Wavelength conversion film and display device including same
A polymer-based wavelength conversion film with organic photoluminescent dyes addresses the limitations of existing materials by achieving high quantum efficiency and color gamut, enhancing light emission efficiency and stability.
Patent Information
- Application Number
- JP2024525483
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-12
- Filing Date
- 2022-11-11
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing photoluminescent materials, such as inorganic photoluminescent materials and quantum dots, are expensive, have low luminous efficiency, and are limited in emission range, while organic quantum dots face health concerns and stability issues, necessitating the development of cost-effective, high-efficiency, and stable wavelength conversion films.
A wavelength conversion film comprising a polymer matrix with specific organic photoluminescent dyes, such as BODIPY and naphthalimide groups, that absorb blue light and emit narrow ranges of green and red light, achieving high quantum efficiency and color gamut, with optional scattering centers to enhance light transmission.
The film achieves internal quantum yields over 80% and external quantum yields over 50%, with a color gamut exceeding 90% of BT.2020 standards, providing efficient and cost-effective light emission.
Smart Images

Figure 2024544851000001_ABST
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims priority to U.S. Provisional Patent Application No. 63 / 278,923, filed November 12, 2021, which is incorporated by reference in its entirety.
[0002] The present disclosure relates to wavelength conversion films and light emitting display devices including the same. [Background technology]
[0003] Photoluminescent materials are materials that emit light after absorbing energy in the form of light or electricity. Photoluminescent materials can be classified into inorganic photoluminescent materials (or dyes), organic photoluminescent dyes, nanocrystalline photoluminescent materials, etc., depending on the components that make up the photoluminescent material and the light-emitting mechanism.
[0004] In recent years, various attempts have been described to modify the spectrum of light sources using such photoluminescent materials. Photoluminescent materials absorb light of a certain wavelength from a light source, convert it to light of a longer wavelength in the visible range, and emit it. Depending on the emission properties of the photoluminescent material, the brightness, color purity, color gamut, etc. of the emitted light may be significantly improved. Inorganic photoluminescent materials can be formed from parent compounds such as sulfides, oxides, or nitrides, and activator ions, and can be used in high-quality display devices with excellent physical and chemical stability, as well as high reproducibility of color purity. However, these inorganic photoluminescent materials have disadvantages in that they are very expensive, have low luminous efficiency, and are limited to emitting light in the near-ultraviolet or blue range above 400 nm.
[0005] Quantum dot technology has achieved high levels of quantum efficiency and color gamut. However, cadmium-based quantum dots can be highly toxic and are restricted in many countries due to health safety concerns. In addition, some quantum dots have much lower quantum efficiency in converting blue LED light to green or red light. In addition, quantum dots can have low stability when exposed to moisture and oxygen and often require expensive encapsulation processes. The cost of quantum dots can be high because it can be difficult to control the size uniformity during quantum dot manufacturing.
[0006] Therefore, there is a need for new photoluminescent films that have high quantum efficiency, high color gamut output, and lower cost compared to quantum dot and other existing photoluminescent dye-containing films. Summary of the Invention
[0007] Some embodiments include a wavelength conversion film comprising a polymer matrix, a first photoluminescent dye that absorbs blue wavelength light and emits a narrow range of green wavelength light with an emission spectrum having a full width at half maximum less than 40 nm, a second photoluminescent dye that absorbs blue or green wavelength light and emits a narrow range of red wavelength light with an emission spectrum having a full width at half maximum less than 55 nm, and light scattering centers, wherein the first photoluminescent dye, the second photoluminescent dye, and the light scattering centers are disposed within the polymer matrix.
[0008] In some embodiments, the first photoluminescent dye can include an optionally substituted BODIPY group, a linking group, and an optionally substituted isoquinoline group. [ka] and / or [ka] It could be.
[0009] In some embodiments, the first photoluminescent dye can include an optionally substituted BODIPY group, a linking group, and an optionally substituted naphthalimide group. In some embodiments, the first photoluminescent dye can include [ka] It could be.
[0010] In some embodiments, the second photoluminescent dye can include an optionally substituted BODIPY group, a linking group, and an optionally substituted isoquinoline group. In some embodiments, the second photoluminescent dye can include [ka] [ka] and / or [ka] It could be.
[0011] In some embodiments, the second photoluminescent dye can include an optionally substituted BODIPY group, a linking group, and an optionally substituted naphthalimide group. In some embodiments, the second photoluminescent dye can include [ka] It could be.
[0012] In some embodiments, the second photoluminescent dye can include an optionally substituted BODIPY group, a linking group, and an optionally substituted perylene group. In some embodiments, the second photoluminescent dye can include [ka] may include.
[0013] In some embodiments, the film may have an internal quantum yield of greater than 80%. In some embodiments, the film may have an external quantum yield of greater than 50%. In some embodiments, the film may have a color gamut of greater than 90% of the BT.2020 or Rec.2020 standard. In some embodiments, the film may have a thickness of less than 50 microns.
[0014] Some embodiments include light emitting devices that include the photoluminescent wavelength conversion films described herein.
[0015] Some embodiments include a backlit device having a blue light source that includes the photoluminescent wavelength conversion film described herein.
[0016] These and other embodiments are described in further detail below. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a schematic diagram of one embodiment of a display device incorporating the improved WLC films described herein. [Diagram 2] FIG. 1 is a schematic diagram of one embodiment of a display device incorporating the improved WLC films described herein. [Diagram 3] FIG. 1 is a schematic diagram of one embodiment of a display device incorporating the improved WLC films described herein. [Figure 4] FIG. 1 is a schematic diagram of a test setup including embodiments of the films described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present disclosure relates to wavelength conversion films that include photoluminescent compounds (or dyes) that have high quantum efficiency, high color gamut output, and low cost.
[0019] As used herein, the term "BODIPY" refers to a compound of the formula: [ka] “R” refers to an optionally substituted chemical moiety having the formula:
[0020] The BODIPY moiety contains a dipyrromethene complexed with a disubstituted boron atom, typically a BF2 unit. The IUPAC name for the BODIPY core is 4,4-difluoro-4-bora-3a,4a-diaza-s-indacene.
[0021] As used herein, the term "perylene" or "perylene derivative" refers to a compound of the formula: [ka] refers to an optionally substituted chemical moiety having the formula:
[0022] As used herein, the term "naphthalimide" or "naphthalic acid derivative" refers to a compound of the formula: [ka] where X is NR, and R may be a linking group or an aryl group.
[0023] As used herein, the term "isoquinoline" or "isoquinoline derivative" or "xanthenoisoquinoline derivative" refers to a compound of the formula: [ka] where X is NR, R can be a linking group or an aryl group, and Y can be a hydrogen group, a C1-C3 alkyl, or an aryl group, such as a benzyl group.
[0024] As used herein, the term "naphthalimide" or "naphthalimide derivative" refers to a compound of the formula: [ka] (In the formula, R 0 may be hydrogen (H), substituted or unsubstituted aryl, or CF; X may be oxygen (O) or sulfur (S); R 1 refers to an optionally substituted chemical moiety having hydrogen, substituted or unsubstituted aryl (which may be, for example, phenyl, fluoroalkylphenyl (eg, 4-trifluoromethylphenyl), etc.), or C1-C5 alkyl).
[0025] In some embodiments, the BODIPY moiety is attached to a perylene moiety having a linking group. In some embodiments, the BODIPY moiety is attached to a naphthalimide moiety having a linking group. In some embodiments, the BODIPY moiety is attached to an isoquinoline moiety having a linking group. In some embodiments, the BODIPY moiety is attached to a naphthalimide moiety having a linking group.
[0026] Use of the terms "may" or "may be" should be interpreted as shorthand for "is" or "is not," or "does" or "does not," or "will" or "will not," etc. For example, the statement "the film may include scattering centers disposed within a polymer matrix" should be interpreted as, for example, "in some embodiments, the film includes scattering centers disposed within a polymer matrix" or "in some embodiments, the film does not include scattering centers disposed within a polymer matrix."
[0027] The term ITU-R Recommendation BT.2020 (more commonly known by the abbreviation Rec.2020 or BT.2020) refers to a color display standard for the color gamut. The RGB primaries used by Rec.2020 correspond to monochromatic light sources on the CIE1931 spectral locus. The wavelengths of the Rec.2020 primaries are 630 nm for the red primary, 532 nm for the green primary, and 467 nm for the blue primary. The Rec.2020 color space covers 75.8% (the area within the determined triangle) of the CIE1931 color space. Rec.2020 uses the CIE Standard Illuminant D65 as the white point and the following color coordinates: Xw=0.3127, Yw=0.3290, XR=0.708, YR=0.292, XG=0.17, YG=0.797, XB=0.131, YB=0.046.
[0028] Some embodiments include a wavelength conversion film comprising a polymer matrix, a first organic photoluminescent compound, and a second organic photoluminescent compound. In some embodiments, the film may include a first organic photoluminescent dye that is green emitting and has an emission peak with a full width at half maximum of less than 30 nm or 40 nm. In some embodiments, the film may include a second organic photoluminescent dye that is red emitting and has an emission peak with a full width at half maximum of less than 55 nm. In some embodiments, the film may include light scattering centers. In some examples, the first organic photoluminescent dye (emitting green light), the second organic photoluminescent dye (emitting red light), and the scattering centers are disposed within the polymer matrix. In some embodiments, the film provides a high quantum yield. In some embodiments, the film provides a wide color gamut of more than 90%. A suitable means for determining the percent color gamut is to measure the area under the 1931 CIE color space produced. In some embodiments, the film may have a color gamut of 89%-99.9%, for example, 91%-92%, 92%-93%, 93%-94%, 98%-99.9%, 89%-93%, 93%-96%, and / or 96%-99.9%, or a range defined by any of these values. Some embodiments include an LCD backlight comprising the above-described film.
[0029] In some embodiments, the film may include a polymer matrix. In some embodiments, the polymer matrix may have a transparency of greater than 75%, greater than 80%, greater than 90%, or greater than 95%. In some embodiments, the polymer matrix may include a hydrophilic or hydrophobic polymer. In some embodiments, the polymer matrix may include polyvinyl butyral, polyvinyl acetate, polyvinyl alcohol, or polyacrylate. In some embodiments, the polymer matrix may include polyvinyl butyral (PVB). In some embodiments, the polyacrylate may be a polyalkyl acrylate. In some embodiments, the polyalkyl acrylate may be polymethyl methacrylate (PMMA).
[0030] In some embodiments, the photoluminescent compound (and / or the photoluminescent wavelength conversion film including the photoluminescent compound) has a narrow absorption or emission band, resulting in a small amount of visible wavelength light being emitted. The absorption or emission band can be characterized by a full width at half maximum (FWHM). In this disclosure, FWHM defines the width of the absorption or emission spectrum at half the peak wavelength of absorption or emission in nanometers. In some embodiments, the photoluminescent compound has an absorption band with a FWHM value of 50 nm or less, 40 nm or less, 35 nm or less, 30 nm or less, or 25 nm or less when dispersed in a substantially transparent polymer matrix. In some embodiments, the photoluminescent compound has an emission band with a FWHM value of 50 nm or less, 40 nm or less, 35 nm or less, or 30 nm or less when dispersed in a substantially transparent polymer matrix.
[0031] In some embodiments, the film may include a first organic photoluminescent compound (or dye). In some embodiments, the first organic photoluminescent dye (and / or the photoluminescent wavelength conversion film including the first organic photoluminescent dye) may have an emission peak (green light emission) between 510 nm and 520 nm, or between 520 nm and 530 nm, or a range bounded by any of these values. In some embodiments, the emission spectrum of the first organic photoluminescent dye and / or the photoluminescent wavelength conversion film may have a full width at half maximum (FWHM) of less than 35 nm, less than 30 nm, or less than 20 nm.
[0032] In some embodiments, the first organic photoluminescent dye may include an optionally substituted BODIPY group, a linking group, and an optionally substituted isoquinoline group. In some embodiments, the optionally substituted isoquinoline group may be an optionally substituted isoquinoline derivative group. In some embodiments, the optionally substituted isoquinoline group may be an optionally substituted xanthenoisoquinoline derivative group. In some embodiments, the optionally substituted BODIPY group is covalently bonded to the linking group. In other embodiments, the linking group is covalently bonded to the optionally substituted isoquinoline group. In other embodiments, the linking group is covalently bonded to the optionally substituted isoquinoline derivative group. In other embodiments, the linking group is covalently bonded to the optionally substituted xanthenoisoquinoline derivative group.
[0033] In some embodiments, the first organic photoluminescent dye may include an optionally substituted BODIPY group, a linking group, and an optionally substituted naphthalimide group. In some embodiments, the optionally substituted naphthalimide group may be an optionally substituted naphthalic acid derivative group. In some embodiments, the optionally substituted BODIPY group is covalently bonded to the linking group. In other embodiments, the linking group is covalently bonded to the optionally substituted naphthalimide group. In other embodiments, the linking group is covalently bonded to the optionally substituted naphthalic acid derivative group.
[0034] In some embodiments, the first organic photoluminescent dye can be selected from photoluminescent dyes described in co-pending U.S. Provisional Application No. 63 / 152,309, filed February 22, 2021 (incorporated by reference herein for its discussion of photoluminescent dyes) and U.S. Provisional Application No. 63 / 278,904, filed November 12, 2021 (Attorney Docket No. N3253.10133US02, incorporated by reference herein).
[0035] In some embodiments, the first organic photoluminescent dye is FD-1, FD-2, or FD-3: [ka] [ka] [ka] Or any combination thereof may be selected.
[0036] In some embodiments, the wavelength conversion film may include a second organic photoluminescent dye. In some embodiments, the second organic photoluminescent dye (and / or the photoluminescent wavelength conversion film including the second organic photoluminescent dye) may have an absorption peak (blue light absorption) between 400 nm and 470 nm. In some embodiments, the second organic photoluminescent dye (and / or the photoluminescent wavelength conversion film including the second organic photoluminescent dye) may have an emission peak (red light emission) between 610 nm and 620 nm, or between 620 nm and 630 nm, or a range bounded by any of these values. In some embodiments, the emission spectrum of the second organic photoluminescent dye and / or the photoluminescent wavelength conversion film may have a full width at half maximum (FWHM) of less than 65 nm, less than 55 nm, less than 50 nm, less than 45 nm, less than 40 nm, or less than 35 nm.
[0037] In some embodiments, the second organic photoluminescent dye can include a BODIPY group, a linking group, and a perylene group. In some embodiments, the perylene group can be a perylene derivative group. In some embodiments, the BODIPY group is covalently attached to the linking group. In other embodiments, the linking group is covalently attached to the perylene group. In other embodiments, the linking group is covalently attached to the perylene derivative group.
[0038] In some embodiments, the second organic photoluminescent dye may include a BODIPY group, a linking group, and an isoquinoline group. In some embodiments, the isoquinoline group may be an isoquinoline derivative group. In some embodiments, the BODIPY group is covalently bonded to the linking group. In other embodiments, the linking group is covalently bonded to the isoquinoline group. In other embodiments, the linking group is covalently bonded to the isoquinoline derivative group.
[0039] In some embodiments, the second organic photoluminescent dye may include a BODIPY group, a linking group, and a naphthalimide group. In some embodiments, the naphthalimide group may be a naphthalimide derivative group. In some embodiments, the BODIPY group is covalently bonded to the linking group. In other embodiments, the linking group is covalently bonded to the naphthalimide group. In other embodiments, the linking group is covalently bonded to the naphthalimide derivative group.
[0040] In some embodiments, the first organic photoluminescent dye can be selected from photoluminescent dyes described in co-pending U.S. Provisional Application No. 63 / 248,863, filed September 27, 2021, which is incorporated herein by reference for its discussion of photoluminescent dyes, U.S. Provisional Application No. 63 / 278,904, filed November 19, 2021, which is incorporated herein by reference (Attorney Docket No. N3252.10147US02), and PCT Patent Publication WO 2020 / 210761, which is incorporated herein by reference. In some embodiments, the second ... SD-1, SD-2, SD-3, SD-4, or SD-5: [ka] [ka] [ka] [ka] [ka] Or any combination thereof may be selected.
[0041] In some embodiments, the first photoluminescent compound can absorb light from within the UV / blue absorption spectrum and emit light within the green emission spectrum to enhance the perceived emitted green light. In other embodiments, the second photoluminescent compound can absorb light from within the green and / or blue absorption spectrum and emit light within the red emission spectrum to enhance the perceived emitted red light. In some embodiments, the first photoluminescent dye and the second photoluminescent dye can absorb light from within the UV / blue absorption spectrum and emit light at other wavelengths, and the combined resulting light can be perceived as white light. In some examples, the perceived white light can have a color temperature described as cool. In some embodiments, the perceived white light can have a color temperature described as warm.
[0042] In some embodiments, the first photoluminescent dye and the second photoluminescent dye may absorb about 60%-70% of the light emitted from the light source in the blue spectrum. In some embodiments, the resulting white light contains 30%-50% blue light, 20%-30% red light emitted from the wavelength conversion film, and 20%-30% green light emitted from the wavelength conversion film. The thickness of the film can be adjusted to tune the percentage of blue light absorbed by the wavelength conversion film and the percentage of blue light that passes through the wavelength conversion film and constitutes the resulting white light. In some embodiments, the photoluminescent wavelength conversion film can have any suitable thickness, such as less than about 500 μm, less than about 200 μm, or less than about 100 μm, such as about 1 μm to 20 μm, about 10 μm to 40 μm, about 20 μm to 30 μm, about 30 μm to 40 μm, about 40 μm to 50 μm, about 50 μm to 80 μm, about 80 μm to 120 μm, about 120 μm to 200 μm, about 200 μm to 300 μm, or about 300 μm to 500 μm.
[0043] In some embodiments, the thickness of the wavelength conversion film may be decreased or increased according to the Beer-Lambert law. In particular, the Beer-Lambert law may be used to derive the relationship between the film thickness and the concentration of the first photoluminescent dye and the second photoluminescent dye to achieve 60%-70% of the blue light emitted from the light source. In some embodiments, the dye concentration may be decreased or the thickness may be increased to allow for 60%-70% absorption of the blue light. In some embodiments, the dye concentration may be increased or the thickness may be decreased to allow for 60%-70% absorption of the blue light. In some embodiments, the photoluminescent wavelength conversion film may have a suitable thickness of more than 20 μm and less than 30 μm for most dye concentrations, as shown in Table 1 in the Examples section below.
[0044] In some embodiments, the length of the linking group can be adjusted to optimize the solubility of the first and second photoluminescent dyes. In some embodiments, the solubility of the first and second photoluminescent dyes can be greater than 0.15%. In some embodiments, the solubility of the first and second photoluminescent dyes can be about 0.03% to 0.8%, about 0.8% to 2%, or about 2% to 3%, or a solubility within a range bounded by any of the above values.
[0045] The ratio of the amounts of the first photoluminescent dye and the second photoluminescent dye can be adjusted to tailor the color properties of the photoluminescent wavelength conversion film. For example, the weight ratio of the first photoluminescent dye to the second photoluminescent dye may be about 0.01 to 100 (1 mg of the first photoluminescent dye and 100 mg of the second photoluminescent dye is a ratio of 0.01), about 0.01 to 0.2, about 0.2 to 0.4, about 0.4 to 0.6, about 0.6 to 0.8, about 0.8 to 1, about 1 to 2, about 2 to 3, about 3 to 4, about 4 to 5, about 5 to 6, about 6 to 7, about 7 to 8, about 8 to 9, about 9 to 10, about 10 to 20, about 20 to 40, about 40 to 70, about 70 to 100, about 0.43, about 0.91, about 1.8, or about 3.0.
[0046] In some embodiments, the film may include scattering centers disposed within the polymer matrix. In some embodiments, the scattering centers may be solid particles that include a scattering material having a refractive index (RI) different from the refractive index of the polymer matrix material. The scattering material may be a material whose refractive index is different from the RI of the polymer matrix. The scattering material may be useful for increasing the external quantum yield, for example, by reducing total internal reflection.
[0047] [Table 1A]
[0048] In some embodiments, the difference in RI between the polymer matrix material and the light scattering material may be at least 0.05, 0.1, at least 0.2, at least 0.3, at least 0.4, or at least 0.5, up to 1 or 2.
[0049] In some embodiments, the scattering material may be silicone beads. In some embodiments, the scattering centers may include air pores defined within the polymer matrix. In some embodiments, the scattering centers may have an average diameter of 1 micron (μm) to 10 microns (μm), about 1 μm to 2 μm, about 2 μm to 3 μm, about 3 μm to 4 μm, about 4 μm to 5 μm, about 5 μm to 6 μm, about 6 μm to 7 μm, about 7 μm to 8 μm, about 8 μm to 9 μm, about 9 μm to 10 μm, or about any value within a range defined by any of these values. In some embodiments, the scattering centers may be substantially uniformly dispersed within the polymer matrix. In some embodiments, the top portion of the film, e.g., distal from the blue light emitting source, may have more than 50% scattering centers. In some embodiments, the scattering centers may be uniformly distributed throughout the polymer matrix.
[0050] In some embodiments, the photoluminescent wavelength conversion film can have an internal quantum yield (IQE) at the red or green emission maximum that is at least about 70%, at least about 80%, or at least about 90%, and / or at most about 80%, at most about 90%, or at most about 100%. In some embodiments, the photoluminescent wavelength conversion film can have an external quantum yield (EQE) at the red or green emission maximum that is at least about 50%, at least about 60%, at least about 70%, at least about 80%, or at least about 90%, and / or at most about 80%, at most about 90%, or at most about 100%.
[0051] In some embodiments, the display device may be represented by device 10. As shown in FIG. 1 , device 10 may include a light source 12. In some embodiments, display device 10 may include a wavelength conversion (WLC) film 16. In some embodiments, WLC film 16 may be optically coupled to light source 12 and may increase the efficiency in transmitting generated light from light source 12 to viewer 20.
[0052] In some embodiments, a display device may be represented generally by FIG. 2. As shown in FIG. 2, a display device, such as device 10, may include a light source 12. In some embodiments, display device 10 may include a back reflector 14. In some embodiments, display device 10 may include a wavelength conversion (WLC) film 16. In some embodiments, display device 10 may include a mask 18. In some embodiments, WLC film 16 may be optically coupled to light source 12 and may increase efficiency in transmitting generated light from light source 12 to viewer 20.
[0053] In some embodiments, the display device may be represented diagrammatically by FIG. 3. As shown in FIG. 3, the display device is illustrated, where the device 10 may include a light source 12. In some embodiments, the display device 10 may include a back reflector 14. In some embodiments, the display device 10 may include a wavelength conversion (WLC) film 16. In some embodiments, the display device may include a mask 18. In some embodiments, the WLC film 16 may be optically coupled to the light source 12 and / or may be sandwiched between the light source 12 and the viewer 20 and / or the mask 18 to increase the efficiency of transmitting generated light from the light source 12 to the viewer 20.
[0054] 3 and 4, in some embodiments, the display device 10 can include one or more brightness enhancing films (BEF) 22, such as Vikuiti brand BEF (3M, Minneapolis, Minn., USA). In some embodiments, the display device 10 can include one or more polarizers and / or brightness enhancing films, such as dual brightness enhancing films (DBEF) 24, such as DBEF II (3M, Minneapolis, Minn., USA). In some embodiments, the use of one or more brightness enhancing films can be referred to as an optical film stack.
[0055] Some embodiments include a method for producing an LED light source. In some embodiments, the method may include producing a wet wavelength-shifting polymer layer with an organic solvent and a photoluminescent dye as described herein. In some embodiments, the method may include mixing a polymer and / or monomer with an organic solvent. In some embodiments, the polymer and / or monomer precursor may be dispersed, dissolved and / or mixed with a solvent. In some embodiments, a solvent may be used in producing a material layer. In some embodiments, the solvent may be a non-polar solvent. In some embodiments, the non-polar solvent may include, but is not limited to, xylene, cyclohexanone, acetone, toluene, methyl ethyl ketone, or any combination thereof. In some embodiments, the solvent may be a polar solvent. In some embodiments, the polar solvent may include ethanol, dimethylformamide (DMF), or a combination thereof. In some embodiments, the solvent may be a combination of a non-polar solvent and a polar solvent.
[0056] In some embodiments, the method may include immersing the wet polymeric photocatalyst WLC layer in an aqueous solution. In some embodiments, the aqueous solution may include water. In some embodiments, the aqueous solution may include at least 90% water. In some embodiments, the water may be deionized water. In some embodiments, the wet polymeric photocatalyst WLC layer may be immersed in the aqueous solution for between 5 minutes and about 1 hour.
[0057] In some embodiments, the method may include removing the wet polymeric photocatalyst WLC layer from the aqueous solution. In some embodiments, the method may include drying the wet polymeric photocatalyst WLC layer. It is believed that producing the polymeric photocatalyst WLC layer in this manner results in a plurality of air pores defined on the emitting or distal surface of the polymeric photocatalyst WLC layer. In some embodiments, the air pores are substantially entirely within about 1 micron to about 5 microns from the emitting surface of the polymeric photocatalyst WLC layer.
[0058] In some embodiments, the polymeric material comprises an aqueous solution of about 2% to about 50% by weight of polymer, about 2% to 5% by weight, about 5% to 10% by weight, about 10% to 15% by weight, about 15% to 20% by weight, about 20% to 25% by weight, about 25% to 30% by weight, about 30% to 35% by weight, about 35% to 40% by weight, about 40% to 45% by weight, about 45% to 50% by weight, about 2.5% to 30% by weight, about 5% to 15% by weight, about 15% to 25% by weight, about 25% to 35% by weight, or about 30% by weight, or about any value within a range bounded by any of these values.
[0059] Embodiment Embodiment 1. A wavelength conversion film, A polymer matrix; a first photoluminescent dye that absorbs blue wavelength light and emits a narrow range of green wavelength light with an emission spectrum having a full width at half maximum of less than 30 nm; a second photoluminescent dye that absorbs blue or green wavelength light and emits a narrow range of red wavelength light with an emission spectrum having a full width at half maximum of less than 55 nm; A light scattering center; Including, A wavelength conversion film, wherein a first photoluminescent dye, a second photoluminescent dye and light scattering centers are disposed in a polymer matrix.
[0060] Embodiment 2. The wavelength conversion film of embodiment 1, wherein the first photoluminescent dye comprises a BODIPY group, a linking group, and an isoquinoline group.
[0061] Embodiment 3. The first photoluminescent dye comprises: [ka] or [ka] The wavelength conversion film of embodiment 2, selected from
[0062] Embodiment 4. The wavelength conversion film of embodiment 1, wherein the first photoluminescent dye comprises a BODIPY group, a linking group, and a naphthalimide group.
[0063] Embodiment 5. The first photoluminescent dye is [ka] The wavelength conversion film of embodiment 4, selected from
[0064] Embodiment 6. The wavelength conversion film of embodiment 1, wherein the second photoluminescent dye comprises a BODIPY group, a linking group, and an isoquinoline group.
[0065] Embodiment 7. The second photoluminescent dye is [ka] [ka] or [ka] The wavelength conversion film of embodiment 6, selected from
[0066] Embodiment 8. The wavelength conversion film of embodiment 1, wherein the second photoluminescent dye comprises a BODIPY group, a linking group, and a naphthalimide group.
[0067] Embodiment 9. The second photoluminescent dye is [ka] The wavelength conversion film of embodiment 8, selected from
[0068] Embodiment 10. The wavelength conversion film of embodiment 1, wherein the second photoluminescent dye comprises a BODIPY group, a linking group, and a perylene group.
[0069] Embodiment 11. The second photoluminescent dye is [ka] The wavelength conversion film of embodiment 8, selected from
[0070] Embodiment 12. The wavelength conversion film of any one of embodiments 1 to 11, wherein the wavelength conversion film has an internal quantum yield of more than 80%.
[0071] Embodiment 13. The wavelength conversion film of any one of embodiments 1 to 11, wherein the wavelength conversion film has an external quantum yield of more than 50%.
[0072] Embodiment 14. The wavelength conversion film of any one of embodiments 1 to 11, wherein the wavelength conversion film has a color gamut exceeding 90% of the BT.2020 standard.
[0073] Embodiment 15. The wavelength conversion film of any one of embodiments 1 to 11, wherein the wavelength conversion film has a thickness of 10 μm to 40 μm.
[0074] Embodiment 16. A light-emitting device comprising the wavelength conversion film of any one of embodiments 1 to 15.
[0075] Embodiment 17. A backlit device having a blue light source, comprising the wavelength conversion film of any one of embodiments 1 to 15. EXAMPLES
[0076] It has been discovered that embodiments of films containing the photoluminescent complexes described herein have improved performance compared to other forms of color conversion films. These advantages are further demonstrated by the following examples, which are intended to be merely illustrative of the present disclosure and in no way limiting of its scope or underlying principles.
[0077] Synthesis of the first photoluminescent dye Synthesis procedure for compound FD-1: [ka]
[0078] Compound FD-1.1: A mixture of ethyl 2,4-dimethyl-1H-pyrrole-3-carboxylate (1.0 g, 6.0 mmol), 4-hydroxy-2,6-dimethylbenzaldehyde (0.449 g, 3.0 mmol) and tosylic acid (50 mg, 0.29 mmol) in 50 mL of 1,2-dichloroethane was degassed and stirred at room temperature overnight. LCMS analysis showed m / e + = 467 shows one major peak.
[0079] To the resulting solution was added DDQ (0.817 g, 3.6 mmol) and the mixture was stirred at room temperature for 30 min. LCMS analysis showed that all starting materials were m / e + = 465 was converted to the desired product.
[0080] With ice bath cooling, 1.7 mL of triethylamine and 2.2 mL of BF3-diethyl ether were added successively to the mixture from step 2. The whole was heated at 50° C. for 1 h. LCMS analysis showed about 30% conversion. To this mixture was added another 1 mL of triethylamine and 1 mL of BF3-diethyl ether, and the whole was heated at 50° C. for another 1 h. LCMS analysis showed that all starting material was m / e + =513, m / e - = 512, indicating conversion to the desired BODIPY product. The reaction mixture was loaded directly onto silica gel and purified by flash chromatography using an eluent of hexane / ethyl acetate (0% -> 30% ethyl acetate). The main desired peak was collected and the solvent was removed to give an orange solid (1.0 g, 65% yield). LCMS (APCI): C 27 H 32 Calculated for BF2N2O5 (M+H): 513.2; Found: 513. 1 H NMR (400 MHz, chloroform-d) δ 7.26 (s, 3H), 6.68 (s, 2H), 4.29 (q, J = 7.1 Hz, 4H), 2.84 (s, 6H), 2.05 (s, 6H), 1.34 (t, J = 7.1 Hz, 6H).
[0081] Compound FD-1.2: A mixture of 2-nitrophenol (6.6 g, 48 mmol), KOH powder (2.4 g, 43 mmol) was mixed and stirred under vacuum for 30 min, then copper powder (0.4 g) was added followed by 100 mL of anhydrous DMF. The mixture was stirred for 5 min, then 4-chloronaphthalic anhydride (5.1 g, 22 mmol) was added. The whole was degassed and heated at reflux for 1.5 h. After cooling to room temperature, 100 mL of 20% hydrochloric acid was added dropwise to the resulting reaction mixture, which was allowed to stand for 2 h. The precipitate was collected by filtration and then dried under vacuum overnight to give a tan solid (4.6 g). This was further purified by stirring in refluxing acetic acid (50 mL) for 2 h and then cooled to room temperature. Filtration and drying in air gave a yellow solid (3.0 g, 41% yield). Confirmed by LCMS (APCI): C 18 H 10Calculated for NO6 (M+H): 336.0; Found: 336. 1 H NMR(400MHz,chloroform-d) δ 8.80(dd,J=8.5,1.2Hz,1H), 8.72(dd,J=7.3,1.2Hz,1H), 8.50(d,J=8.2Hz,1H), 8.19(dd,J=8.2,1.7Hz,1H), 7.90(dd,J=8. 5,7.3Hz,1H), 7.79(td,J=7.9,1.7Hz,1H), 7.54(td,J=8.0,1.3Hz,1H), 7.39(dd,J=8.3,1.2Hz,1H), 6.89(d,J=8.2Hz,1H).
[0082] Compound FD-1.3: A mixture of compound FD-1.2 4-(2-nitrophenoxyl)-1,8-naphthalic anhydride (2.0 g, 6 mmol) and iron powder (<10 μm, 0.91 g, 16 mmol) in acetic acid (75 mL) was heated to reflux for 30 minutes. The resulting solution was poured into water (220 mL). The resulting precipitate was collected by filtration, washed with water, and thoroughly dried in air and then under vacuum to give a yellow solid (1.65 g, 90% yield). Confirmed by LCMS (APCI): C 18 H 12 Calculated for NO4 (M+H): 306.1; Found: 306.
[0083] Compound FD-1.4: Compound FD-1.3 4-(2-aminophenoxy)-1,8-naphthalic anhydride (1.5 g, 4.9 mmol) was dispersed in acetic acid (35 mL) and cooled to 0° C. Pre-cooled hydrochloric acid (3 mL, 37 mmol) was added under stirring, followed by dropwise addition of sodium nitrite solution (3.29 g, 46 mmol) in 12 mL of water at 0° C. The whole was stirred at 0° C. for 1 h, then transferred to an addition funnel and added dropwise to refluxing copper sulfate solution (5.08 g, 20 mmol, in 50 mL of water) over 1 h. After cooling to room temperature, the precipitate was collected by filtration, washed with water, and then dried in air and then in vacuum to give a yellow solid (0.92 g, 65% yield). Confirmed by LCMS (APCI): C 18Calculated for H8O4 (M-): 288.0; Found: 288. 1 H NMR(400MHz,chloroform-d) δ 8.61(dd,J=17.1,8.1Hz,2H), 8.09(d,J=8.0Hz,1H), 7.97(d,J=7.9Hz,1H), 7.59(t,J=7.7Hz,1H), 7.40(t,J=8.1Hz,2H), 7.33(d,J=8.4Hz,1H).
[0084] Compound FD-1.5: A mixture of compound FD-1.4 1H,3H-isochromeno[6,5,4-mna]xanthene-1,3-dione (100 mg, 0.347 mmol), 4-(4-aminophenyl)butyric acid (125 mg, 0.7 mmol) in 5 mL of DMF was heated in a microwave reactor at 165° C. for 2.5 hours. To this mixture was added 15 mL of acetone, and the resulting precipitate was collected by filtration and dried in air to give a yellow solid (120 mg, 77% yield). Confirmed by LCMS (APCI): C 28 H 19 Calculated for NO5 (M-): 449.1; Found: 449. 1 H NMR(400MHz,DMSO-d6) δ 8.38(d,J=41.6Hz,4H), 7.81~6.97(m,8H), 2.69~2.64(m,2H), 2.26(t,J=7.2Hz,2H), 1.87(p,J=7.2Hz,2H).
[0085] Compound FD-1: A mixture of compound FD-1.5 (45 mg, 0.1 mmol), compound FD-1.1 (40 mg, 0.078 mmol), DMAP / TsOH salt (59 mg, 0.2 mmol) and DIC (0.1 mL, 0.63 mmol) in 5 mL of DCM was stirred at room temperature overnight and then at 45° C. for 2 h. The reaction mixture was loaded onto silica gel and purified by flash chromatography using an eluent of DCM / ethyl acetate (0%→10% ethyl acetate). The desired product peak was collected and concentrated under reduced pressure. The resulting solid was further washed with methanol and dried in air to give an orange solid (46 mg, 62% yield). Confirmed by LCMS (APCI): C 55 H 49 Calculated for BF2N3O9 (M+H): 944.3; Found: 944. 1 H NMR(400MHz,d2-TCE) δ 8.54(dd,J=18.7,8.1Hz,2H), 7.40~7.25(m,5H), 7.20(d,J=8.3Hz,2H), 6.93(s,2H), 4.19(q,J=7.1Hz,4H), 2.80(t,J= 7.6Hz,2H), 2.75(s,6H), 2.62(t,J=7.4Hz,2H), 2.10(t,J=7.6Hz,2H), 2.06(s,6H), 1.65(s,6H), 1.25(t,J=7.1Hz,6H).
[0086] Synthesis procedure of compound FD-2 [ka]
[0087] Compound FD-2.1: A mixture of ethyl 2,4-dimethyl-1H-pyrrole-3-carboxylate (1.0 g, 6.0 mmol), 4-hydroxy-2,6-dimethylbenzaldehyde (0.449 g, 3.0 mmol) and p-toluenesulfonic acid (p-TsOH) (50 mg, 0.29 mmol) in 50 mL of dichloroethane (DCE) was degassed and stirred at room temperature overnight. Liquid chromatography-mass spectrometry (LCMS) showed m / e +The main peak at m / e = 467 indicates the reaction is complete. To the mixture obtained above, 2,3-dichloro-5,6-dicyano-1,4-benzoquinone (DDQ) (0.817 g, 3.6 mmol) was added and the whole was stirred at room temperature for 30 minutes. LCMS analysis showed m / e + The main peak at m / e = 465 indicates the reaction is complete. Triethylamine (1.7 mL, 12 mmol) and BF3-diethyl ether (2.2 mL, 18 mmol) were added to the mixture obtained above while cooling with an ice batch, and the mixture was stirred at 50°C for 1 h. An additional 1 mL of triethylamine and 1 mL of BF3-diethyl ether were added, and the whole was heated for another 1 h. LCMS analysis showed that all the dipyrrolemethine starting material was in the m / e range of 1.0 to 1.5 m / s. + = 513 of the BODIPY product. After cooling to room temperature, the reaction mixture was loaded onto silica gel and purified by flash chromatography using an eluent of hexane / ethyl acetate (0% -> 30% ethyl acetate). The desired fractions were collected. After removal of the solvent, the desired product was obtained as an orange solid (1.0 g, 65% yield). 1 H NMR (400 MHz, chloroform-d) δ 6.68 (s, 2H), 4.29 (q, J = 7.1 Hz, 4H), 2.84 (s, 6H), 2.05 (s, 6H), 1.34 (t, J = 7.1 Hz, 6H). LCMS (APCI+): C 27 H 32 Calculated for BF2N2O5 (M+H)=513.2; Found: 513.
[0088] Compound FD-2: A mixture of compounds FD-2.1 (100 mg, 0.195 mmol), FD-2.2 (4-(4-(6-(4-(diphenylamino)phenyl)-1,3-dioxo-1H-benzo[de]isoquinolin-2(3H)-yl)phenyl)butyric acid) (132 mg, 0.22 mmol), diisopropylcarbodiimide (DIC) (0.1 mL, 0.63 mmol) and dimethylaminopyridine (DMAP) / p-TsOH (118 mg, 0.4 mmol) in dichloromethane (DCM) (6 mL) was stirred at room temperature overnight, then loaded onto silica gel and purified by flash chromatography using an eluent of DCM / ethyl acetate (0%→5% ethyl acetate). The main desired orange fraction was collected. After removal of the solvent, the resulting solid was reprecipitated in DCM / MeOH. After filtration and drying in air the desired product was obtained as an orange solid (145 mg, 68% yield). 1 H NMR(400MHz,d2-TCE) δ 8.56(dd,J=7.4,4.7Hz,2H), 8.43(d,J=8.3Hz,1H), 7.79~7.64(m,2H), 7.4 1~7.18(m,10H), 7.18~7.12(m,6H), 7.03(t,J=7.3Hz,2H), 6.93(s,2H), 4.1 9(q,J=7.1Hz,4H), 2.81(t,J=7.6Hz,2H), 2.75(s,6H), 2.62(t,J=7.4Hz,2 H), 2.11(t,J=7.5Hz,2H), 2.06(s,6H), 1.65(s,6H), 1.25(t,J=7.1Hz,6H). LCMS(APCI-):C 67 H 59 Calculated for BF2N4O8 (M-)=1096.4; Found: 1096.
[0089] Synthesis procedure of compound FD-3 [ka]
[0090] Procedure for the synthesis of FD-3.1 - 2-(4-(9-bromo-1,3-dioxo-1H-xantheno[2,1,9-def]isoquinolin-2(3H)-yl)phenyl)acetic acid: A mixture of SD-2.6 (400.0 mg, 1.1 mmol), 4-aminophenylacetic acid (329.4 mg, 2.2 mmol) and DMAP (9.3 mg, 0.080 mmol) in DMF (8 mL) was degassed at room temperature. The mixture was then heated to 165° C. and maintained at this temperature for 3 h. TLC and LCMS showed about 95% conversion without observable side reactions. The mixture was cooled to 50° C. It was then poured into an acetone solution (40 mL) and pre-cooled by a water-ice bath. The mixture was maintained at 0° C. for 2 h and continued to stir at room temperature overnight. The solid was collected by vacuum filtration and washed with acetone (4 mL). It was then dried in a vacuum oven at 100° C. for 3 h to give pure compound FD-3.1 as a tan solid (395.0 mg, 73% yield). MS (APCI): C 26 H 14 Calculated for BrNO5 ([M+H]+)=500 Found: 500. 1 H NMR(400MHz,CDCl2CDCl2) δ 8.65(d,J=8.0Hz,1H), 8.62(d,J=8.0Hz,1H), 8.21(dd,J=6.4Hz,2.4Hz,1H), 7.99(bs,1H), 7.95(t,J=7.6Hz ,1H), 7.67(dd,J=8.4Hz,2.4Hz,1H), 7.53(d,J=8.0Hz,2H), 7.37(d,J=8.4Hz,1H), 7.32(m,3H), 2.94(s,2H).
[0091] Procedure for the synthesis of compound SD-5.1 - 2-(4-(1,3-dioxo-9-(4-(trifluoromethyl)phenyl)-1H-xantheno[2,1,9-def]isoquinolin-2(3H)-yl)phenyl)acetic acid: A 100 mL vial was fitted with a stir bar. Into this vial, compound FD-3.1 (400.0 mg, 0.80 mmol), 4-(trifluoromethyl)phenylboronic acid (262.2 mg, 1.6 mmol), Pd(dppf)Cl2 (41.0 mg, 0.056 mmol) and K2CO3 (298.0 mg, 2.2 mmol) in THF / DMF / H2O (22 ml / 4.4 ml / 2.2 ml) were degassed at room temperature. The reaction mixture was heated to 80° C. and the reaction was maintained at this temperature overnight. The reaction was monitored using TLC. After completion, the reaction was worked up by the addition of 0.1 N HCl (150 ml) and EtOAc (150 ml). The aqueous phase was further extracted with THF (150 ml×3). The combined organic phase was dried over anhydrous Na2SO4, concentrated under a rotavapor, and purified by flash chromatography using DCM (0%→40%, containing 0.1% TFA) in EtOAc as eluent to give the pure RL-naphthalimide derivative SD-5.1 as a yellow / tan solid (363.0 mg, 80% yield). MS (APCI): C 33 H 18 Calculated for F3NO5 ([M+H]+)=566. Found: 566. 1 H NMR(400MHz,DMSO-d6) 8.76(m,1H), 8.56(m,2H), 8.52(dd,J=8.0Hz,J=3.2Hz,1H), 8.15(m,2H), 8.06(m,1H), 7.94(d,J=8.0Hz,2H ), 7.66(dd,J=8.0Hz,J=4.0Hz,1H), 7.53(m,1H), 7.45(d,J=8.0Hz,2H), 7.33(d,J=8.0Hz,2H), 3.72(s,2H).
[0092] Procedure for compound FD-3: A mixture of compound SD-5.1 (50 mg, 0.089 mmol), compound FD-2.1 (30 mg, 0.059 mmol), DMAP / TsOH salt (15 mg, 0.051 mmol) and EDC·HCl (60 mg, 0.31 mmol) in 5 mL of DCM was stirred at room temperature overnight. The reaction mixture was loaded onto silica gel and purified by flash chromatography using an eluent of DCM / ethyl acetate (0%→10% ethyl acetate). The desired product peak was collected and concentrated under reduced pressure. The resulting solid was reprecipitated with ethyl acetate / methanol and dried in air to give an orange solid (45 mg, 72%). LCMS (APCI-): C 60 H 47 Calculated for BF5N3O9: 1059.33; Found: 1059. 1 H NMR (400MHz, methylene chloride-d2) δ 8.73(d,J=7.9Hz,1H), 8.66(d,J=8.3Hz,1H), 8.39(d,J=2.2Hz,1H), 8.17(d,J= 8.0Hz,1H), 7.86(dt,J=11.4,8.4Hz,5H), 7.64(d,J=8.3Hz,2H), 7.57(d,J=8.6H) z,1H), 7.43(d,J=8.3Hz,1H), 7.41~7.35(m,2H), 7.09(s,2H), 4.30(q,J=7.1Hz, 4H), 4.05(s,2H), 2.84(s,6H), 2.18(s,6H), 1.77(s,6H), 1.36(t,J=7.1Hz,6H).
[0093] Synthesis procedure for the second photoluminescent dye Synthesis procedure for compound SD-1 [ka]
[0094] Compound SD-1.1 (2-(4-bromophenyl)-4-phenyl-1H-pyrrole): Synthesized according to literature procedure: Synlett, 2016, 27(11), 1738-1742.
[0095] Compound SD-1.2: A mixture of SD-1.1 (2-(4-bromophenyl)-4-phenyl-1H-pyrrole) (1.0 g, 3.36 mmol), 2,4,6-trimethylbenzaldehyde (0.249 g, 1.68 mmol) and tosylic acid (50 mg) in 1,2-dichloroethane (80 mL) was heated at 50° C. for 24 h. LCMS analysis showed that the main peak had an m / e + = 727, indicating the desired product. To this mixture was added DDQ (454 mg, 2 mmol) and stirred at room temperature for 1 h. LCMS analysis showed m / e - One major peak at m / z = 724 indicates the reaction is complete. To this mixture was added triethylamine (0.85 mL, 6 mmol), BF3-diethyl ether (1.1 mL, 9 mmol) at 0 °C. The whole was heated at 50 °C for 1 h. Additional triethylamine (0.5 mL) and BF3-diethyl ether (0.5 mL) were added and the mixture was heated at 50 °C for another 1 h. LCMS showed m / e - The main peak at 0.05% C = 772 indicates the reaction is complete. The mixture was diluted with 50 mL of DCM, washed twice with water and once with brine, then concentrated to 100 mL, loaded onto silica gel, and purified by flash chromatography using an eluent of hexane / DCM (40% -> 100% DCM). After collecting the main desired peak and removing the solvent under reduced pressure, the desired product was obtained as a purple solid (1.06 g, 81.6% yield). Confirmed by LCMS (APCI): C 42 H 31 Calculated for BBr2F2N2 (M-): 770.1; Found: 770. 1 H NMR(400MHz,chloroform-d) δ 7.81~7.73(m,4H), 7.61~7.53(m,4H), 6.99~6.90(m,2H), 6.85(dd,J=8.3,6.9H z,4H), 6.78~6.71(m,4H), 6.42(s,2H), 6.00(s,2H), 1.98(s,6H), 1.85(s,3H).
[0096] Compound SD-1.3: A mixture of compound SD-1.2 (160 mg, 0.207 mmol), 4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)phenol (184 mg, 0.828 mmol), Pd(dppf)Cl2 (16 mg, 0.022 mol), potassium carbonate (140 mg, 1.01 mmol) in THF / water (8 mL / 1 mL) was degassed and then heated at 80 °C for 120 min. The resulting mixture was diluted with 20 mL of DCM, loaded onto silica gel, and purified by flash chromatography using an eluent of DCM / ethyl acetate (0% → 20% ethyl acetate). After collecting the main desired peak and removing the solvent under reduced pressure, the desired product was obtained as a dark solid (130 mg, 79% yield). 1 H NMR(400MHz,TCE-d2) δ 7.98~7.91(m,4H), 7.62~7.54(m,4H), 7.54~7.46(m,4H), 6.92~6.85(m,4H), 6.84(d,J=2.1Hz,2H), 6. 82~6.74(m,4H), 6.73~6.66(m,4H), 6.46(s,2H), 5.92(s,2H), 4.88(s,2H), 1.92(s,6H), 1.78(s,3H).
[0097] Compound SD-1: A mixture of compound SD-1.3 (80 mg, 0.1 mmol), compound SD-1.4 (100 mg, 0.222 mmol), DMAP / TsOH salt (59 mg, 0.2 mmol), and DIC (0.15 mL) in 6 mL of DCM was stirred at room temperature overnight and then at 45 °C for 2 h. The resulting mixture was loaded onto silica gel and purified by flash chromatography using an eluent of DCM / ethyl acetate (0% → 10% ethyl acetate). The desired di-coupled product was collected as the second major peak. After removal of the solvent, washing with methanol and drying in air, the desired product was obtained as a dark solid (100 mg, 60% yield). 1 Confirmed by 1 H NMR. 1H NMR(400MHz,d2-TCE) δ 8.49(dd,J=16.0,8.1Hz,4H), 7.99(d,J=8.2Hz,6H), 7.85(d,J=8.0Hz,2H), 7.63(dd, J=8.5,3.7Hz,8H), 7.50(t,J=7.8Hz,2H), 7.42~7.25(m,8H), 7.25~7.08(m,10H), 6.8 4(dt,J=36.5,7.3Hz,6H), 6.70(d,J=7.5Hz,4H), 6.48(s,2H), 5.93(s,2H), 2.80(t,J =7.7Hz,4H), 2.63(t,J=7.4Hz,4H), 2.11(t,J=7.7Hz,4H), 1.92(s,6H), 1.78(s,3H).
[0098] Synthesis procedure for compound SD-2 General procedure for the preparation of compounds SD-2.1, SD-2.2 and SD-2.3 [ka]
[0099] Compound SD-2.1: To a solution of 1-benzosuberone (10.0 mmol, 1.46 mL) in 3:1 HO / EtOH (32.5 mL) at room temperature, NHOH·HCl (15.0 mmol, 1.04 g) and sodium acetate (25.0 mmol, 2.05 g) were added and the reaction mixture was stirred at 95 °C for 1 h. It was then cooled to room temperature, filtered, washed with water (150 mL), and lyophilized for 16 h to give 1.64 g of 6,7,8,9-tetrahydro-5H-benzo[7]annulen-5-one oxime (94% yield) as a colorless solid, which was used in the subsequent synthetic step without further purification.
[0100] To a solution of 6,7,8,9-tetrahydro-5H-benzo[7]annulen-5-one oxime (5.71 mmol, 1.00 g) in DMSO (9.00 mL) at room temperature was added KOH (17.1 mmol, 959 mg), and the reaction mixture was heated to 140 °C, after which 1,2-dichloroethane (11.4 mmol, 897 μL) in DMSO (2.00 mL) was added via syringe pump over 3 h. The mixture was then cooled to room temperature, quenched with 1M aqueous NH4Cl (30.0 mL), and extracted with CHCl (3 × 30.0 mL). The combined organics were dried (MgSO4) and concentrated under reduced pressure. Flash chromatography (hexanes → 9:1 hexanes / EtOAc) afforded 262 mg of SD-2.1 (25% yield) as a yellow solid. 1 H NMR(400MHz,chloroform-d) δ 8.18(br s,1H), 7.34(dd,J=7.8,1.3Hz,1H), 7.25~7.19(m,1H), 7.16(dd,J=7.6,1.6Hz,1H), 7.13~7.07(m,1H), 6 .84(t,J=2.8Hz,1H), 6.17(t,J=2.8Hz,1H), 2.91(t,J=6.8Hz,2H), 2.86~2.80(m,2H), 2.07~1.98(m,2H); 13 C NMR (101 MHz, chloroform-d) δ 140.4, 131.8, 129.3, 126.8, 125.9, 125.2, 123.2, 121.8, 118.3, 111.1, 34.9, 27.8, 26.7.
[0101] Compound SD-2.3: A 100 mL two-neck round bottom flask was fitted with an air condenser and a stir bar. Compounds SD-2.1 1,4,5,6-tetrahydrobenzo[6,7]cyclohepta[1,2-b]pyrrole (813.1 mg, 4.4 mmol) and SD-2.2 4-hydroxy-2,6-dichlorobenzaldehyde (424.3 mg, 2.2 mmol) were added to the flask, followed by anhydrous dichloroethane (55 ml). The reaction mixture was sparged with Ar for 30 minutes, followed by the addition of TFA (4 drops). The reaction solution was stirred overnight at room temperature. The reaction was cooled to 0° C. in an ice-water bath, followed by the addition of p-chloranil (731.8 mg, 2.98 mmol). The reaction was maintained at 0° C. for 30 minutes. Then, BF3·OEt2 (3.0 mL, 24.1 mmol) and Et3N (1.9 mL, 13.3 mmol) were added at 0 °C. The reaction mixture was heated to 50 °C for 3 h. The reaction mixture was loaded onto silica gel and purified by flash chromatography using DCM in hexanes (0% → 80% → 90%) as eluent to give pure BODIPY SD-2.3 as a brown-gold solid (476.0 mg, 36% yield). MS (APCI): C 33 H 24 Calculated for BCl2F2N2O ([MH]-)=584 Found: 584. 1 H NMR(400MHz,CDCl3)8.09(dd,J=4.0Hz,2.0Hz,2H), 7.32(dddd,J=13.2Hz,7.2Hz,7.2Hz,2.0Hz,4H),7.22(dd,J=6.4Hz,2.0Hz,2H ), 6.99(s,2H), 6.43(s,2H), 5.77(bs,1H), 2.63(dd,J=6.8Hz,6.8Hz,4H), 2.32(bs,4H), 2.03(ddd,J=14.0Hz,6.8Hz,6.8Hz,4H).
[0102] [ka]
[0103] Compound SD-2.4: A mixture of 4-bromo-1,8-naphthalic anhydride (2.77 g, 10 mmol), 4-bromo-2-nitrophenol (3.27 g, 15 mmol) was degassed under vacuum for 30 minutes, then anhydrous NMP (50 mL) was added, followed by sodium hydroxide (0.2 g, 5 mmol) and copper powder (0.318 g, 5 mmol). The mixture was sparged with argon for 20 minutes and then heated at 180° C. overnight under argon atmosphere. After cooling to room temperature, 50 mL of 20% aqueous hydrochloric acid was added dropwise to the solution, followed by 50 mL of water. The resulting mixture was allowed to stand for 3 hours, then filtered to collect the precipitate, which was dried under vacuum to give 4.6 g of crude product. The crude product was dispersed in 30 mL of acetone and stirred at room temperature overnight to dissolve the impurities. Filtration and drying under vacuum gave a brownish yellow solid (3.3 g, 80% yield) as the desired product. LCMS(APCI+):C 18 Calculated for H9BrNO6 (M+H)=413.95; Found: 414. 1 H NMR(400MHz,TCE-d2) δ 8.70(dd,J=8.4,1.2Hz,1H), 8.63(dd,J=7.3,1.2Hz,1H), 8.41(d,J=8.3Hz,1H), 8.2 4(d,J=2.4Hz,1H), 7.89~7.79(m,2H), 7.20(d,J=8.7Hz,1H), 6.82(d,J=8.3Hz,1H).
[0104] Compound SD-2.5: A mixture of compound SD-2.4 (1.5 g, 3.6 mmol), iron powder (0.60 g, 10.8 mmol) in acetic acid (50 mL) was heated at 125° C. for 30 min. After cooling to room temperature, 100 mL of water was added to the mixture with stirring. The resulting mixture was filtered, washed with water, and dried in air and vacuum to give a solid (1.35 g, 82% yield). LCMS (APCI-): C 18 H 10 Calculated for BrNO4=382.98; Found: 383. 1H NMR (400MHz, DMSO-d6) δ 9.01~8.26 (m, 3H), 7.96 (s, 1H), 6.93 (dd, J=85.2, 36.5Hz, 4H), 5.54 (s, 2H).
[0105] Compound SD-2.6: Compound SD-2.5 (2.65 g, 6.9 mmol) was dispersed in acetic acid (50 mL) / water (10 mL) and cooled to 0° C. Pre-cooled hydrochloric acid (2.8 mL, 34.5 mmol) was added under stirring, followed by dropwise addition of sodium nitrite solution (3.57 g, 52 mmol) in 15 mL of water at 0° C. The whole was stirred at 0° C. for 1 h, then transferred to an addition funnel and added dropwise to copper sulfate solution (12 g, 47 mmol, in 140 mL of water) at 130° C. over 1 h. After cooling to room temperature, the precipitate was collected by filtration, washed with water (100 mL×3), and then stirred in 50 mL of acetone at 40° C. for 30 min. Filtration and drying in air followed by vacuum gave a brown-yellow solid (1.76 g, 70% yield). LCMS (APCI+): C 18 Calculated for H8BrO4 (M+H)=366.95; found: 367. 1 H NMR(400MHz,d2-TCE) δ 8.51(dd,J=12.3,8.1Hz,2H), 8.12(d,J=2.3Hz,1H), 7.86(d,J=7.9Hz,1H), 7.60(dd,J=8.8,2.3Hz,1H), 7.28(d,J=8.3Hz,1H), 7.23(d,J=8.8Hz,1H).
[0106] Compound SD-2.7: A mixture of compound SD-2.6 (550 mg, 1.5 mmol), 4-(4-aminophenyl)butyric acid (537 mg, 3 mmol) and DMAP (12.2 mg, 0.1 mmol) in 10 mL of DMF was heated in a microwave reactor at 165° C. for 2.5 h. The resulting solution was added dropwise to 50 mL of acetone with stirring. A precipitate formed, which was filtered and dried overnight in a vacuum oven at 60° C. to give the desired product as a brownish yellow solid (0.49 g, 62% yield). LCMS (APCI-): C 28 H 18Calculated for BrNO5=527.04; Found: 527. 1 H NMR(400MHz,DMSO-d6) δ 8.54(d,J=2.3Hz,1H), 8.41(dd,J=9.9,8.0Hz,2H), 8.33(d,J=7.9Hz,1H), 7.71(dd,J=8.8,2.3Hz,1H), 7.39(dd,J=8. 6,4.2Hz,2H), 7.25(d,J=8.0Hz,2H), 7.17(d,J=7.9Hz,2H), 2.63~2.55(m,2H), 2.27~2.15(m,2H), 1.87~1.73(m,2H).
[0107] Compound SD-2.8: A mixture of compound SD-2.7 (385 mg, 0.729 mmol), phenylboronic acid (178 mg, 1.45 mmol), Pd(dppf)Cl2 (36 mg, 0.05 mmol), potassium carbonate (276 mg, 2 mmol) in a co-solvent of THF / DMF / water (20 L / 4 mL / 2 mL) was degassed and then heated at 80 °C overnight. The mixture was worked up with 200 mL of ethyl acetate and 50 mL of 0.6 N aqueous hydrochloric acid. The aqueous phase was extracted with ethyl acetate (100 mL x 2). The organic phase was collected, washed with brine (100 mL x 2), dried over sodium sulfate, then dry-loaded onto silica gel and purified by flash chromatography using an eluent of DCM / EA (0% -> 40% EA with 0.1% TFA). The main desired fraction was collected and the solvent was removed under reduced pressure to give a yellow solid (250 mg, 65% yield). LCMS(APCI-):C 34 H 23 Calculated for NO5=525.16; Found: 525. 1 H NMR(400MHz,TCE-d2) δ 8.55(dd,J=19.5,8.1Hz,2H), 8.20(d,J=2.1Hz,1H), 8.01(d,J=8.1Hz,1H), 7.72(dd,J=8.6,2.1Hz,1H), 7.62(d,J=7.3 Hz,2H), 7.51~7.28(m,7H), 7.17(d,J=8.2Hz,2H), 2.72(t,J=7.7Hz,2H), 2.39(t,J=7.3Hz,2H), 1.99(q,J=7.2Hz,2H).
[0108] Compound SD-2: A mixture of compound SD-2.3 (31 mg, 0.053 mmol), compound SD-2.8 (43 mg, 0.082 mmol), EDC·HCl (100 mg, 0.52 mmol) and DMAP / p-TsOH (16 mg, 0.054 mmol) in DCM (8 mL) was stirred at room temperature overnight. The resulting mixture was then loaded onto silica gel and purified by flash chromatography using an eluent of DCM / ethyl acetate (0%→5% ethyl acetate). The main red fraction was collected and concentrated under reduced pressure to about 1 mL, after which 10 mL of methanol was added. The resulting precipitate was filtered and dried in air to give a dark red solid (41 mg, 70.8% yield). LCMS (APCI-): C 67 H 46 Calculated for BCl2F2N3O5=1091.29; Found: 1091. 1 H NMR(400MHz,d2-TCE) δ 8.56(dd,J=19.3,8.1Hz,2H), 8.21(d,J=2.2Hz,1H), 8.02(d,J=8.1Hz,1H), 7.97(t,J=4.7Hz ,2H), 7.73(dd,J=8.6,2.1Hz,1H), 7.63(dd,J=7.2,1.7Hz,2H), 7.50~7.41(m,3H), 7.38(dd,J =8.0,2.2Hz,3H), 7.34~7.25(m,7H), 7.25~7.18(m,4H), 6.40(s,2H), 2.82(t,J=7.5Hz,2H), 2.67(t,J=7.4Hz,2H), 2.60~2.49(m,4H), 2.24(s,4H), 2.18~2.07(m,2H), 2.03~1.90(m,4H).
[0109] Synthesis procedure for compound SD-3 [ka] General procedure for preparation of SD-3.2 [ka]
[0110] AlCl3 (78.0 g, 585 mmol, 31.9 mL, 1.80 equiv) was added to anhydrous DCM (1.50 L) at 0°C-10°C. The mixture was stirred at 0°C for 30 min. To this mixture was added a mixture of compound SD-3.1A (88.1 g, 585 mmol, 72.2 mL, 1.80 equiv) in anhydrous DCM (100 mL) at 0°C-10°C under N2. To this mixture was added compound SD-3.1 (82 g, 325 mmol, 1.00 equiv) in small portions and the mixture was stirred at 25°C-30°C for 30 min. The mixture was stirred at 50°C for 12 h. Thin layer chromatography (TLC) (petroleum ether / ethyl acetate = 10 / 1) showed the reaction was complete. The mixture was cooled to 25°C-30°C and poured into water (1.00 L). The mixture was separated and the aqueous phase was extracted with DCM (500 mL x 2). The combined organic layers were dried over Na2SO4 and concentrated. The product was purified by MPLC (100 mesh-200 mesh silica gel, DCM). SD-3.2 (82.0 g, 223 mmol, 68.8% yield) was obtained as an orange solid. LCMS (APCI+), C 25 H 18 Calculated for O3=366.1; Found: 366. 1 H NMR (400 MHz, chloroform-d) δ 8.57 (dd, J = 8.6, 1.0 Hz, 1H), 8.30–8.17 (m, 4H), 7.97 (d, J = 8.1 Hz, 1H), 7.78 (d, J = 8.1 Hz, 1H), 7.73 (d, J = 8.1 Hz, 1H), 7.64–7.48 (m, 3H), 3.75 (s, 3H), 3.41 (t, J = 6.5 Hz, 2H), 2.86 (t, J = 6.5 Hz, 2H).
[0111] General procedure for the preparation of compound SD-3.3 [ka] Trifluoroacetic acid (TFA) (231 g, 2.03 mol, 150 mL, 9.90 equiv.) was added to a mixture of SD-3.2 (75.0 g, 204 mmol, 1.00 equiv.) in anhydrous DCM (600 mL) at 0°C-10°C. The mixture was stirred at 0°C-10°C for 30 min. Triethylsilane (Et3SiH) (71.4 g, 614 mmol, 98.1 mL, 3.00 equiv.) was added to this mixture at 0°C-10°C, and the mixture was stirred at 25°C for 16 h. TLC (petroleum ether / ethyl acetate=3 / 1) showed the reaction was complete. The mixture was concentrated to give the crude product. The crude product was triturated with methyl tertiary butyl ether (MTBE) (400 mL) at 25°C-30°C for 30 min. The mixture was filtered, and the filter cake was washed with MTBE (100 mL). The filter cake was dried under vacuum. The mother liquor was concentrated and purified by silica gel chromatography (100 mesh to 200 mesh silica gel, petroleum ether / ethyl acetate=100 / 1→2 / 1). Compound SD-3.3 (62.0 g, 176 mmol, 85.9% yield) was obtained as a yellow solid. 1 H NMR(400MHz,CDCl3) δ 8.27~8.08(m,4H), 7.91(d,J=8.3Hz,1H), 7.68(dd,J=5.5,7.9Hz,2H), 7.53(t,J=8.0Hz,1H), 7.48(dt,J=1.5,7.9H) z,2H), 7.34(d,J=7.7Hz,1H), 3.71(s,3H), 3.07(t,J=7.8Hz,2H), 2.47(t,J=7.2Hz,2H), 2.12(quin,J=7.5Hz,2H).
[0112] General procedure for the preparation of compound 3.4 [ka] n-Bromosuccinimide (NBS) (88.4 g, 496 mmol, 3.40 equiv.) was added in small portions to a mixture of SD-3.3 (51.5 g, 146 mmol, 1.00 equiv.) in CHCl3 (2.00 L) at 25 °C. The mixture was stirred at 25 °C for 16 h while keeping in the dark. LCMS (ET39890-22-P1A) showed the reaction was complete. The mixture was washed with Na2SO3 (1N, 1.00 L). The mixture was separated and the aqueous phase was extracted with DCM (200 mL). The combined organic layers were concentrated to give the crude product. The product was purified by silica gel chromatography (100 mesh to 200 mesh silica gel, petroleum ether / ethyl acetate = 1 / 0 → 1 / 1). SD-3.4 (69.2 g, 102 mmol, 69.9% yield, 87.0% purity) was obtained as a reddish-brown oil. LCMS (APCI+), C 25 H 17 Calculated for Br3O2=585.88; Found: 589.
[0113] General procedure for preparation of SD-3.5 [ka] SD-3.4A (228 g, 1.19 mol, 151 mL, 10.0 equiv) was added to a mixture of SD-3.4 (70.0 g, 119 mmol, 1.00 equiv) and CuI (113 g, 594 mmol, 5.00 equiv) in DMA (490 mL) at 25 °C. The mixture was stirred at 160 °C under N2 for 3 h. LCMS (ET39890-26-P1A) showed the reaction was complete. The mixture was cooled to 25 °C-30 °C and diluted with water (1.50 L) and ethyl acetate (EtOAc) (1.00 L). The mixture was filtered through a Celite pad. The filter cake was washed with EtOAc (500 mL x 2). The combined filtrate was separated and the aqueous phase was extracted with EtOAc (500 mL x 2). The combined organic layers were concentrated to give the crude product. The product was purified by silica gel chromatography (100 mesh to 200 mesh silica gel, petroleum ether / ethyl acetate=1 / 0→1 / 1). SD-3.5 (40.0 g, 71.9 mmol, 60.5% yield) was obtained as a reddish-brown oil.
[0114] General procedure for the preparation of compound SD-3.6 [ka] Sodium hydroxide (NaOH) (8.63 g, 215 mmol, 3.00 equiv) was added to a mixture of SD-3.5 (40.0 g, 71.9 mmol, 1.00 equiv) in tetrahydrofuran (THF) (200 mL), methanol (MeOH) (200 mL) and H2O (200 mL) at 25 °C. The mixture was stirred at 25 °C for 2 h. TLC (petroleum ether / ethyl acetate = 10 / 1) showed the reaction was complete. The mixture was acidified with hydrogen chloride (HCl) solution (1N) to pH = 1-2. The mixture was concentrated to remove the solvent. The residue was diluted with water (150 mL) and extracted with EtOAc (100 mL x 2). The combined organic layers were concentrated. The crude product was purified by silica gel chromatography (100 mesh-200 mesh silica gel, petroleum ether / ethyl acetate = 1 / 0 → 0 / 1). SD-3.6 (26.2 g, 48.1 mmol, 66.9% yield, 99.6% purity) was obtained as a yellow solid. 1 HNMR (400MHz, CDCl3) δ 8.37~7.93(m,6H), 7.91~7.50(m,2H), 3.47~3.13(m,2H), 2.68~2.53(m,2H), 2.26~2.13(m,2H).
[0115] General procedure for the preparation of compound SD-3 [ka]
[0116] Compound SD-3.7: To a solution of 2,6-dichloro-4-hydroxybenzaldehyde (0.335 mmol, 64 mg), 4-(tris(trifluoromethyl)perylene-3-yl)butyric acid (0.369 mmol, 200 mg) and DMAP·pTsOH salt (0.034 mmol, 10 mg) in CHCl (1.68 mL) was added DIC (1.34 mmol, 210 μL) and the reaction mixture was stirred at room temperature for 2 h. It was then filtered through Celite and concentrated under reduced pressure. Flash chromatography (toluene) afforded 187 mg of SD-3.7 (78% yield) as a yellow solid. 1 H NMR (400 MHz, chloroform-d) δ 10.50–10.33 (m, 1H), 8.48–7.50 (m, 8H), 7.19–7.14 (m, 2H), 3.45–3.25 (m, 2H), 2.83–2.59 (m, 2H), 2.33–2.03 (m, 2H).
[0117] Compound SD-3: To a solution of SD-2.1 (0.461 mmol, 84 mg) and SD-3.7 (0.210 mmol, 150 mg) in CHCl (4.50 mL) was added p-TsOH·HO (0.021 mmol, 3 mg) and the reaction mixture was stirred at room temperature for 1 h. Then DDQ (0.252 mmol, 57 mg) was added and the mixture was stirred at room temperature for 1 h. Triethylamine (TEA) (1.26 mmol, 175 μL) was added and the mixture was stirred at room temperature for 1 h, after which BF·OEt (1.89 mmol, 233 μL) was added and the mixture was stirred at room temperature for 2 h. It was then diluted with EtOAc (30.0 mL), washed with 3M HCl (3×30.0 mL), dried (MgSO) and concentrated under reduced pressure. Flash chromatography (4:1 toluene / hexanes→toluene) afforded 106 mg of SD-3 (45% yield) as a purple solid. 1 H NMR (400MHz, methylene chloride-d2) δ 8.61~7.60(m,10H), 7.39~7.11(m,8H), 6.54~6.40(m,2H), 3.46~3.30(m,2H), 2.90~2.55(m,6H), 2.39~2.09(m,6H), 2.08~1.94(m,4H).
[0118] Synthesis procedure for compound SD-4 [ka]
[0119] General procedure for the synthesis of compound SD-4 A 10 mL vial was fitted with a stir bar. Compound SD-2.3 (25.0 mg, 0.043 mmol), FD-1.5 (24.0 mg, 0.053 mmol), EDC·HCl (40.9 mg, 0.21 mmol) and DMAP·TsOH (25.6 mg, 0.085 mmol) were added to the vial, followed by anhydrous DCM (1.5 ml). The reaction mixture was heated to 40° C. overnight. After the reaction was cooled to room temperature, the reaction mixture was loaded onto silica gel and purified by flash chromatography using DCM in EtOAc (0%→5%) as the eluent to give pure RL-naphthalimide-BODIPY 1605-23-3 as a dark purple solid. The solid was further triturated with MeOH (10 ml) to give RL-naphthalimide-BODIPY SD-4 (21.0 mg, 48% yield). MS (APCI): C 61 H 41 Calculated for Cl2F2N3O5 ([MH]-)=1015. Found: 1015. 1 H NMR(400MHz,CDCl3) δ 8.66(dd,J=18.4Hz,7.6Hz,2H), 8.10(m,3H), 7.99(d,J=8.0Hz,1H), 7.56(ddd,J=8.0Hz,8.0Hz,1.6Hz,1H), 7.36(m,13H), 7.22(dd,J=6.8 Hz,2.0Hz,2H), 6.45(s,2H)2.88(t,J=7.6Hz,2H), 2.72(t,J=7.2Hz,2H), 2.63(m,4H), 2.20(m,6H), 2.04(ddd,J=6.8Hz,6.8Hz,6.8Hz,4H).
[0120] Synthesis procedure for compound SD-5 [ka]
[0121] General procedure for the synthesis of compound SD-5 A 25 mL vial was fitted with a stir bar. Compound SD-2.3 (40.0 mg, 0.068 mmol), 1605-99 SD-5.1 (77.5 mg, 0.137 mmol), EDC·HCl (65.2 mg, 0.340 mmol) and DMAP·TsOH (41.1 mg, 0.137 mmol) were added to the vial, followed by anhydrous DCM (4 ml). The reaction mixture was heated to 40° C. overnight. After the reaction was cooled to room temperature, the reaction mixture was loaded onto silica gel and purified by flash chromatography using DCM in EtOAc (0%→4%) as the eluent to give pure RL-naphthalimide-BODIPY SD-5 as a dark blue solid. The solid was further triturated with MeOH (15 ml) to give RL-naphthalimide-BODIPY SD-5 (46.0 mg, 60% yield). MS (APCI): C 66 H 41 Calculated for BCl2F5N3O5 ([MH]-)=1132. Found: 1132. 1 H NMR(400MHz,CDCl2CDCl2) δ 8.69(d,J=8.0Hz,1H), 8.65(d,J=8.0Hz,1H), 8.30(d,J=2.0Hz,1H), 8.11(d,J=8.0Hz,1H), 8.06(m,2H), 7.82(m,5H), 7.65( m,2H), 7.55(d,J=8.0Hz,1H), 7.39(m,9H), 7.30(m,2H), 6.48(s,2H), 4.07(s,2H), 2.63(m,4H), 2.33(bs,3H), 2.06(m,4H).
[0122] Preparation of polymer solutions Preparation of 25% PMMA polymer solution Weigh out 30 g of PMMA polymer (unknown grade) and add to a 250 mL glass bottle. Measure 90 mL of cyclopentanone or toluene using a graduated cylinder and add to the same glass bottle. Stir the solution with a stir bar on a stirring station and heat to 50° C. until completely dissolved.
[0123] Preparation of dye-polymer solutions 0.2 mg FD-1, 0.16 mg compound SD-3 and 150 mg silicone particles (TSR9000, momentive). To this solution, add 4 mL of 25% PMMA solution. The solution is mixed thoroughly by vortexing for 1 minute, followed by sonication for 15 minutes, and then stirred at a gentle speed on a stir plate.
[0124] Film Production Individual dye-polymer films The basic optical properties were evaluated based on the dye-polymer film. Scattering centers (20% silica beads, average size 2μm-3μm) and appropriate weight of dye were dissolved in 3mL of the above 25% PMMA / toluene solution to obtain a 2mmol / L dye-polymer solution. The solution was thoroughly mixed by vortexing for 1min, followed by sonication for 15min. Several 1''×1'' glass substrates were washed with soapy water and air-blow dried. The glass substrates were then placed on a spin-coater holder and the dye-polymer solution was poured onto the glass substrate. The spin speed was set to 1000RPM to spin-coat the film for 20s. The wet coating was then dried at room temperature for 1h and heated at 130℃ for 30min.
[0125] Green and red dye-polymer films In order to mix blue light with R,G,B colors to convert it to white light, both green and red dyes were mixed into one film. A 2''x2'' glass substrate is washed with soapy water and air blow dried. The glass substrate is then placed on a spin coater holder and the dye-polymer solution was poured onto the glass substrate. The film is spin coated with a spin speed set to 1000 RPM. The wet coating is then dried at room temperature for 1 hour and heated at 130°C for 30 minutes. After the film is dry, it is immersed in water for 5 minutes to separate the film from the glass.
[0126] Further example films were made by varying the weight amounts of the first photoluminescent dye, the second photoluminescent dye, the scattering particles, and / or the polymer matrix material as shown in Table 1 below.
[0127] [Table 1B]
[0128] Characterization of dye compounds Absorption and Emission Spectra The absorbance and emission spectra of the individual dyes in the polymer films were measured by UV-vis (Shimadzu uv-vis 3600 spectrophotometer) and Fluorolog 3 (Horiba, Ltd.), respectively.
[0129] Absolute quantum yield of dye The absolute quantum yield of the dye film was measured at a wavelength of 450 nm by an absolute PL quantum yield spectrometer C11347 (Hamamatsu Photonics).
[0130] Characterization of blue light conversion WLC films External quantum yield of WLC films in LED backlight devices The external quantum yield and other optical properties of the WLC films in LED backlit display applications were tested using a test setup configured as described in Figure 4. BEF means brightness enhancement film Vikuiti BEF (3M). DBEF means polarizer / enhancement film (3M). A blue LED edge-lit backlight was part of the kindle device. MCPD means multi-channel photon detection (MCPD-9800, Otsuka Electronics Co., Ltd.).
[0131] EQE is represented by the formula:
number
[0132] Color gamut - BT.2020 ratio A color gamut is a certain complete subset of colors. A color gamut can be represented by a triangle in a chromaticity diagram. The three corners of the triangle are the primary colors. The more colors a display can show, the larger the area of the triangle and therefore the wider the color gamut. BT.2020 is the color gamut standard for UHD projectors and TVs recommended by the ITU (International Telecommunication Union).
[0133] After converting the optical spectrum measured by the configuration shown in Figure 4 into the gamut triangle of the CIE 1931 chromaticity diagram, the area of the triangle was estimated and divided by the area of the BT.2020 triangle to obtain the BT.2020 ratio referred to herein. The larger this ratio, the wider the color gamut of the WLC film. To achieve a wide color gamut, the emission spectral shape of each primary color should be as narrow as possible. A narrow spectral shape can be characterized as a small FWHM of the emission spectrum.
[0134] Comparative Example Table 2 below shows Comparative Example 1 and Comparative Example 2, which are examples disclosed in US Patent Application No. 63 / 001,924. Red dye SD-X corresponds to SD-1 in US Patent Application No. 63 / 001,924. As can be seen from Table 2, Example 1 has a large color gamut (94% BT.2020 ratio), but its red emission spectrum FWHM is 68 nm, which is not very narrow. Example 2 has a smaller color gamut (88% BT.2020 ratio), but its red emission spectrum FWHM is narrower.
[0135] [Table 2]
[0136] Working Example The films of both the examples listed in Table 4 below and the comparative examples listed in Table 2 above were fabricated by the methods described above in the section entitled "Film Fabrication." Examples 3-9 in Table 5 were made using the dyes shown in Tables 2 and 3. All of the green-emitting dyes listed have a FWHM of less than 25 nm, and most of the red-emitting dyes have a FWHM of less than 44 nm. All of the dyes have an internal quantum yield of greater than 80%, with some having a quantum yield of greater than 95%.
[0137] The transmittance of these Examples 3-11 in Table 5 was evaluated by the method described above in the section entitled "Characterization of Blue Light Conversion WLC Films." The majority of the examples show an EQE of greater than 51%, an average increase of 10% compared to the comparative examples in Table 2. This is primarily due to the internal quantum yields of the dyes in Tables 3 and 4. In addition, all films have FWHM of the green emission spectrum less than 33 nm, and FWHM of the red emission spectrum less than 63 nm, and BT.2020 ratios greater than 90%.
[0138] [Table 3]
[0139] [Table 4]
[0140] [Table 5]
Claims
1. A wavelength conversion film, A polymer matrix; a first photoluminescent dye that absorbs blue wavelength light and emits green wavelength light with an emission spectrum having a full width at half maximum of less than 40 nm; a second photoluminescent dye that absorbs blue or green wavelength light and emits red wavelength light with an emission spectrum having a full width at half maximum of less than 55 nm; A light scattering center; Including, the first photoluminescent dye, the second photoluminescent dye, and the light scattering centers are disposed in the polymer matrix.
2. 2. The wavelength conversion film of claim 1, wherein the first photoluminescent dye comprises an optionally substituted BODIPY group, a linking group, and an optionally substituted isoquinoline group.
3. The first photoluminescent dye is 【Chemistry 1】 or 【Chemistry 2】 The wavelength conversion film according to claim 2 .
4. 2. The wavelength conversion film of claim 1, wherein the first photoluminescent dye comprises an optionally substituted BODIPY group, a linking group, and an optionally substituted naphthalimide group.
5. The first photoluminescent dye is 【Chemistry 3】 The wavelength conversion film according to claim 4 .
6. 2. The wavelength conversion film of claim 1, wherein the second photoluminescent dye comprises an optionally substituted BODIPY group, a linking group, and an optionally substituted isoquinoline group.
7. The second photoluminescent dye is 【Chemistry 4】 【Chemistry 5】 or 【Chemistry 6】 The wavelength conversion film according to claim 6 .
8. 2. The wavelength conversion film of claim 1, wherein the second photoluminescent dye comprises an optionally substituted BODIPY group, a linking group, and an optionally substituted naphthalimide group.
9. The second photoluminescent dye is 【Chemistry 7】 9. The wavelength conversion film according to claim 8 ,
10. 2. The wavelength conversion film of claim 1, wherein the second photoluminescent dye comprises an optionally substituted BODIPY group, a linking group, and an optionally substituted perylene group.
11. The second photoluminescent dye is 【Chemistry 8】 9. The wavelength conversion film according to claim 8 ,
12. 12. The wavelength conversion film according to claim 1, wherein the wavelength conversion film has an internal quantum yield of more than 80%.
13. 12. The wavelength conversion film according to claim 1, wherein the wavelength conversion film has an external quantum yield of more than 50%.
14. The wavelength conversion film according to any one of claims 1 to 11, wherein the wavelength conversion film has a color gamut exceeding 90% of the BT.2020 standard.
15. 12. The wavelength conversion film according to claim 1, wherein the wavelength conversion film has a thickness of 10 μm to 40 μm.
16. A light emitting device comprising the wavelength conversion film of any one of claims 1 to 15.
17. 16. A backlit device having a blue light source comprising the wavelength conversion film of any one of claims 1 to 15.