Silicone Polyether
Patent Information
- Application Number
- JP2024533290
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-20
- Filing Date
- 2022-10-12
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional methods for producing silicone polyethers require the use of organic solvents and surfactants, which can be undesirable in certain applications due to their mobility and potential interference with the desired properties of the final product.
A method for producing silicone polyethers in an oil-in-water emulsion using a hydrosilylation reaction without the need for additional surfactants, by combining polyorganohydrogensiloxane, polyoxyalkylene, and a hydrosilylation catalyst in water, allowing for the formation of a surfactant-free emulsion.
The method results in a stable emulsion that is substantially free of surfactants, enhancing the suitability of silicone polyethers for applications where surfactant presence is undesirable, such as hydrophobization, while maintaining stability and performance.
Smart Images

Figure 2024545068000001 
Figure 2024545068000002 
Figure 2024545068000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS: This application claims the benefit under 35 U.S.C. §119(e) of U.S. Provisional Patent Application No. 63 / 291,553, filed December 20, 2021. U.S. Provisional Patent Application No. 63 / 291,553 is incorporated herein by reference.
[0002] The present invention relates to a new class of silicone polyethers, including methods for their preparation and use. [Background technology]
[0003] Silicone polyethers ("SPEs") represent a well-known class of polyorganosiloxane-polyoxyalkylene copolymers. A wide variety of polymer architectures are known, including block, branched, raked, and gemini architectures. SPEs are used in a wide variety of applications, including surfactants, foaming agents, solubilizers, and softeners. They are also known to add leveling, slip, and mar resistance properties to coating formulations, and for use as additives in personal care products. SPEs are classically made by the well-known platinum-catalyzed hydrosilylation reaction between the -SiH groups of the polyorganohydrogensiloxane and the unsaturated aliphatic hydrocarbon groups (e.g., vinyl, allyl, etc.) of the polyoxyalkylene. Such reactions are most commonly carried out neat or in organic solvents (e.g., alcohols, hydrocarbons, ethers, etc.). See, for example, U.S. Patent No. 6,346,553, U.S. Patent No. 6,987,157, U.S. Patent No. 8,008,407, U.S. Patent No. 8,541,514, U.S. Patent No. 10,385,212, and European Patent No. 349,877. Summary of the Invention
[0004] In one aspect, the invention includes a novel class of SPEs represented by formula (I). In another aspect, the invention includes a method for preparing such SPEs, comprising combining a) a polyorganohydrogensiloxane ("-SiH polymer") represented by formula (VI) and b) a polyoxyalkylene represented by formula (VII) in the presence of c) a hydrosilylation catalyst. In an aspect of the invention, the subject method comprises combining the aforementioned components a), b) and c) in water. In yet another aspect of the invention, the subject method comprises combining the aforementioned components a), b) and c) in water to form an oil-in-water emulsion and carrying out in-situ hydrosilylation to form the subject SPE as a reaction product in the emulsion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0005] The subject invention comprises a class of silicone polyethers (SPEs) represented by formula (I): [ka] During the ceremony, R is the same or different and is selected from H (hydrogen) and hydrocarbon groups containing 1 to 18 carbon atoms, more preferably 1 to 8 carbon atoms, with the proviso that R contains less than 80, 50, or 25 mole % H. In selected embodiments, R contains 0 to 25 or 0 to 5 mole % H. Representative hydrocarbon groups include a) alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, cyclohexyl, and heptyl; b) aryl groups such as phenyl, tolyl, xylyl, and naphthyl; and c) aralkyl groups such as benzyl and phenethyl, with methyl and phenyl groups being preferred, and methyl being most preferred. In one class of embodiments, R contains at least 20, 50, 75, 90, or even 95 mole % methyl groups ( 29 As determined by Si NMR).
[0006] m is an integer of 0 to 100, 0 to 70, or 0 to 40.
[0007] n is an integer from 10 to 500, from 20 to 200, from 40 to 100, or from 50 to 70.
[0008] Z may be the same or different and is selected from Y, OH (hydroxyl), and the following formula: (II): [ka] (wherein R is as defined above, R' is an aliphatic divalent hydrocarbon (e.g., alkylene) group having 2 to 4 carbon atoms, and t is 10 to 800).
[0009] Y is represented by the following formula: (III): [ka] (In the formula, symbol [ka] represents a covalent bond to the silicon atom of repeat unit n in formula I).
[0010] R 1 are the same or different and are selected from aliphatic hydrocarbon groups (eg, alkyl groups) containing 8 to 20 carbon atoms.
[0011] R 2 is represented by the following formula: (IV):-(AO) q -X (In the formula, A are the same or different and are selected from aliphatic divalent hydrocarbon (e.g., alkylene) groups having 2 to 4 carbon atoms, with the proviso that: (AO) q contains at least 3 (e.g., 8 to 40 or 10 to 40) ethylene oxide moieties. For example, in one class of embodiments, R 2 is expressed by the following formula: (V):-(CH 2CH 2 O-) q X (In the formula, and q is an integer of 3 to 40.
[0012] X (shown in both Formula IV and Formula V) is the same or different and is selected from H (hydrogen) and an aliphatic hydrocarbon (eg, alkyl) group having 1 to 4 carbon atoms.
[0013] R 3 are the same or different and are aliphatic divalent hydrocarbon (e.g., alkylene) groups containing 1 to 4 carbon atoms. In one class of embodiments, R 3 is a methylene group.
[0014] Z is additionally subject to the proviso that it contains: i) 10 to 80 mol % of Y, ii) 0 to 60 mol % OH, and iii) 0 to 60 mole percent of organosiloxane groups of formula II.
[0015] In another embodiment, Z comprises greater than 40 mole % Y, and the sum of OH and organosiloxane is less than 60 mole %.
[0016] In another class of embodiments, the subject SPEs have the formula: (Ia): [ka] In the formula, R, m, n, R 1 , R 2 and R 3 is as defined above, but R is preferably methyl, m is preferably 0 to 40, n is preferably 20 to 200, and R 1 are the same or different and are preferably selected from alkyl groups containing 8 to 20 carbon atoms, R 3 are the same or different and are preferably selected from alkylene groups containing 1 to 4 carbon atoms.
[0017] The subject SPEs may be prepared by combining component a) a polyorganohydrogensiloxane (-SiH polymer) and component b) a polyoxyalkylene in the presence of component c) a hydrosilylation catalyst. Each component (a, b, and c) is described in more detail below. Although the subject combination of components a), b), and c) is unique, the techniques for combining these components may employ conventional methods. For example, components a), b), and c) may be combined neat or in an organic solvent. However, in a preferred embodiment, the aforementioned components are combined and reacted to form a silicone polyether reaction product in situ in water. In an even more preferred embodiment, the aforementioned components are combined to form a discontinuous oil phase in a continuous water phase, i.e., an oil-in-water emulsion, and a hydrosilylation reaction takes place between components a) and b) to form a silicone polyether reaction product in situ as part of the discontinuous oil phase. Such a process is often referred to as mechanical suspension polymerization (MSP). Components a), b) and c) can be combined in any order, along with additional optional components as described below, although it is preferred that at least a portion (e.g., a majority by weight) of components a) and b) are combined in water by mixing to form a discontinuous (oil) phase prior to adding the majority of component c). The initial water or emulsion formed from the addition of the aforementioned components may optionally be heated to facilitate the hydrosilylation reaction. The water used to prepare the emulsion may be from any source and may optionally be purified, for example, by filtration, distillation, reverse osmosis techniques, and the like.
[0018] Unlike conventional methods of forming oil-in-water emulsions, the preparation of the subject emulsions does not require the use of surfactants (emulsifiers) other than component b). When component b) reacts with component a), the resulting emulsions containing silicone polyether reaction products may be substantially free of surfactants. That is, by selecting the appropriate molar ratio of alkenyl groups of component b) to SiH groups of component a), all or substantially all of the initial surfactant (component b) used to prepare the initial emulsion reacts with component a) to form the subject silicone polyether reaction products and are no longer present intact in the final emulsion. This attribute is beneficial in many applications, including the use of such emulsions in various hydrophobization applications, particularly where the presence of mobile surfactants is undesirable. Thus, while conventional non-reactive surfactants may be used to prepare the subject emulsions, in one class of embodiments, the subject emulsions are prepared without non-reactive surfactants (i.e., surfactants that do not react with component a to form covalent bonds). In this manner, the resulting emulsions of the subject silicone polyether reaction products are substantially free of surfactants. As used herein, the term "substantially free" means less than 1 wt.%, preferably less than 0.5 wt.%, more preferably less than 0.1 wt.%, and even more preferably less than 0.01 wt.%, based on the total weight of the suspension. For clarity, in this context, the silicone polyether reaction product itself is not considered a "surfactant."
[0019] Mixing may be used to facilitate the formation of the emulsion. Mixing may be performed using any known technique. Exemplary mixing devices include homogenizers, sonolators, rotor-stator turbines, colloid mills, microfluidizers, sonicators, blades, helices, and combinations thereof. Exemplary methods are described in U.S. Pat. No. 6,013,682, U.S. Pat. No. 8,877,293, and U.S. Patent Application Publication No. 2015 / 0010711. A homogenizer or sonic probe may be used to achieve the desired particle size. The particles of the discontinuous oil phase preferably have a volume weighted median of particle size distribution "Dv(0.5)" of 100 to 7000 nm, more preferably 200 to 3000 nm, as measured via laser diffraction according to ISO 13320 (2009) using a Malvern 3000. As used herein, the term "particles" refers to oil phase droplets.
[0020] Component a): Polyorganohydrogensiloxane ("SiH polymer") The class of polyorganohydrogensiloxanes applicable to the present invention is not particularly limited and includes a wide range of commercially available materials. Applicable polymers may have a viscosity of 5 to 1000 cSt, more preferably 10 to 500 cSt, measured at 25° C. according to ASTM D2196-05. Different polyorganohydrogensiloxanes, for example, having different chemical structures, molecular weights and / or viscosities, may be used in combination. A preferred class of SiH polymers is represented by the formula: (VI): [ka] (wherein R, m, and n are as defined above).
[0021] As indicated, the subject SiH polymers contain -SiH groups which may be located at terminal (end) and / or intermediate (pendant) positions on the polysiloxane backbone. However, in preferred embodiments, the -SiH groups are located primarily at pendant positions, i.e. 29More than 95% by weight, more preferably more than 99% by weight, of all -SiH groups are located at pendant positions along the polysiloxane chain as determined by Si NMR. Applicable commercially available SiH polymers include SYL-OFF™ 7672 crosslinker, SYL-OFF™ 7678 crosslinker, SYL-OFF™ SL 7028 crosslinker, SYL-OFF™ 7682-000 crosslinker, and XIAMETER™ MHX-1107 fluid 30 cSt (all available from Dow Chemical Co.).
[0022] Component (b): Polyoxyalkylene A class of polyoxyalkylenes applicable to the present invention is represented by the formula: (VII): [ka] (In the formula, R 1 , R 2 and R 3 is as defined above, and R 4 are the same or different and are selected from alkenyl and alkynyl).
[0023] The subject polyoxyalkylenes preferably have a hydrophile-lipophile balance (HLB) of 3 to 35, or more preferably 6 to 15, calculated according to the Davis method (JT Davises, Gas / Liquid and Liquid / Liquid Interfaces. Proc. 2nd Int. Congress Surface Activity, vol. 1, A quantitative kinetic theory of emulsion type, I. Physical chemistry of the emulsifying agent. Butterworths, London (1957)) using the following formula: HLB=7+Σ(hydrophilic group)+Σ(hydrophobic group). Commercially available examples of applicable polyoxyalkylenes include ADEKA® REASOAP ER10, ADEKA® REASOAP ER20, and ADEKA® REASOAP ER30 available from Adeka.
[0024] Component c): Hydrosilylation catalyst The hydrosilylation catalyst applicable to the present invention is not particularly limited, and may include platinum, rhodium, iridium, palladium, ruthenium, or a combination thereof.The hydrosilylation catalyst may be, for example, fine platinum powder, platinum black, platinum acetylacetonate, chloroplatinic acid, alcohol solution of chloroplatinic acid, olefin complex of chloroplatinic acid, complex of chloroplatinic acid and alkenylsiloxane (e.g., divinyltetramethyldisiloxane diluted in dimethylvinylsiloxy endblocked polydimethylsiloxane, which may be prepared according to the method described in U.S. Pat. No. 3,419,593), complex of chloroplatinic acid and divinyltetramethyldisiloxane as described in U.S. Pat. No. 5,175,325, or thermoplastic resin containing the aforementioned platinum catalyst.In other embodiments, the hydrosilylation catalyst is a platinum vinylsiloxane complex, such as Karstedt's catalyst or Speier's catalyst, or a combination thereof. Additional examples of applicable catalysts are described in US Patent No. 2,823,218, US Patent No. 3,159,60, US Patent No. 3,220,972, US Patent No. 3,296,291, US Patent No. 3,419,359, US Patent No. 3,445,420, US Patent No. 3,516,946, US Patent No. 3,697,473, US Patent No. 3,715,334, US Patent No. 3,814,730, US Patent No. 3,814,731, US Patent No. 3,890,359, US Patent No. 3,923,705, US Patent No. 3,989,668, US Patent No. 4,123,604, US Patent No. 4,784,879, and US Patent No. 5,036,117. The hydrosilylation catalyst may be a single catalyst or a combination of two or more catalysts. Commercially available examples of applicable hydrosilylation catalysts include SYL-OFF™ 4000 catalyst.
[0025] The molar ratio of component b) to the SiH groups of component a) is preferably less than 1:1, for example 1:1 to 1:2. Using this molar ratio ensures that component b) is completely reacted and that the resulting silicone polyether reaction product (and the corresponding emulsion containing it) is substantially free of residual surfactant. The concentration of component c) (hydrosilylation catalyst) used in the present invention can be determined by routine experimentation. Typically, an effective amount of catalyst is in the range of providing 0.1 to 3000 parts per million (ppm) of actual metal (e.g., platinum) based on the weight of components a) and b).
[0026] Optional ingredient d): alkenyl-functional polyorganosiloxane The method for preparing the subject SPE may include combining an alkenyl-functional polyorganosiloxane as an additional optional component ("component d"). The class of applicable polymers is not particularly limited, so long as it contains at least one, and more preferably at least two, alkenyl functional groups (e.g., vinyl, allyl, etc.). The alkenyl groups may be present at either or both terminal and pendant positions along the siloxane backbone of the polyorganosiloxane, but are preferably located only at the terminals. For example, in a preferred embodiment, the subject alkenyl-functional polyorganosiloxane has the general formula: Vi-[Si(R' 2 )O] v -Si(R' 2)Vi, where R' is the same or different and is selected from the same hydrocarbon radicals as defined above for R, Vi is a vinyl radical, and v is an integer resulting in a polymer having a viscosity ranging from 5 to 100,000 as measured at 25°C according to ASTM D2196-05. R' is preferably methyl. When present, optional component d) is preferably used in an amount such that the molar ratio of its alkenyl functional groups to the -SiH groups of component a) is 2:1 to 0.1:1. Representative polymers are described in U.S. Pat. No. 1,038,5212. Commercially available examples of applicable polymers include SILASTIC™ SFD 128, SILASTIC™ SFD-120, and DOWSIL™ SFD-119, all of which are available from The Dow Chemical Company.
[0027] Optional ingredient e): Oil The method for preparing the subject SPE may include combining one or more oils as an additional optional component ("component e"). Applicable oil classes are not particularly limited and include i) hydrocarbon-based oils of mineral, vegetable, or synthetic origin, such as paraffin oil, hydrogenated isoparaffin, hydrogenated liquid polydecene, petrolatum, olive oil, linseed oil, etc., and ii) non-reactive polyorganosiloxanes, i.e., "silicones." Oils that are liquid at room temperature are preferred. Representative silicones include non-volatile species, as well as both linear and branched species. Representative classes include polyalkylsiloxanes, polyarylsiloxanes, polyalkylarylsiloxanes, polysiloxane gums, polysiloxane elastomers, and combinations thereof. A preferred group includes DOWSIL™ 200 fluids (trimethylsilyl terminated polydimethylsiloxanes) including those having a viscosity of about 5 to about 200,000 cSt (centistokes) measured at 25° C. according to ASTM D4283-98 (2015). Combinations of different polyorganosiloxanes may be used together. When present, optional component e) preferably constitutes 10 to 80% or 20 to 70% by weight of the discontinuous oil phase of the emulsion.
[0028] When used, optional components d) and / or e) are preferably combined with components a) and b) when forming the initial emulsion of components a) and b).The alkenyl-functional polyorganosiloxane can participate in the hydrosilylation reaction of component a), for example, leading to the formation of organosiloxane groups represented by formula (II) on the silicone polyether reaction product, while component e) is preferably non-reactive and does not directly participate in the hydrosilylation reaction (for example, does not break or form covalent bonds).Therefore, component e) remains in the discontinuous oil phase of the final emulsion that comprises the silicone polyether reaction product.
[0029] In another embodiment, alcohol may be added to the resulting silicone polyether reaction product emulsion. The subject emulsions are surprisingly stable even after the addition of sufficient alcohol to form an emulsion with antimicrobial properties. For example, the subject emulsions remain stable upon the addition of sufficient alcohol to constitute at least 10%, 25%, 50%, 60%, 70%, 80%, or even 90% by weight of the total weight of the emulsion. In other embodiments, the alcohol constitutes 5-95%, 10-90%, or 25-75% by weight of the total weight of the emulsion. The choice of alcohol typically depends on the intended application. However, C 10 alcohols such as methanol, ethanol, n-propanol, isopropanol, butanol, t-butanol, 2-butanol, pentanol, hexanol, and combinations thereof are preferred. 1 ~C 6 Monohydric alcohols are generally preferred. In a subclass of embodiments, 2 ~C 4 Monohydric alcohols, such as ethanol, 1-propanol and 2-propanol, and combinations thereof, are preferred. The remaining proportion of the continuous phase of the subject emulsions may comprise water.
[0030] Many embodiments of the invention have been described, and in some instances, certain embodiments, options, ranges, components, or other features have been characterized as "preferred". Such designations of "preferred" features should in no way be construed as essential or critical aspects of the invention. Expressed ranges include specifically specified endpoints. As used herein, the terms "molecular weight" and "Mw" refer to weight average molecular weight measured by gel permeation chromatography (GPC) using an Agilent Technologies 1260 Infinity chromatograph and toluene as the solvent. The instrument is equipped with three columns, a PL gel 5 μm, 7.5×50 mm guard column, and two PL gel 5 μm, Mixed-C 7.5×300 mm columns. Calibration is performed using polystyrene standards. Samples were made by dissolving the polymer in toluene (approximately 1 mg / mL), and then the samples were immediately analyzed by GPC (flow rate of 1 mL / min, column temperature of 35° C., run time of 25 minutes). Particle size measurements were determined as the volume weighted median of the particle size distribution (Dv50) using a Mastersizer™ 3000 laser diffraction particle size analyzer from Malvern Instruments according to ISO 13320 (2009). EXAMPLES
[0031] All preparations and tests are carried out at room temperature (RT) at standard pressure (1 atmosphere or 760 mm Hg) unless otherwise indicated. Percentages are weight percent (wt%) unless otherwise noted. The materials shown in Table 1 below were used in the preparation of the sample emulsions. The polyorganosiloxane structures are shown in Table 1 using the following conventional structure nomenclature: M-monofunctional (R 3 SiO 1 / 2 ), D-bifunctional (R 2 SiO 2 / 2 ), T-trifunctional (RSiO 3 / 2 ), Q-Tetrafunctional (SiO 4 / 2).
[0032] For the polymers listed in Table 1, R is methyl and is not shown as per convention. However, hydrogen substituents are shown in superscript. For further information regarding the use of this nomenclature, see Chemistry and Technology of Silicones, Noll, Academic Press, 1968. [Table 1] [ka]
[0033] Unless otherwise stated, sample emulsions were prepared with the ingredients specified in the table above. Emulsions were prepared by the classical phase inversion process, which involves the sequential addition of water to oil in the presence of polyoxyalkylene, which eventually undergoes phase inversion to form a water-in-oil emulsion. According to this method, the specified oil, SiH polymer, and alkenyl-functional polyorganosiloxane (if used) were mixed first, followed by the addition of the specified polyoxyalkylene, inversion water, and hydrosilylation catalyst (if used), followed by the remaining water, in sequence. Unless otherwise stated, all ingredients were mixed at 3500 rpm for 30 seconds using a dental mixer (Hauschild SPeedMixer). The reaction between the polyoxyalkylene and the SiH polymer was allowed to occur at room temperature (RT) for approximately one week, after which the particle size distribution was measured (Malvern Metasizer 3000). An emulsion prepared without catalyst was used as a comparison.
[0034] The stability of the sample emulsions was measured after the emulsions were allowed to cure for approximately one week. The stability of the sample emulsions was tested as prepared and / or after the addition of isopropanol (i.e., 1 g of emulsion was mixed with 5 g of isopropanol). The stability of the emulsions was visually assessed according to the following criteria: (1) completely flocculated, (2) partially flocculated / creamy, and (3) no signs of flocculation.
[0035] Example 1: Examples were prepared using the components specified in Table 2 below. To evaluate hydrophobic performance, sample emulsions were applied to paper, i.e. (LENETA FORM N2A-2) and pine wood blocks. Sample emulsions applied to paper were prepared using DOWSIL™ 200 Fluid 100,000 cSt, while those applied to pine wood were prepared using DOWSIL™ 200 Fluid 12,500 cSt. For paper, sample emulsions were applied as 120 μm thick coatings, which were dried overnight at room temperature and analyzed using the Sessile Drop Method (Biolin Scientific Theta Optical). Water contact angles were estimated based on images captured 19 seconds after deposition of a 2.5 μl drop and averaged over three measurements. For pine wood, sample emulsions were first diluted to 10 wt. % silicone (i.e., the sum of components a and e) and 5.6 mg / cm 2 The samples were coated with an average density of 0.1 ml and then allowed to dry at room temperature for about one week. Then, 10 minutes after applying a 0.1 ml water drop, the wet performance of each sample was evaluated using the following numerical scale of 1 to 5 using the average of three measurements. [Table 2]
[0036] As shown by the test results reported in Table 2, inventive sample No. 4 showed statistically significant improvement in hydrophobicity for both paper and pine wood, along with improved stability in isopropanol (IPA) compared to comparative sample Nos. 1-3 and 5-6. Interestingly, the addition of catalyst had little effect on the performance of the comparative samples (i.e., 1 vs. 2 and 5 vs. 6). [Table 3]
[0037] Example 2: Sample emulsions Nos. 7-9 were prepared using the ingredients specified in Table 3 below. Each sample was tested for stability according to the methods described above. Each sample utilized a different type of polyoxyalkylene, all of which were selected from the types described in the claims. As shown below, each emulsion had good stability. [Table 4]
[0038] Example 3: (for comparison) To demonstrate the technical effect of the polyoxyalkylene structure, a comparative sample emulsion (number 10) was prepared using a polyoxyalkylene species (allyl polyether 1) not included in the claims. That is, allyl polyether 1 has a similar number of repeating alkoxy (EO) units and alkyl groups as the claimed type, but allyl polyether 1 has a different structure. See the respective structures provided above. During preparation, comparative sample number 10 demulsified and underwent phase separation over the course of the reaction. Without being bound by theory, it is believed that the location of the allyl groups in allyl polyether 1 partitions into the silicone discontinuous phase during the reaction, rather than remaining at the water-oil interface. This results in the emulsion becoming unstable. [Table 5]
[0039] Example 4: Samples Nos. 11-15 demonstrate the stability of the subject emulsions in isopropanol (IPA) when prepared with a wide variety of oils. The samples were prepared according to the method previously described with the following exceptions, using the ingredients listed in Table 5 below. Samples 13 and 14 were first mixed in a dental mixer according to the method previously described, then mixed with a rotor-stator disperser (ULTRA-TURRAX homogenizer) at 11000 rpm, and then finally mixed with a dental mixer at 3500 rpm for 30 seconds. [Table 6]
[0040] Example 5: This example illustrates the ability to include additional reactive polymers (e.g., SiH Polymer 2 and SILASTIC™ SFD 128 polymer) in the subject emulsions, for example, to increase molecular weight and crosslinking while still maintaining good emulsion stability. In this example, hydrosilylation is believed to occur not only within the emulsion droplets (e.g., between SiH Polymer 2 and SILASTIC™ SFD 128 polymer) to form branched polymers, but also at the interface between the polyoxyalkylene and SiH Polymer 1. That is, the addition of other reactive polymers (e.g., SiH Polymer 2 and SILASTIC™ SFD 128 polymer) does not interfere with the improved alcohol stability of emulsions containing the subject silicone polyether reaction products. [Table 7]
[0041] Example 6: Sample emulsions were prepared using the ingredients listed in Table 7 and then tested for stability in isopropanol. As shown by the test results reported below, the location of the SiH groups in the SiH polymer had a significant effect on stability, i.e., SiH polymers 3 and 5-7 had SiH groups located only at terminal positions, while SiH polymers 1 and 4 had SiH groups located at pendant positions along the polyorganosiloxane backbone. 1 H NMR analysis showed that the NMR spectrum was Si-CH 2 In contrast to SiH Polymer Nos. 1 and 4 in Sample Emulsion Nos. 16 and 19, which showed evidence of hydrosilylation by the formation of - (0.7-0.4 ppm) and a decrease in Si-H intensity (4.7 ppm), it was determined that the SiH groups of SiH Polymer Nos. 3 and 5-7 remained largely unreacted in Sample Nos. 18 and 20-22. Thus, the location of the SiH bond has a significant effect on reaction with the subject polyoxyalkylenes, which in turn affects emulsion stability. Although SiH Polymer 2 had SiH groups at pendent locations, there was an insufficient number of SiH groups available to stabilize the resulting emulsion. [Table 8]
[0042] Example 7: A silicone polyether reaction product was prepared neat by blending 0.6 g of SiH polymer 1 and 4 g of polyoxyalkylene (ADEKA® REASOAP ER-10) with 0.1 g of SYL-OFF4000 catalyst and allowed to react at room temperature for approximately one week. After one week, the initially liquid blend formed a powdery solid. 4.60 g of the solid was then combined with 60.00 g of silicone oil (DOWSIL® 200 fluid 12500 cSt) and 35.4 g of inverted water, followed by mixing for 30 seconds at 3500 rpm using a dental mixer (Hauschild SPeedMixer). A coarse emulsion (Sample No. 24) was then formed, with large droplets surrounded by jelly-like particles. Unlike when formed in situ as part of a water-in-oil emulsion, the subject silicone polyether reaction product, when prepared neat, was unable to form a comparable stable emulsion. That is, the preformed silicone polyether reaction products did not function as effective surfactants.
Claims
1. A silicone polyether represented by the formula: 【Chemistry 1】 During the ceremony, R is the same or different and is selected from H and a hydrocarbon group containing 1 to 18 carbon atoms, with the proviso that R contains less than 80 mole % H; m is an integer from 0 to 100; n is an integer from 10 to 500, Z is the same or different and is selected from Y, OH, and an organosiloxane group represented by the formula: (II): 【Chemistry 2】 wherein R is as defined above, R′ is an aliphatic divalent hydrocarbon group having 2 to 4 carbon atoms, and t is 10 to 800; Y is represented by the following formula: 【Chemistry 3】 During the ceremony, R 1 are the same or different and are selected from aliphatic hydrocarbon groups containing 8 to 20 carbon atoms; R 2 is represented by the following formula: -(AO) q -X (in the formula, A are the same or different and are selected from aliphatic divalent hydrocarbon groups having 2 to 4 carbon atoms, provided that (AO) q contains at least three ethylene oxide moieties, q is an integer from 3 to 40, X is the same or different and is selected from H and an aliphatic hydrocarbon group having 1 to 4 carbon atoms; R 3 are the same or different and are aliphatic divalent hydrocarbon radicals containing 1 to 4 carbon atoms, However, Z is i) 10 to 80 mol % of Y; ii) 0 to 60 mol % OH; iv) 0 to 60 mole percent of said organosiloxane groups of formula II.
2. R 2 is expressed by the following formula: -(CH 2 CH 2 O-) q X In the formula: q is an integer from 3 to 40, 2. The silicone polyether of claim 1, wherein X is the same or different and is selected from H and alkyl groups having 1 to 4 carbon atoms.
3. R 3 The silicone polyether according to claim 1 or 2, wherein is a methylene group.
4. R 1 4. The silicone polyether according to claim 1, wherein: are the same or different and are selected from alkyl groups containing from 8 to 20 carbon atoms.
5. 5. The silicone polyether of claim 1, wherein R comprises at least 90 mole percent methyl groups.
6. 6. The silicone polyether of claim 1, wherein Z contains more than 40 mol % of Y and the sum of OH and organosiloxane is less than 60 mol %.
7. A silicone polyether represented by the formula: 【Chemistry 4】 During the ceremony, R is the same or different and is selected from H and a hydrocarbon group containing 1 to 18 carbon atoms, with the proviso that R contains less than 80 mole % H; m is an integer from 0 to 100; n is an integer from 10 to 500, R 1 are the same or different and are selected from aliphatic hydrocarbon groups containing 8 to 20 carbon atoms; R 2 is represented by the following formula: -(AO) q -X (in the formula, A are the same or different and are selected from aliphatic divalent hydrocarbon groups having 2 to 4 carbon atoms, provided that (AO) q contains at least three ethylene oxide moieties, q is an integer from 3 to 40, X is the same or different and is selected from H and an aliphatic hydrocarbon group having 1 to 4 carbon atoms; R 3 are the same or different and are aliphatic divalent hydrocarbon groups containing 1 to 4 carbon atoms.
8. 1. A method for preparing a silicone polyether comprising the steps of: a) a polyorganohydrogensiloxane represented by the following formula: 【Chemistry 5】 During the ceremony, R is the same or different and is selected from H and a hydrocarbon group containing 1 to 18 carbon atoms, with the proviso that R contains less than 80 mole % H, m is an integer from 0 to 100, and n is an integer from 10 to 500; b) a polyoxyalkylene having the formula: 【Chemistry 6】 During the ceremony, R 1 are the same or different and are selected from aliphatic hydrocarbon groups containing 8 to 20 carbon atoms; R 2 is represented by the following formula: -(AO) q -X (In the formula, A are the same or different and are selected from aliphatic divalent hydrocarbon groups having 2 to 4 carbon atoms, provided that (AO) q contains at least three ethylene oxide moieties, q is an integer from 3 to 40, X is the same or different and is selected from H and an aliphatic hydrocarbon group having 1 to 4 carbon atoms; R 3 are the same or different and are aliphatic divalent hydrocarbon radicals containing 1 to 4 carbon atoms, R 4 are the same or different and are selected from alkenyl and alkynyl; and c) combining with a hydrosilylation catalyst.
9. i) combining components a), b), and c) in water to form an emulsion; 10. The method of claim 8, further comprising the step of: ii) conducting a hydrosilylation reaction between components a) and b) to form the silicone polyether reaction product in situ.
10. i) combining component a) and component b) in water by mixing to form an emulsion; 10. The method of claim 8 or 9, further comprising the step of: ii) adding component c) to the emulsion of step i) to form a silicone polyether reaction product in situ.
11. 11. The method of claim 8, 9 or 10, further comprising the step of adding an alcohol to the emulsion containing the silicone polyether reaction product to form an emulsion containing at least 10% by weight alcohol.
12. 12. The method of claim 8, 9, 10 or 11, wherein the emulsion comprising the silicone polyether reaction product is substantially free of surfactants.
13. 13. The method of claim 8, 9, 10, 11 or 12, wherein said step of combining component a) and component b) further comprises: d) combining an alkenyl-functional polyorganosiloxane.
14. 14. The method of claim 8, 9, 10, 11, 12 or 13, wherein the step of combining component a) and component b) further comprises e) combining an oil selected from at least one of i) a polydimethylsiloxane and ii) a hydrocarbon-based oil.
15. 15. The method of claim 14, wherein the hydrocarbon-based oil is selected from at least one of a mineral oil and a vegetable oil.
Citation Information
Patent Citations
Silicone polyether foam control agent
WO2020263379A1
Silicone polyether with branched pendant polyether group
WO2024242852A1
Cited By
Recyclable release liner and composite composition for preparing the same
JP2025517063A
Silicone polyether having branched chain-like pendant polyether groups
JP2026518145A