Crosslinkable fluoropolymer
Crosslinking fluoropolymers at room temperature using keto-functional monomers and agents like DAAM and ADH addresses the challenge of crosslinking difficulties, enhancing toughness and melt viscosity in fluoropolymers.
Patent Information
- Application Number
- JP2024538289
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-11-16
- Publication Date
- 2024-12-06
AI Technical Summary
Existing fluoropolymers are difficult to crosslink, typically requiring radiation or high temperatures, and it is challenging to incorporate keto-functional monomers into their backbone.
A method for crosslinking fluoropolymers at room temperature using keto-functional monomers like DAAM or AAEM and cross-linking agents such as ADH or HMDA, allowing for the formation of crosslinked fluoropolymers without heat or radiation, and incorporating these monomers into the polymer backbone through chain transfer mechanisms.
The method results in fluoropolymers with increased toughness and melt viscosity, enabling easier processing and improved mechanical properties.
Smart Images

Figure 2024545470000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THEINVENTION This invention describes a novel approach to crosslinking fluoropolymers that can be prepared in 1K (one-pack self-crosslinking) and applied at room temperature. No heat or radiation is required for the crosslinking reaction. These features are not shown in a single prior art. [Background technology]
[0002] Related Technology Background There are several patents that describe crosslinkable fluoropolymers, but none of them use the 1K crosslinking chemistry described in this invention.
[0003] Russian Patent No. 2414762 describes a radiation crosslinked fluoropolymer composition comprising a fluoropolymer, triallyl isocyanurate and zinc oxide.
[0004] WO 2009 / 052163 describes a fluoropolymer composition obtained by crosslinking a block copolymer containing a hydrofluorocarbon and a polyamide-based crosslinking agent at 500° F. (260° C.) The crosslinked block copolymer is compatible with both non-hydrofluorocarbon-based fluoropolymers and engineering resins.
[0005] Japanese Patent No. 3171688 describes a composition containing a maleimide group (I), a fluorine-containing alicyclic structure polymer, and an NH2- and fluorine-containing alicyclic structure polymer. This composition is crosslinked by heating at 100 to 300°C.
[0006] Fluoropolymers are difficult to crosslink. Usually, crosslinking of fluoropolymers requires radiation or high temperature.
[0007] Due to the difference in reactivity, it is very difficult to copolymerize keto-functional monomers such as DAAM and AAEM with fluorinated monomers. Surprisingly, the present invention demonstrates that keto-functional monomers can become part of a polymer by incorporating the keto-functional monomer into the backbone of the fluoropolymer or by attaching an oligomer (containing the keto-functional monomer) to the fluoropolymer via a chain transfer mechanism. The resulting fluorinated keto-functional copolymers can be reacted with dihydrazides and diamines such as adipic acid dihydrazide (ADH) and hexamethylenediamine (HMDA) to form crosslinked fluoropolymers at room temperature or in a melt process.
[0008] The present invention uses ketohydrazide crosslinking based on keto-functional monomers such as AAEM (acetoacetoxyethyl methacrylate) or DAAM (diacetone acrylamide) and crosslinkers such as ADH (adipic acid dihydrazide) or hexamethylenediamine (HMDA).
[0009] The present invention provides novel fluoropolymers that can be crosslinked during the application process. Prior art crosslinkable fluoropolymers usually require special treatments such as heating or radiation. The crosslinking chemistry used in the present invention does not require heating or radiation. The crosslinking reaction can be carried out at ambient temperature. Furthermore, the crosslinking system of the present invention is a 1K system in which all components are packed in one container and the user does not need to mix or blend. The 1K system is much easier to use compared to the 2K crosslinking system in which the components are stored in two containers and the user needs to blend them before use. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Russian Patent No. 2414762 [Patent Document 2] International Publication No. 2009 / 052163 [Patent Document 3] Patent No. 3171688 Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention provides a composition comprising a fluorinated keto-functional copolymer that includes a keto-functional monomer unit, such as a DAAM or AAEM monomer unit, as part of the copolymer. The fluorinated keto-functional copolymer can be crosslinked. Additionally, the present invention provides a method for crosslinking a fluorinated keto-functional copolymer by melt processing the fluorinated keto-functional copolymer in the presence of a dihydrazide or diamine, or by providing a solution comprising the fluorinated keto-functional copolymer and a crosslinking agent, and then drying the solution. [Means for solving the problem]
[0012] Aspects of the invention Aspect 1: A composition comprising a fluorinated copolymer, the fluorinated copolymer comprising fluoro-monomeric units and keto-functional monomeric units incorporated as part of the polymer.
[0013] Aspect 2: The composition of aspect 1, wherein the copolymer comprises at least 95% by weight of fluorine-containing monomer units.
[0014] Aspect 3: The composition of aspect 1 or 2, wherein the fluorine monomer comprises VDF.
[0015] Aspect 4: The composition of any one of Aspects 1 to 3, wherein the fluorine monomer comprises HFP.
[0016] Embodiment 5: The composition of any one of embodiments 1 to 4, wherein the keto-functional monomer comprises DAAM.
[0017] Embodiment 6: The composition of any one of embodiments 1-4, wherein the keto-functional monomer comprises AAEM.
[0018] Aspect 7: The composition of any of Aspects 1-6, wherein the fluorinated copolymer has a melt viscosity greater than 5 kP, preferably greater than 7 kP.
[0019] Embodiment 8: The composition of any of embodiments 1-7, further comprising a crosslinker.
[0020] Embodiment 9: The composition of embodiment 8, wherein the crosslinker comprises AHD.
[0021] Example 10: The composition of example 8, wherein the crosslinker comprises hexamethylenediamine.
[0022] Aspect 11. The fluorinated copolymer has a compressive strength of 500,000 lb / in prior to crosslinking. 3 (3,450,000kN·m / m 3 11. The composition of any one of embodiments 1 to 10, having a toughness greater than 100.
[0023] Aspect 12: The composition of any of aspects 1-11, wherein the fluorinated copolymer is crosslinked and exhibits an increase in toughness of at least 25%, preferably at least 30%, and more preferably at least 35% compared to a non-crosslinked fluorinated copolymer.
[0024] Aspect 13. The fluorinated copolymer is crosslinked and has a strength of 900,000 lb / in 3 (6,200,000kN·m / m 3 12. The composition of any one of embodiments 1 to 11, wherein the composition exhibits a toughness greater than 100%.
[0025] Aspect 14: A method of crosslinking a fluoropolymer, comprising providing a fluorinated copolymer comprising keto-functional monomer units, blending the fluorinated copolymer with a crosslinking agent, and melt processing the blend of the fluorinated copolymer and the crosslinking agent.
[0026] Aspect 15: A method of crosslinking a fluoropolymer, comprising providing a fluorinated copolymer comprising keto-functional monomer units in the form of a latex, blending a crosslinker into the latex comprising the fluorinated copolymer, and then drying the latex.
[0027] Aspect 16: The method of any one of Aspects 14-15, wherein the fluoropolymer comprises vinylidene fluoride monomer units.
[0028] Example 17 The method of any one of Examples 14 to 16, wherein the fluoropolymer comprises a DAAM monomer unit.
[0029]
[0031] Aspect 18: The method of any one of aspects 14-17, wherein the crosslinking agent comprises a dihydrazide or a diamine.
[0030] Example 19: The method of any one of Examples 14 to 18, wherein the crosslinker comprises AHD.
[0031] Example 20: The method of any of Examples 14-18, wherein the crosslinker comprises hexamethylenediamine. [Brief description of the drawings]
[0032] [Figure 1] FIG. 1 is the stress strain curves of Examples 8 and 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Detailed Description of the Invention All documents cited in this application are incorporated herein by reference.
[0034] As used herein, percentages are weight percent (wt%) unless otherwise specified, and molecular weights are weight average molecular weight (Mw) unless otherwise specified. Molecular weights are measured by gel permeation chromatography (GPC) using PMMA (polymethylmethacrylate) standards.
[0035] Melt viscosity is based on ASTM D3835 at 230°C for 100 seconds. -1 This was measured by capillary rheometry at 1000 K.
[0036] "PVDF" means polyvinylidene fluoride.
[0037] "Copolymer" means a polymer having two or more different monomer units, including terpolymers and higher order polymers. "Polymer" is used to mean both homopolymers and copolymers. For example, as used herein, "PVDF" and "polyvinylidene fluoride" are used to mean both homopolymers and copolymers unless otherwise specified. "Fluoropolymer" is used to mean a polymer containing a fluorinated monomer. The polymer may be homogeneous, heterogeneous, or random, and may have a gradient distribution of comonomer units.
[0038] Ethylenic means that the monomer has a polymerizable carbon-carbon double bond.
[0039] Keto-functional monomers are ethylenic monomers that contain a ketone moiety and that when polymerized into a fluoropolymer retain the keto functionality and allow the keto functionality to be utilized for crosslinking, such as DAAM and AAEM.
[0040] The fluoropolymers of the present invention are fluorinated keto-functional copolymers.
[0041] In some embodiments, the present invention relates to copolymers that include a keto-functional monomer and a fluorine monomer, preferably vinylidene fluoride ("VDF"), in the backbone of the copolymer, and that are crosslinkable using a crosslinking agent.
[0042] The present invention relates to a process for producing a crosslinked fluoropolymer.
[0043] It is an object of the present invention to provide a fluoropolymer that can be crosslinked at room temperature or during melt processing.
[0044] The crosslinkable fluoropolymers of the present invention with keto functionality can be prepared in two ways. In the first way, a keto-functional monomer is copolymerized with a fluoromonomer to produce a fluoro-keto-functional copolymer. For example, VDF can be copolymerized with DAAM to produce a VDF / DAAM copolymer. A crosslinker can then be added to the copolymer latex or spray-dried copolymer after polymerization. In the second way, a keto-functional oligomer is first prepared by emulsion polymerization. This keto-functional oligomer latex is then added to a fluoromonomer polymerization. The fluoropolymer chains react with the keto-functional oligomer by a chain transfer mechanism to produce a PVDF-b-keto-functional block copolymer. A crosslinker is then added to the copolymer latex or spray-dried. In both ways, the fluorinated-keto-functional copolymer crosslinks when it is dried (in the case of a latex) or melt-processed.
[0045] In a preferred embodiment, the keto-functional monomer is DAAM and the crosslinker is ADH.
[0046] Fluorinated Keto-Functional Copolymers: The copolymer contains a fluorinated monomer unit and a keto-functional monomer unit. The fluorinated monomer unit accounts for the majority of the copolymer, accounting for 95% by weight or more, preferably 95 to 99.99% by weight, more preferably 97 to 99.99% by weight of the entire polymer.
[0047] The copolymers of the present invention are free of acrylate ester monomer units that do not have keto functionality. The comonomers of the present invention may contain acrylate ester monomer units that have keto functionality. The copolymers of the present invention prior to crosslinking are thermoplastic.
[0048] Monomer: The present invention incorporates keto-functional monomers or oligomers, such as diacetone acrylamide (DAAM), acetoacetoxyethyl methacrylate (AAEM) or oligomers thereof, into the fluoropolymer, which imparts ketone functionality to the fluorinated copolymer and can be reacted with a crosslinking agent to obtain a crosslinked fluoropolymer.
[0049] The present invention provides fluorinated copolymers that contain a fluorinated ethylenic monomer and a keto-functional monomer in the backbone of the copolymer or in the form of an oligomer in which the keto-functional monomer is attached to a fluoropolymer. This can be achieved in two ways. First, the keto-functional monomer is directly copolymerized with the fluorinated monomer. Second, an oligomer containing the keto-functional monomer can be first prepared and then the fluorinated monomer can be polymerized in the presence of the keto-functional oligomer to form the copolymer. Preferably, the keto-functional monomer is DAAM or AAEM.
[0050] Exemplary fluorinated ethylene monomers "fluoromonomers" include vinylidene fluoride (VDF), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), chlorotrifluoroethylene (CTFE), 1,2-difluoroethylene, perfluorobutylethylene (PFBE), hexafluoropropene (HFP), vinyl fluoride (VF), pentafluoropropene, 2,3,3,3-tetrafluoropropene, trifluoropropene, fluorinated (alkyl) vinyl ethers such as perfluoroethyl vinyl ether (PEVE), and perfluoro-2-propoxypropyl vinyl ether, perfluoromethyl vinyl ether (PMVE), perfluoropropyl vinyl ether (PPVE), perfluorobutyl vinyl ether (P ... perfluoro(1,3-dioxole) and perfluoro(2,2-dimethyl-1,3-dioxole) (PDD), C4 or higher partially or perfluorinated α-olefins, C3 or higher partially or perfluorinated cyclic alkenes, partially fluorinated aryl or fluorinated aryl monomers, and combinations thereof.
[0051] The other monomer units in these polymers may include any monomer that contains a polymerizable C=C double bond. Additional monomers include 2-hydroxyethyl allyl ether, 3-allyloxypropanediol, allyl monomer, ethane, propene, acrylic acid, and methacrylic acid.
[0052] Examples of fluorinated keto-functional copolymers in the compositions of the present invention include polyvinylidene fluoride (PVDF), polyhexafluoropropylene (PHFP), chlorotrifluoroethylene (CTFE), polytetrafluoroethylene (PTFE), polyperfluoromethylvinylether (PMVE), and combinations thereof, as well as copolymers and terpolymers thereof.
[0053] Preferably, the fluorinated keto-functional copolymer of the present invention contains 75% or more by weight of vinylidene fluoride monomer units. The fluoropolymer may contain a fluorocomonomer. For example, a predominantly VDF copolymer may contain HFP or TFE. Preferred comonomers include TFE, HFP, 2,3,3,3-tetrafluoropropene "1234yf", and 1,3,3,3-tetrafluoropropene.
[0054] Vinylidene fluoride copolymers include those that contain at least 75% by weight, preferably at least 80% by weight, and more preferably at least 95% by weight, vinylidene fluoride copolymerized with a keto-functional comonomer and one or more fluorinated comonomers.
[0055] In a preferred embodiment, the fluorinated keto functional copolymer is also acid functionalized, preferably an acid functionalized PVDF.
[0056] Methods for producing acid-functionalized fluoropolymers are known in the art. WO 2019 / 199753, WO 2016 / 149238 and U.S. Pat. No. 8,337,725 (the contents of each of which are incorporated herein by reference) provide some known methods for producing acid-functionalized fluoropolymers.
[0057] In some embodiments, the copolymer is VDF / HFP / DAAM or VDF / HFP / AAEM containing up to 29.99 wt.%, preferably up to 24.99 wt.%, more preferably up to 19.99 wt.%, or up to 9.99 wt.% hexafluoropropene (HFP) units based on the total monomer units. In all cases, the amount of DAAM or AAEM is at least 0.01 wt.%, and the total weight percent monomer units in the copolymer add up to 100%.
[0058] Preferably, the keto-functional fluorinated copolymer is such that the melt viscosity before crosslinking is at least 5 kPoise or more, preferably at least 7 kPoise or more, in some embodiments, the melt viscosity before crosslinking is at least 10 kPoise or more.
[0059] Polymerization process: Fluoropolymers such as polyvinylidene-based polymers can be prepared by any process known in the art, preferably using aqueous free radical emulsion polymerization, but also suspension, solution and supercritical CO2 polymerization processes. Processes such as emulsion and suspension polymerization are preferred and are described in U.S. Pat. No. 6,187,885 and European Patent No. 0,120,524. Keto-functional fluorinated copolymers are preferably prepared by emulsion polymerization.
[0060] In a typical emulsion polymerization process, a reactor is charged with deionized water, optionally a water-soluble surfactant capable of emulsifying the reactant mass during polymerization, and an optional paraffin wax antifouling agent. The mixture is stirred and deoxygenated. A predetermined amount of an optional chain transfer agent (CTA) is then introduced into the reactor, the temperature of the reactor is raised to a desired level, and monomer (e.g., a fluorinated monomer such as vinylidene fluoride, a keto-functional monomer, and optionally one or more other comonomers) is fed into the reactor. Once the initial charge of monomer has been introduced and the pressure in the reactor has reached a desired level, an initiator is introduced to start the polymerization reaction. The temperature of the reaction can vary depending on the characteristics of the initiator used, and one skilled in the art will know how to do so. Typically, the temperature is between about 30°C and 150°C, preferably between about 60°C and 120°C. Once the desired amount of polymer is reached in the reactor, the monomer feed is stopped, but the initiator feed is optionally continued to consume the residual monomer. Residual gases (including unreacted monomers) are vented and the latex is recovered from the reactor.
[0061] Surfactants: Preferably, the polymerizations of the present invention are carried out in the absence of a surfactant, however, a surfactant can be added to the polymerization process.
[0062] If used, the surfactant used in the polymerization can be any surfactant known in the art to be useful in PVDF emulsion polymerization, including perfluorinated, partially fluorinated, and non-fluorinated surfactants. Preferably, the PVDF emulsion is fluorosurfactant-free and no fluorosurfactants are used in any part of the polymerization. Non-fluorinated surfactants useful in PVDF polymerization can be both ionic and non-ionic in nature, including, but not limited to, 3-allyloxy-2-hydroxy-1-propanesulfonate, polyvinylphosphonic acid, polyvinylsulfonic acid, and salts thereof, polyethylene glycol and / or polypropylene glycol, and block copolymers thereof, alkylphosphonates, and siloxane-based surfactants.
[0063] Chain transfer agent: A chain transfer agent may be added to the polymerization to control the molecular weight of the product. The chain transfer agent may be added to the polymerization all at once at the beginning of the reaction, or may be added gradually or continuously throughout the reaction. The amount and method of addition of the chain transfer agent depends on the activity of the particular chain transfer agent used and the desired molecular weight of the polymer product. The amount of chain transfer agent added to the polymerization reaction is about 0 to 5 weight percent, preferably 0.05 to about 5 weight percent, and more preferably about 0.1 to about 2 weight percent, based on the total weight of monomers added to the reaction mixture. Examples of chain transfer agents useful in the present invention include, but are not limited to, oxygenated compounds such as alcohols (preferably having 3 to 10 carbons), carbonates, ketones, esters, and ethers. Those that can function as chain transfer agents include, but are not limited to, acetone, ethyl acetate, diethyl ether, methyl-t-butyl ether, isopropyl alcohol; bis(alkyl)carbonates (wherein the alkyl has 1-9 carbon atoms), such as bis(ethyl)carbonate, bis(isobutyl)carbonate; ethane, propane, and those described in US Patent Application Publication No. 2018 / 0072829, low molecular weight polymeric chain transfer agents containing one or more different functional groups, such as polyacrylic acid, polylactic acid, polyphosphonic acid, polysulfonic acid, and polymaleic acid. Some surfactants may also function as chain transfer agents.
[0064] Although not preferred, a paraffin-based antifoulant can be used if desired, as can any long chain saturated hydrocarbon wax or oil. The reactor loading of paraffin is 0.01% to 0.3% by weight based on the total weight of monomers used.
[0065] Buffer: The polymerization reaction mixture may optionally contain a buffer to maintain a controlled pH throughout the polymerization reaction. The pH is preferably controlled within the range of about 4 to about 8 to minimize undesirable color development in the product.
[0066] The buffer has at least one pK in the range of about 4 to about 10, preferably about 4.5 to about 9.5. a value and / or pK b The buffer may include an organic or inorganic acid or an alkali metal salt thereof having a value of 0.01 to 0.01, or a base or salt of the organic or inorganic acid. Preferred buffers in the practice of the invention include, for example, phosphate buffers and acetate buffers. A "phosphate buffer" is one or more salts of phosphoric acid. An "acetate buffer" is a salt of acetic acid.
[0067] The polymerization generally results in a latex having a solids level of 10-60% by weight, preferably 10-50% by weight, and an intensity average primary particle size of less than 500 nm, preferably less than 400 nm, more preferably less than 300 nm. The intensity average particle size is generally at least 20 nm, preferably at least 50 nm. The fluoropolymer particles in the dispersion have a primary particle size in the range of 50-600 nm, preferably 100-500 nm. The primary particle size of the latex is measured by dynamic light scattering using a NICOMP™380 submicron particle sizer. The data is reported as intensity average particle size (diameter).
[0068] The polymer or copolymer can be isolated using standard techniques such as oven drying, spray drying, shear coagulation or acid coagulation followed by drying, or can be retained in an aqueous medium for subsequent application or use.
[0069] Crosslinker: In the present invention, dihydrazides or diamines are preferred crosslinking agents, with adipic dihydrazide (ADH) and hexamethylenediamine (HMDA) being the most preferred.
[0070] Crosslinking of fluorinated keto-functional copolymers: Keto-functional monomers are typically incorporated into the fluoropolymer during the preparation of the polymer in an emulsion polymerization process, and crosslinkers are post-added to the fluorinated keto-functional copolymer after polymerization. Each crosslinker can react with two keto-functional groups to crosslink the fluorinated keto-functional copolymer chains. The crosslinking reaction occurs after water / solvent evaporation or during melt processing.
[0071] The fluorinated keto-functional copolymers can be crosslinked by melt processing in either latex or powder form.
[0072] The fluorinated keto-functional copolymer in a latex form can be combined with a crosslinker (preferably ADH, which is water soluble) to obtain an aqueous composition of fluorinated keto-functional copolymer and dissolved crosslinker. When the latex is dried, the crosslinker reacts with the keto-functional monomers in the fluoroplastic, crosslinking the polymer. Heat or vacuum is not required, but can be used to speed up drying. As an example, the fluorinated keto-functional copolymer can be used in a coating process. A latex composition containing the fluorinated keto-functional copolymer can be coated onto a substrate and dried. Upon drying, the crosslinker reacts with the keto functionality, resulting in crosslinking.
[0073] Alternatively, the fluorinated keto-functional copolymer can be spray-dried into a powder and then crosslinked by blending the keto-functional copolymer with a crosslinking agent that reacts with the keto-functional groups in the copolymer during melt processing. The fluorinated keto-functional copolymer is generally melt-processed at a temperature at least 20 degrees above the melting point of the fluorinated keto-functional copolymer. When the keto-functional copolymer melts, the crosslinking agent reacts with the keto-functional groups in the fluoropolymer to cause crosslinking. In one embodiment, the keto-functional unit comprises DAAM and the crosslinking agent comprises ADH. Melt processing includes extrusion and melt molding. Any process can be used in which the copolymer is melted and molded into a desired shape.
[0074] After crosslinking, the fluorinated keto-functional copolymers exhibit higher melt viscosity and improved mechanical properties. The melt viscosity is increased by at least 50% and the toughness is increased by at least 20%, preferably 30%, compared to the same copolymer before crosslinking. Preferably, the fluorinated copolymer has a melt viscosity of 500,000 lb / in before crosslinking. 3 (3,450,000kN·m / m 3 Preferably, the fluorinated copolymer has a toughness of greater than 900,000 lb / in after crosslinking. 3 (6,200,000kN·m / m 3 ) and has a toughness exceeding that of
[0075] use: The fluorinated keto-functional copolymers of the present invention may find use in many applications such as coatings, industrial parts, chemical processes, and membranes.
[0076] The fluorinated keto-functional copolymers of the present invention can be used to prepare coatings that are resistant to chemical penetration.
[0077] In a further aspect, the present invention also relates to articles made from compositions comprising the fluorinated keto-functional copolymers.
[0078] In a further aspect, the invention relates to a method of making a molded article, said method comprising processing a composition comprising a fluorinated keto-functional copolymer.
[0079] The fluorinated keto functional copolymers of this invention can be processed into articles of desired shape by molding (injection molding, extrusion), calendaring or extrusion.
[0080] The fluorinated keto-functional copolymers of the present invention can be used in a variety of applications, including batteries and coatings.
[0081] The invention, its features and the various advantages it offers will become clearer on reading the following examples, provided as illustrative and non-limiting examples. EXAMPLES
[0082] The melt viscosity (MV) of the resin was measured in accordance with ASTM D3835 using a DYNISCO LCR-7000 at 230°C for 100 seconds. -1 The measurement was performed by capillary rheometry under the following conditions.
[0083] Light scattering test method for latex particle size: Measure the particle size of latex particles using a Nicomp CW380 particle size analyzer (light scattering method). Use the volume average particle size.
[0084] The incorporation rate of keto-functional monomer (DAAM) into PVDF is 19 Measurements were made by F-NMR.
[0085] The test methods for yield stress, break stress, toughness, and Young's modulus were measured using a type 1 tensile bar according to ASTM D683, 23° C., 50 mm / min.
[0086] Example 1: Preparation of VDF-DAAM copolymer To a 2 gallon autoclave was added 3000 g of deionized water. The autoclave was purged with argon / nitrogen three times (stirring stopped during venting) followed by a low flow argon / nitrogen purge for 15 minutes with a slow stirrer at 15 rpm. The autoclave was sealed, stirred at 72 rpm, heated to 100°C, and pressurized to 650 psi with vinylidene fluoride. A 3.0 wt% potassium persulfate (KPS) and 1.0 wt% sodium acetate (SAT) aqueous feed was started at 60.0 mL / h. Once the pressure began to drop, the KPS / SAT feed rate was reduced to 25.0 mL / h and pressure was maintained by additional VDF feeds. A 5.0 wt% DAAM solution feed was started at 150.0 mL / h to feed a total of 1700 mL of VDF. Feeds continued in this manner until a total of 1800 g of VDF had been fed to the autoclave. The reaction temperature was reduced to 83° C. while feeding KPS / SAT at 10.0 mL / h for an additional 30 min. The pressure was then allowed to reduce spontaneously over 10 min, at which point the reactor was vented to atmospheric pressure and cooled to room temperature. The product was discharged from the reactor and spray dried. ADH can be added before or after spray drying at a molar ratio of DAAM / ADH=2 / 1. The particle size was 217 nm by light scattering.
[0087] This example shows that VDF / DAAM copolymers can be prepared. Table 1 shows that the MV more than doubles after crosslinking with ADH.
[0088] Example 2: Preparation of VDF-HFP-DAAM copolymer (without surfactant) To a 2 gallon autoclave was added 3200 g of deionized water. The autoclave was purged with argon / nitrogen three times (stirring stopped during venting), followed by a low flow argon / nitrogen purge for 15 minutes with a slow stirrer at 15 rpm. The autoclave was sealed, stirred at 72 rpm, heated to 100°C, and pressurized to 650 psi with 58 mL of HFP and 494 mL of vinylidene fluoride. A 3.0 wt% potassium persulfate (KPS) and 1.0 wt% sodium acetate (SAT) aqueous solution feed was started at 60.0 mL / h. Once pressure began to drop, the KPS / SAT feed rates were reduced to 25.0 mL / h and pressure was maintained by additional VDF feeds. HFP was fed at 30.0 mL / h up to a total of 108.0 mL of HFP. A feed of 5.0 wt % DAAM solution was started at 150.0 mL / h to feed a total of 1700 mL VDF. Feeds continued in this manner until a total of 1800 g VDF had been fed to the reactor. The reaction temperature was reduced to 83° C. over an additional 30 minutes while feeding KPS / SAT at 10.0 mL / h. The pressure was then allowed to reduce spontaneously over 10 minutes, at which point the reactor was vented to atmospheric pressure and cooled to room temperature. The product was discharged from the reactor and spray dried. Light scattering was at 300 nm.
[0089] This indicates that a copolymer of VDF / HFP / DAAM can be prepared. Table 1 shows that the MV is more than doubled after crosslinking with ADH.
[0090] Example 3: Preparation of VDF-HFP-DAAM copolymer with PAA functional groups To a 2 gallon autoclave was added 3200 g of deionized water. The autoclave was purged with argon / nitrogen three times (stirring stopped while venting), followed by a low flow argon / nitrogen purge for 15 minutes with a slow stirrer at 15 rpm. The autoclave was sealed, stirred at 72 rpm, heated to 100°C, and pressurized to 650 psi with 58 mL of HFP and 494 mL of vinylidene fluoride. A 3.0 wt% potassium persulfate (KPS) and 5.0 wt% polyacrylic acid (PAA) aqueous solution feed was started at 120.0 mL / h. Once pressure began to drop, the KPS / SAT feed rate was reduced to 30.0 mL / h and pressure was maintained by additional VDF feed. HFP was fed at 30.0 mL / h up to a total of 108.0 mL of HFP. A feed of 5.0 wt % DAAM solution was started at 200.0 mL / h to feed a total of 1650 mL VDF. Feeds continued in this manner until a total of 1700 g VDF had been fed to the reactor. The reaction temperature was maintained at 100° C. with KPS / SAT fed at 10.0 mL / h for an additional 30 minutes. The pressure was then allowed to spontaneously reduce over 10 minutes, at which point the reactor was vented to atmospheric pressure and cooled to room temperature. The product was discharged from the reactor and spray dried. The particle size was 218 nm.
[0091] This indicates that copolymers of VDF / HFP / DAAM with acid functionality can be prepared. Table 1 shows that the MV more than doubles after crosslinking with ADH.
[0092] Effect of crosslinking on melt viscosity: The melt viscosity (MV) of VDF-DAAM and VDF-HFP-DAAM copolymers (examples 1, 2 and 3) was measured with and without the addition of ADH. Without ADH, the copolymers are not crosslinked. The MV of all three copolymers was in the mid 20 kP. The addition of ADH was achieved by sealing the copolymer powder (spray-dried powder) and ADH powder in a plastic container and shaking the container for 30 minutes. The melt viscosity was then measured for the powder blends. Crosslinking of DAAM / ADH occurred during the melting process. After crosslinking, the MV increased significantly.
[0093] [Table 1]
[0094] Example 4: Preparation of VDF-HFP-DAAM copolymer latex A 2 gallon autoclave was charged with 2650 g of deionized water and 2.9 g of Sartomer® SR604 polypropylene glycol monomethacrylate (PPGMA) surfactant. The autoclave was purged with argon / nitrogen three times (stirring stopped while venting), followed by a low flow argon / nitrogen purge for 15 minutes with a slow stirrer at 15 rpm. The autoclave was sealed, stirred at 72 rpm, heated to 100°C, and pressurized to 650 psi with 220.0 mL of HFP and vinylidene fluoride. A 4.0 wt% potassium persulfate (KPS) and 4.0 wt% sodium acetate (SAT) aqueous feed was started at 240.0 mL / h. Once pressure began to drop, the KPS / SAT feed rates were reduced to 15.0 mL / h and pressure was maintained with additional VDF feed. HFP was fed at 150.0 mL / h to a total of 420.0 mL of HFP. A feed of 5.0 wt % DAAM solution was started at 200.0 mL / h to a total of 1400 mL of VDF. Feeds continued in this manner until a total of 1480 g of VDF had been fed to the reactor. The reaction temperature was maintained at 83° C. for an additional 40 minutes. The pressure was then allowed to spontaneously reduce over 10 minutes, at which point the reactor was vented to atmospheric pressure and cooled to room temperature. 60.0 g of a 30.0 wt % ALS (ammonium lauryl sulfate (surfactant)) solution was added to the reactor with stirring at 30 rpm. The product was discharged from the reactor. The particle size is 125 nm. The solids content is 35%. The melt viscosity is 232° C. at 100 s. -1 The molecular weight is Mn 170,000 g / mol. The melting temperature is 112.5°C. The %HFP by F-NMR is 18.1% by weight.
[0095] This indicates that it is possible to produce a VDF / HFP / DAAM copolymer. The particle size was reduced by adding a surfactant.
[0096] Example 5A: Preparation of p-DAAM Oligomer Latex To a 2 liter reactor was added 800 g of deionized water. The reactor was purged with nitrogen. The reactor was stirred at 160 rpm and heated to 80° C. (atmospheric pressure). 60.0 g of 16.7 wt % ammonium persulfate (APS) aqueous solution was added as a shot to the reactor. A monomer mixture feed (20.0 g DAAM, 2.0 g acrylic acid (AA), 250.0 g deionized water) was started at 272.0 mL / h. After the monomer mixture feed was completed, the reaction temperature was maintained at 80° C. for an additional 30 minutes. The reactor was then cooled to room temperature. Agitation was stopped and the latex product was discharged from the reactor. This p-DAAM latex was used directly for the preparation of PVDF-b-pDAAM block copolymer without further purification. This p-DAAM oligomer had a Mn of 1600 g / mol by GPC using polymethyl methacrylate standards.
[0097] Example 5B: Preparation of PVDF with DAAM functional copolymer A 2 gallon autoclave was charged with 3200 g of deionized water and 300.0 g of 2.5 wt% p-DAAM oligomer latex (from Example 5A). The autoclave was purged with argon / nitrogen three times (stirring stopped while venting), followed by a low flow argon / nitrogen purge for 15 minutes with a slow stirrer at 15 rpm. The autoclave was sealed, stirred at 72 rpm, heated to 100°C, and pressurized to 650 psi with vinylidene fluoride. A 3.0 wt% aqueous potassium persulfate (KPS) feed was started at 100.0 mL / h. Once the pressure began to drop, the KPS feed rate was reduced to 25.0 mL / h and the pressure was maintained by feeding additional VDF. An additional 500.0 g of 2.5 wt% p-DAAM oligomer latex was fed at 350.0 mL / h. Feeds continued in this manner until a total of 1800.0 g VDF had been fed to the reactor. The reaction temperature was maintained at 100° C. for 30 minutes while KPS was fed at 15.0 mL / h. The pressure was then allowed to spontaneously reduce over 10 minutes, at which point the reactor was vented to atmospheric pressure and cooled to room temperature. The product was discharged from the reactor and spray dried. The copolymer has a melt viscosity of 34.9 kP before crosslinking and 48.9 kP after crosslinking by adding ADH in a molar ratio of DAAM / ADH=2 / 1 based on the feed rate to the reactor.
[0098] This indicates that DAAM is incorporated into the PVDF polymer via chain transfer.
[0099] Example 6: Preparation of VDF-DAAM copolymer A 2 gallon autoclave was charged with 3000 g of deionized water and 7.4 g of an aqueous PAA solution (PAA CP-10s, 50 wt% in water). The autoclave was purged with argon / nitrogen three times (stirring stopped during venting), followed by a low-flow argon / nitrogen purge for 15 minutes with a slow stirrer at 15 rpm. The autoclave was sealed, stirred at 72 rpm, heated to 100°C, and pressurized to 650 psi with polyvinylidene fluoride. A 4.0 wt% potassium persulfate (KPS) and 1.0 wt% sodium acetate (SAT) aqueous solution feed was started at 60.0 mL / h. Once pressure began to drop, the KPS / SAT feed rates were reduced to 25.0 mL / h and pressure was maintained with additional VDF feed. A feed of 5.0 wt% DAAM solution was started at 150.0 mL / h to a total of 1700 mL VDF. Feeds continued in this manner until a total of 1800 g VDF was fed to the autoclave. The reaction temperature was reduced to 83°C while feeding KPS at 10.0 mL / h for an additional 30 minutes. The pressure was then allowed to reduce spontaneously for 10 minutes, at which point the reactor was vented to atmospheric pressure and cooled to room temperature. The product was discharged from the reactor and spray dried. ADH can be added before or after spray drying at a molar ratio of DAAM / ADH=2 / 1. The latex particle size is 249 nm by light scattering. The melt viscosity of this copolymer is 8.8 kP alone and 18.6 kP after crosslinking with ADH.
[0100] Example 7: Preparation of VDF-DAAM copolymer A 2 gallon autoclave was charged with 3000 g of deionized water and 3.4 g of aqueous PAA (PAA CP-10s, 50 wt% in water). The autoclave was purged with argon / nitrogen three times (stirring stopped while venting), followed by a low-flow argon / nitrogen purge for 15 minutes with a slow stirrer at 15 rpm. The autoclave was sealed, stirred at 72 rpm, heated to 100 °C, and pressurized to 650 psi with polyvinylidene fluoride. A 3.0 wt% potassium persulfate (KPS) and 1.0 wt% sodium acetate (SAT) aqueous solution feed was started at 60.0 mL / h. Once pressure began to drop, the KPS / SAT feed rates were reduced to 25.0 mL / h and pressure was maintained by additional VDF feeds. A 5.0 wt% DAAM solution feed was started at 150.0 mL / h to feed a total of 1700 mL of VDF. Feeding continued in this manner until a total of 1800 g VDF had been fed to the autoclave. The reaction temperature was reduced to 83° C. for an additional 30 min while feeding KPS at 10.0 mL / h. The pressure was then allowed to reduce spontaneously over 10 min, at which point the reactor was vented to atmospheric pressure and cooled to room temperature. The product was discharged from the reactor and spray dried. ADH can be added before or after spray drying at a molar ratio of DAAM / ADH=2 / 1. The latex particle size is 233 nm by light scattering. The melt viscosity of this copolymer is 27.8 kP alone and 47.5 kP after crosslinking with ADH.
[0101] Measurement of the amount of DAAM incorporated into fluoropolymers: The incorporation of DAAM into PVDF was confirmed by NMR, with 13% of the total DAAM feed being copolymerized with PVDF.
[0102] [Table 2]
[0103] Example 8: Preparation of VDF-DAAM copolymer This sample was prepared similarly to Example 1. The resulting copolymer latex was spray dried without the addition of ADH. The melt viscosity of the dried copolymer was 20.1 kP.
[0104] Example 9: Preparation of VDF-DAAM copolymer This sample was prepared in the same manner as in Example 1. The resulting copolymer latex was spray-dried with ADH (molar ratio of DAAM / ADH=2 / 1). The melt viscosity of the dried copolymer was 43.1 kP.
[0105] Effect of crosslinking on tensile strength The tensile strength of the VDF-DAAM copolymer was measured with and without the addition of ADH. Example 8 was spray dried without the addition of ADH, and the copolymer was not crosslinked. For Example 9, ADH was added to the copolymer latex and then spray dried. Example 9 was crosslinked in this manner. The tensile properties of these two samples were tested.
[0106] [Table 3]
[0107] The yield stress, yield strain, and Young's modulus were similar for the two copolymers.
[0108] The toughness of the crosslinked copolymer (Example 9) is significantly (45%) higher than the uncrosslinked copolymer (Example 8) since Example 9 breaks at a much longer strain.
[0109] The curve is shown in FIG.
Claims
1. A composition comprising a fluorinated copolymer, the fluorinated copolymer comprising fluoro-monomer units and keto-functional monomer units incorporated as part of the polymer.
2. The composition of claim 1 , wherein the copolymer comprises at least 95% by weight of fluorine-containing monomer units.
3. The composition according to claim 1 or 2, wherein the fluorine monomer comprises VDF.
4. The composition according to claim 1 or 2, wherein the fluorine monomer comprises HFP.
5. The composition of claim 1 or 2, wherein the keto-functional monomer comprises DAAM.
6. 3. The composition of claim 1 or 2, wherein the keto-functional monomer comprises AAEM.
7. 3. The composition according to claim 1 or 2, wherein the fluorinated copolymer has a melt viscosity greater than 5 kP, preferably greater than 7 kP.
8. The composition of claim 1 or 2, further comprising a crosslinking agent.
9. The composition of claim 8 , wherein the crosslinker comprises AHD.
10. The composition of claim 8 , wherein the crosslinker comprises hexamethylenediamine.
11. The fluorinated copolymer has a viscosity of 500,000 lb / in before crosslinking. 3 (3,450,000kN・m / m 3 2. The composition of claim 1, having a toughness greater than 100%.
12. 8. The composition of claim 7, wherein the fluorinated copolymer is crosslinked and exhibits an increase in toughness of at least 25%, preferably at least 30%, more preferably at least 35% compared to a non-crosslinked fluorinated copolymer.
13. The fluorinated copolymer is crosslinked and has a crosslinking capacity of 900,000 lb / in 3 (6,200,000kN・m / m 3 8. The composition of claim 7, wherein the composition exhibits a toughness greater than 100%.
14. 1. A method for crosslinking a fluoropolymer, comprising: providing a fluorinated copolymer comprising keto-functional monomer units; blending said fluorinated copolymer with a crosslinking agent; and melt processing the blend of said fluorinated copolymer and said crosslinking agent.
15. 1. A method for crosslinking a fluoropolymer, comprising providing a fluorinated copolymer comprising keto-functional monomer units in the form of a latex, blending a crosslinking agent into the latex comprising the fluorinated copolymer, and then drying the latex.
16. 16. The method of claim 14 or 15, wherein the fluoropolymer comprises vinylidene fluoride monomer units.
17. 16. The method of claim 14 or 15, wherein the fluoropolymer comprises DAAM monomer units.
18. 16. The method of claim 14 or 15, wherein the cross-linking agent comprises a dihydrazide or a diamine, preferably AHD.
19. The method of claim 14 or 15, wherein the cross-linking agent comprises AHD.
20. 16. The method of claim 14 or 15, wherein the cross-linking agent comprises hexamethylenediamine.
Citation Information
Patent Citations
Nonspherical particle preparation method based on change of hydrophilicities and crosslinking degrees of seeds
CN104292378A
Aqueous curable resin composition and coated material
JP2000344986A
Fluorine-containing aqueous dispersed composition
JP2005162994A
Novel oil-and water-repellent composition of polymers of fluoroalkyl monomers and diacetone acrylamide or diacetone methacrylamide
US3838104A
Porous film of vinylidene fluoride resin and method for producing same
WO2004092257A1