Method for Producing Silicon-Containing Materials
By depositing silicon within porous particles and then etching off excess silicon, the method addresses the stability issues in silicon-containing anodes, enhancing the cycle life and capacity retention of lithium-ion batteries.
Patent Information
- Application Number
- JP2024532795
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-12-02
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-12-02
AI Technical Summary
Existing methods for producing silicon-containing materials for lithium-ion battery anodes face challenges such as low cycle stability due to volume changes and irreversible capacity loss caused by the formation of thick silicon layers, which interact with the electrolyte and form a continuous solid electrolyte interphase (SEI), leading to rapid degradation.
A method involving the deposition of silicon within porous particles followed by controlled etching to remove excess silicon, resulting in a silicon-containing material with a controlled silicon layer thickness and improved stability.
The method enhances the cycling stability and reduces irreversible capacity loss by minimizing the adverse effects of thick silicon layers, leading to improved performance and capacity retention in lithium-ion batteries.
Smart Images

Figure 2024544769000001 
Figure 2024544769000002 
Figure 2024544769000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for utilizing silicon-containing materials by removing excess silicon from the particle surface, and to the use of the silicon-containing materials thus obtained as active materials for the anodes of lithium-ion batteries. [Background technology]
[0002] As a storage medium for electrical power, lithium-ion batteries are currently the most practical electrochemical energy stores with the highest energy density. Lithium-ion batteries are mainly used in the field of portable electronics, for tools, and for electrically driven transport such as bicycles, scooters, or automobiles. Graphitic carbon is currently widely used as an active material for the negative electrode ("anode") of the corresponding battery. However, a drawback is the relatively low electrochemical capacity of such graphitic carbon, which is theoretically a maximum of 372 mAh per gram of graphite, thus corresponding to only about one tenth of the electrochemical capacity theoretically achievable with lithium metal. An alternative active material for the anode uses the addition of silicon, as described for example in EP1730800B1, US10,559,812B2, US10,819,400B2, or EP3335262B1. Silicon forms a binary electrochemically active alloy with lithium, which allows very high electrochemically achievable lithium contents of up to 3579 mAh per gram of silicon [M. Obrovac, V. Chevrier Chem. Rev. 2014, 114, 11444].
[0003] The intercalation and deintercalation of lithium ions in silicon suffers from the drawback of a very significant volume change, which can reach up to 300% in the case of complete intercalation. Such volume change imposes significant mechanical loads on the silicon-containing active material, which may eventually lead to its decomposition. This process, also called electrochemical polishing, leads to a loss of electrical contact in the active material and the electrode structure, thus resulting in a sustained and irreversible loss of capacity of the electrode.
[0004] Furthermore, the surface of the silicon-containing active material reacts with the constituents of the electrolyte, and a passivating protective layer (solid electrolyte interphase interface, SEI) is continuously formed. The formed components are no longer electrochemically active. The lithium bound there is no longer available to the system, leading to a significant and continuous loss of capacity of the battery. Due to the extreme changes in the volume of silicon during the charge / discharge process of the battery, the SEI periodically collapses, which means that the not yet occupied surface of the silicon-containing active material is exposed and then undergoes further SEI formation. Since the amount of mobile lithium in a complete cell corresponding to the usable capacity is limited by the cathode material, it is increasingly consumed and the capacity of the cell drops to an unacceptable extent from the performance point of view after only a few cycles.
[0005] The decrease in capacity over the course of multiple charge and discharge cycles is also called fading or continuous loss of capacity, and is generally irreversible.
[0006] A series of silicon-carbon composite particles have been described as active materials for the anode of lithium ion batteries, where silicon is incorporated into porous carbon particles starting from a gas or liquid precursor.
[0007] For example, US 10,147,950 B2 describes the deposition of silicon from monosilane SiH4 in porous carbon at high temperatures of 300°C to 900°C in a tube furnace or equivalent furnace type, preferably with particle agitation, by a CVD ("chemical vapor deposition") or PE-CVD ("plasma-enhanced chemical vapor deposition") process. It uses a mixture of 2 mol% monosilane and nitrogen as an inert gas. The low concentration of silicon precursor in the gas mixture leads to very long reaction times. Furthermore, US 10,147,950 B2 discloses several possible combinations of different temperature ranges from 300°C to 900°C and different pressure ranges from 0.01 to 100 bar for carrying out the deposition of silicon on and in the porous starting material.
[0008] US10,424,786B1 describes a similar procedure, in which the silicon precursor is introduced as a mixture with an inert gas at a total pressure of 1.013 bar. WO2012 / 097969A1 describes the deposition of ultrafine silicon particles in the range of 1-20 nm by heating silane as silicon precursor on a porous carbon support at 200°C-950°C, the silane being diluted with an inert gas to prevent weak agglomeration of the deposited silicon particles or the formation of a thick layer, and the deposition being carried out in the pressure range of 0.1-5 bar.
[0009] Motevalian et al., Ind. Eng. Chem. Res. 2017, 56, 14995, describe the deposition of silicon layers at high pressure, but not in the presence of a porous matrix. Again, the silicon precursor used, in this case monosilane SiH4, is only present in low concentrations of up to 5 mol% in the total gas volume.
[0010] The above mentioned methods have various significant drawbacks. The silicon precursors are usually used at low absolute and partial pressures and therefore at low concentrations, which requires long reaction times to achieve a high silicon ratio in the silicon-containing material, since otherwise a thick Si layer would form on the outside of the particles. These thick silicon layers are detrimental in that they come into contact with the electrolyte and, in the course of cycling, lead to a high degree of structuring of the particle surface in combination with a continuous regeneration of the SEI. Furthermore, the optimal adjustment of the process parameters requires an accurate knowledge of all reaction parameters, which usually have to be determined empirically. In addition, the porous matrices used exhibit a certain range of variation in terms of their pore and particle size distribution, so that over-infiltration by the silicon precursor, which results in a thick silicon layer, cannot be excluded. If, for productivity reasons, infiltration occurs at a relatively high concentration of the Si precursor and / or at a relatively high temperature, a thick Si layer is also formed. In the course of these empirical studies, the production of batches of materials with unfavorable product properties is inevitable. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] European Patent No. 1730800 [Patent Document 2] U.S. Pat. No. 10,559,812 [Patent Document 3] U.S. Patent No. 10,819,400 [Patent Document 4] European Patent No. 3335262 [Patent Document 5] U.S. Patent No. 10,147,950 [Patent Document 6] U.S. Pat. No. 10,424,786 [Patent Document 7] International Publication No. 2012 / 097969 [Non-patent literature]
[0012] [Non-Patent Document 1] M.Obrovac, V.Chevrier Chem.Rev.2014, 114, 11444 [Non-Patent Document 2] Motevalian et al., Ind. Eng. Chem. Res. 2017, 56, 14995 Summary of the Invention [Problem to be solved by the invention]
[0013] Against this background, the objective was to find a method for utilizing batches of materials with adverse product properties that would allow the use of silicon-containing materials as active materials in anodes of lithium-ion batteries with high cycling stability. [Means for solving the problem]
[0014] The present invention provides a method for producing an etched silicon-containing material, comprising the steps of: In a first step, silicon is deposited in the pores and on the surface of the porous particles by pyrolysis of a silicon precursor on the porous particles to form a silicon-containing material; A method is provided in which in a second step a portion of the deposited silicon of the silicon-containing material is removed by etching off.
[0015] Surprisingly, this objective has been achieved by a method in which silicon applied in excess to a particle surface is essentially removed from said surface in a controlled manner via an etching treatment of the over-infiltrated particles.
[0016] The adverse effects of grain structuring caused by thick Si layers during cycling are surprisingly overcome by the method according to the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The silicon-containing material is preferably composed of silicon-containing particles.They can be obtained, for example, by pyrolyzing one or more silicon precursors in the presence of one or more porous particles, whereby silicon is deposited in the pores and on the surface of the porous particles.
[0018] The silicon-containing material can be produced in any desired reactor that is conventional for the deposition of silicon from silicon precursor.Preferably, the reactor is selected from the group that includes fluidized bed reactor, rotary tubular furnace that can be oriented in any desired configuration from horizontal to vertical, and fixed bed reactor that can be operated as an open or closed system, for example as a pressure reactor.Particularly preferred is a reactor that allows the porous particles and the silicon-containing material formed during deposition to be homogeneously mixed with the silicon precursor.This is advantageous for the deposition of silicon in the pores and on the surface of the porous particles as homogeneous as possible.The most preferred reactor is a fluidized bed reactor, a rotary tubular furnace or a pressure reactor, in particular a fluidized bed reactor or a pressure reactor.
[0019] The silicon precursors used contain at least one reactive component capable of reacting under selected conditions, e.g., thermal treatment, to give silicon. The reactive components are preferably monosilane SiH4, disilane Si2H6, and higher linear, branched or cyclic homologs, neopentasilane Si5H 12 , Cyclohexasilane Si6H 12silanes such as chlorosilanes MeHSiCl3, dichlorosilanes H2SiCl2, chlorosilanes H3SiCl, tetrachlorosilane SiCl4, hexachlorodisilane Si2Cl6, and higher linear, branched or cyclic homologues such as 1,1,2,2-tetrachlorodisilane Cl2HSi-SiHCl2, chlorinated and partially chlorinated oligo- and polysilanes such as chlorine-containing silanes such as trichloromethylsilane MeSiCl3, dichlorodimethylsilane Me2SiCl2, chlorotrimethylsilane Me3SiCl, tetramethylsilane Me4Si, dichloromethylsilane MeHSiCl2, chloromethylsilane MeH2SiCl, methylsilanes MeH3Si, chlorodimethylsilane Me2HSiCl, dimethylsilane Me2H2Si, trimethylsilane Me3SiH, methylchlorosilanes, or mixtures of the listed silicon compounds.
[0020] The reactive component may also contain further reactive constituents, such as dopants based on compounds containing boron, nitrogen, phosphorus, arsenic, germanium, iron or nickel, preferably selected from the group comprising ammonia NH3, diborane B2H6, phosphane PH3, germane GeH4, arsine AsH3, iron pentacarbonyl Fe(CO)4 and nickel tetracarbonyl Ni(CO)4.
[0021] Further reactive constituents which may be present in the reactive component include hydrogen, hydrocarbons, for example aliphatic hydrocarbons having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, such as methane, ethane, propane, butane, pentane, isobutane, hexane, cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, unsaturated hydrocarbons having 1 to 10 carbon atoms, such as ethene, acetylene, propene or butene, isoprene, butadiene, divinylbenzene, vinylacetylene, cyclohexadiene, cyclooctadiene, cyclic unsaturated hydrocarbons, such as cyclopropene, cyclobutene, cyclopentene, cyclohexene, cyclohexadiene, cyclopentadiene, dicyclopentadiene or norbornadiene, aromatic hydrocarbons, such as benzene, toluene, p-, m-, o-xylene, styrene (vinylbenzene), ethylbenzene, diphenylmethane or naphthalene, further aromatic hydrocarbons such as phenol, o-, m-, p-cresol, cymene, nitrobenzene, chlorobenzene, pyridine, anthracene or phenanthrene, myrcene, geraniol, thioterpineol, norbornane, borneol, isoborneol, bornane, camphor, limonene, terpinene, pinene, pinane, carene, phenol, aniline, anisole, furan, furfural, furfuryl alcohol, hydroxymethylfurfural, bishydroxymethylfuran and mixed fractions containing a large number of such compounds, such as those from natural gas condensates, petroleum distillates or coke oven condensates, mixed fractions from the product streams of fluid catalytic crackers (FCC), steam crackers or Fischer-Tropsch synthesis plants or more generally hydrocarbon-containing material streams from wood, natural gas, petroleum and coal processing.
[0022] The process for Si deposition is preferably carried out in an inert gas atmosphere, such as a nitrogen or argon atmosphere.
[0023] This process may be carried out in a conventional manner requiring routine adjustments that are normal to those skilled in the art, as is otherwise customary for the deposition of silicon from silicon precursors.
[0024] The porous particles for the process according to the invention are preferably selected from the group comprising amorphous carbon in the form of hard carbon, soft carbon, mesocarbon microbeads, natural or synthetic graphite, single-walled and multi-walled carbon nanotubes and graphene, oxides such as silicon dioxide, aluminum oxide, silicon-aluminum mixed oxide, magnesium oxide, lead oxide and zirconium oxide, carbides such as silicon carbide and boron carbide, nitrides such as silicon nitride and boron nitride, as well as other ceramic materials as may be described by the following formula: Al a B b C c Mg d N e O f S g , where 0≦a, b, c, d, e, f, g≦1, at least two coefficients a~g>0, and a*3+b*3+c*4+d*2+g*4≧e*3+f*2.
[0025] The ceramic material may be, for example, a binary, ternary, quaternary, pentanary, hexanary or heptanary compound. Ceramic materials having the following formula are preferred: Non-stoichiometric Boron Nitride BN z (In the formula, z=0.2~1) Non-stoichiometric carbon nitride CN z (In the formula, z=0.1~4 / 3) Boron carbonitride B x CN z (In the formula, x=0.1 to 20 and z=0.1 to 20, and x*3+4≧z*3) Boron Nitride Oxide BN z O r (wherein z=0.1 to 1 and r=0.1 to 1, and 3≧r*2+z*3) Boron Carbonitride Oxide B x CN z O r (In the formula, x=0.1 to 2, z=0.1 to 1, and r=0.1 to 1, and x*3+4≧r*2+z*3) Silicon Carboxide Si x COz (In the formula, x=0.1 to 2 and z=0.1 to 2, and x*4+4≧z*2) Silicon carbonitride Si x CN z (wherein x=0.1 to 3 and z=0.1 to 4, and x*4+4≧z*3) Silicon boron carbonitride Si w B x CN z (In the formula, w=0.1 to 3, x=0.1 to 2, and z=0.1 to 4, and w*4+x*3+4≧z*3) Silicon borocarboxide Si w B x CO z (In the formula, w=0.10 to 3, x=0.1 to 2, and z=0.1 to 4, and w*4+x*3+4≧z*2) Silicon borocarbonitride oxide Si v B w CN x O z (wherein v=0.1 to 3, w=0.1 to 2, x=0.1 to 4, and z=0.1 to 3, and v*4+w*3+4≧x*3+z*2) and Aluminum borosilicocarbonitride oxide Al u B v S x CN w O z (In the formula, u = 0.1 to 2, v = 0.1 to 2, w = 0.1 to 4, x = 0.1 to 2, and z = 0.1 to 3, and u*3 + v*3 + x*4 + 4 ≧ w*3 + z*2).
[0026] Porous particles have a particle size of 0.1-7 g / cm, as measured by helium pycnometry. 3 , particularly preferably 0.3 to 3 g / cm 3 This is in accordance with the gravimetric capacity (mAh / cm) of a lithium-ion battery. 3 ) is advantageous in increasing the
[0027] Preferably, as porous particles, amorphous carbon, silicon dioxide, boron nitride, silicon carbide and silicon nitride or mixed materials based on these materials are used, particularly preferred is the use of amorphous carbon, boron nitride and silicon dioxide.
[0028] The porous particles preferably have a diameter percentile d of ≧0.5 μm, particularly preferably ≧1.5 μm, most preferably ≧2 μm. 50 The diameter percentile d 50 is preferably ≦20 μm, particularly preferably ≦12 μm, most preferably ≦8 μm.
[0029] The volume weighted particle size distribution of the porous particles is preferably determined by the diameter percentile d 10 ≧0.2μm~d 90 ≦20.0 μm, particularly preferably d 10 ≧0.4μm~d 90 ≦15.0 μm, most preferably d 10 ≧0.6μm~d 90 ≦12.0 μm.
[0030] The porous particles preferably have a diameter percentile d of ≦10 μm, particularly preferably ≦5 μm, particularly preferably ≦3 μm, most preferably ≦2 μm. 10 The diameter percentile d 10 is preferably ≧0.2 μm, particularly preferably ≧0.5, most preferably ≧1 μm.
[0031] The porous particles preferably have a diameter percentile d of ≧4 μm, particularly preferably ≧8 μm. 90 The diameter percentile d 90 is preferably ≦18 μm, particularly preferably ≦15, most preferably ≦13 μm.
[0032] The volume-weighted particle size distribution of the porous particles preferably has a width d 90 -d 10 has.
[0033] The volume-weighted particle size distribution of the silicon-containing material producible by the method according to the invention preferably has a width d 90 -d 10 has.
[0034] The volume weighted particle size distribution of the porous particles can be determined according to ISO 13320 by static laser scattering using the Mie model on a Horiba LA 950 measuring instrument using ethanol as the dispersion medium for the porous particles.
[0035] The particles may be, for example, in isolated or agglomerated form. The porous particles are preferably not agglomerated, and preferably not agglomerated. Agglomeration generally means that in the course of the production of the porous particles, primary particles are first formed and then coalesce and / or the primary particles are linked to each other, for example via covalent bonds, thus forming agglomerates. The primary particles are usually isolated particles. The aggregates or isolated particles may form agglomerates. Agglomerates are loose accumulations of agglomerates or primary particles linked to each other, for example via van der Waals interactions or hydrogen bonds. Agglomerates that have agglomerated can be easily broken back into agglomerates again by standard kneading and dispersion processes. Agglomerates can only be partially, if at all, broken down into primary particles by such processes. The presence of the porous particles in the form of agglomerates, agglomerates or isolated particles can be visualized, for example, using a conventional scanning electron microscope (SEM). In contrast, static light scattering methods for determining particle size distribution or particle size of matrix particles cannot distinguish between strong and weak agglomerates.
[0036] The porous particles may have any desired morphology, i.e. for example, crushed, flaky, spherical or acicular, with crushed or spherical particles being preferred. The morphology can be characterized, for example, by the sphericity ψ or the sphericity S. According to Wadell's definition, the sphericity ψ is the ratio of the surface area of a sphere of equal volume to the actual surface area of the object. For a sphere, ψ has a value of 1. According to this definition, the porous particles for the method according to the invention preferably have a sphericity ψ of 0.3 to 1.0, particularly preferably 0.5 to 1.0, most preferably 0.65 to 1.0.
[0037] Sphericity S is the ratio of the circumference of an equivalent circle having the same area A as the projection of the particle onto the surface to the measured circumference U of this projection.
number
[0038] The porous particles preferably have a diameter of ≧0.2 cm 3 / g, particularly preferably ≧0.6 cm 3 / g, most preferably ≥ 1.0 cm 3 / g, which allows high-capacity lithium-ion batteries to be obtained. The gas-accessible pore volume was determined by gas sorption measurements with nitrogen according to DIN 66134.
[0039] The porous particles preferably have open pores. Open pores generally means that the pores are connected to the surface of the particle, for example via channels, and are preferably capable of mass exchange with the environment, in particular gaseous compounds. This can be demonstrated by gas sorption measurements (analysis according to Brunauer, Emmett and Teller, "BET"), i.e. the specific surface area. The porous particles preferably have a specific surface area of ≥ 100 m 2 / g, particularly preferably ≥ 500m 2 / g, particularly preferably ≥ 1000m 2 / g, most preferably ≥ 1500m 2 / g. The BET specific surface area is determined in accordance with DIN 66131 (with nitrogen).
[0040] The pores of the porous particles may have any desired diameter, i.e. generally in the range of macropores (more than 50 nm), mesopores (2-50 nm) and micropores (less than 2 nm). The porous particles may be used in any desired mixture of different pore types. Preference is given to using porous particles with less than 30% macropores based on the total pore volume, particularly preferred are porous particles with no macropores, very particularly preferred are porous particles with at least 50% pores with an average pore diameter of less than 5 nm. Very particularly preferably, the porous particles only have pores with a pore diameter of less than 2 nm (determination method: in the mesopore range pore size distribution according to BJH (gas adsorption) according to DIN 66134 and in the micropore range pore size distribution according to Horvath-Kawazoe (gas adsorption) according to DIN 66135, in the macropore range the pore size distribution is evaluated by mercury porosimetry according to DIN ISO 15901-1).
[0041] Preferably, 0.3 cm 3 / g, particularly preferably less than 0.15 cm 3 The porous particles have a gas inaccessible pore volume of less than 1 / g. This can also increase the capacity of lithium ion batteries. The gas inaccessible pore volume can be determined using the following formula: Gas inaccessible pore volume = 1 / pure material density - 1 / skeletal density.
[0042] Pure material density is the theoretical density of a porous particle based on the phase composition or density of the pure material (the density of the material as if it had no closed pores). Pure material density data can be found by one of skill in the art, for example, at the Ceramic Data Portal of the National Institute of Standards (NIST, https: / / srdata.nist.gov / CeramicDataPortal / scd). For example, the pure material density of silicon oxide is 2.20 g / cm 3 The density of the pure material of boron nitride is 2.25g / cm 3 The density of the pure silicon nitride is 3.44 g / cm 3 The density of pure silicon carbide is 3.21 g / cm 3 Skeletal density is the actual density of the porous particles (gas accessible) as determined by helium pycnometry.
[0043] For the sake of clarity, it should be noted that porous particles are different from silicon-containing materials.Porous particles act as the starting material for producing silicon-containing materials.Preferably, there is no silicon located in the pores of porous particles and on the surface of porous particles, more specifically, there is no silicon obtained by depositing silicon precursors.
[0044] The silicon-containing material obtainable by depositing silicon in the pores and on the surface of porous particles by the method according to the invention preferably has a diameter percentile d in the range of 0.5 to 20 μm. 50 d 50 A value of at least 1.5 μm is preferred, and at least 2.0 μm is particularly preferred. Diameter percentile d 50 is preferably at most 13 μm, particularly preferably at most 8 μm.
[0045] The volume weighted particle size distribution of the silicon-containing material is preferably determined by the diameter percentile d 10≧0.2μm~d 90 ≦20.0 μm, particularly preferably d 10 ≧0.4μm~d 90 ≦15.0 μm, most preferably d 10 ≧0.6μm~d 90 ≦12.0 μm.
[0046] The silicon-containing material preferably has a diameter percentile d of ≦10 μm, particularly preferably ≦5 μm, particularly preferably ≦3 μm, most preferably ≦1 μm. 10 The diameter percentile d 10 is preferably ≧0.2 μm, particularly preferably ≧0.4 μm, most preferably ≧0.6 μm.
[0047] The silicon-containing material preferably has a diameter percentile d of ≧5 μm, particularly preferably ≧10 μm. 90 The diameter percentile d 90 is preferably ≦20 μm, particularly preferably ≦15 μm, most preferably ≦12 μm.
[0048] The volume-weighted particle size distribution of the silicon-containing material preferably has a width d 90 -d 10 The volume-weighted particle size distribution of the silicon-containing material preferably has a width d 90 -d 10 has.
[0049] The silicon-containing material is preferably in the form of particles.The particles can be in isolated form or weakly aggregated form.The silicon-containing material is preferably not strongly aggregated, and preferably not strongly aggregated.The terms isolated, weakly aggregated, and non-strongly aggregated have already been further defined above with respect to porous particles.The presence of the silicon-containing material in the form of strong aggregate or weakly aggregated can be visualized, for example, by using a conventional scanning electron microscope (SEM).
[0050] The silicon-containing material may have any desired morphology, i.e., for example, crushed, flaked, spherical, or acicular, with crushed or spherical particles being preferred.
[0051] According to Wadell's definition, sphericity ψ is the ratio of the surface area of a sphere of equal volume to the actual surface area of the object. For a sphere, ψ has the value 1. According to this definition, the silicon-containing material obtainable by the method according to the invention preferably has a sphericity ψ of 0.3 to 1.0, particularly preferably 0.5 to 1.0, most preferably 0.65 to 1.0.
[0052] Sphericity S is the ratio of the circumference of an equivalent circle having the same area A as the projection of the particle onto the surface to the measured circumference U of this projection.
number
[0053] The cycling stability of lithium-ion batteries can be further enhanced by the morphology, material composition, especially the specific surface area or internal porosity of silicon-containing materials.
[0054] The silicon-containing material contains, based on the total weight of the silicon-containing material, preferably 10% by weight to 90% by weight, more preferably 20% by weight to 80% by weight, particularly preferably 30% by weight to 60% by weight, and particularly preferably 40% by weight to 50% by weight of porous particles.
[0055] The silicon-containing material preferably contains 10% to 90% by weight, more preferably 20% to 80% by weight, particularly preferably 30% to 60% by weight, and particularly preferably 40% to 50% by weight of silicon obtained by deposition from a silicon precursor, based on the total weight of the silicon-containing material (preferably determined by elemental analysis such as ICP-OES).
[0056] When the porous particles contain a silicon compound, for example in the form of silicon dioxide, the weight percent values mentioned above can be determined for silicon obtained by deposition from a silicon precursor by subtracting the mass of silicon of the porous particles, determined by elemental analysis, from the mass of silicon of the silicon-containing material, determined by elemental analysis, and dividing the result by the mass of the silicon-containing material.
[0057] The volume of silicon present in a silicon-containing material and obtained via deposition from a silicon precursor is determined by the density of silicon (2.336 g / cm 3 The mass fraction of silicon obtained via deposition from a silicon precursor in the total mass of the silicon-containing material divided by the mass fraction of the silicon-containing material.
[0058] The pore volume P of the silicon-containing material results from the sum of the gas-accessible pore volume and the gas-inaccessible pore volume. The Gurwitsch gas-accessible pore volume of the silicon-containing material can be determined by gas sorption measurements with nitrogen according to DIN 66134.
[0059] The gas inaccessible pore volume of a silicon-containing material can be determined using the following formula: Gas inaccessible pore volume = 1 / pure material density - 1 / skeletal density.
[0060] The pure material density of the silicon-containing material is the theoretical density that can be calculated from the sum of the theoretical pure material densities of the components present in the silicon-containing material multiplied by the weight-related percentage of each of the total materials.As an example, for the silicon-containing material in which silicon is deposited on porous particles, this results in the following: Pure material density = theoretical pure material density of silicon * fraction of silicon (wt%) + theoretical pure material density of porous particles * fraction of porous particles (wt%).
[0061] The pore volume P of the silicon-containing material is in the range of 0 vol.% to 400 vol.%, preferably in the range of 100 vol.% to 350 vol.%, particularly preferably in the range of 200 vol.% to 350 vol.%, based on the volume of silicon present in the silicon-containing material and obtained from deposition from the silicon precursor.
[0062] The pores present in the silicon-containing material may be gas-accessible or gas-inaccessible. The volume ratio of gas-accessible pores to gas-inaccessible pores of the silicon-containing material can generally be in the range of 0 (no gas-accessible pores) to 1 (all pores are gas-accessible). The volume ratio of gas-accessible pores to gas-inaccessible pores of the silicon-containing material is preferably in the range of 0 to 0.8, particularly preferably in the range of 0 to 0.3, and particularly preferably in the range of 0 to 0.1.
[0063] The pores of the silicon-containing material may have any desired diameter, for example within the range of macropores (>50 nm), mesopores (2-50 nm) and micropores (<2 nm). The silicon-containing material may also contain any desired mixture of different pore types. Preferably, the silicon-containing material contains at most 30% macropores, based on the total pore volume, with silicon-containing materials without macropores being particularly preferred, and silicon-containing materials having at least 50% pores, based on the total pore volume, with an average pore diameter of less than 5 nm being very particularly preferred. Particularly preferably, the silicon-containing material has only pores with a diameter of at most 2 nm.
[0064] The silicon-containing material preferably has silicon structures with a structure size of at least one dimension of up to 1000 nm, more preferably less than 100 nm, particularly preferably less than 5 nm (determination method: scanning electron microscopy (SEM) and / or high-resolution transmission electron microscopy (HR-TEM)).
[0065] The silicon-containing material preferably comprises a silicon layer having a layer thickness of less than 1000 nm, more preferably less than 100 nm, particularly preferably less than 5 nm (determination method: scanning electron microscope (SEM) and / or high-resolution transmission electron microscope (HR-TEM)). The silicon-containing material may also contain silicon in the form of particles. The silicon particles preferably have a diameter of at most 1000 nm, more preferably less than 100 nm, particularly preferably less than 5 nm (determination method: scanning electron microscope (SEM) and / or high-resolution transmission electron microscope (HR-TEM)). Here, the data on the silicon particles preferably relate to the diameter of the circumference of the particle in the microscopic image.
[0066] Furthermore, the deposited silicon from the silicon precursor in the silicon-containing material may contain a dopant, for example selected from the group including Li, Fe, Al, Cu, Ca, K, Na, S, Cl, Zr, Ti, Pt, Ni, Cr, Sn, Mg, Ag, Co, Zn, B, P, Sb, Pb, Ge, Bi, rare earths or combinations thereof. Lithium and / or tin are preferred. The content of dopant in the silicon-containing material is preferably up to 1 wt.%, particularly preferably up to 100 ppm, based on the total weight of the silicon-containing material, which can be determined by ICP-OES.
[0067] Silicon-containing materials generally exhibit surprisingly high stability under compressive load and / or shear stress.The compressive load stability and shear stability of silicon-containing materials are evident, for example, from the fact that silicon-containing materials have little, if any, change in their porous structure in SEM under compressive load (e.g., during electrode compression) and shear stress (e.g., during electrode preparation).
[0068] The silicon-containing material may optionally contain additional elements such as carbon. The carbon is preferably in the form of a thin layer with a layer thickness of at most 1 μm, preferably less than 100 nm, particularly preferably less than 5 nm, very particularly preferably less than 1 nm (measurable by SEM or HR-TEM). The carbon layer may be present here both in the pores and on the surface of the silicon-containing material. The order of different layers in the silicon-containing material is also arbitrary. Thus, firstly, on the porous particles, there may be a layer of a further material different from the porous particles, such as carbon, on which there may be a silicon layer or a layer of silicon particles. Similarly, on the silicon layer or on the layer of silicon particles, there may be a layer of a further material that may be different from or identical to the material of the porous particles, regardless of whether a further layer of a material different from the material of the porous particles is present between the porous particles and the silicon layer or layer of silicon particles.
[0069] The silicon-containing material preferably contains ≦50% by weight, particularly preferably ≦40% by weight, particularly preferably ≦20% by weight of additional elements.The silicon-containing material preferably contains ≧1% by weight, particularly preferably ≧3% by weight, particularly preferably ≧2% by weight of additional elements.The figures in weight percent refer to the total weight of the silicon-containing material.In an alternative embodiment, the silicon-containing material does not contain any additional elements.
[0070] In the second step, some of the deposited silicon from the silicon-containing material is removed by etching off. Here, excess silicon, also called coarse silicon, is removed. Fine silicon is desired and remains on and in the etched silicon-containing material.
[0071] Preferably, the amount of excess silicon in the deposited silicon after etching is less than 3% by weight, particularly preferably less than 1% by weight, particularly preferably less than 0.1% by weight.
[0072] Fine and coarse silicon in a sample can be determined by TGA measurements due to the reaction of silicon with oxygen to form SiO2. The distinguishability of different silicon species can be explained by the fact that thin silicon layers show a higher reactivity towards oxygen than thick layers or Si particles. This has the consequence that in TGA measurements, thin Si layers react (gain in mass) even at low temperatures (400-650 ° C), while thick layers / coarse silicon structures show a reaction only at temperatures above 700 ° C. Ideally, silicon-containing composites used as anode active materials do not show an increase in mass in TGA measurements under oxygen-containing atmospheres at temperatures above 800 ° C. This method further allows the determination of the content of elemental silicon. Silicon previously oxidized and passivated by contact with air no longer takes part in the reaction and is therefore not taken into account in the TGA measurements.
[0073] To calculate the coarse silicon present, the residual mass (mres) from the TGA method and the mass difference (mdiff) due to oxidation of the coarse silicon are required. Using the molar mass of O2 (32 g / mol) and the molar mass of SiO2 (60.08 g / mol), the percentage of coarse silicon in the deposited silicon can be calculated by the following formula:
number
[0074] If it is desired to calculate the excess silicon of said material, the percentage of coarse silicon must be multiplied by the percentage of deposited silicon of said material.
[0075] Silicon can be removed from surfaces industrially in many ways. Liquid or gaseous etching media are particularly suitable for this. For liquid etching media, on the one hand, wet chemical routes based on HF under oxidizing conditions (e.g., HNO3 and acetic acid - HNA, as a mixture with CP4) have been established, while on the other hand, wet chemical treatments using basic solutions, e.g., solutions containing KOH, tetramethylammonium hydroxide (TMAH), NaOH, LiOH, CsOH, NH4OH, Mg(OH)2, Ca(OH)2, Ba(OH)2, ethylenediamine (EDP), have also been established. These wet chemical etching procedures can be carried out at room temperature (25°C), but also at elevated temperatures below the boiling point of the solution to accelerate the reaction. In addition to increasing the temperature, energy can also be introduced into the system via microwave or ultrasonic treatment. Etching processes below room temperature (<25°C) are also conceivable.
[0076] In addition to wet-chemical etching processes, etching processes via the gas phase are also known, in which, for example, XeF2 or SF6 can be used as gaseous etching medium and a plasma is induced.
[0077] The etching can be carried out either iteratively (starving of etching medium) while monitoring the coarse silicon content, or with the etching adjusted to the amount of coarse silicon (calculated amount of etching medium).
[0078] After etching, the etched silicon-containing material is preferably washed with a washing medium, preferably water.
[0079] After washing, the etched silicon-containing material is preferably separated from the washing medium and dried.
[0080] The etched silicon-containing material is preferably at most 80 m 2 / g, particularly preferably 30m 2 / g, particularly preferably less than 10m 2 / g. The BET specific surface area is determined according to DIN 66131 (with nitrogen). Therefore, when the silicon-containing material is used as an active material of the anode of a lithium-ion battery, the SEI formation can be reduced and the initial coulombic efficiency can be increased.
[0081] The present invention further provides the use of the etched silicon-containing material as an active material in an anode material for a lithium-ion battery anode, and the use of such an anode for producing a lithium-ion battery.
[0082] The anode material is preferably based on a mixture comprising the etched silicon-containing material obtainable by the method according to the invention, one or more binders, optionally graphite as further active material, optionally one or more further conductive components and optionally one or more additives.
[0083] The use of an additional conductive component in the anode material can reduce the contact resistance within the electrode and between the electrode and the current collector, thereby improving the current carrying capacity of the lithium-ion battery according to the invention. Preferred additional conductive components are, for example, conductive carbon black, carbon nanotubes or metal particles, such as copper.
[0084] The anode material preferably contains 0% to 95% by weight, particularly preferably 0% to 40% by weight, most preferably 0% to 25% by weight of one or more further conductive components, based on the total weight of the anode material.
[0085] The etched silicon-containing material may be present in the anode for a lithium-ion battery preferably to the extent of 5% to 100% by weight, particularly preferably 30% to 100% by weight, most preferably 60% to 100% by weight, based on all active material present in the anode material.
[0086] Preferred binders are polyacrylic acid or its alkali metal salts, in particular the lithium or sodium salts, polyvinyl alcohol, cellulose or cellulose derivatives, polyvinylidene fluoride, polytetrafluoroethylene, polyolefins, polyimides, in particular polyamide-imides, or thermoplastic elastomers, in particular ethylene-propylene-diene terpolymers. The alkali metal salts, in particular the lithium or sodium salts, of the aforementioned binders are also particularly preferred. All or preferably part of the acid groups of the binder may be in the form of a salt. The binder preferably has a molar mass of 100000 to 1000000 g / mol. Mixtures of two or more binders may be used.
[0087] The graphite used can be typically natural or synthetic graphite. The graphite particles preferably have a diameter percentile d 10 >0.2μm~d 90 <200 μm.
[0088] Examples of additives are pore formers, dispersants, levelling agents or dopants such as elemental lithium.
[0089] A preferred formulation for the anode material preferably contains 5 wt% to 95 wt% silicon-containing material, 0 wt% to 90 wt% further conductive component(s), 0 wt% to 90 wt% graphite, 0 wt% to 25 wt% binder and 0 wt% to 80 wt% additives, the figures in wt% referring to the total weight of the anode material and the percentages of all components of the anode material adding up to 100 wt%.
[0090] The components of the anode material are preferably processed into an anode ink or paste, preferably using a rotor-stator machine, high energy mill, planetary kneader, agitator bead mill, vibrating plate or ultrasonic equipment, preferably in a solvent selected from the group including water, hexane, toluene, tetrahydrofuran, N-methylpyrrolidone, N-ethylpyrrolidone, acetone, ethyl acetate, dimethylsulfoxide, dimethylacetamide and ethanol and mixtures of these solvents.
[0091] The anode ink or paste preferably has a pH of 2 to 8.5 (at 20° C., measured, for example, using a WTW pH340i pH meter equipped with a SenTix RJD probe).
[0092] The anode ink or paste can be applied to a copper foil or another current collector, for example, by a doctor blade. Other coating processes, such as spin coating, roller coating, dip or slot die coating, painting or spraying, can also be used in accordance with the present invention.
[0093] Prior to coating the copper foil with the anode material according to the invention, the foil may be treated with a commercially available primer, for example based on polymeric resins or silanes, which may provide improved adhesion to the copper but which generally have no substantial electrochemical activity themselves.
[0094] The anode material is usually dried to constant weight. The drying temperature is guided by the components used and the solvent used. The drying temperature is preferably between 20° C. and 300° C. The layer thickness, i.e. the dry layer thickness of the anode coating, is preferably between 2 and 500 μm.
[0095] Finally, the electrode coating may be calendered to set a defined porosity. The electrodes thus produced preferably have a porosity between 15% and 85%, which can be measured by mercury porosimetry according to DIN ISO 15901-1. Preferably, 25% to 85% of the pore volume thus determined is provided by pores with a pore diameter of 0.01 to 2 μm.
[0096] The present invention further provides a lithium ion battery comprising a cathode, an anode containing an etched silicon-containing material, two conductive connections to the electrodes, a separator, an electrolyte in which the separator and the two electrodes are impregnated, and a housing to contain the above components.
[0097] In the context of the present invention, the term lithium-ion battery also includes a cell. A cell generally includes a cathode, an anode, a separator, and an electrolyte. In addition to one or more cells, a lithium-ion battery preferably further includes a battery management system. A battery management system is generally used to control the battery, for example using electronic circuits, in particular to detect the state of charge, for over-discharge protection or over-charge protection.
[0098] Preferred cathode materials for use in accordance with the present invention may be lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt oxide (doped or undoped), lithium manganese oxide (spinel), lithium nickel cobalt manganese oxide, lithium nickel manganese oxide, lithium iron phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium vanadium phosphate or lithium vanadium oxide.
[0099] The separator is generally an electrically insulating, ion-permeable membrane, preferably made of polyolefin, such as polyethylene (PE) or polypropylene (PP), or polyester or a corresponding laminate. Alternatively, as is customary in battery manufacturing, the separator may be made of or coated with a glass or ceramic material. As is known, the separator separates the first electrode from the second electrode, thus preventing a conductive connection (short circuit) between the electrodes.
[0100] The electrolyte is preferably a solution containing one or more lithium salts (=conductive salts) in an aprotic solvent. The conductive salts are preferably selected from the group comprising lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium perchlorate, lithium tetrafluoroborate, lithium imide, lithium methide, lithium trifluoromethanesulfonate, LiCF3SO3, lithium bis(trifluoromethanesulfonimide) LiN(CF3SO2)2 and lithium borates. The concentration of the conductive salt is preferably between 0.5 mol / l and the solubility limit of the salt in question, based on the solvent. Particularly preferably, the concentration is between 0.8 and 1.2 mol / l.
[0101] The solvents used are preferably cyclic carbonates, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethoxyethane, diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, acetonitrile, organic carbonates or nitriles, used individually or as mixtures thereof.
[0102] The electrolyte preferably contains a film-forming agent such as vinylene carbonate or fluoroethylene carbonate. As a result, it is possible to achieve a significant improvement in the cycle stability of the anode containing the etched silicon-containing material obtained by the method according to the present invention. This is mainly due to the formation of a solid electrolyte interfacial interface at the surface of the active particles. The proportion of the film-forming agent in the electrolyte is preferably between 0.1% and 20.0% by weight.
[0103] In order to match the actual capacities of the electrodes of a lithium-ion cell to one another as best as possible, it is advantageous to balance the materials of the positive and negative electrodes with respect to their absolute capacities. Of particular importance in this context is the fact that at the first or initial charge / discharge cycle (known as activation) of a secondary lithium-ion cell, a coating layer forms on the surface of the electrochemically active material in the anode. This coating layer is called the "solid electrolyte interphase" (SEI) and generally consists mainly of electrolyte decomposition products and a certain amount of lithium, which is therefore no longer available for further charge / discharge reactions. The thickness and composition of the SEI depend on the anode material used and the type and quality of the electrolyte solution used.
[0104] In the case of graphite, the SEI is particularly thin: in graphite, there is typically a loss of 5% to 35% of the mobile lithium during the first charging step, with a corresponding decrease in the reversible capacity of the battery.
[0105] In the case of an anode with an etched silicon-containing active material obtained by the method according to the invention, there is preferably a loss of mobile lithium of at most 30%, particularly preferably at most 20% and most preferably at most 10% in the first charging step, which is much lower than the values described in the prior art such as US 10,147,950 B1.
[0106] All of the substances and materials utilized in the manufacture of such lithium ion batteries as described above are known, and the manufacture of the components of such batteries and their assembly to form the batteries is carried out according to methods known in the art of battery manufacturing.
[0107] The etched silicon-containing material obtained by the method according to the invention is characterized by a significantly improved electrochemical behavior, resulting in lithium-ion batteries with high volumetric capacity and excellent performance characteristics. The etched silicon-containing material obtained by the method according to the invention is permeable to lithium ions and electrons, thus allowing charge transport. The SEI in lithium-ion batteries can be significantly reduced by the etched silicon-containing material obtained by the method according to the invention. In addition, due to the design of the etched silicon-containing material obtained by the method according to the invention, the SEI peels off from the surface of the active material, if at all, at least to a much lesser extent. All this results in high cycle stability of the corresponding lithium-ion battery, the anode of which contains the etched silicon-containing material obtained by the method according to the invention.
[0108] The following examples serve to further elucidate the invention described herein.
[0109] The following analytical methods and instruments were used for characterization:
[0110] <Scanning electron microscopy (SEM / EDX)> Microscopic analysis was performed using a Zeiss Ultra 55 scanning electron microscope and an energy dispersive Oxford X-Max 80N X-ray spectrometer. Prior to analysis, the samples were subjected to deposition of carbon using a Safematic Compact Coating Unit 010 / HV to prevent charging phenomena. Cross sections of silicon-containing materials were prepared using a Leica TIC 3X ion cutter at 6 kV.
[0111] <Inorganic analysis / elemental analysis> The C content reported in the examples was determined with a Leco CS230 analyzer. For the determination of O and, where appropriate, N or H content, a Leco TCH-600 analyzer was used. Qualitative and quantitative determination of the other reported elements was carried out by ICP (inductively coupled plasma) optical emission spectrometry (Optima 7300 DV, Perikin Elmer). For this purpose, the samples were subjected to acid digestion (HF / HNO3) in a microwave (Microwave 3000, manufactured by Anton Paar). The ICP-OES determination was guided by ISO 11885 ("Water quality - Determination of selected elements by inductively coupled plasma optical emission spectrometry (ICP-OES) (ISO 11885:2007), German version of EN ISO 11885:2009"), which is used for the analysis of acidic aqueous solutions (e.g., acidified drinking water, wastewater and other water samples as well as aqua regia extracts of soil and sediments).
[0112] <Determination of particle size> In the context of the present invention, the particle size distribution was determined in accordance with ISO 13320 by static laser scattering using a Horiba LA 950. In the preparation of the samples, special care must be taken to disperse the particles in the measuring solution to ensure that what is measured is the size of the individual particles and not the size of weak aggregates. For the measurement, the particles were dispersed in ethanol. For this purpose, prior to measurement, the dispersion was treated with ultrasound at 250 W for 4 minutes in a Hielscher UIS250v laboratory ultrasonic device equipped with an LS24d5 sonotrode if necessary.
[0113] <BET specific surface area measurement> The specific surface area of the material was measured by the BET method (determination according to DIN ISO 9277:2003-05 using nitrogen) by gas adsorption with nitrogen using a Sorptomatic 199090 device (Porotec) or a SA-9603MP device (Horiba).
[0114] <Bone density> The skeletal density, i.e. the density of the porous solid based on the volume of the external gas-accessible pore space only, was determined by He pycnometry according to DIN 66137-2.
[0115] <Gas accessible pore volume> The Gurwitsch gas-accessible pore volume was determined by gas sorption measurements with nitrogen in accordance with DIN 66134.
[0116] <Thermogravimetric analysis (TGA) and determination of coarse silicon> The reactivity of the powders towards oxygen was determined by TGA measurements in pure oxygen in the temperature window of 25-1000°C using a heating rate of 5 K / min.
[0117] The following materials and equipment were used in carrying out the examples.
[0118] The SiH4 used, quality 4.0, was obtained from Linde GmbH.
[0119] <Porous particles used> Porous carbon particles were used having the following characteristics: BET specific surface area: 2140m 2 / g Gurvich PV:1.01cm 3 / g EXAMPLES
[0120] [Comparative Example 1: Production of over-infiltrated Si / C composite]
[0121] <Production of silicon-containing materials using monosilane SiH4 as silicon precursor>
[0122] In step 1, the autoclave was charged with the porous material in an amount of 10.04 g and closed. In step 2, the autoclave was first evacuated. Then, a SiH4 in an amount of 16.6 g was applied at a pressure of 15.5 bar. In step 3, the autoclave was heated to a temperature of 420° C. over 2.5 hours, and in step 4, the temperature was maintained for 60 minutes. In step 5, the autoclave was cooled to room temperature over 12 hours. After cooling, a pressure of 37.6 bar remained in the autoclave. In step 6, the pressure of the autoclave was reduced to 1 bar, and then purged 5 times with nitrogen, 5 times with lean air with an oxygen content of 5%, 5 times with lean air with an oxygen content of 10%, and then 5 times with air. In step 7, a silicon-containing material in an amount of 22 g was isolated in the form of a black fine solid. The silicon content was 57.5% by weight.
[0123] Example 2: (BeS06956) Removal of excess silicon by etching with sodium hydroxide solution in an amount tailored to the coarse silicon content
[0124] First, 0.2 g of NaOH in 99.8 ml of demineralized water was placed in a 250 ml round-bottom flask and 9 g of the material from Example 1 was gradually added. The resulting suspension was stirred in a water bath at 40° C. for 10 minutes and then passed through a paper filter (filter paper 413, VWR). The powder thus obtained was then suspended in 200 ml of water and again isolated by filtration. This procedure was repeated until the pH of the filtrate obtained was 8.0. The filter cake obtained was dried to constant weight at 80° C. in a drying cabinet.
[0125] The properties of the treated Si composite are shown in Table 1 (excess silicon 0.0 wt%, BET specific surface area 64 m 2 / g). The silicon content was 48.0 wt.%.
[0126] [Examples 3, 4 and 6: Electrochemistry of Comparative Examples 1 and 2, and Comparative Example 5]
[0127] Electrochemical characterization of silicon-containing materials used as active materials in the anodes of lithium-ion batteries.
[0128] 29.71 g of polyacrylic acid (dried to constant weight at 85 °C, Sigma-Aldrich, M w Polyacrylic acid (approximately 450000 g / mol) and 756.6 g deionized water were stirred on a shaker (290 L / min) for 2.5 hours until the polyacrylic acid was completely dissolved. Lithium hydroxide monohydrate (Sigma-Aldrich) was added to the solution in small portions until the pH was 7.0 (measured with a WTW pH340i pH meter and SenTix RJD probe). The solution was then mixed on a shaker for an additional 4 hours.
[0129] 3.87g of neutralized polyacrylic acid solution and 0.96g of graphite (Imerys, KS6L C) were first placed in a 50ml container and mixed in a planetary mixer (SpeedMixer, DAC 150 SP) at 2000 rpm. Then, 3.40g of silicon-containing material from Example 1 or Example 2 was stirred at 2000 rpm for 1 minute. Then, 1.21g of 8% conductive carbon black dispersion and 0.8g of deionized water were added and charged into the planetary mixer at 2000 rpm. This was followed by dispersion in a dissolver at 3000 rpm for 30 minutes at a constant 20°C. The ink was degassed again in the planetary mixer at 1500 rpm for 5 minutes. The finished dispersion was then applied to a copper foil (Schlenk Metallfolien, SE-Cu58) having a thickness of 0.03 mm using a film stretching frame (Erichsen, model 360) with a gap clearance of 0.1 mm. The anode coating thus produced was then dried for 60 minutes at 50° C. and 1 bar air pressure. The average basis weight of the dried anode coating was 1.9 mg / cm 2 and the coating density is 0.9 g / cm 3 It was.
[0130] The electrochemical study was carried out in a two-electrode button cell (CR2032 type, Hosen). The electrode coating was used as the counter electrode or negative electrode (Dm = 15 mm). The content and concentration of the coating were 94.0% and 15.9 mg / cm.2 A coating based on lithium-nickel-manganese-cobalt oxide 6:2:2 (obtained from SEI) with an average basis weight of was used as the working or positive electrode (Dm=15 mm). A glass fiber filter paper (Whatman, GD Type D) saturated with 60 μl of electrolyte was used as the separator (Dm=16 mm). The electrolyte used consisted of a 1.0 molar solution of lithium hexafluorophosphate in a 1:4 (v / v) mixture of fluoroethylene carbonate and diethyl carbonate. The cell was assembled in a glove box (<1 ppm H2O, O2). The moisture content in the dry matter of all components used was less than 20 ppm.
[0131] Electrochemical tests were carried out at 20°C. The cells were charged by cc / cv (constant current / constant voltage) method at a constant current of 12 mA / g (corresponding to C / 10) for the first cycle and 60 mA / g (corresponding to C / 2) for the subsequent cycles, and when the voltage limit of 4.2 V was reached, the cells were charged at a constant voltage until the current dropped below 1.2 mA / g (corresponding to C / 100) or 15 mA / g (corresponding to C / 8). The cells were discharged by cc (constant current) method at a constant current of 12 mA / g (corresponding to C / 10) for the first cycle and 60 mA / g (corresponding to C / 2) for the subsequent cycles until the voltage limit of 2.5 V was reached. The specific current chosen was based on the weight of the coating on the positive electrode. The ratio of the charge capacity to the discharge capacity of the cell is called the coulombic efficiency. The electrodes were selected so as to establish a cathode:anode capacitance ratio of 1:1.2.
[0132] Comparative Example 5: Excessive removal of excess silicon by etching with sodium hydroxide solution in an amount matched to the coarse silicon content
[0133] First, 0.4 g of NaOH in 99.8 ml of demineralized water was placed in a 250 ml round-bottom flask and 6.05 g of the material from Example 1 was added gradually. The resulting suspension was stirred in a water bath at 40° C. for 10 minutes and then passed through a paper filter (filter paper 413, VWR). The powder thus obtained was then suspended in 200 ml of water and again isolated by filtration. This procedure was repeated until the pH of the filtrate obtained was 8.0. The filter cake obtained was dried to constant weight at 80° C. in a drying cabinet.
[0134] The properties of the treated Si composite are shown in Table 1 (excess silicon 0.0 wt%, BET specific surface area 170 m 2 / g). The silicon content was 41.6 wt.%.
[0135] [Table 1]
Claims
1. 1. A method for producing an etched silicon-containing material, comprising: In a first step, silicon is deposited in the pores and on the surfaces of the porous particles by pyrolysis of a silicon precursor on said porous particles to form a silicon-containing material; In a second step, a portion of the deposited silicon of said silicon-containing material is removed by etching off.
2. 2. The method of claim 1, wherein a liquid or gaseous etching medium is used in the second step.
3. 3. The method according to claim 1 or 2, wherein the etching off is carried out by wet chemical treatment with a basic solution.
4. The basic solution may be KOH, tetramethylammonium hydroxide (TMAH), NaOH, LiOH, CsOH, NH 4 OH, Mg(OH) 2 , Ca(OH) 2 , Ba(OH) 2 4. The method of claim 3, further comprising the step of:
5. Method according to any one of claims 1 to 4, wherein before said etching off, the rough silicon to be etched off is determined as follows: The reactivity of the powders towards oxygen was determined and calculated by TGA (thermogravimetric analysis) measurements in pure oxygen in the temperature range 25-1000°C using a heating rate of 5 K / min; (mres) is the residual mass after performing TGA; (mdiff) is the mass difference resulting from the oxidation of coarse silicon, O 2 Molar mass (32 g / mol) and SiO 2 Using the molar mass of 1,000,000 mol (60.08 g / mol), the proportion of coarse silicon in the deposited silicon is calculated according to the formula shown in Equation 1. [0010]
6. A method according to any one of claims 1 to 5, wherein rough silicon is etched off.
7. The method according to any one of claims 1 to 6, wherein the amount of coarse silicon in the deposited silicon after etching is less than 1 wt%.
8. The method according to any one of claims 1 to 7, wherein after etching the etched silicon-containing material is washed with a washing medium, separated from the washing medium and dried.
9. The surface area of the etched silicon-containing material is 80 m 2 The method according to any one of claims 1 to 8, wherein the molecular weight is less than 1 / g.
10. An etched silicon-containing material producible by the method according to any one of claims 1 to 9.
11. 11. An anode material comprising the etched silicon-containing material of claim 10.
12. An anode comprising a current collector coated with the anode material of claim 11.
13. 13. A lithium ion battery comprising a cathode, an anode according to claim 12, two conductive connections to the electrodes, a separator, an electrolyte in which the separator and the two electrodes are impregnated, and a housing containing the above components.
Citation Information
Patent Citations
Polycrystal silicon etched component
JP1978064637A
Method of forming semiconductor structure
JP2007088486A
Planarizing solution for planarizing low temperature polysilicon film panel
JP2008277715A
Improved polycrystalline texturing composition and method
JP2012238849A
Structured particle
JP2018152346A