Battery including a high concentration electrolyte and a negative electrode having a metal substrate and a protective layer
A battery with a copolymer protective layer and specific electrolyte composition addresses lithium metal secondary battery issues by reducing resistance and preventing SEI layer growth, improving performance and stability.
Patent Information
- Application Number
- JP2024535286
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-13
- Filing Date
- 2022-12-13
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2042-12-13
AI Technical Summary
Lithium metal secondary batteries face issues with high reactivity leading to electrolyte decomposition, electron density non-uniformity, and dendrite formation, which reduce coulombic efficiency and electrochemical stability, causing a reduction in battery lifetime.
A battery design featuring a negative electrode with a protective layer composed of a copolymer and a first lithium salt, combined with an electrolyte containing an organic non-fluorinated liquid and a fluorinated liquid, which minimizes resistance and prevents the formation of a thick, resistive solid electrolyte interface (SEI) layer.
The protective layer decreases uncompensated resistance and charge transfer resistance, enhancing the battery's performance and stability by absorbing reactive lithium and maintaining lithium ion conductivity, thereby prolonging the battery's lifespan.
Smart Images

Figure 2024545207000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a battery that includes a negative electrode that includes a metal substrate and a protective layer disposed directly on at least a portion of the metal substrate, and a high concentration electrolyte. [Background technology]
[0002] As the development of small and lightweight electronic products, electronic devices, communication devices, etc. progresses rapidly and the need for electric vehicles to address environmental issues becomes increasingly important, there is a demand for improved performance of secondary batteries used as power sources for these products. Among them, lithium metal secondary batteries have been attracting attention as high-performance batteries due to their high energy density and high reference electrode potential.
[0003] Due to the high reactivity of lithium metal, side reactions between lithium and liquid electrolytes occur during the charging and discharging of the battery, which promotes the decomposition of the electrolyte. In addition, due to various reasons, non-uniformity of electron density may occur on the lithium metal surface during the operation of the battery. As a result, dendritic lithium dendrites are generated on the electrode surface, making the electrode surface very rough and possibly causing damage to the separator. These side reactions reduce the coulombic efficiency and / or electrochemical stability of the lithium metal battery, causing a decrease in the life of the lithium battery.
[0004] Therefore, various attempts have been made to stabilize the lithium metal and prevent or reduce side reactions between the electrolyte and the lithium metal.
[0005] Korean Patent Application Publication No. 20030042288(A) describes a lithium secondary battery that can suppress dendrite growth on the surface of a lithium metal negative electrode by a crosslinked polymer protective film formed on the surface of the lithium metal, the polymer being crosslinked 1,6-hexanediol diacrylate or a copolymer of 1,6-hexanediol diacrylate and oligoethylene glycol diacrylate. The battery further includes a gel electrolyte polymer consisting of a mixture of ethylene carbonate, propylene carbonate, and 1M LiClO4 in poly(vinylidene fluoride-co-hexafluoropropylene).
[0006] US 2016 / 0372743 A1 relates to a battery having a coating on the lithium metal anode to prevent direct contact between the lithium metal and a volatile liquid electrolyte. The coating consists of either a single layer polymer of PVDF homopolymer, ionic liquid and LiFSI, or a dual layer polymer coating having a first outer layer of PVDF, ionic liquid and LiFSI and a second inner layer of poly(styrene-acrylonitrile) and LiFSI. The battery further includes an electrolyte consisting of 2M LiFSI in ethylene carbonate.
[0007] US Patent No. 6,902,848 (B1) discloses a lithium battery comprising a negative electrode laminated with a gel electrolyte and a liquid electrolyte consisting of 1.5-6 M LiBF4 in γ-butyrolactone. The gel electrolyte consists of cross-linked poly(ethylene glycol)-based acrylate monomers.
[0008] However, a drawback of coating the anode with a protective layer is that it introduces an additional source of resistance into the battery. Anodes coated with polymers have increased resistance, specifically increased uncompensated resistance R u and / or increased charge transfer resistance R ct This increased resistance causes a voltage drop during operation of the battery, which also consumes some of the useful energy as waste heat.
[0009] Therefore, it is necessary to realize a battery having a protective layer around the negative electrode while simultaneously minimizing the increase in battery resistance.
[0010] It is an object of the present invention to provide a battery that includes a negative electrode having a metal substrate with a protective layer around the metal substrate in combination with a high concentration electrolyte. Summary of the Invention
[0011] The object of the present invention is to a. A negative electrode, A metal substrate; a protective layer disposed directly on at least a portion of the metal substrate; the protective layer comprises a copolymer and a first lithium salt; A negative electrode; b. a positive electrode; c. An electrolyte composition comprising: i. an organic non-fluorinated liquid comprising a second lithium salt; ii. Fluorinated liquids; An electrolyte composition comprising: This is accomplished by providing a battery comprising:
[0012] The inventors have surprisingly found that the combination of a protective layer comprising a copolymer disposed on a metallic substrate of a negative electrode and an electrolyte comprising a second lithium salt, an organic non-fluorinated liquid, and a fluorinated liquid reduces the resistance of the battery, in particular the uncompensated resistance R, as demonstrated in the accompanying examples. u and charge transfer resistance R ct In particular, it has been found that a negative electrode containing a copolymer obtained by the reaction between poly(ethylene glycol) diacrylate (PEGDA) and N-hydroxyethylacrylamide (HEAA) exhibits a low uncompensated resistance R in the presence of an electrolyte containing a fluorinated liquid such as 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE). u and charge transfer resistance R ctFurthermore, the inventors have surprisingly found that the protective layer according to the invention functions as a self-healing polymer film, as demonstrated in the accompanying examples. The protective layer according to the invention is a mechanically robust polymer that also has self-healing properties, and is the result of a careful balance between polymer chain mobility, the amount of hydrogen-bonding motifs, and the degree of crosslinking.
[0013] As will be appreciated by those skilled in the art, metallic lithium spontaneously reacts with electrolyte solvents and salt anions to form a passivation layer known as the solid electrolyte interface (SEI). The SEI layer is inherently non-uniform in composition, morphology and ionic conductivity, resulting in the formation and growth of dendrites, which leads to safety issues and poor battery performance. This SEI layer continues to grow due to reaction with the liquid electrolyte, resulting in a thick, highly resistive layer. Without wishing to be bound by any theory, the inventors believe that the protective layer of the present invention on the metal substrate physically separates the highly reactive metallic lithium from the electrolyte while maintaining lithium ion conductivity through the membrane, thereby limiting the formation of the solid electrolyte interface (SEI) layer. Thus, the protective layer prevents continued growth of the layer by preventing contact between the electrolyte and the metal substrate, resulting in a thinner SEI layer with lower resistance.
[0014] While self-healing polymers (see, for example, I. Gadwal, Macromol 2021, 1, 18-36) and high-concentration lithium-based electrolytes diluted with hydrofluoroethers (see, for example, S. Lin et al., ACS Appl. Mater. Interfaces 2020, 12, 30, 33710-33718) are known in the art, the inventors are the first to demonstrate that the combination of a protective layer according to the present invention having self-healing properties and an electrolyte according to the present invention comprising a fluorinated liquid results in a battery exhibiting reduced resistance. [Brief description of the drawings]
[0015] [Figure 1]SEM (scanning electron microscope) images of each of the three polymer formulations 1-a, 1-b and 1-c (see Table 1). [Diagram 2] Uncompensated resistance (Ru) measured for each Li-Li symmetric coin cell 20 hours after cell construction for unprotected lithium anodes and protected anodes using polymer formulations 1-a, 1-b, and 1-c in 4.5 M LiFSI electrolyte in DME. [Diagram 3] Uncompensated resistance (Ru) measured for each Li-Li symmetric coin cell 20 hours after cell construction for unprotected lithium anodes and protected anodes using polymer formulations 2-a, 2-b, 2-c, and 2-d in 4.5 M LiFSI electrolyte in DME. [Figure 4] SEM micrographs of polymer films containing various amounts of HEAA, each of which was cut with a scalpel, imaged, and then immersed in 4.5 M LiFSI in DME overnight (16 h), followed by rinsing in pure DME and imaged again. [Diagram 5] Total specific discharge capacity of Li-NMC pouch cells containing protected anodes with various PEG to HEAA ratios (cycling regime was C / 3 to D / 1, potential was held at the top and bottom of charging). [Figure 6] Coulombic efficiency of Li-NMC pouch cells containing protected anodes with various PEG to HEAA ratios (cycle regime was C / 3-D / 1, potential was held at the top and bottom of charging). [Figure 7A] (a) Polymer membrane conductivity without thermal annealing (4.5 M LiFSI in DME) vs. TTE (3:1, v / v). (b) Polymer membrane conductivity with thermal annealing (4.5 M LiFSI in DME) vs. TTE (3:1, v / v). [Figure 7B](a) Polymer membrane conductivity without thermal annealing (4.5 M LiFSI in DME) vs. TTE (3:1, v / v). (b) Polymer membrane conductivity with thermal annealing (4.5 M LiFSI in DME) vs. TTE (3:1, v / v). [Figure 8] Total specific discharge capacity of Li-NMC pouch cells containing protected anodes with various PEG to HEAA ratios subjected to thermal annealing (cycling regime was C / 3-D / 1, potential was held at the top and bottom of charging). [Figure 9] Coulombic efficiency of Li-NMC pouch cells containing protected anodes with various PEG to HEAA ratios subjected to thermal annealing (cycling regime was C / 3-D / 1, potential was held at the top and bottom of charging). [Figure 10] Coulombic efficiency of Li-NMC pouch cells containing protected anodes with various concentrations of electrolyte in the electrolyte composition. [Figure 11A] Coulombic efficiency versus temperature for Li-NMC pouch cells containing protected anodes. [Figure 11B] Coulombic efficiency versus temperature for Li-NMC pouch cells containing protected anodes. [Figure 11C] Coulombic efficiency versus temperature for Li-NMC pouch cells containing protected anodes. [Figure 11D] Coulombic efficiency versus temperature for Li-NMC pouch cells containing protected anodes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] In order to enable the practice of the invention, preferred embodiments are described in detail in the drawings and the following detailed description. Although the invention has been described with reference to these specific preferred embodiments, it will be understood that the invention is not limited to these preferred embodiments. On the contrary, the invention encompasses numerous alternatives, modifications and equivalents, as will become apparent from a consideration of the following detailed description and the accompanying drawings.
[0017] The term "comprising" as used in the present specification and claims should not be interpreted as being limited to the means recited thereafter, nor does it exclude other elements or steps. It should be interpreted as specifying the presence of the recited features, integers, steps, or ingredients as mentioned, but without excluding the presence or addition of one or more other features, integers, steps, or ingredients, or groups thereof. Thus, the scope of the expression "a composition comprising components A and B" should not be limited to a composition consisting of components A and B only. It means that in the context of the present invention, the only relevant components of the composition are A and B. Thus, the terms "comprising" and "including" encompass the more restrictive terms "consisting essentially of" and "consisting of".
[0018] As used herein, "optional" or "optionally" means that the event or circumstance described thereafter may or may not occur, and the description includes instances where the event or circumstance occurs and instances where the event or circumstance does not occur.
[0019] As used herein, the term "alkyl" has its broadest meaning as generally understood in the art and can include moieties that are linear or branched, or combinations thereof. In particular, the term "alkyl", alone or in combination, refers to a linear or branched alkane-derived group, such as, for example, C F~G Alkyl defines a straight or branched alkyl group having F to G carbon atoms, for example C 1~4 Alkyl defines a straight or branched chain alkyl group having 1 to 4 carbon atoms, for example, methyl, ethyl, 1-propyl, 2-propyl (isopropyl), 15-butyl, 2-butyl, 2-methyl-2-propyl (tert-butyl), 2-methyl-1-propyl (isobutyl), etc.
[0020] The term "alkanediyl", alone or in combination, means a divalent radical derived from a straight or branched chain alkyl.
[0021] As used herein, "uncompensated anti(R u The term "cell resistance" is defined as the resistance value including the cell resistance and any small additional resistances. The main contribution to the cell resistance comes from e.g. the ionic conductivity of the liquid electrolyte and / or the ionic conductivity of the polymer protective layer. Small resistance contributions are e.g. metallic parts such as cables / contacts.
[0022] As used herein, charge transfer resistance (R ct ) is a measure of the rate of oxidation-reduction reactions occurring in an electrochemically active material (i.e., the rate of electron transfer, which is the limiting process for the charge transfer process from one atom or compound to another, resulting from the electronic and ionic resistances at the electrode-electrolyte interface).
[0023] battery As described above, the first aspect of the present invention is a. A negative electrode (i.e., an anode) for a battery, A metal substrate; a protective layer disposed directly over at least a portion of the metal substrate, Formula (I)
[0024] [ka] (In the formula, R 1 =H or CH3, R 2 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 3 and R 3 is hydrogen or C 1~4 alkyl; X 1=NH or O, and n is an integer selected from 5 to 150, preferably 8 to 100, and more preferably 10 to 50; Formula (II)
[0025] [ka] (In the formula, R 4 =H or CH3, R 5 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 6 and R 6 is hydrogen or C 1~4 alkyl; X 2 =NH or O, and X 3 =SH, NH2 or OH, m being an integer selected from 1 to 10, preferably from 1 to 5, more preferably m=1, a copolymer having a weight ratio of the first monomer to the second monomer of 1:5-8:1 (w / w); and a protective layer comprising a first lithium salt; a negative electrode (i.e., anode) for the battery, comprising: b. a positive electrode; c. An electrolyte composition comprising: i. an organic non-fluorinated liquid comprising a second lithium salt; ii. Fluorinated liquids; Including, an electrolyte composition having a molar ratio of the second lithium salt to the fluorinated liquid of 1:2 to 1:0.15 (mol / mol); The present invention provides a battery comprising:
[0026] In a preferred embodiment, the present invention provides a conductive layer, which is composed of a protective layer according to the present invention and a fluoropolymer additive. As will be understood by those skilled in the art, the battery of the present invention comprises: a. A negative electrode, A metal substrate according to the present invention; A conductive layer comprising a protective layer and a fluoropolymer additive according to the present invention. A negative electrode comprising: b. a positive electrode according to the present invention; c. an electrolyte composition according to the present invention; Includes.
[0027] metal base material One embodiment of the present invention is an anode according to the present invention, comprising a metal substrate. In a preferred embodiment, the metal substrate comprises a conductive metal, preferably stainless steel, copper, nickel, iron, cobalt, lithium, lithium alloy or a combination thereof, more preferably stainless steel, copper, nickel, lithium, lithium alloy or a combination thereof. In a more preferred embodiment, the metal substrate is a lithium metal substrate or a lithium metal alloy substrate, preferably a lithium metal substrate. As will be understood by those skilled in the art, the metal substrate can be a metal deposited on a supporting foil, such as stainless steel, copper, nickel, iron, cobalt, or a lithium or lithium alloy layer made as a foil or as a layer deposited on a surface.
[0028] Fluoropolymer Additives As described above, the conductive layer according to the present invention comprises a protective layer according to the present invention and a fluoropolymer additive, the conductive layer being disposed directly on at least a portion of the metal substrate, the fluoropolymer additive being selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), vinylidene fluoride-chlorotrifluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer, polychlorotrifluoroethylene, vinylidene fluoride. -pentafluoropropylene copolymer, propylene tetrafluoroethylene copolymer, ethylene chlorotrifluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene copolymer, and combinations thereof, preferably, the fluoropolymer additive is polyvinylidene fluoride or poly(vinylidene fluoride-co-hexafluoropropylene), most preferably poly(vinylidene fluoride-co-hexafluoropropylene).
[0029] In a preferred embodiment, the fluoropolymer additive is present in an amount of less than 75 wt% based on the total weight of the conductive layer, preferably less than 50 wt% based on the total weight of the conductive layer, and most preferably less than 20 wt%. In a preferred embodiment, the fluoropolymer additive is present in an amount of greater than 0.05 wt% based on the total weight of the conductive layer, preferably greater than 5 wt% based on the total weight of the conductive layer, and most preferably greater than 10 wt%. In a preferred embodiment, the fluoropolymer additive is present in an amount of 0.05 wt% to 75 wt% based on the total weight of the conductive layer, preferably 5 wt% to 50 wt% based on the total weight of the conductive layer, and more preferably 10 wt% to 20 wt%.
[0030] In a preferred embodiment of the invention, the weight ratio of copolymer to fluoropolymer additive is 1:5-8:1 (w / w), preferably 1:2-5:1 (w / w), more preferably 1:2-4:1, and most preferably 2:1-4:1.
[0031] In one embodiment of the present invention, the fluoropolymer additive has a weight average molecular weight M of more than 1,000 g / mol, preferably more than 10,000 g / mol, more preferably more than 100,000 g / mol, and most preferably more than 300,000 g / mol. w In one embodiment of the present invention, the fluoropolymer additive has a weight average molecular weight M of less than 1,000,000 g / mol, preferably less than 800,000 g / mol, more preferably less than 750,000 g / mol, and most preferably less than 600,000 g / mol. w In one embodiment of the present invention, the fluoropolymer additive has a weight average molecular weight M of 1,000 g / mol to 1,000,000 g / mol, preferably 10,000 g / mol to 800,000 g / mol, more preferably 100,000 g / mol to 750,000 g / mol, and most preferably 300,000 g / mol to 600,000 g / mol. w A preferred example of a fluoropolymer additive, particularly poly(vinylidene fluoride-co-hexafluoropropylene), has a weight average molecular weight M of about 400,000 g / mol or a weight average molecular weight M of about 455,000 g / mol. w Fluoropolymer additives such as poly(vinylidene fluoride-co-hexafluoropropylene) can be purchased commercially from suppliers such as Sigma-Aldrich.
[0032] In one embodiment of the present invention, the fluoropolymer additive has a number average molecular weight M of more than 250 g / mol, preferably more than 2,500 g / mol, more preferably more than 25,000 g / mol, and most preferably more than 75,000 g / mol. nIn one embodiment of the present invention, the fluoropolymer additive has a weight average molecular weight M of less than 250,000 g / mol, preferably less than 200,000 g / mol, more preferably less than 190,000 g / mol, and most preferably less than 150,000 g / mol. n In one embodiment of the present invention, the fluoropolymer additive has a weight average molecular weight M of 250 g / mol to 250,000 g / mol, preferably 2,500 g / mol to 400,000 g / mol, more preferably 25,000 g / mol to 190,000 g / mol, and most preferably 75,000 g / mol to 150,000 g / mol. n A preferred example of a fluoropolymer additive, particularly poly(vinylidene fluoride-co-hexafluoropropylene), has a number average molecular weight M of about 130,000 g / mol. n or a number average molecular weight M of about 110,000 g / mol n Fluoropolymer additives such as poly(vinylidene fluoride-co-hexafluoropropylene) can be purchased commercially from suppliers such as Sigma-Aldrich.
[0033] The inventors have found that the addition of a fluoropolymer additive increases the conductivity of the conductive layer, improves the wettability of the conductive layer, and enables the printing of a uniform film of the conductive layer, as demonstrated in the accompanying examples.
[0034] Copolymer One embodiment of the present invention comprises: Formula (I)
[0035] [ka] (In the formula, R 1 =H or CH3, R 2 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 3 and R 3 is hydrogen or C1~4 alkyl; X 1 =NH or O, and n is an integer selected from 5 to 150, preferably 8 to 100, and more preferably 10 to 50; Formula (II)
[0036] [ka] (In the formula, R 4 =H or CH3, R 5 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 6 and R 6 is hydrogen or C 1~4 alkyl; X 2 =NH or O, and X 3 =SH, NH2 or OH, and m is an integer selected from 1 to 10, preferably 1 to 5, more preferably m=1.
[0037] One embodiment of the present invention is a compound of formula (I) 1 is H or CH3, preferably H; R 2 is C 2~6 Alkanediyl, preferably C 2~4 Alkanediyl, more preferably C2 alkanediyl, and alkanediyl is a halide, C 1~4 Alkyl, CF3 or OR 3 and R 3 is hydrogen or C 1~4 alkyl; X 1 =NH or O, preferably O, and n is an integer selected from 5 to 150, preferably 8 to 100, more preferably 10 to 50.
[0038] A preferred embodiment of the present invention is a first monomer according to the present invention, the first monomer having formula (III)
[0039] [ka] (wherein o is an integer selected from 5 to 150, preferably 8 to 100, more preferably 10 to 50). In particular, the first monomer represented by formula (III) is poly(ethylene glycol) diacrylate (PEGDA).
[0040] A preferred embodiment of the present invention is a first monomer according to the present invention, which has a number average molecular weight M of more than 50 g / mol, preferably more than 100 g / mol, more preferably more than 200 g / mol, even more preferably more than 550 g / mol, most preferably more than 700 g / mol. n A preferred embodiment of the present invention is a first monomer according to the present invention, which has a number average molecular weight M of less than 20,000 g / mol, preferably less than 7,000 g / mol, more preferably less than 4,000 g / mol, even more preferably less than 2,000 g / mol, and most preferably less than 1,000 g / mol. n A preferred embodiment of the present invention is a first monomer according to the present invention, the first monomer having a number average molecular weight M of 50 g / mol to 20,000 g / mol, preferably 100 g / mol to 7,000 g / mol, more preferably 200 g / mol to 4,000 g / mol, even more preferably 550 g / mol to 2,000 g / mol, and most preferably 700 g / mol to 1,000 g / mol. n Particular examples have an average M of 250 g / mol, 575 g / mol, 700 g / mol, 4,000 g / mol or 6,000 g / mol. n A preferred example of the first monomer according to the invention is PEGDA having a number average molecular weight M of 250 g / mol, 575 g / mol or 700 g / mol, preferably 700 g / mol. nPEGDA can be purchased commercially from suppliers such as Sigma-Aldrich.
[0041] As demonstrated in the examples below, the first monomer according to the present invention, in particular PEGDA, improves the Li-ion conductivity of the copolymer according to the present invention, the protective layer according to the present invention and / or the conductive layer according to the present invention.
[0042] One embodiment of the present invention is a second monomer represented by formula (II), wherein R 4 =H or CH3, preferably H; R 5 is C 2~6 Alkanediyl, preferably C 2~4 Alkanediyl, more preferably C2 alkanediyl, and alkanediyl is a halide, C 1~4 Alkyl, CF3 or OR 6 and R 6 is hydrogen or C 1~4 alkyl; X 2 =NH or O, preferably NH; X 3 =SH, NH2 or OH, preferably OH; m is an integer selected from 1 to 10, preferably 1 to 5, and most preferably m=1.
[0043] A preferred embodiment of the present invention is a second monomer according to the present invention, the second monomer having formula (IV)
[0044] [ka] The second monomer, particularly represented by formula (IV), is N-(2-hydroxyethyl)acrylamide (HEAA). HEAA can be purchased commercially from suppliers such as Sigma-Aldrich and TCI Chemicals.
[0045] As demonstrated in the following examples, the introduction of a second monomer according to the present invention, particularly N-(2-hydroxyethyl)acrylamide (HEAA), into a copolymer provides the copolymer with self-healing properties. The first monomer according to the present invention comprises a hydrogen bond acceptor, such as a carbonyl functional group of the first monomer represented by formula (I), preferably an ester functional group of the first monomer represented by formula (III). The second monomer according to the present invention comprises a hydrogen bond acceptor, such as a carbonyl functional group of the second monomer represented by formula (II), preferably an amide functional group of the second monomer represented by formula (IV). The second monomer according to the present invention comprises a hydrogen bond donor, such as a substituent X of the second monomer represented by formula (II). 3 The hydrogen bond donor present in the second monomer may be hydrogen, for example a thiol, amino or hydroxyl functional group, preferably a hydrogen of a hydroxyl group of the second monomer represented by formula (IV). The inventors believe that the hydrogen bond donor present in the second monomer may form hydrogen bonds with a hydrogen bond acceptor present in a further second monomer of the invention and / or a hydrogen bond acceptor present in the first monomer of the invention. The inventors believe that the hydrogen bonding properties of the copolymer result in the self-healing properties of the copolymer and / or the protective layer. The hydrogen bonds present in the copolymer according to the invention have a relatively weak bond strength (1.9-6.9 kcal.mol -1 ), which means that they can be broken down and reformed at ambient temperatures.
[0046] As will be understood by those skilled in the art, the copolymer according to the present invention can be obtained by a crosslinking step (i.e. radical polymerization) of the corresponding vinyl monomer, for example the first monomer according to the present invention and the second monomer according to the present invention. In an embodiment of the present invention, the initiator that can be used for the radical polymerization depends on the crosslinking reaction, and all known photoinitiators or thermal initiators can be used, and preferably photoinitiators are used. Examples of photoinitiators include benzoin, benzoin ethyl ether, benzoin isobutyl ether, alpha methyl benzoin ethyl ether, benzoin phenyl ether acetophenone, dimethoxyphenylacetophenone, 2,2-diethoxyacetophenone, 1,1-dichloroacetophenone, trichloroacetophenone, benzophenone, p-chlorobenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-2-methylpropiophenone, benzoyl benzoate, anthraquinone, 2-ethylanthraquinone, 2-chloroanthraquinone, 2-methyl-1-(4-methylthiophenyl)-morpholinopropanone-1,2-hydroxy-2-methyl-1-phenylpropan-1-one (Darocure 1173), 2-methyl-4'-(methylthio)-2-morpholinopropiophenone (Irgacure 907), phenylbis(2,4,6-trimethylbenzoyl)-phosphine oxide (Irgacure 819), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,1-hydroxycyclohexyl phenyl ketone (Irgacure 184), Michler's ketone, benzyl dimethyl ketal, thioxanthone, isopropyl thioxanthone, chlorothioxanthone, benzyl disulfide, butanediol, carbazole, fluorenone, alpha acyl oxime ester, and combinations thereof. Examples of thermal initiators include peroxide (-OO-) series, benzoyl peroxide, cumyl hydroperoxide, and the like. Azo compounds (-N=N-) series, azobisisobutyronitrile, azobisovaleronitrile, and the like may also be used.In a preferred embodiment of the invention, the photoinitiator is phenylbis-(2,4,6-trimethylbenzoyl)-phosphine oxide (Irgacure 819) or 2-methyl-4'-(methylthio)-2-morpholinopropiophenone (Irgacure 907), preferably Irgacure 819.
[0047] The content of the initiator is not particularly limited in the present invention, but is preferably within a range that does not affect the properties of the copolymer, electrode, and liquid electrolyte according to the present invention present in the battery. In an embodiment of the present invention, the initiator is used in a range of 1 wt% to 15 wt% based on the total weight of the conductive layer, preferably in a range of 1 wt% to 5 wt%, and more preferably in a range of 2 wt% to 4 wt% based on the total weight of the conductive layer.
[0048] In an embodiment of the present invention, the crosslinking step giving the copolymer according to the present invention is carried out in an organic liquid capable of dissolving the first monomer according to the present invention, the second monomer according to the present invention and / or the copolymer according to the present invention. Preferably, the organic liquid is a non-aqueous organic liquid. In this case, as non-aqueous organic liquid, well-known liquids such as carbonates, esters, ethers, ketones, alcohols or aprotic liquids can be used. For example, the aprotic organic liquid is selected from the group consisting of N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 1-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxene, diethyl ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triesters, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, ethyl propionate, and combinations thereof. Preferred examples of organic liquids are acetonitrile or tetrahydrofuran.
[0049] In an embodiment of the present invention, the crosslinking step includes applying heat or irradiating with active energy rays, where the thermal crosslinking may use a method for heating, and the active energy rays may be by irradiating with far infrared rays, ultraviolet rays or electron beams.
[0050] In an embodiment of the present invention, the crosslinking step is carried out by thermal crosslinking or photocrosslinking, preferably photocrosslinking. In an embodiment of the present invention, thermal crosslinking can be carried out at a temperature of 50°C to 200°C, preferably at a temperature of 80°C to 110°C, and the heating time for crosslinking is 30 minutes to 48 hours, more preferably 8 hours to 24 hours. If the heating temperature and time are less than the above ranges, crosslinking is difficult to be formed sufficiently, and if the heating temperature and time exceed the above ranges, side reactions may occur or material stability may decrease. In a preferred embodiment of the present invention, photocrosslinking including active energy ray irradiation is carried out for 10 seconds to 5 hours, preferably 1 minute to 1 hour, and most preferably 2 minutes to 10 minutes. In a preferred embodiment of the present invention, photocrosslinking is carried out at a temperature of 5°C to 60°C, preferably 10°C to 50°C, and most preferably 20°C to 40°C. If the time of active ray irradiation is less than the above ranges, crosslinking is difficult to be formed sufficiently, and if it exceeds the above ranges, side reactions may occur or material stability may decrease.
[0051] As will be understood by the person skilled in the art, the copolymer can be obtained by reaction of at least two monomers, being a first monomer represented by formula (I) and a second monomer represented by formula (II), but is not limited to being obtainable by reaction between only two different monomers, for example it can also be obtained by reaction between three monomers, in particular a first monomer according to the invention, a second monomer according to the invention and a third monomer represented by formula (V) or formula (VI), the third monomer being different from the first and second monomers:
[0052] [ka] (In the formula, R 7 is H or CH3, R 8 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 9 and R 9 is hydrogen or C1~4 X is selected from alkyl 4 =NH or O, and p is an integer selected from 5 to 150, preferably 8 to 100, and more preferably 10 to 50; or
[0053] [ka] (In the formula, R 10 is H or CH3, R 11 is C 2~6 Alkanediyl, which is a halide, C 1~4 Alkyl, CF3 or OR 12 and R 12 is hydrogen or C 1~4 X is selected from alkyl 5 =NH or O, and X 6 =SH, NH2 or OH, and q is an integer selected from 1 to 10, preferably 1 to 5, more preferably q=1).
[0054] A preferred embodiment of the present invention is a copolymer obtainable by reaction between up to two monomers, the first monomer being represented by formula (I) and the second monomer being represented by formula (II).
[0055] A highly preferred embodiment of the present invention is a copolymer obtainable by reaction between up to two monomers, the first being poly(ethylene glycol) diacrylate and the second being 2-hydroxyethylacrylamide.
[0056] In a preferred embodiment, the weight ratio of the first monomer to the second monomer is 1:5-8:1, preferably 1:3-7:1, more preferably 1:2-5:1, and most preferably 1:2-2:1.
[0057] In a preferred embodiment, the copolymer is present in an amount greater than 20 wt% based on the total weight of the conductive layer, preferably greater than 30 wt% based on the total weight of the conductive layer, and most preferably greater than 50 wt%. In a preferred embodiment, the copolymer is present in an amount less than 80 wt% based on the total weight of the conductive layer, preferably less than 75 wt% based on the total weight of the conductive layer, and most preferably less than 70 wt%. In a preferred embodiment, the copolymer is present in an amount ranging from 20 wt% to 80 wt% based on the total weight of the conductive layer, preferably in the range of 30 wt% to 75 wt% based on the total weight of the conductive layer, and more preferably in the range of 50 wt% to 70 wt%.
[0058] In a preferred embodiment, the copolymer is present in an amount of more than 20% by weight based on the total weight of the protective layer, preferably more than 30% by weight based on the total weight of the protective layer, and most preferably more than 35% by weight. In a preferred embodiment, the copolymer is present in an amount of less than 80% by weight based on the total weight of the protective layer, preferably less than 75% by weight based on the total weight of the protective layer, and most preferably less than 50% by weight. In a preferred embodiment, the copolymer is present in an amount ranging from 20% to 80% by weight based on the total weight of the protective layer, preferably in the range of 30% to 75% by weight based on the total weight of the protective layer, and more preferably in the range of 35% to 50% by weight based on the total weight of the protective layer.
[0059] A particular example of a copolymer according to the invention is a copolymer of formula (VII)
[0060] [ka] (wherein o is an integer selected from 5 to 150, preferably 8 to 100, more preferably 10 to 50, and r, s, and t are integers independently selected from 1 to 10, preferably 2 to 8, most preferably 3 to 6. However, as will be understood by one skilled in the art, the copolymer according to the present invention is not limited to formula (VII), which is shown as an exemplary embodiment.
[0061] In a highly preferred embodiment of the present invention, the copolymer according to the present invention, and therefore the protective layer according to the present invention and the conductive layer according to the present invention, have self-healing properties, as demonstrated in the examples below.
[0062] In a preferred embodiment of the present invention, the copolymer, protective layer and / or conductive layer according to the present invention are subjected to a thermal annealing step. As will be understood by those skilled in the art, thermal annealing is a common process used in materials chemistry to relieve stress, improve uniformity and improve contact with the substrate. In particular, thermal annealing involves increasing the temperature T of the part coated by the coating from initially room temperature to a maximum (operating) temperature T max The thermal annealing step is a process in which the temperature is raised to a temperature T, preferably above the recrystallization temperature of the copolymer according to the invention and / or the protective layer according to the invention, until the end of the operation (e.g. cutting), and then lowered back to room temperature. In a very preferred embodiment, the thermal annealing step is carried out at a temperature in the range of 40°C to 100°C, preferably in the range of 50°C to 90°C, more preferably in the range of 60°C to 80°C, after UV curing of the copolymer, and / or the duration of the thermal annealing is 5 minutes to 10 hours, preferably 15 minutes to 5 hours, most preferably 30 minutes to 90 minutes. In a very preferred embodiment, the thermal annealing step according to the invention is carried out in dry air. The inventors have surprisingly found that the thermal annealing step improves the conductivity of the copolymer. In addition, each copolymer subjected to the thermal annealing step appears more homogeneous and has better contact with the Li surface. Furthermore, the inventors have found that the charge transfer resistance (R ct ) was found to decrease.
[0063] First Lithium Salt As noted above, the protective layer according to the present invention comprises a first lithium salt.
[0064] In one embodiment of the present invention, the first lithium salt is Li2CO3, Li2O, Li2C2O4, LiOH, LiX 7 ,ROCO2Li,HCOLi,R 13OLi, Li2O, Li2C2O4, (R 13 OCO2Li)2, (CH2OCO2Li)2, Li2S, LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2) 3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, LiB(C2O4)2 (in the formula, R 13 = Hydrocarbon and X 7 =F, Cl, I or Br) and combinations thereof, preferably selected from the group consisting of LiSCN, LiN(CN)2, LiClO4, Liil, LiBF4, LiAsF6, LiCF3SO3, LiCF3(SO3)2, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, LiB(C2O4)2 and combinations thereof, more preferably the first lithium salt is LiN(SO2CF3)2 or LiN(SO2F)2, and most preferably the first lithium salt is LiN(SO2F)2.
[0065] In a preferred embodiment of the present invention, the amount of the first lithium salt is greater than 5 wt% based on the total weight of the conductive layer, preferably greater than 10 wt% based on the total weight of the conductive layer, most preferably greater than 40 wt% based on the total weight of the conductive layer. In a preferred embodiment of the present invention, the amount of the first lithium salt is less than 70 wt% based on the total weight of the conductive layer, preferably less than 65 wt% based on the total weight of the conductive layer, most preferably less than 60 wt%. In a preferred embodiment of the present invention, the amount of the first lithium salt is 5 wt% to 70 wt% based on the total weight of the conductive layer, preferably 10 wt% to 65 wt% based on the total weight of the conductive layer, more preferably 40 wt% to 60 wt%.
[0066] In a preferred embodiment of the present invention, the amount of the first lithium salt is greater than 10% by weight based on the total weight of the protective layer, preferably greater than 40% by weight based on the total weight of the protective layer, most preferably greater than 50% by weight based on the total weight of the protective layer. In a preferred embodiment of the present invention, the amount of the lithium salt is less than 70% by weight based on the total weight of the protective layer, preferably less than 65% by weight based on the total weight of the protective layer, most preferably less than 60% by weight. In a preferred embodiment of the present invention, the amount of the lithium salt is 10% to 70% by weight based on the total weight of the protective layer, preferably 40% to 65% by weight based on the total weight of the protective layer, more preferably 50% to 65% by weight.
[0067] The inventors have found that the addition of lithium salt improves the Li-ion conductivity of the protective layer and / or conductive layer and prevents the protective layer and / or conductive layer from depleting the lithium ions present in the electrolyte. Furthermore, the addition of a higher lithium salt content to the protective layer reduces the uncompensated resistance R u decreases.
[0068] protective layer In one embodiment of the present invention, the protective layer has a thickness of 1 μm to 10 μm, preferably 2 μm to 7 μm, and more preferably 3 μm to 6 μm.
[0069] In one embodiment of the present invention, the protective layer is disposed directly on at least a portion of the metal substrate, and preferably, the protective layer is disposed directly on the entire surface of the metal substrate. As will be understood by those skilled in the art, the negative electrode according to the present invention comprises a protective layer according to the present invention, and the protective layer forms an outer layer on the metal substrate. In other words, the protective layer is coated on a portion of the surface of the metal substrate, i.e., the protective layer forms a coating on a portion of the surface of the metal substrate, preferably on the entire surface of the metal substrate.
[0070] In a preferred embodiment of the invention, the protective layer according to the invention has an ionic conductivity of more than 0.01 mS / cm, preferably more than 0.015 mS / cm, more preferably more than 0.05 mS / cm. In a preferred embodiment of the invention, the protective layer has an ionic conductivity of less than 0.5 mS / cm, preferably less than 0.2 mS / cm, more preferably less than 0.1 mS / cm. In a preferred embodiment of the invention, the protective layer according to the invention has an ionic conductivity in the range of 0.01 mS / cm to 0.5 mS / cm, preferably in the range of 0.015 mS / cm to 0.2 mS / cm, most preferably in the range of 0.05 mS / cm to 0.1 mS / cm. The ionic conductivity of the protective layer is measured by the uncompensated resistance R by electronic impedance spectroscopy (EIS) in a symmetric Li-Li cell. u and ionic conductivity is measured after cell construction (meaning, for example, in a battery including a negative electrode and electrolyte composition according to the present invention).
[0071] A further aspect of the present invention is a method for preparing a protective layer according to the present invention, comprising the following steps: i) adding a first monomer as defined above, a second monomer as defined above, an initiator as defined above, and a first lithium salt as defined above to an organic liquid as defined above; ii) subjecting the mixture obtained in step i) to a crosslinking step as defined above; iii) optionally subjecting the crosslinked mixture of step ii) to a thermal annealing step as defined above; Includes.
[0072] A further aspect of the present invention is a protective layer obtainable by the process for preparing a protective layer according to the present invention.
[0073] Conductive Layer In one embodiment of the present invention, the conductive layer has a thickness of 1 μm to 10 μm, preferably 2 μm to 7 μm, and more preferably 3 μm to 6 μm.
[0074] In one embodiment of the present invention, the conductive layer is disposed directly on at least a portion of the metal substrate, and preferably, the conductive layer is disposed directly on the entire surface of the metal substrate. As will be understood by those skilled in the art, the negative electrode according to the present invention comprises the conductive layer according to the present invention, and the conductive layer forms an outer layer on the metal substrate. In other words, the conductive layer is coated on a portion of the surface of the metal substrate, i.e., the conductive layer forms a coating on a portion of the surface of the metal substrate, preferably on the entire surface of the metal substrate.
[0075] In a preferred embodiment of the invention, the conductive layer according to the invention has an ionic conductivity of more than 0.005 mS / cm, preferably more than 0.01 mS / cm, more preferably more than 0.015 mS / cm. In a preferred embodiment of the invention, the protective layer has an ionic conductivity of less than 1.5 mS / cm, preferably less than 1.2 mS / cm, more preferably less than 1 mS / cm. In a preferred embodiment of the invention, the conductive layer according to the invention has an ionic conductivity in the range of 0.005 mS / cm to 1.5 mS / cm, preferably in the range of 0.01 mS / cm to 1.2 mS / cm, most preferably in the range of 0.015 mS / cm to 1 mS / cm. The ionic conductivity of the protective layer is measured by the uncompensated resistance R by electronic impedance spectroscopy (EIS) in a symmetric Li-Li cell. u and ionic conductivity is measured after cell construction (meaning, for example, in a battery including a negative electrode and electrolyte composition according to the present invention).
[0076] A further aspect of the present invention is a method for preparing a conductive layer according to the present invention, comprising the following steps: i) adding a first monomer as defined above, a second monomer as defined above, an initiator as defined above, a lithium salt as defined above and a fluoropolymer additive as defined above to an organic liquid as defined above; ii) subjecting the mixture obtained in step i) to a crosslinking step as defined above; iii) optionally subjecting the crosslinked mixture of step ii) to a thermal annealing step as defined above; Includes.
[0077] A further aspect of the present invention is a conductive layer obtainable by the process for preparing a conductive layer according to the present invention.
[0078] negative electrode A further aspect of the present invention is a negative electrode according to the present invention, a. Metal base material, b. a protective layer obtainable by the method for preparing a protective layer according to the invention, disposed directly on at least a portion of a metal substrate, and / or a conductive layer obtainable by the method for preparing a conductive layer according to the invention, disposed directly on at least a portion of a metal substrate; Includes.
[0079] A further aspect of the present invention is a method for producing a process comprising the steps of: i) adding a first monomer as defined above, a second monomer as defined above, an initiator as defined above, a lithium salt as defined above and, optionally, a fluoropolymer additive as defined above to an organic liquid as defined above; ii) coating the mixture obtained in step i) onto at least a portion of a metal substrate, preferably onto the entire surface of the metal substrate; iii) subjecting the coated metal substrate of step ii) to a crosslinking step as defined above; iv) optionally subjecting the crosslinked coated metal substrate of step iii) to a thermal annealing step as defined above; A method for preparing a negative electrode for a battery comprising:
[0080] In one embodiment of the present invention, the amount of solids (i.e., the sum of the first monomer, the second monomer, the initiator, the lithium salt, and the fluoropolymer additive) is greater than 1% by weight based on the total weight of the solids and the liquids, preferably greater than 2% by weight based on the total weight of the solids and the liquids, and most preferably greater than 3% by weight. In one embodiment of the present invention, the amount of solids (i.e., the sum of the first monomer, the second monomer, the initiator, the lithium salt, and the fluoropolymer additive) is less than 10% by weight based on the total weight of the solids and the liquids, preferably less than 8% by weight based on the total weight of the solids and the liquids, and most preferably less than 5% by weight. In one embodiment of the present invention, the amount of solids (i.e., the sum of the first monomer, the second monomer, the initiator, the lithium salt, and the fluoropolymer additive) is between 1% and 10% by weight based on the total weight of the solids and the liquids, preferably between 2% and 8% by weight based on the total weight of the solids and the liquids, and most preferably between 3% and 5% by weight.
[0081] The coating step can be carried out using methods used in conventional wet processes as understood by those skilled in the art, for example, spin coating, spray coating, doctor blade coating, dip coating.
[0082] Optionally, the coating step is followed by a drying step, which is carried out at a temperature equal to or higher than the boiling point of the organic liquid and equal to or lower than the glass transition temperature T of the copolymer according to the invention and / or the protective layer according to the invention. g It may be suitably carried out at the following temperatures: A drying step may also be carried out in order to remove any liquid remaining on the surface of the metal substrate and at the same time improve the adhesion of the copolymer according to the invention and / or the protective layer according to the invention.
[0083] A further aspect of the present invention is an anode obtainable by the process for preparing an anode for a battery according to the present invention.
[0084] battery A further aspect of the present invention is a. an anode according to the invention or obtainable by the method for preparing an anode for a battery according to the invention; b. a positive electrode; c. an electrolyte composition preferably disposed between the positive and negative electrodes; d. optionally, a separator; A battery comprising:
[0085] In a preferred embodiment of the invention, the battery is a lithium metal battery, preferably a lithium metal secondary battery.
[0086] positive electrode The material of the positive electrode (i.e., cathode) is not particularly limited, and examples thereof include transition metal compounds having a structure capable of diffusing lithium ions, or specialized metal compounds thereof, and oxides of lithium. In particular, LiCoO2, LiNiO2, LiMnO4, LiFePO4, etc. may be mentioned. A preferred positive electrode material is a mixed metal oxide containing lithium, nickel, and optionally manganese, cobalt, and / or aluminum.
[0087] In a preferred embodiment of the invention, the positive electrode comprises a positive electrode material selected from the group consisting of lithium nickel-manganese-cobalt oxide, lithium nickel-manganese oxide, lithium nickel-cobalt-aluminum oxide, lithium cobalt oxide, lithium iron phosphate, lithium iron manganese phosphate, lithium iron cobalt phosphate, lithium sulfide, sulfur and aluminum, preferably the positive electrode material is lithium nickel-manganese-cobalt oxide or lithium nickel-cobalt-aluminum oxide.
[0088] The positive electrode can be formed by pressing the positive electrode materials listed above together with known conductive auxiliary or binders, or the positive electrode active material together with known conductive auxiliary or binders, into an organic liquid such as pyrrolidone, which can be obtained by applying the mixture and coating it on a current collector such as aluminum foil, followed by drying.
[0089] electrolyte composition In one embodiment of the invention, a battery according to the invention comprises an electrolyte composition, preferably a liquid electrolyte composition, hi a preferred embodiment, disposed between the positive electrode and the negative electrode.
[0090] In one embodiment of the present invention, the electrolyte composition comprises: i. an organic non-fluorinated liquid comprising a second lithium salt; ii. a fluorinated liquid; Includes.
[0091] In a preferred embodiment of the invention, the organic non-fluorinated liquid is selected from the group consisting of N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxene, diethyl ether, allyl ether, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), tetraethylene glycol dimethyl ether (tetraglyme), butyl diglyme, polyethylene glycol, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, ethyl methoxymethane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidone, methyl propionate, propionate, Preferably, the organic non-fluorinated liquid is selected from the group consisting of 1,3-dioxolane, 1,4-dioxane, tetrahydrofuran, allyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, butyl diglyme, dimethyl ether, diethyl ether, polyethylene glycol, acetonitrile, dimethyl sulfoxide, sulfolane, trimethyl phosphate, triethyl phosphate, dimethyl methyl phosphonate, hexamethyldisiloxane, hexamethylcyclotrisiloxane, 1,2-dimethoxymethane or 1,2-diethoxyethane, most preferably, the non-fluorinated organic liquid is 1,2-dimethoxymethane or 1,2-dimethoxyethane.
[0092] In a preferred embodiment of the present invention, the second lithium salt is Li2CO3, Li2O, Li2C2O4, LiOH, LiX 8 , R14 OCO2Li, HCOLi, R 14 OLi, Li2O, Li2C2O4, (R 14 OCO2Li)2, (CH2OCO2Li)2, Li2S, LiSCN, LiN(CN)2, LiClO4, LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiC(CF3SO2) 3, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, LiB(C2O4)2 (in the formula, R 14 = Hydrocarbon and X 8 =F, Cl, I or Br), preferably selected from the group consisting of LiSCN, LiN(CN)2, LiClO4, LiI, LiBF4, LiAsF6, LiCF3SO3, LiCF3(SO3)2, LiN(SO2C2F5)2, LiN(SO2CF3)2, LiN(SO2F)2, LiSbF6, LiPF3(CF2CF3)3, LiPF3(CF3)3, LiB(C2O4)2 and combinations thereof, more preferably the lithium salt is LiN(SO2CF3)2 or LiN(SO2F)2, and most preferably the lithium salt is LiN(SO2F)2.
[0093] In a highly preferred embodiment, the first lithium salt and the second lithium salt described above are the same lithium compound.
[0094] In a preferred embodiment of the invention, the concentration of the second lithium salt in the organic non-fluorinated liquid is greater than 1 M, preferably greater than 2 M, most preferably greater than 3 M. In a preferred embodiment of the invention, the concentration of the second lithium salt in the organic non-fluorinated liquid is less than 10 M, preferably less than 8 M, most preferably less than 6 M. In a preferred embodiment of the invention, the concentration of the second lithium salt in the organic non-fluorinated liquid is in the range of 1 M to 10 M, preferably in the range of 2 M to 8 M, most preferably in the range of 3 M to 6 M.
[0095] In one embodiment, the fluorinated liquid is a fluorinated ether, a fluorinated carbonate, or a fluorinated aromatic compound. In a preferred embodiment, the fluorinated liquid is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl)ether (BTFE), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), tris(2,2,2-trifluoroethyl)orthoformate (TFEO), methoxynonafluorobutane (MOFB), ethoxynonafluorobutane (EOFB), di(2,2,2-trifluoroethyl)carbonate (DTFEC), tris(2,2,2-trifluoroethyl)orthoformate (TFEO), tris(hexafluoroisopropyl)orthoformate (THFiPO), tris(2,2-difluoroethyl)orthoformate (T DFEO), bis(2,2,2-trifluoroethyl)methyl orthoformate (BTFEMO), tris(2,2,3,3,3-pentafluoropropyl) orthoformate (TPFPO), tris(2,2,3,3-tetrafluoropropyl) orthoformate (TTPO) and combinations thereof, preferably the fluorinated liquid is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl)ether (BTFE) or 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), and most preferably 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE).
[0096] In a preferred embodiment, the molar ratio of the second lithium salt to the organic non-fluorinated liquid is from 1:3 to 1:0.5 (mol / mol), preferably from 1:2 to 1:0.60 (mol / mol), more preferably from 1:1.60 to 1:0.80 (mol / mol), and most preferably from 1:1.50 to 1:10.
[0097] In a preferred embodiment, the molar ratio of the second lithium salt to the organic non-fluorinated liquid is from 1:2 to 1:0.15 (mol / mol), preferably from 1:1.85 to 1:0.25 (mol / mol), more preferably from 1:1.70 to 1:0.35 (mol / mol), even more preferably from 1:1.50 to 1:0.35 (mol / mol), and most preferably from 1:1 to 1:0.40 (mol / mol).
[0098] In a preferred embodiment, the molar ratio of organic non-fluorinated liquid to fluorinated liquid is 1:2 to 1:0.10 (mol / mol), preferably 1:1.50 to 1:0.20 (mol / mol), more preferably 1:1.20 to 1:0.25 (mol / mol), even more preferably 1:1 to 1:0.30 (mol / mol), and most preferably 1:0.85 to 1:0.30 (mol / mol).
[0099] In a preferred embodiment of the invention, the volume ratio of organic non-fluorinated liquid to fluorinated liquid is 6:1 to 1:2 (vol / vol), preferably 5:1 to 1:1 (vol / vol), most preferably 4:1 to 2:1 (vol / vol).
[0100] As will be understood by the person skilled in the art, the organic liquid according to the present invention is the liquid used in the crosslinking step to give the copolymer according to the present invention, while the organic non-fluorinated liquid according to the present invention is the liquid present in the electrolyte composition according to the present invention.
[0101] As will be appreciated by those skilled in the art, fluorinated liquids according to the present invention include at least one fluoride substituent, while organic non-fluorinated liquids do not have fluoride substituents.
[0102] Separator In order to prevent short circuit between the positive and negative electrodes, a separator is usually inserted between the cathode and the anode. The material and shape of the separator are not particularly limited, but it is preferable that the separator is an insulating and chemically stable material that can easily pass the electrolyte composition. Examples of the separator include microporous films and sheets made of various polymer materials. Specific examples of the polymer materials include polyolefin polymers, nitrocellulose, polyacrylonitrile, polyvinylidene fluoride, polyethylene, and polypropylene. From the viewpoint of electrochemical stability and chemical stability, polyolefin polymers are preferable.
[0103] others In a preferred embodiment of the invention, the cells of the invention have a coulombic efficiency of at least 93%, preferably at least 94%, more preferably at least 95%, even more preferably at least 96%, even more preferably at least 97%, and most preferably at least 98%. Coulombic efficiency is evaluated using the following general formula:
[0104]
number
[0105] use A further aspect of the present invention is the uncompensated resistance R u The present invention provides a use of a battery according to the present invention for reducing
[0106] A further aspect of the present invention is the charge transfer resistance R ct The present invention provides a use of a battery according to the present invention for reducing EXAMPLES
[0107] The invention is further illustrated in the following examples.
[0108] Description of cell preparation and test method All coin cells tested were of the CR2032 type. The cells were prepared by stacking the cathode casing, the cathode (pre-soaked in electrolyte), the Cellguard separator, a 50 μL drop of electrolyte, the anode, the spacer, the wave spring, and the anode casing in that order on top of each other. The cells were pressurized with a pressure of 80 kg / cm using an MTI manual pressurization machine. 2 Pressure welding was performed at a pressure of 1000 MPa.
[0109] Li-Li pouch cells were prepared according to the following: format = 1Li (58 x 58 mm) / 1Sep (62 x 62 mm) / 1Li (50 x 50 mm), "nominal capacity" = 0.1 Ah, separator = alumina coated Targray SH220W22, lithium = 100 μm thick (coated or uncoated), electrolyte loading = 3.00 μL mAh. -1 (i.e., 0.3 mL), C rate = C / 5 D / 5 (standard regime) or C / 3 D / 1, with potential hold (new regime), cycle temperature = 25°C.
[0110] Li-NMC pouch cells were prepared according to the following: format = 3Li (58 × 58 mm) / 4Sep (62 × 62 mm) / 2NMC (56 × 54 mm), nominal capacity = 0.48 Ah (cathode surface capacity = 4 mAh cm -2 ), separator = Targray SH220W22 coated with alumina, lithium = 100 μm thickness, electrolyte loading = 2.00 μL mAh -1 (i.e., 0.97 mL) or 1.75 μL mAh -1 i.e., 0.85 mL), C rate = C / 5 D / 5 (standard regime) or C / 3 D / 1, with potential hold (new regime), cycle temperature = 25 °C. The NMC cathode contained LiNi 0.6 Mn 0.2 Co 0.2 It contains O2, carbon black and PVDF in a weight ratio of 92:4:4.
[0111] Uncompensated resistance R uis measured by electrochemical impedance spectroscopy (Nyquist plot) of Li-Li symmetric coin cells containing lithium metal anodes with and without protective layer coating. Frequencies between 1 MHz and 1 Hz were applied in the tests.
[0112] Charge transfer resistance R ct is measured by electrochemical impedance spectroscopy (Nyquist plot) of Li-Li symmetric coin cells containing lithium metal anodes with and without protective layer coating. Frequencies between 1 MHz and 1 Hz were applied in the tests.
[0113] The ionic conductivity of the protective layer was measured by the uncompensated resistance R by electronic impedance spectroscopy (EIS) in a symmetric Li-Li cell. u The ionic conductivity is measured after the cell is constructed.
[0114] Cross sections of the protective layer were analyzed using a scanning electron microscope (SEM). A JEOL benchtop SEM was used (samples were imaged in the SEM under vacuum, secondary electron imaging, probe current set to standard, accelerating voltage of the SEM column).
[0115] The polymer-protected anode is prepared by adding the monomer, lithium salt, initiator and fluoropolymer additive into an organic liquid in the amounts specified in the table below. These mixtures are coated onto the anode and subjected to UV curing with Irgacure 819 as a photoinitiator for 5 minutes UV curing time. Optionally, thermal annealing of the polymer is performed after UV curing the polymer-protected anode at 70° C. for 1 hour.
[0116] Example 1 To evaluate the effect of the amount of fluoropolymer additive, the following polymer formulations 1-a, 1-b and 1-c were prepared (see Table 1, M of PEGDA = 700 g / mol). nPoly(ethylene glycol) diacrylate with LiTFSI=LiN(SO2CF3)2, PVDF-HFP=poly(vinylidene fluoride-co-hexafluoropropylene), THF=tetrahydrofuran).
[0117] [Table 1]
[0118] FIG. 1 shows the effect of decreasing the weight percent of the fluoropolymer additive in the polymer formulation on the film continuity, showing that while coatings of formulations 1-a and 1-b formed homogenous films on the lithium substrate, excessively decreasing the amount of PVDF-HFP (9 to 1, formulation 1-c) resulted in a much lower uncompensated resistance (R u FIG. 2 demonstrates the effect on conductivity, with the optimal PEG to PVDF-HFP ratio of 3:1 providing a continuous polymer film and a reduced R compared to formulation 1-a. u is declining.
[0119] Example 2 To evaluate the effect of lithium salts, the following polymer formulations 2-a, 2-b, 2-c and 2-d were prepared (see Table 2, M of PEGDA = 700 g / mol). n Poly(ethylene glycol) diacrylate with LiTFSI=LiN(SO2CF3)2, LiFSI=LiN(SO2F)2, PVDF-HFP=poly(vinylidene fluoride-co-hexafluoropropylene), THF=tetrahydrofuran).
[0120] [Table 2]
[0121] The conductivity data from each of the polymer formulations in Table 2 is shown in Figure 3. The problem of low membrane salt content (10 wt%) in the polymer formulations is apparent because over the first 20 hours, the R of the Li-Li coin cells decreased as the resistive polymer formulation absorbed salt from the electrolyte. u This process should be prevented because the R of each of the cells is decreased due to the improved conductivity of the polymer membrane in each example. Increasing the salt content of the polymer formulation from 10% to 50% by weight of the total weight of the formulation u (Formulations 2-b and 2-d show similar uncompensated resistances of about 45-47 Ω.) The R u The stability of indicates that the transfer of ions between the polymer membrane and the electrolyte is in equilibrium from the cell construction, avoiding depletion of the electrolyte salt.
[0122] Example 3 To evaluate the effect of N-hydroethylacrylamide monomer, the following polymer formulations 4-a, 4-b, 4-c, and 4-d were prepared (see Table 3, M of PEGDA = 700 g / mol). n Poly(ethylene glycol) diacrylate with 1,2-diphenyl ether, HEAA = N-hydroxyethylacrylamide, PVDF-HFP = poly(vinylidene fluoride-co-hexafluoropropylene), THF = tetrahydrofuran).
[0123] [Table 3]
[0124] A protective layer of each formulation was coated onto a lithium substrate, cured, and cut by drawing a scalpel across the coated surface. The cut samples were imaged by SEM, and then the samples were immersed overnight (16 hours) in 4.5 M LiFSI in 1,2-dimethoxyethane (DME). The films were rinsed with pure DME to remove excess LiFSI salt to allow for clearer SEM micrographs, then dried and observed under SEM. The results for each of the polymer formulations in Table 3 are shown in Figure 4.
[0125] As expected, formulation 4-a (0 wt% HEAA) (1:0) does not show self-healing properties due to the lack of hydrogen bond donors. The protectant containing the lowest amount of HEAA (formulation 4-b) also shows no evidence of self-healing under these conditions. Increasing the HEAA content to a 3:1 weight ratio of PEGDA to HEAA results in the polymer membrane resealing at the site of the incision made. Finally, formulation 4-d (1:1 w / w ratio of PEGDA to HEAA) also shows substantial self-healing properties (see FIG. 4). In addition, it is noteworthy that formulation 4-d appears to have better adhesion to the Li metal surface when viewed under SEM compared to the other formulations.
[0126] Each polymer formulation was then tested in a Li-NMC cell against a reference cell (no polymer). -1 Cells with a loading of (4.5 M LiFSI in DME) vs. TTE (3 to 1, vol / vol, TTE = 1,1,2,2-tetra-fluoroethyl 2,2,3,3-tetrafluoropropyl ether) were cycled at a fixed volumetric pressure of 0.06 MPa using foam (80 × 80 mm) with a cycle scheme of C / 3 to D / 1. Each polymer-protected cell performed similarly to the reference cell (see Figures 5 and 6).
[0127] In the next step, the conductivity of each polymer formulation was evaluated before and after thermal annealing (70° C. in dry air for 1 h). The results are shown in FIG. 7(a) and FIG. 7(b), respectively. Clearly, thermal annealing improves the conductivity of the polymer films; approximately 0.1 mS cm -1 Increasing the membrane conductivity to a minimum threshold of 0.1% is believed to be essential for successful anode protection. Higher conductivity results in a lower energy barrier to plating under the polymer membrane, which helps lower dendrite penetration, reduce the amount of dead lithium, and extend the functionality of the electrolyte and lithium anode. It was also observed that each polymer formulation appeared more homogeneous and made better contact with the lithium surface.
[0128] Each polymer formulation after annealing was then tested in a Li-NMC cell against a reference cell (no polymer). -1 Cells with a loading of (4.5 M LiFSI in DME) vs. TTE (3 to 1, vol / vol, TTE = 1,1,2,2-tetra-fluoroethyl 2,2,3,3-tetrafluoropropyl ether) were cycled at a fixed volumetric pressure of 0.06 MPa using foam (80 × 80 mm) with a cycle regime of C / 3 to D / 1. Each thermally annealed polymer-protected cell performed similarly, up to 20% better compared to the reference cell (see Figures 8 and 9).
[0129] Example 4 A systematic screening of electrolytes was performed by diluting a 5.23 M LiFSI solution in DME (1:1 molar ratio of LiFSI to DME) with various volumetric ratios of TTE. The pouch cells were tested at 25 °C in a voltage window of 3.0 V to 4.3 V in the standard regime of C / 5 to D / 5 with an initial cycle at a slower rate of C / 10 to D / 10. The electrolyte ratio was 2 μL mAh -1As shown in FIG. 10, no TTE addition (5.23M LiFSI in DME) or large amounts of TTE addition (5.23M LiFSI in DME vs. TTE 1:2 vol / vol) show a decrease in cycle life compared to other dilutions (5.23M LiFSI in DME vs. TTE 3:1, 2:1, and 1:1 vol / vol). The imperfect results for (5.23M LiFSI in DME vs. TTE 3:1 vol / vol) are attributed to poor cell construction.
[0130] Example 5 Charge transfer resistance R for lithium metal substrates not coated with polymer (bare Li) or coated with Formulations 4-a, 4-b, and 4-c ct and uncompensated resistance R u was measured (see FIG. 11) at different cycling temperatures and evaluated. In the presence of 4.5 M LiFSI in DME with TTE ((4.5 M LiFSI in DME) vs. TTE 3 vs. 1 v / v), the polymer film with more HEAA in the backbone exhibited a significantly higher charge transfer resistance R compared to the polymer protected anode without TTE present in the electrolyte composition. ct Drop in resistance and uncompensated resistance R u This indicates a decrease in
Claims
1. a. A negative electrode, A metal substrate; a protective layer disposed directly over at least a portion of the metal substrate, Formula (I) 【Chemistry 1】 (In the formula, R 1 = H or CH 3 and R 2 is C 2~6 alkanediyl, the alkanediyl being a halide, C 1~4 Alkyl, CF 3 OR 3 and R 3 is hydrogen or C 1~4 alkyl; X 1 =NH or O, and n is an integer selected from 5 to 150, preferably 8 to 100, more preferably 10 to 50; Formula (II) 【Chemistry 2】 (In the formula, R 4 = H or CH 3 and R 5 is C 2~6 alkanediyl, the alkanediyl being a halide, C 1~4 Alkyl, CF 3 OR 6 and R 6 is hydrogen or C 1~4 alkyl; X 2 =NH or O, X 3 = SH, NH 2 or OH, m being an integer selected from 1 to 10, preferably from 1 to 5, more preferably m=1, and a protective layer comprising a first lithium salt; A negative electrode comprising: b. a positive electrode; c. an electrolyte composition comprising: i. an organic non-fluorinated liquid comprising a second lithium salt; ii. a fluorinated liquid; Including, an electrolyte composition having a molar ratio of the second lithium salt to the fluorinated liquid of from 1:2 to 1:0.15 (mol / mol); Including batteries.
2. 2. The battery of claim 1, wherein the molar ratio of the second lithium salt to the organic non-fluorinated liquid is from 1:3 to 1:0.5 (mol / mol), preferably from 1:2 to 1:0.60 (mol / mol), more preferably from 1:1.60 to 1:0.80 (mol / mol), and most preferably from 1:1.50 to 1:
10.
3. 3. The battery according to claim 1 or 2, wherein the molar ratio of the organic non-fluorinated liquid to the fluorinated liquid is from 1:2 to 1:0.10 (mol / mol), preferably from 1:1.50 to 1:0.20 (mol / mol), more preferably from 1:1.20 to 1:0.25 (mol / mol), even more preferably from 1:1 to 1:0.30 (mol / mol), and most preferably from 1:0.85 to 1:0.30 (mol / mol).
4. The negative electrode includes a conductive layer consisting of the protective layer of claim 1 and a fluoropolymer additive, and the fluoropolymer additive is selected from the group consisting of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), vinylidene fluoride-chlorotrifluoroethylene copolymer, ethylene tetrafluoroethylene copolymer, polychlorotrifluoroethylene, vinylidene fluoride-pentafluoropropylene copolymer, pro 2. The battery of claim 1, wherein the fluoropolymer additive is selected from the group consisting of vinylidene fluoride-tetrafluoroethylene copolymer, ethylene chlorotrifluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, vinylidene fluoride-perfluoromethylvinyl ether-tetrafluoroethylene copolymer, and combinations thereof, preferably, the fluoropolymer additive is polyvinylidene fluoride or poly(vinylidene fluoride-co-hexafluoropropylene), most preferably poly(vinylidene fluoride-co-hexafluoropropylene).
5. 5. The battery of claim 4, wherein the weight ratio of said copolymer to said fluoropolymer additive is 1:10 to 10:1 (w / w), preferably 1:5 to 8:1 (w / w), more preferably 1:2 to 5:1 (w / w), even more preferably 1:2 to 4:1 (w / w), most preferably 2:1 to 4:1 (w / w).
6. The first lithium salt is Li 2 CO 3 , Li 2 O., Li 2 C 2 O 4 , LiOH, LiX 7 , R 13 O.C.O. 2 Li, HCOLi, R 13 OLi, Li 2 O., Li 2 C 2 O 4 , (ROCO 2 Li) 2 , (CH 2 O.C.O. 2 Li) 2 , Li 2 S, LiSCN, LiN(CN) 2 , LiClO 4 , LiBF 4 , LiAsF 6 , LiPF 6 , LiCF 3 SO 3 , LiC(CF 3 SO 2 ) 3 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 F) 2 , LiSbF 6 , LiPF 3 (CF 2 CF 3 ) 3 , LiPF 3 (CF 3 ) 3 , LiB(C 2 O 4 ) 2 (In the formula, R 13 = Hydrocarbon and X 7 = F, Cl, I or Br) and combinations thereof, preferably LiSCN, LiN(CN) 2 , LiClO 4 , LiI, LiBF 4 , LiAsF 6 , LiCF 3 SO 3 , LiCF 3 (SO 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 F) 2 , LiSbF 6 , LiPF 3 (CF 2 CF 3 ) 3 , LiPF 3 (CF 3 ) 3 , LiB(C 2 O 4 ) 2 and combinations thereof, more preferably the lithium salt is LiN(SO 2 CF 3 ) 2 Or LiN(SO 2 F) 2 and most preferably, the lithium salt is LiN(SO 2 F) 2 2. The battery of claim 1 ,
7. The first monomer has the formula (III): 【Chemistry 3】 2. The battery of claim 1, represented by the formula: wherein o is an integer selected from 5 to 150, preferably 8 to 100, more preferably 10 to 50.
8. The second monomer is represented by formula (IV): 【Chemistry 4】 2. The battery of claim 1 , wherein:
9. 2. The battery of claim 1, wherein the weight ratio of the first monomer to the second monomer is from 1:20 to 20:1 (w / w), preferably from 1:10 to 14:1 (w / w), more preferably from 1:5 to 12:1 (w / w), even more preferably from 1:3 to 10:1 (w / w), and most preferably from 1:2 to 2:1 (w / w).
10. 2. The battery of claim 1, wherein the copolymer is obtained by reaction of the first monomer with the second monomer with the use of a photoinitiator.
11. The battery of claim 1 , wherein the copolymer is subjected to a thermal annealing process.
12. The second lithium salt is Li 2 CO 3 、Li 2 O、Li 2 C 2 O 4 、LiOH、LiX 8 、R 14 OCO 2 Li、HCOLi、R 14 OLi、Li 2 O、Li 2 C 2 O 4 、(ROCO 2 Li) 2 、(CH 2 OCO 2 Li) 2 、Li 2 S、LiSCN、LiN(CN) 2 、LiClO 4 、LiBF 4 、LiAsF 6 、LiPF 6 、LiCF 3 SO 3 、LiC(CF 3 SO 2 ) 3 、LiN(SO 2 C 2 F 5 ) 2 、LiN(SO 2 CF 3 ) 2 、LiN(SO 2 F) 2 、LiSbF 6 、LiPF 3 (CF 2 CF 3 ) 3 、LiPF 3 (CF 3 ) 3 、LiB(C 2 O 4 ) 2 (wherein R 14 =hydrocarbon and X 8 =F, Cl, I or Br), preferably, LiSCN, LiN(CN) 2 、LiClO 4 、LiI、LiBF 4 、LiAsF 6 、LiCF 3 SO 3 , LiCF 3 (SO 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 F) 2 , LiSbF 6 , LiPF 3 (CF 2 CF 3 ) 3 , LiPF 3 (CF 3 ) 3 , LiB(C 2 O 4 ) 2 and combinations thereof, more preferably the lithium salt is LiN(SO 2 CF 3 ) 2 Or LiN(SO 2 F) 2 and most preferably, the lithium salt is LiN(SO 2 F) 2 2. The battery of claim 1 ,
13. The organic non-fluorinated liquid is selected from the group consisting of N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxene, diethyl ether, allyl ether, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), tetraethylene glycol dimethyl ether (tetraglyme), butyl diglyme, polyethylene glycol, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, ethyl methoxymethane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidone, methyl propionate, ethyl propionate, 1 2. The battery of claim 1, wherein the organic non-fluorinated liquid is selected from the group consisting of 1,3-dioxolane, 1,4-dioxane, tetrahydrofuran, allyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, butyl diglyme, dimethyl ether, diethyl ether, polyethylene glycol, acetonitrile, dimethyl sulfoxide, sulfolane, trimethyl phosphate, triethyl phosphate, dimethyl methyl phosphonate, hexamethyldisiloxane, hexamethylcyclotrisiloxane, 1,2-dimethoxyethane or 1,2-diethoxyethane, and most preferably the non-fluorinated organic liquid is 1,2-dimethoxyethane.
14. The fluorinated liquid is selected from the group consisting of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl)ether (BTFE), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), tris(2,2,2-trifluoroethyl)orthoformate (TFEO), methoxynonafluorobutane (MOFB), ethoxynonafluorobutane (EOFB), di(2,2,2-trifluoroethyl)carbonate (DTFEC), tris(2,2,2-trifluoroethyl)orthoformate (TFEO), tris(hexafluoroisopropyl)orthoformate (THFiPO), tris(2,2-difluoroethyl)orthoformate (TDFEO), bis(2,2 2. The battery of claim 1, wherein the fluorinated liquid is selected from the group consisting of 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl)ether (BTFEMO), tris(2,2,3,3,3-pentafluoropropyl)orthoformate (TPFPO), tris(2,2,3,3-tetrafluoropropyl)orthoformate (TTPO) and combinations thereof, preferably the fluorinated liquid is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), bis(2,2,2-trifluoroethyl)ether (BTFE) or 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), and most preferably 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE).
15. 2. The battery of claim 1, wherein the positive electrode comprises a positive electrode material selected from the group consisting of lithium nickel-manganese-cobalt oxide, lithium nickel-manganese oxide, lithium nickel-cobalt-aluminum oxide, lithium cobalt oxide, lithium iron phosphate, lithium iron manganese phosphate, lithium iron cobalt phosphate, lithium sulfide, sulfur, and aluminum, preferably the positive electrode material is lithium nickel-manganese-cobalt oxide or lithium nickel-cobalt-aluminum oxide.
Citation Information
Patent Citations
Polymeric solid electrolyte and lithium secondary battery adopting the same
JP1998116516A
Negative electrode for lithium metal battery and lithium metal battery including the same
JP2017204468A
Polymer for electrode protection layer and secondary battery using same
JP2021507464A
Lithium polymer secondary battery having protective thin film of crosslinked polymer and method for producing the same
KR1020030042288A
Electrodes Including a Passivation Layer
US20190379040A1