Perovskite-silicon based stacked solar cell and method for producing same
A two-step method for forming perovskite layers on textured silicon-based cells in stacked solar cells addresses the deposition challenge, ensuring efficient light trapping and voltage adjustment, thus improving the solar cell's performance.
Patent Information
- Application Number
- JP2024527766
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-12
- Filing Date
- 2022-05-16
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2042-05-16
AI Technical Summary
The challenge in manufacturing perovskite-silicon-based stacked solar cells is the difficulty in uniformly depositing perovskite layers on the textured light-trapping structures of silicon-based cells without compromising the efficiency gains of the textured structure, leading to increased manufacturing costs.
A method involving a two-step process where a first perovskite layer is formed by solution spin-coating on a textured silicon-based cell, followed by a second layer using perovskite framework vacuum deposition, ensuring conformal coverage and maintaining the textured structure while adjusting the band gap and open-circuit voltage.
This approach maintains the light-trapping and reflection-reducing effects of the textured structure, achieving high short-circuit current and open-circuit voltage, thereby enhancing the photoelectric conversion efficiency of the stacked solar cells.
Smart Images

Figure 2024544962000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to the technical field of stacked solar cells, in particular to a perovskite-silicon based stacked solar cell and a method for manufacturing the same.
[0002] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to a Chinese patent application, application number 202111369100.8, entitled "Perovskite-silicon based stacked solar cell and manufacturing method thereof," filed with the China Patent Office on November 12, 2021, all of which are incorporated herein by reference. [Background technology]
[0003] A perovskite-silicon based stacked solar cell is fabricated by using a silicon-based cell as the bottom cell and a perovskite cell as the top cell, connected in between by a tunnel recombination layer.
[0004] In the manufacturing process of perovskite-silicon-based stacked solar cells, each functional layer of the perovskite cell needs to be uniformly spin-coated on the pyramidal textured light trapping structure of the silicon-based cell, but the thickness of each functional layer of the perovskite cell is only a few hundred nanometers, and it is difficult to deposit it on the pyramidal textured light trapping structure of the micron order by solution spin coating. If the bottom cell is polished to reduce the roughness of the textured light trapping structure, it is possible to manufacture the perovskite cell by solution spin coating, but the improvement in cell efficiency due to the textured light trapping structure will be lost and the manufacturing cost will be greatly increased. Therefore, how to obtain an efficient perovskite-silicon-based stacked solar cell while maintaining the textured structure of the bottom cell is currently an issue that needs to be urgently solved. Summary of the Invention
[0005] The objective of the present application is to provide a perovskite-silicon based stacked solar cell and a manufacturing method thereof, which can be used to obtain a perovskite-silicon based stacked solar cell that has both a high open circuit voltage and a high short circuit current while maintaining the texture structure of the bottom cell.
[0006] In a first aspect, the present application provides a method for producing a method for manufacturing a pharmaceutical composition comprising: Providing a substrate including a textured silicon-based bottom cell, a charge recombination layer, and a first carrier transport layer, which are stacked in sequence; forming a perovskite light absorbing layer consisting of two perovskite layers, a first perovskite layer and a second perovskite layer, on a first carrier transport layer having a textured structure, wherein the first perovskite layer is manufactured by a solution process and the second perovskite layer is manufactured by a perovskite framework vacuum deposition process.
[0007] In the above technical solution, the first perovskite layer and the second perovskite layer formed on the first carrier transport layer having a texture structure constitute a perovskite light absorbing layer, in which the first perovskite layer is manufactured by a solution method, and the second perovskite layer is manufactured by a perovskite skeleton vacuum deposition method. The perovskite skeleton vacuum deposition method includes first forming a mixture of PbX2 and CsY by vacuum deposition to form a perovskite skeleton, in which X and Y are chlorine ions (Cl - ), bromide ion (Br - ), iodine ion (I - ), and thiocyanate ion (SCN -), and the mixture of the two may be a mixture of two or more materials, preferably a mixture of lead iodide and cesium iodide or a mixture of lead iodide and cesium bromide, and then using a conventional solution coating method such as solution spin coating, knife coating, spraying, etc., the perovskite skeleton is covered with an organic amine solution and reacted to form a perovskite thin film. The formed second perovskite layer can conformally cover the peaks and slopes of the texture structure, and the first perovskite layer formed by the solution method can be deposited at the bottom of the texture structure to partially fill it. On this basis, the perovskite light absorbing layer composed of the above two perovskite layers combines the advantages of both the solution method and the vacuum deposition method, while avoiding the disadvantages of the two methods. Not only can the good light trapping effect and reflection reduction effect of the texture structure be effectively maintained to obtain a high short circuit current, but the solution components can also be easily adjusted to obtain the required wide band gap and high open circuit voltage. From this, it can be seen that, compared with the prior art, the manufacturing method of the perovskite-silicon based stacked solar cell provided in the present application effectively balances the tradeoff between maintaining the shape of the textured structure and adjusting the perovskite composition, and greatly expands the process control window and the range of component and material selection for the manufacture of highly efficient stacked cells.
[0008] In some possible implementations, when the average vertical distance from the bottom to the top of the texture structure of the first carrier transport layer is L, the average thickness of the first perovskite layer manufactured by the solution method is in the range of more than 0 and less than 1 / 2L. At this time, the first perovskite layer manufactured by the solution method is deposited at the bottom of the texture structure of the first carrier transport layer, and the thickness is less than half the height of the texture structure. On this basis, the formed perovskite light absorbing layer can maintain good texture characteristics, that is, when the perovskite light absorbing layer is irradiated with light, the texture structure can improve the photoelectric conversion efficiency through the light trapping effect and the reflection reduction effect. When the thickness of the first perovskite layer manufactured by the solution method is more than half the height of the texture structure, the texture structure of the formed perovskite light absorbing layer has a small height, a high light reflectance, and a low photoelectric conversion efficiency.
[0009] In some possible implementations, the step of forming a perovskite light absorbing layer consisting of two perovskite layers, a first perovskite layer and a second perovskite layer, on a first carrier transport layer having a textured structure includes the steps of manufacturing the first perovskite layer by a solution method on the first carrier transport layer having a textured structure, and then manufacturing the second perovskite layer by a perovskite skeleton vacuum deposition method.
[0010] In the situation where the above technical solutions are adopted, the perovskite light absorbing layer can be manufactured by a two-step method of solution method followed by perovskite skeleton vacuum deposition method. Specifically, a first perovskite layer is first formed on a first carrier transport layer having a textured structure by a solution method, and then a second perovskite layer is formed on the first perovskite layer by a perovskite skeleton vacuum deposition method. On this basis, the first perovskite layer manufactured by the solution method is deposited on the bottom of the textured structure of the first carrier transport layer, and the band gap of the perovskite can be adjusted by changing the components of the perovskite solution. The second perovskite layer manufactured by the perovskite skeleton vacuum deposition method conformally covers the first perovskite layer and the textured structure that is not completely filled without changing the textured structure, so that the textured structure is maintained to obtain good light trapping effect and reflection reduction properties, and the textured structure is guaranteed to be covered, avoiding short circuits caused by the electrodes directly contacting the textured structure. The stacked battery manufactured by this method combines the advantages of the conventional stacked battery solutions, avoids the shortcomings faced by the conventional techniques, and effectively balances the contradiction between maintaining the shape of the textured structure and adjusting the solution components.
[0011] In some possible implementations, the step of forming a perovskite light absorbing layer consisting of two perovskite layers, a first perovskite layer and a second perovskite layer, on a first carrier transport layer having a textured structure includes the step of manufacturing the second perovskite layer on the first carrier transport layer having a textured structure by a perovskite framework vacuum deposition method, and then manufacturing the first perovskite layer by a solution method.
[0012] In the situation where the above technical solutions are adopted, the perovskite light absorbing layer can be manufactured by a two-step method of perovskite skeleton vacuum deposition followed by a solution method. Specifically, a second perovskite layer is first formed on a first carrier transport layer having a textured structure by a perovskite skeleton vacuum deposition method, and then a first perovskite layer is formed on the second perovskite layer by a solution method. On this basis, the second perovskite layer manufactured by the perovskite skeleton vacuum deposition method is conformally bonded to the textured structure of the first carrier transport layer, and the textured structure is maintained to obtain good light trapping effect and reflection reduction characteristics. The first perovskite layer manufactured by the solution method is deposited at the bottom of the textured structure, which is advantageous for obtaining a high open circuit voltage.
[0013] In some possible implementations, the step of forming a perovskite light absorbing layer consisting of two perovskite layers, a first perovskite layer and a second perovskite layer, on a first carrier transport layer having a textured structure includes the steps of depositing a perovskite framework on the first carrier transport layer having a textured structure by a vacuum deposition method, and then manufacturing the first perovskite layer by a solution method, where the solution used in the solution method includes an excess of an organic amine. In the process of forming the first perovskite layer, the material in the perovskite framework is reacted with the organic amine to form the second perovskite layer.
[0014] In the above technical solution, the method of first preparing the second perovskite layer by vacuum deposition of the perovskite skeleton and then preparing the first perovskite layer by solution method may first vacuum deposit the perovskite skeleton, and then simultaneously prepare the first and second perovskite layers in a one-step method. When the solution used in the solution method is applied to the perovskite skeleton, the excess organic amine contained in the solution reacts with the perovskite skeleton to produce the second perovskite layer. The produced second perovskite layer conformally covers the textured structure. The first perovskite layer produced by the solution method is deposited on the bottom of the textured structure covered by the second perovskite layer and partially fills it, forming a perovskite light-absorbing layer.
[0015] In some possible implementations, the solute of the solution used in the solution process is Cs or a mixed perovskite component containing FA or MA, Cs x FA y MA z PbBr m I n (x+y+z=1, m+n=3), and the solvent is one or more of N,N-dimethylformamide and dimethylsulfoxide. In the method for simultaneously manufacturing the first and second perovskite layers in a one-step process by first vacuum-depositing a perovskite skeleton, the solution used not only contains lead iodide and a mixture of formamidine hydroiodide, methylammonium bromide, and formamidine hydrobromide in the above-mentioned mixing ratio, but also contains an organic amine component in excess of the stoichiometric ratio. The excess organic amine component reacts with the perovskite skeleton to produce a second perovskite layer that conformally covers the texture structure.
[0016] In some possible implementations, the perovskite framework vacuum deposition method includes first forming a perovskite framework by vacuum deposition, and then reacting the perovskite framework with an organic amine to form a second perovskite layer, where the perovskite framework is a mixture formed of two or more of PbX2 and CsY, where X and Y are Cl,- , Br - , I - , SCN - The mixture is preferably a mixture of lead iodide and cesium iodide or a mixture of lead iodide and cesium bromide. The organic amine is one or more of formamidine hydroiodide, methylammonium bromide, and formamidine hydrobromide. The main component of the perovskite framework is preferably a mixture of lead iodide and cesium iodide or a mixture of lead iodide and cesium bromide. When the perovskite framework is vacuum-deposited, lead iodide and cesium iodide, or lead iodide and cesium bromide can be vacuum-deposited together as necessary, thereby adjusting the size of the band gap of the perovskite to obtain a high open circuit voltage.
[0017] In some possible implementations, the concentration of the solution used in the solution method is 0.2 mol / L-3 mol / L. In the process of first vacuum-depositing the perovskite skeleton, and then simultaneously manufacturing the first perovskite layer and the second perovskite layer in a one-step method, if the concentration of the solution used in the solution method is too small, the solvent in the solution used in the solution method will quickly dissolve the lead iodide in the perovskite skeleton during the coating process, and the lead iodide will be blown away from the texture structure, damaging the perovskite skeleton, and may not be able to form a uniform and continuous perovskite thin film. Preferably, if the concentration of the solution used in the solution method is greater than 1 mol / L, the solvent will dissolve the lead iodide in the perovskite slowly during the coating process, and there will be no time to dissolve the lead iodide in the lower layer, thereby ensuring the shape retention of the perovskite thin film in the texture structure.
[0018] In some possible implementations, the perovskite framework vacuum deposition method includes spin-coating an organic amine solution onto the perovskite framework, where the spin-coating speed is 500 rpm to 6000 rpm, and the thickness of the perovskite framework is in the range of 50 nm to 1000 nm.
[0019] In some possible implementations, after forming the perovskite light absorbing layer, the method for manufacturing the perovskite-silicon based stacked solar cell further includes sequentially forming a second carrier transport layer, a transparent conductive layer and an electrode on the perovskite light absorbing layer.
[0020] In a second aspect, the present application further provides a perovskite-silicon based stacked solar cell manufactured by the method for manufacturing a perovskite-silicon based stacked solar cell described above.
[0021] The beneficial effects of the perovskite-silicon based stacked solar cell provided in the second aspect are the same as those of the method for manufacturing the perovskite-silicon based stacked solar cell described in the first aspect or any possible implementation of the first aspect, and detailed description thereof will be omitted here.
[0022] In a third aspect, the present application further provides a perovskite-silicon based stacked solar cell, comprising a silicon based bottom cell having a textured structure, a charge recombination layer and a first carrier transport layer, which are stacked in sequence, and a perovskite light absorbing layer covering the first carrier transport layer having a textured structure, the perovskite light absorbing layer being composed of two perovskite layers, a first perovskite layer and a second perovskite layer, the first perovskite layer being fabricated by a solution process, and the second perovskite layer being fabricated by a perovskite framework vacuum deposition process.
[0023] The beneficial effects of the perovskite-silicon based stacked solar cell provided in the third embodiment are the same as those of the method for producing the perovskite-silicon based stacked solar cell described in the first embodiment, and detailed description thereof will be omitted here.
[0024] In some possible implementations, the first perovskite layer is distributed at least in the valleys of the texture structure of the first carrier transport layer, and the average thickness of the first perovskite layer is 1 / 2 or less of the height of the texture structure. A part of the structure of the second perovskite layer is distributed at least on the slopes and the top of the texture structure, and maintains the same texture shape on the slopes and the top. The perovskite-silicon based stacked solar cell formed based on this has good shape retention on the one hand, and the good light trapping effect and reflection reduction effect of the texture structure are maintained, making it easy to obtain a high short circuit current, and on the other hand, the manufacture of such a perovskite-silicon based stacked solar cell can be achieved more easily than directly forming a conformal perovskite structure, and the solution components can be easily adjusted to obtain the required wide band gap and high open circuit voltage.
[0025] In some possible implementations, the first carrier transport layer has a thickness in the range of 5 nm to 200 nm, and the perovskite light absorbing layer has an average thickness in the range of 100 nm to 3000 nm.
[0026] In some possible implementations, the average thickness of the first perovskite layer is in the range of 100 nm to 300 nm, and the thickness of the second perovskite layer is in the range of 100 nm to 3000 nm.
[0027] The above has outlined the technical solution of the present application. In order to make the technical solution of the present application more clearly understood and implemented according to the contents of the specification, and to make the above and other objectives, features and advantages of the present application more comprehensible, the following particularly sets forth specific embodiments of the present application. [Brief description of the drawings]
[0028] In order to more clearly describe the technical solutions in the embodiments of the present application or related technologies, the following provides a brief description of the drawings used in the description of the embodiments or related technologies. Of course, the drawings described below are part of the embodiments of the present application, and those skilled in the art may conceive of other drawings based on these drawings without any creative effort. [Figure 1] FIG. 1 is a schematic diagram of a perovskite light-absorbing layer produced only by a solution process in the prior art. [Diagram 2] FIG. 1 is a schematic diagram of a perovskite light-absorbing layer produced only by vacuum deposition in the prior art. [Diagram 3] FIG. 2 is a schematic diagram of a first carrier transport layer having a texture structure provided in an embodiment of the present application. [Figure 4] FIG. 1 is a schematic diagram of the preparation of a first perovskite layer by a solution process provided in an embodiment of the present application. [Diagram 5] FIG. 2 is a schematic diagram of the preparation of a second perovskite layer by a vacuum deposition method provided in an embodiment of the present application. [Figure 6] FIG. 2 is a schematic diagram of the preparation of a second perovskite layer by vacuum deposition first provided in an embodiment of the present application. [Figure 7] FIG. 2 is a schematic diagram of the preparation of a first perovskite layer by a solution process provided in an example of the present application. [Figure 8] FIG. 1 is a structural schematic diagram of a perovskite-silicon-based stacked solar cell provided in an embodiment of the present application. [Figure 9] FIG. 2 is a schematic diagram of the texture structure of a perovskite-silicon based stacked solar cell provided in the examples of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] In order to make the objectives, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be described clearly and completely below with reference to the drawings in the embodiments of the present application, and it should be understood that the described embodiments are only a part of the embodiments of the present application, and are not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without any creative efforts are all within the scope of protection of the present application.
[0030] It should be understood that when an element is referred to as being "fixed to" or "mounted on" another element, it may be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or indirectly connected to the other element.
[0031] Additionally, the terms "first" and "second" are used for descriptive purposes only and should not be understood to indicate or imply the relative importance or quantity of the technical features indicated. Thus, a feature qualified as "first" or "second" may indicate or imply the inclusion of one or more of that feature. In the present description, unless expressly and specifically limited, "plurality" means two or more than two. Unless expressly and specifically limited, "some" means one or more than one.
[0032] In the description of this application, orientations or positional relationships indicated by terms such as "upper," "lower," "front," "rear," "left," "right," etc. are orientations or positional relationships indicated based on the drawings, and the purpose thereof is merely to facilitate and simplify the description of this application, and it should be understood that such orientations or positional relationships should not be construed as limiting this application, since they do not expressly or imply that the devices or elements shown necessarily have a specific orientation or are constructed and operated in a specific orientation.
[0033] Organic-inorganic hybrid perovskite solar cells have attracted widespread attention worldwide as a new type of solar cell with high efficiency and low cost. In just a few years, the photoelectric conversion efficiency of perovskite cells has rapidly increased from 3.8% in 2009 to more than 25%, approaching the efficiency of commercialized silicon-based solar cells. Crystalline silicon cells are a highly efficient crystalline silicon photovoltaic cell technology, and their cell efficiency (26.7%) is approaching the theoretical limit efficiency (29.4%). Stacked cell technology is an effective means to break through the efficiency of traditional crystalline silicon photovoltaic cells. As a multi-component cell, the absorption spectrum band gap of perovskite cells can be tuned within the range of 1.5-1.8 eV by component formulation. Perovskite is an ideal stacked top cell material. The crystalline silicon-perovskite stacked battery is a crystalline silicon battery that absorbs solar energy of 800-1200 nanometers as the bottom battery, and a perovskite battery that absorbs solar energy of 300-800 nanometers as the top battery. The middle is connected through a charge recombination layer to form a battery with both ends connected in series. The overall open circuit voltage of the stacked battery is the superposition of the voltages of the top and bottom batteries, and the current of the stacked battery requires good current matching between the upper and lower batteries. The crystalline silicon-perovskite stacked battery is expected to achieve a photoelectric conversion efficiency of more than 30%.
[0034] At present, some literature has reported that crystalline silicon-perovskite stacked cells have achieved conversion efficiencies of more than 25%. A typical perovskite cell fabricates each functional layer in the device by the method of solution spin coating. High-efficiency crystalline silicon cells generally use a double-sided textured light trapping structure to enhance the absorption and utilization of solar light, and further improve the conversion efficiency of the cell. The micro-sized pyramidal textured light trapping structure in crystalline silicon cells is a major challenge for the fabrication of perovskite top cells by solution processing. The difficulty is that the thickness of each functional layer in a perovskite cell is generally several hundred nanometers, and it is difficult to deposit it uniformly and conformally on the micro-sized pyramidal textured surface. The current solution is to polish the crystalline silicon bottom cell to reduce the roughness of the texture, which allows the fabrication of perovskite top cells by solution processing. This method can fabricate perovskite top cells and stacked cells by solution processing, but in addition to sacrificing the improvement of cell efficiency due to the texture structure and its light trapping effect, the polishing process significantly increases the manufacturing cost of the entire battery, making it difficult to reflect the advantages of the efficiency improvement of the stacked cell. The key to achieving high efficiency of the stacked cell is how to leave the texture structure of the bottom cell and directly fabricate the perovskite cell on the bottom cell texture. There are currently two technical solutions to fabricate a perovskite stacked cell on a textured crystalline silicon bottom cell. As shown in Figures 1 and 2, one is to first conformally deposit a lead iodide thin film on the texture, and then spin-coat an organic amine solution to react in situ to produce perovskite. In this method, lead iodide plays the role of anchoring and ensures that the perovskite is conformally deposited with the undulations of the texture. The other is to fabricate a small texture (e.g., a texture of 2 microns size) substrate and directly spin-coat a perovskite solution on the small texture in a one-step method to fabricate a perovskite thin film.In one-step spin coating on small textures, the thickness of the perovskite thin film needs to be adjusted by parameters such as solution concentration and rotation speed so that it can completely cover the pyramid apex of the texture without becoming too thick. Both of the above two solutions have limitations. In the first solution, the deposited lead iodide thin film is dense, so the reactivity of the components is low, and the spin-coated organic amine solution is difficult to penetrate to the bottom and completely react with lead iodide, so it is difficult to ensure that the organic amine reacts uniformly and completely with the lead iodide thin film when spin-coated to form large-sized perovskite crystal particles, and therefore it is difficult to obtain a wide band gap perovskite top cell and a high open circuit voltage by adjusting the components. At present, it has been reported in the literature that the highest conversion efficiency by this method is only 25.4%, and the difficulty lies in the limited nature of the component adjustment. The second solution allows easy adjustment of the components to obtain a wide bandgap and high open circuit voltage, but the thin film formed does not retain its shape, filling the valleys of the texture at the bottom and forming a flat thin film at the top, which loses the reflection reducing properties of the texture, resulting in high reflectivity and low absorption, resulting in low current. Therefore, in order to obtain a stacked battery with both high open circuit voltage and high current, and to obtain a highly efficient crystalline silicon-perovskite stacked battery, it is necessary to develop a method for depositing perovskite thin films in large textured crystalline silicon cells.
[0035] To solve the above technical problems, the embodiments of the present application provide a method for manufacturing a perovskite-silicon based stacked solar cell.
[0036] As shown in FIGS. 3 to 8, the method for fabricating a perovskite-silicon based stacked solar cell provided in the present application includes the following steps:
[0037] A substrate is provided that includes a silicon-based bottom cell having a textured structure, a charge recombination layer 107, and a first carrier transport layer 108, which are stacked in sequence.
[0038] First, prepare a silicon-based battery. Take an n-type silicon-based bottom battery as an example, and its manufacturing method may be as follows:
[0039] An n-type crystalline silicon wafer 101 is prepared. In practical applications, the n-type crystalline silicon wafer 101 can be a commercial grade silicon wafer having a resistivity of 1 Ω.cm to 10 Ω.cm and a thickness of 50 μm to 300 μm.
[0040] The n-type crystalline silicon wafer 101 undergoes sequential texturing and cleaning processes to form a textured n-type crystalline silicon wafer 101. The n-type crystalline silicon wafer 101 converts photons into photo-generated carriers (electron-hole pairs) as the light absorbing layer of the silicon-based bottom cell.
[0041] An intrinsic amorphous silicon passivation layer is deposited on both sides of the n-type crystalline silicon wafer 101 to form a first passivation layer 102 located on the front side of the n-type crystalline silicon wafer 101 and a second passivation layer 103 located on the back side of the n-type crystalline silicon wafer 101. The first passivation layer 102 and the second passivation layer 103 mainly serve to passivate the dangling bonds on the surface of the n-type crystalline silicon wafer 101.
[0042] In practical applications, the intrinsic amorphous silicon passivation layer can be fabricated by processes such as plasma enhanced chemical vapor deposition (PECVD), hot filament chemical vapor deposition, catalytic chemical vapor deposition, etc. The thicknesses of the first passivation layer 102 and the second passivation layer 103 can both be 1 nm to 20 nm.
[0043] A phosphorus-doped n-type amorphous / microcrystalline silicon layer 104 is deposited on the first passivation layer 102 to form a front emitter. In practical applications, the n-type amorphous / microcrystalline silicon layer 104 can be manufactured by processes such as PECVD, hot filament chemical vapor deposition, catalytic chemical vapor deposition, etc. The thickness of the n-type amorphous / microcrystalline silicon layer 104 may be 1 nm to 30 nm.
[0044] A boron-doped p-type amorphous / microcrystalline silicon layer 105 is deposited on the second passivation layer 103 to form a back-surface field structure. In practical applications, the p-type amorphous / microcrystalline silicon layer 105 can be fabricated by processes such as PECVD, hot filament chemical vapor deposition, catalytic chemical vapor deposition, etc. The thickness of the p-type amorphous / microcrystalline silicon layer 105 may be 1 nm to 30 nm.
[0045] A first transparent conductive layer 106 is formed on the p-type amorphous / microcrystalline silicon layer 105. The first transparent conductive layer 106 mainly plays a role of collecting photo-generated carriers and transporting the photo-generated carriers to the back metal electrode 113. Specifically, the material of the first transparent conductive layer 106 may be one or more of, but not limited to, indium tin oxide (ITO), tungsten-doped indium oxide (In2O3:W, abbreviated as IWO), indium zinc oxide (IZO), and titanium-doped indium oxide thin film (ITiO).
[0046] In practical applications, a magnetron sputtering process can be used to fabricate the first transparent conductive layer 106. The thickness of the first transparent conductive layer 106 may be 30 nm to 120 nm.
[0047] The above process steps produce a silicon-based bottom cell. Because the crystalline silicon substrate has a textured structure, the functional layers formed on the crystalline silicon substrate, including the first passivation layer 102, the second passivation layer 103, the n-type amorphous / microcrystalline silicon layer 104, the p-type amorphous / microcrystalline silicon layer 105, and the first transparent conductive layer 106, also have textured structures.
[0048] A charge recombination layer 107 is deposited on the n-type amorphous / microcrystalline silicon layer 104 to realize tunnel recombination collection of photo-generated carriers. The charge recombination layer 107 may be a charge recombination layer 107 made of transparent metal oxides such as tin-doped indium oxide (ITO), zinc-doped indium oxide (IZO), tungsten-doped indium oxide (IWO), titanium-doped indium oxide (ITiO), fluorine-doped tin oxide (FTO), aluminum-doped zinc oxide (AZO), etc. In practical applications, the charge recombination layer 107 can be manufactured using a magnetron sputtering process.
[0049] Of course, the charge recombination layer 107 may be a charge recombination layer 107 made of highly doped silicon, opposite to the PN junction of the bottom cell. For example, in the charge recombination layer 107 mainly composed of an n-type doped microcrystalline silicon layer 1070 and a p-type doped microcrystalline silicon layer 1071, the p-type doped microcrystalline silicon layer 1071 is adjacent to the perovskite cell described later, and the n-type doped microcrystalline silicon layer 1070 is adjacent to the silicon-based bottom cell. Specifically, the n-type doped microcrystalline silicon layer 1070 may be a phosphorus doped microcrystalline silicon layer, and the p-type doped microcrystalline silicon layer 1071 may be a boron doped microcrystalline silicon layer. In practical applications, the charge recombination layer 107 may be manufactured using processes such as PECVD, hot filament chemical vapor deposition, and catalytic chemical vapor deposition. The thickness of each of the n-type doped microcrystalline silicon layer 1070 and the p-type doped microcrystalline silicon layer 1071 may be 1 nm to 30 nm.
[0050] Forming the perovskite cell on the charge recombination layer 107 specifically includes the following steps:
[0051] A first carrier transport layer 108 is formed on the charge recombination layer 107 to realize vertical transport of the photogenerated carriers. The material of the first carrier transport layer 108 may be, but is not limited to, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), 2,2',7,7'-tetrakis-(dimethoxydiphenylamine)-spirofluorene (Spiro-OMeTAD), 2,2',7,7'-tetrakis(di-p-tolylamino)spiro-9,9'-difluorene (Spiro-TTB), or nickel oxide (NiO).
[0052] In practical applications, the first carrier transport layer 108 can be fabricated using processes such as magnetron sputtering, laser pulse deposition, thermal evaporation coating, chemical vapor deposition, solution coating, gel-sol or hydrothermal nanoparticle synthesis, etc. The thickness range of the first carrier transport layer 108 may be from 5 nm to 200 nm.
[0053] A perovskite light absorbing layer 109 is formed on the first carrier transport layer 108. The components of the perovskite light absorbing layer 109 are a combination of one or more perovskite structure materials. The chemical formula of the perovskite material may be ABX3, where A is one or more of CH3NH3 cation, C4H9NH3 cation, NH2=CHNH2 cation, and Cs cation; B is Pb 2+ , Sn 2+ and X is one or a combination of two of the following: - , Cl - , Br - One or more of the following:
[0054] As shown in Figures 3 to 7, the manufacture of the perovskite light-absorbing layer 109 includes the following steps.
[0055] A perovskite light absorbing layer 109 consisting of two perovskite layers, a first perovskite layer 1090 and a second perovskite layer 1091, is formed on a first carrier transport layer 108 having a textured structure. The first perovskite layer 1090 is manufactured by a solution process. The second perovskite layer 1091 is manufactured by a perovskite framework vacuum deposition process.
[0056] At this time, the first perovskite layer 1090 and the second perovskite layer 1091 formed by the two-step method on the first carrier transport layer 108 having a texture structure constitute the perovskite light absorbing layer 109, where the first perovskite layer 1090 is manufactured by a solution method, and the second perovskite layer 1091 is manufactured by a perovskite skeleton vacuum deposition method. The perovskite skeleton vacuum deposition method here involves first forming a mixture of PbX2 and CsY by vacuum deposition to form a perovskite skeleton, where X and Y are chlorine ions (Cl - ), bromide ion (Br - ), iodine ion (I - ) and thiocyanate ion (SCN -), and the mixture of the two may be a mixture of two or more materials, preferably a mixture of lead iodide and cesium iodide or a mixture of lead iodide and cesium bromide. Then, using a conventional solution coating method such as solution spin coating, knife coating, spraying, etc., the perovskite skeleton is covered with an organic amine solution and reacted to form a perovskite thin film. The formed second perovskite layer 1091 can conformally cover the peaks and slopes of the texture structure, and the first perovskite layer 1090 formed by the solution method can be deposited on the bottom of the texture structure to partially fill it. On this basis, the perovskite light absorbing layer 109 consisting of the above two perovskite layers combines the advantages of both the solution method and the perovskite skeleton vacuum deposition method, while avoiding the disadvantages of the two methods. Not only was the good light trapping effect and reflection reduction effect of the textured structure effectively maintained to obtain a high short circuit current, but the solution components could also be easily adjusted to obtain the required wide band gap and high open circuit voltage. This shows that, compared with the prior art, the manufacturing method of the perovskite-silicon based stacked solar cell provided in the present application effectively balances the tradeoff between maintaining the shape of the textured structure and adjusting the perovskite components, and greatly expands the process control window and the range of components and materials to be selected for the manufacture of highly efficient stacked cells.
[0057] In addition, when the average vertical distance from the bottom to the top of the texture structure of the first carrier transport layer 108 is L, the average thickness of the first perovskite layer 1090 manufactured by the solution method is greater than 0 and less than 1 / 2L. At this time, the first perovskite layer 1090 manufactured by the solution method is deposited at the bottom of the texture structure of the first carrier transport layer 108, and the thickness is less than half the height of the texture structure. Based on this, the formed perovskite light absorbing layer 109 can maintain good texture characteristics, that is, when the perovskite light absorbing layer 109 is irradiated with light, the texture structure can improve the photoelectric conversion efficiency due to the light trapping effect and the reflection reduction effect. When the thickness of the first perovskite layer 1090 manufactured by the solution method is greater than half the height of the texture structure, the texture structure of the formed perovskite light absorbing layer 109 has a small height, a high light reflectance, and a low photoelectric conversion efficiency. The thickness of the first perovskite layer 1090 produced by the solution process is defined as the height of the solution deposited on the textured structure in the vertical direction from the contact point with the textured structure to the highest point of deposition of the solution, and the average thickness of the first perovskite layer 1090 is therefore the average value of these heights.
[0058] As shown in Figures 3, 4 and 5, in some possible implementations, the perovskite light absorbing layer 109 can be manufactured by a two-step method of a solution method followed by a perovskite skeleton vacuum deposition method. Specifically, the step of forming the perovskite light absorbing layer 109 consisting of two perovskite layers, the first perovskite layer 1090 and the second perovskite layer 1091, on the first carrier transport layer 108 having a textured structure includes a step of manufacturing the first perovskite layer 1090 on the first carrier transport layer 108 having a textured structure by a solution method, and then a step of manufacturing the second perovskite layer 1091 by a perovskite skeleton vacuum deposition method. Based on this, the first perovskite layer 1090 is first formed on the first carrier transport layer 108 having a textured structure by a solution method, and then the second perovskite layer 1091 is formed on the first perovskite layer 1090 by a perovskite skeleton vacuum deposition method. On this basis, the first perovskite layer 1090 produced by the solution method is deposited on the bottom of the textured structure of the first carrier transport layer 108, and the band gap of the perovskite can be adjusted by changing the composition of the perovskite solution. The second perovskite layer 1091 produced by the perovskite skeleton vacuum deposition method conformally covers the first perovskite layer 1090 and the textured structure that is not completely filled, thereby maintaining the textured structure to obtain good light trapping effect and reflection reduction properties, while ensuring that the textured structure is covered and avoiding short circuit caused by the electrode 113 directly contacting the textured structure. The stacked battery produced by this method combines the advantages of the traditional stacked battery solutions, avoids the shortcomings faced by the prior art, and effectively balances the contradiction between maintaining the shape of the textured structure and adjusting the solution composition.
[0059] 9 is an exemplary diagram of the texture structure of the perovskite-silicon-based stacked solar cell provided in the present embodiment. As shown in FIG. 9, in the pyramidal structure of the texture structure, the second perovskite layer 1091 produced by the perovskite skeleton vacuum deposition method is stepped.
[0060] As shown in Figures 3, 6 and 7, in some possible implementations, the perovskite light absorbing layer 109 can be manufactured by a two-step method of a perovskite skeleton vacuum deposition method followed by a solution method. Specifically, the step of forming the perovskite light absorbing layer 109 consisting of two perovskite layers, the first perovskite layer 1090 and the second perovskite layer 1091, on the first carrier transport layer 108 having a textured structure includes the steps of manufacturing the second perovskite layer 1091 on the first carrier transport layer 108 having a textured structure by a perovskite skeleton vacuum deposition method, and then manufacturing the first perovskite layer 1090 by a solution method. Based on this, a second perovskite layer 1091 is first formed on the first carrier transport layer 108 having a textured structure by a perovskite skeleton vacuum deposition method, and then a first perovskite layer 1090 is formed on the second perovskite layer 1091 by a solution method. Based on this, the second perovskite layer 1091 manufactured by the perovskite skeleton vacuum deposition method is conformally bonded to the textured structure of the first carrier transport layer 108, and the textured structure is maintained to obtain good light trapping effect and reflection reduction characteristics. The first perovskite layer 1090 manufactured by the solution method is deposited at the bottom of the textured structure, which is advantageous for obtaining a high open circuit voltage.
[0061] In some possible implementations, in the method of first manufacturing the second perovskite layer 1091 by a perovskite skeleton vacuum deposition method and then manufacturing the first perovskite layer 1090 by a solution method, the perovskite skeleton may be first vacuum-deposited, and then the first perovskite layer 1090 and the second perovskite layer 1091 may be simultaneously manufactured by a one-step method. Specifically, the step of forming the perovskite light absorbing layer 109 consisting of two perovskite layers, the first perovskite layer 1090 and the second perovskite layer 1091, on the first carrier transport layer 108 having a textured structure includes the step of depositing the perovskite skeleton by a vacuum deposition method on the first carrier transport layer 108 having a textured structure, and then manufacturing the first perovskite layer 1090 by a solution method. Here, the solution used in the solution method contains an excess of an organic amine. In the process of forming the first perovskite layer 1090, the material in the perovskite skeleton is reacted with an organic amine to form a second perovskite layer 1091. On this basis, when the solution used in the solution process is applied to the perovskite skeleton, the excess organic amine contained in the solution reacts with the perovskite skeleton to generate a second perovskite layer 1091. The generated second perovskite layer 1091 conformally covers the textured structure. The first perovskite layer 1090 manufactured by the solution process is deposited and partially filled at the bottom of the textured structure covered by the second perovskite layer 1091, forming the perovskite light absorbing layer 109.
[0062] In some instances, the solute of the solution used in the solution process is Cs or a mixed perovskite component containing FA or MA, Cs x FA y MA z PbBr m I n(x+y+z=1, m+n=3), and the solvent is one or more of N,N-dimethylformamide (DMF) and dimethylsulfoxide (DMSO). In the method of first vacuum-depositing a perovskite skeleton and then simultaneously manufacturing the first perovskite layer 1090 and the second perovskite layer 1091 in a one-step process, the solution used not only contains lead iodide and a mixture of formamidine hydroiodide, methylammonium bromide, and formamidine hydrobromide that satisfy the above-mentioned blend ratio, but also contains an organic amine component that exceeds the stoichiometric ratio. The excess organic amine component reacts with the perovskite skeleton to produce the second perovskite layer 1091 that conformally covers the texture structure.
[0063] In some examples, the perovskite framework vacuum deposition method includes first forming a perovskite framework by vacuum deposition, and then reacting the perovskite framework with an organic amine to form a second perovskite layer 1091. Here, the perovskite framework is a mixture formed of two or more of PbX2 and CsY. X and Y are chlorine ions (Cl - ), bromide ion (Br - ), iodine ion (I - ) and thiocyanate ion (SCN - ), respectively. The mixture is preferably a mixture of lead iodide and cesium iodide or a mixture of lead iodide and cesium bromide. The organic amine is one or more of formamidine hydroiodide, methylammonium bromide, and formamidine hydrobromide. The main component of the perovskite framework is preferably a mixture of lead iodide (PbI2) and cesium iodide (CsI), or a mixture of lead iodide (PbI2) and cesium bromide (CsBr). When the perovskite framework is vacuum-deposited, lead iodide and cesium iodide, or lead iodide and cesium bromide, can be vacuum-deposited together as necessary, thereby adjusting the size of the band gap of the perovskite to obtain a high open circuit voltage.
[0064] In practical applications, the thickness of the perovskite framework ranges from 50 nm to 1000 nm.
[0065] In practical application, the organic amine solution can be applied to the perovskite skeleton, followed by annealing and drying for 5-30 minutes at a temperature of 100°C-200°C to form the second perovskite layer 1091. When the perovskite skeleton is a mixture of lead iodide (PbI2) and cesium bromide (CsBr), the evaporation rate of lead iodide can be 0.1 Å / s-10 Å / s and the evaporation rate of cesium bromide can be 0.05 Å / s-0.2 Å / s during the vacuum deposition process. When the organic amine solution is a mixture of formamidine hydroiodide (FAI) and formamidine hydrobromide (FABr), the solvent can be selected from ethanol or isopropyl alcohol.
[0066] In some examples, the concentration of the solution used in the solution method is 0.2 mol / L to 3 mol / L. In the process of first vacuum-depositing the perovskite skeleton, and then simultaneously manufacturing the first perovskite layer 1090 and the second perovskite layer 1091 by a one-step method, if the concentration of the solution used in the solution method is too low, the solvent in the solution used in the solution method will quickly dissolve the lead iodide in the perovskite skeleton during the coating process, and the lead iodide will be blown away from the texture structure, damaging the perovskite skeleton, and it may not be possible to form a uniform and continuous perovskite thin film. Preferably, if the concentration of the solution used in the solution method is greater than 1 mol / L, the solvent will dissolve the lead iodide in the perovskite slowly during the coating process, and there will be insufficient time to dissolve the lead iodide in the lower layer, thereby ensuring the shape retention of the perovskite thin film in the texture structure. In the method of first vacuum-depositing a perovskite skeleton and then simultaneously producing the first perovskite layer 1090 and the second perovskite layer 1091 in a one-step process, the concentration of the solution used is 0.1 mol / L to 3 mol / L.
[0067] In practical applications, the solution used in the solution method is Cs 0.05 FA 0.8 MA 0.15 PbBr 0.6 I2.4 Alternatively, the solution may be a N,N-dimethylformamide (DMF) / dimethylsulfoxide (DMSO) (4:1) solution of the above. In the process of producing the first perovskite layer 1090 by the solution method, after applying the solution onto the first carrier transport layer 108 having a textured structure by the solution method, the solution is first surface-dried by a method such as poor solvent or air knife blowing, and then annealing and drying treatment are performed at a temperature of 70°C to 190°C for 5 min to 60 min to form the first perovskite layer 1090. The average thickness of the first perovskite layer 1090 is in the range of 100 nm to 300 nm.
[0068] In practical applications, first, the perovskite framework is vacuum-deposited, and then the first perovskite layer 1090 and the second perovskite layer 1091 are simultaneously fabricated in a one-step process. When the perovskite framework is a mixture of lead iodide (PbI2) and cesium bromide (CsBr), the solution used in the solution process is a mixture of the perovskite component (Cs 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 ), excess formamidine hydroiodide (FAI), and formamidine hydrobromide (FABr) in DMF / DMSO (4:1), where the concentration ranges of FAI and FABr may be 0.1 mol / L to 3 mol / L. In the process of manufacturing the second perovskite layer 1091 by the perovskite skeleton vacuum deposition method, the solution is spin-coated on the perovskite skeleton, and then extracted with a poor solvent (such as anisole), and then annealed at a temperature of 100°C to 200°C for 5 min to 30 min, finally forming the perovskite light absorbing layer 109.
[0069] In some examples, the perovskite framework vacuum deposition method includes spin-coating an organic amine solution onto the perovskite framework, where the spin-coating speed is 500 rpm to 6000 rpm, and the thickness of the perovskite framework is in the range of 50 nm to 1000 nm.
[0070] In practical applications, the thickness of the second perovskite layer 1091 ranges from 100 nm to 3000 nm. Since the perovskite light absorbing layer 109 is composed of one first perovskite layer 1090 manufactured by a solution method and one second perovskite layer 1091 manufactured by a perovskite skeleton vacuum deposition method, the vertical distance from the contact point with the upper part of the texture structure of the first carrier transport layer 108 to the highest point covered by the perovskite light absorbing layer 109 is defined as the thickness of the perovskite light absorbing layer 109. The average thickness of the perovskite light absorbing layer 109 ranges from 100 nm to 3000 nm.
[0071] As shown in FIG. 8, a second carrier transport layer 111 is formed on the perovskite light absorbing layer 109 to realize vertical transport of photogenerated carriers. The material of the second carrier transport layer 111 is C 60 The catalyst may be, but is not limited to, one or more of: [6,6]-phenyl-C61-butyric acid methyl ester (PCBM), tin dioxide (SnO2), titanium dioxide (TiO2).
[0072] In practical applications, a LiF, C layer is first deposited on the perovskite light absorbing layer 109 as the second carrier transport interface layer 110 using a vacuum deposition process. 60 The thin film layer or PCBM thin film layer can be manufactured, and then the second carrier transport layer 111 made of SnO2 or TiO2 can be manufactured using atomic layer deposition (ALD), chemical vapor deposition, physical vapor deposition, solution coating, etc. The thickness of the second carrier transport layer 111 can be 1 nm to 30 nm. It can be understood that in practical applications, the second carrier transport interface layer 110 can be omitted.
[0073] When the second carrier transport interface layer 110 includes a second carrier transport interface layer 1100 and a second carrier transport interface layer 2101, the second carrier transport interface layer 1100 can be vacuum deposited LiF, and the second carrier transport interface layer 2101 can be vacuum deposited C 60 The thickness of LiF may be in the range of 0.1 nm to 10 nm, and C 60The thickness range is 1 nm to 20 nm.
[0074] 8, a second transparent conductive layer 112 is formed on a second carrier transport layer 111 to achieve the purpose of lateral transport of electrons to an electrode 113 and reducing light reflection. The thickness of the second transparent conductive layer 112 is in the range of 30 nm to 200 nm. The material and manufacturing method of the second transparent conductive layer 112 may refer to the first transparent conductive layer 106, and will not be described in detail here.
[0075] An electrode 113 is formed on the first transparent conductive layer 106 and the second transparent conductive layer 112 to collect current. In practical applications, the thin gate line and main gate line of the electrode 113 can be manufactured by screen printing or mask deposition. The material of the electrode 113 can be a metal with good conductivity such as silver, copper, aluminum, etc. The thickness of the electrode 113 is in the range of 100 nm to 500 nm.
[0076] The manufacturing method of the perovskite-silicon-based stacked solar cell described in the embodiment of the present application is not limited to n-type silicon wafers, but can also be applied to p-type crystalline silicon cells, TOPCON cells, polycrystalline silicon cells, ingot single crystal silicon cells, and other perovskite cells integrated with the perovskite stacked cells, and can also be applied to other types of perovskite stacked cells, including copper indium gallium selenium-perovskite stacked cells, perovskite-perovskite stacked cells, gallium arsenide-perovskite stacked cells, organic photovoltaic-perovskite stacked cells, etc., and has good versatility and compatibility. In the manufacturing method of the perovskite-silicon-based stacked solar cell described above, the first carrier is a hole and the second carrier is an electron, so that the manufactured first carrier transport layer 108 is a hole transport layer and the manufactured second carrier transport layer 111 is an electron transport layer. The manufacturing method of the perovskite-silicon based stacked solar cell provided in the embodiments of the present application is not limited to the inverted perovskite top cell structure with a hole transport layer as a substrate, but can also be applied to the normal perovskite top cell structure with an electron transport layer as a substrate, that is, the functional layers of the cell structure can be, from bottom to top, a textured silicon based cell, a tunnel junction or metal oxide composite layer, an electron transport layer, a first perovskite layer and a second perovskite layer, a hole transport layer, a buffer layer, a metal oxide transparent electrode, and an electrode.
[0077] As shown in Figure 8, an embodiment of the present application further provides a perovskite-silicon based stacked solar cell, which is obtained by the manufacturing method of the perovskite-silicon based stacked solar cell described above.
[0078] The beneficial effects of the perovskite-silicon based stacked solar cell provided in the examples of the present application are the same as the beneficial effects of the manufacturing method of the perovskite-silicon based stacked solar cell described above.
[0079] An embodiment of the present application further provides a perovskite-silicon based stacked solar cell, which includes a silicon based bottom cell having a textured structure, a charge recombination layer and a first carrier transport layer, which are sequentially stacked, and a perovskite light absorbing layer covering the first carrier transport layer having a textured structure, wherein the perovskite light absorbing layer is composed of two perovskite layers, a first perovskite layer and a second perovskite layer, where the first perovskite layer is prepared by a solution process and the second perovskite layer is prepared by a perovskite framework vacuum deposition process.
[0080] In some possible implementations, the first perovskite layer is distributed at least in the valleys of the texture structure of the first carrier transport layer, and the average thickness of the first perovskite layer is 1 / 2 or less of the height of the texture structure. A part of the structure of the second perovskite layer is distributed at least on the slopes and the top of the texture structure, and maintains the same texture shape on the slopes and the top. The perovskite-silicon based stacked solar cell formed based on this has good shape retention on the one hand, and the good light trapping effect and reflection reduction effect of the texture structure are maintained, making it easy to obtain a high short circuit current, and on the other hand, the manufacture of such a perovskite-silicon based stacked solar cell can be achieved more easily than directly forming a conformal perovskite structure, and the solution components can be easily adjusted to obtain the required wide band gap and high open circuit voltage.
[0081] In addition, the layer distributed in the valleys of the textured structure of the first carrier transport layer may be referred to as a second perovskite layer, and the layer distributed on the slopes and top of the textured structure may be referred to as a first perovskite layer.
[0082] In some possible implementations, the thickness of the first carrier transport layer is in the range of 5 nm to 200 nm. The average thickness of the perovskite light absorbing layer is in the range of 100 nm to 3000 nm. The thickness of the second carrier transport layer is in the range of 1 nm to 30 nm.
[0083] In some possible implementations, the average thickness of the first perovskite layer is in the range of 100 nm to 300 nm, and the thickness of the second perovskite layer is in the range of 100 nm to 3000 nm.
[0084] In order to demonstrate the performance of the perovskite-silicon based stacked solar cell manufactured by the manufacturing method of the perovskite-silicon based stacked solar cell provided in the examples of the present application, the following will compare the examples with comparative examples.
[0085] Example 1 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0086] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0087] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0088] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0089] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0090] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0091] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0092] In the seventh step, a hole transport layer (thickness 15 nm) of spiro-TTB material is fabricated on the tunnel recombination layer using a vacuum deposition process, and the evaporation rate is 0.2 Å / s.
[0093] In the eighth step, a perovskite component (Cs) with a concentration of 1.2 mol / L was deposited on the textured hole transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 A DMF / DMSO (4:1) solution of the above was spin-coated at a spin-coating speed of 2000 rpm, and after extraction treatment with anisole, the material was annealed at 100° C. for 20 min to form a first perovskite layer (average thickness 200 nm).
[0094] In the ninth step, a vacuum deposition process is used to form lead iodide and cesium bromide on the first perovskite layer, where the rate of cesium bromide (CsBr) is 0.1 Å / s and the rate of lead iodide (PbI2) is 2 Å / s, with a total thickness of 400 nm.
[0095] A mixed solution of FAI and FABr is prepared, the molar concentration ratio of FAI to FABr is 3:1, and the solvent is ethanol or isopropyl alcohol. 80 μL of the mixed solution of FAI and FABr is spin-coated on the lead iodide and cesium bromide layers and reacted to form a second perovskite layer (thickness 550 nm).
[0096] The second perovskite layer is annealed at a temperature of 150° C. for 20 min to form a perovskite light absorbing layer (average thickness 550 nm).
[0097] In the tenth step, a thin layer of LiF (1 nm thick) and C were deposited on the perovskite light absorbing layer using a vacuum deposition process. 60 A thin film layer (10 nm thick) is then fabricated, followed by an electron transport interface layer (11 nm thick).
[0098] In the 11th step, an electron transport layer (thickness 10 nm) made of SnO2 material is fabricated using the atomic layer deposition process (ALD).
[0099] In a twelfth step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the electron transport layer using a magnetron sputtering process.
[0100] In a thirteenth step, a silver electrode is formed on the first transparent conductive layer and the second transparent conductive layer using a screen printing process.
[0101] Example 2 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0102] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0103] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0104] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0105] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0106] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0107] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0108] In the seventh step, a hole transport layer (thickness 15 nm) of spiro-TTB material is fabricated on the tunnel recombination layer using a vacuum deposition process, and the evaporation rate is 0.2 Å / s.
[0109] In the eighth step, a perovskite component (Cs) with a concentration of 0.2 mol / L was deposited on the textured hole transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 A DMF / DMSO (4:1) solution of the compound was spin-coated at a spin-coating speed of 500 rpm, and after extraction with anisole, the material was annealed at 70° C. for 60 min to form a first perovskite layer (average thickness 100 nm).
[0110] In the ninth step, a vacuum deposition process is used to form lead iodide and cesium bromide on the first perovskite layer, where the rate of cesium bromide (CsBr) is 0.05 Å / s and the rate of lead iodide (PbI2) is 0.1 Å / s, with a total thickness of 50 nm.
[0111] A mixed solution of FAI and FABr is prepared, the molar concentration ratio of FAI to FABr is 3:1, and the solvent is ethanol or isopropyl alcohol. 70 μL of the mixed solution of FAI and FABr is spin-coated on the lead iodide and cesium bromide layers and reacted to form a second perovskite layer (thickness 100 nm).
[0112] The second perovskite layer is annealed at a temperature of 100° C. for 30 min to form a perovskite light absorbing layer (average thickness 100 nm).
[0113] In the tenth step, a thin layer of LiF (1 nm thick) and C were deposited on the perovskite light absorbing layer using a vacuum deposition process. 60 A thin film layer (10 nm thick) is then fabricated, followed by an electron transport interface layer (11 nm thick).
[0114] In the 11th step, an electron transport layer (thickness 10 nm) made of SnO2 material is fabricated using the atomic layer deposition process (ALD).
[0115] In a twelfth step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the electron transport layer using a magnetron sputtering process.
[0116] In a thirteenth step, a silver electrode is formed on the first transparent conductive layer and the second transparent conductive layer using a screen printing process.
[0117] Example 3 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0118] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0119] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0120] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0121] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0122] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0123] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0124] In the seventh step, a hole transport layer (thickness 15 nm) of spiro-TTB material is fabricated on the tunnel recombination layer using a vacuum deposition process, and the evaporation rate is 0.2 Å / s.
[0125] In the eighth step, a perovskite component (Cs) with a concentration of 3 mol / L was deposited on the textured hole transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 A DMF / DMSO (4:1) solution of the compound was spin-coated at a spin-coating speed of 6000 rpm, and after extraction with anisole, the material was annealed at 190° C. for 5 min to form a first perovskite layer (average thickness 300 nm).
[0126] In the ninth step, a vacuum deposition process is used to form lead iodide and cesium bromide on the first perovskite layer, where the rate of cesium bromide (CsBr) is 0.2 Å / s, the rate of lead iodide (PbI2) is 10 Å / s, and the total thickness is 1000 nm.
[0127] A mixed solution of FAI and FABr is prepared, the molar concentration ratio of FAI to FABr is 3:1, and the solvent is ethanol or isopropyl alcohol. 90 μL of the mixed solution of FAI and FABr is spin-coated on the lead iodide and cesium bromide layers and reacted to form a second perovskite layer (thickness 3000 nm).
[0128] The second perovskite layer is annealed at a temperature of 200° C. for 5 min to form a perovskite light absorbing layer (average thickness 3000 nm).
[0129] In the tenth step, a thin layer of LiF (1 nm thick) and C were deposited on the perovskite light absorbing layer using a vacuum deposition process. 60 A thin film layer (10 nm thick) is then fabricated, followed by an electron transport interface layer (11 nm thick).
[0130] In the 11th step, an electron transport layer (thickness 10 nm) made of SnO2 material is fabricated using the atomic layer deposition process (ALD).
[0131] In a twelfth step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the electron transport layer using a magnetron sputtering process.
[0132] In a thirteenth step, a silver electrode is formed on the first transparent conductive layer and the second transparent conductive layer using a screen printing process.
[0133] Example 4 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0134] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0135] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0136] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0137] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0138] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0139] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0140] In the seventh step, a hole transport layer (thickness 15 nm) of spiro-TTB material is fabricated on the tunnel recombination layer using a vacuum deposition process, and the evaporation rate is 0.2 Å / s.
[0141] In the eighth step, lead iodide and cesium bromide are formed on the hole transport layer using a vacuum deposition process, where the rate of cesium bromide (CsBr) is 0.1 Å / s, the rate of lead iodide (PbI2) is 2 Å / s, and the total thickness is 400 nm.
[0142] In the ninth step, a perovskite component (Cs) was deposited on the textured hole transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 ), and a DMF / DMSO (4:1) solution of FAI and FABr was spin-coated, where the concentrations of the perovskite components were 1.2 mol / L, the FAI concentration was 0.5 mol / L, and the FABr concentration was 0.1 mol / L. The spin-coating speed was 2000 rpm, and after extraction treatment with anisole, the layer was annealed at 120°C for 20 min to form a perovskite light-absorbing layer (average thickness 550 nm).
[0143] In the tenth step, a thin layer of LiF (1 nm thick) and C were deposited on the perovskite light absorbing layer using a vacuum deposition process. 60 A thin film layer (10 nm thick) is then fabricated, followed by an electron transport interface layer (11 nm thick).
[0144] In the 11th step, an electron transport layer (thickness 10 nm) made of SnO2 material is fabricated using the atomic layer deposition process (ALD).
[0145] In a twelfth step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the electron transport layer using a magnetron sputtering process.
[0146] In a thirteenth step, a silver electrode is formed on the first transparent conductive layer and the second transparent conductive layer using a screen printing process.
[0147] Example 5 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0148] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0149] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0150] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0151] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0152] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0153] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0154] In the seventh step, a hole transport layer (thickness 15 nm) of spiro-TTB material is fabricated on the tunnel recombination layer using a vacuum deposition process, and the evaporation rate is 0.2 Å / s.
[0155] In the eighth step, lead iodide and cesium bromide are formed on the hole transport layer using a vacuum deposition process, where the rate of cesium bromide (CsBr) is 0.05 Å / s, the rate of lead iodide (PbI2) is 0.1 Å / s, and the total thickness is 50 nm.
[0156] In the ninth step, a perovskite component (Cs) was deposited on the textured hole transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 ), and a DMF / DMSO (4:1) solution of FAI and FABr was spin-coated, where the concentrations of the perovskite components were 0.1 mol / L, the FAI concentration was 0.1 mol / L, and the FABr concentration was 0.5 mol / L. The spin-coating speed was 500 rpm, and after extraction treatment with anisole, the material was annealed at 100°C for 30 min to form a perovskite light-absorbing layer (average thickness 100 nm).
[0157] In the tenth step, a thin layer of LiF (1 nm thick) and C were deposited on the perovskite light absorbing layer using a vacuum deposition process. 60 A thin film layer (10 nm thick) is then fabricated, followed by an electron transport interface layer (11 nm thick).
[0158] In the 11th step, an electron transport layer (thickness 10 nm) made of SnO2 material is fabricated using the atomic layer deposition process (ALD).
[0159] In a twelfth step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the electron transport layer using a magnetron sputtering process.
[0160] In a thirteenth step, a silver electrode is formed on the first transparent conductive layer and the second transparent conductive layer using a screen printing process.
[0161] Example 6 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0162] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0163] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0164] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0165] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0166] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0167] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0168] In the seventh step, a hole transport layer (thickness 15 nm) of spiro-TTB material is fabricated on the tunnel recombination layer using a vacuum deposition process, and the evaporation rate is 0.2 Å / s.
[0169] In the eighth step, lead iodide and cesium bromide are formed on the hole transport layer using a vacuum deposition process, where the rate of cesium bromide (CsBr) is 0.2 Å / s, the rate of lead iodide (PbI2) is 10 Å / s, and the total thickness is 1000 nm.
[0170] In the ninth step, a perovskite component (Cs) was deposited on the textured hole transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 ), and a DMF / DMSO (4:1) solution of FAI and FABr was spin-coated, where the concentrations of the perovskite components were 3 mol / L, the FAI concentration was 3 mol / L, and the FABr concentration was 3 mol / L. The spin-coating speed was 6000 rpm, and after extraction treatment with anisole, the layer was annealed at 200°C for 5 min to form a perovskite light-absorbing layer (average thickness 3000 nm).
[0171] In the tenth step, a thin layer of LiF (1 nm thick) and C were deposited on the perovskite light absorbing layer using a vacuum deposition process. 60A thin film layer (10 nm thick) is then fabricated, followed by an electron transport interface layer (11 nm thick).
[0172] In the 11th step, an electron transport layer (thickness 10 nm) made of SnO2 material is fabricated using the atomic layer deposition process (ALD).
[0173] In a twelfth step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the electron transport layer using a magnetron sputtering process.
[0174] In a thirteenth step, a silver electrode is formed on the first transparent conductive layer and the second transparent conductive layer using a screen printing process.
[0175] Example 7 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0176] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0177] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0178] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0179] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus.19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0180] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0181] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0182] In the seventh step, a hole transport layer (thickness 15 nm) of spiro-TTB material is fabricated on the tunnel recombination layer using a vacuum deposition process, and the evaporation rate is 0.2 Å / s.
[0183] In the eighth step, lead iodide and cesium bromide are formed on the hole transport layer using a vacuum deposition process, where the rate of cesium bromide (CsBr) is 0.05 Å / s, the rate of lead iodide (PbI2) is 0.1 Å / s, and the total thickness is 50 nm.
[0184] A mixed solution of FAI and FABr is formulated, the molar concentration ratio of FAI to FABr is 3:1, and the solvent is ethanol or isopropyl alcohol. 90 μL of the mixed solution of FAI and FABr is spin-coated on the lead iodide and cesium bromide layers to react with each other, and then anneal the first perovskite layer at a temperature of 100°C for 30 min to form the first perovskite layer (average thickness 100 nm).
[0185] In the ninth step, a perovskite component (Cs) was deposited on the textured hole transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4A DMF / DMSO (4:1) solution of the perovskite component was spin-coated at a concentration of 0.1 mol / L at a spin-coating speed of 500 rpm, and extracted with anisole, followed by annealing at 70°C for 60 min to form a perovskite light-absorbing layer (average thickness 100 nm).
[0186] In the tenth step, a thin layer of LiF (1 nm thick) and C were deposited on the perovskite light absorbing layer using a vacuum deposition process. 60 A thin film layer (10 nm thick) is then fabricated, followed by an electron transport interface layer (11 nm thick).
[0187] In the 11th step, an electron transport layer (thickness 10 nm) made of SnO2 material is fabricated using the atomic layer deposition process (ALD).
[0188] In a twelfth step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the electron transport layer using a magnetron sputtering process.
[0189] In a thirteenth step, a silver electrode is formed on the first transparent conductive layer and the second transparent conductive layer using a screen printing process.
[0190] Example 8 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0191] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0192] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0193] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0194] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0195] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0196] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0197] In the seventh step, a vacuum deposition process is used to deposit C on the tunnel recombination layer. 60 An electron transport layer of the material (thickness 15 nm) was fabricated, and the evaporation rate was 0.2 Å / s.
[0198] In the eighth step, lead iodide and cesium bromide are formed on the electron transport layer using a vacuum deposition process, where the rate of cesium bromide (CsBr) is 0.2 Å / s, the rate of lead iodide (PbI2) is 10 Å / s, and the total thickness is 1000 nm.
[0199] A mixed solution of FAI and FABr is formulated, the molar concentration ratio of FAI to FABr is 3:1, and the solvent is ethanol or isopropyl alcohol. 90μL of the mixed solution of FAI and FABr is spin-coated on the lead iodide and cesium bromide layers to react with each other, and then the first perovskite layer is annealed at a temperature of 200℃ for 5min to form the first perovskite layer (average thickness 300nm).
[0200] In the ninth step, a perovskite component (Cs) was deposited on the textured electron transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 A DMF / DMSO (4:1) solution of the perovskite component was spin-coated at a concentration of 3 mol / L at a spin-coating speed of 6000 rpm, and after extraction with anisole, the layer was annealed at 190°C for 5 min to form a perovskite light-absorbing layer (average thickness 300 nm).
[0201] In the tenth step, a hole transport layer (thickness 10 nm) made of spiro-TTB is deposited on the perovskite light absorbing layer using a vacuum deposition process, and the evaporation rate is 0.1 Å / s.
[0202] In the 11th step, NiO was deposited using the atomic layer deposition process (ALD). x Fabricate a buffer layer (thickness 10 nm) of the material.
[0203] In a twelfth step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the hole transport layer using a magnetron sputtering process.
[0204] In a thirteenth step, a silver electrode is formed on the first transparent conductive layer and the second transparent conductive layer using a screen printing process.
[0205] Example 9 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0206] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0207] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0208] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0209] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0210] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0211] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0212] In the seventh step, a vacuum deposition process is used to deposit C on the tunnel recombination layer. 60 An electron transport layer of the material (thickness 15 nm) was fabricated, and the evaporation rate was 0.2 Å / s.
[0213] In the eighth step, lead iodide and cesium bromide are formed on the electron transport layer using a vacuum deposition process, where the rate of cesium bromide (CsBr) is 0.1 Å / s, the rate of lead iodide (PbI2) is 5 Å / s, and the total thickness is 500 nm.
[0214] A mixed solution of FAI and FABr is formulated, the molar concentration ratio of FAI to FABr is 3:1, and the solvent is ethanol or isopropyl alcohol. 90 μL of the mixed solution of FAI and FABr is spin-coated on the lead iodide and cesium bromide layers to react with each other, and then the first perovskite layer is annealed at a temperature of 150 °C for 20 min to form the first perovskite layer (average thickness 200 nm).
[0215] In the ninth step, a perovskite component (Cs) was deposited on the textured electron transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 A DMF / DMSO (4:1) solution of the perovskite component was spin-coated at a concentration of 1.5 mol / L at a spin-coating speed of 3000 rpm, and after extraction with anisole, the layer was annealed at 130°C for 30 min to form a perovskite light-absorbing layer (average thickness 3000 nm).
[0216] In the tenth step, a hole transport layer (thickness 10 nm) made of spiro-TTB is deposited on the perovskite light absorbing layer using a vacuum deposition process, and the evaporation rate is 0.1 Å / s.
[0217] In the 11th step, NiO was deposited using the atomic layer deposition process (ALD). x Fabricate a buffer layer (thickness 10 nm) of the material.
[0218] In a twelfth step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the hole transport layer using a magnetron sputtering process.
[0219] In a thirteenth step, a silver electrode is formed on the first transparent conductive layer and the second transparent conductive layer using a screen printing process.
[0220] Comparative Example 1 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0221] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0222] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0223] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0224] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0225] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0226] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0227] In the seventh step, a hole transport layer (thickness 15 nm) of spiro-TTB material is fabricated on the tunnel recombination layer using a vacuum deposition process, and the evaporation rate is 0.2 Å / s.
[0228] In the eighth step, lead iodide and cesium bromide are formed on the hole transport layer using a vacuum deposition process, where the rate of cesium bromide (CsBr) is 0.1 Å / s, the rate of lead iodide (PbI2) is 2 Å / s, and the total thickness is 400 nm.
[0229] A mixed solution of FAI and FABr is prepared, the molar concentration ratio of FAI to FABr is 3:1, and the solvent is ethanol or isopropyl alcohol. 80 μL of the mixed solution of FAI and FABr is spin-coated on the lead iodide and cesium bromide layers to react with each other and form a perovskite thin film (thickness 550 nm).
[0230] The perovskite thin film is annealed at a temperature of 150° C. for 20 min to form a perovskite light absorbing layer (average thickness 550 nm).
[0231] In the ninth step, a thin layer of LiF (1 nm thick) and C were deposited on the perovskite light absorbing layer using a vacuum deposition process. 60 A thin film layer (10 nm thick) is then fabricated, followed by an electron transport interface layer (11 nm thick).
[0232] In the tenth step, an electron transport layer (thickness 10 nm) made of SnO2 material is fabricated using the atomic layer deposition process (ALD).
[0233] In an eleventh step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the electron transport layer using a magnetron sputtering process.
[0234] In a twelfth step, a screen printing process is used to form silver electrodes on the first transparent conductive layer and the second transparent conductive layer.
[0235] Comparative Example 2 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0236] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0237] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0238] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0239] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0240] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0241] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0242] In the seventh step, a hole transport layer (thickness 15 nm) of spiro-TTB material is fabricated on the tunnel recombination layer using a vacuum deposition process, and the evaporation rate is 0.2 Å / s.
[0243] In the eighth step, a perovskite component (Cs) with a concentration of 2.1 mol / L was deposited on the textured hole transport layer using a spin-coating process. 0.05 FA 0.8 MA 0.15 PbBr 0.6 I 2.4 A DMF / DMSO (4:1) solution of the above was spin-coated at a spin-coating speed of 2000 rpm, and after extraction treatment with anisole, the layer was annealed at 100°C for 20 min to form a perovskite light-absorbing layer (average thickness 2500 nm).
[0244] In the ninth step, a thin layer of LiF (1 nm thick) and C were deposited on the perovskite light absorbing layer using a vacuum deposition process. 60 A thin film layer (10 nm thick) is then fabricated, followed by an electron transport interface layer (11 nm thick).
[0245] In the tenth step, an electron transport layer (thickness 10 nm) made of SnO2 material is fabricated using the atomic layer deposition process (ALD).
[0246] In an eleventh step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the electron transport layer using a magnetron sputtering process.
[0247] In a twelfth step, a screen printing process is used to form silver electrodes on the first transparent conductive layer and the second transparent conductive layer.
[0248] Comparative Example 3 The method for manufacturing the perovskite n-type silicon-based stacked solar cell provided in the embodiment of the present application is specifically as follows.
[0249] In the first step, a commercial grade n-type silicon wafer with resistivity of 3 Ω.cm, thickness of 180 μm, and texture dimension of 4 μm is prepared. The silicon wafer is sequentially subjected to texturing and cleaning processes to produce a textured n-type single crystal silicon substrate.
[0250] In the second step, an intrinsic amorphous silicon passivation layer (5 nm thick) is deposited on both sides of the n-type single crystal silicon substrate using a PECVD apparatus to form a first passivation layer located on the front side of the n-type single crystal silicon substrate and a second passivation layer located on the back side of the n-type single crystal silicon substrate.
[0251] In the third step, phosphorus doping (doping concentration 10) was performed on the first passivation layer using a PECVD apparatus. 20 cm -3 ) and deposit an n-type amorphous silicon layer (thickness 10 nm) to form the front emitter.
[0252] In the fourth step, boron doping (doping concentration 10) was performed on the second passivation layer using a PECVD apparatus. 19 cm -3 ) and a p-type amorphous silicon layer (thickness 10 nm) is deposited to form a back surface field structure.
[0253] In the fifth step, a first transparent conductive layer (100 nm thick) made of ITO material is fabricated on the p-type amorphous silicon layer using a magnetron sputtering process.
[0254] In the sixth step, an n-type doped microcrystalline silicon layer and a p-type doped microcrystalline silicon layer are sequentially deposited on the n-type amorphous silicon layer using a PECVD apparatus to form a tunnel recombination layer (thickness: 8 nm).
[0255] In the seventh step, a vacuum deposition process is used to deposit C on the tunnel recombination layer.60 An electron transport layer of the material (thickness 15 nm) was fabricated, and the evaporation rate was 0.2 Å / s.
[0256] In the eighth step, lead iodide and cesium bromide are formed on the electron transport layer using a vacuum deposition process, where the rate of cesium bromide (CsBr) is 0.1 Å / s, the rate of lead iodide (PbI2) is 2 Å / s, and the total thickness is 400 nm.
[0257] A mixed solution of FAI and FABr is prepared, the molar concentration ratio of FAI to FABr is 3:1, and the solvent is ethanol or isopropyl alcohol. 80 μL of the mixed solution of FAI and FABr is spin-coated on the lead iodide and cesium bromide layers to react with each other and form a perovskite thin film (thickness 550 nm).
[0258] The second perovskite layer is annealed at a temperature of 150° C. for 20 min to form a perovskite light absorbing layer (average thickness 550 nm).
[0259] In the ninth step, a hole transport layer (thickness 10 nm) made of spiro-TTB is fabricated on the perovskite light absorbing layer using a vacuum deposition process.
[0260] In the tenth step, NiO was deposited on the hole transport layer using atomic layer deposition (ALD). x Fabricate a buffer layer (thickness 10 nm) of the material.
[0261] In an eleventh step, a second transparent conductive layer (100 nm thick) made of ITO material is formed on the hole transport layer using a magnetron sputtering process.
[0262] In a twelfth step, a screen printing process is used to form silver electrodes on the first transparent conductive layer and the second transparent conductive layer.
[0263] In order to verify the performance of the stacked solar cell, the performance parameters such as photoelectric conversion efficiency, fill factor, open circuit voltage, short circuit current, etc. of the devices manufactured in Example 1, Example 4, Example 8, Comparative Example 1, Comparative Example 2 and Comparative Example 3 under the same effective area were tested, and the comparison of the performance parameters is shown in Table 1.
[0264] [Table 1]
[0265] As can be seen from Table 1, the perovskite-silicon based stacked solar cell provided in the examples of the present application has improved open circuit voltage and short circuit current as well as improved conversion efficiency compared to a general stacked solar cell manufactured only by a solution process or vacuum deposition process. As can be seen from the above, the perovskite-silicon based stacked solar cell manufactured by the manufacturing method provided in the examples of the present application can achieve both a high open circuit voltage and a high short circuit current, and also has improved photoelectric conversion efficiency.
[0266] In the above description of the embodiments, the particular features, structures, materials, or characteristics may be combined in any suitable manner in any one or more embodiments or examples.
[0267] The above are merely specific embodiments of the present application, and the scope of protection of the present application is not limited thereto. Any changes or replacements that a person skilled in the art can easily think of within the technical scope described in the present application are included in the scope of protection of the present application. Therefore, the scope of protection of the present application shall be equivalent to the scope of protection of the claims.
[0268] The above-described embodiment of the device is merely illustrative, and the units described herein as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, i.e., they may be located in one place or distributed among multiple network units. Some or all of the modules may be selected according to actual needs to achieve the purpose of the solution of the embodiment. Those skilled in the art can understand and implement it without any creative effort.
[0269] The terms "one embodiment," "an embodiment," or "one or more embodiments" used herein mean that a particular feature, structure, or characteristic described in the embodiment is included in at least one embodiment of the present application. Note also that various instances of the phrase "in one embodiment" do not necessarily refer to the same embodiment.
[0270] In the specification provided herein, numerous specific details have been set forth. However, it will be understood that embodiments of the present application may be practiced without these specific details. In some instances, well-known methods, structures and techniques have not been shown in detail in order not to obscure the understanding of this specification.
[0271] Finally, it should be noted that the above embodiments are merely for illustrating the technical solutions of the present application, and are not intended to limit the same. Although the present application has been described in detail with reference to the above embodiments, those skilled in the art can naturally understand that modifications to the technical solutions described in the above embodiments, or equivalent replacements for some of the technical features thereof, are possible, and such modifications or replacements do not deviate the essence of the relevant technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application. [Explanation of symbols]
[0272] 101 n-type crystalline silicon wafer 102 First passivation layer 103 Second passivation layer 104 n-type amorphous / microcrystalline silicon layer 105 p-type amorphous / microcrystalline silicon layer 106 First transparent conductive layer 107 Charge recombination layer 1070 n-type doped microcrystalline silicon layer 1071 p-type doped microcrystalline silicon layer 108 First carrier transport layer 109 Perovskite light absorbing layer 110 Second carrier transport interface layer 1100 Second carrier transport interface layer 1101 Second carrier transport interface layer II 111 Second carrier transport layer 112 Second transparent conductive layer 113 Electrode 1090 First Perovskite Layer 1091 Second Perovskite Layer
Claims
1. Providing a substrate including a silicon-based bottom cell having a textured structure, a charge recombination layer, and a first carrier transport layer, which are stacked in sequence; forming a perovskite light absorbing layer consisting of two perovskite layers, a first perovskite layer and a second perovskite layer, on the first carrier transport layer having a textured structure, wherein the first perovskite layer is manufactured by a solution process and the second perovskite layer is manufactured by a perovskite framework vacuum deposition process.
2. 2. The method for producing a perovskite-silicon based stacked solar cell according to claim 1, wherein the average thickness of the first perovskite layer produced by a solution process ranges from greater than 0 to less than or equal to ½L, where L is the average vertical distance from the bottom to the top of the texture structure of the first carrier transport layer.
3. The step of forming a perovskite light absorbing layer composed of two perovskite layers, a first perovskite layer and a second perovskite layer, on the first carrier transport layer having a texture structure includes: Producing a first perovskite layer on the first carrier transport layer having a textured structure by a solution process; and then producing a second perovskite layer by perovskite framework vacuum deposition.
4. The step of forming a perovskite light absorbing layer composed of two perovskite layers, a first perovskite layer and a second perovskite layer, on the first carrier transport layer having a texture structure includes:
2. The method for producing a perovskite-silicon based stacked solar cell according to claim 1, comprising the steps of: producing a second perovskite layer on the first carrier transport layer having a textured structure by a perovskite framework vacuum deposition method; and then producing a first perovskite layer by a solution method.
5. The step of forming a perovskite light absorbing layer composed of two perovskite layers, a first perovskite layer and a second perovskite layer, on the first carrier transport layer having a texture structure includes:
2. The method for producing a perovskite-silicon based stacked solar cell according to claim 1, comprising the steps of depositing a perovskite framework on the first carrier transport layer having a textured structure by a vacuum deposition method, and then producing a first perovskite layer by a solution method, wherein a solution used in the solution method contains an excess of an organic amine, and during the process of forming the first perovskite layer, a material in the perovskite framework reacts with the organic amine to form a second perovskite layer.
6. The solute of the solution used in the solution method is a mixed perovskite component Cs containing Cs, FA or MA. x F.A. y M.A. z PbBr m I n 6. The method for producing a perovskite-silicon based stacked solar cell according to any one of claims 1 to 5, wherein (x+y+z=1, m+n=3) and the solvent comprises one or more of N,N-dimethylformamide and dimethylsulfoxide.
7. The perovskite skeleton vacuum deposition method includes first forming a perovskite skeleton by vacuum deposition, and then reacting the perovskite skeleton with an organic amine to form a second perovskite layer; The perovskite framework is composed of two or more PbX 2 and CsY, wherein X and Y are Cl - , B - , I - , S.C.N. - and the organic amine is one or more of formamidine hydroiodide, methylammonium bromide, and formamidine hydrobromide.
8. The method for producing a perovskite-silicon-based stacked solar cell according to claim 6, wherein the concentration of the solution used in the solution method is 0.2 mol / L to 3 mol / L.
9. The method for producing a perovskite-silicon based stacked solar cell according to any one of claims 1 to 5, wherein the perovskite framework vacuum deposition method includes spin-coating an organic amine solution onto the perovskite framework, the rotation speed of spin-coating is 500 rpm to 6000 rpm, and the thickness of the perovskite framework is in the range of 50 nm to 1000 nm.
10. The method for producing a perovskite-silicon based stacked solar cell according to any one of claims 1 to 5, further comprising the steps of sequentially forming a second carrier transport layer, a transparent conductive layer and an electrode on the perovskite light absorbing layer after forming the perovskite light absorbing layer.
11. A perovskite-silicon based stacked solar cell manufactured by the method for manufacturing a perovskite-silicon based stacked solar cell according to any one of claims 1 to 10.
12. The present invention includes a silicon-based bottom cell having a textured structure, a charge recombination layer, and a first carrier transport layer, which are stacked in sequence, and a perovskite light absorbing layer covering the first carrier transport layer having a textured structure; The perovskite light absorbing layer is composed of two perovskite layers, a first perovskite layer and a second perovskite layer, the first perovskite layer being manufactured by a solution process and the second perovskite layer being manufactured by a perovskite framework vacuum deposition process.
13. 13. The perovskite-silicon-based stacked solar cell according to claim 11 or 12, wherein the first perovskite layer is distributed at least in valleys of a textured structure of the first carrier transport layer, and an average thickness of the first perovskite layer is ½ or less of a height of the textured structure, and a portion of the structure of the second perovskite layer is distributed at least on a slope and a top part of the textured structure, and the slope and the top part maintain the same texture shape as the slope and the top part.
14. The perovskite-silicon based stacked solar cell of claim 11 or 12, wherein the first carrier transport layer has a thickness in the range of 5 nm to 200 nm, and the perovskite light absorbing layer has an average thickness in the range of 100 nm to 3000 nm.
15. 13. The perovskite-silicon based stacked solar cell of claim 11 or 12, wherein the average thickness of the first perovskite layer is in the range of 100 nm to 300 nm, and the thickness of the second perovskite layer is in the range of 100 nm to 3000 nm.
Citation Information
Patent Citations
Organic / inorganic hybridized perovskite solar battery and preparation method thereof
CN103700769A
Perovskite thin film and preparation method thereof, and application of perovskite thin film
CN110534653A
Preparation method of perovskite laminated solar cell and laminated solar cell
CN112186105A
Method of manufacturing photoelectric converter and method of manufacturing electronic equipment
JP2010206061A
Method for depositing a perovskite material
JP2018518845A
Cited By
Perovskite / silicon laminated solar cell with selective passivation contact structure and preparation method thereof
CN119744071A