Viscosity index improvers for lubricants based on polyisobutylene phenyl acrylate comb copolymers

The synthesis of comb copolymers with PIB macromonomers and acrylate monomers addresses the challenges of high viscosity and poor handling in existing polymers, resulting in improved lubricating oils with low bulk viscosity, high viscosity index, and high shear stability.

JP2024545443AActive Publication Date: 2024-12-06BASF SE
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024533269
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-06
Filing Date
2022-11-29
Publication Date
2024-12-06
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

Existing comb polymers used in lubricating oils face challenges in synthesis difficulty, high viscosity during manufacturing, and poor handling performance, leading to issues with rheological behavior, viscosity index, and shear stability.

Method used

The development of comb copolymers comprising PIB macromonomers and acrylate monomers, synthesized through a polymerization process using polyisobutenephenol and (meth)acrylic anhydride, which are designed to have specific molecular weights and compositions to improve handling and rheological properties.

Benefits of technology

The comb copolymers exhibit low bulk viscosity at temperatures below 100°C, high viscosity index, and high shear stability, enhancing the performance of lubricating oils under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545443000001_ABST
    Figure 2024545443000001_ABST
Patent Text Reader

Abstract

The present invention relates to a comb copolymer comprising, in polymerized form, a PIB macromonomer of formula (I) and an acrylate monomer of formula (II).The present invention further relates to a process for the preparation of the PIB macromonomer of formula (I) by reacting a polyisobutene phenol of formula (III) with (meth)acrylic anhydride; a lubricant comprising a base oil, the comb copolymer, and further lubricant additives; and the use of the comb copolymer for improving the viscosity index of the lubricant. [Formula 1] JPEG2024545443000008.jpg20170H2C=C(R 7 )COOR 8 (II) [chemical 2] JPEG2024545443000009.jpg19170
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a comb copolymer comprising, in polymerized form, a PIB macromonomer of formula (I) and an acrylate monomer of formula (II). The present invention further relates to a method for preparing the PIB macromonomer of formula (I) by reacting a polyisobutene phenol of formula (III) with (meth)acrylic anhydride; a lubricant comprising a base oil, the comb copolymer, and further lubricant additives; and the use of the comb copolymer for improving the viscosity index of the lubricant. Combinations of the preferred embodiments with other preferred embodiments are within the scope of the present invention. [Background technology]

[0002] Comb polymers are useful additives for lubricating oils. Polyisobutylene (PIB)-based macromonomers are useful comonomers in comb polymers. However, they are difficult to synthesize. Summary of the Invention [Problem to be solved by the invention]

[0003] The objective was to find an improved synthesis of macromonomers and comb polymers and improved lubricants containing comb polymers. A further objective is to improve lubricants containing polymers, which have good rheological behavior, low polymer processing rate, high viscosity index, good low temperature properties (e.g., low temperature crankcase simulation), high viscosity under severe operating conditions (e.g., high temperature high shear HTHS viscosity test), and high shear stability. Comb polymers are often difficult to handle because they exhibit very high viscosities at the temperatures applied during lubricant manufacture. Therefore, comb polymers with improved handling properties are also desired, for example comb polymers with low bulk viscosity at temperatures below 100°C. [Means for solving the problem]

[0004] The purpose of this is to produce, in polymeric form, (A) PIB macromonomer of formula (I) [ka] (In the formula, R 1 ~R 5 is hydrogen, C1-C 20 -Alkyl, C1-C 20 -Alkyloxy, C8~C 7500 -Polyisobutyl and C8-C 7500 -polyisobutenyl; R 1 ~R 5 At least one of them is C8~C 7500 -Polyisobutyl group or C8-C 7500 - a polyisobutenyl group, R 6 is hydrogen or methyl); (B) an acrylate monomer of formula (II) H2C=C(R 7 )COOR 8 (II) (R 7 is hydrogen or methyl, and R 8 is C 1~36 This was solved by a comb copolymer containing

[0005] The PIB macromonomer may have a molecular weight of 300 to 10,000 g / mol, preferably 400 to 5000 g / mol, in particular 800 to 2500 g / mol.

[0006] The molecular weight of the PIB macromonomer can be determined by GPC using polystyrene standards (eg DIN 55672-1).

[0007] Preferably, R 1 ~R 5 One of the following (preferably R 3 ) is C8~C 7500 -Polyisobutyl or C8~C 7500 -polyisobutenyl. Preferably, PIB is R 3 is C8~C 7500-Polyisobutyl group, or C8-C 7500 -polyisobutenyl group. Preferably, C8 to C 7500 -Polyisobutyl group or C8-C 7500 - the moiety R is not a polyisobutenyl group 1 ~R 5 is selected from the group hydrogen, methyl, or tert-butyl. In particular, R 3 is C8~C 7500 -Polyisobutyl group, or C8-C 7500 - a polyisobutenyl group, R 1 , R 2 , R 4 , and R 5 is selected from the group hydrogen, methyl or tert-butyl.

[0008] R 6 is H or methyl, preferably methyl.

[0009] The synthesis of PIB macromonomers is known, for example, from K. Maenz and D. Stadermann, Angew. Makromol. Chem. 1996, 242, 183-197 “Macromonomers based on low-molecular weight polyisobutenes”. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The comb copolymer may comprise up to 60 wt%, preferably up to 45 wt%, in particular up to 30 wt% PIB macromonomer. In another embodiment, the comb copolymer may comprise up to 65 wt%, preferably up to 55 wt%, in particular up to 45 wt% PIB macromonomer.

[0011] Typically, the comb copolymer comprises 5 to 55 wt%, preferably 10 to 45 wt%, especially 15 to 25 wt% of the PIB macromonomer. In another embodiment, the comb copolymer comprises 5 to 60 wt%, preferably 10 to 60 wt%, especially 15 to 50 wt% of the PIB macromonomer.

[0012] The wt% of a monomer typically refers to the weight% based on the weight of all monomers in the comb copolymer. The sum of all wt% of all monomers (e.g., PIB macromonomer, hydrophobic monomer, and hydrophilic monomer) in the comb copolymer is typically 100 wt%.

[0013] R in acrylate monomer 7 can be H or methyl, with methyl being preferred. In formulae (II), (IIa) and (IIb), R 7 may be different or the same.

[0014] R in acrylate monomer 8 may be linear, branched or cyclic alkyl, preferably linear or branched alkyl, especially branched alkyl.

[0015] R 8 is preferably C 1~18 alkyl, in particular C 1~14 is selected from alkyl.

[0016] Suitable R 8 is methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, nonyl, decyl, stearyl, 2-hexyldecyl, lauryl, octadecyl, heptadecyl, nonadecyl, eicosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, behenyl, 2-octyldodecyl, 2-decyltetradecyl, 2-dodecylhexadecyl, 2-tetradecyloctydecyl, or mixtures thereof. 8 contains at least two different alkyl groups, for example two or three alkyl groups.

[0017] Typically, the comb copolymer comprises 25 to 90 wt %, preferably 35 to 85 wt %, especially 45 to 80 wt % of acrylate monomers.

[0018] In a preferred embodiment, the acrylate monomer is a hydrophobic acrylate monomer of formula (IIa): H2C=C(R 7 )COOR 8a (IIa) (In the formula, R 7 is hydrogen or methyl, R 8a is C 5~22 alkyl), and Hydrophilic acrylate monomers of formula (IIb) H2C=C(R 7 )COOR 8b (IIb) (In the formula, R 7 is hydrogen or methyl, R 8b , C 1~4 (which is alkyl).

[0019] R in hydrophobic acrylate monomers 8a may be linear, branched or cyclic alkyl, preferably linear or branched alkyl, especially branched alkyl.

[0020] Suitable R 8a is pentyl, hexyl, heptyl, octyl, 2-ethylhexyl, 2-propylheptyl, 2-butyloctyl, nonyl, decyl, stearyl, lauryl, 2-hexyldecyl, octadecyl, heptadecyl, nonadecyl, eicosyl, henicosyl, docosyl, tricosyl, tetracosyl, pentacosyl, hexacosyl, heptacosyl, octacosyl, nonacosyl, triacontyl, behenyl, 2-octyldodecyl, 2-decyltetradecyl, 2-dodecylhexadecyl, 2-tetradecyloctydecyl, or mixtures thereof.

[0021] R 8a is preferably C 6~18 Alkyl, especially C 6~14 In a preferred embodiment, R 8a is linear or branched C 6~14 In another preferred embodiment, R 8a is branch C6~10 In another preferred embodiment, R 8a is 2-ethylhexyl, 2-propylheptyl, dodecyl or tetradecyl, especially 2-ethylhexyl. In another preferred form, the hydrophobic acrylate monomer is 2-ethylhexyl methacrylate.

[0022] The comb copolymer may comprise at least 10 wt%, preferably at least 15 wt%, especially at least 25 wt% of hydrophobic acrylate monomers. In another embodiment, the comb copolymer may comprise at least 3 wt%, preferably at least 5 wt%, especially at least 8 wt% of hydrophobic acrylate monomers.

[0023] The comb copolymer may comprise up to 90 wt%, preferably up to 80 wt%, in particular up to 75 wt% of hydrophobic acrylate monomers. In another embodiment, the comb copolymer may comprise up to 60 wt%, preferably up to 40 wt%, in particular up to 25 wt% of hydrophobic acrylate monomers.

[0024] Typically, the comb copolymer may comprise 15 to 85 wt%, preferably 20 to 80 wt%, especially 25 to 75 wt% of the hydrophobic acrylate monomer. In another embodiment, the comb copolymer may comprise 3 to 75 wt%, preferably 5 to 75 wt%, especially 10 to 75 wt% of the hydrophobic acrylate monomer. In yet another embodiment, the comb copolymer may comprise 3 to 60 wt%, preferably 5 to 40 wt%, especially 10 to 25 wt% of the hydrophobic acrylate monomer.

[0025] R in hydrophilic acrylate monomers 8b may be linear, branched or cyclic alkyl, preferably linear or branched alkyl, especially branched alkyl.

[0026] Suitable R 8b are methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, sec-butyl, and tert-butyl.

[0027] R 8b is preferably methyl or butyl. In another preferred embodiment, R 8b is methyl or methyl and at least one C 2~4 In another preferred embodiment, R 8b is methyl. In another preferred embodiment, R 8b is a mixture of methyl and butyl, e.g., n-butyl.

[0028] The comb copolymer may comprise at least 1 wt%, preferably at least 5 wt%, especially at least 8 wt% of hydrophilic acrylate monomers. In another embodiment, the comb copolymer may comprise at least 15 wt%, preferably at least 25 wt%, especially at least 35 wt% of hydrophilic acrylate monomers.

[0029] The comb copolymer may comprise up to 50 wt%, preferably up to 40 wt%, in particular up to 35 wt% of hydrophilic acrylate monomers. In another embodiment, the comb copolymer may comprise up to 75 wt%, preferably up to 65 wt%, in particular up to 55 wt% of hydrophilic acrylate monomers.

[0030] Typically, the comb copolymer comprises 3 to 45 wt%, preferably 3 to 40 wt%, especially 5 to 35 wt% of hydrophilic acrylate monomers. In another embodiment, the comb copolymer may comprise 3 to 50 wt%, preferably 5 to 50 wt%, especially 8 to 50 wt% of hydrophilic acrylate monomers. In yet another embodiment, the comb copolymer may comprise 5 to 75 wt%, preferably 8 to 65 wt%, especially 35 to 55 wt% of hydrophilic acrylate monomers.

[0031] Typically, the comb copolymer comprises 15-85 wt% hydrophobic acrylate monomers and 3-45 wt% hydrophilic acrylate monomers. Preferably, the comb copolymer comprises 20-80 wt% hydrophobic acrylate monomers and 3-40 wt% hydrophilic acrylate monomers. In another embodiment, the comb copolymer comprises up to 75 wt% hydrophobic acrylate monomers and at least 5 wt% hydrophilic acrylate monomers.

[0032] Typically, the comb copolymer comprises - 5-55 wt% PIB macromonomer; - 15-85 wt. % of a hydrophobic acrylate monomer; - 1 to 50 wt. % of a hydrophilic acrylate monomer; The sum of all monomers is 100 wt %.

[0033] In another aspect, the comb copolymer is - 5-55 wt% PIB macromonomer; - 10-85 wt. % of a hydrophobic acrylate monomer; - 1 to 50 wt. % of a hydrophilic acrylate monomer; The sum of all monomers is 100 wt %.

[0034] In another aspect, the comb copolymer is - 5-55 wt% PIB macromonomer; - 5 to 80 wt. % of a hydrophobic acrylate monomer; - 8 to 65 wt. % of a hydrophilic acrylate monomer; The sum of all monomers is 100 wt %.

[0035] Typically, the comb copolymer comprises - 10-45 wt% PIB macromonomer; - 20-80 wt. % of a hydrophobic acrylate monomer; - 3 to 45 wt. % of a hydrophilic acrylate monomer; The sum of all monomers is 100 wt %.

[0036] In another aspect, the comb copolymer is - 5-55 wt% PIB macromonomer; - 5-35 wt. % of a hydrophobic acrylate monomer; - 20 to 60 wt % of a hydrophilic acrylate monomer; The sum of all monomers is 100 wt %.

[0037] The comb copolymer may comprise further monomers different from the PIB macromonomer, the hydrophobic monomer or the hydrophilic monomer. As further comonomers the following may be employed: - hydroxyl-, epoxy- or amino-functional (meth)acrylates, vinylaromatics, such as styrene, α-methylstyrene, vinyltoluene or p-(tert-butyl)styrene; - acrylic and methacrylic acid; - acrylamide and methacrylamide; - maleic acid and its imides and C1-C10-alkyl esters; - fumaric acid and its imides and C1-C10-alkyl esters; - itaconic acid and its imides and C1-C10-alkyl esters; - Acrylonitrile and methacrylamide.

[0038] The comb copolymer may comprise up to 15 wt%, preferably up to 5 wt%, in particular up to 1 wt% of further monomers. In an alternative embodiment, the comb copolymer does not comprise further monomers.

[0039] The comb copolymers may have a molecular weight Mn of 10,000 to 1,500,000 g / mol, preferably 20,000 to 1,000,000 g / mol and in particular 50,000 to 200,000 g / mol.

[0040] The comb copolymers may have a molecular weight Mw of 50,000 to 2,000,000 g / mol, preferably 100,000 to 1,000,000 g / mol, in particular 200,000 to 600,000 g / mol.

[0041] The comb copolymer may have a polydispersity index (PDI) of 1.5 to 5.0, preferably 2.0 to 4.5, especially 2.9 to 4.3.

[0042] The molecular weight of the comb copolymers can be determined by GPC using polystyrene standards (eg DIN 55672-1).

[0043] The kinematic viscosity (KV100, typically measured with a Brookfield viscometer) of the comb copolymer in a 30 wt % solution of base oil (e.g., Nexbase® 3030) at 100° C. is 2 / s, preferably less than 300 mm 2 / s or less, especially 150 mm 2 / s.

[0044] The comb copolymers can be prepared by conventional free radical polymerization, such as bulk or solution polymerization, with solution polymerization being preferred.

[0045] In solution polymerization, the reaction mixture may include a diluent, monomer, polymerization initiator, and optionally a chain transfer agent, and optionally a crosslinker. The diluent may be any inert hydrocarbon. The concentration of total monomer may range from about 30 to 100%. As used herein, "total monomer load" means the combined amount of all monomers in the initial reaction mixture.

[0046] The diluent may be any inert hydrocarbon or dicarboxylic acid ester, the dicarboxylic acid ester being a diester of at least one linear or branched C2-C20 dicarboxylic acid with at least one linear or branched C1-C20 monoalcohol. The dicarboxylic acid ester is preferably derived from the reaction of a dicarboxylic acid with an aliphatic alcohol. Preferred dicarboxylic acids are adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid, and mixtures thereof. The dicarboxylic acid ester component is preferably formed from such a dicarboxylic acid by esterification with a medium-sized aliphatic alcohol, which may be linear or branched, preferably a C5-C20 alcohol, more preferably a C9-C15 aliphatic alcohol, most preferably nonanol, isodecanol, isotridecanol, and 2-propylheptanol. The diluent is preferably di-(2-propylheptyl)-adipate.

[0047] Preferably, the comb copolymer is present in a diluent which is a dicarboxylic acid ester, preferably a diester of at least one linear or branched C2-C20 dicarboxylic acid and at least one linear or branched C1-C20 monoalcohol, in particular di-(2-propylheptyl)-adipate.

[0048] Suitable polymerization initiators include initiators that dissociate when heated to produce free radicals, such as peroxide compounds such as benzoyl peroxide, t-butyl perbenzoate, t-butyl peroctoate, and cumene hydroperoxide; and azo compounds such as azoisobutyronitrile and 2,2'-azobis(2-methylbutanenitrile). The mixture contains about 0.001 weight percent to about 5.0 weight percent of the initiator based on the total monomer mixture. For example, 0.02 weight percent to about 4.0 weight percent, 0.02 weight percent to about 3.5 weight percent are contemplated. Typically, about 0.02 weight percent to about 2.0 weight percent is used.

[0049] Suitable chain transfer agents include mercaptans and alcohols. For example, tridecyl mercaptan, dodecyl mercaptan, and ethyl mercaptan can be used as chain transfer agents, as well as difunctional mercaptans, such as hexanedithiol. The choice of the amount of chain transfer agent to use is based on the desired molecular weight of the polymer being synthesized. Chain transfer agents are often added to the reaction mixture or monomer feed in amounts of 0.001 to 3% by weight based on the monomer mixture.

[0050] All components are charged into a reaction vessel equipped with a stirring rod, a thermometer, and a reflux condenser, and the polymerization reaction can be carried out by heating to a temperature of about 50°C to about 125°C for about 0.5 to about 15 hours with stirring under a nitrogen atmosphere.

[0051] The present invention also relates to a process for the preparation of the PIB macromonomer of formula (I). [ka] In the formula, R 1 ~R 5 is hydrogen, C1-C 20 -Alkyl, C1-C 20 -Alkyloxy, C8~C 7500 -Polyisobutyl and C8-C 7500 -polyisobutenyl, R 1 ~R 5 At least one of them is C8~C 7500 -Polyisobutyl group or C8-C 7500 - a polyisobutenyl group, R 6 is hydrogen or methyl, Polyisobutenephenol of formula (III) [ka] is reacted with (meth)acrylic anhydride.

[0052] The polyisobutene phenols of formula (III) can be prepared as described in WO 2018 / 024563. The polyisobutene phenols may have a molecular weight of 300 to 10,000 g / mol, preferably 400 to 5000 g / mol, in particular 800 to 2500 g / mol.

[0053] The (meth)acrylic anhydride is preferably present in a molar excess relative to the polyisobutene phenol, for example at least a 1.1-fold, 1.5-fold or 2-fold molar excess.

[0054] The reaction between polyisobutenephenol and (meth)acrylic anhydride can be carried out at a reaction temperature in the range of 0 to 120°C, preferably 10 to 100°C.

[0055] The reaction between polyisobutenephenol and (meth)acrylic anhydride can be carried out in an organic solvent, such as a hydrocarbon solvent.

[0056] Following reaction of the PIB-amine with meth)acrylic anhydride, the remaining (meth)acrylic anhydride is typically hydrolyzed to form (meth)acrylic acid, which can be removed by distillation or extraction with water.

[0057] The present invention also provides (i) a base oil; (ii) a comb copolymer or a comb copolymer obtainable by the process according to the invention, (iii) further lubricant additives.

[0058] The lubricant may comprise at least 0.1 wt%, preferably at least 0.5 wt%, especially at least 1 wt% of the comb copolymer. In another embodiment, the lubricant may comprise 0.1-20 wt%, preferably 0.1-150 wt%, especially at least 0.1-10 wt% of the comb copolymer.

[0059] The lubricant may comprise at least 30 wt%, preferably at least 50 wt%, in particular at least 70 wt% of the base oil. The lubricant may comprise 30 to 99.9 wt%, preferably 50 to 99 wt%, in particular 70 to 95 wt% of the base oil.

[0060] The lubricant may be present in an amount of up to 20 wt%, preferably up to 15 wt%, in particular up to It may contain up to 10 wt% of further lubricant additives.

[0061] A lubricant generally refers to a composition capable of reducing friction between surfaces, preferably metal surfaces, such as the surfaces of a mechanical device. A mechanical device may be a mechanism consisting of devices operating on mechanical principles. Suitable mechanical devices are bearings, gears, joints, and induction devices. The mechanical device may be operated at temperatures ranging from -30°C to 80°C. A lubricant is generally a lubricating fluid, a lubricating oil, or a lubricating grease.

[0062] Lubricants are usually specially formulated for virtually any type of machine and manufacturing process. The type and concentration of base oil and / or lubricant additives used in these lubricants may be selected based on the requirements of the machine or process being lubricated, the qualities desired by the machine manufacturer and user, and government regulations. Typically, each lubricant has a unique set of performance requirements. In addition to proper lubrication of the machine or process, these requirements include maintaining the quality of the lubricant itself, and the impact of use and disposal of the lubricant on energy use, environmental quality, and the health of the user.

[0063] Representative lubricants are automotive lubricants (e.g., gasoline engine oils, diesel engine oils, gas engine oils, gas turbine oils, automatic transmission fluids, gear oils) and industrial lubricants (e.g., industrial gear oils, pneumatic tool lubricants, high temperature oils, gas compressor oils, hydraulic fluids, metal working oils).

[0064] Examples of lubricants include accelerator lubrication, medium and heavy duty oils, industrial engine oils, marine engine oils, automotive engine oils, crankshaft oils, compressor oils, refrigeration oils, hydrocarbon compressor oils, ultra-low temperature lubricants, high temperature lubricants, steel rope lubricants, textile machine oils, refrigeration oils, aerospace lubricants, aviation turbine oils, transmission oils, gas turbine oils, spindle oils, spin oils, traction fluids, transmission oils, plastic transmission oils, passenger car transmission oils, truck transmission oils. , industrial transmission oils, industrial gear oils, insulating oils, gauge oils, brake fluids, transmission fluids, shock absorber oils, thermal distribution medium oils, transformer oils, greases, chain oils, minimum quantity lubricants for metalworking operations, oils for warm and cold working, oils for water-based metalworking fluids, oils for neat metalworking fluids, oils for semi-synthetic metalworking fluids, oils for synthetic metalworking fluids, drilling fluids for geotechnical investigations, hydraulic oils, biodegradable lubricants or lubricating greases or waxes, chain saw oils, mold release agents, molding fluids, gun, pistol and rifle lubricants or watch lubricants, and food grade approved lubricants.

[0065] The lubricant typically has a viscosity of at least 10, 50, 100, 150, 200, 300, 400, 500, 600, 900, 1400, or 2000 mm 2 In another embodiment, the lubricant may have a kinematic viscosity of 200 to 30,000 mm / s at 40°C. 2 / s (cSt), preferably 500 to 10,000 mm 2 / s, especially 1000~5000mm 2 The composition may have a kinematic viscosity of 1.0 / s at 40°C.

[0066] The lubricant is typically at least 2, 3, 5, 10, 20, 30, 40, or 50 mm 2 In another embodiment, the lubricant may have a kinematic viscosity of 10 to 5000 mm / s at 100° C. 2 / s (cSt), preferably 30 to 3000 mm 2 / s, especially 50~2000mm 2 The composition may have a kinematic viscosity at 100° C. of 1.0 μm / s.

[0067] The lubricant may have a viscosity index (VI) of at least 150, 160, 170, 180, 190 or 200.

[0068] The base oil may be selected from the group consisting of mineral oils (Group I, II or III oils), polyalphaolefins (Group IV oils), polymerized and copolymerized olefins, alkylnaphthalenes, alkylene oxide polymers, silicone oils, phosphate esters and carboxylate esters (Group V oils). Preferably, the base oil is selected from Group I, Group II, Group III base oils, or mixtures thereof, according to the API definition. The definition of base oil is the same as that described in the American Petroleum Institute (API) publication "Engine Oil Licensing and Certification System", Industry Services Department, Fourteenth Edition, December 1996, Addendum 1, December 1998. The publication classifies base oils as follows: a) Group I base oils contain less than 90% saturates (ASTM D2007) and / or more than 0.03% sulfur (ASTM D2622) and have a viscosity index greater than or equal to 80 and less than 120 (ASTM D2270). b) Group II base oils contain greater than or equal to 90 percent saturates and less than or equal to 0.03 percent sulfur and have a viscosity index greater than or equal to 80 and less than 120. c) Group III base oils contain greater than or equal to 90 percent saturates and less than or equal to 0.03 percent sulfur and have a viscosity index greater than or equal to 120. d) Group IV base oils contain polyalphaolefins. Polyalphaolefins (PAOs), including known PAO materials, typically comprise relatively low molecular weight hydrogenated polymers or oligomers of alphaolefins, including but not limited to C2 to about C32 alphaolefins, with C8 to C16 alphaolefins, such as 1-octene, 1-decene, and 1-dodecene being preferred. Preferred polyalphaolefins are poly-1-octene, poly-1-decene, and poly-1-dodecene. e) Group V base oils include base oils not listed in Groups I to IV. Examples of Group V base oils include alkyl naphthalenes, alkylene oxide polymers, silicone oils, and phosphate esters.

[0069] Synthetic base oils include hydrocarbon oils and halo-substituted hydrocarbon oils, such as polymerized and copolymerized olefins (e.g., polypropylene, propylene-isobutylene copolymers, chlorinated polybutylene, poly(1-hexene), poly(1-octene), poly(1-decene)); alkylbenzenes (e.g., dodecylbenzene, tetradecylbenzene, dinonylbenzene, di(2-ethylhexyl)benzene); polyphenyls (e.g., biphenyl, terphenyl, alkylated polyphenols); and alkylated diphenyl ethers and alkylated diphenyl sulfides and their derivatives, analogs, and congeners.

[0070] Alkylene oxide polymers and interpolymers and their derivatives in which the terminal hydroxyl groups have been modified by esterification, etherification, etc., constitute another class of known synthetic base oils. These include, for example, polyoxyalkylene polymers prepared by polymerization of ethylene oxide or propylene oxide, as well as alkyl and aryl ethers of polyoxyalkylene polymers (e.g., methyl-polyisopropylene glycol ether having a molecular weight of 1000 or diphenyl ethers of polyethylene glycols having a molecular weight of 1000-1500); and their mono- and polycarboxylic acid esters, such as acetate esters of tetraethylene glycol, mixed C3-C8 fatty acid esters, and C13 oxo acid diesters.

[0071] Silicone-based oils, such as polyalkyl-, polyaryl-, polyalkoxy- or polyaryloxy silicone oils and silicate oils, constitute another useful class of synthetic base oils; such base oils include tetraethyl silicate, tetraisopropyl silicate, tetra-(2-ethylhexyl) silicate, tetra-(4-methyl-2-ethylhexyl) silicate, tetra-(p-tert-butyl-phenyl) silicate, hexa-(4-methyl-2-ethylhexyl) disiloxane, poly(methyl) siloxane, and poly(methylphenyl) siloxane. Other synthetic base oils include liquid esters of phosphorus-containing acids (e.g., tricresyl phosphate, trioctyl phosphate, diethyl ester of decylphosphonic acid), and polymeric tetrahydrofurans.

[0072] Suitable lubricant additives may be selected from viscosity index improvers, polymeric thickeners, antioxidants, corrosion inhibitors, detergents, dispersants, antifoam agents, dyes, anti-wear additives, extreme pressure additives (EP additives), anti-wear additives (AW additives), friction modifiers, metal deactivators, pour point depressants.

[0073] Viscosity index improvers include high molecular weight polymers that increase the relative viscosity of oils at high temperatures compared to their relative viscosity at low temperatures. Viscosity index improvers include polyacrylates, polymethacrylates, alkyl methacrylates, vinylpyrrolidone / methacrylate copolymers, polyvinylpyrrolidones, polybutenes, olefin copolymers such as ethylene-propylene copolymers or styrene-butadiene copolymers, or polyalkenes such as PIB, styrene / acrylate copolymers, and polyethers, and combinations thereof. The most common Vl improvers are methacrylate polymers and copolymers, acrylate polymers, olefin polymers and copolymers, and styrene-butadiene copolymers. Other examples of viscosity index improvers include polymethacrylates, polyisobutylenes, α-olefin polymers, α-olefin copolymers (e.g., ethylene-propylene copolymers), polyalkylstyrenes, phenol condensates, naphthalene condensates, styrene-butadiene copolymers, and the like. Of these, preferred are polymethacrylates having a number average molecular weight of 10,000 to 300,000, and α-olefin polymers or α-olefin copolymers having a number average molecular weight of 1,000 to 30,000, in particular ethylene-α-olefin copolymers having a number average molecular weight of 1,000 to 10,000. The viscosity index improvers can be used alone or in the form of a mixture, conveniently added in an amount ranging from 0.05% to 20.0% by weight based on the weight of the base stock.

[0074] Suitable (polymeric) thickeners include, but are not limited to, polyisobutene (PIB), oligomeric copolymers (OCP), polymethacrylates (PMA), copolymers of styrene and butadiene, or high viscosity esters (complex esters).

[0075] Antioxidants include phenolic antioxidants, such as hindered phenolic antioxidants, or non-phenolic antioxidants.

[0076] Useful phenolic antioxidants include hindered phenols. These phenolic antioxidants may be ashless (metal-free) phenolic compounds or neutral or basic metal salts of certain phenolic compounds. Representative phenolic antioxidant compounds are hindered phenols, which contain sterically hindered hydroxyl groups, including derivatives of dihydroxyaryl compounds in which the hydroxyl groups are in the o- or p-position relative to each other. Representative phenolic antioxidants include hindered phenols substituted with alkyl groups having six or more carbon atoms, and alkylene-linked derivatives of these hindered phenols. Examples of such phenolic materials are 2-t-butyl-4-heptylphenol; 2-t-butyl-4-octylphenol; 2-t-butyl-4-dodecylphenol; 2,6-di-t-butyl-4-heptylphenol; 2,6-di-t-butyl-4-dodecylphenol; 2-methyl-6-t-butyl-4-heptylphenol; and 2-methyl-6-t-butyl-4-dodecylphenol. Other useful hindered monophenolic antioxidants include, for example, hindered 2,6-di-alkylphenol propionate derivatives. Bisphenolic antioxidants can also be used in conjunction with the present invention. Examples of ortho-bonded phenols include: 2,2'-bis(4-heptyl-6-t-butyl-phenol); 2,2'-bis(4-octyl-6-t-butyl-phenol); and 2,2'-bis(4-dodecyl-6-t-butyl-phenol). Examples of para-bonded bisphenols include, for example, 4,4'-bis(2,6-di-t-butyl-phenol) and 4,4'methylene-bis(2,6-di-t-butylphenol).

[0077] Non-phenolic antioxidants that can be used include aromatic amine antioxidants, which can be used on their own or in combination with phenols. Representative examples of non-phenolic antioxidants include: alkylated and non-alkylated aromatic amines, such as those of formula R 8 R 9 R10 N aromatic monoamines, where R 8 is an aliphatic, aromatic or substituted aromatic group; R 9 is an aromatic or substituted aromatic group, R 10 is H, alkyl, aryl, or R 11 S(O) x R 12 and R 11 is an alkylene, alkenylene or aralkylene group; R 12 is a higher alkyl group, or an alkenyl, aryl, or alkaryl group, and x is 0, 1, or 2. 8 may contain from 1 to about 20 carbon atoms, preferably from about 6 to 12 carbon atoms. The aliphatic group is a saturated aliphatic group. Preferably, R 8 and R 9 are both aromatic or substituted aromatic groups, and the aromatic groups may be fused ring aromatic groups such as naphthyl. 8 and R 9 may be linked together with other groups such as S.

[0078] Typical aromatic amine antioxidants have alkyl substituents of at least about 6 carbon atoms. Examples of aliphatic groups include hexyl, heptyl, octyl, nonyl, and decyl. Generally, aliphatic groups do not contain more than about 14 carbon atoms. General types of amine antioxidants useful in the present compositions include diphenylamines, phenylnaphthylamines, phenothiazines, imidodibenzyls, and diphenylphenylenediamines. Mixtures of two or more aromatic amines are also useful. Polymeric amine antioxidants can also be used. Specific examples of aromatic amine antioxidants useful in the present invention include: p,p'-dioctyldiphenylamine; t-octylphenyl-alphanaphthylamine; phenyl-alphanaphthylamine; and p-octylphenyl-alphanaphthylamine. Sulfurized alkylphenols and their alkali or alkaline earth metal salts are also useful antioxidants.

[0079] Corrosion inhibitors can include a variety of oxygen-, nitrogen-, sulfur-, and phosphorus-containing materials, metal-containing compounds (salts, organometallics, etc.), and non-metal-containing or ashless materials. Corrosion inhibitors include, for example, hydrocarbyl-, aryl-, alkyl-, arylalkyl-, and alkylaryl-type detergents (neutral, overbased), sulfonates, phenates, salicylates, alcoholates, carboxylates, salixarates, phosphites, phosphates, thiophosphates, amines, amine salts, amine phosphates, amine sulfonates, alkoxylated amines, ether amines, polyether amines, amides, imides, azoles, diazoles, triazoles, benzotriazoles, benzothiadol ... The additive types may include, but are not limited to, heterocyclic amines, heterocyclic sulfides, thiazoles, thiadiazoles, mercaptothiadiazoles, dimercaptothiadiazoles (DMTD type), imidazoles, benzimidazoles, dithiobenzimidazoles, imidazolines, oxazolines, Mannich reaction products, glycidyl ethers, anhydrides, carbamates, thiocarbamates, dithiocarbamates, polyglycols, and the like, or mixtures thereof.

[0080] Detergents include detergents that adhere to dirt particles and prevent them from adhering to critical surfaces. Detergents can also adhere to the metal surface itself to keep it clean and prevent corrosion from occurring. Detergents include calcium alkyl salicylates, calcium alkyl phenates, and calcium alkaryl sulfonates using alternative metal ions such as magnesium, barium, or sodium. Examples of detergents and dispersants that can be used include metal-based detergents such as neutral and basic alkaline earth metal sulfonates, alkaline earth metal phenates, and alkaline earth metal salicylates, alkenyl succinimides and alkenyl succinimide esters and their boron hydrogen, phenates, salienius complex detergents, and ashless dispersants modified with sulfur compounds. These agents can be used singly or in the form of mixtures, conveniently added in amounts ranging from 0.01% to 1.0% by weight based on the weight of the base stock, and they can also be high total base number (TBN), low TBN, or high / low TBN mixtures.

[0081] Dispersants are lubricant additives that help prevent the formation of sludge, varnish, and other deposits on critical surfaces. Dispersants may be succinimide dispersants (e.g., N-substituted long chain alkenyl succinimides), Mannich dispersants, ester-containing dispersants, condensation products of fatty hydrocarbyl monocarboxylic acylating agents with amines or ammonia, alkylaminophenol dispersants, hydrocarbyl-amine dispersants, polyether dispersants, or polyetheramine dispersants. In one embodiment, succinimide dispersants include polyisobutylene-substituted succinimides, where the polyisobutylene from which the dispersant is derived may have a number average molecular weight of about 400 to about 5000, or about 950 to about 1600. In one embodiment, dispersants include borated dispersants. Typically, borated dispersants include succinimide dispersants, including polyisobutylene succinimides, where the polyisobutylene from which the dispersant is derived may have a number average molecular weight of about 400 to about 5000. Borated dispersants are described in more detail above in the description of extreme pressure agents.

[0082] The antifoaming agent may be selected from silicones, polyacrylates, and the like. The amount of antifoaming agent in the lubricant compositions described herein may range from 0.001 wt% to 0.1 wt% based on the total weight of the formulation. As a further example, the antifoaming agent may be present in an amount of about 0.004 wt% to about 0.008 wt%.

[0083] Suitable extreme pressure agents are sulfur-containing compounds. In one embodiment, the sulfur-containing compound may be a sulfurized olefin, a polysulfide, or a mixture thereof. Examples of sulfurized olefins include sulfurized olefins derived from propylene, isobutylene, pentene; polysulfides including organic sulfides and / or benzyl disulfides; bis-(chlorobenzyl) disulfide; dibutyl tetrasulfide; di-tertiary butyl polysulfide; and sulfurized methyl ester of oleic acid, sulfurized alkylphenol, sulfurized dipentene, sulfurized terpene, sulfurized Diels-Alder adduct, alkylsulfenyl N'N-dialkyldithiocarbamate; or a mixture thereof. In one embodiment, the sulfurized olefins include sulfurized olefins derived from propylene, isobutylene, pentene, or a mixture thereof. In one embodiment, the sulfur-containing compound of the extreme pressure additive includes dimercaptothiadiazole or derivative, or a mixture thereof. Examples of dimercaptothiadiazoles include compounds such as 2,5-dimercapto-1,3,4-thiadiazole or hydrocarbyl-substituted 2,5-dimercapto-1,3,4-thiadiazoles or oligomers thereof. Hydrocarbyl-substituted 2,5-dimercapto-1,3,4-thiadiazole oligomers are typically formed by forming sulfur-sulfur bonds between 2,5-dimercapto-1,3,4-thiadiazole units to form derivatives or oligomers of two or more of the thiadiazole units. Suitable 2,5-dimercapto-1,3,4-thiadiazole derived compounds include, for example, 2,5-bis(tert-nonyldithio)-1,3,4-thiadiazole or 2-tert-nonyldithio-5-mercapto-1,3,4-thiadiazole. The number of carbon atoms of the hydrocarbyl substituent of the hydrocarbyl-substituted 2,5-dimercapto-1,3,4-thiadiazole typically includes 1 to 30, or 2 to 20, or 3 to 16. The extreme pressure additive includes a compound containing boron and / or sulfur and / or phosphorus. The extreme pressure agent may be present in the lubricant composition at 0 wt% to about 20 wt%, or about 0.05 wt% to about 10.0 wt%, or about 0.1 wt% to about 8 wt% of the lubricant composition.

[0084] Examples of anti-wear additives include organic borates, organic phosphites such as didodecyl phosphite, organic sulfur-containing compounds such as sulfurized sperm oil or sulfurized terpenes, zinc dialkyldithiophosphates, zinc diaryldithiophosphates, phosphosulfurized hydrocarbons, and any combination thereof.

[0085] Friction modifiers can include metal-containing compounds or materials and ashless compounds or materials, or mixtures thereof. Metal-containing friction modifiers can include metal salts or metal-ligand complexes, where the metal can include alkali metals, alkaline earth metals, or transition group metals. Such metal-containing friction modifiers can also have low ash properties. Transition metals can include Mo, Sb, Sn, Fe, Cu, Zn, and the like. Ligands can include hydrocarbyl derivatives of alcohols, polyols, glycerol, partial ester glycerol, thiols, carboxylates, carbamates, thiocarbamates, dithiocarbamates, phosphates, thiophosphates, dithiophosphates, amides, imides, amines, thiazoles, thiadiazoles, dithiazoles, diazoles, triazoles, and other polar molecular functional groups containing effective amounts of O, N, S, or P, alone or in combination. In particular, Mo-containing compounds such as Mo-dithiocarbamates, Mo(DTC), Mo-dithiophosphates, Mo(DTP), Mo-amines, Mo(Am), Mo-alcoholates, Mo-alcohol-amides, and the like, may be particularly effective.

[0086] Ashless friction modifiers may include lubricant materials containing an effective amount of polar groups, such as hydroxyl-containing hydrocarbyl base oils, glycerides, partial glycerides, glyceride derivatives, and the like. Polar groups in friction modifiers may include hydrocarbyl groups containing effective amounts of O, N, S, or P, alone or in combination. Other friction modifiers that may be particularly effective include, for example, salts of fatty acids (both ash-containing and ashless derivatives), fatty alcohols, fatty amides, fatty esters, hydroxyl-containing carboxylates, and equivalent synthetic long-chain hydrocarbyl acids, alcohols, amides, esters, hydroxycarboxylates, and the like. In some cases, fatty organic acids, fatty amines, and sulfurized fatty acids may be used as suitable friction modifiers. Examples of friction modifiers include fatty acid esters and amides, organomolybdenum compounds, molybdenum dialkylthiocarbamates, and molybdenum dialkyldithiophosphates.

[0087] Suitable metal deactivators include benzotriazole and its derivatives, such as 4- or 5-alkylbenzotriazoles (e.g., triazoles) and their derivatives, 4,5,6,7-tetrahydrobenzotriazole, and 5,5'-methylenebisbenzotriazole; Mannich bases of benzotriazoles or triazoles, such as 1-[bis(2-ethylhexyl)aminomethyl)triazole and 1-[bis(2-ethylhexyl)aminomethyl)benzotriazole; and alkoxyalkylbenzotriazoles, such as 1-(nonyloxymethyl)benzotriazole, 1-(1-butoxyethyl)benzotriazole, and 1-(1-cyclohexyloxybutyl)triazole, and combinations thereof. Further non-limiting examples of the one or more metal deactivators include 1,2,4-triazole and its derivatives, such as 3-alkyl (or aryl)-1,2,4-triazoles, and Mannich bases of 1,2,4-triazoles, such as 1-[bis(2-ethylhexyl)aminomethylene 1-1,2,4-triazole; alkoxyalkyl 1-1,2,4-triazoles, such as 1-(1-butoxyethyl)-1,2,4-triazole; and acylated 3-amino-1,2,4-triazoles, imidazole derivatives, such as 4,4'-methylenebis(2-undecyl-5-methylimidazole) and bis[(N-methyl)imidazol-2-yl]-carbinol octyl ether, and combinations thereof. Further non-limiting examples of the one or more metal deactivators include sulfur-containing heterocyclic compounds, such as 2-mercaptobenzothiazole, 2,5-dimercapto-1,3,4-thiadiazole, and derivatives thereof; and 3,5-bis-[di(2-ethylhexyl)aminomethyl]-1,3,4-thiadiazolin-2-one, and combinations thereof. Further non-limiting examples of the one or more metal deactivators include amino compounds, such as salicylidene propylene diamine, salicylamino guanidine, and salts thereof, and combinations thereof.The one or more metal deactivators are not particularly limited in amount in the composition, but are typically present in an amount of about 0.01 to about 0.1, about 0.05 to about 0.01, or about 0.07 to about 0.1 wt % based on the weight of the composition. Alternatively, the one or more metal deactivators may be present in an amount less than about 0.1 wt %, less than about 0.7 wt %, or less than about 0.5 wt % based on the weight of the composition.

[0088] Pour point depressants (PPDs) include polymethacrylates, alkylated naphthalene derivatives, and combinations thereof. Commonly used additives such as alkyl aromatic polymers and polymethacrylates are also useful for this purpose. Typically, treat rates range from 0.001 wt% to 1.0 wt%, based on the weight of the base stock.

[0089] Demulsifiers include trialkyl phosphates and various polymers and copolymers of ethylene glycol, ethylene oxide, propylene oxide, or mixtures thereof.

[0090] The present invention further relates to the use of a comb copolymer or a comb copolymer obtainable by the process according to the invention for improving the viscosity index of a lubricant. EXAMPLES

[0091] Example 1 Polyisobutylene phenol ("PIB-phenol 1000") was prepared from polyisobutene (Mn 1000 g / mol) and phenol catalyzed by BF3-phenol complex according to WO 2018 / 024563. It was obtained as a 70 wt% solution in a hydrogenated highly isoparaffinic hydrocarbon solvent (KV100 3.0 mm2 / s, VI 111, pour point -30°C) with an average molecular weight of 1350 g / mol (calculated from OH number OHN) and an average number of isobutene units of 22.5.

[0092] 907 g of PIB-Phenol 1000, 0.39 g of 2,6-di-tert-butyl-4-methylphenol BHT, 67.6 g of methacrylic anhydride MAAh were heated to 86° C. After 4 hours, 0.5 g of NaOH (50 wt % in water) was added. After 12 hours, an additional 23.1 g of MAAh was added. After a total reaction time of 16 hours, 150 g of water was added and stirred for 11 hours at a bath temperature of 95° C. Excess MAAh and water were distilled off in vacuum. 922 g of product solution was obtained. The conversion was quantitative as determined by 1H NMR. Neither MAAh nor methacrylic acid MAA could be identified.

[0093] Example 2 Polyisobutylene phenol ("PIB-phenol 2300") was prepared from polyisobutene (Mn 2300 g / mol) and phenol catalyzed by BF3-phenol complex according to WO 2018 / 024563. It was obtained without solvent and had an average molecular weight of 3300 g / mol (calculated from OHN) and an average number of isobutene units of 57.1.

[0094] 277g PIB-Phenol 2300, 119g hydrogenated highly isoparaffinic hydrocarbon solvent (see Example 1), 0.12g BHT, and 16.5g MAAh were heated to 85°C. After 1.4 hours, 0.13g NaOH (50wt% in water) was added. After a total reaction time of 9 hours, 50g water was added and stirred for 19 hours at a bath temperature of 95°C. The bath temperature was then reduced to 70°C and the aqueous phase was discarded after phase separation.

[0095] An additional 50 g of water was added and the mixture was stirred for 5 min. After phase separation, the aqueous phase was discarded. Excess MAA and water were distilled off in vacuum. 382 g of product solution was obtained. The conversion was quantitative as determined by 1H NMR. Neither MAAh nor MAA could be identified.

[0096] Example 3 To the reactor was added: - 71.4 g of PIB macromonomer of Example 1 (70 wt % solution) - 175g EHMA 2-Ethylhexyl Methacrylate, - 25g MMA (Methyl Methacrylate) - 0.20g TDDM tert-dodecyl mercaptan - 145g Nexbase® 3030

[0097] The monomer weight percentages are as follows: 20 wt% PIB macromonomer, 70 wt% EHMA, 10 wt% MMA.

[0098] The mixture was heated to 95°C under nitrogen with stirring. Once 95°C was reached, 1 / 3 of the total solution of initiator tert-butyl-peroxyethylhexanoate TBPEH was added within 5 minutes (total solution 3g TBPEH in 29.64g Catenex T121). The mixture was stirred for another 10 minutes. Then 2 / 3 of the TBPEH solution was added in three portions during 3 hours: 1st = 1g, 2nd = 2g, 3rd = 2g. The mixture was then treated at 95°C for 1 hour. 5.56g of a 9% solution of TBPEH was finally added and the mixture was stirred at 95°C for another hour.

[0099] After 1 hour, 408.3 g of Nextbase® 3030 (hydrogenated highly isoparaffinic hydrocarbon base stock, Neste, KV40 12 mm 2 / s, KV100 3.0mm 2 / s, VI 111) was added to bring the total polymer content to about 30%. The mixture was stirred for 30 minutes to make it homogenous.

[0100] Molecular weights were determined by GPC using polystyrene calibration: Mn 108,000 g / mol, Mw 392,000 g / mol, PDI 3.6.

[0101] The application test results are as follows: KV100: 357mm 2 / s (30wt% polymer solution) KV40: 36.95mm 2 / s (5wt% of 30wt% polymer solution) KV100: 7.7 mm 2 / s (5wt% of 30wt% polymer solution) VI:186

[0102] The kinematic viscosity at 100°C (KV100) of the lubricants was measured according to ASTM D445 / 446. The higher the viscosity index VI (DIN ISO2909), the smaller the effect of temperature on the kinematic viscosity.

[0103] Example 4 To the reactor was added: - 132.2 g of PIB macromonomer of Example 1 (70 wt % solution) - 52.6 g EHMA 2-Ethylhexyl Methacrylate, - 21.5g MMA Methyl Methacrylate - 60.5g NBMA n-Butyl Methacrylate - 23.8gnoLMA Lauryl methacrylate - 0.15g TDDM tert-dodecyl mercaptan - 127g Nexbase® 3030

[0104] Lauryl methacrylate is a technical mixture containing mainly C12 / C14 methacrylates (70-75% C12, 24-30% C14, with small amounts of C10 and C16).

[0105] The monomer weight percentages are as follows: 37 wt% PIB macromonomer, 21 wt% EHMA, 8.5 wt% MMA, 24 wt% NBMA, and 9.5 wt% LMA.

[0106] The monomers were polymerized as described in Example 3.

[0107] Molecular weights were determined by GPC using polystyrene calibration: Mn 135,000 g / mol, Mw 562,000 g / mol, PDI 4.2.

[0108] The application test results are as follows: KV100: 402mm 2 / s (30wt% polymer solution) KV40: 35.6mm 2 / s (5wt% of 30wt% polymer solution) KV100: 7.5mm 2 / s (5wt% of 30wt% polymer solution) VI:186

[0109] Example 5 To the reactor was added: - 142.9 g of PIB macromonomer of Example 2 (70 wt % solution) - 37.5 g of 2-ethylhexyl methacrylate, - 12.5g methyl methacrylate - 100.0 g n-butyl methacrylate - 0.04g tert-dodecyl mercaptan - 123.9 g Yubas® 3 (hydrogenated light paraffinic mineral oil, SK Lubricants, Korea, CAS 64742-55-8)

[0110] The monomer weight percentages were as follows: 40 wt% PIB macromonomer, 15 wt% EHMA, 5 wt% MMA, 40 wt% NMBA. The monomers were polymerized as described in Example 3. Finally, Yubas® 3 was added to bring the total polymer content to about 30%.

[0111] Molecular weights were determined by GPC using polystyrene calibration: Mn 146,000 g / mol, Mw 387,000 g / mol, PDI 2.6.

[0112] The application test results are as follows: KV100: 519mm 2 / s (30wt% polymer solution) KV100: 6.8mm 2 / s (5 wt% in Chevron (registered trademark) 150R) KV40: 6.88mm2 / s (5 wt% in Chevron (registered trademark) 150R) VI:177

[0113] Chevron® 150R is a Group II paraffinic base oil with a KV40 of 29.4 mm 2 / s, KV100 is 5.25mm 2 / s (ASTM D445), VI is 112.

[0114] The shear stability was less than 1 when measured in a Bosch diesel injection pump according to CEC L-14-93 for 30 cycles, demonstrating the high shear stability of the comb polymer.

[0115] Example 6 To the reactor was added: - 142.9 g of PIB macromonomer of Example 2 (70 wt % solution) - 37.5 g of 2-ethylhexyl methacrylate, - 12.5g methyl methacrylate - 100.0 g n-butyl methacrylate - 0.04g tert-dodecyl mercaptan - 123.9g of Synative® ES2810 (trimethylolpropane esters of fatty acids, KV40 19.1mm 2 / s, KV100 4.4mm 2 / s, commercially available from BASF SE)

[0116] The monomer weight percentages were as follows: 40 wt% PIB macromonomer, 15 wt% EHMA, 5 wt% MMA, 40 wt% NBMA. The monomers were polymerized as described in Example 3. Finally, Synative® ES2810 was added to bring the total polymer content to approximately 30%.

[0117] Molecular weights were determined by GPC using polystyrene calibration: 152,000 Mn g / mol, 378,000 Mw g / mol.

[0118] The application test results are as follows: KV100: 650mm 2 / s (30wt% polymer solution) KV100: 6.88 mm 2 / s (5 wt% in Chevron (registered trademark) 150R) KV40: 31.7mm 2 / s (5 wt% in Chevron (registered trademark) 150R) VI:186

[0119] The shear stability was less than 1 when measured in a Bosch diesel injection pump according to CEC L-14-93 for 30 cycles, demonstrating the high shear stability of the comb polymer.

[0120] Example 7 To the reactor was added: - 142.9 g of PIB macromonomer of Example 2 (70 wt % solution) - 37.5 g of 2-ethylhexyl methacrylate, - 12.5g methyl methacrylate - 100.0 g n-butyl methacrylate - 0.04g tert-dodecyl mercaptan - 123.9 g Yubase® 4 (hydrogenated light paraffinic mineral oil, CAS 64742-54-7, SK Lubricants, Korea)

[0121] The monomer weight percentages were as follows: 40 wt% PIB macromonomer, 15 wt% EHMA, 5 wt% MMA, 40 wt% NBMA. The monomers were polymerized as described in Example 3. Finally, Yubase® 4 was added to bring the total polymer content to about 30%.

[0122] Molecular weights were determined by GPC using polystyrene calibration: 153,000 Mn g / mol, 371,000 Mw g / mol.

[0123] The application test results are as follows: KV100: 677mm 2 / s (30wt% polymer solution) KV100: 6.81 mm 2 / s (5 wt% in Chevron (registered trademark) 150R) KV40: 32.5mm 2 / s (5 wt% in Chevron (registered trademark) 150R) VI:175

[0124] The shear stability was less than 1 when measured in a Bosch diesel injection pump according to CEC L-14-93 for 30 cycles, demonstrating the high shear stability of the comb polymer.

Claims

1. In polymeric form, (A) PIB macromonomer of formula (I) 【Chemistry 1】 (In the formula, R 1 ~R 5 is hydrogen, C 1 ~C 20 -Alkyl, C 1 ~C 20 -Alkyloxy, C 8 ~C 7500 -Polyisobutyl and C 8 ~C 7500 -polyisobutenyl; R 1 ~R 5 At least one of 8 ~C 7500 -polyisobutyl group or C 8 ~C 7500 - a polyisobutenyl group, R 6 is hydrogen or methyl; (B) an acrylate monomer of formula (II) H 2 C=C(R 7 )COOR 8 (II) (In the formula, R 7 is hydrogen or methyl; R 8 is C 1~36 and (b) a cyclic alkyl group.

2. R 1 ~R 5 One of them is C. 8 ~C 7500 -polyisobutyl group or C 8 ~C 7500 2. The comb copolymer of claim 1, wherein the -polyisobutenyl group is

3. R 3 is C 8 ~C 7500 -polyisobutyl group or C 8 ~C 7500 3. A comb copolymer according to claim 1, wherein the R is a polyisobutenyl group.

4. C 8 ~C 7500 -polyisobutyl group or C 8 ~C 7500 - a moiety R which is not a polyisobutenyl group 1 ~R 5 A comb copolymer according to any one of claims 1 to 3, wherein is selected from the group: hydrogen, methyl or tert-butyl.

5. The acrylate monomer is a hydrophobic acrylate monomer of formula (IIa) H 2 C=C(R 7 )COOOR 8a (IIa) (In the formula, R 7 is hydrogen or methyl; R 8a is C 5~36 alkyl), and Hydrophilic acrylate monomers of formula (IIb) H 2 C=C(R 7 )COOR 8b (IIb) (In the formula, R 7 is hydrogen or methyl; R 8b is C 1~4 5. The comb copolymer of claim 1, wherein the aryl group is an alkyl group.

6. A comb copolymer according to any one of claims 1 to 5, comprising 5 to 60 wt% of said PIB macromonomer.

7. A comb copolymer according to any one of claims 1 to 6, comprising 25 to 90 wt% of said acrylate monomers.

8. 7. A comb copolymer according to claim 5 or 6, comprising up to 75 wt% of said hydrophobic acrylate monomers and at least 5 wt% of said hydrophilic acrylate monomers.

9. - 5 to 55 wt. % of PIB macromonomer, - 10 to 85 wt. % of a hydrophobic acrylate monomer, - 1 to 50 wt. % of a hydrophilic acrylate monomer; 7. A comb copolymer according to claim 5 or 6, wherein the sum of all monomers is 100 wt %.

10. Process for preparing the PIB macromonomer of formula (I) 【Chemistry 2】 (In the formula, R 1 ~R 5 is hydrogen, C 1 ~C 20 -Alkyl, C 1 ~C 20 -Alkyloxy, C 8 ~C 7500 -Polyisobutyl and C 8 ~C 7500 -polyisobutenyl; R 1 ~R 5 At least one of 8 ~C 7500 -polyisobutyl group or C 8 ~C 7500 - a polyisobutenyl group, R 6 is hydrogen or methyl; Polyisobutenephenol of formula (III) 【Chemistry 3】 with (meth)acrylic anhydride.

11. 11. The method of claim 10, wherein the (meth)acrylic anhydride is present in a molar excess relative to the polyisobutene phenol.

12. 12. The method of claim 10 or 11, wherein following the reaction, any remaining (meth)acrylic anhydride is hydrolyzed to form (meth)acrylic acid.

13. 13. The method of claim 12, wherein the (meth)acrylic acid is removed by distillation or extraction with water.

14. (i) a base oil; and (ii) a comb copolymer according to any one of claims 1 to 9 or obtainable by the method according to any one of claims 10 to 13, (iii) a further lubricant additive.

15. Use of a comb copolymer according to any one of claims 1 to 9 or obtainable by the process according to any one of claims 10 to 13 for improving the viscosity index of a lubricating oil.

Citation Information

Patent Citations

  • Vinyl-based and comb-like copolymer

    CN110402261A

  • Oil-soluble comb polymer

    JP2008546894A

  • Curable elastomer composition with low-temperature sealing properties

    JP2014517857A

  • Macromonomers containing polyisobutene groups, and their homopolymers or copolymers

    JP2019528343A

  • Macromonomers containing polyisobutene groups, and homopolymers or copolymers thereof

    US20190169346A1