Glass Articles with Improved Surface Quality
By protecting the second surface during the etching process and chemically strengthening the first surface, the method addresses the issue of compromised surface quality in UTG manufacturing, resulting in enhanced bending strength and impact resistance for asymmetric demands in foldable devices.
Patent Information
- Application Number
- JP2024532859
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-12-03
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-12-03
AI Technical Summary
Existing methods for manufacturing ultrathin glass (UTG) result in compromised surface quality due to the slimming process, which affects bending strength and impact resistance, particularly when asymmetric demands are required for foldable electronic devices like smartphones.
The method involves protecting the second surface of the glass article during the etching process to maintain low surface roughness and asymmetrical chamfered structures, while the first surface is optimized for high impact resistance through chemical strengthening.
This approach enhances the UTG's bending strength and impact resistance, ensuring improved performance in foldable electronic devices by maintaining high surface quality and optimizing asymmetric properties.
Smart Images

Figure 2024544001000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to glass articles having improved surface quality and to methods for making glass articles. [Background technology]
[0002] Ultra-thin glass (UTG) has great potential in a variety of applications, such as consumer electronics and optical devices. In particular, given its flexibility, UTG is advantageous for flexible displays, such as in smartphones.
[0003] It is technically challenging to manufacture UTGs at a range of ultra-thin target thicknesses. The conventional approach is to manufacture the glass article at a thicker thickness, especially by downdraw or overflow fusion methods, and then introduce a slimming process to reach the target thickness.
[0004] Due to its thin thickness and fragility, the most commonly applied processing method is stack processing. In stack processing, a stack assembly is formed, which includes a plurality of glass articles and at least one adhesive layer between two adjacent glass articles. Then, such a stack assembly is processed in several stack processing steps, such as cutting to a desired article size, grinding edges, and / or etching to obtain edge chamfer structures.
[0005] However, the above-mentioned slimming process to reach the target thickness is applied after delamination of the stack assembly. The reason is that for slimming to occur, the etching solution applied for slimming must contact the major surfaces of the glass articles. The major surfaces of the glass articles are protected from the etching solution by the adhesive layer that connects the articles to the adjacent articles in the stack assembly. Therefore, the stack assembly is first delaminated by removing the adhesive layer, and then the singulated glass articles are subjected to the slimming process in the etching solution to obtain the desired UTG articles.
[0006] A disadvantage of the slimming process is that it results in an impaired surface quality compared to the original surface quality of the glass article obtained by downdraw. The downdraw method results in a glass article in which both main surfaces are fire-polished. Fire-polished surfaces are characterized by a particularly low surface roughness. Furthermore, fire-polished surfaces are advantageous since they have a low number of surface defects. The surface quality of fire-polished surfaces is extremely good. Good surface quality is particularly advantageous for bending properties. Surface defects can result in a substantial reduction in bending strength. This is especially true for surface defects on the glass surface on the outer side of the bend, which is subjected to tensile stresses during bending.
[0007] There is a need for a UTG with improved flexural strength.
[0008] Furthermore, the UTG should meet other criteria in addition to its bendability. In particular, the UTG should withstand mechanical shocks that typically occur during use in, for example, electronic devices, such as smartphones. High impact resistance is advantageous.
[0009] Interestingly, especially in bendable electronic devices, such as smartphones, the requirements imposed on the UTG are often asymmetrical with respect to its two main surfaces. For example, the devices are generally arranged so that they can be folded, with the surface of the UTG facing the user being on the inside of the bend. This UTG surface therefore faces particularly high demands on its impact resistance, since it is directly exposed to various kinds of external impacts. On the other hand, the opposite UTG surface is on the outside of the bend, so it faces particularly high demands on bending strength due to the tensile stresses induced by the bend.
[0010] Thus, there is a need for a UTG that combines a first surface with particularly high impact resistance and a second surface with particularly high flexural strength.
[0011] A commonly used approach to further enhance the strength of UTG is the introduction of a chamfer structure at its edge. This is typically done during stack processing of the glass article using an etching solution. Since the etchant solution symmetrically accesses the edge of the article, this results in a symmetric chamfer structure that is not optimized with respect to the asymmetric strength requirements mentioned above. Summary of the Invention [Problem to be solved by the invention]
[0012] It is therefore an object of the present invention to overcome the problems of the prior art. In particular, it is an object of the present invention to provide an asymmetric UTG that is optimized for the asymmetric requirements in impact resistance and bending properties, for example in applications in smartphones and other electronic devices. It is also an object of the present invention to provide a method for manufacturing such a UTG. [Means for solving the problem]
[0013] The above problem is solved by the subject matter of the claims.
[0014] The present invention includes the idea of protecting the second surface of the glass article not only during the chamfer etching but also during the subsequent etching steps performed to slim the glass article to the desired thickness. This is advantageous in several ways. The surface roughness of the second surface can be kept low. Protecting the second surface of the glass article during slimming (but not the first surface of the glass article) results in an asymmetry of the chamfer structure that reflects the need for asymmetry suggested by the use of UTG in foldable electronics, e.g. smartphones. The high surface quality of the second surface makes it ideal to form the outer surface of the bend and to withstand the tensile stresses that arise there. In particular, the second surface can be provided with a high ball-on-ring breaking force and a high two-point bending strength.
[0015] On the other hand, the first surface of the UTG is very well suited to face the user of the electronic device, since it has a high impact resistance, especially when the UTG is chemically strengthened. This is unexpected. Without wishing to be bound by a particular theory, the high impact resistance of the first surface can be explained at least in part on the basis of its relatively high density. The first surface corresponds to the area of the glass article that was located in the interior of the article before the slimming process. Thus, a slower cooling rate occurs during manufacture, resulting in a higher density. The higher density is associated with a higher CS value achievable when chemically strengthening.
[0016] The glass articles of the present invention are very well suited for use in foldable electronic devices, particularly where a first surface of the glass article faces the outside of the device and thus requires high impact resistance, and a second surface of the glass article is the outer surface of the bend and thus requires high bending strength due to the tensile stresses that arise.
[0017] In a first aspect, the present invention provides a glass article having a thickness of 10 μm to 150 μm, a first surface, a second surface, and at least one edge connecting the first surface and the second surface; and The surface roughness R of the second surface a (arithmetic mean roughness) is up to 0.30 nm. Regarding the glass article.
[0018] In a second aspect, the present invention provides a glass article having a thickness of 10 μm to 150 μm, a first surface, a second surface, and at least one edge connecting the first surface and the second surface; the first surface and the second surface are essentially parallel to each other; The end has three surfaces: - a vertical surface that is essentially perpendicular to said first surface and to said second surface; - a first connecting surface connecting said vertical surface and said first surface; and a second connecting surface connecting said vertical surface and said second surface; A chamfered structure including The chamfer structure is - a tangent A to the first connecting surface is at a distance d from a tangent C to the normal surface 1 intersects with a tangent line B to the first surface at - the tangent D to the second connecting surface is at a distance d from the tangent C to the normal surface; 2 Intersects with tangent line E to the second surface at profile, where -d 1 and d 2 Both of and are measured perpendicular to a tangent C to said vertical surface, - the tangents A to E are obtained by fitting each tangent to the corresponding surface of the profile of the chamfer structure; The chamfer structure is d 1 ≠d 2 is asymmetric so that Regarding the glass article.
[0019] In a third aspect, the present invention provides a glass article having a thickness of 10 μm to 150 μm, a first surface, a second surface, and at least one edge connecting the first surface and the second surface; the first surface has an impact resistance corresponding to a pen drop height of at least 5 mm; and the second surface has a ball-on-ring breaking force of at least 5.0 N and / or a two-point bending strength of at least 2,000 MPa; Regarding the glass article.
[0020] In a fourth aspect, the present invention provides a method for producing a glass article having a first surface and a second surface, in particular a method for producing a glass article of the invention, comprising the following steps: a) providing a glass article; b) forming a stack assembly comprising a plurality of glass articles and at least one adhesive layer between two adjacent glass articles, wherein a first surface of the glass articles is in contact with a first adhesive layer comprising a first adhesive, and a second surface of the glass articles is in contact with a second adhesive layer comprising a second adhesive; c) contacting the stack assembly with a first etching solution; d) delaminating the stack assembly by removing the first adhesive layer, resulting in a sandwich assembly consisting of two glass articles and a second adhesive layer located between the two glass articles. e) contacting the sandwich assembly with a second etching solution; f) delaminating the sandwich assembly by removing the second adhesive layer; The present invention relates to the method comprising the steps of:
[0021] The present invention relates to a method for producing a plurality of glass articles having a first surface and a second surface, in particular a method for producing the glass articles of the present invention, comprising the steps of: a) providing a plurality of glass articles; b) forming a stack assembly including the plurality of glass articles and at least one adhesive layer between two adjacent glass articles, where a first surface of the glass articles contacts a first type of adhesive and a second surface of the glass articles contacts a second type of adhesive; c) contacting said stack assembly or a smaller stack assembly obtained therefrom with a first etching solution; d) delaminating the stack assembly or a smaller stack assembly resulting therefrom by removing the first type of adhesive, resulting in a sandwich assembly consisting of two glass articles and a second type of adhesive located between the two glass articles. e) contacting the sandwich assembly with a second etching solution; f) delaminating the sandwich assembly by removing the second type of adhesive; The present invention also relates to the method comprising the steps of:
[0022] The present invention also relates to a bendable device comprising a glass article of the present invention.
[0023] The present invention relates to a glass article having a thickness of 10 μm to 150 μm, comprising a first surface, a second surface, and at least one end connecting the first surface and the second surface, A) the surface roughness R of the second surface a (arithmetic mean roughness) is a maximum of 0.30 nm, B) the first surface and the second surface are essentially parallel to each other; The end has three surfaces: a vertical surface that is essentially perpendicular to said first surface and to said second surface; - a first connecting surface connecting said vertical surface and said first surface; and a second connecting surface connecting said vertical surface and said second surface; A chamfered structure including The chamfer structure is - a tangent A to the first connecting surface is at a distance d from a tangent C to the normal surface 1 intersects with a tangent line B to the first surface at - the tangent D to the second connecting surface is at a distance d from the tangent C to the normal surface; 2 intersects with a tangent line E to the second surface at profile, where -d 1 and d 2 Both of and are measured perpendicular to a tangent C to said vertical surface, - the tangents A to E are obtained by fitting each tangent to the corresponding surface of the profile of the chamfer structure; The chamfer structure is d 1 ≠d 2 and / or C) the first surface has an impact resistance corresponding to a pen drop height of at least 5 mm, and the second surface has a ball-on-ring breaking force of at least 5.0 N and / or a two-point bending strength of at least 2,000 MPa. The present invention relates to the glass article,
[0024] In some embodiments, the present invention provides a glass article having a thickness of 10 μm to 150 μm, comprising a first surface, a second surface, and at least one edge connecting the first surface and the second surface; A) the surface roughness R of the second surface a (arithmetic mean roughness) is a maximum of 0.30 nm, and B) the first surface and the second surface are essentially parallel to each other; The end has three surfaces: a vertical surface that is essentially perpendicular to said first surface and to said second surface; - a first connecting surface connecting said vertical surface and said first surface; and a second connecting surface connecting said vertical surface and said second surface; A chamfered structure including The chamfer structure is - a tangent A to the first connecting surface is at a distance d from a tangent C to the normal surface 1 intersects with a tangent line B to the first surface at - the tangent D to the second connecting surface is at a distance d from the tangent C to the normal surface; 2 Intersects with tangent line E to the second surface at profile, where -d 1 and d 2 Both of and are measured perpendicular to a tangent C to said vertical surface, - the tangents A to E are obtained by fitting each tangent to the corresponding surface of the profile of the chamfer structure; The chamfer structure is d 1 ≠d 2 Asymmetric as The present invention relates to the glass article,
[0025] In some embodiments, the present invention provides a glass article having a thickness of 10 μm to 150 μm, comprising a first surface, a second surface, and at least one edge connecting the first surface and the second surface; A) the surface roughness R of the second surface a (arithmetic mean roughness) is a maximum of 0.30 nm, and B) the first surface has an impact resistance corresponding to a pen drop height of at least 5 mm, and the second surface has a ball-on-ring breaking force of at least 5.0 N and / or a two-point bending strength of at least 2,000 MPa. The present invention relates to the glass article,
[0026] In some embodiments, the present invention provides a glass article having a thickness of 10 μm to 150 μm, comprising a first surface, a second surface, and at least one edge connecting the first surface and the second surface; A) the first surface and the second surface are essentially parallel to each other; The end has three surfaces: a vertical surface that is essentially perpendicular to said first surface and to said second surface; - a first connecting surface connecting said vertical surface and said first surface; and a second connecting surface connecting said vertical surface and said second surface; A chamfered structure including The chamfer structure is - a tangent A to the first connecting surface is at a distance d from a tangent C to the normal surface 1 intersects with a tangent line B to the first surface at - the tangent D to the second connecting surface is at a distance d from the tangent C to the normal surface; 2 intersects with a tangent line E to the second surface at profile, where -d 1 and d 2 Both of and are measured perpendicular to a tangent C to said vertical surface, - the tangents A to E are obtained by fitting each tangent to the corresponding surface of the profile of the chamfer structure; The chamfer structure is d 1 ≠d 2 and B) the first surface has an impact resistance corresponding to a pen drop height of at least 5 mm, and the second surface has a ball-on-ring breaking force of at least 5.0 N and / or a two-point bending strength of at least 2,000 MPa. The present invention relates to the glass article,
[0027] In some embodiments, the present invention provides a glass article having a thickness of 10 μm to 150 μm, comprising a first surface, a second surface, and at least one edge connecting the first surface and the second surface; A) the surface roughness R of the second surface a (arithmetic mean roughness) is a maximum of 0.30 nm, B) the first surface and the second surface are essentially parallel to each other; The end has three surfaces: a vertical surface that is essentially perpendicular to said first surface and to said second surface; - a first connecting surface connecting said vertical surface and said first surface; and a second connecting surface connecting said vertical surface and said second surface; A chamfered structure including The chamfer structure is - a tangent A to the first connecting surface is at a distance d from a tangent C to the normal surface 1intersects with a tangent line B to the first surface at - the tangent D to the second connecting surface is at a distance d from the tangent C to the normal surface; 2 intersects with a tangent line E to the second surface at profile, where -d 1 and d 2 Both of and are measured perpendicular to a tangent C to said vertical surface, - the tangents A to E are obtained by fitting each tangent to the corresponding surface of the profile of the chamfer structure; The chamfer structure is d 1 ≠d 2 and C) the first surface has an impact resistance corresponding to a pen drop height of at least 5 mm, and the second surface has a ball-on-ring breaking force of at least 5.0 N and / or a two-point bending strength of at least 2,000 MPa. The present invention relates to the glass article,
[0028] The glass article of the present invention can be, for example, a sheet or sheet-like article, in particular a round-shaped article, or a rectangular or square article having a length and a width. Both the length and width of the glass article are preferably much longer than the thickness of the article. For example, the length and / or width can be at least 1 mm, at least 2 mm, at least 5 mm, at least 10 mm, at least 15 mm, at least 20 mm, at least 25 mm, at least 30 mm, at least 40 mm, or at least 50 mm. For example, the length and / or width can be up to 500 mm, up to 400 mm, up to 300 mm, up to 200 mm, up to 150 mm, up to 125 mm, up to 100 mm, or up to 70 mm. The ratio of length to width can be 1:1 or more. In some embodiments, the glass article can have a notch for a front camera, particularly in smartphone applications, and / or a hole or recess for a camera and / or a microphone or speaker.
[0029] In one embodiment of the invention, the glass article may have a length in the range of 10 mm to 500 mm, and / or a width in the range of 5 mm to 400 mm, such as a length and / or width in the range of 10 to 400 mm, 15 to 300 mm, 20 to 200 mm, 25 to 150 mm, 30 to 125 mm, 40 to 100 mm, or 50 to 70 mm. The length and / or width may be, for example, at least 5 mm, at least 10 mm, at least 15 mm, at least 20 mm, at least 25 mm, at least 30 mm, at least 40 mm, or at least 50 mm. The length and / or width may be, for example, up to 500 mm, up to 400 mm, up to 300 mm, up to 200 mm, up to 150 mm, up to 125 mm, up to 100 mm, or up to 70 mm.
[0030] Preferably, the article has exactly one edge connecting its first surface and its second surface. Depending on the shape of the article, the edge may have different sides. For example, in the case of a sheet or sheet-like article having a rectangular or square shape, the edge has four sides, where two opposite sides represent the length of the article and the remaining two opposite sides represent the width of the article. The location of the connection of two adjacent sides of the edge is generally called a corner.
[0031] The glass article of the present invention has a thickness of 10 μm to 150 μm, for example 15 μm to 120 μm, 20 μm to 100 μm, 25 μm to 90 μm, 30 μm to 80 μm, 35 μm to 70 μm, 40 μm to 60 μm, or 45 μm to 50 μm. The thickness of the glass article may be, for example, at least 10 μm, at least 15 μm, at least 20 μm, at least 25 μm, at least 30 μm, at least 35 μm, at least 40 μm, or at least 45 μm. The thickness of the glass article may be, for example, up to 150 μm, up to 120 μm, up to 100 μm, up to 90 μm, up to 80 μm, up to 70 μm, up to 60 μm, or up to 50 μm.
[0032] Average roughness (R a) is a measure of surface texture. It is quantified by the vertical deviation of the actual surface from the ideal morphology. Conventionally, the amplitude parameter characterizes a surface based on the vertical deviation from the mean line of the roughness profile. R a is the arithmetic mean of the absolute values of those vertical deviations, which may be specified in accordance with DIN EN ISO 4287:2010-07.
[0033] Surface Roughness R a is preferably determined using an atomic force microscope (AFM), in particular using the Dimension Icon model from BRUKER. The test area is preferably 2×2 μm 2 or more, or 10×10μm 2 That's all.
[0034] Preferably, the surface roughness R of the second surface a is especially 2×2μm 2 or 10×10 μm 2 For an area of 0.30 nm, more preferably 0.25 nm, more preferably 0.20 nm, more preferably 0.15 nm. a is especially 2×2μm 2 or 10×10 μm 2 For example, the surface roughness R of the second surface may be at least 0.05 nm, at least 0.08 nm, at least 0.10 nm, or at least 0.12 nm. a is especially 2×2μm 2 or 10×10 μm 2 The area may be in the range of, for example, 0.05 to 0.30 nm, 0.08 to 0.25 nm, 0.10 to 0.20 nm, or 0.12 to 0.15 nm.
[0035] Surface roughness R of the first surface a is especially 2×2μm 2 or 10×10 μm 2For example, the surface roughness R of the first surface may be at most 0.80 nm, at most 0.70 nm, at most 0.60 nm, at most 0.50 nm, at most 0.40 nm, at most 0.30 nm, or at most 0.20 nm. a is especially 2×2μm 2 or 10×10 μm 2 For example, the surface roughness R of the first surface may be at least 0.10 nm, at least 0.11 nm, at least 0.12 nm, at least 0.13 nm, at least 0.14 nm, at least 0.15 nm, or at least 0.16 nm. a is especially 2×2μm 2 or 10×10 μm 2 The area may be in the range of, for example, 0.10 to 0.80 nm, 0.11 to 0.70 nm, 0.12 to 0.60 nm, 0.13 to 0.50 nm, 0.14 to 0.40 nm, 0.15 to 0.30 nm, or 0.16 to 0.20 nm.
[0036] Surface roughness R of the first surface a is the surface roughness R of the second surface a For example, the surface roughness R of the first surface may be higher than a and the surface roughness R of the second surface a The absolute value of the difference is especially 2×2μm 2 or 10×10 μm 2 For the first and second surfaces of an area of at least 0.05 nm, at least 0.10 nm, at least 0.15 nm, or at least 0.20 nm. a and the surface roughness R of the second surface a The absolute value of the difference is especially 2×2μm 2 or 10×10 μm 2 For the first and second surfaces of an area of 0.50 nm, 0.40 nm, 0.30 nm, or 0.25 nm, for example, the surface roughness R of the first surface. a and the surface roughness R of the second surface a The absolute value of the difference is especially 2×2μm 2 or 10×10 μm 2The areas of the first surface and the second surface may be in the range of, for example, 0.05 to 0.50 nm, 0.10 to 0.40 nm, 0.15 to 0.30 nm, or 0.20 to 0.25 nm.
[0037] As mentioned above, the glass article of the present invention may also feature an asymmetric chamfer structure. A cross-sectional profile of a glass article having an asymmetric chamfer structure is shown in FIG. 2. The asymmetry can be best observed and explained based on a cross-sectional image of the profile of the chamfer structure shown in FIG. 3. To obtain such an image, the glass article is observed in transmitted light mode using an optical microscope. A magnification of 200x is used. The focus is on the top surface, so the edges appear very sharp. The glass article is positioned so that the top surface is not tilted. Thus, the top surface is perpendicular to the direction of the light. Particularly good quality images are generally obtained using an auto white balance, auto brightness and auto contrast, especially a Nikon Y-TV55 microscope.
[0038] As shown in FIG. 3, the asymmetry of the chamfer structure can be easily accounted for by fitting the tangents to the relevant surfaces in the microscope image (tangent A to the first connecting surface, tangent B to the first surface, tangent C to the normal surface, tangent D to the second connecting surface, and tangent E to the second surface).
[0039] Fitting the tangents to the respective surfaces can be done manually using any suitable image processing software, such as ImageJ, Power Point, Photoshop, etc. It is understood that the skilled person is familiar with further suitable software programs. Fitting the lines can be easily done manually. Without much effort, a sufficiently accurate fit can be obtained. However, if desired, the best fit can be obtained, especially with the support of further software, for example by fitting using the least squares method.
[0040] In particular, as also shown in FIG. 3, the transition of one surface to the other surface cannot always be specified at one specific point. In particular, the second connecting surface, and even more notably the first connecting surface, may deviate from a straight line towards the transition to the second surface or the first surface, respectively. However, this deviation concerns only a small part of the first connecting surface and the second connecting surface. Thus, in order to obtain a tangent to the first connecting surface with as little deviation of the tangent from the first connecting surface as possible, the tangent is fitted so that a best fit is obtained towards the transition of the first connecting surface to the vertical surface, while a larger deviation is acceptable towards the transition of the first connecting surface to the first surface. The same applies analogously to the fitting of the tangent to the second connecting surface.
[0041] As shown in FIG. 3, the tangent A to the first connecting surface is a distance d from the tangent C to the normal surface. 1 Similarly, the tangent line D to the second connecting surface is a distance d from the tangent line C to the normal surface. 2 At d, it intersects with the tangent line E to the second surface. 1 and d 2 Both and are measured perpendicular to the tangent C to the vertical surface. 1 and d 2 The length of the distance d can be measured using any suitable image processing software, such as ImageJ, Powerpoint, Photoshop, etc. 1 and d 2 respectively to the length of the scale bar.
[0042] In the asymmetric chamfer structure, d 1 d 2 In particular, d 1 d 2 Bigger is better.
[0043] d 1 -d 2The absolute value of the difference may be, for example, at least 30%, at least 40%, at least 50%, at least 60%, at least 70%, at least 80%, or at least 90% of the thickness of the glass article. 1 -d 2 The absolute value of the difference may be, for example, up to 200%, up to 180%, up to 160%, up to 140%, up to 120%, up to 110%, or up to 100% of the thickness of the glass article. 1 -d 2 The absolute value of the difference may be in the range of, for example, 30% to 200%, 40% to 180%, 50% to 160%, 60% to 140%, 70% to 120%, 80% to 110%, or 90% to 100% of the thickness of the glass article.
[0044] d 1 -d 2 The absolute value of the difference may be, for example, at least 15 μm, at least 20 μm, at least 25 μm, at least 30 μm, at least 35 μm, or at least 40 μm. 1 -d 2 The absolute value of the difference may be, for example, at most 100 μm, at most 90 μm, at most 80 μm, at most 70 μm, at most 60 μm, or at most 50 μm. 1 -d 2 The absolute value of the difference may be in the range of, for example, 15 to 100 μm, 20 to 90 μm, 25 to 80 μm, 30 to 70 μm, 35 to 60 μm, or 40 to 50 μm.
[0045] Distance d 1 may be, for example, at least 50 μm, at least 60 μm, at least 70 μm, at least 80 μm, or at least 90 μm. 1 may be, for example, at most 200 μm, at most 175 μm, at most 150 μm, at most 125 μm, or at most 100 μm. 1 For example, it may be in the range of 50 to 200 μm, 60 to 175 μm, 70 to 150 μm, 80 to 125 μm, or 90 to 100 μm.
[0046] Distance d 2may be, for example, at least 30 μm, at least 35 μm, at least 40 μm, at least 45 μm, or at least 50 μm. 2 may be, for example, at most 100 μm, at most 90 μm, at most 80 μm, at most 70 μm, or at most 60 μm. 2 For example, it may be in the range of 30 to 100 μm, 35 to 90 μm, 40 to 80 μm, 45 to 70 μm, or 50 to 60 μm.
[0047] The present invention relates to a glass article that is asymmetric in terms of the surface roughness of the first and second surfaces, in terms of chamfer structure, and / or in terms of the impact and bending properties of the first and second surfaces.In particular, the glass article of the present invention can have a first surface that has very good impact resistance and a second surface that has very good bending strength.This is particularly advantageous for using the glass article in bendable devices, such as smartphones, where the first surface faces various external impacts and the second surface is the outer surface of the glass article in a bending state.
[0048] The measure for impact resistance is the pen drop height. The higher the pen drop height, the higher the impact resistance. The pen drop height is the breaking height specified in the pen drop test, in which the glass article is attached to one surface of a 150 μm thick substrate, which consists of, from the side contacting the glass to the side contacting the marble stage, a 25 μm thick layer of pressure sensitive adhesive (PSA) material, a 50 μm thick layer of polyethylene (PE), another 25 μm thick layer of pressure sensitive adhesive (PSA), and another 50 μm thick layer of polyethylene (PE). Under the 150 μm thick substrate is a flat 10 cm thick marble stage with a polished smooth surface. Subsequently, the other surface of the glass article facing upwards (i.e., the surface on which the pen drop height is actually tested) is impacted with a 14 g ballpoint pen (manufactured by Chenguang) with a ball diameter of 0.5 mm made of tungsten carbide, from 5 mm increasing heights until the glass breaks. The breaking height is then recorded as the pen drop height.
[0049] The first surface of the glass article may have an impact resistance corresponding to a pen drop height of at least 5 mm, at least 10 mm, at least 15 mm, at least 20 mm, at least 25 mm, at least 30 mm, at least 35 mm, at least 40 mm, at least 45 mm, at least 50 mm, at least 75 mm, at least 100 mm, at least 150 mm, at least 200 mm, at least 300 mm, at least 400 mm, or at least 500 mm. The first surface of the glass article may have an impact resistance corresponding to a pen drop height of up to 10,000 mm, up to 5,000 mm, up to 4,000 mm, up to 3,000 mm, up to 2,000 mm, up to 1,500 mm, or up to 1,000 mm. In some embodiments, the first surface of the glass article may have an impact resistance corresponding to a pen drop height of up to 500 mm, up to 450 mm, up to 400 mm, up to 350 mm, up to 300 mm, up to 250 mm, up to 200 mm, up to 150 mm, up to 100, or up to 75 mm. The first surface of the glass article may have an impact resistance corresponding to a pen drop height in the range of 5 to 500 mm, 10 to 450 mm, 15 to 400 mm, 20 to 350 mm, 25 to 300 mm, 30 to 250 mm, 35 to 200 mm, 40 to 150 mm, 45 to 100 mm, or 50 to 75 mm. In other embodiments, the first surface of the glass article may have an impact resistance corresponding to a pen drop height in the range of 75 to 10,000 mm, 100 to 5,000 mm, 150 to 4,000 mm, 200 to 3,000 mm, 300 to 2,000 mm, 400 to 1,500 mm, or 500 to 1,000 mm.
[0050] It is also possible to normalize the pen drop height to the thickness of the glass article. Normalized pen drop height is the ratio of the pen drop height (μm) to the square of the thickness of the article (μm 2 For example, if a particular glass article has a pen drop height of 10 mm (=10,000 μm) and the thickness of the article is 50 μm, the normalized pen drop height is 50 times 10,000 μm. 2 μm 2which gives a value of 4.0 per μm for the normalized pen drop height.
[0051] The first surface of the glass article may have an impact resistance corresponding to a normalized pen drop height of at least 4.5 per μm, at least 5.0 per μm, at least 5.5 per μm, at least 6.0 per μm, at least 6.5 per μm, at least 7.0 per μm, at least 7.5 per μm, at least 8.0 per μm, at least 8.5 per μm, at least 9.0 per μm, at least 9.5 per μm, at least 10.0 per μm, or at least 10.5 per μm. The first surface of the glass article may have an impact resistance corresponding to a normalized pen drop height of up to 60.0 per μm, up to 50.0 per μm, up to 45.0 per μm, up to 40.0 per μm, up to 35.0 per μm, up to 30.0 per μm, up to 25.0 per μm, up to 20.0 per μm, up to 18.0 per μm, up to 16.0 per μm, up to 14.0 per μm, up to 12.0 per μm, or up to 11.0 per μm. The first surface of the glass article may have an impact resistance corresponding to a normalized pen drop height in the range of 4.5 to 60.0 per micron, 5.0 to 50.0 per micron, 5.5 to 45.0 per micron, 6.0 to 40.0 per micron, 6.5 to 35.0 per micron, 7.0 to 30.0 per micron, 7.5 to 25.0 per micron, 8.0 to 20.0 per micron, 8.5 to 18.0 per micron, 9.0 to 16.0 per micron, 9.5 to 14.0 per micron, 10.0 to 12.0 per micron, or 10.5 to 11.0 per micron.
[0052] The second surface of the glass article may have an impact resistance corresponding to a normalized pen drop height of at least 2.0 per μm, at least 2.5 per μm, at least 3.0 per μm, at least 3.5 per μm, at least 4.0 per μm, at least 4.5 per μm, at least 5.0 per μm, at least 5.5 per μm, at least 6.0 per μm, at least 6.5 per μm, at least 7.0 per μm, at least 7.5 per μm, or at least 8.0 per μm. The second surface of the glass article may have an impact resistance corresponding to a normalized pen drop height of up to 50.0 per μm, up to 45.0 per μm, up to 40.0 per μm, up to 35.0 per μm, up to 30.0 per μm, up to 25.0 per μm, up to 20.0 per μm, up to 18.0 per μm, up to 16.0 per μm, up to 14.0 per μm, up to 12.0 per μm, up to 10.0 per μm, or up to 9.0 per μm. The second surface of the glass article may have an impact resistance corresponding to a normalized pen drop height in the range of 2.0 to 50.0 per micron, 2.5 to 45.0 per micron, 3.0 to 40.0 per micron, 3.5 to 35.0 per micron, 4.0 to 30.0 per micron, 4.5 to 25.0 per micron, 5.0 to 20.0 per micron, 5.5 to 18.0 per micron, 6.0 to 16.0 per micron, 6.5 to 14.0 per micron, 7.0 to 12.0 per micron, 7.5 to 10.0 per micron, or 8.0 to 9.0 per micron.
[0053] As mentioned above, the pen drop height of the first surface of the glass article is particularly high. In particular, the pen drop height of the first surface of the glass article can be higher than the pen drop height of the second surface of the glass article. The ratio of the pen drop height of the first surface to the pen drop height of the second surface can be, for example, at least 1.05, at least 1.10, at least 1.15, at least 1.20, at least 1.25, at least 1.30, at least 1.35, or at least 1.40. The ratio of the pen drop height of the first surface to the pen drop height of the second surface can be, for example, at most 2.50, at most 2.25, at most 2.00, at most 1.90, at most 1.80, at most 1.70, at most 1.60, or at most 1.50. The ratio of the pen drop height of the first surface to the pen drop height of the second surface may be in the range of, for example, 1.05 to 2.50, 1.10 to 2.25, 1.15 to 2.00, 1.20 to 1.90, 1.25 to 1.80, 1.30 to 1.70, 1.35 to 1.60, or 1.40 to 1.50.
[0054] The second surface of the glass article may be particularly suitable to withstand tensile stresses that arise on the second surface when the glass article is bent such that the second surface is the outer surface of the bend. This is reflected by the second surface having a particularly high ball-on-ring breaking strength and / or two-point bend strength. In particular, the ball-on-ring breaking strength and / or two-point bend strength of the second surface of the glass article may be high compared to the ball-on-ring breaking strength and / or two-point bend strength, respectively, of the first surface.
[0055] As depicted diagrammatically in FIG. 4, the ball-on-ring breaking force can be tested by placing a surface 45 of a glass article 41 on a steel ring 42, the ring 42 having an inner diameter of 4 mm and an outer diameter of 6 mm. The ring 42 is 3 mm deep, the walls of the ring 42 are 1 mm thick, with the tip of the wall having a semicircle with a diameter of 1 mm as a cross section. To test the ball-on-ring breaking force, the edge of the glass article 41 is at least 20 mm away from the center of the ring 42. A tungsten carbide ball 43 having a diameter of 1 mm is pressed against the surface 44 of the glass article 41 along the central axis of the ring 42 at a rate of 5 mm / min until the glass closes. The force at break is recorded as the ball-on-ring breaking force.
[0056] Depending on which surface of the glass article 41 is in contact with the ring 42 or the ball 43, respectively, the ball-on-ring breaking force of the first surface or the second surface of the glass article 41 can be tested. The ball-on-ring test described herein is tailored to identify the ball-on-ring breaking force of a particular surface of the glass article 41 in contact with the steel ring 42. For example, if the first surface of the glass article 41 is the surface 44 in contact with the ball 43 while the second surface of the glass article 41 is the surface 45 in contact with the steel ring 42, the product of the ball-on-ring test is the ball-on-ring breaking force of the second surface. However, if the first surface of the glass article 41 is the surface 45 in contact with the steel ring 42 while the second surface of the glass article 41 is the surface 44 in contact with the ball 43, the product of the ball-on-ring test is the ball-on-ring breaking force of the first surface. It is the surface 45 of the glass article 41 where tensile stress is developed during the ball-on-ring test. Thus, the product of the ball-on-ring test is the ball-on-ring breaking force of surface 45.
[0057] The second surface of the glass article may have a ball-on-ring breaking force of at least 5.0 N, at least 7.5 N, at least 10.0 N, at least 12.5 N, at least 15.0 N, or at least 17.5 N. The second surface of the glass article may have a ball-on-ring breaking force of up to 50.0 N, up to 40.0 N, up to 30.0 N, up to 25.0 N, up to 22.5 N, or up to 20.0 N. The second surface of the glass article may have a ball-on-ring breaking force in the range of 5.0-50.0 N, 7.5-40.0 N, 10.0-30.0 N, 12.5-25.0 N, 15.0-22.5 N, or 17.5-20.0 N.
[0058] The first surface of the glass article may have a ball-on-ring breaking force of at least 1.0 N, at least 2.0 N, at least 5.0 N, at least 7.5 N, at least 10.0 N, or at least 12.5 N. The second surface of the glass article may have a ball-on-ring breaking force of up to 30.0 N, up to 25.0 N, up to 22.5 N, up to 20.0 N, up to 17.5 N, or up to 15.0 N. The second surface of the glass article may have a ball-on-ring breaking force in the range of 1.0-30.0 N, 2.0-25.0 N, 5.0-22.5 N, 7.5-20.0 N, 10.0-17.5 N, or 12.5-15.0 N.
[0059] As mentioned above, the ball-on-ring breaking force of the second surface of the glass article is particularly high. In particular, the ball-on-ring breaking force of the second surface of the glass article can be high compared to the ball-on-ring breaking force of the first surface of the glass article. The ratio of the ball-on-ring breaking force of the second surface to the ball-on-ring breaking force of the first surface can be, for example, at least 1.05, at least 1.10, at least 1.15, at least 1.20, or at least 1.25. The ratio of the ball-on-ring breaking force of the second surface to the ball-on-ring breaking force of the first surface can be, for example, at most 2.00, at most 1.75, at most 1.50, at most 1.40, or at most 1.30. The ratio of the ball-on-ring breaking force of the second surface to the ball-on-ring breaking force of the first surface may be in the range of, for example, 1.05 to 2.00, 1.10 to 1.75, 1.15 to 1.50, 1.20 to 1.40, or 1.25 to 1.30.
[0060] The particularly good bendability of the glass article of the invention is also reflected by a particularly high two-point bending strength (2PB strength) of the second surface. To test the 2PB strength, the glass article is placed in a U-shape between two parallel metal plates. The two plates are large enough to cover the entire glass article. One of the plates is then moved towards the other one, remaining parallel, at a speed of 60 mm / min until the glass article breaks. The 2PB strength is σ = 1.198Ed / (Dd) where σ is the calculated 2PB strength, E is the Young's modulus of the glass, d is the thickness of the glass article, and D is the distance between the two plates at break.
[0061] The product of the 2PB test is the 2PB strength of the surface of the glass article that is the outer surface of the bend. For example, if a glass article is bent such that a first surface of the glass article is the inner surface of the bend while a second surface of the glass article is the outer surface of the bend, the product of the 2PB test is the 2PB strength of the second surface of the glass article.
[0062] The second surface of the glass article may have a 2PB strength of, for example, at least 1500 MPa, at least 1750 MPa, at least 2000 MPa, at least 2250 MPa, at least 2500 MPa, at least 2750 MPa, or at least 3000 MPa. The second surface of the glass article may have a 2PB strength of, for example, up to 10,000 MPa, up to 7500 MPa, up to 6000 MPa, up to 5000 MPa, up to 4500 MPa, up to 4000 MPa, or up to 3500 MPa. The second surface of the glass article may have a 2PB strength in the range of, for example, 1500-10,000 MPa, 1750-7500 MPa, 2000-6000 MPa, 2250-5000 MPa, 2500-4500 MPa, 2750-4000 MPa, or 3000-3500 MPa.
[0063] The first surface of the glass article may have a 2PB strength of, for example, at least 1000 MPa, at least 1250 MPa, at least 1500 MPa, at least 1750 MPa, at least 2000 MPa, at least 2250 MPa, or at least 2500 MPa. The first surface of the glass article may have a 2PB strength of, for example, up to 7500 MPa, up to 5000 MPa, up to 4500 MPa, up to 4000 MPa, up to 3500 MPa, up to 3000 MPa, or up to 2750 MPa. The first surface of the glass article may have a 2PB strength in the range of, for example, 1000-7500 MPa, 1250-5000 MPa, 1500-4500 MPa, 1750-4000 MPa, 2000-3500 MPa, 2250-3000 MPa, or 2500-2750 MPa.
[0064] As mentioned above, the 2PB strength of the second surface of the glass article is particularly high. In particular, the 2PB strength of the second surface of the glass article may be higher than the 2PB strength of the first surface of the glass article. The ratio of the 2PB strength of the second surface to the 2PB strength of the first surface may be, for example, at least 1.05, at least 1.10, at least 1.15, at least 1.20, or at least 1.25. The ratio of the 2PB strength of the second surface to the 2PB strength of the first surface may be, for example, at most 2.00, at most 1.75, at most 1.50, at most 1.40, or at most 1.30. The ratio of the 2PB strength of the second surface to the 2PB strength of the first surface may be, for example, in the range of 1.05 to 2.00, 1.10 to 1.75, 1.15 to 1.50, 1.20 to 1.40, or 1.25 to 1.30.
[0065] The glass articles of the present invention may be chemically strengthened, in particular by subjecting the article to an ion exchange treatment.
[0066] Compressive stress (CS) (also called "compressive stress" or "surface stress") is the stress resulting from the action of substitution on the glass network through the glass surface after ion exchange, while no deformation occurs in the glass.
[0067] The "penetration depth" or "depth of the ion-exchange layer" or "ion-exchange depth" ("depth of layer" or "depth of ion-exchange layer", DoL) is the thickness of the glass surface layer where ion exchange occurs and compressive stresses develop. The compressive stress CS and the penetration depth DoL can be measured optically (in particular by a waveguide mechanism) using a commercially available stress meter FSM6000 (e.g. Luceo Co., Ltd., Tokyo, Japan).
[0068] When CS is induced on one or both sides of a glass sheet, to balance the stresses according to the third principle of Newton's law, a tensile stress must be induced in the central region of the glass, which is called the internal tensile stress (CT). CT can be calculated from the measured CS and DoL values.
[0069] Ion exchange means that glass is hardened or chemically strengthened by an ion exchange process (also called chemical strengthening), and the method is well known to those skilled in the art of glass manufacturing and processing. The strengthening process can be carried out by immersing the glass layer in a salt bath containing monovalent ions to exchange with the alkali ions inside the glass. The monovalent ions in the salt bath have a larger radius than the alkali ions inside the glass. Compressive stress on the glass is formed after ion exchange due to the larger ions breaking into the glass network. After ion exchange, the strength and flexibility of the glass are significantly improved. Furthermore, the CS induced by chemical strengthening improves the bending properties of the strengthened glass layer and increases the scratch resistance of the glass layer. Typical salts used for chemical strengthening are, for example, K. + The optional salt bath for chemical strengthening is a molten salt or salt mixture containing Na + Contains and / or K + The optional salt is a molten salt bath containing NaNO 3 , KNO 3 , NaCl, KCl, Na 2 SO 4 , K 2 SO 4 , Na 2 CO 3 , K 2 CO 3 and K. 2 S 2 O 5 Additives such as NaOH, KOH and other sodium or potassium salts are also used to better control the rate of ion exchange for chemical strengthening. The ion exchange is carried out with, for example, KNO 3 The chemical strengthening may be carried out at temperatures ranging from 300°C to 480°C, in particular from 340°C to 450°C, or from 390°C to 450°C, for example for a time period of 30 minutes to 48 hours, in particular about 20 minutes. The chemical strengthening is not limited to one stage. It may involve multiple stages in one or more salt baths with various concentrations of alkali metal ions to achieve better strengthening performance. Thus, the glass layer to be chemically strengthened may be strengthened in one stage, or in multiple stages, for example in a two-stage process. Two-stage chemical strengthening is especially preferred in the case of Li 2This applies to O-containing glasses because lithium can be exchanged for both sodium and potassium ions.
[0070] The chemically strengthened glass article of the present invention may have a surface compressive stress CS1 at a first surface and a surface compressive stress CS2 at a second surface.
[0071] CS1 and / or CS2 may for example be at least 300 MPa, at least 350 MPa, at least 400 MPa, at least 450 MPa, at least 500 MPa, at least 550 MPa, or at least 600 MPa. CS1 and / or CS2 may for example be up to 1000 MPa, up to 900 MPa, up to 850 MPa, up to 800 MPa, up to 750 MPa, up to 700 MPa, or up to 650 MPa. CS1 and / or CS2 may for example be in the range 300-1000 MPa, 350-900 MPa, 400-850 MPa, 450-800 MPa, 500-750 MPa, 550-700 MPa, or 600-650 MPa.
[0072] In some embodiments, CS1 and / or CS2 may be less than 600 MPa, such as up to 550 MPa, up to 500 MPa, or up to 475 MPa. CS1 and / or CS2 may be in the range of, for example, 300-600 MPa, 350-550 MPa, 400-500 MPa, or 450-475 MPa.
[0073] The surface compressive stress CS1 at the first surface can be higher than the surface compressive stress CS2 at the second surface. The first surface corresponds to a region of the glass article that was located in the interior of the article before the slimming process. Thus, a slower cooling rate occurs during manufacture, resulting in a higher density. The higher density is associated with a higher CS value achievable at the first surface of the glass article when chemically strengthened.
[0074] The absolute value of the CS1-CS2 difference may for example be at least 10 MPa, at least 15 MPa, at least 20 MPa, at least 30 MPa, or at least 50 MPa. The absolute value of the CS1-CS2 difference may for example be up to 100 MPa, up to 90 MPa, up to 80 MPa, up to 70 MPa, or up to 60 MPa. The absolute value of the CS1-CS2 difference may for example be in the range of 10-100 MPa, 15-90 MPa, 20-80 MPa, 30-70 MPa, or 50-60 MPa.
[0075] A chemically strengthened glass article of the present invention may have a first compressive stress layer extending from a first surface of the glass article to a first depth of layer DoL1, and a second compressive stress layer extending from a second surface to a second depth of layer DoL2.
[0076] DoL1 and / or DoL2 may be, for example, at least 2.5 μm, at least 5.0 μm, at least 7.5 μm, or at least 10.0 μm. DoL1 and / or DoL2 may be, for example, up to 20.0 μm, up to 17.5 μm, up to 15.0 μm, or up to 12.5 μm. DoL1 and / or DoL2 may be, for example, in the range of 2.5 to 20.0 μm, 5.0 to 17.5 μm, 7.5 to 15.0 μm, or 10.0 to 12.5 μm.
[0077] DoL1 and / or DoL2 may be adapted to the thickness of the glass article. For example, DoL1 and / or DoL2 may be at least 5.0%, at least 7.5%, at least 10.0%, at least 12.5%, at least 15.0%, or at least 17.5% of the thickness of the glass article. DoL1 and / or DoL2 may be, for example, up to 40.0%, up to 35.0%, up to 30.0%, up to 27.5%, up to 25.0%, or up to 22.5% of the thickness of the glass article. DoL1 and / or DoL2 may be, for example, in the range of 5.0% to 40.0%, 7.5% to 35.0%, 10.0% to 30.0%, 12.5% to 27.5%, 15.0% to 25.0%, or 17.5% to 22.5% of the thickness of the glass article.
[0078] DoL2 can be higher than DoL1. As mentioned above, a slower cooling rate occurs during manufacture at the first surface of the glass article, resulting in a higher density. The higher density at the first surface can be associated with a lower depth of layer DoL1 of the compressive stress layer extending from the first surface toward the center of the glass article compared to a depth of layer DoL2 of the compressive stress layer extending from the second surface of the glass article toward its center. The ratio of DoL2 / DoL1 can be greater than 1.00, for example at least 1.01, at least 1.02, at least 1.03, or at least 1.04. The ratio of DoL2 / DoL1 can be, for example, at most 1.20, at most 1.15, at most 1.10, at most 1.07, or at most 1.05. The ratio of DoL2 / DoL1 may be, for example, in the range of >1.00-1.20, 1.01-1.15, 1.02-1.10, 1.03-1.07, or 1.04-1.05.
[0079] The difference between DoL1 and DoL2 may be associated with a glass article having a certain warpage. In particular, the glass article may have a warpage such that the first surface of the glass article is convex and the second surface of the glass article is concave. Without wishing to be bound by a particular theory, this may be at least partially explained by the larger layer depth DoL2 of the compressive stress layer extending from the second surface towards the center of the glass article not being fully balanced by the smaller layer depth DoL1 of the compressive stress layer extending from the first surface towards the center of the glass article. As a result, the second surface may be "pushed" towards the center of the glass article (resulting in a concave second surface) while the first surface is "pushed" outwards (resulting in a convex first surface). In general, it is well-established in the art that warpage should be avoided. However, in the present case, it has been found that a certain warpage is even advantageous for the bendability of the article. In particular, as mentioned above, the first surface of the glass article of the present invention is particularly suitable for making it the inner surface of the bend, facing the user of a bendable electronic device, e.g. a smartphone. Also, as mentioned above, it is generally the outer surface of the bend that faces certain problems due to tensile forces.However, the problem that occurs towards the inner surface of the bend is so-called crease.Interestingly, the convex first surface of the glass article of the present invention counteracts the crease problem.Therefore, this makes the first surface even more suitable to be the inner surface of the bend.
[0080] The warpage can be measured, for example, by placing the glass article on a flat surface and then recording the longest distance between the lower surface of the glass article and said flat surface as the warpage. The warpage can be measured, for example, by a set of feeler gauges, particularly with a resolution of 0.02 mm.
[0081] The glass article of the present invention may have a warp of at least 0.5 mm, at least 1.0 mm, at least 1.5 mm, or at least 2.0 mm, particularly when the first surface of the glass article is a convex surface and the second surface of the glass article is a concave surface. The glass article of the present invention may have a warp of up to 5.0 mm, up to 4.0 mm, up to 3.0 mm, or up to 2.5 mm, particularly when the first surface of the glass article is a convex surface and the second surface of the glass article is a concave surface. The glass article of the present invention may have a warp in the range of 0.5 to 5.0 mm, 1.0 to 4.0 mm, 1.5 to 3.0 mm, or 2.0 to 2.5 mm, particularly when the first surface of the glass article is a convex surface and the second surface of the glass article is a concave surface. This warp is also referred to as absolute warp and indicates the warp of the glass article.
[0082] However, it is also possible to specify the relative bow of the glass article, in particular the area relative bow and / or the length relative bow.
[0083] The warpage of a glass article may, for example, be shown normalized to the surface area of one of the two major surfaces of the glass article (area relative warpage). Since both major surfaces of a glass article generally have the same or nearly the same surface area, the warpage can be normalized to either one of the two major surfaces to obtain the same results. For example, a glass article having a length of 50 mm and a width of 30 mm will have two major surfaces each with a surface area of 30×50 mm. 2 =1500mm 2 Similarly, each of the two major surfaces of a glass article having a length of 125 mm and a width of 40 mm has a surface area of 125×40 mm. 2 =5000mm 2 Each of the two main surfaces has a surface area of 5000 mm 2 If such a glass article has a warp of 2.0 mm (= 2000 μm), the area relative warp is 2000 μm × 5000 mm 2 Divide by 1 mm 2 This amounts to 0.4 μm per unit area.
[0084] The glass article of the present invention has a thickness of 1 mm or less, particularly when the first surface of the glass article is a convex surface and the second surface of the glass article is a concave surface. 2 At least 0.02μm per 1mm 2 At least 0.05μm per 1mm 2 At least 0.10 μm per mm, or 1 mm 2 The glass article of the present invention may have an areal relative warp of at least 0.25 μm per mm, particularly when the first surface of the glass article is a convex surface and the second surface of the glass article is a concave surface. 2 Maximum 5.0μm, 1mm 2 Maximum 2.5μm, 1mm 2 Up to 1.5μm per mm, or 1mm 2 The glass article of the present invention may have an areal relative warp of up to 1.0 μm per mm, particularly when the first surface of the glass article is a convex surface and the second surface of the glass article is a concave surface. 2 0.02~5.0μm, 1mm 2 0.05~2.5μm, 1mm 2 0.10 to 1.5 μm per mm, or 1 mm 2 The area relative warp may be in the range of 0.25 to 1.0 μm per unit area.
[0085] The warpage of a glass article can also be shown normalized to the longest length of one of the two major surfaces of the glass article (length-relative warpage). Since both major surfaces of a glass article generally have the same or nearly the same longest length, the warpage can be normalized to either one of the two major surfaces to obtain the same results. For a glass article having a major surface with a round shape, the longest length is its diameter. For a glass article having a major surface with a rectangular shape, the longest length is its diagonal. For example, each of the two major surfaces of a glass article having a length of 50 mm and a width of 30 mm has a length of (30 2 mm 2 +50 2 mm 2Similarly, each of the two major surfaces of a glass article having a length of 125 mm and a width of 40 mm has a square root of (125 2 mm 2 +40 2 mm 2 ) = approximately 131.25 mmn longest length. If such a glass article having a longest length of 131.25 mm on each of its two major surfaces has a warp of 2.0 mm (= 2000 μm), the length relative warp would be 2000 μm divided by 131.25 mm, or approximately 15.2 μm per mm.
[0086] The glass articles of the present invention may have a length relative warp of at least 5.0 μm per mm, at least 10.0 μm per mm, at least 12.5 μm per mm, or at least 15.0 μm per mm, particularly when the first surface of the glass article is a convex surface and the second surface of the glass article is a concave surface. The glass articles of the present invention may have a length relative warp of up to 50.0 μm per mm, up to 40.0 μm per mm, up to 30.0 μm per mm, or up to 20.0 μm per mm, particularly when the first surface of the glass article is a convex surface and the second surface of the glass article is a concave surface. The glass article of the present invention may have a relative linear warp in the range of 5.0 to 50.0 μm per mm, 10.0 to 40.0 μm per mm, 12.5 to 30.0 μm per mm, or 15.0 to 20.0 μm per mm, particularly when the first surface of the glass article is a convex surface and the second surface of the glass article is a concave surface.
[0087] The present invention relates to a method for producing a glass article having a first surface and a second surface, in particular a method for producing a glass article of the invention, comprising the following steps: a) providing a glass article; b) forming a stack assembly comprising a plurality of glass articles (e.g., 3-100, or 4-20 glass articles) and at least one (preferably exactly one) adhesive layer between two adjacent glass articles, where a first surface of the glass articles is in contact with a first adhesive layer comprising (or consisting of) a first adhesive, and a second surface of the glass articles is in contact with a second adhesive layer comprising (or consisting of) a second adhesive, c) contacting said stack assembly (or a smaller stack assembly resulting therefrom) with a first etching solution; d) delaminating the stack assembly (or a smaller stack assembly resulting therefrom) by removing the first adhesive layer, resulting in a sandwich assembly consisting of two glass articles and a second adhesive layer located between the two glass articles. e) contacting the sandwich assembly with a second etching solution; f) delaminating the sandwich assembly by removing the second adhesive layer; The present invention also relates to the method, comprising:
[0088] The present invention relates to a method for producing a plurality of glass articles having a first surface and a second surface, in particular a method for producing the glass articles of the present invention, comprising the steps of: a) providing a plurality of glass articles; b) forming a stack assembly including the plurality of glass articles and at least one adhesive layer between two adjacent glass articles, where a first surface of the glass articles contacts a first type of adhesive and a second surface of the glass articles contacts a second type of adhesive; c) contacting said stack assembly or a smaller stack assembly obtained therefrom with a first etching solution; d) delaminating the stack assembly or a smaller stack assembly resulting therefrom by removing the first type of adhesive, resulting in a sandwich assembly consisting of two glass articles and a second type of adhesive located between the two glass articles. e) contacting the sandwich assembly with a second etching solution; f) delaminating the sandwich assembly by removing the second type of adhesive; The present invention also relates to the method, comprising:
[0089] Steps a) to f) are in particular carried out in a given order, in particular step a) is carried out before step b), step b) is carried out before step c), step c) is carried out before step d), step d) is carried out before step e) and / or step e) is carried out before step f), without excluding that the method of the invention may comprise one or more further steps subsequent to any of the above steps a) to f).
[0090] Step a) of providing the glass article or articles may comprise, for example, the downdraw or overflow fusion process. However, it is also possible to subject glass articles which have not been obtained by the downdraw or overflow fusion process to the method according to the invention.
[0091] Step b) of forming the stack assembly utilizes two different types of adhesives, a first adhesive and a second adhesive. The invention includes the idea of protecting the second surface of the glass article(s) from contact with the second etching solution during the second etching step e). In contrast, to achieve slimming of the glass article(s) to the desired thickness, the first surface of the glass article(s) must come into contact with the second etching solution. Thus, the first (type) adhesive is preferably selected such that it can be removed during the delamination step d). This allows the first surface of the glass article(s) to come into contact with the second etching solution during step e). In contrast, the second (type) adhesive is preferably selected such that it is not removed during the delamination step d). This allows the second surface of the glass article(s) to be protected from contact with the second etching solution during step e).
[0092] It will be understood that the selection of the first (type) adhesive and the second (type) adhesive is primarily determined by the delamination process to be applied, particularly in step d). For example, if the delamination step d) is selected to include boiling the stack assembly in hot water to remove the first adhesive, the first (type) adhesive should be selected such that it is removable by boiling in hot water, while the second (type) adhesive should be selected such that it is not removable by boiling in hot water. If other delamination methods are applied in step d), the selection of the first (type) adhesive and the second (type) adhesive can be easily adapted accordingly. The difference between the first (type) adhesive and the second (type) adhesive may not only be that their removability is qualitatively different (e.g., the first (type) adhesive is removable by hot water and the second (type) adhesive is not removable by hot water). Alternatively or additionally, the first (type) adhesive and the second (type) adhesive can be distinguished by a quantitative difference. For example, it may be conceivable that a first (type) adhesive and a second (type) adhesive are both removable by the same delamination principle, but the second (type) adhesive requires a quantitatively greater amount of this delamination principle, e.g. a higher concentration of removal substance, a higher temperature, etc.
[0093] Adhesives are often differentiated by their curing mechanism. For example, adhesives can be cured by applying energy in the form of pressure, radiation, etc. The first and / or second (type) adhesive of the present invention can be, for example, a pressure sensitive adhesive (PSA) or a UV-curable adhesive. For example, the first (type) adhesive can be a PSA and the second (type) adhesive can be a UV-curable adhesive. Alternatively, the first (type) adhesive can be a UV-curable adhesive and the second (type) adhesive can be a PSA. In some embodiments, both the first (type) adhesive and the second (type) adhesive can be a PSA, or both the first (type) adhesive and the second (type) adhesive can be a UV-curable adhesive. It is particularly preferred that both the first (type) adhesive and the second (type) adhesive are UV-curable adhesives.
[0094] According to step c) of the method of the invention, the stack assembly is contacted with a first etching solution. The etching time may for example be 1-120 min, 1-60 min, 1-30 min or 1-20 min, for example 2-15 min or 5-12 min. The etching time may for example be at least 1 min, at least 2 min, at least 5 min or at least 10 min. The etching time may for example be up to 120 min, up to 60 min, up to 30 min, up to 20 min, up to 15 min or up to 12 min. Usually, the smaller the thickness of the glass article(s), the shorter the etching time can be selected.
[0095] The etching temperature may be, for example, 1°C to 80°C, or 20°C to 50°C, for example, 30°C to 45°C.
[0096] The etchant solution is preferably HF and / or NH 4 HF 2 and inorganic acids (e.g., HCl, HNO 3 , H 2 SO 4or mixtures of two or more thereof) and / or with organic acids (e.g. acetic acid, citric acid, oxalic acid or mixtures of two or more thereof). 4 HF 2 The total amount of HF and NH may be, for example, in the range of 0.1% by mass to 10% by mass, for example, 0.5% to 5% by mass, or 1% to 2% by mass. 4 HF 2 The total amount of HF and NH may be, for example, at least 0.1 wt.%, at least 0.5 wt.%, or at least 1 wt.%. 4 HF 2 The total amount of inorganic acids, HF and NH may be, for example, up to 10% by weight, up to 5% by weight, or up to 2% by weight. 4 HF 2 The mass ratio of the total amount of organic acids to the total amount of HF and NH may be, for example, in the range of 0.1:1 to 10:1. 4 HF 2 The mass ratio of the etchant to the total amount of NH may be, for example, in the range of 0.1:1 to 10:1. 4 HF 2 and 3% by weight HNO 3 or the etchant solution may comprise or consist of 2% by weight NH 4 HF 2 , 2% by weight HNO 3 and 5% by weight acetic acid, or the etchant solution may comprise or consist of 1% by weight HF and 1% by weight HNO 3 The etchant solution may include or consist of one or more surfactants, such as an alkylphenol ethoxylate, or ammonium lauryl sulfate, or a mixture of an alkylphenol ethoxylate and ammonium lauryl sulfate.
[0097] In particular, the etching step c) is performed before the first delamination step d). Thus, both the first and second surfaces of the glass article(s) are protected from contact with the first etching solution. Rather, the first etching solution contacts the edge of the glass article. In particular, the etching step c) can be a step of providing at least one edge of the glass article(s) with a chamfer structure.
[0098] The method of the present invention may optionally include one or more further steps following the formation of the stack assembly according to step b) and prior to the etching step e). For example, the stack assembly may be cut into smaller stack assemblies. The method of the present invention may also include a step of edge grinding the stack assembly or smaller stack assemblies obtained therefrom prior to contacting the stack assembly with the first etching solution of step c).
[0099] The glass article or articles prepared in step a) may have a relatively large length and / or width. For example, the glass article(s) prepared in step a) may have a length of about 500 mm and / or a width of about 400 mm. Such dimensions may be too large for various intended applications, such as the use of the glass article of the present invention in foldable electronic devices, such as smartphones. Therefore, it may be desirable to reduce the length and / or width by cutting the glass article(s) into smaller glass articles. Such a cutting step, if desired, is preferably performed subsequent to step b) of forming the stack assembly and prior to etching step c). The optional cutting step results in a smaller stack assembly compared to the stack assembly formed in step b). The term "smaller" relates to a reduction in the length and / or width of the stack assembly obtained in the cutting step compared to the length and / or width of the stack assembly formed in step b). For example, the optional cutting step may result in a stack assembly having a length of about 125 mm and a width of about 40 mm, or a stack assembly having a length of about 50 mm and a width of about 30 mm.
[0100] According to step d) of the method of the invention, the stack assembly (or the smaller stack assembly resulting therefrom) is delaminated by removing the first adhesive layer or the first type of adhesive, respectively. This results in a sandwich assembly consisting of two glass articles and a second adhesive layer or the second type of adhesive, respectively, located between said two glass articles. The delamination step d) can be adapted depending on the first and second (type) adhesive applied in step b) of forming the stack assembly. The delamination step d) is selected such that the first adhesive layer or the first type of adhesive, respectively, is removed, while the second adhesive layer or the second type of adhesive, respectively, is not removed. For example, the delamination step d) can comprise holding the stack assembly (or the smaller stack assembly resulting therefrom) in a delamination liquid at an elevated temperature. The temperature of the delamination liquid may for example be above 40° C. The holding time in the delamination liquid may for example be between 1 and 30 minutes. The delamination liquid may for example be an aqueous solution, in particular water.
[0101] Additionally or alternatively, the stack assembly (or smaller stack assemblies resulting therefrom) can be separated by physical force through the valley created by the two adjacent chamfers, particularly due to the low adhesive strength between the first adhesive layer and the glass article(s).
[0102] According to step e) of the method of the invention, the sandwich assembly is contacted with a second etching solution. The second etching solution may for example comprise HF. The second etching solution may comprise an inorganic acid and / or an organic acid, in particular in addition to HF. The etching time, etching temperature and / or etching solution may be the same as those described above for the first etching step.
[0103] The etching time may be, for example, 1 to 120 minutes, 1 to 60 minutes, 1 to 30 minutes, or 1 to 20 minutes, for example, 2 to 15 minutes, or 5 to 12 minutes. The etching time may be, for example, at least 1 minute, at least 2 minutes, at least 5 minutes, or at least 10 minutes. The etching time may be, for example, up to 120 minutes, up to 60 minutes, up to 30 minutes, up to 20 minutes, up to 15 minutes, or up to 12 minutes. Typically, the thinner the glass article(s), the shorter the etching time can be selected.
[0104] The etching temperature may be, for example, 1°C to 80°C, or 20°C to 50°C, for example, 30°C to 45°C.
[0105] The etchant solution is preferably HF and / or NH 4 HF 2 and inorganic acids (e.g., HCl, HNO 3 , H 2 SO 4 or mixtures of two or more thereof) and / or with organic acids (e.g. acetic acid, citric acid, oxalic acid or mixtures of two or more thereof). 4 HF 2 The total amount of HF and NH may be, for example, in the range of 0.1% by mass to 10% by mass, for example, 0.5% to 5% by mass, or 1% to 2% by mass. 4 HF 2 The total amount of HF and NH may be, for example, at least 0.1 wt.%, at least 0.5 wt.%, or at least 1 wt.%. 4 HF 2 The total amount of inorganic acids, HF and NH may be, for example, up to 10% by weight, up to 5% by weight, or up to 2% by weight. 4 HF 2 The mass ratio of the total amount of organic acids to the total amount of HF and NH may be, for example, in the range of 0.1:1 to 10:1. 4 HF 2 The mass ratio of the etchant to the total amount of NH may be, for example, in the range of 0.1:1 to 10:1. 4 HF 2 and 3% by weight HNO3 or the etchant solution may comprise or consist of 2% by weight NH 4 HF 2 , 2% by weight HNO 3 and 5% by weight acetic acid, or the etchant solution may comprise or consist of 1% by weight HF and 1% by weight HNO 3 The etchant solution may include or consist of one or more surfactants, such as an alkylphenol ethoxylate, or ammonium lauryl sulfate, or a mixture of an alkylphenol ethoxylate and ammonium lauryl sulfate.
[0106] According to step f) of the method of the invention, the sandwich assembly is delaminated by removing the second adhesive layer or the second type of adhesive, respectively. A glass article of the invention can be obtained in the delamination step f). Step f) can be adapted depending on the second (type) adhesive applied in step b) of forming the stack assembly. For example, the delamination step f) can comprise applying radiation, in particular UV radiation, to the sandwich assembly. The radiation can have for example a peak wavelength in the range of 250 nm to 450 nm, in particular 300 nm to 400 nm, or 350 to 395 nm, for example around 365 nm or 390 nm. The radiation intensity can be for example 200 to 1000 mJ / cm 2 The irradiation time may be, for example, 30 seconds to 30 minutes.
[0107] The method of the invention may further comprise a step of chemically strengthening the glass article(s) obtained by delamination step f).
[0108] The invention also relates to a bendable device comprising a glass article of the invention, in particular the device can be bent such that the first surface is located on the inner surface of the bend and the second surface is located on the outer surface of the bend.
[0109] A bendable device may, for example, bend to a bend radius of 1 to 5 mm, such as to a bend radius of 1 mm, 2 mm, 3 mm, 4 mm, or 5 mm.
[0110] The bendable device may for example be an electronic device, in particular a smartphone.
[0111] The present invention also relates to the use of the glass article of the present invention in bendable devices, in particular in bendable electronic devices, such as smartphones. [Brief description of the drawings]
[0112] [Figure 1] FIG. 2 is a diagram showing a schematic view of a profile of a glass article 10. [Diagram 2] FIG. 2 is a diagram showing a schematic view of a profile of a glass article 20. [Diagram 3] FIG. 1 shows a microscope image of a cross section of a glass article having an asymmetric chamfered structure. [Figure 4] Schematic diagram of the ball-on-ring test setup.
[0113] Description of the drawings FIG. 1 shows a schematic profile of a glass article 10 including a first surface 11, a second surface 12, and at least one edge connecting the first surface 11 and the second surface 12. The first surface 11 and the second surface 12 are essentially parallel to each other. The edge has a chamfer structure 16 including three surfaces: (i) a vertical surface 13 that is essentially perpendicular to the first surface 11 and the second surface 12, (ii) a first connecting surface 14 connecting the vertical surface 13 to the first surface 11, and (iii) a second connecting surface 15 connecting the vertical surface 13 to the second surface 12. The chamfer structure 16 of the glass article 10 shown in FIG. 1 is symmetrical.
[0114] 2 shows a schematic profile of a glass article 20 including a first surface 21, a second surface 22, and at least one edge connecting the first surface 21 and the second surface 22. The first surface 21 and the second surface 22 are essentially parallel to each other. The edge has a chamfer structure 26 including three surfaces: (i) a vertical surface 23 that is essentially perpendicular to the first surface 21 and the second surface 22, (ii) a first connecting surface 24 connecting the vertical surface 23 to the first surface 21, and (iii) a second connecting surface 25 connecting the vertical surface 23 to the second surface 22. The chamfer structure 26 of the glass article 20 shown in FIG. 2 is asymmetric.
[0115] FIG. 3 shows a microscope image of a cross section of a glass article having an asymmetric chamfer structure. The image was obtained at 200x magnification. The focus was on the top surface, so the edge appears very sharp. The glass article was positioned so that the top surface was not tilted. Thus, the top surface was perpendicular to the direction of the light. The image was obtained using a Nikon Y-TV55 microscope with automatic white balance, automatic brightness and automatic contrast. In the microscope image, tangents were fitted to the relevant surfaces (tangent A to the first connecting surface, tangent B to the first surface, tangent C to the vertical surface, tangent D to the second connecting surface, and tangent E to the second surface). The fitting of the tangents to each surface was done manually using ImageJ software (version 1.53i of March 24, 2021). As also shown in FIG. 3, the second connecting surface, and even more significantly the first connecting surface, deviated from a straight line toward the transition to the second surface or the first surface, respectively. Thus, the tangents were fitted to obtain the best fit towards the transition of the first connecting surface to the vertical surface, while a larger deviation was acceptable towards the transition of the first connecting surface to the first surface. The same was done for fitting the tangents to the second connecting surface. As shown in FIG. 3, the tangent A to the first connecting surface is a distance d from the tangent C to the vertical surface. 1 Similarly, the tangent line D to the second connecting surface is a distance d from the tangent line C to the normal surface.2 At d, it intersects with the tangent line E to the second surface. 1 and d 2 Both and were measured perpendicular to the tangent line C to the vertical surface using ImageJ software. The measurement was taken as the distance d 1 and d 2 This was done by comparing the length of each distance d with the length of the 100 μm scale bar. 1 is measured to be 99 μm, and the distance d 2 was measured to be 56 μm. The thickness of the glass article was 50 μm.
[0116] FIG. 4 is a schematic, not to scale, diagram of the ball-on-ring test setup. FIG. 4A shows a top / bottom view of the setup. FIG. 4B shows a cross-sectional view of the setup. In the ball-on-ring test, a surface 45 of a glass article 41 is placed on a steel ring 42 having an inner diameter of 4 mm and an outer diameter of 6 mm. The ring is 3 mm deep, the walls of the ring are 1 mm thick, with the tip of the wall having a semicircle with a diameter of 1 mm as a cross section. A tungsten carbide ball 43 with a diameter of 1 mm is pressed against the surface 44 of the glass article 41 along the central axis of the ring at a rate of 5 mm / min until the glass closes. The force at break is recorded as the ball-on-ring break force. EXAMPLES
[0117] Example 1 Example 1: 400 x 500 x 0.07 mm produced directly by downdraw 3 40×125×0.05mm processed from glass mother sheet 3 A stack of mother sheets was formed using alternating layers of two types of acrylate-based UV-curable adhesives. The stack was then cut into a 40×125 mm 2The glass was cut into smaller stacks with a size of 0.05 mm. After edge grinding, polishing and chamfer forming, the smaller stacks were then delaminated between the adhesive layers of type #1 by boiling in hot water, where a sandwich assembly consisting of two glass articles and a second adhesive layer located between the two glass articles is obtained. The sandwich assembly was then immersed in a mixture of HF and inorganic / organic acid, where the glass articles were slimmed from 0.07 mm to 0.05 mm. The assembly was then delaminated between the adhesive layers of type #2 by UV irradiation. The individual glass pieces were then delaminated with pure KNO 3 After chemical strengthening in HF and subsequent photoetching in a mixture of HF and inorganic / organic acids, less than 2 μm thickness was removed from the surface of each of the glass samples.
[0118] Example 2 Example 2: 400 x 500 x 0.07 mm produced directly by downdraw 3 30×50×0.03mm processed from glass mother sheet 3 A stack of mother sheets was formed using alternating layers of two types of acrylate-based UV-curable adhesives. The stack was then cut into 30×50 mm pieces. 2 The glass was cut into smaller stacks with a size of 0.07 mm. After edge grinding, polishing and chamfer forming, the smaller stacks were then delaminated between the adhesive layers of type #1 by boiling in hot water, where a sandwich assembly consisting of two glass articles and a second adhesive layer located between the two glass articles is obtained. The sandwich assembly was then immersed in a mixture of HF and inorganic / organic acid, where the glass articles were slimmed from 0.07 mm to 0.03 mm. The assembly was then delaminated between the adhesive layers of type #2 by UV irradiation. The individual glass pieces were then delaminated with pure KNO 3 After chemical strengthening in HF and subsequent photoetching in a mixture of HF and inorganic / organic acids, less than 2 μm thickness was removed from the surface of each of the glass samples.
[0119] Example 3 Example 3: 400 x 500 x 0.1 mm produced directly by downdraw 3 30×50×0.07mm processed from glass mother sheet 3 A stack of mother sheets was formed using alternating layers of two types of acrylate-based UV-curable adhesives. The stack was then cut into 30×50 mm pieces. 2 The glass was cut into smaller stacks with a size of 0.01 mm. After edge grinding, polishing and chamfer forming, the smaller stacks were then delaminated between the adhesive layers of type #1 by boiling in hot water, where a sandwich assembly consisting of two glass articles and a second adhesive layer located between the two glass articles is obtained. The sandwich assembly was then immersed in a mixture of HF and inorganic / organic acid, where the glass articles were slimmed from 0.1 mm to 0.07 mm. The assembly was then delaminated between the adhesive layers of type #2 by UV irradiation. The individual glass pieces were then delaminated with pure KNO 3 After chemical strengthening in HF and subsequent photoetching in a mixture of HF and inorganic / organic acids, less than 2 μm thickness was removed from the surface of each of the glass samples.
[0120] Comparative Example 1 Comparative Example 1: 400 x 500 x 0.07 mm directly produced by downdraw 3 40×125×0.05mm processed from glass mother sheet 3 Aluminosilicate glass pieces with a size of 40 × 125 mm were used to form a stack of mother sheets using one type of acrylate-based UV-curable adhesive. The stack was then assembled into a 40 × 125 mm 2 The glass was cut into smaller stacks with a size of 0.07 mm to 0.05 mm. Then, after edge grinding, polishing and chamfer forming, the smaller stacks were delaminated between the adhesive layers by boiling in hot water. The individual glass pieces were then slimmed from 0.07 mm to 0.05 mm by immersing in a mixture of HF and inorganic / organic acid. The slimmed individual glass pieces were then dissolved in pure KNO 3After chemical strengthening in HF and subsequent photoetching in a mixture of HF and inorganic / organic acids, less than 2 μm thickness was removed from the surface of each of the glass samples.
[0121] Comparative Example 2 Comparative Example 2: 400 x 500 x 0.07 mm directly produced by downdraw 3 30×50×0.03mm processed from glass mother sheet 3 Aluminosilicate glass pieces having a size of 30×50 mm were used to form a stack of mother sheets using one type of acrylate-based UV-curable adhesive. The stack was then assembled into a 30×50 mm 2 The glass was cut into smaller stacks with a size of 0.07 mm to 0.03 mm. Then, after edge grinding, polishing and chamfer forming, the smaller stacks were delaminated between the adhesive layers by boiling in hot water. The individual glass pieces were then slimmed from 0.07 mm to 0.03 mm by immersing in a mixture of HF and inorganic / organic acid. The slimmed individual glass pieces were then dissolved in pure KNO 3 After chemical strengthening in HF and subsequent photoetching in a mixture of HF and inorganic / organic acids, less than 2 μm thickness was removed from the surface of each of the glass samples.
[0122] Comparative Example 3 Comparative Example 3: 400 x 500 x 0.1 mm directly produced by downdraw 3 30×50×0.07mm processed from glass mother sheet 3 Aluminosilicate glass pieces having a size of 30×50 mm were used to form a stack of mother sheets using one type of acrylate-based UV-curable adhesive. The stack was then assembled into a 30×50 mm 2 The glass was cut into smaller stacks with a size of 0.1 mm to 0.07 mm. Then, after edge grinding, polishing and chamfer forming, the smaller stacks were delaminated between the adhesive layers by boiling in hot water. The individual glass pieces were then slimmed from 0.1 mm to 0.07 mm by immersing in a mixture of HF and inorganic / organic acids. The slimmed individual glass pieces were then dissolved in pure KNO 3After chemical strengthening in HF and subsequent photoetching in a mixture of HF and inorganic / organic acids, less than 2 μm thickness was removed from the surface of each of the glass samples.
[0123] Experimental Results The following table provides a summary of the above examples and their various properties.
[0124] [Table 1]
[0125] The inventive examples (Examples 1-3) have significant asymmetry in some aspects compared to the comparative examples (Comparative Examples 1-3). The comparative examples were designed to match the corresponding examples (Comparative Example 1 matches Example 1, Comparative Example 2 matches Example 2, and Comparative Example 3 matches Example 3) except that the comparative examples were not made from a stack assembly using two different adhesives. Thus, the second surfaces of Examples 1-3 were protected from contact with the etching solution during the slimming stage, while the second surfaces of Comparative Examples 1-3 were not protected during slimming. It was observed in Examples 1-3, but not in Comparative Examples 1-3, that protection of the second surfaces during slimming resulted in various asymmetries.
[0126] a) Surface roughness In Examples 1 and 2, the second surface has a significantly reduced surface roughness R a In contrast, this difference was not observed in the comparative example. a was measured by atomic force microscope (AFM). Model: BRUKER Dimension Icon. Area: 10×10μm. Surface roughness R a was determined in accordance with DIN EN ISO 4287:2010-07.
[0127] b) Asymmetry of chamfer The chamfered structures were highly asymmetric in Examples 1 to 3. In contrast, such asymmetry was not observed in the Comparative Example.
[0128] The symmetry / asymmetry of the chamfered structures was evaluated based on cross-sectional images of the profiles of the chamfered structures shown in Figures 1-3. To obtain such images, the glass articles were observed in transmitted light mode with an optical microscope. A magnification of 200x was used. The focus was on the top surface, so the edges appeared very sharp. The glass articles were positioned so that the top surface was not tilted. Thus, the top surface was perpendicular to the direction of the light. Particularly good quality images were obtained using a Nikon Y-TV55 microscope with auto white balance, auto brightness and auto contrast.
[0129] In the microscopic images, tangents were fitted to the relevant surfaces (tangent A to the first connecting surface, tangent B to the first surface, tangent C to the normal surface, tangent D to the second connecting surface, and tangent E to the second surface), as exemplarily shown in Figure 3. The fitting of the tangents to the respective surfaces was done manually using ImageJ software.
[0130] As shown in FIG. 3, the tangent A to the first connecting surface is a distance d from the tangent C to the normal surface. 1 Similarly, the tangent line D to the second connecting surface is a distance d from the tangent line C to the normal surface. 2 At d, it intersects with the tangent line E to the second surface. 1 and d 2 Both and were measured perpendicular to the tangent C to the vertical surface, as shown in FIG. 3. The distance d 1 and d 2 The length of the distance d is calculated using ImageJ software. 1 and d 2 were measured by comparing the lengths of the scale bars, respectively.
[0131] The asymmetry values referred to in the above table are the difference d 1 -d 2The difference is an absolute value of 40 to 64 μm for Examples 1 to 3. In contrast, for the Comparative Example, the difference was less than 10 μm.
[0132] c) chemical strengthening The asymmetry of the glass article of the present invention with respect to the first and second surfaces is also reflected by an asymmetry during chemical strengthening.
[0133] As shown in the table above, the first surfaces of Examples 1-3 are associated with higher surface compressive stress (CS) but less depth of compressive stress layer (DoL) compared to the second surface of the glass article, no such difference was observed in the comparative examples.
[0134] Interestingly, the difference between the first and second surfaces in terms of chemical strengthening results was associated with the occurrence of warpage in Examples 1 to 3, as also shown in the table above. No warpage was observed in the comparative examples. Warpage was measured by placing the glass article on a flat surface and then recording the longest distance of the bottom surface of the glass article from said flat surface as the warpage, which is typically at one of the four corners. The distance was measured by a set of feeler gauges (resolution was 0.02 mm). The warpage data shown in the table above was taken over the entire sample area, i.e., 40 × 125 mm2, respectively. 2 or 30×50mm 2 Regarding.
[0135] The warpage in Examples 1 to 3 was such that the first surface of the glass article was convex and the second surface of the glass article was concave.
[0136] d) Pen drop height The breaking height is determined in a pen drop test, in which a glass article is attached to one surface of a 150 μm thick substrate, which consists of, from the side contacting the glass to the side contacting the marble stage, a 25 μm thick layer of pressure sensitive adhesive (PSA) material, a 50 μm thick layer of polyethylene (PE), another 25 μm thick layer of pressure sensitive adhesive (PSA), and another 50 μm thick layer of polyethylene (PE). Under the 150 μm thick substrate is a flat 10 cm thick marble stage with a polished smooth surface. Subsequently, the other surface of the glass article facing upwards is impacted with a 14 g ballpoint pen (manufactured by Chenguang) with a ball diameter of 0.5 mm made of tungsten carbide, from a height of 5 mm increasing until the glass breaks. The breaking height is then recorded as the pen drop height.
[0137] The product of the pen drop test is the pen drop height of the surface that is impacted with a ballpoint pen. Since the pen drop height depends significantly on the thickness of the article, in order to compare the properties of articles of different thicknesses, it may be considered to refer to the normalized pen drop height. The normalized pen drop height is the ratio of the pen drop height (μm) to the square of the thickness of the article (μm 2 The results are shown in the table below.
[0138] [Table 2]
[0139] The pen drop height values in the table above are the average of 15 experiments. The standard deviations were 1.2 mm for Example 1, 1.3 mm for Example 2, and 2.2 mm for Example 3.
[0140] The data show that the pen drop height of the first surface was significantly increased. In contrast, the pen drop height of the comparative examples was comparable to the pen drop height of the second surface of Examples 1 to 3 (Comparative Example 1: 12.9 mm, Comparative Example 2: 6.1 mm, Comparative Example 3: 39.5 mm).
[0141] e) 2PB strength In the two-point bend test (2PB test), a glass article is placed in a U-shape between two parallel metal plates. The two plates are large enough to cover the entire glass article. One of the plates is then moved towards the other, parallel to each other, at a speed of 60 mm / min until the glass article breaks. The 2PB strength is σ = 1.198Ed / (Dd) where σ is the calculated strength, E is Young's modulus, d is the thickness of the glass article, and D is the distance between the two plates at break.
[0142] The product of the 2PB test is the 2PB strength of the surface of the glass article that was the outer surface of the bend. For example, if a glass article is bent such that a first surface of the glass article is the inner surface of the bend while a second surface of the glass article is the outer surface of the bend, the product of the 2PB test is the 2PB strength of the second surface of the glass article.
[0143] The following table shows the 2PB strength (MPa) of Examples 1 to 3 in the 2PB test.
[0144] [Table 3]
[0145] The 2PB strength values in the above table are the average values of 30 experiments. The data show that by protecting the second surface from the etching solution during the slimming stage, the 2PB strength of the second surface was greatly increased. In contrast, this was not observed in the comparative examples, because the second surface was not protected. In fact, the 2PB strength of the comparative examples was comparable to the 2PB strength of the first surface of Examples 1 to 3 (Comparative Example 1: 2570 MPa, Comparative Example 2: 2438 MPa, Comparative Example 3: 2451 MPa).
[0146] f) Ball-on-Ring (BoR) Test In the BoR test, a glass article is placed on a steel ring with an inner diameter of 4 mm and an outer diameter of 6 mm. The ring is 3 mm deep, the walls of the ring are 1 mm thick, and the tip of the wall has a semicircle with a diameter of 1 mm as a cross section. The edge of the glass sample was at least 20 mm away from the center of the ring. A tungsten carbide ball with a diameter of 1 mm is then pressed against the glass sample along the central axis of the ring at a rate of 5 mm / min until the glass closes. The force at break is recorded. The BoR test setup is shown diagrammatically in Figure 4.
[0147] Depending on which surface of the glass article is in contact with the ring or ball, respectively, the ball-on-ring breaking strength of the first or second surface of the glass article can be tested. The ball-on-ring test described here is tailored to identify the ball-on-ring breaking strength of a specific surface of the glass article in contact with the steel ring. In particular, it is this surface of the glass article where tensile stresses are developed during the ball-on-ring test. The product of the ball-on-ring test is therefore the ball-on-ring breaking strength of the surface in contact with the steel ring.
[0148] The following table shows the BoR breaking strength (N) of Examples 1 to 3 in the BoR test.
[0149] [Table 4]
[0150] The BoR breakdown force values in the above table are the average values of 15 experiments. The data show that by protecting the second surface from the etching solution during the slimming stage, the BoR breakdown force of the second surface was greatly increased. In contrast, this was not observed in the comparative examples, because the second surface was not protected. In fact, the BoR breakdown force of the comparative examples was comparable to the BoR breakdown force of the first surface of the corresponding examples 1 to 3 (Comparative Example 1: 9.3 N, Comparative Example 2: 8.2 N, Comparative Example 3: 12.6 N). [Explanation of symbols]
[0151] 10, 20 Glass items 11, 21 First Surface 12, 22 Second Surface 13, 23 vertical surface 14, 24 First connecting surface 15, 25 Second connecting surface 16, 26 Chamfered structure 41 Glass items 42 Ring 43 Ball 44, 45 Surface of glass articles
Claims
1. A glass article having a thickness of 10 μm to 150 μm, - comprising a first surface, a second surface, and at least one edge connecting said first surface and said second surface; the surface roughness R of the second surface; a (arithmetic mean roughness) is a maximum of 0.30 nm; The glass article.
2. The surface roughness R of the first surface a The glass article of claim 1, wherein the maximum thickness is 0.80 nm.
3. The surface roughness R of the first surface a The surface roughness R of the second surface a The glass article according to claim 1 or 2, wherein the thickness of the glass article is higher than 100 nm.
4. The surface roughness R of the first surface a and the surface roughness R of the second surface. a The glass article according to any one of claims 1 to 3, wherein the absolute value of the difference between the
5. A glass article having a thickness of 10 μm to 150 μm, - comprising a first surface, a second surface, and at least one edge connecting said first surface and said second surface; the first surface and the second surface are essentially parallel to one another; said end has three surfaces: a vertical surface that is essentially perpendicular to said first surface and to said second surface; a first connecting surface connecting said vertical surface and said first surface, and a second connecting surface connecting said vertical surface and said second surface; A chamfered structure including The chamfered structure is - a tangent A to said first connecting surface is at a distance d from a tangent C to said normal surface 1 intersects with a tangent B to the first surface at - the tangent D to said second connecting surface is at a distance d from the tangent C to said normal surface 2 intersects with a tangent line E to the second surface at profile, where -d 1 and 2 and are both measured perpendicular to a tangent C to said vertical surface, - the tangents A to E are obtained by fitting each tangent to the corresponding surface of the profile of the chamfer structure; The chamfered structure is d 1 ≠d 2 is asymmetric so that The glass article.
6. Difference d 1 -d 2 is at least 30% of the thickness of the glass article.
7. Difference d 1 -d 2 7. The glass article according to claim 5 or 6, wherein the absolute value of is at most 200% of the thickness of the glass article.
8. Difference d 1 -d 2 8. The glass article according to claim 5, wherein the absolute value of is at least 15 μm.
9. Difference d 1 -d 2 9. The glass article according to claim 5, wherein the absolute value of is at most 100 μm.
10. d 1 The glass article according to any one of claims 5 to 9, wherein the thickness is in the range of 50 to 200 μm.
11. d 2 The glass article according to any one of claims 5 to 10, wherein the thickness is in the range of 30 to 100 μm.
12. d 1 d 2 10. The glass article of claim 5, wherein the glass article is greater than 100 mm.
13. A glass article having a thickness of 10 μm to 150 μm, - comprising a first surface, a second surface, and at least one edge connecting said first surface and said second surface; the first surface has an impact resistance corresponding to a pen drop height of at least 5 mm; and the second surface has a ball-on-ring breaking force of at least 5.0 N and / or a two-point bending strength of at least 2,000 MPa; The glass article.
14. 14. A glass article according to any one of claims 1 to 13, wherein the first surface has an impact resistance corresponding to a normalized pen drop height of at least 4.5 per μm.
15. 15. The glass article of any one of claims 1 to 14, wherein the ratio of pen drop height of the first surface to the pen drop height of the second surface is at least 1.
05.
16. 16. The glass article of any one of claims 1 to 15, wherein the ratio of the ball-on-ring breaking force of the second surface to the ball-on-ring breaking force of the first surface is at least 1.
05.
17. 17. The glass article of any one of claims 1 to 16, wherein the ratio of the two-point bending strength of the second surface to the two-point bending strength of the first surface is at least 1.
05.
18. 18. The glass article of any one of claims 1 to 17, wherein the glass article is chemically strengthened.
19. 19. The glass article of claim 18, wherein each of the surface compressive stress CS1 at the first surface of the glass article and the surface compressive stress CS2 at the second surface of the glass article is at least 300 MPa.
20. 20. The glass article of claim 18 or 19, wherein CS1 and CS2 each have a maximum of 1000 MPa.
21. 21. A glass article according to claim 19 or 20, wherein a surface compressive stress CS1 at the first surface is higher than a surface compressive stress CS2 at the second surface.
22. 22. A glass article according to any one of claims 19 to 21, wherein the absolute value of the difference CS1-CS2 is at least 10 MPa.
23. 23. A glass article according to any one of claims 18 to 22, wherein the absolute value of the difference CS1-CS2 is at most 100 MPa.
24. 24. The glass article of any one of claims 18 to 23, wherein the article has a first compressive stress layer extending from a first surface of the glass article to a first depth of layer DoL1 and a second compressive stress layer extending from a second surface to a second depth of layer DoL2, each of DoL1 and DoL2 being in the range of 2.5 to 20.0 μm and / or in the range of 5.0% to 40.0% of the thickness of the glass article.
25. 25. A glass article according to any one of claims 18 to 24, wherein the ratio of DoL2 / DoL1 is in the range from greater than 1.00 to 1.
20.
26. 26. The glass article of any one of claims 1 to 25, having a warp of 5 mm or less.
27. 27. The glass article of any one of claims 1 to 26, having a warp of 0.5 mm or more.
28. The glass article is 1 mm 2 28. The glass article of any one of claims 1 to 27, having an areal relative warp in the range of 0.02 to 5.0 μm per unit area.
29. 29. The glass article of any one of claims 1 to 28, wherein the glass article has a linear relative bow in the range of 5.0 to 50.0 μm per mm.
30. 30. The glass article of any one of claims 26 to 29, wherein a first surface of the glass article is a convex surface and a second surface of the glass article is a concave surface.
31. A method for producing a plurality of glass articles having a first surface and a second surface, in particular the glass articles according to any one of claims 1 to 30, comprising the following steps: a) providing a plurality of glass articles; b) forming a stack assembly including the plurality of glass articles and at least one layer of adhesive between two adjacent glass articles, where a first surface of the glass articles contacts a first type of adhesive and a second surface of the glass articles contacts a second type of adhesive; c) contacting said stack assembly or a smaller stack assembly obtained therefrom with a first etching solution; d) delaminating the stack assembly or a smaller stack assembly resulting therefrom by removing the first type of adhesive, resulting in a sandwich assembly consisting of two glass articles and a second type of adhesive located between the two glass articles. e) contacting the sandwich assembly with a second etching solution; f) delaminating the sandwich assembly by removing the second type of adhesive; The method comprising:
32. 32. The method of claim 31, wherein the first type of adhesive and / or the second type of adhesive is a UV-curable adhesive.
33. 33. The method of claim 31 or 32, wherein step d) comprises maintaining the stack assembly or smaller stack assemblies obtained therefrom in a delaminating liquid at a temperature above 40°C.
34. 34. The method of claim 33, wherein the stack assembly or smaller stack assemblies obtained therefrom are maintained in the delaminating liquid for 1 to 30 minutes.
35. 35. The method of any one of claims 31 to 34, wherein the second etching solution comprises HF.
36. 36. The method of any one of claims 31 to 35, wherein step f) comprises applying UV radiation to the sandwich assembly.
37. UV irradiation has an intensity of 200 to 1000 mJ / cm 2 37. The method of claim 36, wherein the composition is applied at a concentration of from 30 seconds to 30 minutes.
38. 38. The method according to any one of claims 31 to 37, wherein the method further comprises a step of chemically strengthening the glass article obtained by delaminating step f).
39. 39. The method of any one of claims 31 to 38, wherein the method comprises a step of cutting the stack assembly formed in step b) to obtain smaller stack assemblies, the cutting step being performed before step c).
40. 40. The method of any one of claims 31 to 39, further comprising the step of edge grinding the stack assembly or a smaller stack assembly obtained therefrom prior to contacting the stack assembly with the first etching solution of step c).
41. 31. A bendable device comprising a glass article according to any one of claims 1 to 30.
42. 42. The bendable device of claim 41, wherein the device is bendable such that the first surface is on an inner surface of the bend and the second surface is on an outer surface of the bend.
43. 43. A bendable device according to claim 41 or 42, wherein the device is bendable to a bend radius of from 1 mm to 5 mm.
44. 44. A bendable device according to any one of claims 41 to 43, wherein the device is an electronic device, in particular a smartphone.
45. 31. Use of a glass article according to any one of claims 1 to 30 in a bendable device, in particular a bendable electronic device, for example a smartphone.
Citation Information
Patent Citations
Flexible, ultra-thin glass with high contact resistance
JP2020521699A
Glass substrate
WO2019093087A1
Enhanced strenght glass by combining redraw and chemical thinning processes
WO2020040973A1
Foldable apparatus, ribbons, and methods of making
WO2021041857A1