Cold-rolled steel sheet and its manufacturing method

A cold-rolled steel sheet with optimized alloying and microstructure achieves high strength, ductility, and weldability by controlling alloy composition and manufacturing processes, addressing LME and hydrogen embrittlement issues.

JP2024544027AActive Publication Date: 2024-11-26POHANG IRON & STEEL CO LTD

Patent Information

Application Number
JP2024533862
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-06
Filing Date
2022-12-06
Publication Date
2024-11-26
Estimated Expiration
2042-12-06

AI Technical Summary

Technical Problem

Existing high-strength steel sheets face challenges in maintaining weldability, strength, and formability due to issues like Liquid Metal Embrittlement (LME) during spot welding and hydrogen embrittlement, particularly when high tensile strength is required, which also affects corrosion resistance and formability.

Method used

A cold-rolled steel sheet composition with specific alloying elements (C, Si, Al, Mn, Cr, Mo, B, Nb, Ti, P, S, N) and microstructure fractions (retained austenite, fresh martensite, bainite, tempered martensite, ferrite) optimized by relational expressions, combined with a manufacturing process involving heating, hot rolling, cold rolling, continuous annealing, and controlled cooling to achieve desired mechanical properties.

Benefits of technology

The solution provides a cold-rolled steel sheet with tensile strength of 1180 to 1350 MPa, yield strength of 740 to 980 MPa, elongation rate of 8% or more, and hole expandability of 20% or more, while ensuring excellent weldability and resistance to LME, hydrogen embrittlement, and maintaining surface quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544027000001
    Figure 2024544027000001
  • Figure 2024544027000002
    Figure 2024544027000002
  • Figure 2024544027000003
    Figure 2024544027000003
Patent Text Reader

Abstract

TECHNICAL FIELD The present invention relates to a cold-rolled steel sheet and a manufacturing method thereof. One aspect of the present invention is to provide a cold-rolled steel sheet having excellent weldability, strength and formability, and a manufacturing method thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cold-rolled steel sheet having excellent weldability, strength and formability, and a method for producing the same. [Background technology]

[0002] Recently, efforts are being made to secure manufacturing technology for high-strength steel sheets to reduce the weight and improve safety of automobiles, and there is particularly an increasing demand for high-strength steel materials with tensile strengths of 980 MPa or higher. However, since simply improving strength usually results in a decrease in ductility and formability, high-strength steel sheets for cold forming that overcome this and also have formability are highly utilized in terms of improving fuel efficiency through weight reduction, improving part manufacturing / forming productivity, and ensuring the safety of final parts.

[0003] As a method for increasing elongation to improve the formability of steel materials, a method using the TRIP (Transformation Induced Plasticity) phenomenon by introducing retained austenite, as described in Patent Document 1, is widely used. However, in the case of such TRIP steel sheets, a large amount of Si and Al must be added to introduce the retained austenite, which causes LME (Liquid Metal Embrittlement) during spot welding of the steel sheets, limiting the use of plated steel sheets and cold-rolled steel sheets to be welded with plated materials. In addition, when the strength of the steel sheet is increased, there is a possibility of a problem of hydrogen embrittlement, in which assembled parts are suddenly broken during use, so it is necessary to prevent the steel sheet from causing severe corrosion even when exposed to a corrosive environment. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Korean Patent Publication No. 2017-7015003 Summary of the Invention [Problem to be solved by the invention]

[0005] One aspect of the present invention is to provide a cold-rolled steel sheet having excellent weldability, strength and formability, and a method for producing the same. [Means for solving the problem]

[0006] One embodiment of the present invention is a ferroelectric material having, by weight percent, C: 0.14-0.16%, Si: 0.3-0.6%, Al: 0.01-0.3%, Mn: 2.6-3.0%, Cr: 0.01-0.25%, Mo: 0.15-0.4%, B: 0.0001-0.005%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, P: 0.04% or less (excluding 0%), S: 0.01% or less (excluding 0%), N: 0.01% or less (excluding 0%), % excluding), the balance Fe and other unavoidable impurities, and satisfying the following relational expressions 1 and 2, the microstructure of which is composed of retained austenite: more than 1% and not more than 5%, fresh martensite: 10% or more and less than 25%, bainite: less than 20% (excluding 0%), tempered martensite: 55% or more and less than 80%, and ferrite: 5% or less (including 0%), and has excellent weldability, strength, and formability. [Relational expression 1] 234×[C]-29×[Si]-128×[Al]+29×[Mn]+10×[Cr]-17×[Mo]-37×[Nb]-49×[Ti]+100×[B]≧80 [Relationship 2] 5 × [C] + [Si] + 0.5 × [Al] ≦ 1.5 (However, in the above Relational Formulas 1 and 2, the content of each element means weight percent.)

[0007] Another embodiment of the present invention is a method for producing a hot-rolled steel sheet comprising the steps of: heating a slab containing, by weight percent, C: 0.14-0.16%, Si: 0.3-0.6%, Al: 0.01-0.3%, Mn: 2.6-3.0%, Cr: 0.01-0.25%, Mo: 0.15-0.4%, B: 0.0001-0.005%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, P: 0.04% or less (except 0%), S: 0.01% or less (except 0%), N: 0.01% or less (except 0%), the balance being Fe and other inevitable impurities, and satisfying the following relations 1 and 2; finish hot rolling the heated slab at 830-980°C to produce a hot-rolled steel sheet. The present invention provides a method for producing a cold-rolled steel sheet having excellent weldability, strength and formability, the method including the steps of: obtaining a plate; coiling the hot-rolled steel sheet at 450 to 700°C; cold rolling the coiled hot-rolled steel sheet to obtain a cold-rolled steel sheet; continuously annealing the cold steel sheet at a temperature of 800 to 840°C; primarily cooling the continuously annealed steel sheet to a primary cooling end temperature of 550 to 650°C at an average cooling rate of less than 10°C / s; secondarily cooling the primarily cooled steel sheet to a secondary cooling end temperature of 320 to 360°C at an average cooling rate of 10°C / s or more; and reheating the secondarily cooled steel sheet to a temperature range of 380 to 480°C. [Relational expression 1] 234×[C]-29×[Si]-128×[Al]+29×[Mn]+10×[Cr]-17×[Mo]-37×[Nb]-49×[Ti]+100×[B]≧80 [Relationship 2] 5 × [C] + [Si] + 0.5 × [Al] ≦ 1.5 (However, in the above Relational Formulas 1 and 2, the content of each element means weight percent.) Effect of the Invention

[0008] According to one aspect of the present invention, there is provided a cold-rolled steel sheet having excellent weldability, strength and formability, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, a cold rolled steel sheet having excellent weldability, strength and formability according to one embodiment of the present invention will be described.

[0010] First, the alloy composition of the present invention will be described. The contents of the alloy composition mentioned below are expressed in weight percent.

[0011] C: 0.14-0.16% Carbon (C) is an element that ensures the strength of steel material by solid solution strengthening and precipitation strengthening. If the C content is less than 0.14%, it is difficult to ensure a tensile strength (TS) of 1180 MPa class. On the other hand, if the C content exceeds 0.16%, the arc weldability and laser weldability deteriorate, and the risk of LME crack generation increases. Therefore, the C content is preferably in the range of 0.14 to 0.16%. The lower limit of the C content is more preferably 0.145%. The upper limit of the C content is more preferably 0.155%.

[0012] Silicon: 0.3 to 0.6% Silicon (Si) is a core element of TRIP (Transformation Induced Plasticity) steel that acts to increase the residual austenite fraction and elongation by inhibiting the precipitation of cementite. If the Si content is less than 0.3%, almost no residual austenite remains, and the elongation becomes excessively low. On the other hand, if the Si content exceeds 0.6%, it becomes impossible to prevent the deterioration of the physical properties of the welded part due to the formation of LME cracks, and the surface characteristics and platability of the steel material become poor. Therefore, the Si content is preferably in the range of 0.3 to 0.6%. The lower limit of the Si content is more preferably 0.35%. The upper limit of the Si content is more preferably 0.55%, further preferably 0.5%, and even more preferably 0.45%.

[0013] Al: 0.01 to 0.3% Aluminum (Al) is not only an element contained for deoxidizing steel material, but also an element effective in suppressing precipitation of cementite and stabilizing retained austenite. If the Al content is less than 0.01%, the steel material is not sufficiently deoxidized, and the cleanliness of the steel material is impaired. On the other hand, if the Al content exceeds 0.3%, the temperature required for single-phase region heating during annealing becomes high, and the castability of the steel material is impaired. Therefore, the Al content is preferably in the range of 0.01 to 0.3%. The lower limit of the Al content is more preferably 0.02%. The upper limit of the Al content is more preferably 0.25%, and further preferably 0.2%.

[0014] Mn: 2.6-3.0% Manganese (Mn) is an element added to ensure strength. If the Mn content is less than 2.6%, it becomes difficult to ensure strength, while if the Mn content exceeds 3.0%, the transformation rate of bainite slows down, and excessive fresh martensite is formed, making it difficult to obtain high hole expandability. In addition, a band structure is formed due to segregation of Mn, which impairs the material uniformity and formability of the material. Therefore, the Mn content is preferably in the range of 2.6 to 3.0%. The lower limit of the Mn content is more preferably 2.7%. The upper limit of the Mn content is more preferably 2.9%.

[0015] Cr: 0.01~0.25% Chromium (Cr) is an element added to ensure strength and hardenability. When Mn is added alone, an extremely large amount of Mn must be added, exceeding the range of the Mn content of the present invention. However, adding 0.01% or more of Cr can solve this problem. On the other hand, when the Cr content exceeds 0.25%, local corrosion resistance is deteriorated, hydrogen embrittlement cracks may occur, and oxides are formed on the surface, impairing phosphating ability. Therefore, the Cr content is preferably in the range of 0.01 to 0.25%. The lower limit of the Cr content is more preferably 0.05%, and even more preferably 0.1%. The upper limit of the Cr content is more preferably 0.2%, and even more preferably 0.15%.

[0016] Mo: 0.15-0.4% Molybdenum (Mo) is an element added to ensure strength and hardenability. When the Mo content is less than 0.15%, it is difficult to ensure strength and hardenability. On the other hand, when the Mo content exceeds 0.4%, phase transformation is suppressed, making it difficult to introduce a bainite structure, and since Mo is an expensive element, it is economically inefficient to manufacture the steel sheet. Therefore, the Mo content is preferably in the range of 0.15 to 0.4%. The lower limit of the Mo content is more preferably 0.17%. The upper limit of the Mo content is more preferably 0.3%, and more preferably 0.23%.

[0017] B: 0.0001 to 0.005% Boron (B) is an element added to ensure hardening ability. When Mn is added alone, an extremely large amount of Mn must be added, exceeding the range of the Mn content of the present invention, but this problem can be solved by adding 0.0001% or more of the above B. However, when the content of B exceeds 0.005%, B accumulates excessively on the surface, impairing the plating adhesion of the plated material. Therefore, the content of B is preferably in the range of 0.0001 to 0.005%. The lower limit of the B content is more preferably 0.0005%. The upper limit of the B content is more preferably 0.002%, and further preferably 0.0015%.

[0018] Nb: 0.001 to 0.05% Niobium (Nb) is an element added to ensure the strength of the steel sheet and refine the microstructure. When the Nb content is less than 0.001%, it is difficult to obtain the effects of improving the strength and refining the microstructure. On the other hand, when the Nb content exceeds 0.05%, recrystallization is delayed due to localized grain fixation, and the uniformity of the microstructure is impaired. Therefore, the Nb content is preferably in the range of 0.001 to 0.05%. The lower limit of the Nb content is more preferably 0.02%, and even more preferably 0.025%. The upper limit of the Nb content is more preferably 0.04%, and even more preferably 0.035%.

[0019] Ti: 0.001 to 0.05% Titanium (Ti) is an element added to ensure the strength of the steel sheet and refine the microstructure. When the Ti content is less than 0.001%, it is difficult to obtain the effects of improving the strength and refining the microstructure. On the other hand, when the Ti content exceeds 0.05%, castability is impaired due to excessive formation of TiN, and recrystallization is delayed due to localized grain fixation, thereby impairing the uniformity of the microstructure. Therefore, the Ti content is preferably in the range of 0.001 to 0.05%. The lower limit of the Ti content is more preferably 0.01%, and even more preferably 0.015%. The upper limit of the Ti content is more preferably 0.03%, and even more preferably 0.02%.

[0020] P: 0.04% or less (excluding 0%) Phosphorus (P) exists as an impurity in steel, and it is advantageous to control its content as low as possible. However, taking into consideration the case where P is unavoidably contained, the above P content does not include 0% (i.e., exceeds 0%). On the other hand, P may be intentionally added to increase the strength of steel, but if the above P is added in excess, the toughness of the steel deteriorates, so in the present invention, in order to prevent this, it is preferable to limit the upper limit to 0.04%. The above P content is more preferably 0.02% or less, and even more preferably 0.01% or less.

[0021] S: 0.01% or less (excluding 0%) Like the above-mentioned P, sulfur (S) exists as an impurity in steel, and it is advantageous to control its content as low as possible. Moreover, since the above-mentioned S deteriorates the ductility and impact properties of steel materials, it is preferable to limit its upper limit to 0.01%. The above-mentioned S content is more preferably 0.003% or less, and even more preferably 0.001% or less. However, taking into consideration cases where the above-mentioned S is unavoidably contained, 0% is excluded (i.e., it exceeds 0%).

[0022] N: 0.01% or less (excluding 0%) Nitrogen (N) is contained in steel as an impurity, and since a large amount of N may form a large amount of nitrides such as TiN and AlN, it is advantageous to control the N content as low as possible. Therefore, it is preferable to limit the upper limit of the N content to 0.01%. The N content is more preferably 0.05% or less, and even more preferably 0.03% or less. However, taking into account the case where N is inevitably contained, 0% is excluded (i.e., more than 0%).

[0023] In addition to the above-mentioned steel composition, the remainder may contain Fe and inevitable impurities. Inevitable impurities are those that may be mixed in unintentionally in a normal steel manufacturing process, and cannot be completely excluded. A technician in the field of normal steel manufacturing can easily understand the meaning of this. In addition, the present invention does not completely exclude the addition of compositions other than the above-mentioned steel composition.

[0024] Meanwhile, the cold rolled steel sheet of the present invention may selectively further contain one or two of Cu: 0.1% or less (excluding 0%) and Ni: 0.1% or less (excluding 0%).

[0025] Cu: 0.1% or less (excluding 0%) and Ni: 0.1% or less (excluding 0%) The above copper (Cu) and nickel (Ni) are elements that increase the strength of steel. Although the above elements increase the strength and hardenability of steel, if an excessively large amount is added, the target strength grade may be exceeded, and since these elements are expensive, it is economically disadvantageous. Therefore, the upper limit of each of these elements is preferably 0.1% or less. On the other hand, in order to obtain better solid solution strengthening, the lower limit of each of Cu and Ni may be 0.03%.

[0026] Moreover, the cold-rolled steel sheet of the present invention may selectively further contain V: 0.05% or less (excluding 0%).

[0027] V: 0.05% or less (excluding 0%) Vanadium (V) can increase the strength of steel even in small amounts, but since its effect on improving elongation is not significant, it is preferable to control the vanadium content to 0.05% or less.

[0028] In addition, the cold-rolled steel sheet of the present invention preferably satisfies the above-mentioned alloy composition and also satisfies the following relations 1 and 2. In the following relations 1 and 2, the content of each element means weight %.

[0029] [Relational expression 1] 234×[C]-29×[Si]-128×[Al]+29×[Mn]+10×[Cr]-17×[Mo]-37×[Nb]-49×[Ti]+100×[B]≧80

[0030] If the above-mentioned relational expression 1 is not satisfied, the ferrite fraction to be obtained by the present invention may be excessively formed during annealing, and not only the yield strength but also the hole expandability may be deteriorated. In the above-mentioned relational expression 1, the value of the left side is more preferably 90 or more, and even more preferably 100 or more.

[0031] [Relationship 2] 5 × [C] + [Si] + 0.5 × [Al] ≦ 1.5

[0032] Meanwhile, according to an embodiment of the present invention, the addition of a large amount of alloy elements such as C, Si, and Al deteriorates spot weldability, and in particular, when spot welding is performed on galvanized steel sheets, LME (Liquid Metal Embrittlement) is induced. In general, spot welding of steel materials is performed below the minimum current value at which explosion occurs, and the minimum current value at which explosion occurs can be regarded as a condition that can provide the highest heat input when actually performing spot welding. If the LME resistance is high, LME may not occur even at a welding current value above the minimum current value at which explosion occurs. In this case, the AE value, which is defined as the difference between the minimum current value at which LME occurs and the minimum current value at which explosion occurs, has a positive value. That is, when welding is performed below the minimum current value at which explosion occurs during actual spot welding, if LME does not occur, it can be determined that the AE value is 0 or more. Meanwhile, the AE value has a unit of kA.

[0033] The above-mentioned relational formula 2 is a component relational formula derived from the condition for excellent LME resistance, i.e., the AE value is 0 or more, and if the above-mentioned relational formula 2 is not satisfied, there is a problem of reduced LME resistance. In the above-mentioned relational formula 2, the value on the left side is more preferably 1.25 or less, and even more preferably 1.05 or less.

[0034] The microstructure of the cold-rolled steel sheet according to one embodiment of the present invention is preferably composed of retained austenite: more than 1% and not more than 5%, fresh martensite: 10% or more and less than 25% (excluding 0%), bainite: less than 20%, tempered martensite: 55% or more and less than 80%, and ferrite: 5% or less (including 0%). The fraction of the microstructure described below means area %.

[0035] Retained austenite: over 1% and under 5% Retained austenite is a structure that increases the elongation of steel materials due to the TRIP effect, and the higher the percentage of retained austenite, the higher the elongation can be obtained. In the present invention, in order to obtain the required level of elongation, the percentage of retained austenite is preferably more than 1%. However, in order to obtain more than 5% austenite, a large amount of C and Si must be added, and in this case, the LME resistance of spot welding is deteriorated.

[0036] Fresh martensite: 10% to less than 25% Fresh martensite is an advantageous structure for ensuring strength. If the fraction of fresh martensite is less than 10%, the tensile strength of the steel material is insufficient, while the yield strength may be too high. If the fraction of fresh martensite is 25% or more, the strength is too high, resulting in poor hole expandability.

[0037] Bainite: Less than 20% (excluding 0%) Bainite has a lower strength than martensite, but is an advantageous structure for stabilizing retained austenite. However, if the bainite fraction is 20% or more, the martensite fraction becomes relatively low, which may cause a problem of insufficient strength overall.

[0038] Tempered martensite: 55% to less than 80% Tempered martensite is an advantageous structure for ensuring strength and hole expandability. Tempered martensite is formed when a steel sheet is cooled to below the martensite transformation start point (Ms) during secondary cooling after annealing, and then reheated while undergoing tempering heat treatment. If the tempered martensite fraction is less than 55%, the amount of fresh martensite formed during final cooling is excessively large, and therefore the strength is excessively high and the hole expandability is poor. Also, if the tempered martensite fraction is 80% or more, the fresh martensite fraction is low and strength cannot be obtained.

[0039] Ferrite: 5% or less (including 0%) Ferrite is a structure that adversely affects the yield strength and hole expandability, and theoretically, its fraction is preferably 0%. However, it is sometimes formed unavoidably in the manufacturing process, and if its fraction exceeds 5%, the yield strength is reduced and the hole expandability may also be deteriorated, so in the present invention, the upper limit of the ferrite fraction is limited to 5%.

[0040] The cold-rolled steel sheet of the present invention provided as described above has a tensile strength of 1180 to 1350 MPa, a yield strength of 740 to 980 MPa, an elongation of 8% or more, a hole expandability of 20% or more, and an AE value of 0 kA or more. It is possible to simultaneously ensure excellent strength, ductility, hole expandability, and weldability.

[0041] In addition, the cold-rolled steel sheet of the present invention may have a hot-dip galvanized layer or an alloyed hot-dip galvanized layer formed on at least one surface. The present invention does not particularly limit the configuration of the hot-dip galvanized layer, and any hot-dip galvanized layer that is commonly used in the technical field may be suitably applied to the present invention. In addition, the hot-dip galvanized layer may be an alloyed hot-dip galvanized layer that is alloyed with a part of the alloy components of the steel sheet.

[0042] Hereinafter, a method for producing a cold-rolled steel sheet having excellent weldability, strength and formability according to one embodiment of the present invention will be described.

[0043] First, a slab satisfying the above-mentioned alloy composition and relational expressions 1 and 2 is heated. Although not particularly limited, the heating temperature during the slab heating can be 1150 to 1250°C. If the slab heating temperature is less than 1150°C, the next step of hot rolling may not be performed, while if it exceeds 1250°C, a large amount of energy is wasted to increase the slab temperature. Therefore, the slab heating temperature is preferably in the range of 1150 to 1250°C. The lower limit of the slab heating temperature is more preferably 1170°C, and even more preferably 1180°C. The upper limit of the slab heating temperature is more preferably 1230°C, and even more preferably 1220°C.

[0044] Thereafter, the heated slab is finish hot rolled at 830 to 980°C to obtain a hot-rolled steel sheet. If the finish hot rolling temperature (hereinafter also referred to as "FDT") is less than 830°C, the rolling load is large, shape defects increase, and productivity is reduced. On the other hand, if the finish hot rolling temperature exceeds 980°C, the surface quality is reduced due to an increase in oxides caused by excessive high-temperature work. Therefore, the finish hot rolling temperature is preferably in the range of 830 to 980°C. The lower limit of the finish hot rolling temperature is more preferably 850°C, and even more preferably 880°C. The upper limit of the finish hot rolling temperature is more preferably 950°C, and even more preferably 930°C.

[0045] Thereafter, the hot-rolled steel sheet is coiled at 450 to 700°C. If the coiling temperature (hereinafter also referred to as "CT") exceeds 700°C, there is a drawback that coarse internal oxidation of the hot rolling is caused, and the surface characteristics are deteriorated. On the other hand, if the coiling temperature is less than 450°C, there is a drawback that the coiling temperature falls in the transition boiling region, and controllability of the coiling temperature is deteriorated, and the steel sheet shape is deteriorated. Therefore, the coiling temperature is preferably in the range of 450 to 700°C. The lower limit of the coiling temperature is more preferably 500°C. The upper limit of the coiling temperature is more preferably 650°C, and further preferably 620°C.

[0046] Meanwhile, although not particularly limited, after the finish hot rolling, the steel sheet may be cooled to the coiling temperature at an average cooling rate of 10 to 100°C / s. If the average cooling rate is less than 10°C / s, there are disadvantages in that the productivity of the hot rolling decreases and a cooling medium with a decreased cooling capacity during actual production must be deliberately selected, while if it exceeds 100°C / s, there are disadvantages in that the temperature deviation inside the steel sheet becomes non-uniform, resulting in poor shape and excessive strength of the steel sheet.

[0047] Thereafter, the coiled hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. During the cold rolling, the cold reduction may be 30 to 60%. If the cold reduction is less than 30%, it may be difficult to ensure the target thickness accuracy and it may be difficult to correct the shape of the steel sheet. On the other hand, if the cold reduction exceeds 60%, there is a high possibility that cracks may occur at the edge of the steel sheet, and the cold rolling load may become excessively large.

[0048] Thereafter, the cold steel sheet is subjected to continuous annealing at a temperature of 800 to 840°C. The continuous annealing stage is for forming nearly 100% austenite by heating the steel sheet to the austenite single phase region, for use in the subsequent phase transformation. If the continuous annealing temperature (hereinafter also referred to as "SS") is less than 800°C, sufficient recrystallization and austenite transformation do not occur, and ferrite may be generated at a level exceeding 5% by area. On the other hand, if the continuous annealing temperature exceeds 840°C, productivity decreases, coarse austenite may be formed, and the material may deteriorate, and the surface quality may deteriorate, such as peeling of the plated material. On the other hand, the continuous annealing can be performed in a continuous alloying hot-dip plating continuous furnace.

[0049] Meanwhile, although not particularly limited, during the continuous annealing, the atmosphere in the continuous annealing furnace can be controlled with a gas consisting of, by volume, 95% or more nitrogen and the remainder hydrogen. If the nitrogen fraction is less than 95%, and the hydrogen ratio is not increased accordingly, an oxidizing atmosphere is formed in the furnace, and oxides are formed on the steel sheet surface, deteriorating the surface quality, and if the hydrogen ratio is high, process difficulties such as explosion prevention are aggravated.

[0050] Thereafter, the continuously annealed steel sheet is primarily cooled to a primary cooling end temperature (hereinafter also referred to as "SCS") of 550 to 650°C at an average cooling rate of less than 10°C / s. The primary cooling end temperature can be defined as the point at which the secondary cooling (quenching) is started by further applying a quenching device that was not applied in the primary cooling. When the cooling process is divided into primary and secondary cooling and performed stepwise, the temperature distribution of the steel sheet can be uniformed in the gradual cooling stage, and the final temperature and material variations can be reduced, and a desired phase composition can be obtained. If the primary cooling end temperature exceeds 650°C, the cooling amount until the secondary cooling end temperature becomes large, which may cause the steel sheet shape to deteriorate, and if it is less than 550°C, the load of the gradual cooling process becomes large. If the primary cooling rate is 10°C / s or more, the cooling amount in the secondary cooling becomes large, which increases the final temperature variation and material variation. On the other hand, if the primary cooling rate is less than 1°C / s, a large amount of ferrite phase is formed during cooling, and it may be difficult to obtain the target microstructure and material properties. The lower limit of the primary cooling stop temperature is more preferably 570°C. The upper limit of the primary cooling stop temperature is more preferably 630°C. The primary cooling rate is more preferably in the range of 1°C / s or more and less than 10°C / s.

[0051] Thereafter, the steel sheet subjected to the primary cooling is secondarily cooled to a secondary cooling end temperature (hereinafter also referred to as "RCS") of 320 to 360°C at an average cooling rate of 10°C / s or more. The secondary cooling end temperature is set to be equal to or lower than the Ms temperature of the steel sheet so that martensite transformation occurs during cooling, and this martensite finally becomes tempered martensite after a subsequent reheating step. Since the Ms temperature of 1180 MPa-class high elongation steel sheet is almost at a level of 400°C or lower, in the present invention, the secondary cooling end temperature is controlled to a range of 320 to 360°C. If the secondary cooling end temperature is less than 320°C, the amount of initial martensite transformation becomes too large, resulting in high yield strength, and thus poor formability. On the other hand, if the secondary cooling end temperature exceeds 360°C, tempered martensite is not generated, and the fraction of brittle fresh martensite increases, resulting in poor yield strength and hole expandability. If the secondary cooling rate is less than 10°C / s, high-temperature phase transformation occurs during cooling even if the target secondary cooling end temperature is reached, and the target martensite fraction and high strength cannot be obtained. The lower limit of the secondary cooling stop temperature is more preferably 330°C. The upper limit of the secondary cooling stop temperature is more preferably 350°C.

[0052] Meanwhile, as described above, the secondary cooling can further apply a quenching equipment that was not applied in the primary cooling, and the present invention does not particularly limit the type of the quenching equipment, but a preferred example is a hydrogen quenching equipment. More specifically, the hydrogen quenching equipment can use a gas consisting of 5 to 80% hydrogen by volume and the remainder nitrogen. If the hydrogen fraction exceeds 80%, there is a drawback that it becomes difficult to manage the equipment, such as explosion control, and if it is less than 5%, there is a drawback that it becomes difficult to utilize the efficient heat transfer characteristics of hydrogen, which is a light element.

[0053] Thereafter, the second-cooled steel sheet is reheated to a temperature range of 380 to 480°C. Through the above process, interphase carbon partitioning and additional bainite phase transformation necessary for stabilizing the retained austenite are obtained. In the present invention, the end temperature of the heating section is conveniently referred to as the reheating temperature (hereinafter also referred to as "RHS"). If the reheating temperature is less than 380°C, the strength becomes too high and the elongation rate becomes poor. On the other hand, if the reheating temperature exceeds 480°C, the austenite phase remains without being transformed, and the fraction of fresh martensite that transforms during final cooling becomes high, thereby impairing the hole expandability and elongation rate. On the other hand, the temperature at which the transformation of bainite is most active, the so-called nose temperature, is about 400 to 420°C, and in consideration of this, it is more preferable to maintain the reheating temperature in the range of 400 to 420°C.

[0054] Meanwhile, although not particularly limited, the average heating rate during the reheating may be 0.5 to 2.5° C. / s. If the average heating rate is less than 0.5° C. / s, the overall process time may become too long, which may cause a problem of excessive heat treatment, and if it exceeds 2.5° C. / s, it is difficult to ensure the physical properties aimed at in the present invention.

[0055] According to an embodiment of the present invention, after the reheating step, the cold rolled steel sheet may be further subjected to a process of hot-dip galvanizing, galvannealing, or skin pass rolling, if necessary.

[0056] Specifically, the method may further include a step of hot-dip galvanizing the reheated cold-rolled steel sheet in a galvanizing bath at 450 to 470°C. In addition, if necessary, the method may further include a step of subjecting the hot-dip galvanized cold-rolled steel sheet to alloying heat treatment at 470 to 550°C. The alloying heat treatment is for obtaining an appropriate alloying level, and the temperature is determined depending on the surface state of the steel sheet. By controlling the surface state of the steel material, the alloying heat treatment temperature does not exceed 550°C, thereby preventing the softening of the steel sheet and the disappearance of the retained austenite due to excessive tempering. Meanwhile, in order to rapidly advance the alloying, the alloying heat treatment temperature is preferably higher than the hot-dip galvanizing temperature, and therefore the lower limit thereof can be controlled to 470°C. In addition, after the alloying heat treatment, the method may further include a step of cooling the alloyed heat-treated cold-rolled steel sheet to room temperature and then temper rolling it at a rolling reduction of less than 1% in order to correct the shape of the steel sheet and adjust the yield strength. EXAMPLES

[0057] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are intended to illustrate and embody the present invention, and are not intended to limit the scope of the present invention, since the scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.

[0058] (Example) A slab having the alloy composition shown in Table 1 below was prepared, and then reheated at 1180 to 1220°C, and hot rolling, coiling, annealing, primary cooling, secondary cooling, and reheating were performed under the conditions shown in Table 2 below to produce a cold-rolled steel sheet. At this time, the cooling rate after finish hot rolling was 30 to 50°C / s, the cold reduction was 33 to 55%, the gas used during continuous annealing was 95 vol% N-5 vol% H, and the gas used during secondary cooling was 75 vol% H-25 vol% N.

[0059] The microstructure and mechanical properties of the cold rolled steel sheets thus produced were measured, and the results are shown in Table 3 below.

[0060] The microstructure was measured by the point counting method from scanning electron microscope (SEM) photographs, and the fraction of retained austenite was measured by XRD.

[0061] Among the mechanical properties, yield strength (YS), tensile strength (TS) and elongation (EL) were measured by tensile tests in the direction perpendicular to the rolling direction, and the gauge length was 50 mm and the width of the tensile test specimen was 25 mm.

[0062] Among the mechanical properties, the hole expansion rate (HER) was measured according to the ISO 16330 standard, and the holes were sheared using a 10 mm diameter punch with a clearance of 12%.

[0063] On the other hand, the above cold-rolled steel sheets were subjected to hot-dip galvanizing (GI) under the conditions shown in Table 2 below, and some steel types were subjected to galvannealing (GA) and spot welding to measure the AE value, and the results are shown in Table 3 below. The above AE value means the value obtained by subtracting the minimum current value at which LME occurs from the minimum current value at which scattering occurs. In the above spot welding test, the current was increased in 0.5 kA increments from a low current value, and a cooling time was given between each current value to prevent excessive heat from being input to the material. In this way, the current value was increased, and the minimum current value at which the weld nugget exploded was measured, and at the same time, the minimum current value at which LME occurs was measured from the surface and cross section of the weld, and the results are shown in Table 3 below. Regarding the occurrence of LME, when the surface of the weld was observed at 10 times and the cross section at 100 times, if no cracks due to LME were observed, it was evaluated as pass, and if they were observed, it was evaluated as fail.

[0064] In addition, a 10 mm diameter hole was made in the above cold-rolled steel sheet with a punch at a clearance of 12%, and the sheet was immersed in a 0.1 normal concentration hydrochloric acid solution for corrosion for 100 hours, after which the occurrence of hydrogen embrittlement cracks in the punched area was evaluated.

[0065] [Table 1]

[0066] [Table 2]

[0067] [Table 3]

[0068] As shown in Tables 1 to 3 above, in the case of Examples 1 to 4, which satisfy the alloy composition proposed by the present invention, Relational Formulas 1 and 2, and the manufacturing conditions, not only do they have a tensile strength of 1180 to 1350 MPa, a yield strength of 740 to 980 MPa, an elongation of 8% or more, and a hole expandability of 20% or more, but they also have excellent LME properties.

[0069] In contrast, in the case of Comparative Examples 1 and 2, although the alloy composition and Relational Formulas 1 and 2 of the present invention are satisfied, the secondary cooling end temperature is outside the range of the present invention, and therefore the microstructure that the present invention aims to obtain cannot be secured, and the yield strength is too high or the hole expandability is low at less than 20%, resulting in poor formability.

[0070] In the case of Comparative Examples 3 and 4, although the manufacturing conditions of the present invention are satisfied, the alloy composition of the present invention and Relational Formula 1 are not satisfied, and therefore the fine structure that the present invention aims to obtain cannot be secured, and the mechanical properties are inferior.

[0071] It is clear that Comparative Examples 5 and 6, although they satisfy the production conditions of the present invention, do not satisfy the alloy composition and Relational Formula 2 of the present invention, and therefore have inferior LME properties.

[0072] In particular, in the cases of Comparative Examples 4, 5 and 6, it is clear that hydrogen embrittlement cracks occurred due to the addition of excessive Cr.

Claims

1. In weight percent, C: 0.14-0.16%, Si: 0.3-0.6%, Al: 0.01-0.3%, Mn: 2.6-3.0%, Cr: 0.01-0.25%, Mo: 0.15-0.4%, B: 0.0001-0.005%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, P: 0.04% or less (excluding 0%), S: 0.01% or less (excluding 0%), N: 0.01% or less (excluding 0%), the balance being Fe and other unavoidable impurities. The following relations 1 and 2 are satisfied, The microstructure of this cold-rolled steel sheet is composed of retained austenite: more than 1% and less than 5%, fresh martensite: 10% to less than 25%, bainite: less than 20% (excluding 0%), tempered martensite: 55% to less than 80%, and ferrite: 5% or less (including 0%). [Relational expression 1] 234×[C]-29×[Si]-128×[Al]+29×[Mn]+10×[Cr]-17×[Mo]-37×[Nb]-49×[Ti]+100×[B]≧80 [Relationship 2] 5 × [C] + [Si] + 0.5 × [Al] ≦ 1.5 (However, in the above Relational Formulas 1 and 2, the content of each element means weight percent.)

2. The cold-rolled steel sheet according to claim 1, further comprising one or two of Cu: 0.1% or less (excluding 0%) and Ni: 0.1% or less (excluding 0%).

3. The cold-rolled steel sheet according to claim 1, further comprising V: 0.05% or less (excluding 0%).

4. The cold-rolled steel sheet has a tensile strength of 1180 to 1350 MPa, a yield strength of 740 to 980 MPa, an elongation of 8% or more, a hole expandability of 20% or more, and an AE value of 0 kA or more. The cold-rolled steel sheet according to claim 1. (Note that the AE value means the difference obtained by subtracting the minimum current value at which scattering occurs from the minimum current value at which LME occurs.)

5. The cold-rolled steel sheet according to claim 1 , wherein the cold-rolled steel sheet has at least one surface on which a hot-dip galvanized layer or a hot-dip galvannealed layer is formed.

6. a step of heating a slab containing, by weight percent, C: 0.14-0.16%, Si: 0.3-0.6%, Al: 0.01-0.3%, Mn: 2.6-3.0%, Cr: 0.01-0.25%, Mo: 0.15-0.4%, B: 0.0001-0.005%, Nb: 0.001-0.05%, Ti: 0.001-0.05%, P: 0.04% or less (excluding 0%), S: 0.01% or less (excluding 0%), N: 0.01% or less (excluding 0%), the balance being Fe and other inevitable impurities, and satisfying the following relational expressions 1 and 2; Finish hot rolling the heated slab at 830 to 980°C to obtain a hot-rolled steel sheet; coiling the hot-rolled steel sheet at 450 to 700°C; cold rolling the coiled hot-rolled steel sheet to obtain a cold-rolled steel sheet; continuous annealing the cold steel sheet at a temperature of 800 to 840°C; subjecting the continuously annealed steel sheet to a primary cooling end temperature of 550 to 650° C. at an average cooling rate of less than 10° C. / s; Secondarily cooling the primarily cooled steel sheet to a secondary cooling end temperature of 320 to 360° C. at an average cooling rate of 10° C. / s or more; and reheating the second-cooled steel sheet to a temperature in the range of 380 to 480°C. [Relational expression 1] 234×[C]-29×[Si]-128×[Al]+29×[Mn]+10×[Cr]-17×[Mo]-37×[Nb]-49×[Ti]+100×[B]≧80 [Relationship 2] 5 × [C] + [Si] + 0.5 × [Al] ≦ 1.5 (However, in the above Relational Formulas 1 and 2, the content of each element means weight percent.)

7. The method for producing a cold-rolled steel sheet according to claim 6, wherein the slab further contains one or two of Cu: 0.1% or less (excluding 0%) and Ni: 0.1% or less (excluding 0%).

8. The method for producing a cold-rolled steel sheet according to claim 6, wherein the slab further contains V: 0.05% or less (excluding 0%).

9. The method for producing a cold-rolled steel sheet according to claim 6, wherein the heating temperature during the slab heating is 1150 to 1250°C.

10. The method for producing a cold-rolled steel sheet according to claim 6, wherein after the finish hot rolling, the steel sheet is cooled to a coiling temperature at an average cooling rate of 10 to 100 ° C. / s.

11. The method for producing a cold-rolled steel sheet according to claim 6, wherein the cold rolling reduction rate is 30 to 60%.

12. The method for producing a cold-rolled steel sheet according to claim 6, wherein during the continuous annealing, an atmosphere in a continuous annealing furnace is controlled with a gas consisting of, by volume%, 95% or more nitrogen and the remainder hydrogen.

13. The method for producing a cold-rolled steel sheet according to claim 6, wherein a gas consisting of 5 to 80% by volume of hydrogen and the remainder nitrogen is used during the secondary cooling.

14. The method for producing a cold-rolled steel sheet according to claim 6, wherein an average heating rate during the reheating is 0.5 to 2.5 ° C. / s.

15. The method for producing a cold-rolled steel sheet according to claim 6, further comprising the step of hot-dip galvanizing the cold-rolled steel sheet in a galvanizing bath at 450 to 470°C after the reheating step.

16. The method for producing a cold-rolled steel sheet according to claim 15, further comprising the step of subjecting the cold-rolled steel sheet to an alloying heat treatment at 470 to 550° C. after the hot-dip galvanizing step.

17. The method for producing a cold-rolled steel sheet according to claim 16, further comprising the step of cooling the cold-rolled steel sheet to room temperature after the alloying heat treatment, and then temper rolling the cold-rolled steel sheet at a reduction rate of less than 1%.

Citation Information

Patent Citations

  • High-broaching-property DH1180MPa cold-rolled continuously-annealed steel plate and preparation method thereof

    CN113403545A

  • High-strength cold-rolled steel sheet superior in hole expandability, and manufacturing method therefor

    JP2007177272A

  • High-strength steel sheet, and method of producing the same

    JP2013072101A

  • Hot-dip galvanized steel sheet and method for manufacturing the same

    JP2013108154A

  • Ultrahigh strength cold rolled steel sheet excellent in hydrogen embrittlement resistance and manufacturing method therefor

    JP2016050343A

Cited By

  • Cold-rolled steel sheet having excellent strength and formability and method for manufacturing the same

    JP2025539781A