A negative electrode including a metal substrate and a protective layer

A self-healing protective layer composed of a copolymer, fluoropolymer additive, and lithium salt addresses dendrite formation in lithium metal secondary batteries, enhancing battery performance by reducing side reactions and extending cycle life.

JP2024545206AActive Publication Date: 2024-12-05UMICORE(BE)
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024535284
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-13
Filing Date
2022-12-13
Publication Date
2024-12-05
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

Existing lithium metal secondary batteries face issues with dendrite formation, leading to reduced coulombic efficiency, electrochemical stability, and shortened lifespan due to side reactions and electrolyte decomposition, with known protective layers failing to prevent dendrite penetration and film thickness limitations.

Method used

A protective layer comprising a copolymer, fluoropolymer additive, and lithium salt, which exhibits self-healing properties and improved mechanical strength, formed directly on a metal substrate, reducing dendrite growth and enhancing cycling efficiency.

Benefits of technology

The protective layer effectively minimizes dendrite growth, improves membrane conductivity, and extends the cycle life of the battery by providing anodic protection and reducing electrolyte depletion, resulting in improved coulombic efficiency and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545206000001_ABST
    Figure 2024545206000001_ABST
Patent Text Reader

Abstract

The present invention relates to an anode for a battery comprising a metal substrate and a protective layer disposed directly on at least a portion of the metal substrate, the protective layer comprising a copolymer obtainable by reaction between two or more monomers, a fluoropolymer additive, and a lithium salt. The inventors have demonstrated that the protective layer functions as a self-repairing film on the anode.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode for a battery comprising a metal substrate and a protective layer disposed directly on at least a portion of the metal substrate, a method for preparing the negative electrode, a battery comprising the negative electrode, and the use of the protective layer on the negative electrode. [Background technology]

[0002] As the development of small and lightweight electronic products, electronic devices, communication devices, etc. progresses rapidly and the need for electric vehicles to address environmental issues becomes increasingly important, there is a demand for improved performance of secondary batteries used as power sources for these products. Among them, lithium metal secondary batteries have been attracting attention as high-performance batteries due to their high energy density and high reference electrode potential.

[0003] Due to the high reactivity of lithium metal, side reactions between lithium and liquid electrolytes occur during the charging and discharging of the battery, which promotes the decomposition of the electrolyte. In addition, due to various reasons, non-uniformity of electron density may occur on the lithium metal surface during the operation of the battery. As a result, dendritic lithium dendrites are generated on the electrode surface, making the electrode surface very rough and possibly causing damage to the separator. These side reactions reduce the coulombic efficiency and / or electrochemical stability of the lithium metal battery, causing a decrease in the life of the lithium battery.

[0004] Therefore, various attempts have been made to stabilize the lithium metal and prevent or reduce side reactions between the electrolyte and the lithium metal.

[0005] Korean Patent Application Publication No. 20030042288(A) describes a lithium secondary battery capable of suppressing dendrite growth on the surface of a lithium metal negative electrode by a crosslinked polymer protective film formed on the surface of the lithium metal, the polymer being crosslinked 1,6-hexanediol diacrylate or a copolymer of 1,6-hexanediol diacrylate and oligo(ethylene glycol) diacrylate.

[0006] US 2016 / 0372743 A1 relates to a coating on a lithium metal anode to prevent direct contact between the lithium metal and a volatile liquid electrolyte. The coating consists of either a single layer polymer of PVDF homopolymer, ionic liquid and LiFSI, or a dual layer polymer coating having a first outer layer of PVDF, ionic liquid and LiFSI and a second inner layer of poly(styrene-acrylonitrile) and LiFSI.

[0007] However, a drawback of known protective layers remains dendrite penetration, which occurs as lithium is plated onto the anode during charging, and dendrites form and can break through the polymer film, thereby tearing it. The reduction in resistance due to discontinuities in the polymer film leads to localized areas of lower resistance and a greater degree of plating in the affected areas, which exacerbates dendrite formation. Dendrite formation is almost unavoidable in these systems, and the thin thickness of the polymer film (approximately 5-10 μm) makes dendrite formation in polymer protective layers highly likely. This results in a reduction in the coulombic efficiency, electrochemical stability and / or lifespan of the lithium metal battery.

[0008] There is therefore a need to provide a protective layer around the negative electrode that can reform around any holes or discontinuities created by dendrite formation. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Korean Patent Application Publication No. 20030042288(A) [Patent Document 2] US Patent Application Publication No. 2016 / 0372743(A1) [Patent Document 3] China Patent Application Publication No. 111162314(A) [Non-patent literature]

[0010] [Non-Patent Document 1] I. Gadwal, Macromol 2021, 1, 18-36 Summary of the Invention [Problem to be solved by the invention]

[0011] It is an object of the present invention to provide a negative electrode for a battery that includes a metal substrate and a protective layer disposed directly over at least a portion of the metal substrate.

[0012] It is a further object of the present invention to provide a method for preparing a negative electrode for a battery that includes a metal substrate and a protective layer disposed directly on at least a portion of the metal substrate.

[0013] A further object of the present invention is to provide an anode obtainable by the method for preparing an anode for a battery according to the present invention.

[0014] It is a further object of the present invention to provide a battery comprising an anode according to the present invention, a cathode, and an electrolyte composition.

[0015] A further object of the present invention is to provide the use of a protective layer on a negative electrode as a self-repairing film to reduce the growth of dendrites on the negative electrode and / or improve the cycling efficiency of the battery. [Means for solving the problem]

[0016] The object of the present invention is to a. a metal substrate; b. a protective layer disposed directly over at least a portion of the metal substrate, The protective layer is Copolymers obtainable by reaction between two or more monomers; A fluoropolymer additive; A lithium salt; A protective layer comprising: This is accomplished by providing a negative electrode for the battery comprising:

[0017] The inventors have surprisingly found that a protective layer comprising a copolymer, a fluoropolymer additive and a lithium salt functions as a self-healing polymer film, as demonstrated in the accompanying examples. The protective layer according to the invention is a mechanically robust polymer that also has self-healing properties, and is the result of a careful balance between polymer chain mobility, the amount of hydrogen-bonding motifs and the degree of crosslinking.

[0018] Without wishing to be bound by any theory, the inventors believe that the copolymers according to the present invention contain sufficient hydrogen bonds that can be broken and reformed at ambient temperatures resulting in the self-healing properties of the protective layer.

[0019] Although self-healing polymers are known in the art (see, for example, I. Gadwal, Macromol 2021, 1, 18-36), and self-healing polymer electrolytes based on dynamic chemical bonds and their application in secondary lithium batteries have been reported (China Patent Application Publication No. 111162314(A)), the inventors have demonstrated for the first time that the protective film according to the present invention, which exhibits self-healing properties, also provides effective anode protection, reducing lithium dendrite growth and minimizing electrolyte depletion. Furthermore, the protective layer according to the present invention has improved membrane conductivity, as well as enhanced mechanical and chemical properties, as demonstrated in the accompanying examples. Finally, the resulting protected anode also significantly extends the cycle life of the cell compared to an unprotected lithium metal-based reference cell, as shown in the following examples. [Brief description of the drawings]

[0020] [Figure 1] SEM (scanning electron microscope) images of each of the three polymer formulations 1-a, 1-b and 1-c (see also Table 1). [Diagram 2]Uncompensated resistance (Ru) measured for each Li-Li symmetric coin cell over 20 hours after cell construction for unprotected lithium anodes and protected anodes using polymer formulations 1-a, 1-b, and 1-c in 4.5 M LiFSI electrolyte in DME (see also Table 1). [Diagram 3] Uncompensated resistance (Ru) measured for each Li-Li symmetric coin cell over 20 hours after cell construction for unprotected lithium anodes and protected anodes using polymer formulations 2-a, 2-b, 2-c and 2-d in 4.5 M LiFSI electrolyte in DME (see also Table 2). [Figure 4] SEM micrographs of polymer films containing various amounts of HEAA, each of which was cut with a scalpel, imaged, and then immersed in 4.5 M LiFSI in DME overnight (16 h), before being rinsed in pure DME and imaged again. [Diagram 5] Total specific discharge capacity of Li-NMC pouch cells containing protected anodes with various PEG to HEAA ratios (cycling regime was C / 3 to D / 1, potential was held at the top and bottom of charging). [Figure 6] Coulombic efficiency of Li-NMC pouch cells containing protected anodes with various PEG to HEAA ratios (cycle regime was C / 3-D / 1, potential was held at the top and bottom of charging). [Figure 7A] (a) Polymer membrane conductivity without thermal annealing (4.5 M LiFSI in DME) versus TTE (3 to 1, v / v); (b) Polymer membrane conductivity with thermal annealing (4.5 M LiFSI in DME) versus TTE (3 to 1, v / v). [Figure 7B] (a) Polymer membrane conductivity without thermal annealing (4.5 M LiFSI in DME) versus TTE (3 to 1, v / v); (b) Polymer membrane conductivity with thermal annealing (4.5 M LiFSI in DME) versus TTE (3 to 1, v / v). [Figure 8]Total specific discharge capacity of Li-NMC pouch cells containing protected anodes with various PEG to HEAA ratios subjected to thermal annealing (cycling regime was C / 3-D / 1, potential was held at the top and bottom of charging). [Figure 9] Coulombic efficiency of Li-NMC pouch cells containing protected anodes with various PEG to HEAA ratios subjected to thermal annealing (cycling regime was C / 3-D / 1, potential was held at the top and bottom of charging). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] In order to enable the practice of the invention, preferred embodiments are described in detail in the drawings and the following detailed description. Although the invention has been described with reference to these specific preferred embodiments, it will be understood that the invention is not limited to these preferred embodiments. On the contrary, the invention encompasses numerous alternatives, modifications and equivalents, as will become apparent from a consideration of the following detailed description and the accompanying drawings.

[0022] The term "comprising" as used in the present specification and claims should not be interpreted as being limited to the means recited thereafter, nor does it exclude other elements or steps. It should be interpreted as specifying the presence of the recited features, integers, steps, or ingredients as mentioned, but without excluding the presence or addition of one or more other features, integers, steps, or ingredients, or groups thereof. Thus, the scope of the expression "a composition comprising components A and B" should not be limited to a composition consisting of components A and B only. It means that in the context of the present invention, the only relevant components of the composition are A and B. Thus, the terms "comprising" and "including" encompass the more restrictive terms "consisting essentially of" and "consisting of".

[0023] As used herein, "optional" or "optionally" means that the event or circumstance described thereafter may or may not occur, and the description includes instances where the event or circumstance occurs and instances where the event or circumstance does not occur.

[0024] As used herein, the term "alkyl" has its broadest meaning as generally understood in the art and can include moieties that are linear or branched, or combinations thereof. In particular, the term "alkyl", alone or in combination, refers to a linear or branched alkane-derived group, such as, for example, C F~G Alkyl defines a straight or branched alkyl group having F to G carbon atoms, for example C 1~4 Alkyl defines a straight or branched chain alkyl group having 1 to 4 carbon atoms, for example, methyl, ethyl, 1-propyl, 2-propyl (isopropyl), 15-butyl, 2-butyl, 2-methyl-2-propyl (tert-butyl), 2-methyl-1-propyl (isobutyl), etc.

[0025] The term "alkanediyl", alone or in combination, means a divalent radical derived from a straight or branched chain alkyl.

[0026] As used herein, the term “uncompensated resistance (R u The term "cell resistance" is defined as the resistance value including the cell resistance and any small additional resistances. The main contribution to the cell resistance comes from e.g. the ionic conductivity of the liquid electrolyte and / or the ionic conductivity of the polymer protective layer. Small resistance contributions are e.g. metallic parts such as cables / contacts.

[0027] negative electrode As described above, the first aspect of the present invention is a. a metal substrate; b. a protective layer disposed directly over at least a portion of the metal substrate, The protective layer is Formula (I)

[0028] [ka] (In the formula, R 1 =H or CH3, R 2 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 3 and R 3 is hydrogen or C 1~4 alkyl; X 1 =NH or O, and n is an integer selected from 5 to 150, preferably 8 to 100, and more preferably 10 to 50; Formula (II)

[0029] [ka] (In the formula, R 4 =H or CH3, R 5 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 6 and R 6 is hydrogen or C 1~4 alkyl; X 2 =NH or O, and X 3 =SH, NH2 or OH, and m is an integer selected from 1 to 10, preferably 1 to 5, more preferably m=1; A copolymer obtainable by reaction between a copolymer having a weight ratio of the first monomer to the second monomer of 1:5-8:1 (w / w); a fluoropolymer additive selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), vinylidene fluoride-chlorotrifluoroethylene copolymer, ethylene tetrafluoroethylene copolymer, polychlorotrifluoroethylene, vinylidene fluoride-pentafluoropropylene copolymer, propylene tetrafluoroethylene copolymer, ethylene chlorotrifluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, and combinations thereof; A lithium salt; Including, A protective layer having a weight ratio of copolymer to fluoropolymer additive of 1:5 to 8:1 (w / w); The objective of the present invention is to provide a negative electrode (i.e., anode) for the battery, comprising:

[0030] metal base material One embodiment of the present invention is an anode according to the present invention, comprising a metal substrate. In a preferred embodiment, the metal substrate comprises a conductive metal, preferably stainless steel, copper, nickel, iron, cobalt, lithium, lithium alloy or a combination thereof, more preferably stainless steel, copper, nickel, lithium, lithium alloy or a combination thereof. In a more preferred embodiment, the metal substrate is a lithium metal substrate or a lithium metal alloy substrate, preferably a lithium metal substrate. As will be understood by those skilled in the art, the metal substrate can be a metal deposited on a supporting foil, such as stainless steel, copper, nickel, iron, cobalt, or a lithium or lithium alloy layer made as a foil or as a layer deposited on a surface.

[0031] Copolymer One embodiment of the present invention comprises: Formula (I)

[0032] [ka] (In the formula, R 1 =H or CH3, R 2 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 3 and R 3 is hydrogen or C 1~4 alkyl; X 1 =NH or O, and n is an integer selected from 5 to 150, preferably 8 to 100, and more preferably 10 to 50; Formula (II)

[0033] [ka] (In the formula, R 4 =H or CH3, R 5 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 6 and R 6 is hydrogen or C 1~4 alkyl; X 2 =NH or O, and X 3 =SH, NH2 or OH, and m is an integer selected from 1 to 10, preferably 1 to 5, more preferably m=1; It is a copolymer that can be obtained by the reaction between

[0034] One embodiment of the present invention is a compound of formula (I) 1 is H or CH3, preferably H; R 2 is C 2~6 Alkanediyl, preferably C 2~4 Alkanediyl, more preferably C2 alkanediyl, and alkanediyl is a halide, C1~4 Alkyl, CF3 or OR 3 and R 3 is hydrogen or C 1~4 alkyl; X 1 =NH or O, preferably O, and n is an integer selected from 5 to 150, preferably 8 to 100, more preferably 10 to 50.

[0035] A preferred embodiment of the present invention is a first monomer according to the present invention, the first monomer having formula (III)

[0036] [ka] (wherein o is an integer selected from 5 to 150, preferably 8 to 130, more preferably 10 to 100). In particular, the first monomer represented by formula (III) is poly(ethylene glycol) diacrylate (PEGDA).

[0037] A preferred embodiment of the present invention is a first monomer according to the present invention, which has a number average molecular weight M of more than 50 g / mol, preferably more than 100 g / mol, more preferably more than 200 g / mol, even more preferably more than 550 g / mol, most preferably more than 700 g / mol. n A preferred embodiment of the present invention is a first monomer according to the present invention, which has a number average molecular weight M of less than 20,000 g / mol, preferably less than 7,000 g / mol, more preferably less than 4,000 g / mol, even more preferably less than 2,000 g / mol, and most preferably less than 1,000 g / mol. nA preferred embodiment of the present invention is a first monomer according to the present invention, the first monomer having a number average molecular weight M of 50 to 20,000 g / mol, preferably 100 to 7,000 g / mol, more preferably 200 to 4,000 g / mol, even more preferably 550 to 2,000 g / mol, most preferably 700 to 1,000 g / mol. n Particular examples have number average molecular weights M of 250 g / mol, 575 g / mol, 700 g / mol, 4,000 g / mol or 6,000 g / mol. n A preferred example of the first monomer according to the invention is PEGDA having a number average molecular weight M of 250 g / mol, 575 g / mol or 700 g / mol, preferably 700 g / mol. n PEGDA having a variety of number average molecular weights as described above can be purchased commercially from suppliers such as Sigma-Aldrich.

[0038] As demonstrated in the examples below, the first monomer according to the invention, in particular PEGDA, improves the lithium ion conductivity of the copolymer according to the invention and / or of the protective layer according to the invention.

[0039] One embodiment of the present invention is a second monomer represented by formula (II), wherein R 4 =H or CH3, preferably H; R 5 is C 2~6 Alkanediyl, preferably C 2~4 Alkanediyl, more preferably C2 alkanediyl, and alkanediyl is a halide, C 1~4 Alkyl, CF3 or OR 6 and R 6 is hydrogen or C 1~4 alkyl; X 2 =NH or O, preferably NH; X 3 =SH, NH2 or OH, preferably OH; m is an integer selected from 1 to 10, preferably 1 to 5, and most preferably m=1.

[0040] A preferred embodiment of the present invention is a second monomer according to the present invention, the second monomer having formula (IV)

[0041] [ka] The second monomer, particularly represented by formula (IV), is N-(2-hydroxyethyl)acrylamide (HEAA). HEAA can be purchased commercially from suppliers such as Sigma-Aldrich and TCI Chemicals.

[0042] As demonstrated in the following examples, the introduction of a second monomer according to the present invention, particularly N-(2-hydroxyethyl)acrylamide (HEAA), into a copolymer provides the copolymer with self-healing properties. The first monomer according to the present invention comprises a hydrogen bond acceptor, such as a carbonyl functional group of the first monomer represented by formula (I), preferably an ester functional group of the first monomer represented by formula (III). The second monomer according to the present invention comprises a hydrogen bond acceptor, such as a carbonyl functional group of the second monomer represented by formula (II), preferably an amide functional group of the second monomer represented by formula (IV). The second monomer according to the present invention comprises a hydrogen bond donor, such as a substituent X of the second monomer represented by formula (II). 3 The hydrogen bond donor present in the second monomer may be a hydrogen bond donor, such as a thiol, amino or hydroxyl functional group, preferably a hydrogen of a hydroxyl group of the second monomer represented by formula (IV). The inventors believe that the hydrogen bond donor present in the second monomer may form a hydrogen bond with a hydrogen bond acceptor present in a further second monomer according to the invention and / or a hydrogen bond acceptor present in the first monomer according to the invention. The inventors believe that the hydrogen bonding properties of the copolymer result in the self-healing properties of the copolymer and / or the protective layer. The hydrogen bonds present in the copolymer according to the invention have a relatively weak bond strength (1.9-6.9 kcal.mol -1), which means that their hydrogen bonds can be broken and reformed at ambient temperature.

[0043] As will be understood by those skilled in the art, the copolymer according to the present invention can be obtained by a crosslinking step (i.e. radical polymerization) of the corresponding vinyl monomer, for example the first monomer according to the present invention and the second monomer according to the present invention. In an embodiment of the present invention, the initiator that can be used for the radical polymerization depends on the crosslinking reaction, and all known photoinitiators or thermal initiators can be used, and preferably photoinitiators are used. Examples of photoinitiators include benzoin, benzoin ethyl ether, benzoin isobutyl ether, alpha methyl benzoin ethyl ether, benzoin phenyl ether acetophenone, dimethoxyphenylacetophenone, 2,2-diethoxyacetophenone, 1,1-dichloroacetophenone, trichloroacetophenone, benzophenone, p-chlorobenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-2-methylpropiophenone, benzoyl benzoate, anthraquinone, 2-ethylanthraquinone, 2-chloroanthraquinone, 2-methyl-1-(4-methylthiophenyl)-morpholinopropanone-1,2-hydroxy-2-methyl-1-phenylpropan-1-one (Darocure 1173), 2-methyl-4'-(methylthio)-2-morpholinopropiophenone (Irgacure 907), phenylbis(2,4,6-trimethylbenzoyl)-phosphine oxide (Irgacure 819), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,1-hydroxycyclohexyl phenyl ketone (Irgacure 184), Michler's ketone, benzyl dimethyl ketal, thioxanthone, isopropyl thioxanthone, chlorothioxanthone, benzyl disulfide, butanediol, carbazole, fluorenone, alpha acyl oxime ester, and combinations thereof. Examples of thermal initiators include peroxide (-OO-) series, benzoyl peroxide, cumyl hydroperoxide, and the like. Azo compounds (-N=N-) series, azobisisobutyronitrile, azobisovaleronitrile, and the like may also be used.In a preferred embodiment of the invention, the photoinitiator is phenylbis-(2,4,6-trimethylbenzoyl)-phosphine oxide (Irgacure 819) or 2-methyl-4'-(methylthio)-2-morpholinopropiophenone (Irgacure 907), preferably Irgacure 819.

[0044] The content of the initiator is not particularly limited in the present invention, but is preferably within a range that does not affect the properties of the copolymer according to the present invention, the properties of electrodes such as the negative electrode or positive electrode, and the properties of the liquid electrolyte present in the battery. In one embodiment of the present invention, the initiator is used in a range of 1 to 15 wt % based on the total weight of the copolymer, preferably in a range of 1 to 5 wt %, more preferably in a range of 2 to 4 wt % based on the total weight of the copolymer.

[0045] In an embodiment of the present invention, the crosslinking step giving the copolymer according to the present invention is carried out in an organic liquid capable of dissolving the first monomer according to the present invention, the second monomer according to the present invention and / or the copolymer according to the present invention. Preferably, the organic liquid is a non-aqueous organic liquid. In the present invention, as non-aqueous organic liquid, known liquids such as carbonates, esters, ethers, ketones, alcohols or aprotic liquids may be used. For example, the aprotic organic liquid is selected from the group consisting of N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxene, diethyl ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triesters, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, ethyl propionate, and combinations thereof. Preferred examples of organic liquids are acetonitrile or tetrahydrofuran.

[0046] In an embodiment of the present invention, the crosslinking step includes applying heat or irradiating with active energy rays, where the thermal crosslinking may use a method for heating, and the active energy rays may be by irradiating with far infrared rays, ultraviolet rays or electron beams.

[0047] In an embodiment of the present invention, the crosslinking step is carried out by thermal crosslinking or photocrosslinking, preferably photocrosslinking. In an embodiment of the present invention, thermal crosslinking can be carried out at a temperature of 50°C to 200°C, preferably at a temperature of 80°C to 110°C, and the heating time for crosslinking is 30 minutes to 48 hours, more preferably 8 hours to 24 hours. If the heating temperature and time are less than the above ranges, crosslinking is difficult to be formed sufficiently, and if the heating temperature and time exceed the above ranges, side reactions may occur or material stability may decrease. In a preferred embodiment of the present invention, photocrosslinking including active energy ray irradiation is carried out for 10 seconds to 5 hours, preferably 1 minute to 1 hour, and most preferably 2 minutes to 10 minutes. In a preferred embodiment of the present invention, photocrosslinking is carried out at a temperature of 5°C to 60°C, preferably 10°C to 50°C, and most preferably 20°C to 40°C. If the time of active ray irradiation is less than the above ranges, crosslinking is difficult to be formed sufficiently, and if it exceeds the above ranges, side reactions may occur or material stability may decrease.

[0048] As will be understood by the person skilled in the art, the copolymer can be obtained by reaction of at least two monomers, being a first monomer represented by formula (I) and a second monomer represented by formula (II), but is not limited to being obtained by reaction between only two different monomers, but can also be obtained, for example, by reaction between three monomers, in particular a first monomer according to the invention, a second monomer according to the invention, and a third monomer represented by formula (V) or formula (VI), the third monomer being different from the first and second monomers:

[0049] [ka] (In the formula, R 7 is H or CH3, R 8 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 9 and R 9 is hydrogen or C1~4 alkyl; X 4 =NH or O, and p is an integer selected from 5 to 150, preferably 8 to 100, and more preferably 10 to 50; or

[0050] [ka] (In the formula, R 10 is H or CH3, R 11 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 12 and R 12 is hydrogen or C 1~4 alkyl; X 5 =NH or O, and X 6 =SH, NH2 or OH, and q is an integer selected from 1 to 10, preferably 1 to 5, more preferably q=1).

[0051] A preferred embodiment of the present invention is a copolymer obtainable by reaction between up to two monomers, the first monomer being represented by formula (I) and the second monomer being represented by formula (II).

[0052] A highly preferred embodiment of the present invention is a copolymer obtainable by reaction between up to two monomers, the first being poly(ethylene glycol) diacrylate and the second being 2-hydroxyethylacrylamide.

[0053] In a preferred embodiment, the weight ratio of the first monomer to the second monomer is 1:5-8:1 (w / w), preferably 1:3-7:1 (w / w), more preferably 1:2-5:1 (w / w), and most preferably 1:2-2:1 (w / w).

[0054] In a preferred embodiment, the copolymer is present in an amount of more than 20% by weight based on the total weight of the protective layer, preferably more than 30% by weight based on the total weight of the protective layer, and most preferably more than 35% by weight. In a preferred embodiment, the copolymer is present in an amount of less than 80% by weight based on the total weight of the protective layer, preferably less than 70% by weight based on the total weight of the protective layer, and most preferably less than 60% by weight. In a preferred embodiment, the copolymer is present in an amount in the range of 20-80% by weight based on the total weight of the protective layer, preferably in the range of 30-70% by weight based on the total weight of the protective layer, and more preferably in the range of 35-60% by weight.

[0055] A particular example of a copolymer according to the invention is a copolymer of formula (VII)

[0056] [ka] (wherein o is an integer selected from 5 to 150, preferably 8 to 100, more preferably 10 to 50, and r, s, and t are integers independently selected from 1 to 10, preferably 2 to 8, most preferably 3 to 6. However, as will be understood by one skilled in the art, the copolymer according to the present invention is not limited to formula (VII), which is shown as an exemplary embodiment.

[0057] In a highly preferred embodiment of the invention, the copolymer according to the invention, and therefore the protective layer according to the invention, has self-healing properties, as demonstrated in the accompanying examples.

[0058] In a preferred embodiment of the present invention, the copolymer and / or protective layer according to the present invention is subjected to a thermal annealing step. As will be understood by those skilled in the art, thermal annealing is a common process used in materials chemistry to relieve stress, improve uniformity and improve contact with the substrate. In particular, thermal annealing involves increasing the temperature T of the part coated by the coating from initially room temperature to a maximum (operating) temperature T maxThe thermal annealing step is carried out at a temperature in the range of 40-100° C., preferably in the range of 50-90° C., more preferably in the range of 60-80° C., after UV curing of the copolymer, and / or the duration of the thermal annealing is between 5 min and 10 h, preferably between 15 min and 5 h, most preferably between 30 min and 90 min. In a very preferred embodiment, the thermal annealing step according to the invention is carried out in dry air. The inventors have surprisingly found that the thermal annealing step improves the conductivity of the copolymer. In addition, each copolymer subjected to the thermal annealing step appears more homogeneous and has better contact with the lithium metal surface. Furthermore, the inventors have found that the charge transfer resistance (R ct ) was found to decrease.

[0059] Fluoropolymer Additives As mentioned above, the protective layer according to the present invention comprises a fluoropolymer additive, which is selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymers, poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), vinylidene fluoride-chlorotrifluoroethylene copolymers, ethylene-tetrafluoroethylene copolymers, polychlorotrifluoroethylene, vinylidene fluoride-pentafluoropropylene copolymers, The fluoropolymer additive is selected from the group consisting of propylene tetrafluoroethylene copolymer, ethylene chlorotrifluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethylvinyl ether-tetrafluoroethylene copolymer, and combinations thereof, preferably, the fluoropolymer additive is polyvinylidene fluoride or poly(vinylidene fluoride-co-hexafluoropropylene), most preferably poly(vinylidene fluoride-co-hexafluoropropylene).

[0060] In a preferred embodiment, the fluoropolymer additive is present in an amount of less than 75 wt% based on the total weight of the protective layer, preferably less than 50 wt% based on the total weight of the protective layer, and most preferably less than 20 wt%. In a preferred embodiment, the fluoropolymer additive is present in an amount of more than 0.05 wt% based on the total weight of the protective layer, preferably more than 5 wt% based on the total weight of the protective layer, and most preferably more than 10 wt%. In a preferred embodiment, the fluoropolymer additive is present in an amount of 0.05-75 wt% based on the total weight of the protective layer, preferably 5-50 wt% based on the total weight of the protective layer, and more preferably 10-20 wt%.

[0061] In a preferred embodiment of the invention, the weight ratio of copolymer to fluoropolymer additive is 1:5-8:1 (w / w), preferably 1:2-5:1 (w / w), more preferably 1:2-4:1 (w / w), most preferably 2:1-4:1 (w / w).

[0062] In one embodiment of the present invention, the fluoropolymer additive has a weight average molecular weight M of more than 1,000 g / mol, preferably more than 10,000 g / mol, more preferably more than 100,000 g / mol, and most preferably more than 300,000 g / mol. w In one embodiment of the present invention, the fluoropolymer additive has a weight average molecular weight M of less than 1,000,000 g / mol, preferably less than 800,000 g / mol, more preferably less than 750,000 g / mol, and most preferably less than 600,000 g / mol. w In one embodiment of the present invention, the fluoropolymer additive has a weight average molecular weight M of 1,000 to 1,000,000 g / mol, preferably 10,000 to 800,000 g / mol, more preferably 100,000 to 750,000 g / mol, and most preferably 300,000 to 600,000 g / mol. w A preferred example of a fluoropolymer additive, in particular poly(vinylidene fluoride-co-hexafluoropropylene), has a weight average molecular weight M of about 400,000 g / mol. w or a weight average molecular weight M of about 455,000 g / mol w Fluoropolymer additives such as poly(vinylidene fluoride-co-hexafluoropropylene) can be purchased commercially from suppliers such as Sigma-Aldrich.

[0063] In one embodiment of the present invention, the fluoropolymer additive has a number average molecular weight M of more than 250 g / mol, preferably more than 2,500 g / mol, more preferably more than 25,000 g / mol, and most preferably more than 75,000 g / mol. n In one embodiment of the present invention, the fluoropolymer additive has a number average molecular weight M of less than 250,000 g / mol, preferably less than 200,000 g / mol, more preferably less than 190,000 g / mol, and most preferably less than 150,000 g / mol. nIn one embodiment of the present invention, the fluoropolymer additive has a number average molecular weight M of 250 to 250,000 g / mol, preferably 2,500 to 400,000 g / mol, more preferably 25,000 to 190,000 g / mol, and most preferably 75,000 to 150,000 g / mol. n A preferred example of a fluoropolymer additive, particularly poly(vinylidene fluoride-co-hexafluoropropylene), has a number average molecular weight M of about 130,000 g / mol. n or a number average molecular weight M of about 110,000 g / mol n Fluoropolymer additives such as poly(vinylidene fluoride-co-hexafluoropropylene) can be purchased commercially from suppliers such as Sigma-Aldrich.

[0064] The inventors have found that the addition of a fluoropolymer additive increases the conductivity of the protective layer, improves the wetting of the protective layer, and allows for the printing of a uniform film of the protective layer, as demonstrated in the accompanying examples.

[0065] Lithium salts As mentioned above, the protective layer according to the present invention comprises a lithium salt.

[0066] In one embodiment of the present invention, the lithium salt is Li2CO3, Li2O, Li2C2C4, LiOH, LiX 7 ,ROCO2Li,HCOLi,R 13 OLi, Li2O, Li2C2C4, (R 13 OCO2Li)2, (CH2OCO2Li)2, Li2S, LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2) 3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, LiB(C2O4)2 (in the formula, R 13 = Hydrocarbon and X 7=F, Cl, I or Br) and combinations thereof, preferably selected from the group consisting of LiSCN, LiN(CN)2, LiClO4, LiI, LiBF4, LiAsF6, LiCF3SO3, LiCF3(SO3)2, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, LiB(C2O4)2 and combinations thereof, more preferably the lithium salt is LiN(SO2CF3)2 or LiN(SO2F)2, and most preferably the lithium salt is LiN(SO2F)2.

[0067] In a preferred embodiment of the present invention, the amount of lithium salt is more than 5 wt% based on the total weight of the protective layer, preferably more than 10 wt% based on the total weight of the protective layer, most preferably more than 40 wt% based on the total weight of the protective layer. In a preferred embodiment of the present invention, the amount of lithium salt is less than 70 wt% based on the total weight of the protective layer, preferably less than 65 wt% based on the total weight of the protective layer, most preferably less than 60 wt%. In a preferred embodiment of the present invention, the amount of lithium salt is 5-70 wt% based on the total weight of the protective layer, preferably 10-65 wt% based on the total weight of the protective layer, more preferably 40-60 wt%.

[0068] The inventors have found that the addition of lithium salt improves the lithium ion conductivity of the protective layer and prevents the protective layer from depleting the lithium ions present in the electrolyte. Furthermore, the addition of a higher lithium salt content to the protective layer reduces the uncompensated resistance R u decreases.

[0069] protective layer In one embodiment of the present invention, the protective layer has a thickness of 1 to 10 μm, preferably 2 to 7 μm, and more preferably 3 to 6 μm.

[0070] In one embodiment of the present invention, the protective layer is disposed directly on at least a portion of the metal substrate, and preferably, the protective layer is disposed directly on the entire surface of the metal substrate. As will be understood by those skilled in the art, the negative electrode according to the present invention comprises a protective layer according to the present invention, and the protective layer forms an outer layer on the metal substrate. In other words, the protective layer is coated on a portion of the surface of the metal substrate, i.e., the protective layer forms a coating on a portion of the surface of the metal substrate, preferably on the entire surface of the metal substrate.

[0071] In a preferred embodiment of the invention, the protective layer according to the invention has an ionic conductivity of more than 0.01 mS / cm, preferably more than 0.015 mS / cm, more preferably more than 0.05 mS / cm. In a preferred embodiment of the invention, the protective layer has an ionic conductivity of less than 0.5 mS / cm, preferably less than 0.2 mS / cm, more preferably less than 0.1 mS / cm. In a preferred embodiment of the invention, the protective layer according to the invention has an ionic conductivity in the range of 0.01-0.5 mS / cm, preferably in the range of 0.015-0.2 mS / cm, most preferably in the range of 0.05-0.1 mS / cm. The ionic conductivity of the protective layer is measured by the uncompensated resistance R by electronic impedance spectroscopy (EIS) in a symmetric Li-Li cell. u and ionic conductivity is measured after cell construction (meaning, for example, in a battery including a negative electrode and electrolyte composition according to the present invention).

[0072] A further aspect of the present invention is a method for preparing a protective layer according to the present invention, comprising the following steps: i) adding a first monomer as defined above, a second monomer as defined above, an initiator as defined above, a lithium salt as defined above and a fluoropolymer additive as defined above to an organic liquid as defined above; ii) subjecting the mixture obtained in step i) to a crosslinking step as defined above; iii) optionally subjecting the crosslinked mixture of step ii) to a thermal annealing step as defined above; Includes.

[0073] A further aspect of the present invention is a protective layer obtainable by the process for preparing a protective layer according to the present invention.

[0074] others A further aspect of the present invention is a negative electrode according to the present invention, a. a metal substrate as defined above; b. a protective layer obtainable by the method for preparing a protective layer according to the invention, disposed directly on at least a portion of the metal substrate; Includes.

[0075] A further aspect of the present invention is a method for producing a process comprising the steps of: i) adding a first monomer as defined above, a second monomer as defined above, an initiator as defined above, a lithium salt as defined above and a fluoropolymer additive as defined above to an organic liquid as defined above; ii) coating the mixture obtained in step i) onto at least a portion of a metal substrate, preferably onto the entire surface of the metal substrate; iii) subjecting the coated metal substrate of step ii) to a crosslinking step as defined above; iv) optionally subjecting the crosslinked coated metal substrate of step iii) to a thermal annealing step as defined above; A method for preparing a negative electrode for a battery comprising:

[0076] In one embodiment of the present invention, the amount of solids present in the mixture obtained in step i) as defined above (i.e. the sum of the first monomer, the second monomer, the initiator, the lithium salt and the fluoropolymer) is greater than 1% by weight based on the total weight of the solids and the organic liquid, preferably greater than 2% by weight based on the total weight of the solids and the organic liquid, most preferably greater than 3% by weight. In one embodiment of the present invention, the amount of solids (i.e. the sum of the first monomer, the second monomer, the initiator, the lithium salt and the fluoropolymer) is less than 10% by weight based on the total weight of the solids and the organic liquid, preferably less than 8% by weight based on the total weight of the solids and the organic liquid, most preferably less than 5% by weight. In one embodiment of the present invention, the amount of solids (i.e. the sum of the first monomer, the second monomer, the initiator, the lithium salt and the fluoropolymer) is between 1 and 10% by weight based on the total weight of the solids and the organic liquid, preferably between 2 and 8% by weight based on the total weight of the solids and the organic liquid, most preferably between 3 and 5% by weight.

[0077] The coating step can be carried out using methods used in conventional wet processes as understood by those skilled in the art, for example, spin coating, spray coating, doctor blade coating, dip coating.

[0078] Optionally, after the coating step and / or after the thermal annealing step, a drying step is performed at a temperature equal to or higher than the boiling point of the organic liquid and equal to or higher than the glass transition temperature T of the copolymer according to the invention and / or the protective layer according to the invention. g It may be suitably carried out at the following temperatures: A drying step may also be carried out to remove any liquid remaining on the surface of the metal substrate and at the same time improve the adhesion of the copolymer according to the invention and / or the protective layer according to the invention.

[0079] A further aspect of the present invention is an anode obtainable by the method for preparing an anode for a battery according to the present invention.

[0080] battery A further aspect of the present invention is a. a negative electrode according to the invention or obtainable by the method for preparing a negative electrode for a battery according to the invention; b. a positive electrode; c. an electrolyte composition, preferably disposed between the positive and negative electrodes; d. optionally, a separator; A battery comprising:

[0081] In a preferred embodiment of the invention, the battery is a lithium metal battery, preferably a lithium metal secondary battery.

[0082] positive electrode The material of the positive electrode (i.e., cathode) is not particularly limited, and examples thereof include transition metal compounds having a structure capable of diffusing lithium ions, or specialized metal compounds thereof, and oxides of lithium. In particular, LiCoO2, LiNiO2, LiMnO4, LiFePO4, etc. may be mentioned. A preferred positive electrode material is a mixed metal oxide containing lithium, nickel, and optionally manganese, cobalt, and / or aluminum.

[0083] In a preferred embodiment of the invention, the positive electrode comprises a positive electrode material selected from the group consisting of lithium nickel-manganese-cobalt oxide, lithium nickel-manganese oxide, lithium nickel-cobalt-aluminum oxide, lithium cobalt oxide, lithium iron phosphate, lithium iron manganese phosphate, lithium iron cobalt phosphate, lithium sulfide, sulfur and aluminum, preferably the positive electrode material is lithium nickel-manganese-cobalt oxide or lithium nickel-cobalt-aluminum oxide.

[0084] The positive electrode can be formed by pressing the positive electrode material defined above together with a known conductive auxiliary or binder, or the positive electrode active material together with a known conductive auxiliary or binder, into an organic liquid such as pyrrolidone, which can be obtained by applying the mixture and coating it on a current collector such as aluminum foil, followed by drying.

[0085] electrolyte composition In one embodiment of the present invention, the electrolyte composition is a liquid electrolyte composition.

[0086] In one embodiment of the invention, the electrolyte composition comprises an additional lithium salt and an additional organic liquid, preferably an additional non-aqueous organic liquid, more preferably an additional aprotic non-aqueous organic liquid.

[0087] In a preferred embodiment of the invention, the further lithium salt is Li2CO3, Li2O, Li2C2O4, LiOH, LiX 8 ,ROCO2Li,HCOLi,R 14 OLi, Li2O, Li2C2O4, (ROCO2Li)2, (CH2OCO2Li)2, Li2S, LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, Li C(CF3SO2)3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, LiB(C2O4)2 (in the formula, R 14 = Hydrocarbon and X 8 =F, Cl, I or Br), preferably selected from the group consisting of LiSCN, LiN(CN)2, LiClO4, LiI, LiBF4, LiAsF6, LiCF3SO3, LiCF3(SO3)2, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, LiB(C2O4)2 and combinations thereof, more preferably the lithium salt is LiN(SO2CF3)2 or LiN(SO2F)2, and most preferably the lithium salt is LiN(SO2F)2.

[0088] In a highly preferred embodiment, the further lithium salt and the above lithium salt are the same lithium compound.

[0089] As will be understood by a person skilled in the art, the lithium salt according to the present invention is present in the protective layer according to the present invention, while the further lithium salt according to the present invention is present in the electrolyte composition according to the present invention.

[0090] In a preferred embodiment of the invention, the further organic liquid is N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethylsulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxene, diethyl ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethanamide, methyl ether ... Preferably, the further organic liquid comprises a non-fluorinated liquid selected from the group consisting of 1,2-dimethoxyethane or 1,2-diethoxyethane, most preferably 1,2-dimethoxyethane.

[0091] In a preferred embodiment, the further organic liquid further comprises a fluorinated liquid, which is a fluorinated ether, a fluorinated carbonate or a fluorinated aromatic compound. In a preferred embodiment, the fluorinated liquid is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl)ether (BTFE), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), tris(2,2,2-trifluoroethyl)orthoformate (TFEO), methoxynonafluorobutane (MOFB), ethoxynonafluorobutane (EOFB), di(2,2,2-trifluoroethyl)carbonate (DTFEC), tris(2,2,2-trifluoroethyl)orthoformate (TFEO), tris(hexafluoroisopropyl)orthoformate (THFiPO), tris(2,2-difluoroethyl)orthoformate (TD FEO), bis(2,2,2-trifluoroethyl)methyl orthoformate (BTFEMO), tris(2,2,3,3,3-pentafluoropropyl) orthoformate (TPFPO), tris(2,2,3,3-tetrafluoropropyl) orthoformate (TTPO) and combinations thereof, preferably the fluorinated liquid is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl) ether (BTFE) or 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), and most preferably 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE).

[0092] In a preferred embodiment of the invention, the volume ratio of non-fluorinated liquid to fluorinated liquid is from 6:1 to 1:2 (vol / vol), preferably from 5:1 to 1:1 (vol / vol), most preferably from 4:1 to 2:1 (vol / vol).

[0093] As will be understood by the person skilled in the art, the organic liquid according to the present invention is the liquid used in the crosslinking step to give the copolymer according to the present invention, whereas the further organic liquid according to the present invention is the liquid present in the electrolyte composition according to the present invention.

[0094] In one embodiment of the invention, the concentration of the further lithium salt in the further organic liquid is greater than 0.2 M, preferably greater than 2 M, most preferably greater than 4 M. In one embodiment of the invention, the concentration of the further lithium salt in the further organic liquid is less than 10 M, preferably less than 8 M, most preferably less than 6 M. In one embodiment of the invention, the concentration of the further lithium salt in the further organic liquid is in the range 0.2-10 M, preferably in the range 2-8 M, most preferably in the range 4-6 M.

[0095] Separator In order to prevent short circuit between the positive and negative electrodes, a separator is usually inserted between the cathode and the anode. The material and shape of the separator are not particularly limited, but it is preferable that the separator is an insulating and chemically stable material that can easily pass the electrolyte composition. Examples of the separator include microporous films and sheets made of various polymer materials. Specific examples of the polymer materials include polyolefin polymers, nitrocellulose, polyacrylonitrile, polyvinylidene fluoride, polyethylene, and polypropylene. From the viewpoint of electrochemical stability and chemical stability, polyolefin polymers are preferable.

[0096] others In a preferred embodiment of the invention, the cells of the invention have a coulombic efficiency of at least 93%, preferably at least 94%, more preferably at least 95%, even more preferably at least 96%, even more preferably at least 97%, and most preferably at least 98%. Coulombic efficiency is evaluated using the following general formula:

[0097]

number

[0098] use A further aspect of the present invention provides the use of a protective layer as a self-repairing film on a negative electrode comprising a metal substrate, the protective layer being according to the present invention and the metal substrate being according to the present invention.

[0099] A further aspect of the present invention provides the use of a protective layer for reducing dendrite growth on a negative electrode comprising a metal substrate, the protective layer being according to the present invention and the metal substrate being according to the present invention.

[0100] A further aspect of the present invention provides the use of a protective layer on a negative electrode comprising a metal substrate for improving the cycling efficiency of a battery comprising the negative electrode, preferably the cycling efficiency is improved by 20%, the protective layer being according to the present invention, preferably the protective layer being subjected to a thermal annealing step as defined above, the metal substrate being according to the present invention. EXAMPLES

[0101] The invention is further illustrated in the following examples.

[0102] Description of cell preparation and test method All coin cells tested were of the CR2032 type. The cells were prepared by stacking the following in that order on top of each other: cathode casing, cathode (pre-soaked in electrolyte), Cellguard separator, 50 μL electrolyte drop, anode, spacer, wave spring, and anode casing. A pressure of 80 kg / cm was applied using an MTI manual crimping machine. 2 Pressure welding was performed at a pressure of 1000 MPa.

[0103] Li-Li pouch cells were prepared according to the following: format = 1Li (58 x 58 mm) / 1Sep (62 x 62 mm) / 1Li (50 x 50 mm), "nominal capacity" = 0.1 Ah, separator = alumina coated Targray SH220W22, lithium = 100 μm thick (coated or uncoated), electrolyte loading = 3.00 μL mAh.-1 (i.e., 0.3 mL), C rate = C / 5 D / 5 (standard regime) or C / 3 D / 1, with potential hold (new regime), cycle temperature = 25°C.

[0104] Li-NMC pouch cells were prepared according to the following: format = 3Li (58x58mm) / 4Sep (62x62mm) / 2NMC (56x54mm), nominal capacity = 0.48Ah (cathode surface capacity = 4mAh cm -2 ), separator = Targray SH220W22 coated with alumina, lithium = 100 μm thick, electrolyte added = 2.00 μL mAh -1 (i.e., 0.97 mL) or 1.75 μL mAh -1 i.e., 0.85 mL), C rate = C / 5 D / 5 (standard regime) or C / 3 D / 1, with potential hold (new regime), cycle temperature = 25 °C. The NMC cathode contained LiNi 0.6 Mn 0.2 Co 0.2 It contains O2, carbon black and PVDF in a weight ratio of 92:4:4.

[0105] Uncompensated resistance R u is measured by electrochemical impedance spectroscopy (Nyquist plot) of Li-Li symmetric coin cells containing lithium metal anodes uncoated and coated with a protective layer. Frequencies between 1 MHz and 1 Hz were applied in the tests.

[0106] The ionic conductivity of the protective layer was measured by the uncompensated resistance R by electronic impedance spectroscopy (EIS) in a symmetric Li-Li cell. u The ionic conductivity is measured after the cell is constructed.

[0107] Cross sections of the protective layer were analyzed using a scanning electron microscope (SEM). A JEOL benchtop SEM was used (samples were imaged in the SEM under vacuum, secondary electron imaging, probe current set to standard, accelerating voltage of the SEM column).

[0108] The polymer-protected anode is prepared by adding the monomer, lithium salt, initiator and fluoropolymer additive in an organic solvent in the amounts specified in the table below. These mixtures are coated onto the anode and subjected to UV curing with Irgacure 819 as a photoinitiator for 5 minutes UV curing time. Optionally, thermal annealing of the polymer is performed after UV curing the polymer-protected anode at 70° C. for 1 hour. EXAMPLES

[0109] To evaluate the effect of the amount of fluoropolymer additive, the following polymer formulations 1-a, 1-b and 1-c were prepared (see Table 1, M of PEGDA = 700 g / mol). n Poly(ethylene glycol) diacrylate with LiTFSI=LiN(SO2CF3)2, PVDF-HFP=poly(vinylidene fluoride-co-hexafluoropropylene), THF=tetrahydrofuran).

[0110] [Table 1]

[0111] FIG. 1 shows the effect of decreasing the weight percent of the fluoropolymer additive in the polymer formulation on the film continuity, showing that while coatings of formulations 1-a and 1-b formed homogenous films on the lithium substrate, excessively decreasing the amount of PVDF-HFP (9 to 1, formulation 1-c) resulted in a much lower uncompensated resistance (R u ), resulting in discontinuous and patchy films exhibiting a high PEG to PVDF-HFP ratio of 3 to 1. Figure 2 demonstrates the effect on conductivity, with the optimal PEG to PVDF-HFP ratio being 3 to 1, providing a continuous polymer film with reduced Ru when compared to formulation 1-a. EXAMPLES

[0112] To evaluate the effect of lithium salts, the following polymer formulations 2-a, 2-b, 2-c and 2-d were prepared (see Table 2, M of PEGDA = 700 g / mol). n Poly(ethylene glycol) diacrylate with LiTFSI=LiN(SO2CF3)2, LiFSI=LiN(SO2F)2, PVDF-HFP=poly(vinylidene fluoride-co-hexafluoropropylene), THF=tetrahydrofuran).

[0113] [Table 2]

[0114] The conductivity data from each of the polymer formulations in Table 2 is shown in Figure 3. The problem of low membrane salt content (10 wt%) in the polymer formulations is apparent because over the first 20 hours, the R of the Li-Li coin cell decreased as the resistive polymer formulation absorbed salt from the electrolyte. u This process should be prevented because the R of each of the cells is decreased due to the improved conductivity of the polymer membrane in each example. Increasing the salt content of the polymer formulation from 10% to 50% by weight of the total weight of the formulation u (Formulations 2-b and 2-d show similar uncompensated resistances of about 45-47 Ω.) The R u The stability of indicates that the transfer of ions between the polymer membrane and the electrolyte is in equilibrium from the cell construction, avoiding depletion of the electrolyte salt. EXAMPLES

[0115] To evaluate the effect of N-hydroethylacrylamide monomer, the following polymer formulations 3-a, 3-b, 3-c, and 3-d were prepared (see Table 2, M of PEGDA = 700 g / mol). nPoly(ethylene glycol) diacrylate with 1,2-dihydroxyethyl acrylamide, HEAA = N-hydroxyethyl acrylamide, PVDF-HFP = poly(vinylidene fluoride-co-hexafluoropropylene), THF = tetrahydrofuran).

[0116] [Table 3]

[0117] A protective layer of each formulation was coated onto a lithium substrate, cured, and cut by drawing a scalpel across the coated surface. The cut samples were imaged by SEM, and then the samples were immersed overnight (16 hours) in 4.5 M LiFSI in 1,2-dimethoxyethane (DME). The films were rinsed with pure DME to remove excess LiFSI salt to allow for clearer SEM micrographs, then dried and observed under SEM. The results for each of the polymer formulations in Table 3 are shown in Figure 4.

[0118] As expected, formulation 4-a (0 wt% HEAA) (1:0) does not show self-healing properties due to the lack of hydrogen bond donors. The protective layer containing the lowest amount of HEAA (formulation 4-b) also shows no evidence of self-healing under these conditions. Increasing the HEAA content to a 3:1 weight ratio of PEGDA to HEAA results in the polymer membrane resealing at the site of the incision made. Finally, formulation 4-d (1:1 w / w ratio of PEGDA to HEAA) also shows substantial self-healing properties (see FIG. 4). In addition, it is noteworthy that formulation 4-d appears to have better adhesion to the Li metal surface when observed under SEM compared to the other formulations.

[0119] Each polymer formulation was then tested in a Li-NMC cell against a reference cell (no polymer). -1Cells with a loading of (4.5 M LiFSI in DME) vs. TTE (3 to 1, vol / vol, TTE = 1,1,2,2-tetra-fluoroethyl 2,2,3,3-tetrafluoropropyl ether) were cycled at a fixed volumetric pressure of 0.06 MPa using foam (80 × 80 mm) with a cycle regime of C / 3 to D / 1. Each polymer-protected anode cell performed similarly to the reference cell (see Figures 5 and 6).

[0120] In the next step, the conductivity of each polymer blend was evaluated before and after thermal annealing (70° C. in dry air for 1 h). The results are shown in Figure 7(a) and Figure 7(b), respectively. Clearly, thermal annealing improves the conductivity of the polymer blend; it is about 0.1 mS.cm -1 Increasing the membrane conductivity to a minimum threshold of 0.1% is believed to be essential for successful anode protection. Higher conductivity results in a lower energy barrier to plating under the polymer membrane, which helps lower dendrite penetration, reduce the amount of dead lithium, and extend the functionality of the electrolyte and lithium anode. It was also observed that each polymer formulation appeared more homogeneous and made better contact with the lithium surface.

[0121] Each polymer formulation after annealing was then tested in a Li-NMC cell against a reference cell (no polymer). -1 Cells with a loading of (4.5 M LiFSI in DME) vs. TTE (3 to 1, vol / vol, TTE = 1,1,2,2-tetra-fluoroethyl 2,2,3,3-tetrafluoropropyl ether) were cycled at a fixed volumetric pressure of 0.06 MPa using foam (80 × 80 mm) with a cycle regime of C / 3 to D / 1. Each thermally annealed polymer-protected cell performed similarly, up to 20% better compared to the reference cell (see Figures 8 and 9).

Claims

1. 1. A negative electrode for a battery, comprising: a. a metal substrate; b. a protective layer disposed directly over at least a portion of the metal substrate, The protective layer is Formula (I) 【Chemistry 1】 (In the formula, R 1 = H or CH 3 and R 2 is C 2~6 alkanediyl, the alkanediyl being a halide, C 1~4 Alkyl, CF 3 OR 3 and R 3 is hydrogen or C 1~4 alkyl; X 1 =NH or O, and n is an integer selected from 5 to 150, preferably 8 to 100, more preferably 10 to 50; Formula (II) 【Chemistry 2】 (In the formula, R 4 = H or CH 3 and R 5 is C 2~6 alkanediyl, the alkanediyl being a halide, C 1~4 Alkyl, CF 3 OR 6 and R 6 is hydrogen or C 1~4 alkyl; X 2 =NH or O, X 3 = SH, NH 2 or OH, where m is an integer selected from 1 to 10, preferably 1 to 5, more preferably m=1; A copolymer obtainable by reaction between a copolymer, the weight ratio of said first monomer to said second monomer being 1:5 to 8:1 (w / w); a fluoropolymer additive selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), vinylidene fluoride-chlorotrifluoroethylene copolymer, ethylene tetrafluoroethylene copolymer, polychlorotrifluoroethylene, vinylidene fluoride-pentafluoropropylene copolymer, propylene tetrafluoroethylene copolymer, ethylene chlorotrifluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, and combinations thereof; A lithium salt; Including, a protective layer having a weight ratio of said copolymer to said fluoropolymer additive of 1:5 to 8:1 (w / w); a negative electrode for a battery.

2. 2. The anode of claim 1, wherein the fluoropolymer additive is polyvinylidene fluoride or poly(vinylidene fluoride-co-hexafluoropropylene), preferably poly(vinylidene fluoride-co-hexafluoropropylene).

3. The lithium salt is Li 2 CO 3 , Li 2 O., Li 2 C 2 O 4 , LiOH, LiX, R 13 O.C.O. 2 Li, HCOLi, R 13 OLi, Li 2 O., Li 2 C 2 O 4 , (R 13 O.C.O. 2 Li) 2 , (CH 2 O.C.O. 2 Li) 2 , Li 2 S, LiSCN, LiN(CN) 2 , LiClO 4 , LiBF 4 , LiAsF 6 , LiPF 6 , LiCF 3 SO 3 , LiC(CF 3 SO 2 ) 3 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 F) 2 , LiSbF 6 , LiPF 3 (CF 2 CF 3 ) 3 , LiPF 3 (CF 3 ) 3 , LiB(C 2 O 4 ) 2 (In the formula, R 13 = hydrocarbon and X = F, Cl, I or Br) and combinations thereof, preferably LiSCN, LiN(CN) 2 , LiClO 4 , LiI, LiBF 4 , LiAsF 6 , LiCF 3 SO 3 , LiCF 3 (SO 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 F) 2 , LiSbF 6 , LiPF 3 (CF 2 CF 3 ) 3 , LiPF 3 (CF 3 ) 3 , LiB(C 2 O 4 ) 2 and combinations thereof, more preferably the lithium salt is LiN(SO 2 CF 3 ) 2 Or LiN(SO 2 F) 2 and most preferably the lithium salt is LiN(SO 2 F) 2 The negative electrode according to claim 1 or 2,

4. 4. The anode according to any one of claims 1 to 3, wherein the weight ratio of said copolymer to said fluoropolymer additive is 1:2 to 5:1 (w / w), more preferably 1:2 to 4:1 (w / w), most preferably 2:1 to 4:1 (w / w).

5. The first monomer has formula (III): 【Chemistry 3】 The negative electrode according to any one of claims 1 to 4, represented by the formula: (wherein o is an integer selected from 5 to 150, preferably 8 to 100, more preferably 10 to 50).

6. The second monomer has formula (IV): 【Chemistry 4】 The negative electrode according to any one of claims 1 to 5, represented by:

7. 7. The negative electrode according to any one of claims 1 to 6, wherein the weight ratio of the first monomer to the second monomer is from 1:3 to 7:1 (w / w), preferably from 1:2 to 5:1 (w / w), most preferably from 1:2 to 2:1 (w / w).

8. Anode according to any one of claims 1 to 7, wherein said copolymer is obtained by reaction of said first monomer with said second monomer by use of a photoinitiator.

9. 9. The negative electrode according to claim 1, wherein the amount of the lithium salt is 5 to 70 wt %, based on the total weight of the protective layer, preferably 10 to 65 wt %, more preferably 40 to 60 wt %, based on the total weight of the protective layer.

10. The negative electrode according to any one of claims 1 to 9, wherein the protective layer has a thickness of 1 to 10 µm.

11. The negative electrode according to any one of claims 1 to 10, wherein the copolymer is subjected to a thermal annealing step.

12. 1. A method for preparing a negative electrode for a battery, comprising the steps of: i) adding a first monomer according to claims 1 to 11, a second monomer according to claims 1 to 11, a photoinitiator, a lithium salt according to claims 1 to 11, a fluoropolymer additive according to claims 1 to 11 to an organic liquid; ii) coating the mixture of step i) onto at least a portion of a metal substrate; iii) subjecting the coated metal substrate of step ii) to a crosslinking step; iv) optionally subjecting the crosslinked coated metal substrate of step iii) to a thermal annealing step; A method comprising:

13. A negative electrode obtainable by the method according to claim 12.

14. a. The negative electrode according to any one of claims 1 to 11 or 13; b. a positive electrode; c. an electrolyte composition; Including batteries.

15. 15. The battery of claim 14, wherein the positive electrode comprises a positive electrode material selected from the group consisting of lithium nickel manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt aluminum oxide, lithium cobalt oxide, lithium iron phosphate, lithium iron manganese phosphate, lithium iron cobalt phosphate, lithium sulfide, sulfur, and aluminum, preferably the positive electrode material is lithium nickel manganese cobalt oxide or lithium nickel cobalt aluminum oxide.

Citation Information

Patent Citations

  • Negative pole protecting film composite for lithium metal battery, negative pole manufactured using it for lithium metal battery, and lithium metal battery

    JP2005071998A

  • Negative electrode for lithium metal battery and lithium metal battery including the same

    JP2017204468A

  • Polymer for electrode protection layer and secondary battery using same

    JP2021507464A

  • Self-repairing polymer electrolyte based on dynamic chemical bonds and application thereof in secondary lithium battery

    CN111162314A

  • Lithium polymer secondary battery having protective thin film of crosslinked polymer and method for producing the same