How solar modules are manufactured

The use of reflective solder flux with additives on metal interconnects in solar modules addresses shading losses, enhancing power output by 2-5% through improved light scattering and reducing manufacturing complexity and cost.

JP2024544653AInactive Publication Date: 2024-12-03ALPHA ASSEMBLY SOLUTIONS INC

Patent Information

Application Number
JP2024532661
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-16
Filing Date
2022-12-09
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional solar module manufacturing methods using soldering with flux result in shading losses due to metal interconnects covering the surface of solar cells, leading to reduced power output and increased complexity and cost.

Method used

A method involving a reflective solder flux with additives applied to metal interconnects, allowing light to be reflected back onto the solar cells, reducing shading losses and increasing quantum efficiency.

Benefits of technology

The method achieves a 2-5% increase in power output by effectively scattering light onto the solar cells, reducing shading losses and maintaining low cost and simplicity in manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024544653000001_ABST
    Figure 2024544653000001_ABST
Patent Text Reader

Abstract

A method for manufacturing a solar module, the method including connecting a metallic interconnect to two or more solar cells and applying a transparent cover sheet to the two or more solar cells, where connecting the metallic interconnect to each solar cell of the two or more solar cells includes providing a solar cell having a bus bar on a surface thereof, providing a metallic interconnect having solder flux on a contact surface thereof, providing solder between the bus bar and the contact surface thereof, and reflowing the solder to connect the metallic interconnect to the bus bar, where the solder flux includes a reflective additive.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a solar module, a method for connecting a metallic interconnect to a solar cell, a metallic interconnect for a solar cell, a solder flux, a solar module, and a method for manufacturing a metallic interconnect. [Background technology]

[0002] In the assembly of photovoltaic (PV) modules, the interconnection of crystalline silicon (c-Si) solar cells is typically accomplished by using automated combined tabbing and stringing equipment using soldering. Soldering utilizes a flux. The flux reacts with and thereby removes the oxide surface layer of both the solder and the substrate. This ensures that a clean metal is provided during reflow so that wetting and associated bond formation can proceed. Fluxes are typically liquids and consist of a chemical activator package, additives, a solvent system, and optionally rosin or synthetic resins. Historically, the solar industry has used alcohol-based flux formulations.

[0003] To interconnect industrial solar cells with the front grid pattern, flat solder-coated copper wires are typically soldered to 2-20 bus bars on the front and back sides. These wires are thin and wide to minimize resistive power losses in the wires and to minimize stresses in the cells. However, the shading of the cells by these wires represents a significant power loss in the encapsulated module, the so-called "shading loss".

[0004] To eliminate this shading loss, researchers have previously explored cell designs in which all contacts are located or led to the rear side of the cell, but such cell designs are complex and expensive and therefore undesirable.

[0005] An alternative approach, presented by Sachs et al. at the 24th European PVSEC, 23 September 2009, Hamburg, Germany, in "Light-Capturing Interconnect Wire For 2% Module Power Gain", describes forming triangular grooves on the top surface of the ribbon and coating the surface with a reflective layer such as silver. The grooves are designed so that the incident light is reflected upwards towards the glass cover sheet of the module at an angle shallow enough to undergo total internal reflection at the glass-air interface, and downwards onto the solar cells. It is claimed that as much as 80% of the light that strikes the busbar can potentially be recaptured, and experiments with industrial solar cells show a 2% relative gain in encapsulated cell current and power using this light-capturing interconnect wire compared to a control using standard wire. However, such an approach is expensive and works well only for normally incident radiation. Summary of the Invention

[0006] The present invention seeks to address at least some of the problems associated with the prior art, or at least to provide a commercially acceptable alternative thereto.

[0007] The present invention provides a method for manufacturing a solar module, the method comprising the steps of: connecting the metallic interconnect to two or more solar cells; applying a transparent cover sheet to the two or more solar cells; Connecting the metallic interconnect to each solar cell of the two or more solar cells Providing a solar cell having a bus bar on a surface thereof; Providing a metallic interconnect having solder flux on a contact surface thereof; providing solder between the busbar and the contact surface; reflowing the solder to connect the metallic interconnect to the busbar; The solder flux includes a reflective additive.

[0008] Each aspect or embodiment defined in this specification may be combined with any other aspect or embodiment unless expressly indicated otherwise. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature indicated as being preferred or advantageous.

[0009] The inventors have surprisingly found that the resulting solar module exhibits reduced shading losses compared to conventional solar modules.

[0010] Due to the presence of a reflective coating in the flux, following reflow of the solder, the metallic interconnect comprises a reflective coating on its surface. Such a reflective coating may have a reflectivity of at least 10%, more typically at least 20%, even more typically at least 30%, even more typically at least 35%, even more typically about 40%. In use, such a reflective coating increases the scattering of light. Without being bound by theory, it is believed that about 53% of the scattered photons statistically strike the solar cell and induce a current after striking the transparent cover sheet / air boundary at an angle greater than the total internal reflection angle (ΦTIR=42°). This may cause an increase in quantum efficiency up to 45%. This higher quantum efficiency leads to an increase in the short circuit current density and thus a decrease in the optically inactive width of the ribbon.

[0011] Advantageously, compared to conventional solar modules, such reduced shading losses can be provided regardless of the angle of incident radiation. Moreover, compared to conventional methods of manufacturing solar modules, the method of the present invention is simple and low cost.

[0012] The term "solar cell" or "photovoltaic cell" as used herein may encompass an electrical device that converts light energy directly into electricity by the photovoltaic effect, which is a physical and chemical phenomenon. The term "solar module" or "photovoltaic panel" as used herein may encompass multiple solar cells in an integrated group, all oriented in one plane. Photovoltaic modules often have a glass sheet on the side facing the sun to allow light to pass through while protecting the semiconductor wafer.

[0013] The method includes connecting a metallic interconnect to two or more solar cells. As used herein, the term "metallic interconnect" can encompass conductive wires or ribbons. "Metallic" means that the interconnect is formed from or includes a metal or alloy. Such a connection is an electrical connection. Two or more solar cells are connected to each other via a metallic interconnect. Typically, the metallic interconnect comprises a first end and a second end, with one solar cell connected to the first end and another solar cell connected to the second end. Typically, the metallic connector connects the top (i.e., light-facing) surface of one solar cell with the bottom (i.e., non-light-facing surface) of another solar cell, i.e., the metallic interconnect may connect the positive surface of one solar cell to the negative surface of another solar cell.

[0014] The method includes applying a transparent cover sheet to two or more solar cells. Specifically, the transparent cover sheet is applied to the outer surfaces of the two or more solar cells, more specifically to the surfaces that receive incident light during use, i.e., the surfaces that face the sun. The transparent cover sheet can physically protect the solar cells while allowing light to pass through to the underlying solar cells.

[0015] Connecting the metallic interconnect to each solar cell of the two or more solar cells includes providing a solar cell with a bus bar on a surface thereof. The term "bus bar" is a term in the art and as used herein can encompass a metallic strip or bar.

[0016] Connecting the metallic interconnect to each solar cell of the two or more solar cells includes providing the metallic interconnect with solder flux on its contact surface. The term "solder flux" is a term in the art and as used herein may include chemical cleaners, flow agents, or purifiers. Solder flux may improve the wetting properties of the liquid solder by removing oxidized metals from the surfaces to be soldered, keeping air out to prevent further oxidation, and / or facilitating amalgamation. The term "contact surface" as used herein may include the surface that is connected to the solar cells as well as the surface that faces the incident light in the final solar cell module (the "light receiving" surface). When the metallic interconnect is in the form of a ribbon, the contact surface includes both the top and bottom surfaces of the ribbon. Typically, the contact surface includes substantially the entire outer surface of the interconnect.

[0017] Providing solder between the busbar and the contact surface typically involves sandwiching the solder between the busbar and the contact surface. The solder is typically provided to contact both the busbar and the contact surface. As used herein, the term "solder" may encompass a fusible metal alloy used to create a permanent bond between metal workpieces. The solder is melted to adhere to and connect the components after cooling, but alloys suitable for use as solder must have a lower melting point than the components being joined.

[0018] The solder may be pre-applied to the contact surfaces. In other words, the steps "providing a metallic interconnect having solder flux on the contact surfaces" and "providing solder between the busbar and the contact surfaces" may constitute providing a metallic interconnect having solder flux and solder on its contact surfaces, and orienting the solar cell and the metallic interconnect such that the solder is located between the contact surfaces and the busbar.

[0019] The solder flux includes a reflective additive. As used herein, the term "reflective additive" may include species that are capable of reflecting light, particularly solar light. The reflective additive is typically a solid species suspended in the liquid component of the solder flux.

[0020] The reflective additive preferably comprises a dye and / or a pigment. Such species can provide a high level of reflectivity to the reflective coating, thereby reducing the optically inactive width of the interconnect.

[0021] The reflective additive preferably comprises a pigment. Compared to dyes, pigments exhibit increased color fastness, thus reducing the degradation of the solar module's performance over time. Furthermore, compared to dyes, pigments tend to be less flammable, thus reducing the risk of fire.

[0022] Compared to dyes, pigments tend to be less soluble in conventional fluxing fluids and may exhibit lower levels of dispersion. As a result, the pigments are preferably coated with one or more of polyols, silanes, amines, and amine salts. Such species can improve compatibility with the coating, increase dispersion, and / or reduce agglomeration during storage of the flux.

[0023] The reflective additive preferably includes pigments including one or more of iron oxide, zinc oxide, aluminum oxide, titanium dioxide (e.g., foliated TiO2 foam), chromium oxide, perylene, ferric ammonium ferrocyanide, silver (e.g., silver nanoparticles), and aluminum (e.g., aluminum paste). Such species can provide high levels of reflectivity.

[0024] The reflective additive preferably comprises a pigment comprising titanium dioxide, more preferably the titanium dioxide is in the form of flakes, and even more preferably the titanium dioxide flakes are coated with alumina and / or zirconia. Such species are particularly suitable for use in the present invention and can provide particularly high levels of reflectance. Preferably, these species are coated with one or more of polyols, silanes, and amines and amine salts for the reasons discussed above.

[0025] The pigment is preferably in the form of a particle (e.g., powder), more preferably a flake. Such a form may provide a high level of reflectance and light scattering. The particles or flakes preferably have a longest dimension of 0.5 to 5 μm, more preferably 1 to 2 μm. Such a size may allow the pigment to be more easily incorporated into the flux.

[0026] The dye preferably comprises a fluorescent dye (also known as a "laser" dye). The presence of a fluorescent dye can increase the quantum efficiency of the solar module. Examples of such dyes include, but are not limited to, rhodamine-based dyes such as rhodamine b, acid-52, fluorescent green, fluorescein, ATTo series dyes, Cy2, tamra, Cal fluor red 590, and perylene dyes.

[0027] The solder flux may further comprise an optical brightener. As used herein, the term "optical brightener" may include compounds that absorb light in the ultraviolet and violet region of the electromagnetic spectrum (usually 340-370 nm) and re-emit light in the blue region (typically 420-470 nm) by fluorescence. This may cause a "whitening" effect and thus increase reflectance. Suitable optical brighteners include, for example, OB, OB-1, KCB, KSN, FP-127, KB, 4BK, DBH, ER-1, ER-2, ER-3, CXT, VBL, BBU and CBS-X.

[0028] The reflective additive is preferably white or yellow, more preferably white, as such colors provide a high level of reflectance.

[0029] The flux comprises 0.1-15 wt. % of the reflective additive, preferably 0.3-2 wt. % of the reflective additive, based on the total weight of the flux. Such an amount can provide a high level of reflectivity without compromising other functions of the solder flux, such as removing oxidized metals from the surfaces to be soldered, keeping air out to prevent further oxidation, and / or improving the wetting characteristics of the liquid solder.

[0030] The solder flux preferably further comprises an acrylic resin binder, preferably a methacrylic resin binder. The presence of such a binder, which is elastomeric, can provide flexibility to the flux and thus to the resulting reflective coating. As a result, the performance degradation of the solar module, for example due to PID (Power Induced Degradation), is reduced. In addition, there can be a reduction in chipping or flaking during handling or feeding in automated Combined Tubbing and Stringing (CTS) equipment. The flexibility can allow the solar module to take any shape, for example, to be wrapped around automobiles, airplane wings, buildings, robots, and three-dimensional (3-D) displays. Furthermore, the presence of such a binder can make the solder flux substantially "tack-free", even at high operating temperatures. If the flux is sticky, ribbon alignment is compromised. Sticky flux creates alignment problems, which in turn create peel strength problems. Also, sticky or powdery residues can adhere to pulleys, grippers and other machine parts, causing frequent downtime and aesthetic issues. Sticky fluxes can also cause cell breakage. If the flux is sticky or the residues remain sticky after processing, the robotic arm cannot properly pick up the strings. This can cause microcracks in the assembled strings. Additionally, the presence of such binders can make the fluxes particularly compatible with traditional Ethyl Vinyl Acetate (EVA) laminate materials.

[0031] The solder flux preferably comprises 1-10% by weight of acrylic resin binder, preferably 2-6% by weight of acrylic resin binder. Below this range, it may not provide a sufficient level of flexibility and non-stickiness. Above this range, other functions of the solder flux, such as removing oxidized metals from the surfaces being soldered, keeping air out to prevent further oxidation, and / or improving the wetting characteristics of the liquid solder, may be compromised.

[0032] The acrylic resin binder is preferably an acrylic polymer having a carboxyl group, a hydroxyl group, or an amide group, or a mixture thereof, preferably an acrylic polymer having a weight average molecular weight of 5,000 to 500,000 and a glass transition temperature of -20°C to +125°C. Typically useful acrylic polymers contain alkyl methacrylates, alkyl acrylates, hydroxyalkyl acrylates, hydroxyalkyl methacrylates, and may contain styrene, acrylic acid, or methacrylic acid. Amide monomers such as methacrylamide and acrylamide may be used. Glycidyl monomers such as glycidyl acrylate or glycidyl methacrylate may also be used. Isoprene-based liquid rubbers and the like may also be used. Preferred acrylic polymers are alkyl methacrylates having 1 to 18 carbon atoms in the alkyl group, alkyl acrylates having 1 to 18 carbon atoms in the alkyl group, and hydroxyalkyl acrylates or hydroxyalkyl methacrylates having 2 to 4 carbon atoms each in the hydroxyalkyl group.

[0033] The solder flux preferably further comprises a vinyl resin binder. The presence of such a binder, which is elastomeric, can provide flexibility to the flux and thus to the resulting reflective coating. As a result, degradation of the solar module's performance, for example as a result of bending, is reduced. In addition, there can be a reduction in chipping or flaking during handling or feeding in automated composite tabbing and stringing (CTS) equipment. The flexibility can allow the solar module to take any shape, for example, to be wrapped around automobiles, airplane wings, buildings, robots, and three-dimensional (3-D) displays. Furthermore, the presence of such a binder can make the solder flux substantially "tack-free", even at high operating temperatures. If the flux is sticky, ribbon alignment is compromised. Sticky flux creates alignment problems, which in turn create peel strength problems. Also, sticky or powdery residues can adhere to pulleys, grippers, and other machine parts, causing frequent downtime and aesthetic problems. Sticky flux also causes cell failure. If the flux is sticky or if the residue after processing remains sticky, the robotic arm will not be able to properly pick up the string. This can result in microcracks in the assembled string. Additionally, the presence of such binders makes the flux particularly compatible with traditional Polyolefine (POE) and EVA laminate materials.

[0034] The solder flux preferably comprises 0.1-5 wt. % vinyl resin binder, preferably 0.5-2 wt. % vinyl resin binder. Below this range, it may not provide a sufficient level of flexibility and non-stickiness. Above this range, other functions of the solder flux, such as removing oxidized metals from the surfaces being soldered, keeping air out to prevent further oxidation, and / or improving the wetting characteristics of the liquid solder, may be compromised.

[0035] The solder flux preferably contains both an acrylic (preferably a methacrylic) binder and a vinyl resin binder.

[0036] The solder flux is preferably substantially halogen-free, more preferably halogen-free. Compared to halogen-containing solder fluxes, this can reduce the aggressiveness of the solder flux to the materials forming the metal interconnects and the solar cells. This can improve the reliability of the solar module and allow the solar module to pass the accelerated aging test IEC61215. Furthermore, halogen ions remain on the cells and can migrate and cause current short circuits.

[0037] The solder flux preferably further comprises an activator, more preferably an activator comprising a dicarboxylic acid, and even more preferably the dicarboxylic acid is selected from one or more of adipic acid, glutaric acid and succinic acid. Such species may be particularly suitable for removing oxidized metals from the surfaces to be soldered, forcing out air to prevent further oxidation, and / or for improving the wetting properties of the liquid solder.

[0038] The solder flux preferably contains 1 to 5% by weight of an activator.

[0039] The solder flux preferably further comprises one or more of a resin, a rosin, a wetting agent, an antifoaming agent, a plasticizer, and a dispersing agent.

[0040] The solder flux preferably includes an agent for wetting and dispersing the reflective additive (e.g., titanium dioxide). This portion can aid in the wetting and dispersing of the pigment and / or dye in the flux composition. For example, nonionic, cationic and / or amphoteric wetting and dispersing agents can be used. Exemplary dispersing agents include, but are not limited to, polyethylene glycol and its derivatives (e.g., PEG100, PPG), low molecular weight polyacrylics and methacrylics, block copolymers with pigment affinity groups such as BYK2023, BYK2117, BYK180, structured copolymers, Zonyl FSN fluorosurfactants (described as perfluoroalkyl ethoxylates) available from EI DuPont de Nemours & Co., Inc., Fluorad FC-430 (described as fluoroaliphatic polymer esters) available from 3M's Chemical Products Division, and ATSURF fluorosurfactants available from Imperial Chemical Industries. Other exemplary dispersing agents include, but are not limited to, alkoxysilanes (polyalkylene oxide modified heptamethyltrisiloxane), ethers (allyloxypolyethylene glycol methyl ether, polyoxyethylene cetyl ether), polydimethylsiloxane, polyether modified polydimethylsiloxane, polyester modified polydimethylsiloxane, hexadimethylsilane, hexadimethyldisilazane, polyoxyethylene sorbitan monooleate, water-soluble ethylene oxide adducts based on ethylene glycol, water-soluble ethylene oxide-propylene oxide adducts based on propylene glycol, polycarboxylic acids (dicarboxylic acids having at least 3 carbon atoms), dimerized carboxylic acids, polymerized carboxylic acids, etc. A particularly suitable agent is BYK 2117.

[0041] Preferably, the busbars include copper, tin or silver connection pads, and reflowing the solder connects the metallic interconnects to the copper, tin or silver connection pads. Solder flux may enable particularly favorable wetting of the solder to copper, tin and silver.

[0042] The metallic interconnect preferably comprises copper or copper alloy ribbon, which can exhibit a suitable level of electrical conductivity and can be soldered using conventional solders.

[0043] The transparent cover sheet preferably comprises glass, which is particularly suitable for protecting the solar cells while allowing incident light to pass through the solar cells, and the glass is preferably textured.

[0044] The method preferably further comprises laminating the solar cells. Lamination can ensure complete sealing of the delicate and moisture-sensitive interconnected solar cells. Lamination is preferably performed using lamination materials selected from ethyl vinyl acetate (EVA) and polyolefins (POE). The solder flux of the present invention is compatible with such materials. Lamination preferably comprises applying a transparent cover sheet to the side exposed to radiation (the "front sheet") and a polymeric or composite layer to the opposite side (the "back sheet").

[0045] The solder flux may further include a black or blue pigment, the presence of which can provide a desirable aesthetic effect to the metal interconnect in which the solder flux is used, such that the interconnect can exhibit both aesthetic appeal and high reflectivity.

[0046] Suitable black and / or blue pigments include, for example, ferric oxide black, carbon black, graphite, Pigment Black Number 7, iron oxide and chromium(III) oxide pigments (e.g., Sicopal® Black L0095), and Solvent Black 9, 37, 32, 42, 48 and 49, preferably iron oxide and chromium(III) oxide pigments (e.g., Sicopal® Black L0095), Microlith® Black 0066 A and carbon black.

[0047] The solder flux preferably includes an agent for wetting and dispersing the black and / or blue pigment. The agent may be the same as the agent described above for dispersing the reflective additive. Such an agent may be particularly beneficial when the black and / or blue pigment includes carbon black. When the black and / or blue pigment includes carbon black, a particularly suitable agent is BYK 2117.

[0048] In a further aspect, the present invention provides a method for manufacturing a solar module, the method comprising the steps of: Providing a first solar cell having a bus bar on a surface thereof; providing a second solar cell having a bus bar on a surface thereof; Providing a metallic interconnect having a first end and a second end; providing solder between the bus bar and the first end of the first solar cell; reflowing the solder to connect the first end to a bus bar of the first solar cell; providing solder between the bus bar and the second end of the second solar cell; reflowing the solder to connect the second end to a bus bar of a second solar cell; applying a transparent cover sheet to the solar cell; The first end and the second end are coated with a solder flux, the solder flux including a reflective additive.

[0049] The advantages and preferred features of the first aspect of the invention apply equally to this aspect.

[0050] The two steps of applying solder and / or reflowing the solder may be performed sequentially or simultaneously.

[0051] In a further aspect, the present invention provides a method of connecting a metallic interconnect to a solar cell, the method comprising: Providing a solar cell having a bus bar on a surface thereof; Providing a metallic interconnect having solder flux on a contact surface thereof; providing solder between the busbar and the contact surface; and reflowing the solder to connect the metallic interconnect to the bus bar, the solder flux including a reflective additive.

[0052] The advantages and preferred features of the first aspect of the invention apply equally to this aspect.

[0053] In a further aspect, the present invention provides a metallic interconnect for a solar cell, the metallic interconnect having a solder flux on a surface thereof, the solder flux including a reflective additive and being substantially free of a solvent.

[0054] The advantages and preferred features of the first aspect of the invention apply equally to this aspect.

[0055] In automated tabbing and stringing machines, flux is typically applied to the ribbon or cell just prior to soldering. Typically, the flux is sprayed onto the cell / ribbon or the ribbon is dipped into a flux tank. The fluxing operation generates a lot of residue and can contaminate the machine parts. This in turn can increase the machine downtime and contamination on the parts / cells becomes almost inevitable. Furthermore, operations like dip coating can result in non-uniform flux and flux spreading can be observed on the fingers and cell areas. Yellowing and cold solder joints are also common issues associated with standard PV fluxing. Compatibility between traditional EVA (ethylene vinyl acetate) encapsulants and flux residues has also been reported in the literature. Such issues can be avoided by the use of the metallic interconnect of the present invention. The use of a solvent-free "pre-applied" flux reduces the formation of residues and its associated problems. Furthermore, the cost and safety impacts of handling and storing large amounts of flammable (typically alcoholic) solvents are avoided.

[0056] The metallic interconnect has solder flux on its surface, which may be the contact surface as described above, i.e. the surface that is connected to the solar cell.

[0057] The flux is substantially free of solvent, typically completely free of solvent. The flux may contain less than 2% by weight of solvent, typically less than 1% by weight of solvent, and even more typically less than 0.1% by weight of solvent.

[0058] In a further aspect, the present invention provides a solder flux comprising a solid component and optionally a solvent, the solid component comprising a reflective additive.

[0059] The advantages and preferred features of the first aspect of the invention apply equally to this aspect.

[0060] In a preferred embodiment, the solder flux comprises 85 to 95% by weight of a solvent.

[0061] The solvent preferably comprises isopropyl alcohol, which is particularly suitable for use in the flux because it evaporates at typical soldering temperatures, thereby leaving little organic residue on the solder joint that can adversely affect the electrical and mechanical performance of the joint.

[0062] In a preferred embodiment, the solder flux comprises, based on the total weight of the solder flux: 85 to 95% by weight of isopropyl alcohol solvent; 0.5 to 10% by weight of a methacrylic resin binder; 0.1 to 5% by weight of a vinyl resin binder; 1 to 5% by weight of an activator; 0.3-2 wt. % of a reflective additive, preferably the reflective additive comprises titanium dioxide, more preferably in powder (e.g. flake) form; Optionally, 0.1 to 2 wt. % of a wetting agent.

[0063] Such solder fluxes exhibit a particularly favorable combination of high reflectivity, flexibility, non-stickiness, non-aggressiveness and excellent wetting properties.

[0064] In a preferred embodiment, the solder flux is substantially solvent-free, thereby avoiding the disadvantages associated with solvents mentioned above. Such a "solvent-free" solder flux may be applied, for example, using a "hot melt" process.

[0065] In a further aspect, the present invention provides a solder flux comprising a solid component and optionally a solvent, the solid component comprising a black and / or blue pigment.

[0066] The advantages and preferred features of the first aspect of the invention apply equally to this aspect.

[0067] The presence of a black or blue pigment can provide a desirable aesthetic effect to the metallic interconnect in which the solder flux is used.

[0068] Suitable black and / or blue pigments include, for example, ferric oxide black, carbon black, graphite, Pigment Black Number 7, iron oxide and chromium [III] oxide pigments (e.g., Sicopal® Black L0095), and Solvent Black 9, 37, 32, 42, 48 and 49, preferably carbon black and iron oxide and chromium [III] oxide pigments (e.g., Sicopal® Black L0095). Iron oxide and chromium [III] oxide pigments (e.g., Sicopal® Black L0095) are particularly beneficial because they are black but also reflect light, thereby providing a favorable combination of high reflectance and favorable aesthetics.

[0069] In a preferred embodiment of this aspect, the solder flux comprises, based on a total weight of the solder flux: 85-95% by weight of isopropyl alcohol solvent; 0.5 to 10% by weight of a methacrylic resin binder; 0.1 to 5 weight percent of a vinyl resin binder; 1 to 5% by weight of an activator; 0.5 to 2% by weight of a black pigment, the black pigment comprising carbon black and / or iron oxide and chromium (III) oxide pigments; Optionally, 0.1 to 2 wt. % of a wetting agent.

[0070] In another preferred embodiment of this aspect, the solder flux is substantially solvent-free, thereby avoiding the disadvantages associated with solvents mentioned above. Such a "solvent-free" solder flux may be applied, for example, using a "hot melt" process.

[0071] In a further aspect, the present invention provides a solar module manufactured according to the methods described herein.

[0072] The advantages and preferred features of the first aspect of the invention apply equally to this aspect.

[0073] In a further aspect, the present invention provides a method of producing a metallic interconnect as described herein, the method comprising: Providing a metallic interconnect; Providing a solvent-containing solder flux as described herein; applying a solder flux to the metal interconnect; and removing the solvent from the solder flux by evaporation.

[0074] The solder flux may be applied, for example, by one or more of brushing, coating, spraying, spray coating, dipping, and rolling. Evaporation may occur by heating the solder flux, preferably to a temperature above the boiling point of the solvent.

[0075] In a further aspect, the present invention provides a method of producing a metallic interconnect as described herein, the method comprising: Providing a metallic interconnect; Providing a "solvent-free" solder flux as described herein; Melting a solder flux; and applying the molten solder flux to the metallic interconnect.

[0076] The molten solder flux may be applied to the metallic interconnects using, for example, a "hot melt" process. [Brief description of the drawings]

[0077] The invention will now be described with reference to the following non-limiting drawings. [Figure 1] FIG. 1 is a schematic diagram showing the paths of light entering and exiting a conventional solar module. [Diagram 2] FIG. 2 is a schematic diagram showing the paths of light entering and exiting a solar module according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0078] With reference to Figure 1, a conventional solar module (generally designated 1) is shown. The solar cells 2 have bus bars 3 on their surface. To protect the solar cells 2 from air 5, the light receiving side of the module is covered with a sheet 4 made of glass with an EVA film. An interconnect (flat metal ribbon) 6 acts like a mirror and reflects the incoming radiation (indicated by the arrows) from the module. The area covered by the ribbon (approximately 3.5%) is mainly lost due to photoelectric conversion.

[0079] 2, a solar module A according to the invention is shown in which a ribbon 6 is coated with a reflective layer 7. After striking a glass-air surface 8 at an angle greater than the angle of total internal reflection, some of the scattered photons strike the solar cell and induce an electric current.

[0080] The invention will now be discussed with reference to the following non-limiting examples. EXAMPLES

[0081] A flexible, non-sticky coating and reflective flux was prepared by blending different types of coating and binding resins, plasticizers, and organic acids such as adipic and succinic acids. This flux coating imparts color when coated onto the metal ribbon and is inherently reflective. Inorganic pigments were dispersed in the flux. The method for producing this flux is as follows: The resin was precisely measured to the amount of flux required to be prepared and added to a clean, dry mixing vessel equipped with a heating jacket, and the mixture was stirred with the solvent and the temperature was maintained at about 60-70°C until the resin was dissolved. The mixture was maintained near the above mentioned temperature to avoid overheating and evaporation of the mixture. The required number of organic acids are added to the mixture and allowed to dissolve until all solids are dissolved, until the mixture is observed to be transparent. The required amount of plasticizer is then weighed and added to the mixture and mixed for 10 minutes while maintaining the temperature of the mixture at 60-70°C. The vessel was covered with a lid during this entire process. The entire mixture was left to cool to room temperature. For quality control studies, the required amount of flux was removed from this mixture. The required amount of colorant for this formulation was weighed and added to the flux formulation. If a solvent was used, this mixture was sheared on a high shear mixer at 7000-8000 rpm for about 60-70 minutes until the colorant was completely dispersed. For the hot melt process, the colorant was added after the solid mixture became flowable. Intermediate breaks were given to maintain the temperature of the mixture during the high shear mixing process, and the temperature was maintained below 50°C. The resulting mixture was transferred to a container for further use or for coating metal ribbons. Any settling seen must be redispersed before use. The dispersed flux was precoated onto metal ribbons for further applications.

[0082] The flux in this example contains 5% by weight of binding resin, 2% by weight of organic acid, 1% by weight of plasticizer, and 1.5% by weight of inorganic pigment. The flux was coated onto a ribbon and the ribbon was subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%. If the pigment is black, it improves the aesthetics of the panel.

[0083] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux-coated ribbon was subjected to reflectance analysis and had a reflectance of 34-36%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0084] A flexible and reflective flux was prepared by combining different types of coating and binding resins, partially dimerized rosin (Poly-Pale), plasticizers, and organic acids such as adipic acid and succinic acid, as described in Example 1. The flux is inherently reflective and inorganic pigments are dispersed in the flux. The flux in this example contains 1 wt% Ke604 and polypal rosin, 2 wt% binding resin (vinyl polymer), 2 wt% organic acid, 0.5 wt% plasticizer, and 1 wt% inorganic pigment. This flux was coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0085] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 27-30%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0086] A flexible and reflective flux was prepared as described in Example 1 by combining different types of binding resins, partially dimerized rosin (Poly-Pale), plasticizers, rosin, and organic acids such as adipic and succinic acids. The flux is inherently reflective and has pigments dispersed in the flux. This example contains 1% Ke604 and polypal rosin, 2% by weight of binding resin, 2% by weight of organic acid, and added 0.5% by weight of BYK-2023. and 1.1% by weight of pigment. This flux was coated on ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0087] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 30-32%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0088] A flexible and reflective flux was prepared by combining different types of binding resins, plasticizers, and organic acids such as adipic acid and succinic acid as described in Example 1. The flux is inherently reflective and inorganic pigments such as zinc oxide are dispersed in the flux. The flux in this example contains 5% by weight of binding resin, 2.2% by weight of organic acid, 0.8% by weight of plasticizer, and 1.2% by weight of inorganic acid. The flux was coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0089] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 33-35%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0090] A flexible and reflective flux was prepared by combining different types of binding resins, plasticizers, and organic acids such as adipic acid and methylsuccinic acid as described in Example 1. The flux is inherently reflective and an inorganic pigment, titanium dioxide, is dispersed in the flux. The flux in this example contains 5 wt% binding resin, 1.8 wt% adipic acid, 0.4 wt% methylsuccinic acid, 0.8 wt% plasticizer, and 1.2 wt% inorganic pigment. The flux was coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0091] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 33-36%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0092] A flexible and reflective flux was prepared by combining different types of binding resins, plasticizers, and organic acids such as adipic acid and succinic acid as described in Example 1. The flux is inherently reflective and has pigments dispersed in the flux. The flux in this example contains 5% by weight of binding resin, 1.8% by weight of adipic acid, and 0.4% by weight of succinic acid. 0.8% by weight of plasticizer, 1.2% by weight of aluminum paste 100 microns. This flux was coated on ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 0.5%.

[0093] The elasticity of this flux was tested by twisting a flux-coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 24-26%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0094] Example 1 was repeated, except that a fluorescent dye (Acid Red-52) was added to the composition. Fluorescent dyes absorb light at shorter wavelengths and emit light at longer wavelengths, thus improving the quantum efficiency and reflectivity of the coating, which produces wide angle scattering and achieves maximum total internal reflection. This flux was coated onto ribbons, and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0095] The elasticity of this flux was tested by twisting a flux coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 35-38%. The flux was completely tack-free when applied and allowed to dry for 5-6 seconds and tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0096] A reflective hot melt adhesive formulation was prepared as described in Example 1 by combining rosin Ke604, Versamid, organic acids such as adipic and palmitic acids, ceresin wax and pigments. The flux in this example contains 22% Ke604, 9% Versamid, 20% adipic acid, 27% palmitic acid, 15% ceresin wax and 9% pigments by weight. The flux was coated on ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0097] The elasticity of this flux was tested by twisting a flux coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 38-42%. The flux was completely tack-free when applied and allowed to dry for 5-6 seconds and tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0098] A reflective hot melt adhesive formulation was prepared as described in Example 1 by combining rosin Ke604, Versamid, organic acids such as adipic and palmitic acids, ceresin wax and pigments. The flux in this example contains 25% Ke604, 10% Versamid, 23% adipic acid, 15% palmitic acid, 20% ceresin wax and 8% pigments by weight. The flux was coated on ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0099] The elasticity of this flux was tested by twisting a flux coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 40-50%. The flux was completely tack-free when applied and allowed to dry for 5-6 seconds and tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0100] The reflective hot melt adhesive formulation was prepared as described in Example 1. The flux was prepared by combining polymerized rosin Dymerex, Unirez-2940, organic acids such as adipic acid, palmitic acid, benzotriazole, and pigment. The flux in this example contains 18% by weight Dymerex, 26% by weight Unirez-2940, 30% by weight adipic acid, 24% by weight palmitic acid, 1% by weight benzotriazole, and 1% by weight pigment. The flux was coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0101] The elasticity of this flux was tested by twisting a flux coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 40-50%. The flux was completely tack-free when applied and allowed to dry for 5-6 seconds and tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0102] A reflective hot melt adhesive formulation was prepared by combining polymerized rosin Dymerex, Unirez-2940, organic acids such as adipic acid and palmitic acid, benzotriazole and pigment as described in Example 1. The flux in this example contains 20% by weight Dymerex, 24% by weight Unirez-2940, 25% by weight adipic acid, 27.8% by weight palmitic acid, 0.8% by weight benzotriazole and 1.4% by weight pigment. The flux was coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0103] The elasticity of this flux was tested by twisting a flux coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 40-50%. The flux was completely tack-free when applied and allowed to dry for 5-6 seconds and tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0104] By combining different types of binding resins, rosin (unirez-2940), plasticizers, and organic acids such as adipic and suberic acids, flexible and reflective fluxes were prepared as described in Example 1. The fluxes were inherently reflective and had lab-synthesized porous nanocrystalline TiO2 leaf-like foam dispersed in the flux. The fluxes in this example contain 5 wt% binding resin, 1.2 wt% unirez-2940, 1.8 wt% adipic acid and 0.5 wt% succinic acid, 0.8 wt% plasticizer, and 1.2 wt% leaf-like TiO2 foam dispersed in them. The fluxes were coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0105] The elasticity of this flux was tested by twisting a flux coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 14-16%. The flux was partially tacky when applied and allowed to dry for 5-6 seconds and the tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0106] A flexible and reflective flux was prepared by combining different types of binding resins, plasticizers, and organic acids such as adipic acid and succinic acid as described in Example 1. The flux is inherently reflective and has pigments dispersed in the flux. The flux in this example contains 5 wt% binding resin, 1.8 wt% adipic acid, and 0.4 wt% succinic acid; 0.8 wt% plasticizer, and 2 wt% pigment (silver nanoparticles). This flux was coated on ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel.

[0107] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 30-34%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0108] By combining different types of binding resins, KE604, partially dimerized rosin (Poly-Pale), plasticizers, and organic acids such as adipic acid, flexible and reflective fluxes were prepared as described in Example 1. The fluxes are inherently reflective and pigment spacers such as Polygloss 90 and aluminum paste 100 are dispersed in the flux. The fluxes in this example contain 1.6 wt% binding resin, 0.6 wt% Ke604, 0.4 wt% Polypale rosin, 2.2 wt% adipic acid, 0.6 wt% plasticizer, 1.2 wt% pigment polygloss 90, and aluminum paste. The fluxes were coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel.

[0109] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 14-16%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0110] By combining different types of binding resins and polymers (Polyvinylpyrrolidine K30), plasticizers, organic acids such as adipic acid and succinic acid, flexible and reflective fluxes were prepared as described in Example 1. The fluxes are inherently reflective, and pigments and pigment spacers such as Polygloss 90 and aluminum paste 100 are dispersed in the flux. The fluxes in this example contain 5 wt% binding resin and polyvinylpyrrolidine K30, 1.8 wt% adipic acid, 0.2 wt% succinic acid, 0.8 wt% plasticizer, 1.2 wt% pigment Polygloss 90 and aluminum paste. The fluxes were coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0111] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 30-35%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0112] A flexible, reflective UV curable flux was prepared by combining moderately activated rosin anhydride adduct, polypropylene glycol diglycidyl ether, Irgacure 184 (or Ciba Darocur® 1173), adipic acid, and succinic acid as described in Example 1. The flux is inherently reflective and a pigment such as Aluminum Paste-100 is dispersed in the flux. The flux in this example contains 3 wt% rosin anhydride adduct, 4 wt% polypropylene glycol diglycidyl ether, 1 wt% Ciba Darocur® 1173, 1.8 wt% adipic acid, 0.4 wt% succinic acid, and 1.2 wt% inorganic dye Aluminum Paste-100.

[0113] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 14-16%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0114] A flexible, reflective UV curable flux was prepared by combining moderately activated rosin anhydride adduct, polypropylene glycol diglycidyl ether, Irgacure 184 (or Ciba Darocur® 1173), adipic acid, and succinic acid as described in Example 1. The flux is inherently reflective and a pigment such as Aluminum Paste-100 is dispersed in the flux. The flux in this example contains 6 wt% rosin anhydride adduct, 5 wt% polypropylene glycol diglycidyl ether, 2 wt% Ciba Darocur® 1173, 2 wt% adipic acid, 0.6 wt% succinic acid, and 1 wt% inorganic pigment Aluminum Paste-100.

[0115] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 13-15%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0116] A flexible and reflective flux was prepared as described in Example 1 by combining different types of binding resins, KE604, partially dimerized rosin (Poly-Pale), plasticizers, and organic acids such as adipic acid. The flux is inherently reflective and pigment carbon black was dispersed in the flux. The flux in this example contains 1.6 wt% binding resin, 0.6 wt% Ke604, 0.4 wt% Polypale rosin, 2.2 wt% adipic acid, 0.6 wt% plasticizer, and 1 wt% pigment carbon black. The flux was coated onto a ribbon. This resulted in a black coating for the aesthetics of the solar panel.

[0117] The elasticity of this flux was tested by twisting a flux-coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0118] A flexible and reflective flux was prepared by combining different types of binding resins, plasticizers, organic acids such as adipic acid and succinic acid, and dispersants as described in Example 1. The flux is inherently reflective and inorganic pigments such as Polygloss 90 and aluminum paste 100 are dispersed in the flux. The flux in this example contains 5 wt% binding resin, 2.2 wt% adipic acid and succinic acid, 0.6 wt% Disperse-BYK-180, 1.2 wt% pigment polygloss 90 and aluminum paste. The flux was coated on ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0119] The elasticity of this flux was tested by twisting a flux-coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux was subjected to reflectance analysis and had a reflectance of 15-16%. This flux was completely tack-free when applied and immediately dried. Tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0120] The flux in this example, which is a repeat of Example 1, contains equal amounts of 2.5% by weight of two binder resins, 2.2% by weight of organic acids such as adipic acid and succinic acid, 0.8% by weight of plasticizer, and 1.1% by weight of pigment. The flux was coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0121] The elasticity of this flux was tested by twisting a flux coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux coated ribbon was subjected to reflectance analysis and had a reflectance of 34-38%. The flux was completely tack-free when applied and allowed to dry for 5-6 seconds and tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0122] The flux in this example, which is a repeat of Example 1, is 4 wt% binding resin, 2.2 wt% organic acids such as adipic acid and succinic acid, 1 wt% plasticizer, and 1.1 wt% pigment spacer such as polygloss-90 and BLR-698 (TiO2 submicron particles). This flux was coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0123] The elasticity of this flux was tested by twisting a flux-coated ribbon through more than 360° and bending the ribbon through an angle of more than 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux-coated ribbon was subjected to reflectance analysis and had a reflectance of 33-36%. The flux was completely tack-free when applied and allowed to dry for 5-6 seconds and tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0124] The flux in this example, which is a repeat of Example 1, is 3.8 wt% binder resin, 2.2 wt% organic acids such as adipic acid and succinic acid, 0.8 wt% plasticizer, and 0.6% Ke604, 0.4% polypal rosin, and 1.1 wt% pigment spacers polygloss-90 and BLR-698 (TiO2 submicron particles). This flux was coated onto ribbons and the ribbons were subjected to reflectance analysis, and the high reflectivity of these fluxes increased the power output of the solar panel by 2.5%.

[0125] The elasticity of this flux was tested by twisting a flux coated ribbon through 360° and bending the ribbon through an angle of 360° and inspecting for cracks and adhesion of the coating on the ribbon. The flux coated ribbon was subjected to reflectance analysis and had a reflectance of 31-35%. The flux was completely tack-free when applied and allowed to dry for 5-6 seconds and tack was characterized by IPC-TM-650 method 2.4.44 dated March 1998. EXAMPLES

[0126] Example 21 was repeated, except that carbon black was added in addition to the inorganic white pigment (TiO2). EXAMPLES

[0127] Example 21 was repeated, except that carbon black was added to the composition instead of inorganic white pigment (TiO2) and a pigment spacer such as polygloss-90, which is a non-reflective flux used to improve the aesthetics of solar panels. EXAMPLES

[0128] Example 21 was repeated, except that in addition to the inorganic white pigment (TiO2), Solvent Black 27 was added. This gave the ribbon a black coating that was ideal for aesthetic purposes and slightly improved reflectivity.

[0129] A summary of the results of these examples follows.

[0130] [Table 1]

[0131] The foregoing detailed description has been provided by way of illustration and description and is not intended to limit the scope of the appended claims. Many variations of the presently preferred embodiments described herein will be apparent to those of ordinary skill in the art and remain within the scope of the appended claims and their equivalents.

Claims

1. 1. A method for manufacturing a solar module, comprising: connecting a metallic interconnect to two or more solar cells; applying a transparent cover sheet to the two or more solar cells; Connecting the metallic interconnect to each solar cell of the two or more solar cells includes Providing a solar cell having a bus bar on a surface thereof; Providing a metallic interconnect having solder flux on a contact surface thereof; providing solder between the busbar and the contact surface; reflowing the solder to connect the metallic interconnect to the bus bar; The method of claim 1, wherein the solder flux comprises a reflective additive.

2. The method of claim 1 , wherein the reflective additive comprises a dye and / or a pigment.

3. 3. The method of claim 1 or 2, wherein the reflective additive comprises a pigment comprising one or more of iron oxide, zinc oxide, aluminum oxide, titanium dioxide, chromium oxide, and ferric ammonium ferrocyanide.

4. 10. The method of any one of the preceding claims, wherein the reflective additive comprises a pigment comprising titanium dioxide, preferably the titanium dioxide is in the form of flakes, more preferably the titanium oxide flakes are coated with alumina and / or zirconia.

5. 10. The method of any one of the preceding claims, wherein the dye comprises a fluorescent dye.

6. 10. The method of any one of the preceding claims, wherein the solder flux further comprises an optical brightener.

7. 10. The method of any one of the preceding claims, wherein the reflective additive is white or yellow.

8. 10. The method according to any one of the preceding claims, wherein the flux comprises 0.1 to 15 wt. % of a reflective additive, preferably 0.3 to 2 wt. % of a reflective additive, based on the total weight of the solder flux.

9. 10. The method according to any one of the preceding claims, wherein the solder flux further comprises an acrylic resin binder, preferably a methacrylic resin binder.

10. 10. The method of claim 9, wherein the solder flux comprises 1-10 wt. % acrylic resin binder, preferably 2-6 wt. % acrylic resin binder, based on the total weight of the solder flux.

11. 10. The method of any one of the preceding claims, wherein the solder flux further comprises a vinyl resin binder.

12. The method of claim 11, wherein the solder flux comprises 0.1 to 5 wt % vinyl resin binder, preferably 0.5 to 2 wt % vinyl resin binder, based on the total weight of the solder flux.

13. 10. The method of any one of the preceding claims, wherein the solder flux comprises an acrylic resin binder and a vinyl resin binder.

14. 10. The method of any one of the preceding claims, wherein the solder flux further comprises an activator, preferably an activator comprising a dicarboxylic acid, preferably the dicarboxylic acid being selected from one or more of adipic acid, glutaric acid and succinic acid.

15. The method of claim 14, wherein the solder flux comprises 1 to 5 weight percent activator, based on the total weight of the solder flux.

16. 10. The method of any one of the preceding claims, wherein the solder flux further comprises one or more of a resin, a rosin, a wetting agent, an antifoaming agent, a plasticizer, and a dispersing agent.

17. 10. The method of any one of the preceding claims, wherein the busbars comprise copper, tin or silver connection pads, and reflowing the solder connects the metallic interconnects to the copper, tin or silver connection pads.

18. 10. The method of any one of the preceding claims, wherein the metallic interconnect comprises a copper or copper alloy ribbon.

19. 10. A method according to any one of the preceding claims, wherein the transparent cover sheet comprises glass, preferably textured glass.

20. 1. A method for connecting a metallic interconnect to a solar cell, comprising: Providing a solar cell having a bus bar on a surface thereof; Providing a metallic interconnect having solder flux on a contact surface thereof; providing solder between the busbar and the contact surface; reflowing the solder to connect the metallic interconnect to the bus bar; The method of claim 1, wherein the solder flux comprises a reflective additive.

21. 1. A metallic interconnect for a solar cell, the metallic interconnect having a solder flux on a surface thereof, the solder flux including a reflective additive and being substantially free of solvents.

22. A solder flux comprising a solid component and optionally a solvent, said solid component comprising a reflective additive.

23. The solder flux of claim 22, wherein the solder flux comprises 85-95% by weight of a solvent.

24. 24. The solder flux of claim 22 or 23, wherein the solvent comprises isopropyl alcohol.

25. Based on the total weight of the solder flux, 85-95% by weight of isopropyl alcohol solvent; 0.5 to 10% by weight of a methacrylic resin binder; 0.1 to 5 weight percent of a vinyl resin binder; 1-5 wt. % of an activator; 0.3-2% by weight of a reflective additive, preferably said reflective additive comprising titanium dioxide, more preferably in powder form; 25. The solder flux of claim 22, optionally comprising 0.1-2 wt. % of a wetting agent.

26. 23. The solder flux of claim 22, wherein the solder flux is substantially free of solvents.

27. A solder flux comprising a solid component and optionally a solvent, said solid component comprising a black and / or blue pigment.

28. 28. The solder flux of claim 27, wherein the black and / or blue pigments are selected from iron oxide and chromium(III) oxide pigments and carbon black.

29. Based on the total weight of the solder flux, 85-95% by weight of isopropyl alcohol solvent; 0.5 to 10% by weight of a methacrylic resin binder; 0.1 to 5 weight percent of a vinyl resin binder; 1-5 wt. % of an activator; 0.5 to 2% by weight of a black pigment selected from iron oxide and chromium [III] oxide pigments and carbon black; 29. The solder flux of claim 27 or 28, optionally comprising 0.1 to 2 wt. % of a wetting agent.

30. 28. The solder flux of claim 27, wherein the solder flux is substantially free of solvents.

31. A solar module manufactured according to the method of any one of claims 1 to 19.

32. 22. A method for producing the metallic interconnect of claim 21, comprising: Providing a metallic interconnect; Providing a solder flux according to any one of claims 22 to 25; applying the solder flux to the metallic interconnect; and removing the solvent from the solder flux by evaporation.

33. 22. A method for producing the metallic interconnect of claim 21, comprising: Providing a metallic interconnect; Providing a solder flux according to claim 26; Melting the solder flux; and applying the molten solder flux to the metallic interconnect.

Citation Information

Patent Citations

  • Coated metal ribbon for connecting solar cells

    EP3840062A1

  • Method for checking soldering and flux for checking

    JP1982070082A

  • Flux of solder for joining electronic part

    JP1992262892A

  • Method and device of detecting flux application

    JP2013185877A

  • Solar cell module and method of manufacturing solar cell module

    JP2015008221A

Cited By

  • Composite welding aid material, preparation method thereof and photovoltaic module lamination welding process

    CN120587752A