Antistatic sound absorbing material and manufacturing method thereof, speakers and electronic equipment

The antistatic sound-absorbing material with molecular sieve particles and carbon additives addresses static electricity issues, ensuring stable storage and transportation while maintaining acoustic performance for speakers in miniaturized electronics.

JP2024543915AActive Publication Date: 2024-11-26エスエスアイ ニュー マテリアル (ジェンジャン) カンパニー リミテッド
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024531336
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-25
Filing Date
2022-07-29
Publication Date
2024-11-26
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

Existing sound-absorbing materials for speakers generate static electricity during transportation and processing, leading to aggregation and adhesion issues, which affect storage, transportation, and filling processes, and conventional antistatic agents compromise the porous structure and acoustic performance.

Method used

An antistatic sound-absorbing material comprising molecular sieve fine particles, a binder, and an antistatic additive such as graphene, carbon nanotubes, or graphite, with specific ratios and processing methods to prevent static electricity and maintain acoustic performance.

Benefits of technology

The material effectively prevents aggregation and adhesion due to static electricity, improves filling efficiency, and maintains or enhances acoustic performance by using carbon materials with large surface areas and porosity, suitable for miniaturized electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543915000001_ABST
    Figure 2024543915000001_ABST
Patent Text Reader

Abstract

The present invention provides an antistatic sound absorbing material and a manufacturing method thereof, a speaker, and an electronic device. The antistatic sound absorbing material includes molecular sieve particles, a binder, and an antistatic additive, and the total weight of the molecular sieve particles is 100%, and the antistatic additive is 0.5 to 10%. By mounting the antistatic sound absorbing material provided by the present invention in the back cavity of a speaker of an electronic device, it is possible to solve the problems of aggregation and interface adhesion caused by static electricity accumulation generated by friction and collision between materials, reduce wear, improve the filling amount, and ensure long-term use stability.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an antistatic sound absorbing material and its manufacturing method, a speaker and an electronic device, which belongs to the technical field of electroacoustic materials, and further to the technical field of improved sound absorbing materials for audio speakers. [Background technology]

[0002] With electronic products becoming smaller and thinner, the volume of speaker components becomes smaller and smaller.To reduce the resonance frequency of speakers and improve the low-frequency performance of electronic products, the main solution at present is to fill the back cavity of speakers with sound-absorbing particles made of porous material.The main principle is that when the speaker diaphragm moves back and forth, it compresses and decompresses the air in the back cavity to form pressure fluctuations, and the sound-absorbing particles absorb and desorb air according to the characteristics of their own porous material, which reduces the pressure fluctuations to a certain extent, and virtually increases the space of the back cavity to reduce the impact of pressure fluctuations.

[0003] The particle size of sound-absorbing particles currently on the market is generally 100 to 500 μm. When powder particles are rubbed and transported, the electrical balance is destroyed, generating static electricity, increasing the force between particles, and causing the sound-absorbing particles to agglomerate or adhere to the surface of equipment, affecting the storage, transportation, and filling processes of the sound-absorbing particles.

[0004] Currently, in the process of using sound-absorbing particles, a plasma blower is mainly used to blow plasma wind onto the sound-absorbing particles taken out of the package to remove static electricity generated during transportation, but since the sound-absorbing particles are small in volume and lightweight during the filling process, it is not possible to use a plasma blower to blow plasma wind onto the sound-absorbing particles. Therefore, there is no effective means to remove static electricity generated during the transportation process of the module filling line. However, the static electricity generated during this process has a significant impact on the use of the sound-absorbing particles.

[0005] In addition, a certain amount of antistatic agent is mainly added during the molding process of the polymer material to remove static electricity from the material, and the hydrophilic group in the added antistatic agent enhances the hygroscopicity of the material surface and forms a conductive film, which allows the material to have antistatic performance. However, most of the conventional antistatic agents currently used are also polymer materials, and the conductive film formed by them blocks the porous structure of the sound-absorbing particles to a certain extent, reducing the acoustic improvement effect of the sound-absorbing particles.

[0006] Therefore, providing a new antistatic sound-absorbing material and a manufacturing method thereof, a speaker and an electronic device has become a technical problem that needs to be solved as soon as possible in the field. Summary of the Invention

[0007] The present invention has been made to solve the above-mentioned drawbacks and deficiencies, and one of its objects is to provide an antistatic sound absorbing material.

[0008] Another object of the present invention is to provide a method for producing an antistatic sound absorbing material.

[0009] It is still another object of the present invention to provide a speaker having the above-mentioned antistatic sound absorbing material attached to the back cavity.

[0010] Another object of the present invention is to provide an electronic device with the antistatic sound-absorbing material installed in the back cavity, which can be installed in the back cavity of the speaker of the electronic device to solve the problems of aggregation and interface adhesion during transportation, filling and use caused by static electricity accumulation between materials, such as particulate antistatic sound-absorbing materials, thereby reducing wear during these processes, improving the filling amount and ensuring long-term use stability.

[0011] In order to achieve the above object, the present invention provides an antistatic sound-absorbing material comprising molecular sieve microparticles, a binder and an antistatic additive, the total weight of the molecular sieve microparticles being 100%, and the content of the antistatic additive being 0.5 to 10%.

[0012] In one specific embodiment of the antistatic sound absorbing material of the present invention, the antistatic additive comprises one or more of graphene, carbon nanotubes and graphite.

[0013] In the present invention, the fewer the number of graphene layers, the more preferable. In some preferred embodiments of the present invention, the number of graphene layers is 10 or less.

[0014] In one specific embodiment of the antistatic sound absorbing material of the present invention, the carbon nanotubes have an average pore size of 5 to 20 nm and an average length at D50 of 1 to 20 μm, preferably 5 to 15 μm.

[0015] In one specific embodiment of the antistatic sound absorbing material of the present invention, the content of the binder is 4 to 15% when calculated based on the solid content of the binder, with the total weight of the molecular sieve particles being 100%.

[0016] In one specific embodiment of the antistatic sound absorbing material of the present invention, the binder comprises an organic binder and / or an inorganic binder.

[0017] In one specific embodiment of the antistatic sound absorbing material of the present invention, the organic binder comprises one or more of a polyacrylate suspension, a polystyrene acrylate suspension, a polyvinyl acetate suspension, and a polystyrene butadiene suspension.

[0018] In one specific embodiment of the antistatic sound absorbing material of the present invention, the organic binder is contained in an amount of 5 to 12%.

[0019] In one specific embodiment of the antistatic sound absorbing material of the present invention, the inorganic binder includes one or more of kaolin, silica sol, alumina sol, and carboxymethyl cellulose.

[0020] In one specific embodiment of the antistatic sound absorbing material of the present invention, the inorganic binder is contained in an amount of 5 to 10%.

[0021] In one specific embodiment of the antistatic sound absorbing material of the present invention, the molecular sieve particles include one or more of MFI, MEL, FER, CHA, IHW, IWV, ITE, UTL, VET and MTW structure molecular sieves.

[0022] In one specific embodiment of the antistatic sound absorbing material of the present invention, the molecular sieve particles have a specific surface area of ​​300 m 2 / g and the pore volume is 0.16 to 0.32 cm 3 / g, the molar ratio of silicon oxide / aluminum oxide is more than 200, and the average particle size is 0.1 to 30 μm, preferably 0.5 to 10 μm.

[0023] In one specific embodiment of the antistatic sound absorbing material of the present invention, the molecular sieve particles are ZSM-5 molecular sieve particles.

[0024] As a specific embodiment of the antistatic sound absorbing material of the present invention, the shape of the antistatic sound absorbing material includes a granular shape, a lump shape, or a sheet shape.

[0025] In one specific embodiment of the antistatic sound-absorbing material of the present invention, when the antistatic sound-absorbing material is particulate, it has a three-stage pore structure, the size of the first stage pore structure is 0.3 to 0.7 nm, the size of the second stage pore structure is 2 to 30 nm, and the size of the third stage pore structure is 1 to 10 μm.

[0026] In one specific embodiment of the antistatic sound absorbing material of the present invention, when the antistatic sound absorbing material is in a particulate form, the bulk density is 0.32 to 0.64 g / mL.

[0027] As a specific embodiment of the antistatic sound absorbing material of the present invention, when the antistatic sound absorbing material is in a particulate form, the particle size is 50 to 1000 μm, preferably 100 to 700 μm.

[0028] However, when the antistatic sound-absorbing material is particulate, the smaller the particle size, the smaller the bulk density, and the antistatic additive in the antistatic sound-absorbing material significantly improves the phenomenon of aggregation and adhesion. When the antistatic sound-absorbing material is in a lump or sheet form, the situation in which aggregation and adhesion occur is weaker, the volume of the sheet or lump antistatic sound-absorbing material is larger than that of the particulate antistatic sound-absorbing material, and the effect of static electricity is not significant, and the antistatic agent added to the material is mainly for improving the adsorption of micro-substances in the air to the surface of the sheet or lump antistatic sound-absorbing material.

[0029] The present invention also provides a method for producing an antistatic sound-absorbing material, which includes mixing raw materials with a solvent and then molding the mixture to produce the antistatic sound-absorbing material, wherein the raw materials contain molecular sieve microparticles, a binder and an antistatic additive, and the amount of the antistatic additive used is 0.5 to 3% based on the total weight of the molecular sieve microparticles being 100%.

[0030] In one specific embodiment of the method for producing the antistatic sound absorbing material of the present invention, the antistatic additive comprises one or more of graphene, carbon nanotube and graphite.

[0031] In one specific embodiment of the method for producing the antistatic sound absorbing material of the present invention, the antistatic additive is a powder or a slurry.

[0032] In one specific embodiment of the method for producing an antistatic sound absorbing material of the present invention, when the antistatic additive is a powder, the amount used is 0.5 to 10%. When the antistatic additive is a slurry, the amount used is 1 to 10%. However, when the antistatic additive is a slurry, the amount used of the antistatic additive is the amount of solid content of the slurry.

[0033] In one specific embodiment of the method for producing the antistatic sound absorbing material of the present invention, when the antistatic additive is a slurry, the solid content is 3 to 10%, preferably 4 to 7%.

[0034] In one specific embodiment of the method for producing the antistatic sound-absorbing material of the present invention, when the antistatic additive is a slurry, the raw material further contains a dispersant, and the amount of the dispersant used is 0.5 to 2% based on the total weight of the molecular sieve microparticles being 100%.

[0035] In one specific embodiment of the method for producing the antistatic sound absorbing material of the present invention, the dispersant includes one or more of polyglycol ester aqueous solution, polycarboxylate ammonium salt aqueous solution, polycarboxylate sodium salt aqueous solution, polyacrylate aqueous solution, polyacrylate copolymer, where the polyglycol ester includes, but is not limited to, fatty acid polyethylene glycol, polyethylene glycol oleate, etc.

[0036] In one specific embodiment of the method for producing the antistatic sound absorbing material of the present invention, the antistatic additive is carbon nanotube powder or carbon nanotube aqueous slurry.

[0037] In one specific embodiment of the method for producing the antistatic sound-absorbing material of the present invention, the carbon nanotube aqueous slurry has a pH value of 6 to 10 and a viscosity of 1000 to 5000 mPa·s, preferably 1000 to 3000 mPa·s.

[0038] In one specific embodiment of the method for producing the antistatic sound-absorbing material of the present invention, the raw material further contains an auxiliary agent, and the amount of the auxiliary agent used is 0.5 to 1.5% based on the total weight of the molecular sieve microparticles being 100%.

[0039] However, the use of an auxiliary can improve the binding strength between the molecular sieve particles and the binder, thereby reducing powder falling off.

[0040] In one specific embodiment of the method for producing the antistatic sound absorbing material of the present invention, the auxiliary agent includes one or more of ethylene glycol, propylene glycol, glycerin, and dimethyl sulfoxide.

[0041] In one specific embodiment of the method for producing the antistatic sound-absorbing material of the present invention, the binder comprises an organic binder and / or an inorganic binder, the solid content of the organic binder is 30 to 60%, and the solid contents of the silica sol and alumina sol in the inorganic binder are each 30 to 50%.

[0042] In one specific embodiment of the method for producing the antistatic sound-absorbing material of the present invention, the solvent includes, but is not limited to, water, and the amount of the solvent used can be selected according to actual needs.

[0043] In one specific embodiment of the method for producing the antistatic sound-absorbing material of the present invention, the molding includes spray granulation, calcination molding, and drying and demolding in a flat mold, and these three molding methods correspond to granular, block, and sheet-shaped antistatic sound-absorbing materials, respectively.

[0044] In one specific embodiment of the method for producing the above-mentioned antistatic sound-absorbing material of the present invention, the antistatic additive is carbon nanotube powder. Taking the particulate antistatic sound-absorbing material as an example, the method includes the following specific steps:

[0045] First, molecular sieve particles, water, and carbon nanotube powder were mixed in a mass ratio of 1:0.8-1.5:0.005-0.02, and the resulting mixture was placed in a sand mill and wet-ground for 10-90 minutes. The binder and auxiliary agents were then added to the uniformly mixed slurry, which was then spray-granulated to obtain antistatic sound-absorbing particles.

[0046] As a specific embodiment of the method for producing the antistatic sound-absorbing material of the present invention, the antistatic additive is a carbon nanotube slurry. Taking the particulate antistatic sound-absorbing material as an example, the method includes the following specific steps:

[0047] First, the molecular sieve microparticles, water, carbon nanotube slurry and dispersant were mixed in a mass ratio of 1:0.55~1.25:0.005~0.03:0.005~0.02, the resulting mixture was placed in an ultrasonic dispersion device and ultrasonically dispersed for 40~120 minutes, and then added to a solution mixed with a binder and an auxiliary, and then spray-granulated to obtain antistatic sound-absorbing particulate material.

[0048] When carbon nanotube powder is used as the antistatic additive, the carbon nanotube powder and the molecular sieve particles are uniformly dispersed by grinding with a sand mill, the advantage of this method is that the molecular sieve particles and the carbon nanotubes are ground with the same slurry, the powder is uniformly mixed, the carbon nanotubes can better adhere to the surface of the molecular sieve particles, a stable system is formed, and the suspension prepared is less likely to cause aggregation and sedimentation, and the loss of carbon nanotubes in the stable system during subsequent filtration and standing is significantly reduced compared to when the carbon nanotube slurry is directly used, but when the antistatic sound-absorbing material is manufactured using this method, it has a certain effect on the improvement of the acoustic performance of the antistatic sound-absorbing material manufactured. Compared to when carbon nanotube powder is used as the antistatic additive, when the antistatic sound-absorbing material is manufactured using carbon nanotube slurry as the antistatic additive, the carbon nanotube slurry is dispersed in the molecular sieve particle suspension, the viscosity of the dispersion system is high, and the bond between the carbon nanotubes and the molecular sieve particles is poor, which makes it easy to cause aggregation and sedimentation.

[0049] Furthermore, the present invention provides a speaker including one or more acoustic sensors and one or more housings, the one or more acoustic sensors and the one or more housings being combined to form a back cavity of the speaker, and the antistatic sound-absorbing material being installed in the back cavity of the speaker.

[0050] Furthermore, the present invention provides an electronic device having the above-mentioned antistatic sound absorbing material attached to a back cavity of a speaker of the electronic device.

[0051] As a specific embodiment of the electronic device of the present invention, the electronic device includes a smartphone, a TWS earphone, a headphone, a smart glass, a smart watch, a VR device, an AR device, a tablet, or a thin notebook computer.

[0052] The beneficial technical effects that the present invention can achieve include the following: (1) The present invention uses a carbon material (such as graphene, carbon nanotubes, graphite, etc.) as an antistatic additive for the antistatic sound-absorbing material. The carbon material itself has a large specific surface area and a certain porosity. Using the carbon material as an antistatic additive in the sound-absorbing material has little effect on the acoustic effect. The unique pore structure of the carbon material itself works synergistically with the porous structure of the molecular sieve microparticles to further improve the air adsorption and desorption effect. (2) The antistatic sound-absorbing material provided by the present invention is used in the back cavity of a speaker, and the air pressure change in the back cavity is adjusted mainly by adsorbing and desorbing air, thereby improving the low-frequency response of the speaker and improving the acoustic performance of the speaker. Compared with general sound-absorbing materials, the action force (suction force) between the antistatic sound-absorbing materials provided by the present invention is smaller, the frictional charge is released quickly, the static electricity accumulation is weak, and the frictional static electricity between other components in the speaker is also reduced. The particulate antistatic sound-absorbing material has less aggregation and adhesion in the filling and box module, and can effectively reduce the particle aggregation and adhesion to the module, and can improve the filling amount and filling efficiency to a certain extent. The less the aggregation between particles, the better the acoustic improvement effect inside the material. The surface of the block or sheet-shaped antistatic sound-absorbing material is improved in adsorbing micro-substances in the air, reducing the probability of clogging on the surface. (3) The antistatic sound-absorbing material provided by the present invention can be applied to the back cavities of speakers in products that require small size and thinness, such as smartphones, VR devices, AR devices, and TWS earphones, to provide better acoustic performance. [Brief description of the drawings]

[0053] In order to more clearly describe the embodiments of the present invention or the technical solutions in the prior art, the drawings required in the description of the embodiments will be briefly described below. It is self-evident that the drawings in the following description are some embodiments of the present invention, and those skilled in the art can also obtain other drawings based on these drawings without any creative efforts. [Figure 1] FIG. 1 is a schematic diagram (SEM image) of the morphology of the carbon nanotube powder used in the examples of the present invention. [Figure 2a] Figure 2a is a schematic diagram showing the adhesion state of the sound-absorbing particulate material produced in Comparative Example 1 to the PET film at the box filling port. [Figure 2b] Figure 2b is a schematic diagram of the adhesion state of the antistatic sound-absorbing particulate material manufactured in Example 1 of the present invention to the PET film at the box filling port. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0054] The "ranges" disclosed herein are given as lower and upper limits. There may be one or more lower limits and one or more upper limits, respectively. A given range is defined by selecting one lower limit and one upper limit. The selected lower and upper limits define the boundaries of the particular range. All ranges defined in this manner are combinable, and any lower limit can be combined with any upper limit to form a range. For example, for a particular parameter, ranges of 60-120 and 80-110 are listed, with the understanding that ranges of 60-110 and 80-120 are also contemplated. Also, if the minimum range values ​​listed are 1 and 2, and the maximum range values ​​listed are 3, 4, and 5, then the ranges 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are all contemplated.

[0055] In the present invention, unless otherwise specified, the numerical range "a to b" is an abbreviation of any combination of real numbers from a to b, where a and b are both real numbers. For example, the numerical range "0 to 5" indicates that all real numbers between "0 and 5" have already been listed in the text, and "0 to 5" is merely an abbreviation of this combination of numerical values.

[0056] In the present invention, unless otherwise specified, all the embodiments and preferred embodiments mentioned in the present specification can be combined with each other to form new technical solutions.

[0057] In the present invention, unless otherwise specified, all technical features and preferred technical features mentioned in the text can be combined with each other to form new technical solutions.

[0058] In the present invention, unless otherwise specified, the term "comprise" referred to in the text may be open-ended or closed-ended. For example, the term "comprise" may represent the inclusion of other materials and / or elements not listed, or may represent the inclusion of only the listed materials and / or elements.

[0059] In order to more clearly understand the technical features, objectives and beneficial effects of the present invention, the technical solutions of the present invention are described in detail below with reference to the following specific examples, which should not be construed as limiting the scope of the present invention. EXAMPLES

[0060] Example 1 In this embodiment, the antistatic sound-absorbing particles are prepared according to the following specific steps:

[0061] 100 g of ZSM-5 molecular sieve fine particles, 90 g of water, and 0.5 g of carbon nanotube powder were mixed uniformly, and the resulting mixture was placed in a sand mill and polished for 30 minutes, after which it was taken out to obtain liquid A.

[0062] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here is 425, the pore volume is 0.247 mL / g, the average particle diameter is 1.73 μm, and the specific surface area is 385 m 2 / g.

[0063] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm. The morphology of the carbon nanotubes was as shown in FIG.

[0064] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0065] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain antistatic sound absorbing particulate material.

[0066] The antistatic sound-absorbing particulate material produced in this embodiment had an average particle diameter of 364 μm and a bulk density of 0.357 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 0.5% and the polystyrene acrylate was 5.98%. EXAMPLES

[0067] Example 2 In this embodiment, the antistatic sound-absorbing particles are prepared according to the following specific steps:

[0068] 100 g of ZSM-5 molecular sieve fine particles, 90 g of water, and 1 g of carbon nanotube powder were mixed uniformly, and the mixture was placed in a sand mill and polished for 40 minutes, after which it was taken out to obtain liquid A.

[0069] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0070] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0071] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0072] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain antistatic sound absorbing particulate material.

[0073] The antistatic sound-absorbing particulate material produced in this embodiment had an average particle diameter of 366 μm and a bulk density of 0.354 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 0.99% and the polystyrene acrylate was 5.99%. EXAMPLES

[0074] Example 3 In this embodiment, the antistatic sound-absorbing particles are prepared according to the following specific steps:

[0075] 100 g of ZSM-5 molecular sieve fine particles, 90 g of water, and 2 g of carbon nanotube powder were mixed uniformly, and the mixture was placed in a sand mill and polished for 45 minutes, after which it was taken out to obtain liquid A.

[0076] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0077] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0078] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0079] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain antistatic sound absorbing particulate material.

[0080] The antistatic sound-absorbing particulate material produced in this embodiment had an average particle diameter of 362 μm and a bulk density of 0.36 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 2% and the polystyrene acrylate was 6%. EXAMPLES

[0081] Example 4 In this embodiment, the antistatic sound-absorbing particles are prepared according to the following specific steps:

[0082] 100 g of ZSM-5 molecular sieve fine particles, 90 g of water, and 3.5 g of carbon nanotube powder were mixed uniformly, and the resulting mixture was placed in a sand mill and polished for 50 minutes, after which it was taken out to obtain liquid A.

[0083] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0084] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0085] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0086] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain the antistatic sound absorbing particulate material.

[0087] The antistatic sound-absorbing particulate material produced in this embodiment had an average particle size of 366 μm and a bulk density of 0.357 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 3.48% and the polystyrene acrylate was 5.89%. EXAMPLES

[0088] Example 5 In this embodiment, an antistatic sound-absorbing block is provided which is manufactured by the following specific steps:

[0089] 100 g of ZSM-5 molecular sieve fine particles, 90 g of water, and 0.5 g of carbon nanotube powder were mixed uniformly, and the resulting mixture was placed in a sand mill and polished for 30 minutes, after which it was taken out to obtain liquid A.

[0090] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0091] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0092] Liquid B was obtained by uniformly mixing 30 g of water, 14 g of silica sol with a solid content of 30%, and 1 g of propylene glycol.

[0093] Liquid B is added to liquid A to obtain mixed liquid C, and the mixed liquid C is filtered using a 400 mesh filter paper, and then poured into a block mold (a conventional equipment used in the field) and filtered at 450 o C for 4 hours, molded, and then demolded to obtain the antistatic sound absorbing block.

[0094] The antistatic sound absorbing mass produced in this example had a bulk density of 0.389 g / mL, and the total weight of the molecular sieve particles in the mass was 100%, with the carbon nanotubes being 0.5%. EXAMPLES

[0095] Example 6 In this embodiment, an antistatic sound-absorbing sheet material is provided, which is manufactured according to the following specific steps:

[0096] 100 g of ZSM-5 molecular sieve fine particles, 90 g of water, and 1 g of carbon nanotube powder were mixed uniformly, and the mixture was placed in a sand mill and polished for 40 minutes, after which it was taken out to obtain liquid A.

[0097] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0098] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0099] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0100] Liquid B is added to liquid A to obtain mixed liquid C, which is then filtered using a 400 mesh filter paper and placed in a large flat mold (a conventional device used in the art). o C for 30 minutes and then released to obtain an antistatic sound absorbing sheet material.

[0101] The antistatic sound-absorbing sheet material produced in this embodiment had an average thickness of 542 μm and a bulk density of 0.532 g / mL. In the sheet material, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 1% and the polystyrene acrylate was 6%. EXAMPLES

[0102] Example 7 In this embodiment, the antistatic sound-absorbing particles are prepared according to the following specific steps:

[0103] 100g of ZSM-5 molecular sieve particles, 80g of water, 20g of carbon nanotube aqueous slurry (solid content 5%), and 1g of fatty acid polyethylene glycol aqueous solution were mixed uniformly and irradiated with ultrasonic waves for 45 minutes to obtain liquid A.

[0104] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0105] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0106] The pH value of the carbon nanotube aqueous slurry used was 7.2 and the viscosity was 1856 mPa·s.

[0107] Liquid B was obtained by uniformly mixing 20 g of water, 15 g of a polystyrene acrylate suspension with a solid content of 40%, and 1 g of propylene glycol.

[0108] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain antistatic sound absorbing particulate material.

[0109] The antistatic sound-absorbing particulate material produced in this embodiment had an average particle diameter of 373 μm and a bulk density of 0.355 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 0.98% and the polystyrene acrylate was 6%. EXAMPLES

[0110] Example 8 In this embodiment, the antistatic sound-absorbing particles are prepared according to the following specific steps:

[0111] 100g of ZSM-5 molecular sieve particles, 70g of water, 40g of carbon nanotube aqueous slurry (solid content 5%), and 1g of fatty acid polyethylene glycol aqueous solution were mixed uniformly and irradiated with ultrasonic waves for 60 minutes to obtain liquid A.

[0112] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0113] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0114] The pH value of the carbon nanotube aqueous slurry used was 7.2 and the viscosity was 1856 mPa·s.

[0115] Liquid B was obtained by uniformly mixing 20 g of water, 15 g of a polystyrene acrylate suspension with a solid content of 40%, and 1 g of propylene glycol.

[0116] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain antistatic sound absorbing particulate material.

[0117] The antistatic sound-absorbing particulate material produced in this embodiment had an average particle size of 377 μm and a bulk density of 0.361 g / mL. In the particles, the total weight of the molecular sieve particles was 100%, and the carbon nanotubes were 1.98% and the polystyrene acrylate was 5.96%. EXAMPLES

[0118] Example 9 In this embodiment, the antistatic sound-absorbing particles are prepared according to the following specific steps:

[0119] 100g of ZSM-5 molecular sieve particles, 55g of water, 60g of carbon nanotube aqueous slurry (solid content 5%), and 1g of fatty acid polyethylene glycol aqueous solution were mixed uniformly and irradiated with ultrasonic waves for 70 minutes to obtain liquid A.

[0120] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0121] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0122] The pH value of the carbon nanotube aqueous slurry used was 7.2 and the viscosity was 1856 mPa·s.

[0123] Liquid B was obtained by uniformly mixing 20 g of water, 15 g of a polystyrene acrylate suspension with a solid content of 40%, and 1 g of propylene glycol.

[0124] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain antistatic sound absorbing particulate material.

[0125] The antistatic sound-absorbing particulate material produced in this embodiment had an average particle diameter of 381 μm and a bulk density of 0.365 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 0.98% and the polystyrene acrylate was 6%. EXAMPLES

[0126] Example 10 In this embodiment, the antistatic sound-absorbing particles are prepared according to the following specific steps:

[0127] 100 g of S-1 molecular sieve particles (MFI structure), 90 g of water, and 0.5 g of carbon nanotube powder were mixed uniformly, and the resulting mixture was placed in a sand mill and polished for 30 minutes, after which it was taken out to obtain liquid A.

[0128] The carbon nanotubes used herein had an average pore size of 5 to 20 nm, and their average particle size, ie, average length at D50, was ≦10 μm.

[0129] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0130] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain antistatic sound absorbing particulate material.

[0131] The antistatic sound-absorbing particulate material produced in this embodiment had an average particle diameter of 363 μm and a bulk density of 0.361 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 0.5% and the polystyrene acrylate was 5.91%. EXAMPLES

[0132] Example 11 This example provides an antistatic sound-absorbing particulate material, which is different from Example 9 in that 100g of ZSM-35 molecular sieve particles (FER structure) are selected, and other manufacturing steps are the same. The average particle size of the antistatic sound-absorbing particulate material manufactured in this example is 370μm, the bulk density is 0.365g / mL, and in the particles, the total weight of the molecular sieve particles is 100%, and the carbon nanotubes are 0.5% and the polystyrene acrylate is 6%. EXAMPLES

[0133] Example 12 In this embodiment, the antistatic sound-absorbing particles are prepared according to the following specific steps:

[0134] 100 g of ZSM-5 molecular sieve particles, 90 g of water, and 0.5 g of graphene powder were mixed uniformly, and the mixture was placed in a sand mill and polished for 30 minutes. Then, the mixture was taken out to obtain liquid A.

[0135] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0136] The average number of layers of the graphene powder used was 10 layers.

[0137] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0138] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain antistatic sound absorbing particulate material.

[0139] The antistatic sound-absorbing particulate material produced in this embodiment had an average particle diameter of 363 μm and a bulk density of 0.361 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and graphene was 0.5% and polystyrene acrylate was 6%.

[0140] Comparative Example 1 (Comparative Example without Carbon Nanotube / Graphene Powder as Antistatic Additive) In this comparative example, sound-absorbing particles were provided by manufacturing the following specific steps.

[0141] 100 g of ZSM-5 molecular sieve particles and 90 g of water were mixed uniformly to obtain liquid A.

[0142] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0143] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0144] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain the sound-absorbing particulate material.

[0145] The sound-absorbing particulate material produced in this comparative example had an average particle size of 365 μm and a bulk density of 0.358 g / mL.

[0146] Comparative Example 2 (Comparative Example in which the amount of carbon nanotube powder used as an antistatic additive is not within the range described in the claims) In this comparative example, the antistatic sound-absorbing particulate material is prepared according to the following specific steps:

[0147] 100 g of ZSM-5 molecular sieve fine particles, 90 g of water, and 11 g of carbon nanotube powder were mixed uniformly, and the resulting mixture was placed in a sand mill and polished for 50 minutes, after which it was taken out to obtain liquid A.

[0148] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0149] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0150] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0151] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain the antistatic sound absorbing particulate material.

[0152] The antistatic sound-absorbing particulate material produced in this comparative example had an average particle diameter of 366 μm and a bulk density of 0.357 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 10.3% and the polystyrene acrylate was 5.89%.

[0153] Comparative Example 3 (Comparative Example in which the average length of the carbon nanotube powder, which is an antistatic additive, is not within the range described in the claims) In this comparative example, the antistatic sound-absorbing particulate material is prepared according to the following specific steps:

[0154] 100 g of ZSM-5 molecular sieve fine particles, 90 g of water, and 1 g of carbon nanotube powder were mixed uniformly, and the mixture was placed in a sand mill and polished for 40 minutes, after which it was taken out to obtain liquid A.

[0155] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0156] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦25 μm.

[0157] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0158] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain the antistatic sound absorbing particulate material.

[0159] The antistatic sound absorbing particulate material produced in this comparative example had an average particle size of 375 μm and a bulk density of 0.351 g / mL.

[0160] Comparative Example 4 (Comparative Example in which the average length of the carbon nanotube powder, which is an antistatic additive, is not within the range described in the claims) In this comparative example, the antistatic sound-absorbing particulate material is prepared according to the following specific steps:

[0161] 100 g of ZSM-5 molecular sieve fine particles, 90 g of water, and 1 g of carbon nanotube powder were mixed uniformly, and the mixture was placed in a sand mill and polished for 45 minutes, after which it was taken out to obtain liquid A.

[0162] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0163] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦40 μm.

[0164] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0165] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain the antistatic sound absorbing particulate material.

[0166] The antistatic sound absorbing particulate material produced in this comparative example had an average particle size of 379 μm and a bulk density of 0.349 g / mL.

[0167] Comparative Example 5 (Comparative Example in which the amount of carbon nanotube aqueous slurry used as an antistatic additive is not within the range described in the claims) In this comparative example, the antistatic sound-absorbing particulate material is prepared according to the following specific steps:

[0168] 100g of ZSM-5 molecular sieve particles, 50g of water, 80g of carbon nanotube aqueous slurry (solid content 5%), and 1g of fatty acid polyethylene glycol aqueous solution were mixed uniformly and irradiated with ultrasonic waves for 120 minutes to obtain liquid A.

[0169] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0170] The carbon nanotubes used had an average pore size of 5-20 nm and an average particle size, ie, an average length at D50, of ≦10 μm.

[0171] The pH value of the carbon nanotube aqueous slurry used was 7.2 and the viscosity was 1856 mPa·s.

[0172] Liquid B was obtained by uniformly mixing 20 g of water, 15 g of a polystyrene acrylate suspension with a solid content of 40%, and 1 g of propylene glycol.

[0173] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain antistatic sound absorbing particulate material.

[0174] The antistatic sound-absorbing particulate material produced in this comparative example had an average particle diameter of 382 μm and a bulk density of 0.364 g / mL. In the particles, the total weight of the molecular sieve microparticles was 100%, and the carbon nanotubes were 4% and the polystyrene acrylate was 5.91%.

[0175] Comparative Example 6 (Comparative Example of Different Type of Molecular Sieve without Antistatic Additive Carbon Nanotube Powder) In this comparative example, sound-absorbing particles were provided by manufacturing the following specific steps.

[0176] 100 g of S-1 molecular sieve particles and 90 g of water were mixed uniformly to obtain liquid A.

[0177] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0178] Liquid B was added to liquid A to obtain mixed liquid C, which was then filtered using 400 mesh filter paper and granulated to obtain the sound-absorbing particulate material.

[0179] The sound absorbing particulate material produced in this comparative example had an average particle size of 365 μm and a bulk density of 0.360 g / mL.

[0180] Comparative Example 7 (Comparative Example of a Different Type of Molecular Sieve Without the Antistatic Additive Carbon Nanotube Powder) This comparative example provides a sound-absorbing particulate material, and is different from Comparative Example 6 in that 100 g of ZSM-35 molecular sieve particles are selected, and the other manufacturing steps are the same.

[0181] The sound-absorbing particulate material produced in this comparative example had an average particle size of 370 μm and a bulk density of 0.366 g / mL.

[0182] Comparative Example 8 (Comparative Example of Sound Absorbing Block Material that Does Not Use Carbon Nanotube Powder as an Antistatic Additive) In this comparative example, a sound-absorbing block material was provided which was manufactured according to the following specific steps.

[0183] 100 g of ZSM-5 molecular sieve particles and 90 g of water were mixed uniformly, and the mixture was placed in a sand mill and polished for 30 minutes. Then, the mixture was taken out to obtain liquid A.

[0184] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0185] Liquid B was obtained by uniformly mixing 30 g of water, 12 g of a polystyrene acrylate suspension with a solid content of 30%, and 1 g of propylene glycol.

[0186] Liquid B is added to liquid A to obtain mixed liquid C, and the mixed liquid C is filtered using a 400 mesh filter paper, and then poured into a block mold (a conventional equipment used in the field) and filtered at 450 o C for 4 hours, molded, and then demolded to obtain the sound-absorbing block.

[0187] The bulk density of the sound absorbing block produced in this comparative example was 0.392 g / mL.

[0188] Comparative Example 9 (Comparative Example of Sound-Absorbing Sheet Material that Does Not Use Carbon Nanotube Powder as an Antistatic Additive) In this comparative example, a sound-absorbing sheet material was provided that was produced in the following specific steps.

[0189] 100 g of ZSM-5 molecular sieve particles and 90 g of water were mixed uniformly, and the mixture was placed in a sand mill and polished for 40 minutes, after which it was taken out to obtain liquid A.

[0190] The molar ratio of silicon oxide / aluminum oxide of the ZSM-5 molecular sieve particles used here was 425, the pore volume was 0.247 mL / g, the average particle diameter was 1.73 μm, and the specific surface area was 385 m 2 / g.

[0191] Liquid B was obtained by uniformly mixing 30 g of water, 15 g of a polystyrene acrylate suspension having a solid content of 40%, and 1 g of propylene glycol.

[0192] Liquid B is added to liquid A to obtain mixed liquid C, which is then filtered using a 400 mesh filter paper and placed in a large flat mold (a conventional device used in the art). o C for 30 minutes and then released to obtain a sound absorbing sheet material.

[0193] The sound absorbing sheet material produced in this comparative example had an average thickness of 542 μm and a bulk density of 0.534 g / mL.

[0194] Test Example 1 In this test example, the surface resistance of the antistatic sound-absorbing particulate materials produced in Examples 1 to 4 and 7 to 12, the sound-absorbing particulate materials produced in Comparative Examples 1 and 6 to 7, and the antistatic sound-absorbing particulate materials produced in Comparative Examples 2 to 5 were each measured.

[0195] In this test example, the acoustic performance (ΔF0) was measured for speakers whose back cavities were fitted with antistatic sound-absorbing particulate materials produced in Examples 1 to 4 and 7 to 12, sound-absorbing particulate materials produced in Comparison Examples 1 and 6 to 7, and antistatic sound-absorbing particulate materials produced in Comparison Examples 2 to 5.

[0196] Here, the measurements are all performed by methods commonly used in the art. For example, the specific measurement method of the acoustic performance can be performed by referring to the method of "electrical impedance measurement" shown in paragraphs 0049 to 0054 of Chinese Patent CN105049997A. Specifically, the method of "electrical impedance measurement" is used to measure each speaker to obtain an electrical impedance spectrum, and the curve in the electrical impedance spectrum corresponds to the electrical impedance curve, where the frequency corresponding to the highest point of the electrical impedance curve is F0. When the speaker is not equipped with antistatic sound-absorbing particulate material or sound-absorbing particulate material, the measured F0 is F0. 0~キャビティ When antistatic sound-absorbing particles or sound-absorbing particles are attached to the speaker, the measured F0 is expressed as F 0~サンプル又はリファレンス Then, the calculation formula for ΔF0 is as follows:

[0197] ΔF0=F 0~キャビティ -F 0~サンプル或リファレンス .

[0198] In this test example, the acoustic performance was measured in the following environment: a standard acoustic test module with a (1) cc back cavity and a test fill of 0.35 cc.

[0199] Surface resistance measurement is done by BEIJING The measurement was performed using a BEST-212 type smart volume surface resistivity meter manufactured by BEIGUANG JINGYI INSTRUMENT EQUIPMENT CO., LTD., and the measurement voltage was 100V.

[0200] The surface resistance measurement results and acoustic performance (ΔF0) measurement results obtained in this test example are shown in Tables 1, 2, 3, and 4.

[0201] [Table 1] As can be seen from Table 1 above, the surface resistance of the sound-absorbing particles produced by adding carbon nanotube powder and carbon nanotube aqueous slurry is significantly reduced. Here, under the premise of the same solid loading amount, the reduction in the surface resistance of the sound-absorbing particles produced by using carbon nanotube powder as an antistatic additive is more significant than that of the sound-absorbing particles produced by using carbon nanotube aqueous slurry as an antistatic additive. This is due to the following reasons. In this method, the carbon nanotube powder is uniformly mixed with the molecular sieve particles in the same slurry by grinding, so that the carbon nanotubes can adhere better to the surface of the molecular sieve particles to form a stable system, and the suspension prepared by mixing the resulting mixture with the binder and auxiliary agent is also less likely to cause aggregation and sedimentation and has good dispersibility. Furthermore, when the mixture is subsequently filtered and left to stand, the loss of carbon nanotubes in the stable system is significantly reduced compared to when the carbon nanotube slurry is directly used. Compared with the case of using carbon nanotube powder as the antistatic additive, when the antistatic sound-absorbing material is manufactured using carbon nanotube slurry as the antistatic additive, the carbon nanotube slurry is dispersed in the molecular sieve microparticle suspension, the viscosity of the dispersion system is high, the carbon nanotubes and the molecular sieve microparticles are poorly bonded, and the carbon nanotubes are easily aggregated and settled, the stability is poor, and the loss of carbon nanotubes is large when filtered and left. However, during the grinding process, the carbon nanotube powder adheres in large amounts to the surface of the molecular sieve microparticles, which has some effect on the pores of the sound-absorbing particles after molding. Under the premise of the same solid loading amount, the acoustic performance (ΔF0) of the sound-absorbing particulate material manufactured using carbon nanotube aqueous slurry as the antistatic additive is better than that of the sound-absorbing particulate material manufactured using carbon nanotube powder as the antistatic additive.

[0202] As can be seen from Table 1 above, in Comparative Example 1, Example 1, Example 2, Example 3, and Comparative Example 2, the surface resistance of the sound-absorbing particulate material decreases with an increase in the amount of carbon nanotube powder added. This proves that the antistatic performance of the sound-absorbing particulate material is significantly improved, but with an increase in the amount of carbon nanotube powder added, the acoustic performance (ΔF0) of the manufactured sound-absorbing particulate material is also affected to a certain extent, and when the amount of carbon nanotube powder added is 3.5%, the acoustic performance (ΔF0) is attenuated very severely, exceeding 10Hz, and when the amount of carbon nanotube powder added is 11%, the acoustic performance (ΔF0) is further attenuated, approaching 40Hz.

[0203] As can be seen from Table 1 above, in Example 2, Comparative Example 3, and Comparative Example 4, the surface resistance value of the manufactured sound-absorbing particulate material decreases as the average particle diameter of the carbon nanotube powder increases. This proves that the longer the carbon nanotubes, which are the antistatic additive, the more advantageous they are for dissipating static electricity, but the longer the average particle diameter of the carbon nanotubes, which are the antistatic additive, the greater the impact on the surface pores of the manufactured sound-absorbing particulate material, thereby decreasing the acoustic performance (ΔF0) of the sound-absorbing particulate material.

[0204] As can be seen from Table 1 above, in Comparative Example 1, Example 7, Example 8, Example 9, and Comparative Example 5, as the amount of carbon nanotube slurry (in solid content) added increases, the surface resistance value of the manufactured sound-absorbing particulate material decreases, but as the amount of carbon nanotube slurry added increases, the acoustic performance (ΔF0) of the manufactured sound-absorbing particulate material also decreases. When the amount of carbon nanotube slurry (in solid content) added reaches 4%, the decrease in acoustic performance (ΔF0) becomes quite noticeable.

[0205] [Table 2] As can be seen from Table 2 above, when carbon nanotube powder is used as an antistatic additive for sound-absorbing particulate materials manufactured using different molecular sieve microparticles, the surface resistance of the sound-absorbing particulate materials is significantly reduced in all cases, and the effect of the antistatic additive on the acoustic performance (ΔF0) of the sound-absorbing particulate materials is small.

[0206] [Table 3] As can be seen from Table 3 above, when carbon nanotube powder and graphene are used as antistatic additives, both significantly reduce the surface resistance of the manufactured sound-absorbing particulate material, but assuming that other manufacturing conditions are approximately the same, the surface resistance value of the antistatic sound-absorbing particulate material manufactured using carbon nanotube powder as an antistatic additive is lower than that of the antistatic sound-absorbing particulate material manufactured using graphene as an antistatic additive. In addition, the acoustic performance (ΔF0) of the antistatic sound-absorbing particulate material manufactured using carbon nanotube powder as an antistatic additive is superior to that of the antistatic sound-absorbing particulate material manufactured using graphene as an antistatic additive.

[0207] [Table 4] As can be seen from Table 4 above, regardless of whether the antistatic sound-absorbing material is a particle, a lump, or a sheet, when carbon nanotube powder is used as an antistatic additive, the surface resistance of the sound-absorbing particulate material is significantly reduced. Furthermore, regardless of the form of the antistatic sound-absorbing material, adding carbon nanotube powder as an antistatic additive has little effect on its acoustic performance (ΔF0).

[0208] Test Example 2 In this test example, the yield rates of the antistatic sound-absorbing particulate materials produced in Examples 1 to 4 and 7 to 12, the sound-absorbing particulate materials produced in Comparative Examples 1, 6 to 7, and the antistatic sound-absorbing particulate materials produced in Comparative Examples 2 to 5 were determined by a conventional method in the field, and the experimental results obtained are shown in Table 5. Here, the specific process of determining the yield rate of the material includes the following. After forming the fine particles into particles, the particles need to be sieved (to control the particle size) and sorted (to sort the crushed powder) so as to select the good products. Note that the particles that are sieved are all particles with a particle size that is too large or too small, and such particles are generally irregularly shaped particles, and in the sorting step, particles with cracked surfaces are treated as defective crushed powder, and the remaining powders are considered to be good products.

[0209] [Table 5] As can be seen from Table 5 above, with the increase in the amount of carbon nanotube powder added, the yield rate of the resulting product decreases. This is mainly because the carbon nanotube powder generates more irregular particles and crushed powder, and as the average particle size of the carbon nanotube powder increases, the proportion of irregular particles in the resulting product increases significantly, because the longer the length of the carbon nanotube powder is, the more non-uniform its distribution within the particle is, and the poorer the sphericity of the resulting particles.

[0210] As can be seen from Table 5 above, the yield rate of sound-absorbing particulate materials made using carbon nanotube aqueous slurry as an antistatic additive is lower than that of sound-absorbing particulate materials made using carbon nanotube powder as an antistatic additive, assuming the same solid loading. This is because the viscosity of the carbon nanotube aqueous slurry is high, and the viscosity of the mixed system increases as the amount of carbon nanotube aqueous slurry added increases, making granulation and dispersion more difficult and resulting in more irregularly shaped particles and crushed powder.

[0211] Test Example 3 In this test example, the filling amount of a speaker in which the antistatic sound-absorbing particulate material produced in Examples 1 to 4 and the sound-absorbing particulate material produced in Comparison Example 1 were installed in the back cavity was measured, and the measurement results obtained are shown in Table 6.

[0212] Measurement environment for this test example: The volume of the cavity (back cavity) of the speaker module used for filling is 0.2 cc, and the duration of the filling funnel is 10 s.

[0213] [Table 6] As can be seen from Table 6 above, with an increase in the amount of antistatic additive added, the loading amount of sound-absorbing particles under certain conditions gradually increases, but with the decrease in static electricity on the surface of the sound-absorbing particles, the relationship between the static electricity improvement effect and the increase in loading amount is not a linear trend.

[0214] Test Example 4 In this test example, the adhesion state of the sound-absorbing particulate material produced in Comparative Example 1 and the antistatic sound-absorbing particulate material produced in Example 1 of the present invention to the PET film at the box filling port was considered. A schematic diagram of the adhesion state of the sound-absorbing particulate material produced in Comparative Example 1 to the PET film at the box filling port is shown in Figure 2a, and a schematic diagram of the adhesion state of the antistatic sound-absorbing particulate material produced in Example 1 of the present invention to the PET film at the box filling port is shown in Figure 2b.

[0215] As can be seen from Figures 2a and 2b, the antistatic sound-absorbing particulate material prepared by adding the antistatic additive in Example 1 of the present invention adheres better to the PET film at the box inlet than the sound-absorbing particulate material prepared in Comparative Example 1. This proves that the static electricity of the antistatic sound-absorbing particulate material is effectively released.

[0216] The above description is merely a specific embodiment of the present invention and cannot limit the scope of the invention, so that the replacement of equivalent members or equivalent changes and modifications made based on the patent scope of the present invention should all be within the scope of the present invention. In addition, the technical features of the present invention can be freely combined with each other, between technical features and technical inventions, and between technical inventions and technical inventions.

Claims

1. An antistatic sound absorbing material comprising molecular sieve particles, a binder and an antistatic additive, the total weight of the molecular sieve particles being 100%, and the content of the antistatic additive being 0.5 to 10%.

2. 2. The antistatic sound absorbing material according to claim 1, wherein the antistatic additive comprises one or more of graphene, carbon nanotubes and graphite.

3. 3. The antistatic sound absorbing material according to claim 2, wherein the carbon nanotubes have an average pore size of 5 to 20 nm and an average length at D50 of 1 to 20 μm.

4. 4. The antistatic sound absorbing material according to claim 3, wherein the carbon nanotubes have an average pore size of 5 to 20 nm and an average length at D50 of 5 to 15 μm.

5. The antistatic sound-absorbing material according to claim 1, characterized in that the content of the binder is 4 to 15% when calculated based on the solid content of the binder, with the total weight of the molecular sieve particles being 100%.

6. 6. The antistatic sound absorbing material according to claim 5, wherein the binder comprises an organic binder and / or an inorganic binder.

7. 7. The antistatic sound absorbing material according to claim 6, wherein the organic binder comprises one or more of the following: polyacrylate suspension, polystyrene acrylate suspension, polyvinyl acetate suspension, polystyrene butadiene suspension.

8. 8. The antistatic sound absorbing material according to claim 7, characterized in that the organic binder is present in an amount of 5 to 12%.

9. 7. The antistatic sound absorbing material according to claim 6, wherein the inorganic binder comprises one or more of kaolin, silica sol, alumina sol, and carboxymethyl cellulose.

10. 10. The antistatic sound absorbing material according to claim 9, characterized in that the inorganic binder is present in an amount of 5 to 10%.

11. 2. The antistatic sound absorbing material according to claim 1, wherein the molecular sieve particles include one or more of MFI, MEL, FER, CHA, IHW, IWV, ITE, UTL, VET and MTW structure molecular sieves.

12. The specific surface area of ​​the molecular sieve particles is 300 m 2 / g and a pore volume of 0.16 to 0.32 cm 3 / g, the molar ratio of silicon oxide / aluminum oxide is greater than 200, and the average particle size is 0.1 to 30 μm.

13. 13. The antistatic sound absorbing material according to claim 12, characterized in that the molecular sieve fine particles have an average particle size of 0.5 to 10 μm.

14. 12. The antistatic sound absorbing material according to claim 11, wherein the molecular sieve particles are ZSM-5 molecular sieve particles.

15. 2. The antistatic sound-absorbing material according to claim 1, wherein the shape of the antistatic sound-absorbing material includes a granular, lump or sheet shape.

16. The antistatic sound-absorbing material according to claim 15, characterized in that when the antistatic sound-absorbing material is particulate, it has a three-stage pore structure, the size of the first stage pore structure is 0.3 to 0.7 nm, the size of the second stage pore structure is 2 to 30 nm, and the size of the third stage pore structure is 1 to 10 μm.

17. A method for producing an antistatic sound-absorbing material, comprising mixing a raw material with a solvent and then molding the mixture to produce an antistatic sound-absorbing material, wherein the raw material comprises molecular sieve particles, a binder and an antistatic additive, and the amount of the antistatic additive used is 0.5 to 10% based on the total weight of the molecular sieve particles being 100%.

18. 20. The method for manufacturing an antistatic sound absorbing material according to claim 17, wherein the antistatic additive comprises one or more of graphene, carbon nanotubes and graphite.

19. 20. The method for manufacturing an antistatic sound absorbing material according to claim 17, wherein the antistatic additive is a powder or a slurry.

20. When the antistatic additive is a powder, the amount of the antistatic additive used is 0.5 to 10%. The method for producing an antistatic sound absorbing material according to claim 19, characterized in that, when the antistatic additive is a slurry, its usage amount is 1-10%, and, when the antistatic additive is a slurry, the usage amount of the antistatic additive is the usage amount of the solid content of the slurry.

21. The method for producing an antistatic sound absorbing material according to claim 19, characterized in that, when the antistatic additive is a slurry, its solid content is 3-10%.

22. The method for producing an antistatic sound absorbing material according to claim 21, characterized in that when the antistatic additive is a slurry, its solid content is 4-7%.

23. The method for manufacturing antistatic sound-absorbing material according to claim 19, characterized in that, when the antistatic additive is a slurry, the raw material further comprises a dispersant, and the total weight of the molecular sieve microparticles is 100%, the amount of the dispersant used is 0.5-2%.

24. 24. The method for manufacturing an antistatic sound absorbing material according to claim 23, characterized in that the dispersing agent comprises one or more of a polyglycol ester aqueous solution, a polycarboxylic acid ammonium salt aqueous solution, a polycarboxylic acid sodium salt aqueous solution, a polyacrylate aqueous solution, and a polyacrylate copolymer.

25. 18. The method for manufacturing an antistatic sound absorbing material according to claim 17, characterized in that the antistatic additive is carbon nanotube powder or carbon nanotube aqueous slurry.

26. The method for manufacturing an antistatic sound-absorbing material according to claim 25, wherein the pH value of the carbon nanotube aqueous slurry is 6-10, and the viscosity is 1000-5000 mPa·s.

27. The method for manufacturing an antistatic sound-absorbing material according to claim 26, characterized in that the viscosity of the carbon nanotube aqueous slurry is 1000 to 3000 mPa·s.

28. The method for manufacturing antistatic sound-absorbing material according to claim 17, characterized in that the raw material further comprises an auxiliary agent, and the total weight of the molecular sieve microparticles is 100%, and the amount of the auxiliary agent is 0.5 to 1.5%.

29. 30. The method for manufacturing an antistatic sound absorbing material according to claim 28, wherein the auxiliary comprises one or more of ethylene glycol, propylene glycol, glycerin, dimethyl sulfoxide.

30. The method for manufacturing an antistatic sound-absorbing material according to claim 17, characterized in that the binder comprises an organic binder and / or an inorganic binder, the solid content of the organic binder is 30-60%, and the solid contents of silica sol and alumina sol in the inorganic binder are each 30-50%.

31. A speaker comprising one or more acoustic sensors and one or more housings, the one or more acoustic sensors and the one or more housings being combined to form a back cavity of the speaker, the speaker being characterized in that the antistatic sound absorbing material according to claim 1 is attached to the back cavity of the speaker.

32. 10. An electronic device comprising the antistatic sound absorbing material according to claim 1 attached to a back cavity of a speaker of the electronic device.

33. 33. The electronic device of claim 32, comprising a smartphone, a TWS earphone, a headphone, a smart glass, a smart watch, a VR device, an AR device, a tablet, or a thin laptop.

Citation Information

Patent Citations

  • Miniature loudspeaker module with high heat dissipation efficiency and smart phone comprising same

    CN112399289A

  • High-temperature-resistant sound-absorbing material as well as preparation method and application thereof

    CN113060976A

  • Conductive and antistatic liquid and preparation method thereof

    CN113528009A

  • Miniature loudspeaker module and smart phone comprising same

    CN213846935U

  • Sound absorbing material and method for manufacturing the same, and method for improving sound absorbency

    JP2018146744A