Positive electrode material composition, positive electrode sheet and method for producing the same, battery, and power consumption device

The positive electrode material composition with a lithium-containing phosphate core and carbon shell, optimized for graphitization and conductive agent content, addresses the challenge of low energy density and rate performance in lithium phosphate batteries by enhancing both properties simultaneously.

JP2024545384AInactive Publication Date: 2024-12-06CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED

Patent Information

Application Number
JP2024515659
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-11-11
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Batteries using lithium-containing phosphates, such as lithium iron phosphate, face challenges in achieving both high energy density and good rate performance due to low electronic and ionic conductivity, which leads to increased internal resistance and polarization.

Method used

A positive electrode material composition is developed with a core portion of lithium-containing phosphate and a shell portion of carbon material, where the graphitization degree of the active material is between 10% to 50% and the mass percentage content of the conductive agent is between 0% to 1%, optimizing the balance between lithium ion and electron transfer speeds.

Benefits of technology

This composition enhances the energy density and rate performance of the battery by reducing polarization and maintaining a well-matched reaction rate between the positive and negative electrodes, while allowing for higher lithium-containing phosphate content without increasing conductive agent usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545384000001_ABST
    Figure 2024545384000001_ABST
Patent Text Reader

Abstract

The present application provides a positive electrode material composition, a positive electrode sheet and a method for preparing the same, a battery, and a power consuming device, the positive electrode material composition comprising a positive electrode active material and an optional positive electrode conductive agent, the positive electrode active material comprising a core portion and a shell portion located on at least a part of the surface of the core portion, the core portion comprising a lithium-containing phosphate, the shell portion comprising a carbon material, the graphitization degree of the positive electrode active material being g1, and the mass percentage content of the positive electrode conductive agent in the positive electrode material composition being w1, 10%≦g1≦50%, 0%≦w1≦1%. The battery of the present application can achieve both high energy density and good rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present application relates to the field of battery technology, and specifically to a positive electrode material composition, a positive electrode sheet and a method for manufacturing the same, a battery, and a power consuming device. [Background technology]

[0002] In recent years, batteries have been widely used in many fields, including energy storage power systems for hydroelectric, thermal, wind, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, and aerospace. As batteries become more widely used, their safety performance has become increasingly important. Lithium-containing phosphates, such as lithium iron phosphate, are one of the most popular cathode active materials due to their excellent safety performance, low cost, and abundant raw material supply. However, batteries using lithium-containing phosphates have low energy density and poor rate performance. Summary of the Invention

[0003] An object of the present application is to provide a positive electrode material composition that can achieve both high energy density and good rate performance in a battery, a positive electrode sheet and a method for producing the same, a battery, and a power consumption device.

[0004] A first aspect of an embodiment of the present application provides a cathode material composition including a cathode active material and a selectable cathode conductive agent, wherein the cathode active material includes a core portion and a shell portion located on at least a portion of the surface of the core portion, the core portion including a lithium-containing phosphate, and the shell portion including a carbon material, wherein, when a degree of graphitization of the cathode active material is g1 and a mass percentage content of the cathode conductive agent in the cathode material composition is w1, the ranges of 10%≦g1≦50% and 0%≦w1≦1% are satisfied.

[0005] The inventors have found through their research that a battery with a graphitization degree of 10% to 50% and a mass percentage of a positive electrode conductive agent in the positive electrode material composition of 0% to 1% can achieve both high energy density and good rate performance. Although the mechanism is unclear, the inventors believe that this effectively matches the migration rates of lithium ions and electrons, thereby reducing battery polarization, lowering the battery's internal resistance, and ensuring good rate performance. At the same time, this effectively matches the reaction rate of the positive electrode with the reaction rate of the negative electrode, thereby minimizing problems such as excessive accumulation of lithium ions on the negative electrode side during charging, increasing the viscosity of the negative electrode electrolyte, slowing lithium ion transfer, and increasing battery polarization. Furthermore, the inventors believe that reducing the amount of positive electrode conductive agent allows for a higher amount of lithium-containing phosphate, thereby enabling the battery to have a high energy density.

[0006] In any embodiment of the present application, 15%≦g1≦48% and 0%≦w1≦0.8%.

[0007] In any embodiment of the present application, 15%≦g1≦48% and 0%≦w1≦0.6%.

[0008] In any embodiment of the present application, 15%≦g1≦48% and 0%≦w1≦0.4%.

[0009] In any embodiment of the present application, 20%≦g1≦45% and 0%≦w1≦0.6%.

[0010] In any embodiment of the present application, 20%≦g1≦45% and 0%≦w1≦0.4%.

[0011] In any embodiment of the present application, 20%≦g1≦45% and 0%≦w1≦0.2%.

[0012] In any embodiment of the present application, 25%≦g1≦50% and 0%≦w1≦0.2%.

[0013] In any embodiment of the present application, 25%≦g1≦50% and w1 is 0%.

[0014] In any embodiment of the present application, 25%≦g1≦40% and w1 is 0%.

[0015] In any embodiment of the present application, 25%≦g1≦35% and w1 is 0%.

[0016] By further adjusting the graphitization degree g1 of the positive electrode active material and the mass percentage content w1 of the positive electrode conductive agent, the amount of the positive electrode conductive agent used can be further reduced without affecting the rate performance of the battery, thereby further improving the energy density of the battery.

[0017] In any embodiment of the present application, the graphitization degree g1 of the positive electrode active material is obtained by an X-ray diffraction method.

[0018] In any embodiment of the present application, the powder resistivity of the positive electrode active material is greater than 0 and not greater than 30 Ω·cm, and preferably 0.5 Ω·cm to 10 Ω·cm.

[0019] In any embodiment of the present application, the mass percentage content of carbon element in the positive electrode active material is 0.5% to 5%, and preferably 1% to 3.5%.

[0020] When the mass percentage content of carbon element is within the above range, the conductivity of the positive electrode active material can be improved, while the decrease in capacity per gram of the positive electrode active material due to an excessively thick shell can be avoided, and the processing performance of the positive electrode sheet can be prevented from being affected due to an excessively large specific surface area of ​​the positive electrode active material.

[0021] In any embodiment of the present application, the average particle size Dv50 of the positive electrode active material is 0.5 μm to 10 μm, and preferably 1 μm to 4 μm.

[0022] When the average particle size Dv50 of the positive electrode active material is within the above range, it is advantageous to improve the lithium ion and electron transmission performance, thereby further improving the cycle performance and rate performance of the battery, and it is also advantageous to have a high compressed density of the positive electrode sheet, thereby further improving the energy density of the battery.

[0023] In any embodiment of the present application, the positive electrode active material has a powder compaction density of 2.5 g / cm under a force of 3 tons. 3 This is advantageous for improving the energy density of the battery.

[0024] In any embodiment of the present application, the lithium-containing phosphate includes one or more selected from the group consisting of lithium iron phosphate, lithium manganese iron phosphate, and composite materials obtained by coating and / or doping the above materials.

[0025] In any embodiment of the present application, the molecular formula of the lithium-containing phosphate is LiFe 1-x-y Mn x M y PO4, where 0≦x≦1 and 0≦y<1, and M includes one or more transition metal elements other than Fe and Mn and non-transition metal elements, and preferably includes one or more elements selected from V, Nb, Ti, Co, Ni, Sc, Ge, Mg, Al, Zr, Mn, Hf, Ta, Mo, W, Ru, Ag, Sn, and Pb.

[0026] In any embodiment of the present application, the positive electrode conductive agent includes one or more selected from superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0027] In any embodiment of the present application, the mass percentage content w2 of the positive electrode active material in the positive electrode material composition is 97.0% or more, and preferably 97.0% to 98.2%, thereby enabling a battery with high energy density to be obtained.

[0028] In any embodiment of the present application, the positive electrode material composition further includes a positive electrode binder and / or a positive electrode dispersant. The positive electrode binder is used to improve adhesion between positive electrode active material particles and between the positive electrode active material and the positive electrode current collector so that the positive electrode sheet forms a good electronic network. The positive electrode dispersant can improve the stability of the positive electrode slurry, reduce the risk of cracking of the positive electrode membrane layer, and also improve the dispersibility of the positive electrode conductive agent.

[0029] In any embodiment of the present application, the mass percentage content w3 of the positive electrode binder in the positive electrode material composition is 1% to 3%.

[0030] In any embodiment of the present application, the mass percentage content w4 of the positive electrode dispersant in the positive electrode material composition is 0% to 0.5%.

[0031] A second aspect of the present application provides a positive electrode sheet including a positive electrode current collector and a positive electrode film layer provided on the positive electrode current collector, the positive electrode film layer including the positive electrode material composition of the first aspect of the present application.

[0032] In any embodiment of the present application, the areal density of the positive electrode sheet is 300 mg / 1540.25 mm 2 More than 410mg / 1540.25mm 2 Above, 450mg / 1540.25mm 2 More than 500mg / 1540.25mm 2 That's all.

[0033] Currently, in the prior art, it is believed that as the coating weight of the positive electrode sheet increases, the amount of positive electrode conductive agent used must be increased to prevent the internal resistance of the battery from deteriorating. However, the inventors discovered during research that when the positive electrode film layer contains the positive electrode material composition according to the first aspect of the present application, it is possible to achieve both high energy density and good rate performance in the battery, and that as the coating weight of the positive electrode sheet increases, it is not necessary to increase the amount of positive electrode conductive agent used. Instead, the amount of positive electrode conductive agent used can be reduced, and even eliminated, thereby improving the energy density of the battery without affecting the internal resistance and rate performance of the battery. The positive electrode material composition according to the first aspect of the present application contributes to improving the performance of thick-coated and / or high-packed-density battery systems, enabling the battery to achieve both high energy density and good rate performance.

[0034] In any embodiment of the present application, the areal density of the positive electrode sheet is represented by CW, and the unit is mg / 1540.25 mm 2 In this case, the positive electrode sheet satisfies 0≦100000×(w1 / CW)≦3.4, and preferably satisfies 0≦100000×(w1 / CW)≦1.8.

[0035] In any embodiment of the present application, the thickness H of the positive electrode film layer is 70 μm to 145 μm, and preferably 90 μm to 138 μm.

[0036] In any embodiment of the present application, when the thickness of the positive electrode film layer is H and is expressed in μm, the positive electrode sheet satisfies 0≦100000×(w1 / H)≦14, and preferably satisfies 0≦100000×(w1 / H)≦11.

[0037] In any embodiment of the present application, the compressed density PD of the positive electrode sheet is 2.55 g / cm 3 or more, preferably 2.58 g / cm 3 More preferably, it is 2.60 g / cm or more. 3 This is advantageous for improving the energy density of the battery.

[0038] In any embodiment of the present application, the positive electrode sheet further includes a conductive coating positioned between the positive electrode current collector and the positive electrode film layer to increase adhesion between the positive electrode current collector and the positive electrode film layer. Preferably, the conductive coating includes conductive carbon black and a binder. Preferably, the thickness of the conductive coating is greater than 0 μm and less than or equal to 2 μm.

[0039] In any embodiment of the present application, the electrical resistance of the positive electrode sheet is 0.1 Ω to 1 Ω, and preferably 0.1 Ω to 0.6 Ω, which is advantageous for improving the cycle performance and rate performance of the battery.

[0040] In any embodiment of the present application, the positive electrode current collector has a thickness of 10 μm to 18 μm.

[0041] A third aspect of the present application provides a method for producing a positive electrode sheet, the method comprising the steps of: supplying a positive electrode slurry; applying the positive electrode slurry to at least one surface of a positive electrode current collector; and drying and compressing the positive electrode slurry to obtain a positive electrode sheet, the positive electrode slurry including the positive electrode material composition of the first aspect of the present application and a solvent.

[0042] A fourth aspect of the present application provides a battery including the positive electrode material composition of the first aspect of the present application, the positive electrode sheet of the second aspect of the present application, or a positive electrode sheet produced by the production method of the third aspect of the present application.

[0043] A fifth aspect of the present application provides a power consuming device including the battery of the fourth aspect of the present application.

[0044] The battery of the present application can achieve both high energy density and good rate performance. The power consuming device of the present application includes the battery of the present application, and therefore has at least the same advantages as the battery. [Brief explanation of the drawings]

[0045] In order to more clearly explain the technical solutions of the embodiments of the present application, the drawings required in the embodiments of the present application will be briefly described below. It is obvious that the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on the drawings without any creative efforts.

[0046] [Figure 1] 1 is a schematic diagram of one embodiment of a battery cell of the present application. [Figure 2] FIG. 1 is an exploded schematic view of one embodiment of a battery cell of the present application. [Figure 3] 1 is a schematic diagram of one embodiment of a battery module of the present application. [Figure 4] 1 is a schematic diagram of one embodiment of a battery pack of the present application. [Figure 5] 5 is an exploded schematic view of the embodiment of the battery pack shown in FIG. 4. [Figure 6] 1 is a schematic diagram of one embodiment of a power consuming device that includes a battery of the present application as a power source.

[0047] The drawings are not necessarily drawn to scale. 1 battery pack 2 Upper housing 3 Lower housing 4 Battery Module 5 battery cells 51 cases 52 Electrode Assembly 53 Cover plate DETAILED DESCRIPTION OF THE INVENTION

[0048] Hereinafter, with appropriate reference to the drawings, specific embodiments of the present application will be described in detail, including the cathode material composition, cathode sheet and method for producing the same, battery, and power consumption device. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters or redundant description of substantially identical configurations may be omitted. This is to avoid unnecessary redundancy in the following description and to facilitate understanding by those skilled in the art. Note that the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0049] "Ranges" disclosed herein are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, with the selected lower and upper limits defining the boundaries of that particular range. Such defined ranges may be inclusive or exclusive of the end values, and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, reciting ranges of 60 to 120 and 80 to 110 for a particular parameter is understood to also contemplate ranges of 60 to 110 and 80 to 120. Furthermore, reciting minimum range values ​​of 1 and 2 and maximum range values ​​of 3, 4, and 5 also contemplates ranges of 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4, and 2 to 5. Unless otherwise specified, the numerical range "a to b" is represented by the abbreviation for any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0 to 5" indicates that all real numbers between "0 and 5" are listed herein, and "0 to 5" is an abbreviation for combinations of these numerical values. Furthermore, expressing a parameter as an integer greater than or equal to 2 (≧2) is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0050] Unless otherwise stated, all embodiments and preferred embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure content of the present application.

[0051] Unless otherwise stated, all technical features and preferred technical features of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure content of the present application.

[0052] Unless otherwise specified, all steps in the present application may be performed in order or randomly, but are preferably performed in order. For example, when the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed in order, or may include steps (b) and (a) performed in order. For example, when it is stated that the method may further include step (c), it means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or may include steps (a), (c), and (b), or may include steps (c), (a), and (b), etc.

[0053] Unless otherwise specified, the terms "comprise" and "include" used herein mean open-ended and may also be closed-ended. For example, the terms "comprise" and "include" may refer to further "comprising" or "including" other components not listed, or to "comprising" or "including" only the listed components.

[0054] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, any of the following conditions satisfy the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), or A and B are both true (or exist).

[0055] As used herein, the terms "plurality" and "plural types" mean two or more than two.

[0056] Unless otherwise stated, terms used herein have the known meanings commonly understood by those skilled in the art.

[0057] Unless otherwise specified, the numerical values ​​of each parameter referred to in this application can be measured using various test methods commonly used in the field, for example, according to the test methods provided in this application.

[0058] As a key component of batteries, the positive electrode active material has a significant impact on battery performance. Lithium-containing phosphates, such as lithium iron phosphate, are currently one of the most popular positive electrode active materials. However, batteries using lithium-containing phosphates have a lower energy density than ternary positive electrode active materials. To improve the energy density of batteries using lithium-containing phosphates, the coating weight and / or coating thickness of the lithium-containing phosphate is typically increased. However, previous studies have shown that the low electronic and ionic conductivity of lithium-containing phosphates leads to poor battery rate performance. Furthermore, increasing the coating weight and / or coating thickness of the lithium-containing phosphates results in a continuous deterioration of the battery rate performance. Therefore, further reductions in the amount of conductive agent used accelerate the deterioration of battery performance, particularly rate performance. To ensure good rate performance, it is necessary to increase the amount of conductive agent used. However, increasing the amount of conductive agent used results in a reduction in the amount of lithium-containing phosphate used, further reducing the energy density of the battery.

[0059] Therefore, currently, batteries using lithium-containing phosphates cannot effectively combine high energy density with good rate performance.

[0060] In the course of research, the inventors of the present application have found that by rationally adjusting the graphitization degree of the lithium-containing phosphate and the amount of the conductive agent used, it is possible to achieve both high energy density and good rate performance in a battery using the lithium-containing phosphate.

[0061] Positive electrode material composition

[0062] Specifically, a first aspect of an embodiment of the present application provides a positive electrode material composition.

[0063] The positive electrode material composition includes a positive electrode active material including a core portion and a shell portion located on at least a portion of the surface of the core portion, and an optional positive electrode conductive agent, wherein the core portion includes a lithium-containing phosphate and the shell portion includes a carbon material, and wherein, when the degree of graphitization of the positive electrode active material is g1 and the mass percentage content of the positive electrode conductive agent in the positive electrode material composition is w1, the ranges are 10%≦g1≦50%, and 0%≦w1≦1%.

[0064] Through extensive research into the energy density and rate performance of batteries, the inventors of the present application discovered that one of the key factors affecting the rate performance of batteries is the matching of the migration rates of lithium ions and electrons. During battery charging, lithium ions migrate from the bulk phase (or crystal lattice) of the lithium-containing phosphate to the surface, enter the electrolyte through the external electric field, then migrate to the surface of the negative electrode active material (e.g., graphite) through the electrolyte, and then enter the interior of the negative electrode active material (e.g., intercalate between the graphite layers). Simultaneously, electrons flow from the positive electrode to the negative electrode through the external circuit. During battery discharge, lithium ions desorb from the negative electrode active material, enter the electrolyte through the external electric field, migrate to the surface of the positive electrode active material through the electrolyte, and enter the bulk phase (or crystal lattice) of the positive electrode active material. Simultaneously, electrons flow from the negative electrode to the positive electrode through the external circuit. Therefore, the charge and discharge processes of a battery require the joint participation of lithium ions and electrons.

[0065] Lithium-containing phosphates have low electronic conductivity, and the main method currently used to improve their conductivity is to coat the surface of the lithium-containing phosphate with amorphous carbon. Coating with amorphous carbon improves the conductivity of the lithium-containing phosphate while also increasing the lithium-containing phosphate's permeability to the electrolyte, reducing battery polarization and improving the lithium ion migration rate. However, amorphous carbon has poor conductivity, and its effect on improving the conductivity of lithium-containing phosphates is limited. Therefore, in practical applications, a large amount of conductive agent must be used. Increasing the amount of conductive agent used reduces the amount of lithium-containing phosphate used, further reducing the battery's energy density, making it impossible to achieve both high energy density and good rate performance.

[0066] During the course of research, the inventors discovered that selecting a positive electrode active material with a graphitization degree of 10% or higher improves the conductivity of the lithium-containing phosphate, contributing to improved battery rate performance. However, during further research, the inventors discovered that a high graphitization degree of the positive electrode active material is not necessarily a good thing. When the graphitization degree of the positive electrode active material exceeds 50%, the rate performance of the battery using the positive electrode active material does not continue to improve, despite the positive electrode active material's excellent conductivity, and the rate performance of the battery decreases to a different extent as the charging current increases. At the same time, when the graphitization degree of the positive electrode active material exceeds 50%, the compression density of the positive electrode sheet also decreases, thereby reducing the battery's energy density. Furthermore, when the graphitization degree of the positive electrode active material exceeds 50%, it may result in a deterioration in battery cycle performance.

[0067] One factor is that when the graphitization degree of the positive electrode active material exceeds 50%, its excellent conductivity results in a significantly faster reaction rate at the positive electrode than at the negative electrode. During charging, excessive lithium ions accumulate on the negative electrode side, increasing the viscosity of the electrolyte on the negative electrode side, which is unfavorable to lithium ion transport and also increases battery polarization. When the graphitization degree of the positive electrode active material exceeds 50%, the performance of the carbon material in the shell may change qualitatively, with amorphous carbon tending to convert to graphitized carbon (or crystalline carbon). Because the interlayer distance of graphitized carbon (or crystalline carbon) is small, when it coats the surface of a lithium-containing phosphate, it inhibits the rapid insertion and extraction of lithium ions, worsening battery polarization and further impairing the battery's rate performance, especially high-rate charging performance. At the same time, when the graphitization degree of the positive electrode active material exceeds 50%, the nanopore structure of the carbon material decreases, which reduces the permeability of the lithium-containing phosphate to the electrolyte and slows the lithium ion migration rate, thereby further worsening the polarization of the battery and affecting the rate performance.In addition, when the graphitization degree of the positive electrode active material exceeds 50%, the shell part undergoes significant deformation during the lithium ion desorption and insertion process, which reduces the structural stability of the shell part and makes it more likely to fall off from the surface of the lithium-containing phosphate, not only reducing the conductivity of the lithium-containing phosphate but also increasing the irreversible consumption of lithium ions and affecting the cycle performance of the battery.

[0068] Furthermore, the inventors of the present application have further found through their research that when the graphitization degree of the positive electrode active material is 10-50%, using a high content of positive electrode conductive agent reduces the battery's energy density and is also detrimental to improving the battery's rate performance. In this case, the reaction rate of the positive electrode may be significantly faster than that of the negative electrode, resulting in excessive accumulation of lithium ions on the negative electrode side during charging, increasing the viscosity of the electrolyte on the negative electrode side, which is detrimental to lithium ion transport and increases battery polarization. Furthermore, due to the mismatch between the transfer rates of lithium ions and electrons, during battery operation, the electron transfer rate in the external circuit is too fast and the lithium ion transfer rate inside the battery is too slow, resulting in excessive battery polarization. The larger the battery's charging current, the more pronounced the battery polarization becomes, and the battery's rate performance, especially high-rate charging performance, is also poor.

[0069] In further research, the inventors found that a battery with a graphitization degree of 10% to 50% and a mass percentage of a positive electrode conductive agent in the positive electrode material composition of 0% to 1% can achieve both high energy density and good rate performance. Although the mechanism is unclear, the inventors believe that this effectively matches the transfer rates of lithium ions and electrons, thereby reducing battery polarization, lowering the battery's internal resistance, and ensuring good rate performance. At the same time, this effectively matches the reaction rate of the positive electrode with the reaction rate of the negative electrode, thereby minimizing problems such as excessive accumulation of lithium ions on the negative electrode side during charging, increasing the viscosity of the negative electrode electrolyte, slowing lithium ion transfer, and increasing battery polarization. Furthermore, the inventors believe that reducing the amount of positive electrode conductive agent allows for a higher amount of lithium-containing phosphate, thereby enabling the battery to have a high energy density.

[0070] In this application, the graphitization degree of the positive electrode active material refers to the graphitization degree of the carbon material in the shell of the positive electrode active material, and has the meaning known in the art and can be measured using equipment and methods well known in the art. For example, the graphitization degree can be measured using an X-ray diffraction apparatus, referring to JIS K 0131-1996 and JB / T 4220-2011. 002 and obtain the formula g=(0.344-d 002 The graphitization degree of the positive electrode active material can be calculated based on the formula: d 002 is the layer spacing of the C(002) plane in the crystal structure of the positive electrode active material, expressed in nanometers (nm). A Bruker D8 Discover X-ray diffractometer can be used as the test equipment.

[0071] In the present application, when the mass percentage content w1 of the positive electrode conductive agent in the positive electrode material composition is 0%, this indicates that the positive electrode material composition does not contain any positive electrode conductive agent.

[0072] In further research, the inventors have found that by further adjusting the degree of graphitization g1 of the positive electrode active material and the mass percentage content w1 of the positive electrode conductive agent, the amount of the positive electrode conductive agent used can be further reduced without affecting the rate performance of the battery, and thus the energy density of the battery can be further improved.

[0073] In some embodiments, 15%≦g1≦48% and 0%≦w1≦0.8%, preferably 15%≦g1≦48% and 0%≦w1≦0.6%, and more preferably 15%≦g1≦48% and 0%≦w1≦0.4%.

[0074] In some embodiments, 20%≦g1≦45% and 0%≦w1≦0.6%. Preferably, 20%≦g1≦45% and 0%≦w1≦0.4%. More preferably, 20%≦g1≦45% and 0%≦w1≦0.2%.

[0075] In some embodiments, 25%≦g1≦50% and 0%≦w1≦0.2%.

[0076] In some embodiments, 25%≦g1≦50% and w1 is 0%. In further studies, the inventors have found that by further adjusting the graphitization degree g1 of the positive electrode active material and the mass percentage content w1 of the positive electrode conductive agent, it is possible to remove the positive electrode conductive agent while ensuring good rate performance of the battery, thereby further improving the energy density of the battery.

[0077] In some embodiments, 25%≦g1≦40% and w1 is 0%. Preferably, 25%≦g1≦35% and w1 is 0%. By further adjusting the range of the graphitization degree g1 of the positive electrode active material, the battery can have high energy density, good rate performance, and good cycle performance. One factor is that in this case, the layer spacing of the shell portion is large, which improves its structural stability, which is advantageous for improving the electrolyte permeability of the positive electrode sheet and the lithium ion migration rate, and further provides the battery with good cycle performance.

[0078] In some embodiments, the powder resistivity of the positive electrode active material is greater than 0 and less than or equal to 30 Ω·cm, preferably 0.1 Ω·cm to 20 Ω·cm, 0.2 Ω·cm to 15 Ω·cm, 0.5 Ω·cm to 10 Ω·cm, 0.5 Ω·cm to 8 Ω·cm, or 0.5 Ω·cm to 5 Ω·cm.

[0079] In this application, the powder resistivity of a positive electrode active material has a meaning known in the art and can be tested using methods well known in the art. An exemplary test method involves weighing 1 to 5 g of a test sample, adjusting the depth of the powder resistivity meter's feed cavity, adding the test sample to the feed cavity, applying pressure, and recording the powder resistivity of the positive electrode active material at different pressures. The pressure continues to increase until the powder resistivity value no longer changes, at which point the test is stopped and the powder resistivity value is recorded as the powder resistivity of the positive electrode active material. A PRCD 2100 powder resistivity meter from INITIAL ENERGY SCIENCE & TECHNOLOGY (XIAMEN) Co., Ltd. (IEST) can be used as the test equipment.

[0080] In some embodiments, the mass percentage content of carbon element in the positive electrode active material is 0.5% to 5%. For example, the mass percentage content of carbon element in the positive electrode active material may be 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any range thereof, and preferably the mass percentage content of carbon element in the positive electrode active material is 1% to 4%, 1% to 3.5%, 1% to 3.2%, or 1% to 3%.

[0081] When the mass percentage content of carbon element is within the above range, the conductivity of the positive electrode active material can be improved, while the shell part is prevented from being too thick, which reduces the capacity per gram of the positive electrode active material, and the specific surface area of ​​the positive electrode active material is prevented from being too large, which affects the processing performance of the positive electrode sheet.

[0082] In some embodiments, the average particle size Dv50 of the positive electrode active material is 0.5 μm to 10 μm, and may be, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, or any range thereof. Preferably, the average particle size Dv50 of the positive electrode active material is 0.5 μm to 8 μm, 0.5 μm to 6 μm, 0.5 μm to 4 μm, 0.8 μm to 4 μm, or 1 μm to 4 μm.

[0083] When the average particle size Dv50 of the positive electrode active material is within the above range, it is advantageous to improve the lithium ion and electron transmission performance, thereby further improving the cycle performance and rate performance of the battery, and it is also advantageous to have a high compressed density of the positive electrode sheet, thereby further improving the energy density of the battery.

[0084] In this application, the average particle size Dv50 of the positive electrode active material has the meaning known in the art and refers to the particle size corresponding to the cumulative volume distribution percentage of the material reaching 50%. This can be measured using equipment and methods well known in the art. For example, it can be measured using a laser particle size analyzer in accordance with GB / T 19077-2016. A Mastersizer 2000E laser particle size analyzer can be used as the testing equipment.

[0085] In some embodiments, the positive electrode active material has a powder compaction density of 2.5 g / cm under a 3 ton force. 3 or more (≧2.5g / cm 3 This is advantageous for improving the energy density of the battery.

[0086] In this application, the powder compression density of the positive electrode active material has the meaning known in this field and can be measured by devices and methods well-known in this field. For example, referring to GB / T 24533-2009, it can be measured by an electronic pressure tester. As the test device, a UTM7305 type electronic pressure tester can be used. An exemplary test method is as follows. Weigh 1 g of the test sample, put it into a mold with a bottom area of 1.327 cm 2 and apply pressure up to 3 tons, hold the pressure for 30 s, then release the pressure and hold for 10 s. Then, record and calculate the powder compression density of the positive electrode active material under the acting force of 3 tons.

[0087] In some embodiments, the capacity per gram of the positive electrode active material is 157 mAh / g or more (≥157 mAh / g). This is advantageous for improving the energy density of the battery.

[0088] In some embodiments, the lithium-containing phosphate may include one or more of lithium iron phosphate, lithium manganese iron phosphate, and composite materials obtained by coating and / or doping and modifying the above materials.

[0089] In some embodiments, the molecular formula of the lithium-containing phosphate may be LiFe 1-x-y Mn x M y PO4, where 0 ≤ x ≤ 1, 0 ≤ y < 1, preferably 0 ≤ y ≤ 0.1, and M includes one or more selected from transition metal elements and non-transition metal elements other than Fe and Mn, preferably one or more selected from V, Nb, Ti, Co, Ni, Sc, Ge, Mg, Al, Zr, Mn, Hf, Ta, Mo, W, Ru, Ag, Sn, and Pb. As an example, the lithium-containing phosphate includes one or more selected from LiFePO4, LiMnPO4, LiFe 1-x1 Mn x1 PO4 (0 < x1 < 1, preferably 0.5 ≤ x1 ≤ 0.8).

[0090] In some embodiments, the mass percentage content w2 of the positive electrode active material in the positive electrode material composition is 97.0% or more (≧97.0%), preferably 97.0% to 98.2%, thereby enabling a battery with high energy density to be obtained.

[0091] The present application does not particularly limit the type of the positive electrode conductive agent, and materials well known in the art can be used. In some embodiments, the positive electrode conductive agent may include one or more selected from the group consisting of superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0092] In some embodiments, the positive electrode material composition may further include a positive electrode binder. The positive electrode binder is used to improve adhesion between positive electrode active material particles and between the positive electrode active material and the positive electrode current collector so that the positive electrode sheet forms a good electronic network. In the present application, the type of positive electrode binder is not particularly limited. For example, the positive electrode binder may include one or more selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0093] The low content of the positive electrode conductive agent in the positive electrode material composition of the present application allows the content of the positive electrode binder to be reduced, further improving the energy density of the battery. In some embodiments, the mass percentage content w3 of the positive electrode binder in the positive electrode material composition can be 0.5% to 3%, 1% to 3%, 1% to 2.5%, or 1% to 2%.

[0094] In some embodiments, the positive electrode material composition may further include a positive electrode dispersant. The positive electrode dispersant can improve the stability of the positive electrode slurry, reduce the risk of cracking of the positive electrode film layer, and improve the dispersibility of the positive electrode conductive agent. In the present application, the type of positive electrode dispersant is not particularly limited, and, for example, a positive electrode dispersant can be selectively used as needed. For example, the positive electrode dispersant can include one or more selected from a cellulose-based compound, polyalkylene oxide, polyvinyl alcohol, polyvinylpyrrolidone, polyvinyl acetal, polyvinyl ether, polyvinyl sulfonic acid, polyvinyl chloride, chitosan, starch, polyacrylamide, poly(N-isopropylacrylamide), poly(N,N-dimethylacrylamide), polyethyleneimine, polyoxyethylene, poly(2-methoxyethoxyethylene), poly(acrylamide-co-diallyldimethylammonium chloride), acrylonitrile / butadiene / styrene polymer, acrylonitrile / styrene / acrylate polymer, nitrile rubber, and fluororubber. In some embodiments, the mass percentage content w4 of the positive electrode dispersant in the positive electrode material composition may be 0% to 0.5%, and preferably is greater than 0 and less than or equal to 0.5%. When w4 is 0%, it indicates that the positive electrode material composition does not contain a positive electrode dispersant.

[0095] In some embodiments, the positive electrode material composition may simultaneously include a positive electrode binder and a positive electrode dispersant.

[0096] [Method for producing positive electrode active material]

[0097] In some embodiments, a cathode active material having a desired degree of graphitization can be obtained by mixing a cathode active material or a precursor thereof, an organic carbon source, and other optional components and placing the mixture in a protective atmosphere, and controlling the sintering temperature and / or sintering time, or by adding an auxiliary agent such as a graphite catalyst during the sintering process.

[0098] In some embodiments, the sintering temperature may be between 500°C and 1200°C, such as 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, or any range thereof.

[0099] In some embodiments, the sintering time may be 1 hour to 20 hours, such as 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, or any range thereof.

[0100] In some embodiments, the protective gas may include nitrogen, argon, helium, or a combination thereof.

[0101] In the present application, the type of organic carbon source is not particularly limited. In some embodiments, the organic carbon source may include carbonizable organic substances and derivatives thereof, such as one or more of starch, sucrose, glucose, fructose, maltose, chitosan, citric acid, alkanes, olefins, alcohols, esters, and polymers (e.g., polyvinyl alcohol, polyethylene, polypropylene, and polypyrrole).

[0102] In some embodiments, the graphite catalyst may include a metal or metal salt, such as nickel, nickel nitrate, or the like.

[0103] In some embodiments, the graphite catalyst may include a carbonizable organic compound having a cyclic structure and its derivatives. Preferably, the graphite catalyst may include one or more of naphthalene, phenanthrene, anthracene, pyrene, perylene, ferrocene, diphenylphosphine, and triphenylmethane.

[0104] In some embodiments, the graphite catalyst is added in an amount of 5% or less, preferably 3% or less, 2% or less, or 1% or less, based on the mass of the positive electrode active material.

[0105] In some embodiments, other components may be added as needed during the preparation of the positive electrode active material, for example, an additive may be included so that the shell further includes other components other than the carbon material. In some embodiments, the additive may be a component for improving a part of the performance of the battery, such as an additive for improving lithium ion transmission performance or an additive for improving the interface performance of the positive electrode active material, as long as these additive components do not detract from the spirit of the present application.

[0106] Positive electrode sheet

[0107] A second aspect of the present embodiment provides a positive electrode sheet comprising the positive electrode material composition of the first aspect of the present embodiment.

[0108] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer provided on the positive electrode current collector, the positive electrode film layer including the positive electrode material composition according to the first aspect of the present invention. For example, the positive electrode current collector has two surfaces facing each other in the thickness direction, and the positive electrode film layer is provided on one or both of the two facing surfaces of the positive electrode current collector.

[0109] In some embodiments, the positive electrode film layer may further include other positive electrode active materials for batteries known in the art, for example, the other positive electrode active materials may include one or more selected from lithium transition metal oxides and modified compounds thereof. The lithium transition metal oxides may be, for example, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and modified compounds thereof.

[0110] In some embodiments, the areal density of the positive electrode sheet is 300 mg / 1540.25 mm 2More than 410mg / 1540.25mm 2 Above, 450mg / 1540.25mm 2 More than 500mg / 1540.25mm 2 This is advantageous for improving the energy density of the battery.

[0111] Currently, in the prior art, it is believed that as the coating weight of the positive electrode sheet increases, the amount of positive electrode conductive agent used must be increased to prevent the internal resistance of the battery from deteriorating. However, the inventors discovered during their research that when the positive electrode film layer contains the positive electrode material composition according to the first aspect of the present embodiment, the battery can achieve both high energy density and good rate performance, and that as the coating weight of the positive electrode sheet increases, it is not necessary to increase the amount of positive electrode conductive agent used, but rather the amount of positive electrode conductive agent used can be reduced, and even the positive electrode conductive agent can be eliminated, which not only improves the energy density of the battery but also does not affect the internal resistance and rate performance of the battery.

[0112] The positive electrode material composition according to the first aspect of the present invention contributes to improving the performance of thickly coated and / or highly packed battery systems, and enables the battery to achieve both high energy density and good rate performance.

[0113] In some embodiments, the areal density of the positive electrode sheet is CW, and the unit is mg / 1540.25 mm 2 and the positive electrode sheet satisfies 0≦100000×(w1 / CW)≦3.4, and preferably satisfies 0≦100000×(w1 / CW)≦2.4, 0≦100000×(w1 / CW)≦1.8, 0≦100000×(w1 / CW)≦1.5, 0≦100000×(w1 / CW)≦1.

[0114] In some embodiments, the thickness H of the positive electrode film layer is 70 μm to 145 μm, preferably 90 μm to 138 μm.

[0115] In some embodiments, the thickness of the positive electrode film layer is H, expressed in μm, and the positive electrode sheet satisfies 0≦100000×(w1 / H)≦14, preferably 0≦100000×(w1 / H)≦11, 0≦100000×(w1 / H)≦8, or 0≦100000×(w1 / H)≦6.

[0116] In some embodiments, the positive electrode sheet has a compressed density PD of 2.55 g / cm 3 or more, preferably 2.58 g / cm 3 More than 2.60g / cm 3 More than 2.62g / cm 3 Above, ≧2.65g / cm 3 This is advantageous for improving the energy density of the battery.

[0117] In this application, the areal density of a positive electrode sheet has a meaning known in the art and can be tested using methods well known in the art. For example, a single-sided, cold-pressed positive electrode sheet (if the positive electrode sheet is double-sided, the positive electrode film layer on one side can be wiped off first) is taken, punched out into a small disk with an area of ​​S1, and its weight is recorded as M1. The positive electrode film layer is then wiped off from the weighed positive electrode sheet, and the weight of the positive electrode current collector is weighed and recorded as M0. The areal density of the positive electrode sheet = (M1 - M0) / S1.

[0118] In this application, the compression density of the positive electrode sheet has the meaning known in the art and can be tested by a method well known in the art: compression density of the positive electrode sheet = areal density of the positive electrode sheet / thickness of the positive electrode film layer.

[0119] In this application, the thickness of the positive electrode film layer has the meaning known in the art, and can be tested by a method well known in the art, for example, by using a spiral micrometer.

[0120] In some embodiments, the positive electrode sheet may further include a conductive coating positioned between the positive electrode current collector and the positive electrode film layer to increase adhesion between the positive electrode film layer and the positive electrode current collector. Of course, in some embodiments, the conductive coating may not be provided.

[0121] In some embodiments, the conductive coating includes conductive carbon black and a binder. The type of binder is not particularly limited, and any oil-based binder well known in the art can be used. For example, the binder may include one or more binders selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, and tetrafluoroethylene-hexafluoropropylene copolymer.

[0122] In some embodiments, the conductive coating has a thickness of greater than 0 and less than or equal to 2 μm.

[0123] In some embodiments, the electrical resistance of the positive electrode sheet is 0.1Ω to 1Ω, preferably 0.1Ω to 0.8Ω, 0.1Ω to 0.7Ω, or 0.1Ω to 0.6Ω, which is advantageous for improving the cycle performance and rate performance of the battery.

[0124] In this application, the electrical resistance of the positive electrode sheet has a meaning known in the art and can be tested using equipment and methods well known in the art. For example, the test can be performed using a double-probe resistance tester. For example, the test can be performed according to the following test method: A 4 cm x 25 cm sample is taken along the length of the positive electrode sheet, the double-probe resistance tester is started, the single-point mode is selected, and the test area of ​​the input terminal is 1540.25 mm. 2The number of parallel samples is 20, the pressure is 0.4t, and the time interval is 15 seconds. Place the test sample between the two probes, click the operation button on the software, then turn the directional valve downward. After 15 seconds, it will automatically collect one data point. The test method for replacing one point is as above. When all 20 points have been tested, replace the test sample and continue the test. The average of the above test results is the electrical resistance of the positive electrode sheet.

[0125] In some embodiments, the thickness of the positive electrode current collector may be 10 μm to 18 μm, but the present application is not limited thereto.

[0126] In some embodiments, the positive electrode current collector can be a metal foil or a composite current collector. An example of the metal foil is aluminum foil. The composite current collector can include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material can include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. For example, the polymeric material base layer can include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0127] Note that the parameters of each positive electrode sheet described in this application (e.g., areal density, compressed density, thickness, etc.) all refer to the parameters of the positive electrode film layer on one side of the positive electrode current collector. When positive electrode film layers are provided on both sides of the positive electrode current collector, it is considered that the parameters of the positive electrode film layer on either side satisfy the present application and fall within the scope of protection of this application.

[0128] When testing the above-mentioned parameters of the positive electrode sheet, such as areal density, compression density, thickness, and electrical resistance, a freshly prepared and cold-pressed positive electrode sheet can be directly used, or the positive electrode sheet can be obtained from a battery. An exemplary method for obtaining a positive electrode sheet from a battery is to fully discharge the battery, disassemble the positive electrode sheet, immerse the positive electrode sheet in an organic solvent (e.g., dimethyl carbonate) for a certain period of time (e.g., 72 hours or more), and then remove the positive electrode sheet and dry it at a certain temperature for a certain period of time (e.g., drying in a vacuum oven at 80°C for 6 hours or more).

[0129] How to make a positive electrode sheet

[0130] A third aspect of the present embodiment provides a method for producing a positive electrode sheet, which can produce the positive electrode sheet of the second aspect of the present embodiment.

[0131] The method includes the steps of supplying a cathode slurry containing the cathode material composition according to the first aspect of the present embodiment and a solvent, applying the cathode slurry to at least one surface of a cathode current collector, and then drying and compressing the cathode slurry to obtain a cathode sheet.

[0132] In some embodiments, the solvent may include, but is not limited to, N-methylpyrrolidone (NMP).

[0133] battery

[0134] A fourth aspect of an embodiment of the present application provides a battery.

[0135] The battery described in the examples or embodiments of this application refers to a single physical module that includes one or more battery cells and provides higher voltage and capacity. For example, the battery described in this application may include a battery cell, a battery module, or a battery pack. A battery cell is the smallest unit constituting a battery and can independently perform charging and discharging functions. In this application, the shape of the battery cell is not particularly limited and may be cylindrical, rectangular, or any other shape. Figure 1 shows a battery cell 5 with a rectangular structure as an example.

[0136] In some embodiments, a battery cell includes an electrode assembly, and the battery cell may further include a housing and an electrolyte. The electrode assembly typically includes a positive electrode sheet, a negative electrode sheet, etc., and the housing is used to seal the electrode assembly and the electrolyte. The housing may be a hard case such as a hard plastic case, an aluminum case, or a steel case. The housing may be a soft pack, for example, a bag-like soft pack. The soft pack may be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS). The electrode assembly is manufactured by a winding process and / or a lamination process.

[0137] In some embodiments, as shown in FIG. 2 , the exterior may include a case 51 and a cover plate 53. The case 51 includes a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are enclosed to form a receiving cavity. The case 51 has an opening communicating with the receiving cavity, and the cover plate 53 is used to cover the opening and close the receiving cavity. An electrode assembly 52 is packaged in the receiving cavity. The number of electrode assemblies 52 included in the battery cell 5 may be one or more and can be adjusted as needed.

[0138] In some embodiments of the present application, the battery cells may be assembled into a battery module, and the battery module may include multiple battery cells, the specific number of which can be adjusted according to the application and capacity of the battery module. FIG. 3 is a schematic diagram of an example battery module 4. As shown in FIG. 3, in the battery module 4, multiple battery cells 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, any other arrangement may also be used. Furthermore, the multiple battery cells 5 may be fastened by fasteners.

[0139] Preferably, the battery module 4 may further include a housing having an accommodation space in which the plurality of battery cells 5 are accommodated.

[0140] In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules included in the battery pack may be adjusted depending on the application and capacity of the battery pack. FIGS. 4 and 5 are schematic diagrams of an example battery pack 1. As shown in FIGS. 4 and 5, the battery pack 1 may include a battery box and multiple battery modules 4 provided in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 covers the lower housing 3 to form a sealed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in the battery box in any manner.

[0141] [Positive electrode sheet]

[0142] The positive electrode sheet used in the battery of the present application is the positive electrode sheet described in any of the examples of the second aspect of the present application, which allows the battery of the present application to achieve both high energy density and good rate performance.

[0143] [Negative electrode sheet]

[0144] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector and including a negative electrode active material. For example, the negative electrode current collector has two surfaces facing each other in a thickness direction thereof, and the negative electrode film layer is provided on one or both of the two facing surfaces of the negative electrode current collector.

[0145] The negative electrode active material may be any battery negative electrode active material known in the art. Examples of the negative electrode active material include, but are not limited to, one or more of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may include one or more of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy material. The tin-based material may include one or more of elemental tin, tin oxide, and tin alloy material. The present application is not limited to these materials, and other conventional materials known for use as battery negative electrode active materials may be used.

[0146] In some embodiments, the negative electrode film layer may optionally include a negative electrode conductive agent. In the present application, the type of the negative electrode conductive agent is not particularly limited, and the negative electrode conductive agent may include, for example, one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0147] In some embodiments, the negative electrode film layer may include a negative electrode binder, if necessary. In the present application, the type of the negative electrode binder is not particularly limited. For example, the negative electrode binder may include one or more of styrene butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-soluble acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).

[0148] In some embodiments, the negative electrode film layer may contain other additives as needed, such as thickeners, e.g., sodium carboxymethyl cellulose (CMC), PTC thermistor materials, etc.

[0149] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. An example of the metal foil may be copper foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. For example, the polymeric material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0150] The negative electrode film layer is typically formed by applying a negative electrode slurry to a negative electrode current collector, drying, and cold pressing. The negative electrode slurry is typically formed by dispersing a negative electrode active material, an optional conductive agent, an optional binder, and other optional auxiliary agents in a solvent and stirring the mixture uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.

[0151] The negative electrode sheet does not exclude additional functional layers other than the negative electrode film layer. For example, in some embodiments, the negative electrode sheet according to the present application may further include a conductive coating (e.g., typically composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and provided on the surface of the negative electrode current collector. In some embodiments, the negative electrode sheet according to the present application may further include a protective layer covering the surface of the negative electrode film layer.

[0152] [Electrolytes]

[0153] The electrolyte serves to conduct lithium ions between the positive electrode sheet and the negative electrode sheet. The present application does not specifically limit the type of electrolyte, and it can be selected as needed. For example, the electrolyte may include one or more types selected from solid electrolytes and liquid electrolytes (i.e., electrolytic solutions).

[0154] In some embodiments, the electrolyte is an electrolytic solution including an electrolyte salt and a solvent.

[0155] The electrolyte salt may include one or more salts selected from lithium hexafluorophosphate (LiPF), lithium tetrafluoroborate (LiBF), lithium perchlorate (LiClO), lithium hexafluoroarsenate (LiAsF), lithium bisfluorosulfonylimide (LiFSI), lithium bistrifluoromethanesulfonylimide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium disoxalate borate (LiBOB), lithium difluorophosphate (LiPOF), lithium difluorodisoxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).

[0156] The type of the solvent is not specifically limited and can be selected according to actual needs. In some embodiments, by way of example, the solvent may comprise one or more selected from ethylene carbonate (EC), propylene carbonate (PC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).

[0157] In some embodiments, the electrolyte may contain additives as needed. For example, the additives may include a negative electrode film-forming additive, a positive electrode film-forming additive, or an additive that can improve certain battery performance, such as an additive that improves the overcharge performance of the battery, an additive that improves the high-temperature performance of the battery, or an additive that improves the low-temperature power performance of the battery.

[0158] [Separator]

[0159] Batteries using liquid electrolytes and some batteries using solid electrolytes further include a separator. The separator is disposed between the positive electrode sheet and the negative electrode sheet and primarily serves to prevent short circuits between the positive electrode and the negative electrode while allowing lithium ions to pass through. The type of separator is not particularly limited in this application, and any known porous separator with good chemical and mechanical stability can be selected. The separator may be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer may be the same or different.

[0160] In some embodiments, the separator may include a base film and an optional protective coating. The base film may include a nonwoven fabric, film, or composite film having a porous structure, and the material of the base film may include one or more of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, and polyimide.

[0161] The surface of the base film may or may not be provided with a protective coating. In some embodiments, the base film has a protective coating on at least one surface, and the protective coating may be a polymer layer, an inorganic layer, or a mixed layer of polymer and inorganic.

[0162] The inorganic layer includes inorganic particles and a binder, and the inorganic particles include, but are not limited to, one or more of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate.

[0163] The polymer layer comprises a polymer, and the polymer material includes, but is not limited to, one or more of polyamide, polyacrylonitrile, acrylic ester polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, and polyvinylidene fluoride.

[0164] [Production method]

[0165] Methods for fabricating the battery of the present application are well known. In some embodiments, a battery can be formed by assembling a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte. For example, the positive electrode sheet, the separator, and the negative electrode sheet are wound and / or stacked to form an electrode assembly. The electrode assembly is then placed in a housing, dried, and then an electrolyte is injected. A battery cell can be obtained through processes such as chemical formation and capacitance. Multiple battery cells may be further connected in series, parallel, or a combination to form a battery module. Multiple battery modules may also be connected in series, parallel, or a combination to form a battery pack. In some embodiments, multiple battery cells can directly form a battery pack.

[0166] power consumption equipment

[0167]

[0010] Embodiments of the present application further provide a power consuming device including a battery according to the present application. The battery may be used as a power source for the power consuming device or as an energy storage means for the power consuming device. The power consuming device may be, but is not limited to, a mobile device (e.g., a mobile phone, a tablet PC, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf car, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.

[0168] The power consuming device can select a specific type of battery, such as a battery cell, a battery module, or a battery pack, according to its usage needs.

[0169] 6 is a schematic diagram of an example power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the power consuming device, a battery pack or battery module can be employed as a power source.

[0170] Other examples of power consuming devices may be mobile phones, tablet computers, laptops, etc. Such power consuming devices are usually required to be thin and may employ battery cells as a power source.

[0171] Example

[0172] The following examples more specifically describe the disclosure of the present application, but these examples are merely illustrative, and it will be apparent to those skilled in the art that various modifications and variations can be made within the scope of the disclosure of the present application. All parts, percentages, and ratios described in the following examples are based on mass unless otherwise specified. All reagents used in the examples are commercially available or may be synthesized according to conventional methods and can be used as is without further treatment. All devices used in the examples are commercially available.

[0173] Preparation of positive electrode active material

[0174] The washed and dried lithium iron phosphate powder and the organic carbon source glucose are dispersed in the polishing body with the aid of alcohol as a dispersant for 1 hour until they are uniformly mixed. By adjusting the ratio of lithium iron phosphate powder to glucose to 80 wt%:20 wt% or 95 wt%:5 wt%, the carbon content in the final material can be controlled to 0.7% to 3.5%. The polished powder is then divided into two parts: one part is polished directly to a dry powder state, and the other part is polished to a dry powder state after adding a certain amount of stone powder. Next, the two samples are mixed and then ground for 2 hours to disperse. The homogeneously mixed powder is placed in a tubular furnace protected by a nitrogen gas atmosphere. The nitrogen gas flow rate is controlled at 0.02 L / min. The temperature is then first raised to 280°C at a heating rate of 2°C / min and kept at that temperature for 2 hours, which is beneficial for decomposing the glucose and fully carbonizing it, thereby fully coating the carbon material. The temperature is then raised at a rate of 5°C / min to the sintering temperature T and kept at that temperature for a time t. The graphitization degree of the carbon material can be adjusted by adjusting the sintering temperature T and the keeping time t. After completion, the mixture is cooled to room temperature, and carbon-coated lithium iron phosphates with different graphitization degrees are obtained.

[0175] The sintering temperatures T and incubation times t corresponding to the carbon-coated lithium iron phosphates with different degrees of graphitization used in the following examples and comparative examples are shown in Table 1.

[0176] [Table 1]

[0177] Example 1

[0178] Preparation of positive electrode sheet

[0179] The positive electrode active material was carbon-coated lithium iron phosphate (carbon content: 1.5%, graphitization degree: 15%, powder resistivity: 30 Ω·cm, powder compaction density: 2.5 g / cm). 3 The cathode slurry was formed by thoroughly mixing the cathode material (carbon black (Super P) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and polyvinyl alcohol as a dispersant in a mass ratio of 97.4:0.4:2.0:0.2 in an appropriate amount of NMP as a solvent with sufficient stirring. The cathode slurry was uniformly applied to the surface of aluminum foil (15 μm thick) as a cathode current collector, dried, and cold-pressed to obtain a cathode sheet. The surface density of the cathode sheet was 410 mg / 1540.25 mm 2 and the compressed density is 2.6 g / cm 3 is.

[0180] The graphitization degree of the positive electrode active material refers to the graphitization degree of the carbon material in the shell part of the positive electrode active material, and is measured using an X-ray diffraction device in accordance with JIS K 0131-1996 and JB / T 4220-2011. 002 Then, the formula g = (0.344 - d 002 The graphitization degree of the positive electrode active material can be calculated based on the formula: d ) / (0.344-0.3354)×100%. 002 is the layer spacing of the C(002) plane in the crystal structure of the positive electrode active material, expressed in nanometers (nm). A Bruker D8 Discover X-ray diffractometer can be used as the test equipment.

[0181] The powder resistivity of positive electrode active material can be tested using the following steps: Weigh out 1 to 5 g of test sample, adjust the depth of the powder resistivity meter's feed cavity, place the test sample in the feed cavity, apply pressure, and record the powder resistivity of the positive electrode active material at different pressures. When the powder resistivity value no longer changes as the pressure continues to increase, stop the test and record the powder resistivity value at this point as the powder resistivity of the positive electrode active material. The test equipment can be a PRCD 2100 powder resistivity meter from Yuan Neng Technology Co., Ltd.

[0182] The powder compaction density of the positive electrode active material can be measured using an electronic pressure tester in accordance with GB / T 24533-2009. A 1 g test sample was weighed and measured to determine whether the base area was 1.327 cm. 2 The powder was placed in a mold, pressurized to 3 tons, and held for 30 seconds. The pressure was then released and held for 10 seconds. The powder compaction density of the positive electrode active material at a pressure of 3 tons was then recorded and calculated. The test equipment used was a UTM7305 electronic pressure tester.

[0183] Preparation of negative electrode sheet

[0184] The negative electrode active material, graphite, the binder, styrene butadiene rubber (SBR), the thickener, sodium carboxymethyl cellulose (CMC), and the conductive agent, carbon black (Super P), were mixed in a mass ratio of 96.7:1.7:0.7:0.9 with an appropriate amount of deionized water as the solvent and stirred thoroughly to form a uniform negative electrode slurry. The negative electrode slurry was then uniformly applied to the surface of the negative electrode current collector, copper foil (6 μm thick), dried, and cold-pressed to obtain a negative electrode sheet. The surface density of the negative electrode sheet was 180 mg / 1540.25 mm. 2 and the compressed density is 1.65 g / cm 3 is.

[0185] Preparation of electrolyte

[0186] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1 to obtain an organic solvent, and thoroughly dried LiPF6 was dissolved in the organic solvent to prepare an electrolyte solution with a concentration of 1 mol / L.

[0187] Battery construction

[0188] The fabricated positive and negative electrode sheets are die-cut and slit, then wound with a separator to form an electrode assembly, which is then hot-pressed, coated, tab-welded, adapter-sheet-attached, inserted into a case, and top-cover-welded. The assembly is then baked to remove moisture, filled with the above-prepared electrolyte, and subjected to chemical and capacitance processes. Finally, a blue film is applied to complete the fabrication of the battery (i.e., battery cell). The separator, located between the positive and negative electrode sheets, comprises a 5 μm polyethylene base film and a 15 μm Al2O3 coating.

[0189] Examples 2 to 17 and Comparative Examples 2 to 6

[0190] The battery was fabricated in the same manner as in Example 1, except for the parameters of the positive electrode active material, the mass percentage content w2 of the positive electrode active material, and the mass percentage content w1 of the conductive agent. See Tables 1 and 2 for specific parameters.

[0191] Example 18

[0192] The battery was fabricated with a positive electrode sheet surface density of 300 mg / 1540.25 mm 2 and the compressed density is 2.6 g / cm 3 The surface density of the negative electrode sheet is 135 mg / 1540.25 mm 2 and the compressed density is 1.65 g / cm 3 The procedure is similar to that of Example 4, except that:

[0193] Example 19

[0194] The battery was fabricated with a positive electrode sheet surface density of 500 mg / 1540.25 mm 2 and the compressed density is 2.6 g / cm 3 The surface density of the negative electrode sheet is 225 mg / 1540.25 mm 2 and the compressed density is 1.65 g / cm 3 The procedure is similar to that of Example 4, except that:

[0195] Comparative Example 1

[0196] The battery was fabricated in the same manner as in Example 1, except that the positive electrode active material was lithium iron phosphate coated with amorphous carbon, the mass percentage content of the positive electrode active material was 95.8%, and the mass percentage content of the conductive agent was 2.0%.

[0197] Testing Department

[0198] The performance of the battery cells thus fabricated will be tested below. Note that the batteries mentioned in the following performance tests all refer to battery cells.

[0199] (1) Battery volume energy density test

[0200] Battery volumetric energy density (Wh / L) = (battery discharge capacity x battery discharge plateau voltage) / battery volume.

[0201] The discharge capacity of the battery was obtained by testing it as follows: At 25°C, a freshly prepared battery was charged at a constant current of 1 / 3 C to 3.65 V, and then discharged at a constant current of 1 / 3 C to 2.0 V to obtain the discharge capacity of the battery.

[0202] The battery discharge plateau voltage is the potential at which the electrochemical reaction reaches equilibrium, and can be obtained from a battery tester.

[0203] The volume of the battery is tested using the drainage method, in which the battery is placed in pure water during testing, and the volume of the drained water is the volume of the battery.

[0204] (2) Battery rate performance test

[0205] At 25°C, the freshly prepared batteries were charged at constant current at charge rates of 1 / 3C, 1C, 3C, and 5C to the upper cutoff voltage of the battery (corresponding to 100% SOC), then charged at constant voltage until the current reached 0.05C, and then discharged at constant current at 1 / 3C to the lower cutoff voltage of the battery (corresponding to 0% SOC). The discharge energy of the batteries at this time was recorded.

[0206] The discharge energy of the battery obtained at a charge rate of 1 / 3C was 100%, and the discharge energy retention rate of the battery at charge rates of 1C, 3C, and 5C was calculated.

[0207] (3) Testing the DC internal resistance of the battery

[0208] At 25°C, the fresh battery prepared above was charged at a constant current of 1 C to the upper cutoff voltage of the battery (corresponding to 100% SOC), then charged at a constant voltage of 0.05 C, and then discharged at a constant current of 1 C to the lower cutoff voltage of the battery (corresponding to 0% SOC). The discharge capacity at this time was recorded and used as the initial discharge capacity of the battery. The battery was subjected to a cycle charge-discharge test according to the above method until the discharge capacity of the battery decayed to 80% of the initial discharge capacity of the battery, at which point the test was stopped.

[0209] At 25°C, a fresh battery and a battery whose cycle capacity has decayed to 80% of the initial discharge capacity are tested for DC internal resistance to obtain the initial DC internal resistance of the battery and the DC internal resistance of the battery cycled to 80% SOH.

[0210] The DC internal resistance of a battery was measured by adjusting the battery capacity to 50% SOC, then pulse charging it at a rate of 4C for 30 seconds, and recording the voltage before and after the pulse charge. Battery charging DC internal resistance (mΩ) = (voltage at the end of pulse charge - voltage before pulse charge) / charging current.

[0211] (4) Testing the electrical resistance of the positive electrode sheet

[0212] The electrical resistance of the positive electrode sheet can be tested using equipment and methods well known in the art. For example, the test method can be as follows: Take a 4 cm x 25 cm sample along the length of the positive electrode sheet, start the double-probe resistance tester, select the single-point mode, and test the area of ​​the input terminals to 1540.25 mm. 2 The number of parallel samples was 20, the pressure was 0.4t, and the time interval was 15 seconds. The test sample was placed between the two probes, and the software's operation button was clicked, followed by a downward rotation of the directional control valve. After 15 seconds, one data point was automatically collected. The test method for replacing one point was as described above. After testing all 20 points, the test sample was replaced and the test continued. The average of the test results was taken as the electrical resistance of the positive electrode sheet.

[0213] During the test, a freshly prepared positive electrode sheet and a positive electrode sheet disassembled from a battery whose cycle capacity has decayed to 80% of the initial discharge capacity are subjected to a resistance test to obtain the initial resistance of the positive electrode sheet and the electrical resistance of the positive electrode sheet when the battery is cycled to 80% SOH, respectively.

[0214] An exemplary method for obtaining a positive electrode sheet from a battery is to fully discharge the battery, disassemble the positive electrode sheet, and then soak and wash it in dimethyl carbonate (DMC) for at least 72 hours. After the electrolyte solvent, lithium salt, additives, etc. have completely leached out of the positive electrode sheet, the positive electrode sheet is then placed in a vacuum oven and dried. The dried positive electrode sheet was then subjected to a resistance test according to the method described above.

[0215] [Table 2]

[0216] [Table 3]

[0217] The test results in Table 3 show that when the graphitization degree of the positive electrode active material is 10% to 50% and the mass percentage content of the positive electrode conductive agent is 0% to 1%, the battery can achieve both high energy density and good rate performance, and in particular, the battery has good high-rate charging performance.

[0218] In Comparative Examples 1 to 6, none of the positive electrode active material graphitization degree is 10% to 50% and / or the positive electrode conductive agent mass percentage content is 0% to 1%, and therefore none of the batteries can achieve both high energy density and good rate performance.

[0219] In Comparative Example 1, a phosphate coated with amorphous carbon was used as the positive electrode active material. When the surface density of the positive electrode sheet was high, the lithium-containing phosphate itself had poor conductivity. Therefore, even though a high amount of positive electrode conductive agent (2%) was used, a good conductive network could not be formed in the positive electrode, and the battery could not have good rate performance. Furthermore, the volumetric energy density of the battery was also reduced due to the high amount of positive electrode conductive agent used.

[0220] In Comparative Example 2, a carbon-coated lithium-containing phosphate with a graphitization degree of less than 10% was used as the positive electrode active material, which provided a high energy density, but the rate performance of the battery was poor. In Comparative Example 3, a high positive electrode conductive agent of 1.5% was added based on Comparative Example 2 to provide a battery with good rate performance, which significantly reduced the volumetric energy density of the battery and limited the improvement in the discharge energy retention rate at 3C and 5C charge rates.

[0221] In Comparative Example 4, a carbon-coated lithium-containing phosphate with a graphitization degree exceeding 50% was used as the positive electrode active material. In this case, the battery was unable to achieve both high energy density and good rate performance. When the graphitization degree exceeded 50%, the compression density of the positive electrode sheet decreased, further reducing the battery's energy density. Furthermore, in this case, the reaction rate of the positive electrode may be significantly faster than that of the negative electrode, resulting in excessive accumulation of lithium ions on the negative electrode side during charging, increasing the viscosity of the electrolyte on the negative electrode side, which is unfavorable to lithium ion transfer. Furthermore, the rate performance deteriorates more significantly as the battery charging current increases. Summarizing the test results for Examples 1 to 7 and Comparative Example 4, it can be seen that the discharge energy retention rate at a 1C charge rate in Comparative Example 4 is similar to that of Examples 1 to 7, but the discharge energy retention rate at 3C and 5C charge rates in Comparative Example 4 is significantly lower than that of Examples 1 to 7.

[0222] The test results of Examples 3 to 12 and Comparative Example 5 show that when the graphitization degree of the carbon-coated lithium-containing phosphate is 25% to 50%, the cathode conductive agent can be removed despite the high surface density of the cathode sheet, thereby further improving the energy density of the battery and providing the battery with good rate performance, especially good high-rate charge performance. Furthermore, the test results of Examples 4, 8 to 12 and Comparative Example 5 show that increasing the amount of cathode conductive agent used does not significantly improve the rate performance of the battery, and when the amount of cathode conductive agent used exceeds 1%, the discharge energy retention rate of the battery at 3C and 5C charge rates is significantly reduced.

[0223] Summarizing the test results for Examples 1 and 2, Examples 13 to 17, and Comparative Example 6, it was found that when the graphitization degree of the positive electrode active material was low, the positive electrode conductive agent could be removed to achieve a battery with high energy density and good rate performance. However, when the positive electrode sheet contained a relatively low amount of positive electrode conductive agent, for example, when the content of the positive electrode conductive agent was greater than 0 and less than 1%, preferably greater than 0 and less than 0.4%, this contributed to further improvement of the battery's rate performance, particularly its high-rate charging performance. However, it was found that when the amount of positive electrode conductive agent used exceeded 1%, the discharge energy retention rate of the battery at charge rates of 3C and 5C significantly decreased.

[0224] Summarizing the test results of Examples 1, 9, and 14, it can be seen that when the amount of positive electrode conductive agent used is the same, improving the graphitization degree of the carbon-coated lithium-containing phosphate within a certain range contributes to improving the rate performance of the battery, but further increasing the graphitization degree of the carbon-coated lithium-containing phosphate may actually decrease the rate performance of the battery, particularly the discharge energy retention rate at 3C and 5C charge rates of the battery. Therefore, rationally adjusting the graphitization degree of the positive electrode active material and the amount of positive electrode conductive agent used contributes to better achieving both high energy density and good rate performance in the battery, and in particular, the battery can have good high-rate charging performance.

[0225] Summarizing the test results of Examples 4 and 18-19, when the positive electrode sheet contains the combination of positive electrode materials of the present invention, the battery can achieve both high energy density and good rate performance even when the areal density of the positive electrode sheet is increased. Furthermore, unlike prior art research, there is no need to increase the amount of positive electrode conductive agent used, and even the positive electrode conductive agent can be eliminated.

[0226] It should be noted that the present application is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea within the technical scope of the present application and exhibits similar effects is included within the technical scope of the present application. In addition, various modifications that a person skilled in the art can conceive of to the embodiments, as well as other forms constructed by combining some of the components of the embodiments, are also included within the scope of the present application, as long as they do not deviate from the spirit of the present application.

Claims

1. A cathode material composition comprising an active cathode material and an optional cathode conductive agent, The positive electrode active material includes a core portion and a shell portion located on at least a part of the surface of the core portion, the core portion includes a lithium-containing phosphate, and the shell portion includes a carbon material; The graphitization degree of the positive electrode active material is expressed as g 1 The mass percentage content of the positive electrode conductive agent in the positive electrode material composition is w 1 Then, 10%≦g 1 ≦50%, 0%≦w 1 ≦1% of the positive electrode material composition.

2. 15%≦g 1 ≦48% and 0%≦w 1 ≦0.8%, Preferably, 15%≦g 1 ≦48% and 0%≦w 1 ≦0.6%; More preferably, 15%≦g 1 ≦48% and 0%≦w 1 2. The cathode material composition of claim 1, wherein the Cathode Material is ≦0.4%.

3. 20%≦g 1 ≦45% and 0%≦w 1 ≦0.6%; Preferably, 20%≦g 1 ≦45% and 0%≦w 1 ≦0.4%, More preferably, 20%≦g 1 ≦45% and 0%≦w 1 3. The positive electrode material composition according to claim 1, wherein the content of the cation is less than or equal to 0.2%.

4. 25%≦g 1 ≦50% and 0%≦w 1 4. The positive electrode material composition according to claim 1, wherein the content of the cation is less than or equal to 0.2%.

5. 25%≦g 1 ≦50%, and w 1 is 0%, Preferably, 25%≦g 1 ≦40%, and w 1 is 0%, More preferably, 25%≦g 1 ≦35%, and w 1 The positive electrode material composition according to any one of claims 1 to 4, wherein the content of the positive electrode material is 0%.

6. The graphitization degree g of the positive electrode active material 1 The positive electrode material composition according to any one of claims 1 to 5, wherein the positive electrode material composition is obtained by an X-ray diffraction method.

7. The powder resistivity of the positive electrode active material is greater than 0 and less than or equal to 30 Ω cm, preferably 0.5 Ω cm to 10 Ω cm, and / or 7. The positive electrode material composition according to claim 1, wherein the mass percentage content of carbon element in the positive electrode active material is 0.5% to 5%, preferably 1% to 3.5%.

8. The average particle size Dv50 of the positive electrode active material is 0.5 μm to 10 μm, preferably 1 μm to 4 μm, and / or The powder compression density of the positive electrode active material at a force of 3 tons is 2.5 g / cm 3 and / or The lithium-containing phosphate includes one or more selected from lithium iron phosphate, lithium manganese iron phosphate, and composite materials obtained by coating and / or doping the above materials, and preferably has a molecular formula of LiFe 1-x-y Mn x M y P.O. 4 where 0≦x≦1 and 0≦y<1; M includes one or more elements selected from transition metal elements and non-transition metal elements other than Fe and Mn, and preferably includes one or more elements selected from V, Nb, Ti, Co, Ni, Sc, Ge, Mg, Al, Zr, Mn, Hf, Ta, Mo, W, Ru, Ag, Sn, and Pb; and / or The positive electrode material composition according to any one of claims 1 to 7, wherein the positive electrode conductive agent comprises one or more selected from the group consisting of superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

9. The mass percentage content w of the positive electrode active material in the positive electrode material composition 2 The positive electrode material composition according to any one of claims 1 to 8, wherein the content of the positive electrode material is 97.0% or more, and preferably 97.0% to 98.2%.

10. Further comprising a positive electrode binder and / or a positive electrode dispersant, Preferably, the mass percentage content w of the positive electrode binder in the positive electrode material composition 3 is between 1% and 3%, Preferably, the mass percentage content w of the positive electrode dispersant in the positive electrode material composition 4 The positive electrode material composition according to any one of claims 1 to 9, wherein the content of the cation is 0% to 0.5%.

11. A positive electrode sheet comprising a positive electrode current collector and a positive electrode film layer provided on the positive electrode current collector, the positive electrode film layer comprising the positive electrode material composition according to any one of claims 1 to 10.

12. The surface density of the positive electrode sheet is 300 mg / 1540.25 mm 2 That's all. Preferably, 410 mg / 1540.25 mm 2 Above, 450mg / 1540.25mm 2 Above, 500mg / 1540.25mm 2 The positive electrode sheet according to claim 11 .

13. The surface density of the positive electrode sheet is CW, and the unit is mg / 1540.25 mm 2 In this case, the positive electrode sheet has a structure in which 0≦100,000×(w 1 / CW)≦3.4, and preferably 0≦100000×(w 1 The positive electrode sheet according to claim 11 or 12, wherein CW)≦1.8 is satisfied.

14. The positive electrode sheet according to any one of claims 11 to 13, wherein the thickness H of the positive electrode film layer is 70 µm to 145 µm, preferably 90 µm to 138 µm.

15. When the thickness of the positive electrode film layer is H and the unit is μm, the positive electrode sheet has a thickness of 0≦100000×(w 1 / H)≦14, and preferably 0≦100000×(w 1 The positive electrode sheet according to any one of claims 11 to 14, wherein / H)≦11 is satisfied.

16. The compressed density PD of the positive electrode sheet is 2.55 g / cm 3 or more, preferably 2.58 g / cm 3 More preferably, it is 2.60 g / cm 3 The positive electrode sheet according to any one of claims 11 to 15.

17. further comprising a conductive coating located between the positive electrode current collector and the positive electrode film layer; Preferably, the conductive coating comprises conductive carbon black and a binder; The positive electrode sheet according to any one of claims 11 to 16, wherein the conductive coating has a thickness of more than 0 and not more than 2 µm.

18. The electrical resistance of the positive electrode sheet is 0.1 Ω to 1 Ω, preferably 0.1 Ω to 0.6 Ω, and / or The positive electrode sheet according to any one of claims 11 to 17, wherein the positive electrode current collector has a thickness of 10 µm to 18 µm.

19. 11. A method for producing a positive electrode sheet, comprising: supplying a positive electrode slurry; applying the positive electrode slurry to at least one surface of a positive electrode current collector; and obtaining a positive electrode sheet through drying and compressing steps, wherein the positive electrode slurry contains the positive electrode material composition according to any one of claims 1 to 10 and a solvent.

20. A battery comprising the positive electrode material composition according to any one of claims 1 to 10, the positive electrode sheet according to any one of claims 11 to 18, or the positive electrode sheet produced by the production method according to claim 19.

21. 21. A power consuming device comprising the battery of claim 20.

Citation Information

Patent Citations

  • High-conductivity ferrous phosphate lithium cathode material for lithium ion battery and preparation method thereof

    CN102324519A

  • Reversible electrode material

    JP1993074459A

  • Metal carrying porous carbon film, electrode for fuel cell, and fuel cell using the same

    JP2004335459A

  • Metal compound powder and method of manufacturing the same

    JP2012038554A

  • Cobalt-free alkaline secondary battery

    JP2012204177A

Cited By

  • Lithium secondary battery, positive electrode active material, preparation method of positive electrode active material, and electric device

    CN120015902A

  • Lithium ion secondary battery, battery device, and power device

    CN120073043A

  • Battery cell, battery device, electric device, and energy storage device

    CN120319871A

  • Positive electrode sheet, battery comprising same, and electric device

    WO2026143988A1