn guide tube A is opposite to the swirl in the yarn guide tube B, and they do not affect each other due to the division of the groove v. Therefore, the entangled portion formed in yarn guide tube A and the entangled portion formed in yarn guide tube B have opposite entanglement directions, and when the single yarn hits the opposing whorls, a stronger knot can be formed and the entanglement strength is high. Furthermore, the present invention controls the incident airflow pressure of nozzle I to be higher, so that when the entangled portion formed in yarn guide tube A hits the weaker opposing whorls of yarn guide tube B, the entanglement becomes stronger without changing the entanglement direction much. In other words, the interlaced yarn in the present invention has high entanglement strength and is less likely to come loose during weaving.

[0009] Preferably, in the method for increasing the interlace strength of the interlaced yarn, the diameter of the yarn guide tube is 2.5 to 3 mm, the nozzle I and the nozzle II have the same structure and a diameter of 0.5 to 1 mm, the distance between the projection line of the central axis of the hole x on the cross section of the yarn guide tube and the center point of the cross section is 0.5 to 0.8 mm, the pressure of the air flow entering the yarn guide tube A from the nozzle I is 0.1 to 0.3 MPa, and the pressure of the air flow entering the yarn guide tube B from the nozzle II is 0.05 to 0.08 MPa, the value range of d is 18 to 20 mm, and the value range of v is 30 to 50 m / s. The initial tension is 0.01 to 0.05 N (because the feed roller and guide roller are present, the multifilament in the yarn guide tube is stretched, and single yarns with too large an initial tension are less likely to intertwine); t1 is 0.1 to 0.3 ms; the multifilament specification is 3 to 15 tex / 10 to 40 F, and the interlaced yarn is composed of multiple cycle segments along the longitudinal direction, and each cycle segment is composed of an open section and an entangled section that are connected in sequence; the entanglement strength of the interlaced yarn is 97 to 99%. Effect of the Invention

[0010] The advantages of the present invention are: 1. The interlaced yarn obtained has high interlacing strength and is not prone to loosening, simplifying the weaving process by eliminating the need for twisting and sizing processes; 2. The interlacing nozzle used is convenient to process, easy to realize, and has a wide range of applicability. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a schematic diagram showing an apparatus for increasing the interlacing strength of the interlaced yarn of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a cross-sectional structure of a nozzle of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the present invention. Even if various modifications of the present invention are permitted by a person skilled in the art who has read the contents of the present invention, they are also limited within the scope of the claims of the present invention as equivalent forms of the present invention.

[0013] Example 1 The nozzle for increasing the interlacing strength of the interlaced yarn has the following structure: As shown in FIG. 2, the nozzle is a cube of processed metal material, in which the faces a and a', b and b', and c and c' are parallel to each other; the processing is to dig grooves w, v, and u penetrating from face c to face b and b', to open through holes with a diameter of 2.3 to 3 mm from face a to face a', and the through holes pass through the grooves, w, and u to become thread guides, among which the part between groove w and v is called thread guide A6, and the part between groove v and u is called thread guide B7; and to open a hole x from face b to thread guide A. a hole y is drilled from face b' to the yarn guide tube B; the central axes of hole x and hole y are at a twisted position of the central axis of the yarn guide tube, and the projection lines of the central axes of hole x and hole y on the cross section of the yarn guide tube are parallel to each other and symmetrical about the center point of the cross section; hole x becomes nozzle I of yarn guide tube A and hole y becomes nozzle II of yarn guide tube B; nozzles I and II have the same structure and a diameter of 0.5 to 1 mm, and the distance between the projection line of the central axis of hole x on the cross section of the yarn guide tube and the center point of the cross section is 0.5 to 0.8 mm.

[0014] Example 2 The method for increasing the interlace strength of the interlaced multifilament is as follows: (1) Raw material A is polyester POY with a specification of 25tex / 40F; (2) With the DTY technology, as shown in FIG. 1, the multifilaments of the raw material A1 are sequentially subjected to initial tension by the tension adjuster 2, sandwiched between the feed roller 3 and the feed rubber roller 4, introduced into the yarn guide tube of the nozzle 5 (the structure is as shown in Example 1), sandwiched between the guide roller 8 and the guide rubber roller 9, pulled out, and wound up by the take-up roller 10 to become an interlaced yarn of standard 15tex / 40F; in which, the line passing through the pinch point of the feed roller and the pinch point of the guide roller overlaps with the central axis of the yarn guide tube, and the speed of the feed roller and the guide roller is the same; when the multifilaments pass through the yarn guide tube of the nozzle, the injection port I and nozzle II to intermittently inject compressed air into yarn guide tube A and yarn guide tube B, respectively (i.e., the multifilament is successively subjected to the entanglement of the airflow from nozzle I of yarn guide tube A and nozzle II of yarn guide tube B). Specifically, the airflow is injected into the yarn guide tube from nozzle I for time t1, and after a time Δt, the airflow injection into yarn guide tube B from nozzle II begins, and the injection time is t2; furthermore, t1 and t2 are the same, and Δt=d / v, d is the distance between the central axes of nozzle I and nozzle II, and v is the linear velocity of the guide roller; the input airflow pressure of nozzle I is greater than that of nozzle II; specifically, the process parameters and nozzle dimensions are as follows: Initial tension is 0.05N, The diameter of the thread guide tube is 3 mm. The nozzle diameter is 1 mm. t1 is 0.3ms, d is 18mm, v is 35m / s, The pressure of the airflow entering the yarn guide tube A from the nozzle I is 0.3 MPa. The pressure of the airflow entering the yarn duct B from the nozzle II is 0.05 MPa; The obtained interlaced yarn is composed of multiple cycle segments along the longitudinal direction, and each cycle segment is composed of a spread section and an entangled section that are connected in sequence; the entanglement strength of the interlaced yarn is 99%.

[0015] Example 3 The method for increasing the interlace strength of the interlaced multifilament is as follows: (1) Raw material A is polyester POY with a specification of 17tex / 30F; (2) With the DTY technology, as shown in FIG. 1, the multifilaments of the raw material A1 are sequentially subjected to initial tension by the tension adjuster 2, sandwiched between the feed roller 3 and the feed rubber roller 4, introduced into the yarn guide tube of the nozzle 5 (the structure is as shown in Example 1), sandwiched between the guide roller 8 and the guide rubber roller 9, pulled out, and wound up by the take-up roller 10 to become an interlaced yarn of standard 10tex / 40F; in which, the line passing through the pinch point of the feed roller and the pinch point of the guide roller overlaps with the central axis of the yarn guide tube, and the speed of the feed roller and the guide roller is the same; when the multifilaments pass through the yarn guide tube of the nozzle, the injection port I and nozzle II to intermittently inject compressed air into yarn guide tube A and yarn guide tube B, respectively (i.e., the multifilament is successively subjected to the entanglement of the airflow from nozzle I of yarn guide tube A and nozzle II of yarn guide tube B). Specifically, the airflow is injected into the yarn guide tube from nozzle I for time t1, and after a time Δt, the airflow injection into yarn guide tube B from nozzle II begins, and the injection time is t2; furthermore, t1 and t2 are the same, and Δt=d / v, d is the distance between the central axes of nozzle I and nozzle II, and v is the linear velocity of the guide roller; the input airflow pressure of nozzle I is greater than that of nozzle II; specifically, the process parameters and nozzle dimensions are as follows: Initial tension is 0.01N. The diameter of the thread guide tube is 2.5 mm. The nozzle diameter is 0.5 mm. t1 is 0.2ms, d is 20 mm, v is 50m / s, The pressure of the airflow entering the yarn guide tube A from the nozzle I is 0.1 MPa. The pressure of the airflow entering the yarn duct B from the nozzle II is 0.08 MPa; The obtained interlaced yarn is composed of a plurality of cycle segments along the longitudinal direction, and each cycle segment is composed of successively connected spread portions and entangled portions; the entanglement strength of the interlaced yarn is 97%.

[0016] Example 4 The method for increasing the interlace strength of the interlaced multifilament is as follows: (1) Raw material A is polyester POY with a specification of 20tex / 35F; (2) With the DTY technology, as shown in FIG. 1, the multifilaments of the raw material A1 are sequentially subjected to initial tension by the tension adjuster 2, sandwiched between the feed roller 3 and the feed rubber roller 4, introduced into the yarn guide tube of the nozzle 5 (the structure is as shown in Example 1), sandwiched between the guide roller 8 and the guide rubber roller 9, pulled out, and wound up by the take-up roller 10 to become an interlaced yarn of standard 12tex / 35F; in which, the line passing through the pinching point of the feed roller and the pinching point of the guide roller overlaps with the central axis of the yarn guide tube, and the speed of the feed roller and the guide roller is the same; when the multifilaments pass through the yarn guide tube of the nozzle, the injection port I and nozzle II to intermittently inject compressed air into yarn guide tube A and yarn guide tube B, respectively (i.e., the multifilament is successively subjected to the entanglement of the airflow from nozzle I of yarn guide tube A and nozzle II of yarn guide tube B). Specifically, the airflow is injected into the yarn guide tube from nozzle I for time t1, and after a time Δt, the airflow injection into yarn guide tube B from nozzle II begins, and the injection time is t2; furthermore, t1 and t2 are the same, and Δt=d / v, d is the distance between the central axes of nozzle I and nozzle II, and v is the linear velocity of the guide roller; the input airflow pressure of nozzle I is greater than that of nozzle II; specifically, the process parameters and nozzle dimensions are as follows: Initial tension is 0.01N. The diameter of the thread guide tube is 3 mm. The nozzle diameter is 0.5 mm. t1 is 0.1ms, d is 20 mm, v is 50m / s, The pressure of the airflow entering the yarn guide tube A from the nozzle I is 0.1 MPa. The pressure of the airflow entering the yarn duct B from the nozzle II is 0.08 MPa; The obtained interlaced yarn is composed of a plurality of cycle segments along the longitudinal direction, and each cycle segment is composed of successively connected spread portions and entangled portions; the entanglement strength of the interlaced yarn is 98%.

[0017] Example 5 The method for increasing the interlace strength of the interlaced multifilament is as follows: (1) Raw material A is polyester POY with a standard of 14tex / 20F; (2) With the DTY technology, as shown in FIG. 1, the multifilaments of the raw material A1 are sequentially subjected to initial tension by the tension adjuster 2, sandwiched between the feed roller 3 and the feed rubber roller 4, introduced into the yarn guide tube of the nozzle 5 (the structure is as shown in Example 1), sandwiched between the guide roller 8 and the guide rubber roller 9, pulled out, and wound up by the take-up roller 10 to become an interlaced yarn of standard 8tex / 20F; in which, the line passing through the pinch point of the feed roller and the pinch point of the guide roller overlaps with the central axis of the yarn guide tube, and the speed of the feed roller and the guide roller is the same; when the multifilaments pass through the yarn guide tube of the nozzle, the injection port I and nozzle II to intermittently inject compressed air into yarn guide tube A and yarn guide tube B, respectively (i.e., the multifilament is successively subjected to the entanglement of the airflow from nozzle I of yarn guide tube A and nozzle II of yarn guide tube B). Specifically, the airflow is injected into the yarn guide tube from nozzle I for time t1, and after a time Δt, the airflow injection into yarn guide tube B from nozzle II begins, and the injection time is t2; furthermore, t1 and t2 are the same, and Δt=d / v, d is the distance between the central axes of nozzle I and nozzle II, and v is the linear velocity of the guide roller; the input airflow pressure of nozzle I is greater than that of nozzle II; specifically, the process parameters and nozzle dimensions are as follows: Initial tension is 0.05N, The diameter of the thread guide tube is 2.5 mm. The nozzle diameter is 1 mm. t1 is 0.3ms, d is 18mm, v is 30m / s, The pressure of the airflow entering the yarn guide tube A from the nozzle I is 0.3 MPa. The pressure of the airflow entering the yarn duct B from the nozzle II is 0.05 MPa; The obtained interlaced yarn is composed of a plurality of cycle segments along the longitudinal direction, and each cycle segment is composed of successively connected spread portions and entangled portions; the entanglement strength of the interlaced yarn is 99%.

[0018] Comparative Example 1 The interlacing method is almost the same as in Example 2, with the only difference being that compressed air is not injected through the nozzle II. The interlaced yarn obtained has an entanglement strength of 87%. Comparing Comparative Example 1 with Example 2, it can be seen that the entanglement strength of Comparative Example 1 is lower. The reason is that compressed air is not injected from nozzle II, and the multifilament is only subjected to the action of compressed air injected from nozzle I, and the entanglement strength is at the same level as that in the prior art.

[0019] Comparative Example 2 The interlacing method was almost the same as in Example 2, with the only difference being that the pressure of the compressed air injected from nozzle I was 0.3 MPa, the same as the pressure of the compressed air injected from nozzle II. The interlaced yarn obtained has an entanglement strength of 82%. Comparing Comparative Example 2 with Example 2, it can be seen that the entanglement strength of Comparative Example 2 is reduced. The reason is that when the pressure of the compressed air entering from nozzle I is made the same as the pressure of the compressed air entering from nozzle II, the two airflows are in opposite directions but have the same pressure, so that the airflow from nozzle II has a relatively strong untwisting effect on the entanglements formed by nozzle I, reducing the entanglement strength of the yarn.

[0020] Comparative Example 3 The interlacing method is almost the same as in Example 2, with the only difference being that the nozzle used is different from that shown in Example 1, that is, the distance between the projection line of the central axes of holes x and y on the cross section of the yarn guide tube and the center point of the cross section is set to 0. The interlaced yarn obtained has an entanglement strength of 83%. Comparing Comparative Example 3 with Example 2, it can be seen that the entanglement strength of Comparative Example 3 is lower. The reason for this is that when the airflow directions of nozzles I and II are both directly facing the central axis of the yarn guide tube, the airflow reaches the central axis of the yarn directly and then diffuses to both sides, resulting in a weaker and more unstable vortex, which reduces the entanglement of the yarn and reduces the entanglement strength.

[0021] Comparative Example 4 The interlacing processing method is almost the same as in Example 2, with the only difference being that the nozzle used is different from the nozzle shown in Example 1; that is, the projection lines of the central axis of hole x and the central axis of hole y on the cross section of the yarn guide tube are parallel to each other and are not symmetrical about the center point of the cross section, and the distance between the projection line of the central axis of hole x on the cross section of the yarn guide tube and the center point of the cross section is 0, and the distance between the projection line of the central axis of hole y on the cross section of the yarn guide tube and the center point of the cross section is the distance in Example 1. The interlaced yarn obtained had an entanglement strength of 88%. Comparing Comparative Example 4 with Example 2, it can be seen that the entanglement strength of Comparative Example 4 is lower. The reason for this is that when the airflow from nozzle I faces the central axis of the yarn and the airflow from nozzle II faces the side of the yarn, the action of the airflow from nozzle I, which has a higher pressure, reaches the central axis of the yarn, causing a weaker swirl, resulting in a lower entanglement strength.

[0022] Comparative Example 5 The interlacing processing method is almost the same as in Example 2, with the only difference being that the nozzle used is different from the nozzle shown in Example 1; that is, the projection lines of the central axis of hole x and the central axis of hole y on the cross section of the yarn guide tube are parallel to each other and are not symmetrical about the center point of the cross section, and the distance between the projection line of the central axis of hole x on the cross section of the yarn guide tube and the center point of the cross section is the distance in Example 1, and the distance between the projection line of the central axis of hole y on the cross section of the yarn guide tube and the center point of the cross section is 0. The interlaced yarn obtained has an entanglement strength of 90%. Comparing Comparative Example 5 with Example 2, it can be seen that the entanglement strength of Comparative Example 5 is lower. The reason for this is that when the airflow from nozzle I faces the side of the yarn and the airflow from nozzle II faces the central axis of the yarn, the mechanism of action is similar to that of Comparative Example 4, but nozzle I can form a stronger vortex than nozzle II, so that Comparative Example 5 has a higher entanglement strength than Comparative Example 4.

[0023] Comparative Example 6 The interlace processing method is almost the same as in Example 2, with the only difference being that the nozzle used is different from that shown in Example 1, that is, the holes x and y are all formed by the surface b. The interlaced yarn had an entanglement strength of 92%. Comparing Comparative Example 6 with Example 2, it can be seen that the entanglement strength of Comparative Example 6 is lower. The reason for this is that when the airflow directions of nozzle I and nozzle II are the same, there is no twisting action of the opposing airflows, so the entanglement strength of the yarn is lowered.

Claims

1. A method for increasing the entanglement strength of an interlaced multifilament using a DTY spinning process, comprising: The non-interlaced multifilament, the pretension of which is adjusted by a tensor, is gripped by a feed roller and a feed roll and passed through a yarn path of a nozzle, and is gripped by a pull-out roller and a pull-out roll and pulled out, and the interlaced multifilament is wound up by a winding roller to form a yarn. The nozzle is formed by processing a cubic structure, and in the cubic structure, faces a and a', faces b and b', and faces c and c' are parallel to each other, respectively; The processing includes forming grooves w, v, and u on face c, each of which penetrates face b and face b'; a through hole is formed which communicates the surface a with the surface a′ and passes through the grooves w, v, and u to serve as a yarn path for the nozzle; A yarn path between the grooves w and v is defined as a yarn path A. A yarn path between the groove v and the groove u is defined as a yarn path B. a hole x is formed on the surface b, the hole x being in communication with the yarn path A and having a connecting surface with the yarn path A that completely fits into a side wall of the yarn path A; a hole y is formed on the surface b', the hole y being in communication with the yarn path B and having a connection surface with the yarn path B that completely enters the side wall of the yarn path B; a central axis of the hole x and a central axis of the hole y are both perpendicular to a central axis of the yarn path on different planes, the central axes of the hole x and the hole y are parallel to each other as projection lines onto a transverse cross section of the yarn path and are symmetrical with respect to a center point of the transverse cross section, the hole x is an nozzle I of the yarn path A, and the hole y is an nozzle II of the yarn path B, a line connecting a gripping point between the feed roller and the feed roll and a gripping point between the pull-out roller and the pull-out roll overlaps with a central axis of the yarn path; the feed roller and the pull-out roller have the same linear speed; When the multifilament passes through the yarn path of the nozzle, compressed airflows are intermittently blown from nozzles I and II to yarn paths A and B, respectively, and the time for blowing the airflow from nozzle I to yarn path A is defined as t 1 After Δt has elapsed, the airflow is blown from nozzle II to yarn path B, and the blowing time is t 2 Let t 1 and 2 is the same, Δt=d / v, d is the horizontal distance between the central axis of the nozzle I and the central axis of the nozzle II, v is the linear velocity of the pull-out roller, The pressure of the airflow blown from nozzle I to yarn path A is greater than the pressure of the airflow blown from nozzle II to yarn path B. A method for increasing the entanglement strength of interlaced multifilaments.

2. The diameter of the yarn path is 2.5 to 3 mm, The nozzle I and the nozzle II have the same structure and a diameter of 0.5 to 1 mm. The distance between the projection line of the central axis of the hole x onto the cross section of the yarn path and the center point of the cross section is 0.5 to 0.8 mm. A method for increasing the entanglement strength of the interlaced multifilament according to claim 1.

3. The pressure of the airflow ejected from the nozzle I to the yarn path A is 0.1 to 0.3 MPa. The pressure of the airflow ejected from nozzle II to yarn path B is 0.05 to 0.08 MPa. A method for increasing the entanglement strength of the interlaced multifilament according to claim 1.

4. The range of d is 18 to 20 mm, The range of v is 30 to 50 m / s. A method for increasing the entanglement strength of the interlaced multifilament according to claim 1.

5. The pretension is 0.01 to 0.05 N. A method for increasing the entanglement strength of the interlaced multifilament according to claim 1.

6. t 1 is 0.1 to 0.3 ms A method for increasing the entanglement strength of the interlaced multifilament according to claim 1.

7. The interlaced multifilament has a specification of 3 to 15 tex / 10 to 40 F. A method for increasing the entanglement strength of the interlaced multifilament according to claim 1.

8. The interlaced multifilament is composed of a plurality of cycle segments that are continuous in the longitudinal direction, Each cycle segment is composed of a spread portion and an entangled portion connected in sequence. A method for increasing the entanglement strength of the interlaced multifilament according to claim 1.

9. The interlace multifilament has an interlacing strength of 97 to 99%. A method for increasing the entanglement strength of the interlaced multifilament according to claim 1.

Citation Information

Patent Citations

  • Air flow knotting and twisting composite nozzle of carpet spinning interlacer and air flow knotting and twisting method

    CN104480603A

  • Air flow knotting and twisting composite nozzle of carpet spinning interlacer and method

    CN104480604A

  • Vane wheel of multiple vane blower

    JP1982038697A

  • Yarn interlacer

    JP1993222640A

  • Processing nozzle for interlacing yarn

    JP1994101133A