The continuous graphitization process optimizes pore structure and density ratios in artificial graphite, enhancing lithium ion diffusion and electrochemical reactions to improve the performance and reduce costs of negative electrode materials in lithium-ion batteries.

JP2024545485AActive Publication Date: 2024-12-09KAIFENG RUIFENG NEW MATERIAL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024508534
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2022-11-16
Publication Date
2024-12-09
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

Conventional graphitization processes for negative electrode materials in lithium-ion batteries are batch-type operations that require power outages, have slow temperature rise and fall rates, leading to long production cycles and poor control over pore structure, which affects the diffusion and electrochemical performance of graphite materials.

Method used

A continuous graphitization process is employed to control the internal and surface pore volume, specific surface area, and true density of artificial graphite within specific ratios (4.0≦V×S/D≦10) to enhance lithium ion diffusion and electrochemical reaction interfaces, using additives to form pores and control temperature rates for efficient production.

Benefits of technology

The process results in improved lithium storage capacity and rate characteristics of the negative electrode material, reducing energy consumption and production costs while maintaining high performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024545485000001_ABST
    Figure 2024545485000001_ABST
Patent Text Reader

Abstract

The present application provides a negative electrode material and a battery. The negative electrode material includes artificial graphite particles, the artificial graphite particles having pores inside and / or on the surface thereof, and a pore volume of the negative electrode material is V cm 3 / kg, and true density is D g / cm 3 , the specific surface area is S m 2 / g, 4.0≦V×S / D≦10. The negative electrode material and the battery provided by the present application can efficiently increase the active sites on the surface of the negative electrode material, and improve the rate characteristics of the negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application relates to the technical field of anode materials, and more particularly to anode materials and batteries. [Background technology]

[0002] Graphite has the advantages of high electrical conductivity, a large lithium ion diffusion coefficient, a small volume change before and after lithium absorption in its layered structure, a high lithium absorption capacity, and a low lithium absorption potential, making it the currently mainstream negative electrode material for commercial lithium ion batteries.

[0003] Conventional graphitization equipment for graphite anodes mainly includes two types: crucible furnace and box furnace. Both of them are batch-type operations, and the graphitization process requires power outages, so continuous production cannot be realized. In addition, the heating and cooling process of the equipment is particularly limited, and the heating and cooling speed is slow, so the production cycle is long. Generally, the graphitization cycle is within 15 to 50 days. In the graphitization production process, volatile components, impurity elements, etc. in the raw materials escape under high temperature conditions, so that voids are formed inside and / or on the surface of the graphite. Generally, all artificial graphite has a certain number of pore structures, and the presence of pores can increase the diffusion channels of Li+ inside the graphite material and reduce the diffusion resistance of Li+, thereby effectively improving the rate characteristics of the material, while too many pore structures will increase the specific surface area of ​​the material, which will further deteriorate the initial efficiency and cycle performance of the product. In fact, simply improving the pore structure alone cannot achieve optimal rate characteristics, and there is still a lot of room for improvement. Researchers have only studied the effect of a single element on the performance of graphite materials, but have not explored the synergistic effects between multiple elements to maximize the improvement of graphite's rate properties.

[0004] Therefore, at the current mature stage of graphite material development, improving a single parameter cannot meet the market demand for low-cost, high-performance graphite materials. It is necessary to study the synergistic action mechanism of various factors and develop graphite anode materials that meet the market demand. Summary of the Invention [Problem to be solved by the invention]

[0005] In view of the above, the present application provides a new negative electrode material and a battery that address the shortcomings of the prior art by achieving precise adjustment control of the internal and / or surface pore volume, the specific surface area, and the true density, and by combining and maintaining them within a reasonable range, thereby improving the capacity and rate characteristics of the negative electrode material. [Means for solving the problem]

[0006] In a first aspect, the present application provides an anode material, the anode material comprising artificial graphite, the artificial graphite having pores, and a pore volume of the anode material is defined as V cm 3 / kg, and true density is D g / cm 3 , the specific surface area is S m 2 / g, the negative electrode material satisfies 4.0≦V×S / D≦10. The pore volume was measured using an ASAP 2460 device manufactured by Micromeritics, Inc., USA, and calculated within the pore diameter range of 17 Å to 3000 Å using the BJH Desorption cumulative volume of pores model.

[0007] In some embodiments, the particle size D of the negative electrode material 50 is 10 μm to 30 μm.

[0008] In some embodiments, the particle size D of the negative electrode material 10 ≧5 μm.

[0009] In some embodiments, the particle size D of the negative electrode material 90 ≦50 μm.

[0010] In some embodiments, the pore volume of the negative electrode material is defined as V cm 3 / kg, V is 5≦V≦8.

[0011] In some embodiments, the specific surface area of ​​the negative electrode material is S m 2 / g, 1.78≦S≦3.0.

[0012] In some embodiments, the true density of the negative electrode material is D g / cm 3 When set to , 2.210≦D≦2.265.

[0013] In some embodiments, the pores include at least one of micropores and mesopores.

[0014] In some embodiments, the pores have an average pore diameter of 50 Å to 200 Å.

[0015] In some embodiments, the negative electrode material is subjected to X-ray diffraction measurement to determine that the interlayer distance of the (002) crystal plane is d 002 When the 002 ≦3.365 Å.

[0016] In some embodiments, the peak intensity ratio I of the (002) plane to the (110) plane of the artificial graphite particles is determined by X-ray diffraction measurement. 002 / I 110 is 65.0 to 120.0, and the peak intensity ratio I 004 / I 110 is 3.0~6.0.

[0017] In some embodiments, the synthetic graphite comprises synthetic graphite primary particles and / or synthetic graphite secondary particles.

[0018] In some embodiments, the negative electrode material further comprises amorphous carbon.

[0019] In some embodiments, the negative electrode material further includes amorphous carbon, and a mass percentage of the amorphous carbon in the negative electrode material is 0.1 wt % to 5 wt %.

[0020] According to a second aspect, the present application provides a battery comprising the anode material according to the first aspect. Effect of the Invention

[0021] The technical means of the present application have at least the following beneficial effects: The negative electrode material provided by the present application includes artificial graphite, has pores inside and / or on the surface of the artificial graphite, and has a pore volume of V cm 3 / kg, and true density is D g / cm 3 , the specific surface area is S m 2 / g, 4.0≦V×S / D≦10. Generally, the pore volume within a certain range in artificial graphite can increase the diffusion channel of Li ions, and the specific surface area within a certain range can ensure sufficient electrochemical reaction interface, promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce concentration polarization, and are favorable for improving the capacity and rate characteristics of the negative electrode material. The applicant has conducted extensive research based on this and found that after lithium ions diffuse onto the surface of the artificial graphite, if the order of carbon atoms in the artificial graphite is relatively disordered and the degree of ordering is insufficient, the lithium ions are relatively inhibited from entering the interior of the artificial graphite material and combining with the carbon atoms to generate an electrochemical reaction, and the diffusion channel and the area of ​​the electrochemical reaction are not fully utilized, and the order and true density of the artificial graphite are directly related, so that only the area of ​​the lithium ion diffusion channel and the area of ​​the electrochemical reaction are sufficient, and the rate characteristics still have room for significant improvement. In the present application, by controlling the V×S / D of the negative electrode material within the above range, it is advantageous to bond lithium ions with sufficient carbon atoms with low resistance, thereby obtaining a negative electrode material with superior rate characteristics and capacity.

[0022] The negative electrode material provided in the present application is produced and processed by a continuous graphitization process, in which all materials are continuously charged and discharged, and the time and temperature of passing through the high temperature area are matched, and the graphitization process controls the temperature rise and fall rate, so that the volatile components, impurity elements and other substances in the material can be uniformly and quickly released, while controlling the press molding dimensions and introducing a certain amount of additives to realize accurate control of the graphite internal and / or surface pore volume. The synergistic use of the above process methods overcomes the problems of uneven heating of materials due to the temperature gradient at different positions in the graphitization furnace, and the large fluctuations and uncontrollable indexes of the specific surface area, pore volume, true density and other indexes of the produced and processed products, so that the pore volume, specific surface area and true density of the processed material reach the ideal adjustment and control design requirements.

[0023] The negative electrode material provided in the present application uses a continuous graphitization process, so that the energy consumption per unit mass is low, and it has obvious advantages in cost and production cycle, and is environmentally friendly. [Brief description of the drawings]

[0024] [Figure 1] 1 is a scanning electron microscope photograph of the negative electrode material prepared in Example 12 of the present application. [Diagram 2] 1 is a pore size distribution curve of the negative electrode material prepared in Example 12 of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] In order to better explain the present application and facilitate understanding of the technical solution of the present application, the present application is described in more detail below. It should be noted that the following examples are merely simplified examples of the present application, which do not indicate or limit the protection scope of the present application.

[0026] In the field of anode materials, the development of continuous graphitization apparatus has continued for decades, and as early as 1987, a patent (US06619591) disclosed an apparatus capable of performing continuous graphitization treatment on carbon-containing materials. In recent years, applicants have also continued to develop continuous graphitization apparatus, for example, a patent with registration publication number CN211425033U filed in 2019 discloses a vertical continuous kiln for producing anode materials for lithium batteries, which can continuously discharge materials from an outlet and continuously charge materials from a material pipe. Compared with conventional processes, the continuous graphitization process shortens the graphitization time from several days to several hours, and the reduction in energy consumption is quite significant, but the significant reduction in graphitization time results in changes in the microstructure of artificial graphite, especially changes in the pore structure and crystal form inside the artificial graphite, compared with conventional artificial graphite. It has been proven in the industry that such changes make it difficult to meet the required performance of artificial graphite and difficult to improve, so even though continuous graphitization equipment has been in existence for 30 to 40 years, there is no precedent for successful mass production of continuously graphitized artificial graphite anode products.

[0027] In recent years, with the increasing energy scarcity, in order to further reduce the cost of artificial graphite, the applicant continues to develop the application of continuous graphitization equipment, develops an artificial graphite anode material with performance equivalent to or even better than the current normal graphitized anode material, and aims to reduce the energy consumption of the artificial graphite anode material and further reduce the cost. The applicant has developed various means to improve the rapid temperature rise and fall that brings unfavorable changes to artificial graphite products through the development of a large number of preparation processes, and obtains a series of different types of artificial graphite anode materials through product selection. Although these artificial graphite anode materials have different microstructures from normal artificial graphite products, their electrical performances can all be basically equivalent to normal artificial graphite products, and in some respects, the electrical performance and processing performance are better or more stable, and they have the conditions to replace normal artificial graphite products.

[0028] The manufacturing process and related products will be described in more detail below using a manufacturing process developed by the applicant as an example.

[0029] The method for producing the negative electrode material is as follows: S10: A step of press-molding a mixture containing coke powder, a binder, an additive and a solvent to obtain a first precursor, where the additive contains an inorganic compound, the mass ratio of the coke powder to the additive is 100:(1-5), and the press size is φ(10mm-100mm)×(20mm-100mm); S20: Pre-carbonizing the first precursor to obtain a second precursor; S30: The second precursor is placed in a continuous graphitization furnace, and the temperature is increased to 2800°C to 3200°C at a heating rate of 13°C / min to 20°C / min to perform graphitization treatment for 1 to 4 hours, and then the temperature is decreased at a heating rate of 20°C / min to 25°C / min to obtain a negative electrode material, and the step includes controlling the ratio of the heating rate and the heating rate to 0.5 to 1.

[0030] The method for producing the negative electrode material provided by the present application is to press a mixture of coke powder, binder, additives and solvent, pre-carbonize the first precursor, and then place it in a continuous graphitization furnace, so that the heating rate is extremely fast, and after the rapid heating, the second precursor can reach the graphitization temperature in a relatively short time, and the additives are volatilized and released, forming pores in and / or on the surface of the graphite particles, which can serve as additional lithium storage space, improving the lithium storage capacity of the graphite material. In addition, the process of loading and unloading the material in the continuous graphitization furnace is completed within only a few hours, which has a high thermal energy utilization rate and reduces production costs.

[0031] The coke powder is obtained by pulverizing and shaping a coke raw material, the coke raw material including at least one of petroleum coke, needle coke, pitch coke, and isotropic coke.

[0032] In some embodiments, the shaping includes at least one of crushing, spheronization, or classification. The median diameter of the shaped coke powder is 15 μm to 20 μm, and more specifically, may be 15 μm, 15.5 μm, 16 μm, 16.5 μm, 17 μm, 17.5 μm, 18 μm, 18.5 μm, 19 μm, or 20 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable. Controlling the median diameter of the coke powder within the above range through multiple tests is advantageous in terms of achieving both processing performance, capacity, and rate characteristics.

[0033] In some embodiments, the mass content of carbon in the coke powder is 80% or more, and may be specifically 80%, 81%, 82%, 85%, 90%, 95%, or 96%, but is not limited to the recited values, and other unrecited values ​​within the numerical range also apply.

[0034] In some embodiments, the solvent comprises at least one of water, ethanol, acetone, benzene, toluene, quinoline, tetrahydrofuran, and carbon tetrachloride.

[0035] In some embodiments, the binder comprises at least one of petroleum resin, phenolic resin, epoxy resin, coumarone resin, potato starch, wheat starch, corn starch, sweet potato starch, arrowroot starch, and tapioca flour.

[0036] In some embodiments, the additive comprises at least one of boron oxide, boron carbide, boron nitride, silicon carbide, boron nitride, boric acid, boron chloride, and sodium borate, and the additive acts as a graphitization catalyst while being volatilized and released by rapid temperature increase and decrease during the graphitization process, which is advantageous in forming stable pores inside and / or on the surface of the artificial graphite.

[0037] In some embodiments, the mass ratio of coke powder, binder, solvent, and additive is 100:(3-20):(5-50):(1-5), specifically, it may be 100:3:5:1, 100:10:15:1, 100:15:20:5, 100:20:20:1, 100:20:15:3, 100:10:10:5, or 100:15:25:2, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable. Controlling the content of the additive within the above range is favorable for the occurrence of the catalytic graphitization process, while the additive can volatilize at high temperature to form a certain number of pores inside and / or on the surface of the graphite.

[0038] As can be seen, in the examples, when the binder ratio is low (the mass ratio of binder to coke powder is 3 to 10:100), the obtained artificial graphite is mainly composed of primary particles, and in the examples, when the binder ratio is high (the mass ratio of binder to coke powder is 10 to 20:100), the obtained artificial graphite is mainly composed of secondary particles.

[0039] In some embodiments, the mixing method of the mixture includes at least one of mechanical stirring and ultrasonic dispersion.When mechanical stirring is used for mixing, a propeller type stirrer, a turbine type stirrer, a flat blade type stirrer, etc. can be used as long as each component in the mixture is sufficiently mixed uniformly.

[0040] In some embodiments, the stirring speed is 10 r / min to 1000 r / min, specifically, 10 r / min, 50 r / min, 70 r / min, 100 r / min, 120 r / min, 150 r / min, 200 r / min, 300 r / min, 350 r / min, 400 r / min, 500 r / min, or 1000 r / min, etc., but is not limited thereto. Controlling the stirring speed within the above range is advantageous for mixing each component to form a uniform mixture.

[0041] The stirring may be performed at room temperature or in a preheated state. Preferably, the stirring temperature may be controlled to 25°C to 200°C. As can be understood, proper preheating is advantageous for mixing each component to form a uniform mixture.

[0042] In some embodiments, the pressing method includes at least one of extrusion, die pressing, roll pressing, and isostatic pressing.

[0043] In some embodiments, the pressure of the press molding is 5 MPa to 100 MPa, specifically, 5 MPa, 15 MPa, 25 MPa, 30 MPa, 35 MPa, 40 MPa, 45 MPa, 50 MPa, 55 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa, or 100 MPa, etc., and the press molding process can improve the fluidity of the material in the graphitization process while increasing the furnace loading amount and production capacity of the material.

[0044] Controlling the press molding dimensions to φ(10 mm to 100 mm) × (20 mm to 100 mm) during press molding and controlling the press molding dimensions within the above range is advantageous for controlling the specific surface area and is also advantageous for charging and discharging in the graphitization process.

[0045] In some embodiments, the reaction temperature of the pre-carbonization treatment is 500° C. to 1000° C., and may be specifically 500° C., 550° C., 600° C., 700° C., 750° C., 800° C., 850° C., 900° C., or 1000° C., but is not limited to the recited values, and other unrecited values ​​within the range apply as well. As can be understood, a pre-carbonization treatment temperature within the above range is advantageous for discharging substances such as volatile components in the coke raw material.

[0046] In some embodiments, the pre-carbonization treatment is performed for a period of 1 to 10 hours, and may be, for example, 1, 2, 3, 4, 5, 6, 7, 8, or 10 hours, but is not limited to the listed values, and other values ​​not listed within the range are also applicable. Preferably, the pre-carbonization treatment is performed for a period of 1 to 4 hours.

[0047] In some embodiments, the heating rate of the pre-carbonization treatment is 5°C / min to 20°C / min, and specifically may be 5°C / min, 6°C / min, 8°C / min, 10°C / min, 15°C / min, 15.5°C / min, or 20°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range also apply.

[0048] In some embodiments, the temperature drop rate after the pre-carbonization treatment is 10°C / min to 30°C / min, and specifically may be 10°C / min, 15°C / min, 20°C / min, 25°C / min, 25.5°C / min, or 30°C / min, but is not limited to the listed numerical values, and other unlisted numerical values ​​within the numerical range also apply.

[0049] In some embodiments, the pre-carbonization process is carried out in a protective atmosphere that includes at least one of nitrogen gas, helium gas, neon gas, argon gas, krypton gas, and xenon gas.

[0050] In some embodiments, the heating rate for the graphitization treatment may be 13° C. / min, 15° C. / min, 17° C. / min, 18° C. / min, or 20° C. / min, etc., and the heating rate after the graphitization treatment may be 20° C. / min, 21° C. / min, 22° C. / min, 23° C. / min, 24° C. / min, or 25° C. / min, etc.

[0051] In some embodiments, the structure of the continuous graphitization furnace is shown in patent CN211425033U.

[0052] In some embodiments, the graphitization process includes increasing the temperature to 2800° C.-3200° C. at a rate of 13° C. / min-20° C. / min, and maintaining the temperature at 2800° C.-3200° C. for 2 h-4 h. As can be seen, the rapid temperature increase in the graphitization process is favorable for the rapid escape of volatile components inside the coke raw material and for the formation of pores in the product.

[0053] In some embodiments, the graphitization temperature may be, for example, 2800° C., 2850° C., 2900° C., 3000° C., 3100° C., 3150° C., 3180° C., or 3200° C., but is not limited to the recited values, and other unrecited values ​​within the range apply as well.

[0054] In some embodiments, the graphitization treatment is performed for a period of 1 h to 4 h, and may be, for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 3.8 h, or 4 h, but is not limited to the listed values, and other values ​​not listed within the range apply as well. Preferably, the graphitization treatment is performed for a period of 2 h to 3 h.

[0055] In some embodiments, the cooling rate after graphitization is 20° C. / min to 25° C. / min, and may be, specifically, 20° C. / min, 21° C. / min, 22° C. / min, 23° C. / min, 24° C. / min, or 25° C. / min, but is not limited to the listed values, and other values ​​not listed within the range of values ​​also apply. Rapid cooling can reduce the occurrence of material oxidation reactions during the cooling process and is advantageous for controlling the specific surface area of ​​the material, while significantly shortening the graphitization processing cycle and reducing production costs.

[0056] In some embodiments, the ratio of the heating rate to the cooling rate during the graphitization process may be 0.5, 0.6, 0.7, 0.8, 0.9, or 1.0. Controlling the ratio of the heating rate to the cooling rate is advantageous for allowing volatile substances inside the material to escape, and maintains the product of the pore volume and the specific surface area of ​​the material at a relatively constant value.

[0057] As can be seen, after the adhesive is graphitized, a portion of it is difficult to convert into graphitized carbon, and the portion that cannot be converted into graphitized carbon exists on the surface of the artificial graphite particles in the form of amorphous carbon.

[0058] In some embodiments, the graphitization process is followed by at least one of crushing, sieving, and degaussing. Preferably, the carbonization process is followed by crushing, degaussing, and sieving, in that order.

[0059] In some embodiments, the grinding means may be any one of a mechanical grinder, an airflow grinder, and a cryogenic grinder.

[0060] In some embodiments, the sieving method is any one of a fixed sieve, a drum screen, a resonating sieve, a roller sieve, a vibrating sieve, and a chain grizzly, and the mesh number of the sieving is 100 to 500 mesh, specifically, the mesh number of the sieving may be 100 mesh, 200 mesh, 250 mesh, 325 mesh, 400 mesh, 500 mesh, etc., and controlling the particle size of the negative electrode material within the above range contributes to improving the processing characteristics of the negative electrode material.

[0061] In some embodiments, the demagnetizing device is one of a permanent magnet drum type magnetic separator, an electromagnetic iron remover, and a pulsating high gradient magnetic separator, and the demagnetizing is ultimately for controlling the content of magnetic materials in the negative electrode material, for avoiding the discharging effect of magnetic materials on the battery, and for ensuring the safety of the battery during use.

[0062] A negative electrode material containing artificial graphite, having pores inside and / or on the surface of the artificial graphite, and a pore volume of the negative electrode material is V cm 3 / kg, and true density is D g / cm 3 , the specific surface area is S m 2 / g, V×S / D is 4.0≦V×S / D≦10. The pore volume was measured using an ASAP 2460 device manufactured by Micromeritics, Inc., USA, and calculated using the BJH Desorption cumulative volume of pores model within the pore diameter range of 17 Å to 3000 Å.

[0063] The anode material provided in the present application is manufactured and processed by a continuous graphitization process, and the time and temperature of all materials passing through the high temperature region are matched, and the temperature rise and fall rate is controlled, so that the volatile components, impurity elements and other substances in the material can be uniformly and quickly released. At the same time, the introduction of a certain amount of additives realizes precise control of the pores in the graphite interior and / or surface, and the pore volume, specific surface area and true density of the material reach the ideal adjustment and control design requirements. Pores are formed in the graphite interior and / or surface, and the pores can be used as additional lithium storage space, improving the lithium storage capacity of the anode material and causing an increase in the specific surface area. When the anode material is manufactured as an electrode and applied to a battery, after injecting the electrolyte, the pores in the artificial graphite particles are filled with the electrolyte, and during charging and discharging, an electrochemical reaction occurs inside the electrode, and the pores create more lithium ion diffusion channels and electrochemical reaction interfaces in the anode material, promoting the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reducing the concentration polarization, and favoring the improvement of the capacity and rate characteristics of the anode material.

[0064] Generally, the pore volume within a certain range in the artificial graphite can increase the diffusion channel of Li ions, and the specific surface area within a certain range can ensure sufficient electrochemical reaction interface, promote the diffusion of lithium ions at the solid-liquid interface and in the solid phase, reduce concentration polarization, and are favorable for improving the capacity and rate characteristics of the negative electrode material. The applicant has conducted extensive research based on this and found that after lithium ions diffuse onto the surface of the artificial graphite, if the order of carbon atoms in the artificial graphite is relatively disordered and the degree of ordering is insufficient, the lithium ions are relatively inhibited from entering the interior of the artificial graphite material and combining with the carbon atoms to generate an electrochemical reaction, and the diffusion channel and the area of ​​the electrochemical reaction are not fully utilized, and since the degree of ordering and the true density of the artificial graphite are directly related, even if only the area of ​​the lithium ion diffusion channel and the area of ​​the electrochemical reaction are sufficient, the rate characteristics still have room for significant improvement. The present application controls the V×S / D of the negative electrode material within the above range, which is favorable for combining lithium ions with sufficient carbon atoms with low resistance, and obtains a negative electrode material with better rate characteristics and capacity.

[0065] In some embodiments, the particle size D of the negative electrode material 50 is 10 μm to 30 μm. Specifically, it may be 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 20 μm, 25 μm, 30 μm, etc., and is not limited thereto. When the median diameter of the negative electrode material is controlled within the above range, it is advantageous for improving the cycle performance of the negative electrode material.

[0066] In addition, D 10 represents the particle size when the percentage of the cumulative particle size distribution of the powder reaches 10%, and D 50 represents the particle size corresponding to the cumulative particle size distribution percentage reaching 50%, and D 90 represents the particle size corresponding to when the cumulative particle size distribution percentage reaches 90%.

[0067] In some embodiments, the particle size D of the negative electrode material 10 ≧5 μm, specifically, it may be 5 μm, 5.5 μm, 6 μm, 7 μm, 8 μm, 10 μm, etc., and is not limited thereto.

[0068] In some embodiments, the particle size D of the negative electrode material 90 ≦50 μm, specifically, it may be 50 μm, 49 μm, 48 μm, 47 μm, 46 μm, 45 μm, 42 μm, 40 μm, etc., and is not limited thereto.

[0069] In some embodiments, the pore volume of the negative electrode material is defined as V cm 3 / kg, V is 5≦V≦8, and specifically, it may be 5, 5.2, 5.5, 5.8, 6.0, 6.2, 6.5, 6.8, 7.0, 7.5, or 8.0, etc., but is not limited thereto.

[0070] In some embodiments, the specific surface area of ​​the negative electrode material is defined as S m 2 / g, 1.78≦S≦3.0, specifically, 1.78, 1.85, 1.95, 2.00, 2.25, 2.43, 2.57, 2.61, 2.72, 2.85, 3.0, etc., but not limited thereto. As can be understood, if the specific surface area is too large, it is easy to cause the formation of a solid electrolyte membrane, and the irreversible lithium salt is excessively consumed, which reduces the initial efficiency of the battery.

[0071] In some embodiments, the true density of the negative electrode material is defined as D g / cm 3 When set to , 2.210≦D≦2.265 holds. Specifically, D may be 2.210, 2.215, 2.218, 2.220, 2.252, 2.263, 2.260, or 2.265, and is not limited thereto.

[0072] In some embodiments, the pores comprise at least one of micropores and mesopores.

[0073] In some embodiments, the average pore diameter of the pores is between 50 Å and 200 Å. Specifically, the average pore diameter of the pores may be 50 Å, 51 Å, 52 Å, 52.5 Å, 53.8 Å, 56.7 Å, 60 Å, 70 Å, 100 Å, 150 Å, or 200 Å, etc.

[0074] In some embodiments, the negative electrode material is subjected to X-ray diffraction measurement to determine that the interlayer distance of the (002) crystal plane is d 002 When the 002 ≦3.365 Å. The interlayer distance d 002 Since the graphite crystallinity of the artificial graphite particles is high, that is, the degree of graphitization is high, and the capacity of the product is high.

[0075] In some embodiments, the peak intensity ratio I of the (002) plane to the (110) plane of the artificial graphite particles is measured by X-ray diffraction testing. 002 / I 110 is 65.0 to 120.0, and the peak intensity ratio I 004 / I 110 is 3.0 to 6.0. 002 / I 110 and I 004 / I 110 If I is in this range, the material has a relatively high degree of orientation and low cycle expansion. 002 / I 110 Specifically, the ratio may be 65.0, 70.0, 75.0, 80.0, 85.3, 89.2, 90.5, 95.1, 100.0, 111.0, or 120.0, and is not limited thereto. 004 / I 110 Specifically, the ratio may be 3.0, 3.2, 3.5, 3.8, 4.1, 4.2, 4.5, 5.2, 5.8, 5.9, or 6.0, etc., and is not limited thereto.

[0076] In some embodiments, the synthetic graphite comprises synthetic graphite primary particles and / or synthetic graphite secondary particles.

[0077] In some embodiments, the negative electrode material further comprises amorphous carbon, and the mass ratio of the amorphous carbon in the negative electrode material is 0.1 wt% to 5 wt%. The presence of amorphous carbon provides more irregular and more open diffusion paths for lithium ions, which is favorable for improving the rate characteristics of the material.

[0078] In some embodiments, the specific capacity of the negative electrode material is 320mAh / g to 370mAh / g, and specifically may be 320mAh / g, 340mAh / g, 342mAh / g, 345mAh / g, 353mAh / g, 355mAh / g, 357mAh / g, 360mAh / g, 365mAh / g, or 370mAh / g, etc., but is not limited thereto. Preferably, the specific capacity of the negative electrode material is 340mAh / g to 370mAh / g.

[0079] A battery comprising the above negative electrode material.

[0080] As will be apparent to those skilled in the art, the battery manufacturing method described above is merely an example, and other methods commonly used in the art may be adopted without departing from the scope of the present disclosure, and other types of batteries, such as sodium ion batteries, potassium ion batteries, etc., may be manufactured and measured. EXAMPLES

[0081] The embodiments of the present application will be further described below through a number of examples. However, the embodiments of the present application are not limited to the following specific examples. Appropriate modifications can be made within the scope of protection.

[0082] Example 1 The method for producing the negative electrode material of this embodiment is as follows: (1) crushing raw coke raw material of Daqing petroleum coke, and shaping it by a shaping device to obtain crushed and shaped coke powder, and controlling the median diameter to 15 μm; (2) uniformly mixing coke powder, phenolic resin binder, water, and boron oxide in a mass ratio of 100:6:15:2 to obtain a mixture; (3) press-molding the mixture at a pressure of 10 MPa to obtain a first precursor, and the size of the first precursor after press-molding is φ30 mm × 50 mm; (4) pre-carbonizing the first precursor at a temperature of 800° C. for 4 hours and then cooling to obtain a modified second precursor; (5) The second precursor was graphitized at 2900°C in a continuous graphitization furnace to obtain a graphitized product. The temperature rise curve was as follows: the temperature was raised to 2900°C at a temperature rise rate of 15.5°C / min, the temperature was kept at 2900°C for 2.5 hours, and after the temperature hold, the temperature was cooled to 30°C at a temperature drop rate of 22.5°C / min, and the rate ratio of the temperature rise and fall during the graphitization process was controlled to 0.68. (6) The graphitized product is dispersed, demagnetized, and sieved through a 325 mesh sieve to obtain a negative electrode material.

[0083] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0084] Example 2 The method for producing the negative electrode material of this embodiment is as follows: (1) crushing raw coke material of Baosteel pitch coke and shaping it with a shaping device to obtain crushed and shaped coke powder, and controlling the median diameter to 16 μm; (2) uniformly mixing coke powder, petroleum resin, benzene, and boron carbide in a mass ratio of 100:5:20:2 to obtain a mixture; (3) press-molding the mixture at a pressure of 10 MPa to obtain a first precursor, and the size of the first precursor after press-molding is φ30 mm × 50 mm; (4) pre-carbonizing the first precursor at a temperature of 800° C. for 4 hours and then cooling to obtain a modified second precursor; (5) The second precursor was graphitized at 2900°C in a continuous graphitization furnace to obtain a graphitized product. The temperature rise curve was as follows: the temperature was raised to 2900°C at a temperature rise rate of 14°C / min, the temperature was kept at 2900°C for 2.5 hours, and after the temperature hold, the temperature was cooled to 30°C at a temperature drop rate of 22.5°C / min, and the rate ratio of the temperature rise and fall during the graphitization process was controlled to 0.62. (6) The graphitized product is dispersed, demagnetized, and sieved through a 250 mesh sieve to obtain a negative electrode material.

[0085] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0086] Example 3 The method for producing the negative electrode material of this embodiment is as follows: (1) crushing the mature coke raw material of Jinzhou needle coke and shaping it by a shaping device to obtain crushed and shaped coke powder, and controlling the median diameter to 15 μm; (2) uniformly mixing coke powder, phenolic resin binder, water, and boron oxide in a mass ratio of 100:6:15:2 to obtain a mixture; (3) press-molding the mixture at a pressure of 10 MPa to obtain a first precursor, and the size of the first precursor after press-molding is φ30 mm × 50 mm; (4) pre-carbonizing the first precursor at a temperature of 800° C. for 4 hours and then cooling to obtain a modified second precursor; (5) The second precursor was graphitized at 2850°C in a continuous graphitization furnace to obtain a graphitized product. The temperature rise curve was as follows: the temperature was raised to 2850°C at a temperature rise rate of 16°C / min, the temperature was kept at 2850°C for 2.5 hours, and after the temperature hold, the temperature was cooled to 30°C at a temperature drop rate of 22°C / min, and the rate ratio of the temperature rise and fall during the graphitization process was controlled to 0.73. (6) The graphitized product is dispersed, demagnetized, and sieved through a 250 mesh sieve to obtain a negative electrode material.

[0087] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0088] Example 4 The method for producing the negative electrode material of this embodiment is as follows: (1) crushing raw coke raw material of Kyoyo Needle Coke and shaping it with a shaping device to obtain crushed and shaped coke powder, and controlling the median diameter to 18 μm; (2) homogeneously mixing coke powder, petroleum resin, benzene, and sodium borate in a mass ratio of 100:6:15:2 to obtain a mixture; (3) press-molding the mixture at a pressure of 10 MPa to obtain a first precursor, and the size of the first precursor after press-molding is φ30 mm × 50 mm; (4) pre-carbonizing the precursor at a temperature of 800° C. for 4 h and then cooling to obtain a modified second precursor; (5) The second precursor was graphitized at 2850°C in a continuous graphitization furnace to obtain a graphitized product. The temperature rise curve was as follows: the temperature was raised to 2850°C at a heating rate of 16.5°C / min, the temperature was kept at 2850°C for 3 hours, and after the temperature was kept, the temperature was lowered to 30°C at a heating rate of 22°C / min, and the rate ratio of the temperature rise and fall during the graphitization process was controlled to 0.75. (6) The graphitized product is dispersed, demagnetized, and sieved through a 250 mesh sieve to obtain a negative electrode material.

[0089] The negative electrode material includes primary particle artificial graphite and secondary particle artificial graphite, the majority of which is primary particle artificial graphite.

[0090] Example 5 The only difference from Example 1 is that in step (2), coke powder, epoxy resin, water, and boron oxide are uniformly mixed in a mass ratio of 100:6:15:2 to obtain a mixture.

[0091] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0092] Example 6 The only difference from Example 1 is that in step (2), coke powder, coumarone resin, water, and boron oxide are uniformly mixed in a mass ratio of 100:5:15:2 to obtain a mixture.

[0093] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0094] Example 7 The only difference from Example 1 is that in step (2), coke powder, epoxy resin, water, and boron nitride are uniformly mixed in a mass ratio of 100:6:15:2 to obtain a mixture.

[0095] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0096] Example 8 The only difference from Example 1 is that in step (2), coke powder, petroleum resin, toluene, and boric acid are uniformly mixed in a mass ratio of 100:6:15:2 to obtain a mixture.

[0097] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0098] Example 9 The only difference from Example 1 is that in step (2), coke powder, phenol resin, water, and boron oxide are uniformly mixed in a mass ratio of 100:3:15:2 to obtain a mixture.

[0099] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0100] Example 10 The only difference from Example 1 is that in step (2), coke powder, phenol resin, water, and silicon carbide are uniformly mixed in a mass ratio of 100:20:15:2 to obtain a mixture.

[0101] The negative electrode material obtained in this example contains primary artificial graphite particles and secondary artificial graphite particles, with the majority being secondary artificial graphite particles.

[0102] Example 11 The only difference from Example 1 is that in step (2), coke powder, phenol resin, water, and sodium borate are uniformly mixed in a mass ratio of 100:6:5:2 to obtain a mixture.

[0103] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0104] Example 12 The only difference from Example 1 is that in step (2), coke powder, phenol resin, water, and boron oxide are uniformly mixed in a mass ratio of 100:6:50:2 to obtain a mixture.

[0105] As can be seen from the scanning electron microscope photograph in FIG. 1, the negative electrode material obtained in this example contains primary particles and secondary particles, most of which are primary particle artificial graphite. As can be seen from the pore size distribution curve in FIG. 2, the negative electrode material contains pores, and the pores mainly include micropores and mesopores.

[0106] Example 13 The only difference from Example 1 is that in step (2), coke powder, phenol resin, water, and boron chloride are uniformly mixed in a mass ratio of 100:6:15:1 to obtain a mixture.

[0107] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0108] Example 14 The only difference from Example 1 is that in step (2), coke powder, phenol resin, water, and boron oxide are uniformly mixed in a mass ratio of 100:6:15:5 to obtain a mixture.

[0109] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0110] Example 15 The only difference from Example 1 is that the press molding pressure in step (3) is 5 MPa.

[0111] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0112] Example 16 The only difference from Example 1 is that the press molding pressure in step (3) is 100 MPa.

[0113] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0114] Example 17 The only difference from Example 1 is that the temperature of the pre-carbonization treatment of the precursor in step (4) is 500°C.

[0115] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0116] Example 18 The only difference from Example 1 is that the temperature of the pre-carbonization treatment of the precursor in step (4) is 1200°C.

[0117] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0118] Example 19 The only difference from Example 1 is that the graphitization temperature in step (5) is 2800°C.

[0119] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0120] Example 20 The only difference from Example 1 is that the graphitization temperature in step (5) is 3000°C.

[0121] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0122] Example 21 The only difference from Example 1 is that the heat retention time for the graphitization treatment in step (5) is 2 hours.

[0123] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0124] Example 22 The only difference from Example 1 is that the heat retention time for the graphitization treatment in step (5) is 4 hours.

[0125] The negative electrode material obtained in this example contains primary particles of artificial graphite and secondary particles of artificial graphite, with the majority being primary particles of artificial graphite.

[0126] Comparative Example 1 The difference from Example 1 is that the second precursor obtained in step (4) is placed into a graphite crucible, and then the graphite crucible is transferred to an Acheson furnace to obtain a negative electrode material through high-temperature graphitization. The maximum temperature in the graphitization process is 2900°C, the maximum temperature retention time is 2.5 hours, and the graphitization process has a heating rate of 0.7°C / min and a cooling rate of 0.1°C / min to obtain a negative electrode material.

[0127] Comparative Example 2 The raw coke raw material of Daqing petroleum coke is crushed and shaped by a shaping device to obtain crushed and shaped coke powder. The obtained coke powder with a median diameter of 15 μm is directly put into a graphite crucible, and then the graphite crucible is transferred to an Acheson furnace to obtain a negative electrode material through high-temperature graphitization. In the graphitization process, the maximum temperature is 2900°C, and the maximum temperature is kept for 8 hours. In the graphitization process, the heating rate is 0.7°C / min, and the cooling rate is 0.1°C / min to obtain a negative electrode material.

[0128] Comparative Example 3 The raw coke raw material from Daqing petroleum coke was pre-carbonized at a temperature of 800°C for 4 hours, and then charged into a continuous graphitization furnace. The heating curve was as follows: the temperature was increased to 2800°C at a heating rate of 15°C / min, and the temperature was maintained at 2800°C for 2.5 hours. After the temperature was maintained, the temperature was decreased to 30°C at a heating rate of 10°C / min. The rate ratio of temperature increase and decrease in the graphitization process was controlled to 1.5. The graphitized product was crushed and shaped to obtain a negative electrode material, and the median diameter of the crushed negative electrode material was controlled to 15 μm.

[0129] Measurement method (1) The method for measuring the median diameter of the negative electrode material is as follows: The particle size distribution range of the negative electrode material is measured by a Malvern laser granulometer.

[0130] (2) The method for measuring the pore volume and average pore diameter of the negative electrode material is as follows: Measurements were performed using an ASAP 2460 device manufactured by Micromeritics, Inc., USA, and the pore volume V and average pore diameter were calculated within the pore diameter range of 17 Å to 3000 Å using the BJH Desorption cumulative volume of pores model.

[0131] (3) The method for measuring the specific surface area of ​​the negative electrode material is as follows: The measurements were taken using a dynamic rapid specific surface area measuring device JW-DX manufactured by Beijing Jingwei Gaobo Science and Technology Co., Ltd. The unit is m 2 / g.

[0132] (4) The method for measuring the true density of the negative electrode material is as follows: The true density is measured using an Anton Paar Quanta PENTAPYC 5200e true density meter, and the Archimedes principle of gas displacement (density = mass / volume) is applied to obtain the true volume of the material to be measured by using Boll's law (PV = nRT) under certain conditions of inert gas with a small molecular diameter, and the true specific gravity is expressed in g / cm. 3 It is.

[0133] (5) The method for measuring the surface morphology of the negative electrode material is as follows: The surface morphology of the negative electrode material particles was observed using a Hitachi S4800 scanning electron microscope.

[0134] (6) The interlayer distance d of the (002) crystal plane of the material by X-ray diffraction 002 The unit is Å, and it is the ratio of the peak intensity between the (002) plane and the (110) plane, and the peak intensity between the (004) plane and the (110) plane.

[0135] (7) The method for measuring battery performance is as follows: The negative electrode materials prepared in Examples 1-22 and Comparative Examples 1-3, carboxymethyl cellulose (abbreviated as CMC), conductive carbon black (abbreviated as SP), and styrene butadiene rubber (abbreviated as SBR) were mixed uniformly in deionized water in a mass ratio of 95:1.5:1.5:2 for 8 hours by magnetic stirring. The mixed slurry was applied onto copper foil and vacuum dried at 60°C to obtain a working electrode. Metallic lithium was used as the counter electrode and reference electrode, the separator was Celgard2325, and the electrolyte was 1mol·L-1LiPF6-EC (ethylene carbonate) / DMC (dimethyl carbonate) / EMC (ethyl methyl carbonate) (volume ratio 1:1:1), and the assembly of a CR2016 coin battery was completed in a glove box filled with high-purity argon gas.

[0136] The initial discharge capacity / initial discharge efficiency measurements were performed using a LAND battery measuring device, and the charge / discharge conditions were as follows: leave it still for 2 hours, discharge at 0.1C to 0.005V, then discharge at 0.09C, 0.08C...0.02C to 0.001V, leave it still for 15min, charge at 0.1C to 1.5V, and leave it still for 15min.

[0137] The rate characteristics of the button-type half cell are measured in an environment of 25±2°C to obtain the charge / discharge specific capacity and coulombic efficiency at 0.2C, 1C, and 2C.

[0138] The method for measuring the cycle expansion is to manufacture a pole piece from the negative electrode material and assemble it into a mold battery, and then record the expansion rate of the mold battery after 20 cycles using a sensor, where the expansion rate = change in thickness of pole piece d / original thickness of pole piece × 100%.

[0139] The results of performance measurements of the negative electrode materials obtained in the above Examples and Comparative Examples are shown in Table 1 below, and the results of performance measurements of the batteries manufactured using the negative electrode materials are shown in Table 2 below.

[0140] [Table 1]

[0141] [Table 2]

[0142] As can be seen from the measurement data of Examples 1 to 22, pores are formed inside and / or on the surface of the graphite produced in the examples of the present application, improving the high-rate charging performance of the material. When the negative electrode material is applied to a lithium-ion battery as an electrode, lithium ions are sufficiently bonded to the carbon atoms in the artificial graphite with low resistance, and diffuse quickly into the solid-liquid interface and solid phase, reducing concentration polarization and being favorable for improving the rate characteristics of the negative electrode material. Here, since needle coke is used as the coke raw material in Examples 3 and 4, the measured rate characteristics of the battery are inferior to those of other Examples, which is due to the properties of the needle coke itself, and it is not considered that the technical solution of the present application cannot solve the problem of poor rate characteristics.

[0143] In addition, when V×S / D is controlled within the range of 4.0 to 10, the more available active sites there are on the surface of the artificial graphite as a negative electrode material where the reaction of releasing and absorbing lithium occurs, the higher the specific capacity of the negative electrode material tends to be.

[0144] It can be seen that the negative electrode materials produced in the Acheson graphitization furnaces of Comparative Examples 1 and 2 have a certain pore structure, but the V×S / D deviates from the above range, the rate characteristics are significantly reduced when artificial graphite is used as the negative electrode material, and the production process consumes a large amount of energy, the thermal energy utilization rate is high, and the production time and cost are significantly increased.

[0145] In Comparative Example 3, a negative electrode material was produced by adopting a continuous graphitization process, but coke raw material particles were directly fed into a continuous graphitization furnace, and no additives were used, and no other process improvements were made, such as no control of the heating and cooling rate ratio. As a result, V×S / D was outside the above range, and the capacity and multiplication performance were inferior to those of Example 1, which was produced under equivalent process conditions.

[0146] Although the present application has been disclosed above by way of preferred embodiments, the scope of the claims is not limited thereto, and any person skilled in the art may make some possible changes or modifications without departing from the technical idea of ​​the present application, and therefore the scope of protection of the present application should conform to the scope defined in the claims of the present application.

Claims

1. A negative electrode material containing artificial graphite, the artificial graphite having pores in and / or on the surface thereof, the pore volume of the negative electrode material being V cm 3 / kg, and true density D g / cm 3 , and the specific surface area is S m 2 / g, 4.0≦V×S / D≦10, The pore volume is measured using an ASAP 2460 device manufactured by Micromeritics, Inc., USA, and calculated using the BJH Desorption cumulative volume of pores model within a pore diameter range of 17 Å to 3000 Å. A negative electrode material.

2. The negative electrode material according to claim 1, characterized in that it satisfies at least one of the following characteristics (1) to (3). (1) Particle size D of the negative electrode material 50 is between 10 μm and 30 μm; (2) Particle size D of the negative electrode material 10 ≧5 μm; (3) Particle size D of the negative electrode material 90 ≦50 μm.

3. 3. The negative electrode material according to claim 1, wherein at least one of the following characteristics (1) to (3) is satisfied: (1) The pore volume of the negative electrode material is V cm 3 / kg, 5≦V≦8; (2) The specific surface area of ​​the negative electrode material is S m 2 / g, 1.78≦S≦3.0; (3) The true density of the negative electrode material is D g / cm 3 When set to D, 2.210≦D≦2.265 holds.

4. 3. The negative electrode material according to claim 1, wherein the pores include at least one of micropores and mesopores.

5. 5. The negative electrode material according to claim 4, wherein the pores have an average pore diameter of 50 Å to 200 Å.

6. When measured by X-ray diffraction, the interplanar spacing of the (002) plane was d 002 When the 002 3. The negative electrode material according to claim 1, wherein the thickness is ≦3.365 Å.

7. When measured by X-ray diffraction, the peak intensity ratio (I 002 / I 110 ) is 65.0 to 120.0, and the peak intensity ratio (I 004 / I 110 3. The negative electrode material according to claim 1, wherein the σ is 3.0 to 6.

0.

8. 3. The negative electrode material according to claim 1, wherein the artificial graphite contains primary particles of artificial graphite and / or secondary particles of artificial graphite.

9. The negative electrode material according to claim 1 or 2, characterized in that the negative electrode material satisfies at least one of the following characteristics (1) to (2). (1) The negative electrode material further includes amorphous carbon; (2) The negative electrode material further contains amorphous carbon, and the mass ratio of the amorphous carbon in the negative electrode material is 0.1 wt % to 5 wt %.

10. A battery comprising the negative electrode material according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method of manufacturing negative electrode material for nonaqueous secondary battery

    JP2016184581A

  • Negative electrode material for nonaqueous secondary battery, negative electrode for nonaqueous secondary battery, and nonaqueous secondary battery

    JP2021061230A

  • Lithium-ion battery negative electrode active material, lithium-ion battery negative electrode, lithium-ion battery, battery pack, and battery-powered vehicle

    JP2022502827A

  • Carbon material for non-aqueous secondary battery, anode using said carbon material, and non-aqueous secondary battery

    WO2012157590A1

  • Carbon material and nonaqueous secondary battery using carbon material