Polyethylene yarn having improved dimensional stability and functional fabric containing the same
A polyethylene yarn with optimized melt index and molecular properties addresses the processing challenges of low molecular weight yarns and high molecular weight yarns, achieving enhanced dimensional stability and thermal conductivity for functional fabrics.
Patent Information
- Application Number
- JP2024534278
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-08
- Filing Date
- 2022-12-06
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Low molecular weight polyethylene yarns suffer from low strength, high elongation, and poor dimensional stability during post-processing such as weaving and knitting, making them unsuitable for various applications, while high molecular weight yarns are difficult to process due to low melt flowability and require solvent dilution, complicating the manufacturing process.
A polyethylene yarn with a melt index of 5 to 25 g/10 min, maximum thermal shrinkage stress of 0.1 to 0.7 g/d, and specific molecular weight and crystallinity ranges is developed, allowing for improved dimensional stability and thermal conductivity without solvent dilution, enabling efficient spinning and post-processing.
The yarn exhibits excellent dimensional stability and thermal conductivity, maintaining shape integrity during processing and providing a cooling sensation, suitable for functional fabrics with improved durability and comfort.
Smart Images

Figure 2024544235000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyethylene raw yarn having improved dimensional stability and a functional fabric containing the same, and more particularly to a polyethylene raw yarn having improved dimensional stability and exhibiting a small dimensional deformation rate during post-processing such as weaving and cutting, and a functional fabric containing the same. [Background technology]
[0002] Recently, due to the improvement of living standards and population growth, the demand for textiles has been shifting from general-purpose yarns for general clothing and industrial fibers to advanced textile materials with high functionality and performance and various functions. In particular, the development of textile materials with a cooling sensation that gives users a comfortable feeling in summer and in high-temperature working environments is actively underway.
[0003] Cool-sensation fiber materials are imparted with a cool sensation by utilizing the thermal conductivity of the fiber itself, or by adjusting the thermal conductivity of the surface of the fiber material through coating with a metal component having high thermal conductivity, etc. In particular, cool-sensation fiber materials that utilize the thermal conductivity of the fiber itself can be manufactured only through the weaving process of the fabric, and can maintain a cool sensation even after washing, so they are currently being produced in a variety of industrial fields.
[0004] Conventionally, as disclosed in Japanese Patent Publication JP2010-236130A and Korean Patent Publication No. 10-2017-0135342, there have been various attempts to apply the excellent thermal conductivity of high molecular weight polyethylene (HMWPE) fibers to fashion clothing and technical textile fields that require a high cooling sensation, such as sportswear, mountain climbing clothing, and workwear.
[0005] However, such cool-sensing polyethylene raw yarn has a drawback in that it is difficult to manufacture due to the low melt flowability of the raw material when it is manufactured as raw yarn, since it contains high-viscosity high-molecular-weight polyethylene. Therefore, in order to improve the melt flowability of the raw material, the raw material containing high-viscosity high-molecular-weight polyethylene is diluted with a solvent to produce the raw yarn, but this causes additional problems such as a complicated process and difficulty in managing and recovering the solvent.
[0006] Meanwhile, compared to high-viscosity high-molecular-weight polyethylene fibers, low-viscosity low-molecular-weight polyethylene fibers have the disadvantage of being disadvantageous in post-processing such as weaving, knitting, and heat treatment due to their low strength, high elongation, and low dimensional stability. Therefore, low-molecular-weight polyethylene fibers have low industrial applicability compared to high-molecular-weight polyethylene fibers, and cannot be used for various applications. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a polyethylene raw yarn having a small dimensional deformation rate and improved dimensional stability during post-processing such as weaving and cutting, and a functional fabric containing the same that can provide a cooling sensation to the user. [Means for solving the problem]
[0008] The polyethylene raw yarn according to the present invention has a maximum thermal shrinkage stress of 0.1 to 0.7 g / d and a melt index (MI, @190° C.) of 5 to 25 g / 10 min.
[0009] In the polyethylene raw yarn according to one embodiment of the present invention, the raw yarn may have a polydispersity index (PDI) of 5 to 20 and a number average molecular weight (Mn) of 1,000 to 10,000 g / mol.
[0010] In the polyethylene yarn according to one embodiment of the present invention, the yarn may have a tenacity of 6 to 17 g / d and an elongation of 10 to 25%, as measured by ASTM D2256.
[0011] In the polyethylene yarn according to one embodiment of the present invention, the yarn may have a crystallinity of 65 to 85%.
[0012] In one embodiment of the present invention, the polyethylene yarn has a density of 0.92 to 0.97 g / cm 3 may be also possible.
[0013] The functional fabric according to the present invention comprises the polyethylene raw yarn described above.
[0014] In the functional fabric according to an embodiment of the present invention, the fabric has a cool touch sensation of 0.05 to 0.25 W / cm, measured at 20±2°C and 65±2% RH by contacting a 30±2°C hot plate (T-box) with the fabric at 20±2°C. 2 It could be.
[0015] In the functional fabric according to an embodiment of the present invention, the fabric may have a thickness direction thermal conductivity of 0.05 to 0.25 W / mK, measured at 20±2° C. and 65±2% RH by contacting a heat source plate (BT-box) at 30±2° C. with the fabric at 20±2° C.
[0016] In one embodiment of the functional fabric according to the present invention, the fabric has a surface density of 150 to 800 g / m 2 may be also possible.
[0017] The cooling sensation product according to the present invention is produced from the above-mentioned fabric. Effect of the Invention
[0018] The polyethylene yarn according to the present invention has excellent dimensional stability and excellent thermal conductivity, even though it is a low molecular weight polyethylene yarn.
[0019] In addition, the functional fabric according to the present invention contains polyethylene yarn having excellent thermal conductivity and high dimensional stability, so that it has a cool feeling and is prevented from deforming during post-processing, thereby providing excellent quality. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic diagram showing a polyethylene yarn manufacturing apparatus. [Diagram 2] FIG. 1 is a schematic diagram showing an apparatus for measuring the cool contact sensation of fabric. [Diagram 3] FIG. 1 is a schematic diagram showing an apparatus for measuring thermal conductivity in the thickness direction of a fabric. [Figure 4] 1 is a graph showing the heat shrinkage stress of the fabric according to Example 1. [Diagram 5] 1 is a graph showing the heat shrinkage stress of the fabric according to Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Unless otherwise defined, technical and scientific terms used in this specification have the meanings that are commonly understood by those with ordinary knowledge in the technical field to which this invention belongs, and descriptions of known functions and configurations that may unnecessarily obscure the gist of the present invention in the following description and the attached drawings will be omitted.
[0022] Also, as used herein, the singular forms "a," "an," and "the" can be intended to include the plural forms as well, unless the context indicates otherwise.
[0023] Furthermore, units used in this specification, unless otherwise specified, are based on weight, and for example, the unit of % or ratio means % by weight or weight ratio, and unless otherwise defined, % by weight means the weight % of any one component in a total composition.
[0024] In addition, the numerical ranges used herein include the lower limit and the upper limit, and all values within the range, logically derived increments in the form and width of the range defined, all values limited therein, and all possible combinations of upper and lower limits for numerical ranges limited in different forms. Unless otherwise specified in the specification of the present invention, values outside the numerical range that may occur due to experimental error or rounding of values are also included in the defined numerical range.
[0025] As used herein, the term 'comprising' is an open-ended term having the same meaning as terms such as 'comprising,' 'containing,' 'having,' or 'characterized by,' and does not exclude additional, unrecited elements, materials, or steps.
[0026] Conventional cool-sensation polyethylene yarn contains high-viscosity high molecular weight polyethylene, and therefore has a drawback in that it is difficult to manufacture the yarn due to the low melt flowability of the raw material. Therefore, in order to improve the melt flowability of the polyethylene yarn raw material, the raw material containing high-viscosity high molecular weight polyethylene is diluted with a solvent to produce the yarn, but this causes additional problems such as a complicated process and difficulty in managing and recovering the solvent.
[0027] Meanwhile, compared to high-viscosity high-molecular-weight polyethylene raw yarn, low-viscosity low-molecular-weight polyethylene raw yarn has the disadvantage of being disadvantageous in post-processing such as weaving, knitting, and heat treatment due to its low strength, high elongation, and low dimensional stability. Therefore, low-molecular-weight polyethylene raw yarn has low industrial applicability compared to high-molecular-weight polyethylene raw yarn, and is not used for various purposes.
[0028] Therefore, the applicant has developed a polyethylene raw yarn that contains a low-viscosity low-molecular-weight polyethylene but has high dimensional stability, and thus can easily undergo a spinning process due to the inherent high melt flow properties of polyethylene without the need for dilution with a separate solvent. The applicant has also developed a polyethylene raw yarn that has excellent dimensional stability and mechanical properties and has small dimensional deformation during post-processing such as weaving, cutting and dyeing.
[0029] In this specification, polyethylene raw yarn refers to monofilament or multifilament manufactured by using polyethylene chips as raw material through processes such as spinning and drawing. As an example, the polyethylene fiber may include 40 to 500 filaments each having a fineness of 1 to 3 denier, and may have a total fineness of 100 to 1,000 denier.
[0030] The polyethylene yarn of the present invention has a maximum thermal shrinkage stress of 0.1 to 0.7 g / d and a melt index (MI, @190°C) of 5 to 10 g / 10 min, and has an excellent heat shrinkage rate, i.e., excellent dimensional stability, despite containing a low-viscosity, low-molecular-weight polyethylene. Therefore, unlike when containing a high-viscosity, high-molecular-weight polyethylene, there is no need to dilute with a separate solvent during the spinning process, simplifying the process, resulting in very high yarn productivity, and excellent thermal conductivity without deformation during post-processing such as weaving and twisting. In addition, due to its excellent thermal conductivity and dimensional stability, it can be manufactured into a fabric with excellent physical properties such as a cool feeling.
[0031] The dimensional stability of the polyethylene yarn according to the present invention is a property of resisting dimensional deformation caused by heat, pressure, tension, etc., when the yarn is subjected to post-processing such as weaving or knitting into a fabric, and may also mean shape stability. The higher the dimensional stability, the smaller the dimensional deformation rate during post-processing.
[0032] The cool sensation of the fabric containing the polyethylene yarn according to the present invention is a characteristic that allows the user wearing the fabric to feel an appropriate cool sensation, i.e., a cooling feeling, due to the high thermal conductivity of the yarn. Specifically, in the case of polymers, heat is transferred within the polymer (especially in the direction of molecular chains connected through covalent bonds) mainly through lattice vibrations called phonons. In other words, the thermal conductivity of the yarn can be adjusted to be different depending on the structural characteristics of the polymer itself, such as the degree of crystallinity and orientation of the yarn, even if the yarn is made from the same resin.
[0033] As described above, the polyethylene raw yarn may have a maximum heat shrinkage stress of 0.1 to 0.7 g / d, specifically 0.2 to 0.5 g / d, and a melt index (MI, @190°C) of 5 to 25 g / 10 min, specifically 6 to 15 g / 10 min, but is not limited thereto. However, within the above range, it may have better dimensional stability and thermal conductivity. In addition, such polyethylene raw yarn has a low viscosity when melted, and can be spun without a separate solvent in the spinning process, resulting in excellent spinning efficiency.
[0034] In particular, the polyethylene raw yarn may contain low molecular weight polyethylene, and may have a polydispersity index (PDI) of 5 to 20, specifically 8 to 18, more specifically 10 to 15, and a number average molecular weight (Mn) of 1000 to 10,000 g / mol, specifically 2000 to 5000 g / mol. A polyethylene raw yarn having a polydispersity index and a number average molecular weight in the above range has good melt flowability during melt extrusion of the raw yarn, prevents thermal decomposition, and ensures processability such as no yarn breakage during drawing, and can produce a raw yarn with uniform physical properties and provide a raw yarn with excellent durability. At this time, the weight average molecular weight is not limited as long as it satisfies the above PDI value for the above number average molecular weight, but may have a weight average molecular weight lower than that of a normal polyethylene raw yarn for cooling sensation. Specifically, it may be 20,000 to 90,000 g / mol, more specifically 35,000 to 75,000 g / mol.
[0035] In addition, the density of polyethylene yarn is 0.92 to 0.97 g / cm 3 The crystallinity of the polyethylene raw yarn may be 60-90%, specifically 65-85%, during spinning. The crystallinity of the polyethylene raw yarn may be determined together with the size of the crystallites during crystallinity analysis using an X-ray diffraction analyzer. As described above, when the crystallinity satisfies the above range, heat is rapidly diffused and dissipated through lattice vibrations called 'phonons' in the direction of the molecular chains linked through the covalent bonds of the polyethylene, and the function of discharging moisture such as sweat and breath is improved, providing a fabric with excellent cooling sensation.
[0036] The polyethylene yarn may have a strength of 6 to 17 g / d, specifically 10 to 15 g / d, and an elongation of 10 to 25%, specifically 12 to 20%, as measured by ASTM D2256. The polyethylene yarn having the strength and elongation within the above ranges has not only excellent thermal conductivity, but also relatively high flexibility and excellent weaving properties, so that when it is later woven into a fabric, a fabric of better quality can be obtained.
[0037] Hereinafter, a method for producing a polyethylene raw yarn according to one embodiment of the present invention will be described in detail with reference to Fig. 1. The polyethylene raw yarn of the present invention is not limited in its production method as long as it satisfies the above-mentioned ranges of physical properties such as PDI, strength, and elongation, and the following will describe one embodiment.
[0038] First, polyethylene in chip form is fed into an extruder 100 and melted to obtain a polyethylene melt.
[0039] Molten polyethylene is transported through the die 100 by a screw (not shown) in the extruder 100, and is extruded through a number of holes formed in the die 200. The number of holes in the die 200 may be determined depending on the DPF (Denier Per Filament) and fineness of the raw yarn to be produced. For example, when producing a raw yarn having a total fineness of 75 denier, the die 200 may have 20 to 75 holes, and when producing a raw yarn having a total fineness of 450 denier, the die 200 may have 90 to 450 holes, preferably 100 to 400 holes.
[0040] The melting process in the extruder 100 and the extrusion process through the die 200 can be changed and applied depending on the melt index of the polyethylene chips, but specifically, for example, they are preferably performed at 150 to 315°C, preferably 250 to 315°C, and more preferably 265 to 310°C. That is, it is preferable that the extruder 100 and the die 200 are maintained at 150 to 315°C, preferably 250 to 315°C, and more preferably 265 to 310°C.
[0041] If the spinning temperature is less than 150° C., the polyethylene may not be uniformly melted due to the low spinning temperature, making spinning difficult, whereas if the spinning temperature exceeds 315° C., the polyethylene may be thermally decomposed, making it difficult to achieve the desired strength.
[0042] The ratio L / D, which is the ratio of the hole length L to the hole diameter D in the spinneret 200, may be 3 to 40. If L / D is less than 3, a die swell phenomenon occurs during melt extrusion, making it difficult to control the elastic behavior of the polyethylene, resulting in poor spinnability, and if L / D exceeds 40, thread breakage due to necking of the molten polyethylene passing through the spinneret 200 and non-uniform extrusion due to pressure drop may occur.
[0043] As the molten polyethylene is discharged from the holes of the spinneret 200, the polyethylene begins to solidify due to the difference between the spinning temperature and room temperature, forming a semi-solidified filament 11. In this specification, both the semi-solidified filament and the completely solidified filament are collectively referred to as "filament."
[0044] The filaments 11 are completely solidified by being cooled in a cooling section (or "quenching zone") 300. The filaments 11 can be cooled by air cooling.
[0045] The cooling of the filaments 11 in the cooling unit 300 is preferably performed by cooling the filaments 11 to 15 to 40° C. using cooling air having a speed of 0.2 to 1 m / sec. If the cooling temperature is less than 15° C., the filaments 11 may be overcooled, leading to insufficient elongation and thus yarn breakage during drawing, whereas if the cooling temperature exceeds 40° C., the filaments 11 may be solidified non-uniformly, leading to a large deviation in fineness and yarn breakage during drawing.
[0046] In addition, when cooling in the cooling section, multi-stage cooling can be performed to allow more uniform crystallization, which allows for smoother discharge of moisture and sweat and allows for the production of raw yarn with excellent cool sensation. More specifically, the cooling section may be divided into two or more sections. For example, when it is composed of two cooling sections, it is preferable that the temperature is designed to be gradually lower from the first cooling section to the second cooling section. Specifically, for example, the first cooling section may be set to 40 to 90°C, and the second cooling section may be set to 15 to 50°C.
[0047] Also, by setting the wind speed in the first cooling section to the highest, it is possible to produce fibers with a smoother surface. Specifically, the first cooling section may use cooling wind with a wind speed of 0.8 to 1.2 m / sec to cool to 40 to 90°C, and the second cooling section may use cooling wind with a wind speed of 0.3 to 1.0 m / sec to cool to 15 to 50°C. By adjusting the conditions in this way, it is possible to produce raw yarn with a higher crystallinity and a smoother surface.
[0048] Next, the cooled and completely solidified filaments 11 are bundled in a bundler 400 to form a multifilament 10.
[0049] As illustrated in Fig. 1, the polyethylene raw yarn of the present invention can be manufactured through a direct spin-draw (DSD) process. That is, the multifilament 10 is directly transferred to a multi-stage drawing section 500 including a plurality of godet roller sections GR1...GRn, where it is multi-stage drawn at a total draw ratio of 2 to 20 times, preferably 3 to 15 times, and then wound up by a winder 600. In addition, during the multi-stage drawing, a shrinkage drawing (relaxation) of 1 to 5% is imparted in the final drawing section, thereby providing a raw yarn with better durability.
[0050] Alternatively, the polyethylene raw yarn of the present invention can be produced by once winding the multifilament 10 as an undrawn yarn and then drawing the undrawn yarn. That is, the polyethylene raw yarn of the present invention can be produced through a two-step process of once producing an undrawn yarn by melt spinning polyethylene and then drawing the undrawn yarn.
[0051] If the total draw ratio applied in the drawing process is less than 2, the final polyethylene raw yarn cannot have a crystallinity of 60% or more, and there is a risk of feathering (filling) being induced on the fabric made from the raw yarn.
[0052] On the other hand, if the total draw ratio exceeds 15 times, yarn breakage may occur, and the strength of the finally obtained polyethylene raw yarn may not be adequate, resulting in poor weaving properties of the polyethylene raw yarn and the fabric produced using the same may be too stiff, causing inconvenience to users.
[0053] Once the linear speed of the first godet roller unit GR1, which determines the spinning speed of the melt spinning of the present invention, is determined, the linear speeds of the remaining godet roller units are appropriately determined so that a total draw ratio of 2 to 20, preferably 3 to 15, is applied to the multifilament 10 in the multi-stage drawing unit 500.
[0054] According to an embodiment of the present invention, the heat-setting of the polyethylene raw yarn is performed through the multi-stage drawing section 500 by appropriately setting the temperature of the godet roller units GR1...GRn of the multi-stage drawing section 500 in the range of 40 to 140°C. Specifically, for example, the multi-stage drawing section may be composed of three or more, specifically, three to five, drawing sections. Also, each drawing section may be composed of a plurality of godet roller units.
[0055] Specifically, for example, the multi-stage drawing section may include four drawing sections, in which the fiber is drawn to a total draw ratio of 7 to 15 times in the first to third drawing sections, and then contracted and drawn (relaxed) by 1 to 3% in the fourth drawing section. The total draw ratio refers to the final draw ratio of the fiber after the first to third drawing sections compared to the fiber before drawing.
[0056] More specifically, the first stretching section may be performed at 40 to 120°C and the total stretch ratio may be 2 to 5 times. The second stretching section may be performed at a higher temperature than the first stretching section, specifically at 90 to 140°C, and stretching may be performed to a total stretch ratio of 5 to 8 times. The third stretching section may be performed at 90 to 140°C and stretching may be performed to a total stretch ratio of 7 to 15 times. The fourth stretching section may be performed at the same or lower temperature as the third stretching section, specifically at 90 to 140°C, and stretching (relaxation) may be performed by shrinking and stretching by 1 to 3%.
[0057] The multistage drawing section 500 simultaneously performs multistage drawing and heat setting of the multifilament 10, and the multistage drawn multifilament 10 is wound by a winder 600 to complete the polyethylene raw yarn of the present invention.
[0058] The functional fabric according to the present invention contains the above-mentioned polyethylene yarn, and by containing the polyethylene yarn having excellent thermal conductivity and high dimensional stability, it can have a cooling sensation property and at the same time excellent quality.
[0059] The functional fabric according to the present invention may use the polyethylene yarn described above alone, or may further contain a different type of yarn to impart other functionality. However, from the viewpoint of simultaneously having a cool sensation and dimensional stability, it is preferable to use the polyethylene yarn alone.
[0060] Specifically, the functional fabric can have excellent cool sensation by including the above-mentioned raw yarn. In detail, the cool sensation measured by contacting a 20±2°C fabric with a 30±2°C hot plate (T-box) at 20±2°C and 65±2% RH is 0.05 to 0.25 W / cm 2 The thermal conductivity in the thickness direction measured by contacting a heat source plate (BT-box) of 30±2°C with a material of 20±2°C at 20±2°C and 65±2% RH can be 0.05~0.25W / mK. More specifically, the cool feeling to the touch is 0.07~0.20W / cm 2 The thermal conductivity in the thickness direction may be 0.07~0.20W / mK. When the functional fabric having such a cooling sensation is manufactured or processed into a product and worn by a user, it can provide an appropriate cooling sensation that allows the user to feel comfortable in a high temperature environment.
[0061] In addition, the functional fabric can have excellent dimensional stability by including the polyethylene yarn. Specifically, when the functional fabric is manufactured by weaving or knitting using the polyethylene yarn, the dimensional deformation rate of the final fabric is almost zero compared to the designed dimensions, so that there are almost no defective products and the fabric can have excellent quality.
[0062] In addition, the functional fabric can have excellent dimensional stability even under harsh conditions at high temperatures by containing raw yarn having a specific heat shrinkage stress as described above. Specifically, under conditions of 90±2°C and 65±2% RH, the dimensional deformation rate of the fabric expressed by the following formula 1 can be -2.0% to 2.0%, preferably -1.8% to 1.8%, and more preferably -1.5% to 1.5%.
[0063] [Formula 1] Dimensional deformation rate (%) = {(FS1-FS0) / (FS0)} x 100
[0064] (In the above formula, FS0 is the dimension (mm) of the functional fabric measured after leaving it at room temperature (20±2°C, 65±2% RH) for 24 hours, and FS1 is the dimension (mm) of the functional fabric measured after leaving it at 90±2°C, 65±2% RH for 24 hours.)
[0065] In this way, functional fabrics have excellent dimensional stability even under harsh conditions, and therefore can have excellent post-processability because dimensional stability is ensured during post-processing where various external forces such as heat and pressure are applied.
[0066] In addition, functional fabrics are available in sizes from 150 to 800 g / m 2 The fabric may be a woven or knitted fabric having a weight per unit area (i.e., areal density) of 150 g / m 2 If the surface density of the fabric is less than 800g / m, the fabric will not be dense enough and many voids will exist in the fabric, which will reduce the cooling sensation of the fabric. 2 If it exceeds this value, the fabric will be too dense in structure, causing problems with the feel felt by the user, and the high weight will cause problems in use.
[0067] Such fabrics can be processed into cooling products that require appropriate cooling sensation. The products can be any conventional textile products, but preferably can be summer clothes, sportswear, masks, and work clothes for imparting cooling sensation to the human body.
[0068] Hereinafter, the present invention will be described in more detail with reference to the following examples. However, the following examples are merely a reference for explaining the present invention in detail, and the present invention is not limited thereto, and may be realized in various forms.
[0069] In addition, unless otherwise defined, all technical and scientific terms have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention belongs. The terms used in the description of this application are merely for the purpose of effectively describing a particular embodiment and are not intended to limit the present invention. In addition, the unit of additives not specifically described in the specification may be weight percent. EXAMPLES
[0070] The physical properties were measured as follows.
[0071] [Measurement of yarn physical properties] <1. Thermal shrinkage stress> Both ends of the polyethylene yarn were tied to make a loop-shaped sample, and both sides of the loop-shaped sample were placed in the hot chamber of a thermal stress tester (Kanebo Eng., Japan, KE-2), and both sides of the loop sample were hooked onto a load cell and a preload ring, respectively, to measure the maximum thermal shrinkage stress under the following conditions: Here, the circumference of the loop was 10 cm.
[0072] -Load cell: A load cell capable of measuring up to 500gf -Initial temperature: room temperature (20±2℃) - Heating rate: 300℃ / 120sec -Initial load: 0.06667g / d
[0073] The thermal shrinkage stress values were obtained as a graph through an output device (Type 3086 XT Recorder, Yokogawa, Hokushin Electric, Tokyo, Japan).
[0074] <2. Number average molecular weight (Mw) (g / mol), weight average molecular weight (Mw) (g / mol) and polydispersity index (PDI)> The polyethylene raw yarn was completely dissolved in the following solvent, and then the weight average molecular weight (Mw) and polydispersity index (Mw / Mn: PDI) of the polyethylene raw yarn were determined using the following gel permeation chromatography (GPC).
[0075] -Analytical equipment: Tosoh HLC-8321 GPC / HT -Column: PLgel guard (7.5 x 50 mm) + 2 x PLgel mixed-B (7.5 x 300 mm) -Column temperature: 160°C -Solvent: Trichlorobenzene (TCB) + 0.04wt.% dibutylhydroxytoluene (BHT) (after drying with 0.1% CaCl2) -Injector, Detector temperature: 160℃ -Detector:RI Detector -Flow rate: 1.0ml / min -Injection volume: 300mL -Sample concentration: 1.5mg / mL -Standard sample: polystyrene
[0076] <3. Strength (g / d) and elongation (%)> The deformation-stress curves of polyethylene raw yarns were obtained using a universal tensile tester (Instron Engineering Corp, Canton, Mass.) according to the ASTM D2256 method. The sample length was 250 mm, the tensile speed was 300 mm / min, and the initial load was set at 0.05 g / d. The strength (g / d) and elongation (%) were calculated from the stress and elongation at the break point, and the initial modulus (g / d) was calculated from the tangent line that gave the maximum slope near the origin of the curve. Five measurements were taken for each raw yarn, and the average value was calculated.
[0077] <4. Crystallinity> The crystallinity of the polyethylene yarn was measured using an XRD (X-ray Diffractometer) [manufacturer: PANalytical, model name: EMPYREAN]. Specifically, the polyethylene yarn was cut to prepare a sample having a length of 2.5 cm, and the sample was fixed to a sample holder, and then the measurement was performed under the following conditions.
[0078] -Light source (X-ray Source):Cu-Kα radiation -Power: 45KV x 25mA - Mode: Continuous scan mode -Scan angle range: 10~40° -Scan speed: 0.1° / sec
[0079] [Fabric property measurement] <1. Cool sensation to the touch> The measurements were conducted at the Korea Clothing Testing and Research Institute using a KES-F7 (Thermo Labo II) device in a test environment of 20±2°C and 65±2% RH.
[0080] Specifically, a fabric sample having a size of 20cm x 20cm was prepared and left for 24 hours under conditions of 20±2°C temperature and 65±2% RH. Then, in a test environment of 20±2°C temperature and 65±2% RH, the contact coolness (Qmax) of the fabric was measured using a KES-F7 THERMO LABO II (Kato Tech Co., LTD.) device. Specifically, as illustrated in FIG. 2, the fabric sample 23 was placed on a base plate (also called a 'Water-Box') 21 maintained at 20°C, and a hot plate (T-Box) 22a (contact area: 3cm x 3cm) heated to 30°C was placed on the fabric sample 23 for only 1 second. That is, the other side of the fabric sample 23, one side of which is in contact with the base plate 21, was instantaneously brought into contact with the T-Box 22a. The contact pressure applied to the fabric sample 23 by the T-Box 22a was 6gf / cm. 2Then, the Qmax value displayed on a monitor (not shown) connected to the device was recorded. This test was repeated 10 times, and the arithmetic mean of the Qmax values was calculated.
[0081] <2. Thermal conductivity> After preparing a fabric sample having a size of 20 cm x 20 cm, it was left for 24 hours under the conditions of a temperature of 20 ± 2 ° C and a RH of 65 ± 2%. Then, the thermal conductivity and heat transfer coefficient of the fabric were measured using a KES-F7 THERMO LABO II (Kato Tech Co., LTD.) device in a test environment of a temperature of 20 ± 2 ° C and a RH of 65 ± 2%. Specifically, as illustrated in FIG. 3, the fabric sample 23 was placed on a base plate 21 maintained at 20 ° C, and a BT-Box 22b (contact area: 5 cm x 5 cm) heated at 30 ° C was placed on the fabric sample 23 for 1 minute. While the BT-Box 22b was in contact with the fabric sample 23, heat was continuously supplied to the BT-Box 22b so that the temperature of the BT-Box 22b was maintained at 30 ° C. The amount of heat supplied to maintain the temperature of the BT-Box 22b (i.e., heat flow loss) was displayed on a monitor (not shown) connected to the device. This test was repeated five times and the arithmetic mean of the heat flow loss was calculated.The thermal conductivity and heat transfer coefficient of the fabric were then calculated using Equations 2 and 3 below.
[0082] [Formula 2]: K = (WD) / (A.ΔT) [Formula 3]:k=K / D
[0083] Here, K is the thermal conductivity (W / cm.°C), D is the thickness (cm) of the fabric sample 23, and A is the contact area of the BT-Box 22b (=25 cm 2 ), ΔT is the temperature difference between the two sides of the fabric sample 23 (=10°C), W is the heat flow loss (Watt), and k is the heat transfer coefficient (W / cm 2 .℃).
[0084] <3.Dimensional stability> After preparing a fabric sample having a size of 20 cm x 20 cm, the sample was left for 24 hours under conditions of 20 ± 2°C temperature and 65 ± 2% RH. After that, the dimensions of one edge of the fabric sample were measured.
[0085] Then, after leaving it for 24 hours under the conditions of 90±2°C temperature and 65±2% RH, the dimensions were measured again by the above method. Then, the dimensional deformation rate of the fabric was calculated according to the following formula 1.
[0086] [Formula 1] Dimensional deformation rate (%) = {(FS1-FS0) / (FS0)} x 100
[0087] (In the above formula, FS0 is the functional fabric dimension (mm) measured after weaving the functional fabric and leaving it at room temperature (20±2°C, 65±2% RH) for 24 hours, and FS1 is the functional fabric dimension (mm) measured after weaving the functional fabric and leaving it at 90±2°C, 65±2% RH for 24 hours.)
[0088] [Example 1] <Production of polyethylene yarn> Using the apparatus illustrated in FIG. 1, a polyethylene yarn containing 200 filaments and having a total denier of 400 was produced.
[0089] First, 0.93 g / cm 3 Polyethylene chips having a density of 1000 g / mol and a weight average molecular weight (Mw) of 8,500 g / mol were fed into an extruder 100 and melted. The molten polyethylene was extruded through a die 200 having 200 holes. The ratio of hole length (L) to hole diameter (D) in the die 200, L / D, was 6. The die temperature was 270°C.
[0090] The filaments 11 formed while being discharged from the nozzle holes of the spinneret 200 were sequentially cooled in the cooling section 300 consisting of two sections. In the first cooling section, the filaments were cooled to 60° C. by cooling air with a wind speed of 1.0 m / sec, and in the second cooling section, the filaments were finally cooled to 30° C. by cooling air with a wind speed of 0.5 m / sec. After being cooled, the filaments were bundled into a multifilament yarn 10 by a bundler 400.
[0091] Next, the multifilament yarn was transferred to the drawing section 500. The drawing section was composed of a multi-stage drawing section consisting of four sections, and was composed of a total of four stages of godet roller units, and each godet roller unit was composed of two to six godet rollers.
[0092] Specifically, the first stretching section was stretched to a total stretch ratio of 2 times at a maximum stretching temperature of 80°C, the second stretching section was stretched to a total stretch ratio of 1.5 times at a maximum stretching temperature of 120°C, the third stretching section was stretched to a total stretch ratio of 1.3 times at a maximum stretching temperature of 120°C, and the fourth stretching section was stretched and heat-set so as to be shrunk (relaxed) by 2% compared to the third stretching section at a maximum stretching temperature of 120°C.
[0093] The drawn multifilament yarn was then wound on a winder 600. The winding tension was 0.8 g / d.
[0094] The physical properties of the produced yarn were measured and are shown in Table 1 below.
[0095] The measured heat shrinkage stress graph is shown in FIG.
[0096] <Manufacturing of functional fabrics> The polyethylene yarn thus produced was woven to a surface density of 500 g / m 2 The physical properties of the functional fabric thus produced were measured and are shown in Table 3 below.
[0097] [Examples 2 to 9] A fabric was manufactured in the same manner as in Example 1, except that the raw yarn conditions were changed as shown in Table 1 below. The physical properties of the fabric manufactured in the same manner as in Example 1 were measured and are shown in Table 3 below. The measured heat shrinkage stress graph for Example 7 is shown in FIG.
[0098] [Comparative Examples 1 to 2] A fabric was manufactured in the same manner as in Example 1, except that the raw yarn conditions were changed as shown in Table 2 below. In addition, the physical properties of the fabric manufactured in the same manner as in Example 1 were measured and are shown in Table 4 below.
[0099] [Comparative Example 3] The yarn and fabric were manufactured in the same manner as in Example 1, except that the yarn conditions were changed and the number of drawing sections was set to 2 as shown in Table 2 below. In addition, the physical properties of the fabric manufactured in the same manner as in Example 1 were measured and are shown in Table 4 below.
[0100] [Comparative Example 4] The yarn and fabric were manufactured in the same manner as in Example 1, except that the yarn conditions were changed as shown in Table 2 below, and the number of drawing sections was set to 6. In addition, the physical properties of the fabric manufactured in the same manner as in Example 1 were measured and are shown in Table 4 below.
[0101] [Table 1]
[0102] [Table 2]
[0103] [Table 3]
[0104] [Table 4]
[0105] Referring to Tables 1 to 4, it was confirmed that the fabrics according to the examples have an appropriate cool feeling and excellent dimensional stability. In particular, in the case of Comparative Example 4, although the fabric was manufactured using raw yarn with a relatively high degree of crystallinity, a large amount of fluff was generated during the manufacture of the fabric, resulting in low cool feeling to the touch and low thermal conductivity.
[0106] As described above, the present invention has been described using specific and limited examples and drawings. However, this is merely provided to assist in a more general understanding of the present invention, and the present invention is not limited to the above examples. Various modifications and variations can be made from such descriptions by those having ordinary knowledge in the field to which the present invention pertains.
[0107] Therefore, the concept of the present invention should not be limited to the described embodiments, and all things that are equivalent or have equivalent variations to the scope of the claims, as well as the scope of the claims, should be considered to fall within the scope of the concept of the present invention. [Explanation of symbols]
[0108] 10: Multifilament 11: Filament 21: Base plate 23: Fabric 22a:T-box 22b:BT-box 100: Extruder 200: Base 300: Cooling section 400:Focusing part 500: Stretching part 600: Winder
Claims
1. The maximum thermal shrinkage stress is 0.1 to 0.7 g / d; A polyethylene raw yarn having a melt index (MI, @190°C) of 5 to 25 g / 10 min.
2. The polyethylene raw yarn according to claim 1, wherein the raw yarn has a polydispersity index (PDI) of 5 to 20 and a number average molecular weight (Mn) of 1,000 to 10,000 g / mol.
3. 2. The polyethylene raw yarn according to claim 1, wherein the raw yarn has a tenacity of 6 to 17 g / d and an elongation of 10 to 25%, as measured by ASTM D2256.
4. The polyethylene yarn according to claim 1, wherein the yarn has a crystallinity of 65 to 85%.
5. The raw yarn has a density of 0.92 to 0.97 g / cm 3 The polyethylene raw yarn according to claim 1,
6. A functional fabric comprising the polyethylene yarn according to any one of claims 1 to 5.
7. The fabric has a cool touch of 0.05 to 0.25 W / cm2 when measured at 20±2°C and 65±2% RH by contacting a 30±2°C hot plate (T-box) with the fabric at 20±2°C. 2 The functional fabric according to claim 6,
8. The functional fabric according to claim 6, wherein the fabric has a thickness direction thermal conductivity of 0.05 to 0.25 W / mK, measured at 20±2°C and 65±2% R.H by contacting a heat source plate (BT-box) at 30±2°C with the fabric at 20±2°C.
9. The fabric has a surface density of 150 to 800 g / m 2 The functional fabric according to claim 6,
10. A cooling product produced from the fabric of claim 6.
Citation Information
Patent Citations
Melt-spun high-strength polyethylene fiber
JP3172189B2
About the corpse brute which appears and disappears in nighttime the axial storehouse work idyllic binding together string where the extirpation function is included and the manufacturing method.
KR1020120095733A
A polyethylene multifilament fiber with high tenacity and its manufacturing process
KR1020160059653A
Semiconductor device, power diode, and rectifier
KR1020200040724A
Improved Anti-squeal shim
KR102776822B1