Alumina-based fused grain
The alumina-based fused grains with a tailored chemical composition and controlled calcination process address the inefficiencies of prior art, achieving superior machining efficiency and energy efficiency for both hard and stainless steels.
Patent Information
- Application Number
- JP2024536107
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-15
- Filing Date
- 2022-12-15
- Publication Date
- 2024-12-05
AI Technical Summary
Existing alumina-based fused grains used as abrasives face challenges in achieving high performance and energy efficiency, with compositions optimized for fused grains not applicable to sintered grains and vice versa, and there is a need to enhance their effectiveness while maintaining or exceeding the energy efficiency of prior art granules.
A specific chemical composition for alumina-based fused grains, including MgO: 2.5%~5.8%, Cr2O3: 0.2%~4.5%, and Al2O3: remainder, with optional calcination at controlled temperatures, resulting in a microstructure with Cr partially in metallic form at crystal boundaries, enhancing mechanical cohesion and abrasive properties.
The proposed composition and manufacturing process result in alumina-based fused grains with improved machining efficiency and reduced energy consumption, suitable for both hard steels and stainless steels, with enhanced abrasive performance.
Smart Images

Figure 2024545254000001 
Figure 2024545254000002 
Figure 2024545254000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an alumina-based fused grain, to a mixture of said grains, to a method for producing said grains, and to an abrasive tool comprising said mixture of grains. The present invention also relates to the use of the grains according to the invention for abrading steel surfaces. [Background technology]
[0002] Abrasive tools are generally classified according to how the abrasive grains are prepared: free abrasives (powder of the abrasive grains, not attached to a backing, used in a spray or suspension), coated abrasives (a cloth or paper backing on which the abrasive grains are arranged in several layers), and bonded abrasives (round stones, sticks, etc.).
[0003] In bonded abrasive grains, the grains are pressed with an organic or vitreous bond, commonly a bond consisting essentially of a silicated oxide. The grains must have good mechanical abrasive properties in themselves and good mechanical cohesion with the bond, i.e., the interface must be solid.
[0004] Among the abrasive grains, a distinction is made between fused grains and sintered grains, which have different microstructures. Therefore, the problems posed by sintered grains and fused grains, and the technical solutions adopted to solve them, are generally different. Therefore, a composition developed to produce fused grains cannot be used a priori to produce sintered grains with the same properties, or vice versa.
[0005] International Publication No. WO2004 / 094554 describes aluminous fused grains containing 1.5% to 6.5% MgO, expressed as a percentage by weight on an oxide basis.
[0006] US Patent No. 2,279,260 describes a Cr alloy containing more than 8% by weight. 2 O 3 In order to limit the formation of spinel within the grains, the presence of more than 2% MgO is required to incorporate at least one acidic oxide, e.g., SiO 2 , TiO 2 , ZrO 2 Or B 2 O 3 , requires the existence of Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, in order to improve the performance of alumina-based melts, in particular To increase the efficiency in applications where the molten grain is used as an abrasive while maintaining an energy efficiency greater than or substantially equivalent to that of prior art grains, or Similarly, in order to increase the energy efficiency while maintaining an efficacy higher than or substantially equivalent to that of the prior art granules, The need continues.
[0008] One object of the present invention is to meet, at least in part, this need. [Means for solving the problem]
[0009] According to the invention, this object is achieved by a fused grain, which may optionally be calcined, having the following chemical analysis, in weight percent on an oxide basis: MgO: 2.5%~5.8%; Cr 2 O 3 :0.2%~4.5%; MgO, Cr 2 O 3 and Al 2 O 3 Other oxides≦1.5%; Al 2 O 3 : Remaining to 100%.
[0010] As will be seen in more detail in the remainder of this specification, the inventors have discovered that the above chemical composition provides greater efficiency and / or energy efficiency than that of known alumina fused grains.
[0011] The fused grains according to the present invention may also have one or more of any of the following characteristics: as a percentage by weight based on the oxides: MgO≧2.7%, preferably MgO≧2.9%, preferably MgO≧3.1%, preferably MgO≧3.5%, preferably MgO≧4.0%, and / or preferably MgO≦5.5%, preferably MgO≦5.2%, preferably MgO≦5.1%, preferably MgO≦5%; As weight percent based on oxide, Cr 2 O 3 ≧0.3%, preferably Cr 2 O 3 ≧0.35%, preferably Cr 2 O 3 ≧0.4%, preferably Cr 2 O 3 ≧0.7%, preferably Cr 2 O 3 ≧1.0% and / or Cr 2 O 3 ≦4.0%, preferably Cr 2 O 3 ≦3.5%, preferably Cr 2 O 3 ≦3.0%, preferably Cr 2 O 3 ≦2.7%, preferably Cr 2 O 3 ≦2.5%, preferably Cr2 O 3 ≦2.2%, preferably Cr 2 O 3 ≦2%; MgO, Cr 2 O 3 and Al 2 O 3 the content of oxides other than, expressed as a percentage by weight based on the oxides, is less than 1.4%, preferably less than 1.3%, preferably less than 1.0%, preferably less than 0.9%, preferably less than 0.8%, preferably less than 0.7%, preferably less than 0.6%, preferably less than 0.5%, preferably less than 0.4%; As weight percent based on oxide, Na 2 O≦0.3%, preferably Na 2 O ≤ 0.1%; As weight percent based on oxide, SiO 2 ≦0.3%, preferably SiO 2 ≦0.1%; the carbon content, as a weight percentage based on the weight of the molten grain, is greater than 20 ppm, preferably greater than 50 ppm, preferably greater than 100 ppm, and / or less than 0.5%, preferably less than 0.3%, preferably less than 0.15%, preferably less than 0.1%; The amount of hydrogen gas released by hot acid etching is 15 cm 3 / Over 100g, preferably 30cm 3 / Over 100g, preferably 50cm 3 / Over 100g and / or 500cm 3 / Less than 100g, preferably 400cm 3 / Less than 100g, preferably 300cm 3 / Less than 100g, preferably 200cm 3 / 100g or less; the content of the oxide compound is, as a weight percentage based on the weight of the molten granules, greater than 96%, preferably greater than 97%; the fused grains have a microstructure consisting essentially of alumina crystallites, the crystallites being separated by boundaries at which the element Cr is located, at least partially in metallic form; and preferably For a mixture of the grains, the amount of hydrogen gas released by hot acid etching, expressed as the volume of gas per 100 g of grains, was 15 cm 3 / Over 100g and 500cm 3 / 100g or less, and / or the molten granules having a carbon content, as a weight percent based on the weight of the molten granules, greater than 20 ppm and less than 0.4%; The microstructure consists essentially of fused grain alumina crystals, wherein the crystals are composed of MgO, preferably substantially entirely non-stoichiometric and / or stoichiometric MgAl 2 O 4 Spinel form and / or non-stoichiometric and / or stoichiometric MgCr 2 O 4 The Cr elements are preferably at least partially separated by a boundary that is in the form of a spinel. 3+ and preferably is inserted into the crystal lattice of the alumina crystals in the form For a mixture of the grains, the amount of hydrogen gas released by hot acid etching, expressed as the volume of gas per 100 g of grains, was 15 cm 3 / 100g or less, and / or The molten grains have a carbon content, as a weight percent based on the weight of the molten grains, of less than 500 ppm.
[0012] In certain embodiments, MgO≧2.9% and MgO≦5.5%, and Cr 2 O 3 ≧0.3% and Cr 2 O 3 ≦4.0%, as well as MgO, Cr 2 O 3 and Al 2 O 3 The content of oxides other than those mentioned above is less than 1.3%; MgO≧3.1% and MgO≦5.2%, and Cr 2 O 3 ≧0.4% and Cr 2 O 3 ≦3.5%, as well as MgO, Cr 2 O 3 and Al2 O 3 The content of oxides other than those mentioned above is less than 1.0%; MgO≧3.5% and MgO≦5.1%, and Cr 2 O 3 ≧0.7% and Cr 2 O 3 ≦3.0%, as well as MgO, Cr 2 O 3 and Al 2 O 3 The content of oxides other than those mentioned above is less than 0.5%; MgO≧4.0% and MgO≦5.0%, and Cr 2 O 3 ≧1.0% and Cr 2 O 3 ≦2.5%, as well as MgO, Cr 2 O 3 and Al 2 O 3 The content of oxides other than 0.4% is less than 0.4%; The content of the oxide compound is more than 96%, preferably more than 97%, in each instance, as a weight percentage based on the weight of the molten granules.
[0013] In one embodiment, the fused grains according to the present invention have the following chemical analysis, as weight percentages based on the weight of the oxides: MgO: 2.5%~5.5%; Cr 2 O 3 :0.2%~3%; MgO, Cr 2 O 3 and Al 2 O 3 Other oxides≦1%; Al 2 O 3 : Remaining to 100%.
[0014] The invention also relates to a mixture of grains, which contains, in percentage by weight, more than 80% of fused grains according to the invention.
[0015] The present invention also provides a method for producing a molten grain mixture, the method comprising the steps of: a) mixing raw materials to form a feedstock suitable for the production of said grain mixture; b) melting said feedstock in a reducing medium until a molten material is obtained; c) cooling the molten material to completely solidify in less than 3 minutes to obtain a solid mass; d) optionally, in particular if no granules are obtained in step c), grinding the solid mass; e) Optionally, selecting a particle size. The method further comprises the steps of:
[0016] The element Cr is not conventionally introduced as an impurity in the Mg or Al sources in sufficient amounts to cause the content in the molten grain to exceed 0.2%. Preferably, the element Cr is intentionally, preferably by controlled addition, introduced into the feedstock to preferably contain more than 90 wt.%, preferably more than 95 wt.%, of Cr. 2 O 3 The addition of a powder having the desired content is carried out.
[0017] The manufacturing process according to the invention may also have one or more of the following optional features: The process comprises, after step c), preferably after step d), and preferably after step e) if the process comprises step e), a step f) of calcining the mixture of grains produced, wherein the calcination is preferably carried out in an oxidizing atmosphere, at a temperature preferably above 800° C., preferably below 1700° C., and wherein the maximum temperature reached during the calcination is preferably maintained for at least 30 minutes; In one embodiment, the calcination is carried out in an oxidizing atmosphere and at a temperature above 1280°C, preferably below 1700°C, where the maximum temperature reached during calcination is preferably maintained for at least 30 minutes: the resulting calcined fused grains have a microstructure consisting essentially of alumina crystallites, where the crystallites are composed of MgO, preferably substantially entirely non-stoichiometric and / or stoichiometric MgAl 2 O 4Spinel form and / or non-stoichiometric and / or stoichiometric MgCr 2 O 4 The Cr elements are preferably at least partially separated by a boundary that is in the form of a spinel. 3+ in the form of a crystalline lattice of the alumina crystals; if the fused grains obtained before step f) are according to the preferred embodiment described above, the amount of hydrogen gas released by hot acid etching, expressed as the volume of gas per 100 g of grains, is 15 cm 3 / 100g, and / or the calcined fused granules have a carbon content, as a weight percentage based on the weight of the fused granules, of less than 500 ppm; The method comprises, after step c), or after step d) if the method comprises step d), or after step e), if the method comprises step e), a step f) of calcination, preferably in an oxidizing atmosphere, at a temperature preferably above 800° C., or below 1280° C., wherein the maximum temperature reached during the calcination is preferably maintained for at least 30 minutes; the calcined fused grains obtained then have a microstructure consisting essentially of alumina crystallites, wherein said crystallites are separated by boundaries in which the element Cr is located, at least partially in metallic form; if the fused grains obtained before step f) are according to the preferred embodiment described above, the release of hydrogen gas by hot acid etching, expressed as a volume of gas per 100 g of grains, is greater than 15 cm 3 / Over 100g and 500cm 3 / 100g; and / or the calcined fused granules have a carbon content, as a weight percentage based on the weight of the fused granules, of greater than 30 ppm and less than 0.4%.
[0018] In one embodiment, the method does not include a step f) of firing after step c), or after step d), or after step e), at a temperature greater than 800° C. and less than 1700° C. In other words, the molten grains are used as abrasive grains, in particular bound by a binder, and agglomerated or deposited on a backing to form an abrasive tool without firing.
[0019] The present invention also relates to an abrasive tool comprising grains bonded by a binder and bonded or deposited on a support, the grains being, for example, in the form of a grinding wheel or deposited on a backing, such as a belt or disc, which is noted in that at least a portion of the molten grains, preferably more than 50%, preferably more than 70%, preferably more than 80%, preferably more than 90%, preferably more than 95%, preferably more than 99%, preferably all, by weight, are in accordance with the present invention.
[0020] The abrasive tool may in particular be a truing grinding wheel, a precision grinding wheel, a sharpening grinding wheel, a cut-off grinding wheel, a grinding wheel for machining from the body, a fettling or roughing grinding wheel, a regulating grinding wheel, a portable grinding wheel, a foundry grinding wheel, a drill grinding wheel, a mounted grinding wheel, a cylinder grinding wheel, a cone grinding wheel, a disk grinding wheel or a segmented grinding wheel, or any other type of grinding wheel.
[0021] In general, the present invention relates to a method for treating a surface, preferably a steel surface, which comprises abrading said surface with a mixture of grain according to the invention or with grain produced according to the method according to the invention.
[0022] Preferably, the method comprises: Producing a grain mixture according to the invention, preferably according to a manufacturing process according to the invention, then abrading said surface with said mixture of grains, preferably in the form of an abrasive tool according to the invention. Includes.
[0023] The grains according to the invention are especially recommended for the processing of steels, especially stainless steels and hard steels.
[0024] In one embodiment, the surface is made of hard steel and the fused grains of the mixture have a microstructure consisting essentially of alumina crystals, where the crystals are separated by boundaries at which the element Cr is located, at least partially in metallic form, and the release of hydrogen gas by hot acid etching, expressed as a volume of gas per 100 g of grain, is less than 15 cm 3 / Over 100g and 500cm 3 / 100g and / or has a carbon content of more than 20 ppm and less than 0.4%, preferably less than 500 ppm, as a percentage by weight based on the weight of the molten granules and / or is produced according to a method comprising a step f) of calcining, preferably carried out in an oxidizing atmosphere and at a calcination temperature of less than or equal to 1280° C. Preferably, the molten granules are according to the first particular embodiment detailed below.
[0025] In one embodiment, the surface is made of stainless steel, and then the resulting fired fused grain has a microstructure consisting essentially of alumina crystallites, where the crystallites are composed of MgO, preferably substantially entirely non-stoichiometric and / or stoichiometric MgAl 2 O 4 Spinel form and / or non-stoichiometric and / or stoichiometric MgCr 2 O 4The alumina grains are separated by boundaries that are in spinel form, at least a portion of the Cr element is inserted into the crystal lattice of the alumina crystals, and preferably have a hydrogen gas release rate by hot acid etching of 15 cm3 as a weight percentage based on the weight of the fused grains, expressed as a volume of gas per 100 g of grains. 3 / 100g and / or has a carbon content of less than 500 ppm, as a weight percentage based on the weight of the fused granules, and / or is produced according to a method comprising a step f) of calcining, preferably carried out in an oxidizing atmosphere, at a calcination temperature of more than 1280° C., preferably less than 1700° C. Preferably, the fused granules are according to the second particular embodiment detailed below.
[0026] definition
[0027] The oxide content of the grains according to the invention is "MgO, Cr 2 O 3 and Al 2 O 3 The terms "compounds" refer to "oxides other than oxides" and relate to the overall content of each of the corresponding chemical elements expressed in their most stable oxide form, according to standard industry practice. Thus, suboxides, and optionally nitrides, oxynitrides, carbides, oxycarbides, carbonitrides, or metallic species of the elements listed above are included.
[0028] The term "impurities" refers to unavoidable components that are inevitably mixed with the raw materials. In particular, impurities are compounds belonging to the groups of oxides, nitrides, oxynitrides, carbides, oxycarbides, carbonitrides, and metallic species of sodium and other alkali metals, iron, and vanadium. As an example, in the sources of Al and Mg, SiO 2 , Fe 2 O 3 Or Na 2 O can be mentioned.
[0029] A "precursor" of an oxide is understood to mean a component capable of providing said oxide during the production of the grains or grain mixtures according to the invention.
[0030] A "grain" is a particle having all dimensions less than 20 mm.
[0031] "Alumina-based grain" refers to grain that contains greater than 85% alumina by weight, as a percentage on an oxide basis.
[0032] "Molten granules" or more generally "molten product" are understood to mean solid granules (or products) obtained by solidification by cooling of a molten material.
[0033] A "molten material" is a mass that has been liquefied by heating a feedstock, which may contain a small amount of solid particles, but the amount of these is insufficient to give the mass structure. To keep its shape, the molten material must be contained in a container. The oxide-based molten grains according to the invention are conventionally obtained by melting at above 1900°C.
[0034] The "median size" of a powder refers to the size that separates the particles into first and second populations of equal weight, where the first and second populations contain only particles having sizes equal to or greater than the median size, or individually less than the median size. The median size of a powder can be determined using a particle size distribution generated using a laser particle sizer.
[0035] In this specification, unless otherwise stated, all grain compositions are given as weight percentages based on the total weight of oxides in the grain. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] The following description is intended to be illustrative and not limiting of the invention.
[0037] Molten grains
[0038] The chemical composition of the molten grains according to the invention, preferably the mixture of grains according to the invention, preferably has one or more of the following optional characteristics: as a percentage by weight based on the oxides: MgO≧2.7%, preferably MgO≧2.9%, preferably MgO≧3.1%, preferably MgO≧3.5%, preferably MgO≧4.0%, and / or preferably MgO≦5.5%, preferably MgO≦5.2%, preferably MgO≦5%; As weight percent based on oxide, Cr 2 O 3 ≧0.3%, preferably Cr 2 O 3 ≧0.35%, preferably Cr 2 O 3 ≧0.4%, preferably Cr 2 O 3 ≧0.7%, preferably Cr 2 O 3 ≧1.0% and / or Cr 2 O 3 ≦4.0%, preferably Cr 2 O 3 ≦3.5%, preferably Cr 2 O 3 ≦3.0%, preferably Cr 2 O 3 ≦2.7%, preferably Cr 2 O 3 ≦2.5%, preferably Cr 2 O 3 ≦2.3%, preferably Cr 2 O 3 ≦2.2%, preferably Cr 2 O 3 ≦2%; MgO, Cr 2 O 3 and Al 2 O 3 the content of oxides other than, as a percentage by weight based on the oxides, is preferably less than 1.4%, preferably less than 1.3%, preferably less than 1.0%, preferably less than 0.9%, preferably less than 0.8%, preferably less than 0.7%, preferably less than 0.6%, preferably less than 0.5%, preferably less than 0.4%; MgO, Cr 2 O 3 and Al 2 O 3 The oxides other than are preferably impurities; The Na 2 The O content, as a percentage by weight based on the oxide, is preferably less than 0.3%, preferably less than 0.25%, preferably less than 0.2%, preferably less than 0.15%, preferably less than 0.1%; The SiO 2 the content, as a percentage by weight based on the oxide, is preferably less than 0.3%, preferably less than 0.2%, preferably less than 0.15%, preferably less than 0.1%, preferably less than 0.08%, preferably less than 0.05%; the content of oxide compounds is, as a weight percentage based on the weight of the molten granules, greater than 96%, preferably greater than 97%, preferably greater than 98%, or greater than 99%, or greater than 99.4%, or greater than 99.5%, or greater than 99.6%, or greater than 99.7%; In one embodiment, the fused grains are unsintered and the carbon content, as a weight percentage based on the weight of the fused grains, is greater than 20 ppm, preferably greater than 30 ppm, preferably greater than 50 ppm, preferably greater than 100 ppm, and / or preferably less than 0.5%, preferably less than 0.4%, preferably less than 0.3%, preferably less than 0.25%, preferably less than 0.2%, preferably less than 0.15%, preferably less than 0.1%, preferably less than 0.08%.
[0039] In one embodiment, the molten grain is a molten grain that has been calcined. The amount of hydrogen gas released by the hot acid etching, expressed as the volume of gas per 100 g of grain, depends on the conditions under which the molten grain is calcined. It is measured as detailed in the examples.
[0040] In one embodiment, the fused grains are unsintered and preferably have a hydrogen gas release rate of 15 cm3 for a mixture of the grains, expressed as a volume of gas per 100 g of grain, upon hot acid etching. 3 / Over 100g, preferably 30cm 3 / Over 100g, preferably 50cm 3 / 100g and / or preferably 500cm 3 / Less than 100g, preferably 400cm 3 / Less than 100g, preferably 300cm 3 / Less than 100g, preferably 200cm 3 / 100g or less.
[0041] In a first particular embodiment, the fused grains have a microstructure consisting essentially of alumina crystals, the crystals being separated by boundaries at which the element Cr is located, at least partially in metallic form. 2 O 3 , MgO and Cr 2 O 3 The oxide other than the above is substantially entirely located at the boundary.
[0042] Preferably, the amount of hydrogen gas released by hot acid etching of the mixture of grains, expressed as the volume of gas per 100 g of grains, is 15 cm 3 / Over 100g, preferably 30cm 3 / Over 100g, preferably 50cm 3 / 100g and preferably 500cm 3 / Less than 100g, preferably 400cm 3 / Less than 100g, preferably 300cm 3 / Less than 100g, preferably 200cm 3 / 100g or less.
[0043] In this first particular embodiment, the molten grain preferably has a carbon content, as a weight percentage based on the weight of the molten grain, of greater than 20 ppm, preferably greater than 30 ppm, preferably greater than 50 ppm, preferably greater than 70 ppm, preferably greater than 100 ppm, and preferably less than 0.4%, preferably less than 0.3%, preferably less than 0.2%, preferably less than 0.15%, preferably less than 0.1%, preferably less than 800 ppm, preferably less than 600 ppm, preferably less than 500 ppm.
[0044] The fused grains according to this first embodiment preferably have a chemical analysis with the same preferences as those set forth above, except for carbon content and amount of hydrogen gas evolved by hot acid etching.
[0045] The fused and calcined grains according to the first particular embodiment are preferably produced according to a method according to the invention comprising a step f) of calcining in an oxidizing atmosphere, preferably at a temperature above 800° C., preferably above 900° C., and preferably below 1280° C., preferably below 1200° C., preferably below 1150° C., preferably below 1100° C., wherein the maximum temperature reached during said calcination is preferably maintained for at least 30 minutes, preferably at least 1 hour, preferably at least 2 hours.
[0046] The fused and sintered grain according to the first particular embodiment is particularly well suited for the machining of hard steel.The invention therefore relates to a polishing method according to the invention, in which the fused and sintered grain according to the first particular embodiment is applied to a surface made of hard steel in order to polish it.
[0047] In a second particular embodiment, the fused grains have a microstructure consisting essentially of alumina crystallites, where the crystallites are composed of MgO, preferably substantially entirely non-stoichiometric and / or stoichiometric MgAl 2 O 4 Spinel form and / or non-stoichiometric and / or stoichiometric MgCr 2 O 4 The Cr elements are preferably at least partially separated by a boundary that is in the form of a spinel. 3+ is inserted into the crystal lattice of the alumina crystals in the form of 2 O 3 , MgO and Cr 2 O 3 The oxide other than the oxide is located substantially entirely at the interface.
[0048] Preferably, the amount of hydrogen gas released by hot acid etching of the mixture of grains, expressed as the volume of gas per 100 g of grains, is 15 cm 3 / Less than 100g, preferably 10cm 3 / Less than 100g, preferably 5cm 3 / Less than 100g, preferably 1cm 3 / 100g or less.
[0049] In this second particular embodiment, the molten grains preferably have a carbon content, as a weight percentage based on the weight of the molten grain, of greater than or equal to 0 ppm and less than 500 ppm, preferably less than 400 ppm, preferably less than 300 ppm, preferably less than 200 ppm.
[0050] Fused grains according to this second embodiment preferably have the same preferred chemical analysis as described above, except for carbon content and hydrogen gas evolution upon hot acid etching.
[0051] The fused and calcined grains according to the second particular embodiment are preferably produced according to a method according to the invention comprising a step f) of calcining in an oxidizing atmosphere at a temperature above 1280° C., preferably above 1300° C., preferably below 1700° C., preferably below 1600° C., preferably below 1500° C., wherein the maximum temperature reached during said calcination is preferably maintained for at least 30 minutes, preferably at least 1 hour, preferably at least 2 hours.
[0052] The fused and sintered grain according to the second particular embodiment is particularly well suited for the machining of stainless steels.The invention therefore relates to a polishing method according to the invention, in which the fused and sintered grain according to the second particular embodiment is applied to a surface made of stainless steel in order to polish it.
[0053] The fused grains according to the invention therefore surprisingly make it possible to obtain high-performance machining of both hard and stainless steels, in particular as a function of the baking treatment applied to them.
[0054] Grain mixture
[0055] The mixture of grains according to the invention preferably comprises, as a percentage by weight, more than 85%, preferably more than 90%, preferably more than 95%, preferably more than 99%, preferably substantially 100% fused grains according to the invention.
[0056] Preferably, the grain mixture according to the invention complies with the grain size distribution of the mixture or grit as specified by FEPA Standard 43-GB-1984, R1993 and FEPA Standard 42-GB-1984, R1993.
[0057] Preferably, the grain mixture according to the invention is made using Ro-Tap 登録商標 The weight oversize, as a weight percentage, on a 16 mm screen, preferably on a 9.51 mm screen, as measured using a sieve shaker, is less than 1%.
[0058] Method for Producing a Molten Granule Mixture According to the Invention
[0059] The fused grains according to the invention can be produced according to the above-mentioned steps a) to e) which are conventional for the production of fused alumina-based grains, the parameters of which can, for example, take the values of the process used for the examples below.
[0060] In step a), the raw materials are conventionally weighed to the desired composition and then mixed to form the feedstock.
[0061] The Al, Mg and Cr in the feedstock are present virtually entirely in the molten grains. However, the elements Mg and Cr, especially in the form of oxides, can undergo fly-off phenomena during melting. The skilled person knows how to adjust the composition of the feedstock accordingly.
[0062] It therefore presents no difficulty for a person skilled in the art to select the raw materials of the feedstock so that the solid mass obtained at the end of step c) has a composition in accordance with that of the granules according to the invention.
[0063] The elements Mg and Cr are preferably oxides MgO and Cr 2 O 3 They are also conventionally introduced into the feedstock in the form of precursors of these oxides, for example MgCO 3 and / or chromium hydroxide. The element Al is preferably introduced at least in part into the form of Al 2 O 3 and / or in the form of a precursor of this oxide, for example in the form of aluminum hydroxide and / or boehmite. 2 O 3 and partly in metallic form into the feedstock.
[0064] In a preferred embodiment, the feedstock comprises a compound that generates a reducing medium during melting.
[0065] Preferably, the compound is selected from a carbon source, a metal and mixtures thereof. Preferably, the carbon source is selected from carbon, petroleum coke, pitch, coal and mixtures thereof, preferably petroleum coke. Preferably, the metal is aluminum.
[0066] More preferably, the compounds which generate the reducing medium during melting and which are used in the feedstock are petroleum coke and aluminum.
[0067] The skilled person knows how to determine the amount of compounds in the feedstock which generate a reducing medium during melting, in order to obtain melting in a reducing medium in step b).
[0068] Preferably, the feedstock comprises an amount of compounds which form a reducing medium during melting that is greater than 1% by weight, preferably greater than 1.5% by weight, and preferably less than 5% by weight, preferably less than 4% by weight, based on the feedstock.
[0069] In step b), an electric arc furnace, preferably of the Heroult type with graphite electrodes, is preferably used, but any known furnace may be used, for example an induction furnace or a plasma furnace, provided that it makes it possible to melt the feedstock in a reducing medium.
[0070] Melting in a reducing medium is preferably obtained by the presence in the feedstock of compounds which generate a reducing medium during melting and / or by the electrodes being immersed in a bath of molten material.
[0071] Preferably, the feedstock contains elements which generate reducing agents during melting.
[0072] Preferably, the raw materials are melted at atmospheric pressure.
[0073] Preferably, an electric arc furnace is used with a vessel of 70 liters capacity and a melting energy before casting of more than 2 kWh / kg of raw materials at a power of more than 220 kW, or an electric arc furnace of a different capacity used under equivalent conditions. The skilled person knows how to determine such equivalent conditions.
[0074] In step c), the cooling must be rapid, i.e., such that the molten material is completely solidified in less than 3 minutes. For example, the cooling can result by casting into a mold, as described in US Pat. No. 3,993,119, or by quenching.
[0075] Preferably, the molten material is completely solidified in less than 2 minutes, preferably less than 1 minute, preferably less than 40 seconds, preferably less than 30 seconds.
[0076] If in step c) it is not possible to obtain a mixture of grains directly or if these grains do not have a suitable particle size for the target application, comminution (step d) can be carried out according to conventional techniques.
[0077] In step e), size selection, e.g. by screening or cyclone, can be carried out if the previous steps do not result in a mixture of grains with a suitable grain size for the target application.
[0078] The process according to the invention preferably comprises a calcining step f) after step c) or, preferably, after step d) if the process comprises step d) or, preferably, after step e) if the process comprises step e).
[0079] The baking temperature is adapted to the nature of the surface to be polished, in particular when this surface is made of steel.
[0080] The calcination is preferably carried out in an oxidizing atmosphere at a temperature above 800° C. and preferably below 1700° C., where the maximum temperature reached during the calcination is preferably maintained for a period of at least 30 minutes, preferably at least 1 hour, preferably at least 2 hours.
[0081] Preferably, step f) is carried out at atmospheric pressure.
[0082] Preferably, step f) is carried out in air.
[0083] Advantageously, by carrying out step f), it is possible to further increase the effectiveness and / or the energy efficiency of the molten granules according to the invention.
[0084] In a first embodiment, in particular when the molten grains are intended for machining hard steel, in particular for machining hard steel after being incorporated into an abrasive tool, the method comprises a step f) of calcining, preferably in an oxidizing atmosphere, preferably in air, at a temperature of preferably more than 800°C, preferably more than 900°C and less than or equal to 1280°C, preferably less than 1200°C, preferably less than 1150°C, preferably less than 1100°C, wherein the maximum temperature reached during calcining is preferably maintained for a period of at least 30 minutes, preferably at least 1 hour, preferably at least 2 hours.
[0085] In a second embodiment, in particular when the molten grains are intended for machining stainless steels, in particular after being incorporated into an abrasive tool, the method comprises a step f) of calcining in an oxidizing atmosphere, preferably in air, at a temperature preferably above 1280° C., preferably above 1300° C. and preferably below 1700° C., preferably below 1600° C., preferably below 1500° C., wherein the maximum temperature reached during calcination is preferably maintained for a period of at least 30 minutes, preferably at least 1 hour, preferably at least 2 hours.
[0086] Method for manufacturing an abrasive tool according to the present invention
[0087] Methods for manufacturing abrasive tools are well known and can be used to manufacture abrasive tools according to the present invention.
[0088] The abrasive tool may in particular be formed by agglomerating grain according to the invention with a binder, in particular in the form of a grinding wheel, for example by pressing, or by adhering grain according to the invention with a binder to a backing, for example a belt or disk.
[0089] The binder can be inorganic, in particular glass (for example, a binder consisting of an oxide, essentially consisting of one or more silicates, can be used) or organic.
[0090] Organic binders are very suitable. They can be especially thermosetting resins. They are preferably selected from the group consisting of phenolic resins, epoxy resins, acrylate resins, polyester resins, polyamide resins, polybenzimidazole resins, polyurethane resins, phenoxy resins, phenol-furfural resins, aniline-formaldehyde resins, urea-formaldehyde resins, cresol-aldehyde resins, resorcinol-aldehyde resins, urea-aldehyde resins or melamine-formaldehyde resins, and mixtures thereof.
[0091] The binder may also incorporate organic or inorganic fillers, such as hydrated inorganic fillers (e.g., aluminum trihydrate or boehmite) or non-hydrated inorganic fillers (e.g., molybdenum oxide), cryolite, halogens, fluorspar, iron sulfide, zinc sulfide, magnesia, silicon carbide, silicon chloride, potassium chloride, manganese dichloride, potassium or zinc fluoroborate, potassium fluoroaluminate, calcium oxide, potassium sulfate, copolymers of vinylidene chloride and vinyl chloride, polyvinylidene chloride, polyvinyl chloride, and mixtures thereof. The binder may also include reinforcing fibers, such as glass fibers.
[0092] Conventionally, the mixture of grains according to the invention is mixed with a binder and, optionally, with an organic or inorganic filler. The resulting mixture, in which the binder conventionally represents 2% to 60%, preferably 20% to 40%, by volume, is shaped, for example, placed in a mold or deposited on a backing. The binder is then activated, for example by heating, to bond the grains to each other and / or to any backing material. After hardening of the binder and, optionally, after removal from the mold, an abrasive tool according to the invention is obtained.
[0093] Working Example
[0094] The following non-limiting examples are given for the purpose of illustrating the present invention.
[0095] Measurement protocol
[0096] The following measurement protocol was used to determine certain properties of the fused grain mixtures, which allows to nicely simulate the actual behavior of the grains when they are used for attrition.
[0097] To evaluate the abrasive performance of the grain mixture, a single layer of 1 gram of the mixture was applied to a metal wheel having a diameter of 12.7 cm, where the fused grains were bonded using a phenolic resin.
[0098] The surface of a plate made of 52100 hard steel or 304L stainless steel having dimensions of 20.5 cm x 7.6 cm x 6.0 cm is then machined with the obtained wheel in a constant reciprocating motion under a water spray, keeping the cutting depth constant at 20 μm and the wheel rotation speed constant at 3600 rpm. The total energy E generated by the wheel during machining is tot is recorded.
[0099] After the wheel is completely worn down, the weight of machined steel (i.e., the weight of steel removed by the grinding operation) "Ma ", weight of consumed grindstone "M m ”, and the volume of steel removed by the grinding operation “V a " is measured.
[0100] To evaluate the effectiveness, the ratio S of the weight of the machined steel divided by the weight of the grain consumed during machining is conventionally calculated (S = M a / M m ).
[0101] To evaluate the energy efficiency, the specific energy Es of a machining process is conventionally calculated, which is equal to the energy required to remove a unit volume of steel (Es = E tot / V a ).
[0102] To determine the composition of the fused grains, beads of a mixture of these grains are produced by melting the mixture and then chemically analyzed by X-ray fluorescence, except for the measurement of carbon content.
[0103] The carbon content of the molten grain is measured using a CS744 model carbon-sulfur analyzer sold by LECO.
[0104] The median size of a powder is routinely measured using an LA950V2 model laser particle sizer sold by Horiba.
[0105] After hot etching of the grains with a mixture of hydrochloric and hydrofluoric acids, the amount of hydrogen gas released by the hot acid etching is determined, and thus the reoxidation of suboxidized species (suboxides down to metals) is evaluated.
[0106] For this purpose, after magnetic separation, the particles are milled in a milling chamber made of oxidized material (for example alumina-zirconia-silica fused material) until a powder is obtained which passes through a sieve with a square mesh with 160 μm openings. 5 g of the powder are taken and then sieved on a 100 cm 3 The mixture is placed in a polypropylene reactor with a volume of 1000 g, and then 25 ml of the following acid mixture is added: 250 ml of 40% HF, 375 ml of 37% HCl, and 375 ml of water (for 1 liter). After the reactor is closed, etching is carried out in a water bath at 85° C. for 25 minutes with periodic stirring. After cooling the reactor, approximately 0.5 ml is withdrawn with a syringe through the septum and injected into a gas chromatograph (with 5 angstrom molecular sieves for the separation column and argon as carrier gas) equipped with a thermal conductivity detector. The results are expressed as the amount of gas under normal conditions per 100 g of ground grain.
[0107] This release is referred to as "hydrogen gas release due to hot acid etching."
[0108] Manufacturing Protocol
[0109] The example mixtures below were prepared from the following raw materials: Impurity, Na 2 O, CaO, Fe 2 O 3 , MgO, TiO 2 , SiO 2 an alumina powder having a purity of greater than 99.6% by weight and having a median diameter of 80 μm; Bayoxide by Lanxess 登録商標 C >98.5% by weight Cr, sold under the designation GN-R 2 O 3 Pigmentary chromium oxide with Cr content 2 O 3 powder; Magnesia powder having a purity of greater than 99% by weight, with greater than 85% by weight of the particles passing through a 45 μm screen mesh.
[0110] Reference Example 1 ("Reference"), which is outside the present invention, is a molten grain mixture according to the teachings of International Publication No. WO2004 / 094554 and serves as a comparison to Example 2.
[0111] The grain mixture of Example 2 was prepared according to the present invention according to the following manufacturing method: a) mixing raw materials to form a feedstock, wherein the feedstock comprises 1% by weight aluminum metal chips and 0.5% by weight petroleum coke; b) melting the feedstock in a single-phase electric arc furnace of the Heroult type equipped with graphite electrodes having a furnace vessel diameter of 0.8 m, a voltage of 125 V, a current of 1800 A and a specific supplied electric energy of 2 kWh / kg charged; c) quenching the molten material by means of an apparatus for casting between thin metal plates, as shown in US Pat. No. 3,993,119, to obtain a completely solid sheet constituting a solid mass; d) grinding the cooled solid mass of step c) to obtain a mixture of particles; e) Ro-Tap 登録商標 Selection is carried out by sorting out particles having a size of 500-600 μm using a sieve shaker.
[0112] Table 1 below gives the chemical composition of these mixtures and the results obtained.
[0113] The percent improvement in the S ratio is calculated by the following formula: 100×(ratio S of the mixture of the example being considered−ratio S of the mixture of Reference Example 1) / ratio S of the mixture of Reference Example 1.
[0114] A positive and high value of the percentage of significant improvement in the ratio S is sought, preferably with a decrease in the specific energy (positive value of the percentage decrease in the specific energy Es described below) without a significant increase in the specific energy. We consider an improvement of more than 5% in the ratio S to be significant.
[0115] Preferably, the ratio S is improved by more than 10%, preferably more than 15%, preferably more than 20%, preferably more than 25%, preferably more than 30%, preferably more than 35%.
[0116] The percentage reduction in specific energy, Es, is calculated by the following formula: 100×(Es of the mixture of Reference Example 1−Es of the mixture of the example to be considered) / Es of the mixture of Reference Example 1.
[0117] The percentage decrease in the specific energy Es during the test is required to be positive and high, without degradation and preferably with an improvement in the ratio S compared to the reference. We consider a decrease in the specific energy Es of more than 5% to be significant. Preferably, the specific energy is decreased by more than 10% (compared to the reference), preferably by more than 15%.
[0118] [Table 1]
[0119] Comparison between Reference Example 1 and Example 2 according to the present invention shows that the mixture contains 2.5% to 5.8% MgO and 0.4% Cr. 2 O 3 The positive effect of the presence of Cr 2 O 3 content, the specific S is improved by 4% and the specific energy is reduced by 12% when machining 52100 hard steel.
[0120] Example 2 shows that the green molten grains make it possible to reduce the specific energy, and the ratio S does not increase significantly.
[0121] The following additional examples were made: the grain mixture of Example 1 and the grain mixture of Example 2 were subjected to calcination heat treatment to obtain a grain mixture according to Example 3 and a grain mixture according to Example 4, respectively. The calcination was performed at 1000° C. in air, the temperature of 1000° C. was maintained for 2 hours, and the ramp rate to the temperature of 1000° C. was equal to 300° C. / hour.
[0122] The results obtained with these mixtures are provided in Table 2 below.
[0123] [Table 2]
[0124] Comparison between Reference Example 3 and Example 4 according to the present invention shows that the Cr content is 0.4%. 2 O 3 The effect of the presence of and in particular of a firing process carried out at a temperature of 1000° C. is shown: when machining 52100 hard steel, the specific S is improved by 47% and the specific energy is reduced by 45%.
[0125] The grains of Example 4 have a microstructure consisting essentially of alumina crystallites, which are separated by boundaries along which the element Cr, and substantially all elements other than Al, Mg and Cr, are located, at least partially in metallic form.
[0126] The following additional examples were made: the grain mixture of Example 1 and the grain mixture of Example 2 were subjected to a calcination heat treatment to obtain a grain mixture according to Example 5 and a grain mixture according to Example 6, respectively. The calcination was carried out at 1400° C. in air, the temperature of 1400° C. was maintained for 2 hours, and the ramp rate to the temperature of 1400° C. was equal to 300° C. / hour.
[0127] The results obtained with these mixtures are provided in Table 3 below.
[0128] [Table 3]
[0129] Comparison between Reference Example 5 and Example 6 according to the present invention shows that the Cr content is 0.4%. 2 O 3 The effect of the presence of and in particular of a firing process carried out at a temperature of 1400° C. is shown: when machining 304L stainless steel, the specific S is improved by 32% and the specific energy is reduced by 21%.
[0130] The following additional examples were generated:
[0131] The grain mixtures of Examples 7 to 11 were prepared according to the following manufacturing method: a) mixing raw materials to form a feedstock, the feedstock comprising 2% by weight aluminum metal chips and 0.5% by weight petroleum coke; b) melting the feedstock in a single-phase electric arc furnace of the Heroult type equipped with graphite electrodes having a furnace vessel diameter of 0.8 m, a voltage of 215 V, a current of 1040 A and a specific supplied electric energy of 3 kWh / kg charged; c) quenching the molten material by means of an apparatus for casting between thin metal plates, as shown in US Pat. No. 3,993,119, to obtain a completely solid sheet constituting a solid mass; d) grinding the cooled solid mass of step c) to obtain a mixture of particles; e) Ro-Tap 登録商標 Selection is carried out by sorting out particles having a size of 500-600 μm using a sieve shaker.
[0132] Table 4 below provides the chemical composition of these mixtures.
[0133] [Table 4]
[0134] Table 5 below shows the results obtained for the mixtures of grains of Reference Example 1 and Examples 2, 7, 8 and 9, as well as the MgO and Cr content for each of these examples. 2 O 3 provides the remainder of the content.
[0135] [Table 5]
[0136] Comparison of Reference Example 1, Examples 2, 7, and 8 according to the invention, and Example 9 outside the invention shows that the Cr content in the mixture containing 3.1% to 4.1% MgO is 2 O 3 Show the effect of the presence of: 0.4%~4.1% Cr 2 O 3 In the case of the content of , the specific S is improved by 4%, 31% and 19% in Examples 2, 7 and 8, respectively, and the specific energy is reduced by 12%, 6% and 15% in Examples 2, 7 and 8, respectively. 5% Cr 2 O 3 In the case of Example 9 having a content of 0.1g / g, the specific S improved by 25%, but the specific energy increased by 17%.
[0137] A comparison of Reference Example 1 with Example 7 according to the invention (having MgO contents of 3.6% and 3.1%, respectively) shows that the grains of Example 7 have a 31% improvement in specific S and a 6% reduction in specific energy compared to the grains of Reference Example 1.
[0138] Table 6 below shows the results obtained for the mixtures of grains of Reference Example 1 and Examples 10 and 11, as well as the MgO and Cr content for each of these examples. 2 O 3 provides the remainder of the content.
[0139] [Table 6]
[0140] Comparison of Reference Example 1, Example 10 according to the present invention, and Example 11 outside the present invention shows that the MgO content is 7%, Cr 2 O 3 The grains of Example 11, having a MgO content of 1.7%, show a 34% reduction in specific S and a 7% reduction in specific energy compared to the reference grains, unlike the grains of Example 10, which have an MgO content of 5.2% and a Cr 2 O 3 It has a content of 2%, which shows a 9% reduction in specific S and a 6% reduction in specific energy compared to the reference grain.
[0141] As has now been demonstrated, the present invention provides a mixture of alumina-based fused grains that have better efficacy and energy efficiency than known alumina-based grains.
[0142] Of course, the invention is not limited to the described embodiments, which are provided by way of illustrative and non-limiting examples.
[0143] In particular, molten grains according to the present invention are not limited to any particular shape or size.
Claims
1. Fused grain having the following chemical analysis as weight percent based on the following oxides: MgO: 2.5%-5.8%; Cr 2 O 3 :0.2%~4.5%; MgO, Cr 2 O 3 and Al 2 O 3 Other oxides≦1.5%; Al 2 O 3 : Remaining up to 100%.
2. Cr 2 O 3 ≦4.0%, and / or MgO, Cr 2 O 3 and Al 2 O 3 The content of oxides other than those mentioned above is less than 1.3%. The molten granules according to claim 1.
3. MgO: 2.5%-5.5%; Cr 2 O 3 :0.2%~3%; MgO, Cr 2 O 3 and Al 2 O 3 Other oxides≦1%; Al 2 O 3 : Remaining to 100% The molten granules of claim 2 .
4. MgO≧2.9%, and / or MgO≦5.5%, and / or Cr 2 O 3 ≧0.3%, and / or The content of the oxide compound is greater than 96% by weight based on the weight of the molten grains; The molten granules according to any one of claims 1 to 3.
5. MgO≧3.1%, and / or MgO≦5.2%, and / or Cr 2 O 3 ≧0.4%, and / or MgO, Cr 2 O 3 and Al 2 O 3 and / or The content of the oxide compound is greater than 97% by weight based on the weight of the molten granules; The molten granules according to claim 4.
6. MgO≧3.5%, and / or MgO≦5.1%, and / or Cr 2 O 3 ≧0.7%, and / or Cr 2 O 3 ≦3.0%, and / or MgO, Cr 2 O 3 and Al 2 O 3 The content of oxides other than those mentioned above is less than 0.5%. The molten granules according to claim 5.
7. MgO≧4.0%, and / or MgO≦5.0%, and / or Cr 2 O 3 ≧1.0%, and / or Cr 2 O 3 ≦2.5%, and / or MgO, Cr 2 O 3 and Al 2 O 3 The content of oxides other than those mentioned above is less than 0.4%. The molten granules according to claim 6.
8. As weight percent based on oxide, Na 2 O≦0.3%, and / or As weight percent based on oxide, SiO 2 ≦0.3% The molten granules according to any one of claims 1 to 7.
9. Na as weight percent on oxide basis 2 O≦0.1%, and / or SiO as weight percent based on oxide 2 ≦0.1% The molten grain of claim 8 .
10. a carbon content, expressed as a weight percentage based on the weight of the molten grain, of greater than 20 ppm and less than 0.5%; and / or The amount of hydrogen gas released by hot acid etching of the mixture of the particles is 15 cm 3 / Over 100g and 500cm 3 / 100g or less, The molten granules according to any one of claims 1 to 9.
11. the carbon content is greater than 50 ppm, as a weight percentage based on the weight of the molten grain; and / or the carbon content is less than 0.3% as a weight percentage based on the weight of the molten grains; and / or The amount of hydrogen gas released by hot acid etching of the mixture of the particles was 30 cm 3 / 100g and / or The amount of hydrogen gas released by hot acid etching of the mixture of the particles was 400 cm 3 / 100g or less, The molten granules according to claim 10.
12. the carbon content is less than 0.15%, as a weight percentage based on the weight of the molten grains; and / or The amount of hydrogen gas released by hot acid etching of the mixture of the particles was 50 cm 3 / 100 and / or The amount of hydrogen gas released by hot acid etching of the mixture of the particles was 300 cm 3 / 100g or less, The molten granules according to claim 11.
13. the carbon content is less than 0.1% as a weight percentage based on the weight of the molten grains; and / or The amount of hydrogen gas released by hot acid etching of the mixture of the particles was 200 cm 3 / 100g or less, The molten granules of claim 12.
14. The fused grains according to any one of claims 1 to 9, wherein the fused grains have a microstructure consisting essentially of alumina crystallites, wherein the crystallites are separated by boundaries at which the element Cr is located, at least partially in metallic form.
15. For a mixture of said grains, the amount of hydrogen gas released by hot acid etching, expressed as the volume of gas per 100 g of grains, is 15 cm 3 / Over 100g and 500cm 3 / 100g and / or The molten granules have a carbon content, as a weight percentage based on the weight of the molten granules, of greater than 20 ppm and less than 0.4%. The molten granules of claim 14.
16. The fused grains have a microstructure consisting essentially of alumina crystallites, where the crystallites are composed of MgO, preferably substantially entirely non-stoichiometric and / or stoichiometric MgAl 2 O 4 Spinel form and / or non-stoichiometric and / or stoichiometric MgCr 2 O 4 Fused grains according to any one of claims 1 to 9, separated by boundaries which are in spinel form, at least a portion of the Cr element being intercalated within the crystal lattice of the alumina crystals.
17. For a mixture of said grains, the amount of hydrogen gas released by hot acid etching, expressed as the volume of gas per 100 g of grains, is 15 cm 3 / 100g and / or 17. The molten grain of claim 16, wherein the molten grain has a carbon content, as a weight percent based on the weight of the molten grain, of less than 500 ppm.
18. A mixture of grains comprising, as a percentage by weight, more than 80% of molten grains according to any one of claims 1 to 17.
19. 20. A method for producing a mixture of molten grains according to claim 18, comprising the steps of: a) mixing raw materials to form a feedstock suitable for the production of said mixture of grains; b) melting said feedstock in a reducing medium until a molten material is obtained; c) cooling the molten material so that it completely solidifies in less than 3 minutes to obtain a solid mass. The method comprises the successive steps of:
20. 20. The method according to claim 19, further comprising, after step c), a step d) of grinding the solid mass obtained at the end of step c) and / or a step e) of selecting a particle size.
21. 21. The method according to claim 19 or 20, which does not comprise a step f) of calcination at a temperature above 800° C. and below 1700° C. after step c), or after step d), or after step e).
22. 21. The method according to claim 19 or 20, comprising a step f) of calcining at a temperature above 800°C and below 1700°C.
23. 23. The method of claim 22, wherein the calcination step f) is carried out in an oxidizing atmosphere.
24. 24. The method according to claim 22 or 23, wherein the firing temperature is 1280°C or less.
25. 24. The method of claim 22 or 23, wherein the calcination temperature is greater than 1280°C.
26. A method for treating a surface, comprising abrading said surface with a mixture of grains according to claim 18 or with a mixture of grains produced according to the method according to any one of claims 19 to 25.
27. the surface is hard steel and the mixture of grains comprises, as a percentage by weight, more than 80% of fused grains according to claim 14 and / or has been produced according to the method of claim 24; or The surface is stainless steel, and the mixture of grains comprises, by weight percentage, greater than 80% of the fused grains of claim 16 and / or are produced according to the method of claim 25.
27. The method of claim 26.
28. 18. An abrasive tool comprising grains bonded by a binder and bonded or deposited on a support, at least a portion of the grains being fused grains according to any one of claims 1 to 17.
29. 29. The abrasive tool of claim 28, comprising greater than 80% fused grain of any one of claims 1-17.
30. 30. The abrasive tool of claim 28 or 29 in the form of a wheel, belt or disc.
31. 26. A method of making an abrasive tool, the method comprising adding a binder to grains followed by agglomerating the grains or depositing the grains on a backing, wherein at least a portion of the grains, preferably substantially all of the grains, are fused grains made according to the method of any one of claims 19 to 25.