Resin products with excellent hydrophilicity and water retention properties

The resin product with amorphous resin and microgrooves addresses the challenge of maintaining hydrophilicity and water retention by enhancing surface wettability and retention through specific groove configurations.

JP3249407UActive Publication Date: 2024-12-09TANAZAWA HAKKOSHA CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024003376U
Authority / Receiving Office
JP · JP
Patent Type
Utility models
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-09
Estimated Expiration
2034-10-11

AI Technical Summary

Technical Problem

Existing resin molded products face issues with maintaining long-term hydrophilicity and water-retention properties due to coating peeling off from friction, moisture adhesion, light irradiation, and deterioration, requiring a process that involves applying and drying a treatment liquid.

Method used

A resin product with amorphous resin and microgrooves on its surface, having specific dimensions and configurations, such as widths, depths, and intervals, which enhance hydrophilicity and water retention.

Benefits of technology

The resin product achieves high wettability and excellent water retention by accumulating water within the grooves, maintaining these properties even when oriented vertically or downward.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0003249407000001_ABST
    Figure 0003249407000001_ABST
Patent Text Reader

Abstract

This invention provides a resin product with excellent hydrophilicity and water retention properties by devising materials and shapes. [Solution] The resin product 1 of the present invention, which has excellent hydrophilicity and water retention properties, is made of an amorphous resin and has a plurality of grooves 2 formed on its surface, each having a width of 1.0 mm or less and a depth of 0.06 mm or more. When the surface is immersed in water for 10 seconds and then vertically removed from the water, it is preferable that water 4 accumulates to a depth of at least half the depth of the grooves. The grooves preferably have a width of 0.05 mm or more and a depth of 1.0 mm or less. In addition, it is preferable that the distance between adjacent grooves is 0.05 mm to 1.0 mm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This invention relates to a resin product that has excellent hydrophilicity and water retention properties. [Background technology]

[0002] Resin molded products are used in the exterior parts of automobiles, the outer walls of buildings, the interior parts of bathrooms, home appliances, etc. In order to increase the hydrophilicity and water retention of these resin molded products, Patent Document 1 discloses that a treatment liquid containing hydrophilic and water-retentive polyether urethane and polyhydric alcohol and / or sugar is applied to the surface of the resin molded product as a substrate, and then dried to form a coating. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-307548 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0004] However, forming such a coating requires a process of applying a treatment liquid and drying it, and the coating can peel off due to friction on the surface, adhesion of moisture, exposure to light, deterioration over time, etc., and there is a problem that the hydrophilicity and water retention of the surface of the resin molded product cannot be maintained for a long period of time.

[0005] The purpose of this invention is to provide a resin product with excellent hydrophilicity and water retention properties by devising materials and shapes. [Means for solving the problem]

[0006] The resin products of this invention have excellent hydrophilicity and water retention properties, Made of amorphous resin, The surface has multiple grooves with a width of 1.0 mm or less and a depth of 0.06 mm or more.

[0007] It is preferable that when the surface is immersed in water for 10 seconds and then vertically removed from the water, water is pooled to a depth of at least half the depth of the grooves.

[0008] The groove preferably has a width of at least 0.05 mm and a depth of at most 1.0 mm.

[0009] The grooves are preferably spaced apart from each other by a distance of 0.05 mm to 1.0 mm.

[0010] A configuration in which a quadrangular pyramidal convex portion is formed between adjacent grooves may be used.

[0011] It is preferable that the corners of the protrusions formed between adjacent grooves are chamfered. Effect of the Invention

[0012] According to the resin product of the present invention, by forming the grooves as specified above in the amorphous resin, the wettability of the surface can be made extremely high, and the product can have excellent hydrophilicity and water retention properties. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a cross-sectional view of a resin product according to the present invention. [Diagram 2] FIG. 2 is a plan view of FIG. [Diagram 3] FIG. 3 is a cross-sectional view of a resin product in which quadrangular pyramidal convex portions are formed between adjacent grooves. [Figure 4] FIG. 4 is a plan view of FIG. [Diagram 5] FIG. 5 is a cross-sectional view of a resin product in which chamfered convex portions are formed between adjacent grooves. [Figure 6] FIG. 6 is a cross-sectional view showing a state in which water has accumulated in the groove of the resin product according to the present invention. [Figure 7] FIG. 7 is a schematic diagram of the water immersion test. [Figure 8]FIG. 8 is a surface diagram of each test example, divided into three regions, in the plate used in the water immersion test. [Figure 9] FIG. 9 is a photograph of the surface of Example 1 after a water immersion test. [Figure 10] FIG. 10 is a photograph of the surface of Comparative Example 1 after the water immersion test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, one embodiment of the present invention will be described with reference to the drawings.

[0015] The resin product of the present invention is composed of an amorphous resin. When the temperature of an amorphous resin is lowered from a heated / molten state to a certain level, the molecules of the resin solidify in a random structure with irregular entanglement. Examples of amorphous resins include, but are not limited to, acrylonitrile-butadiene-styrene (ABS), polycarbonate (PC), polystyrene (PS), polyvinyl chloride (PVC), PMMA (polymethyl methacrylate), modified polyphenylene ether (m-PPE), polyethersulfone (PES / PESU), polyetherimide (PEI), and polyamideimide (PAI). Amorphous resins have a low degree of crystallinity, small voids between the polymers, and good hydrophilicity and water retention.

[0016] In addition, in contrast to amorphous resins, there are crystalline resins, which have crystalline portions in which the molecules are regularly arranged when the temperature of the heated and melted resin is lowered and solidified. For example, polypropylene (PP) and polyethylene (PE) are known as this type of resin. As shown in the examples described later, when the configuration of the groove 2 of the present invention is applied to a crystalline resin, the hydrophilicity and water retention properties of amorphous resins were not observed. Therefore, the resin product of the present invention employs amorphous resins.

[0017] As shown in Fig. 1, the resin product 1 of the present invention has grooves 2 formed on its surface. Adjacent grooves 2, 2 are partitioned by convex portions 3. Referring to the plan view of Fig. 2, the grooves 2 are configured to spread and be connected in a lattice shape. It is preferable that the grooves 2 are formed on the entire surface of the resin product 1, but they may be formed on one surface of the resin product 1.

[0018] It is preferable that the width W of the groove 2 is 1.0 mm or less and the depth D is 0.06 mm or more, and it is desirable that the groove width W is 0.8 mm or less and the groove depth D is 0.075 mm or more. The narrower the groove width W and the deeper the groove depth D, the better the water can be retained in the groove 2 due to surface tension and the like.

[0019] On the other hand, the lower limit of the groove width W is 0.05 mm, and preferably 0.1 mm. If the groove width W is smaller than this, it becomes difficult to process the groove 2 by injection molding. Of course, if the groove 2 is formed by laser processing, the groove width W can be formed narrower than this.

[0020] The upper limit of the groove depth D is 1.0 mm, and preferably 0.8 mm. If the groove depth D is too deep, it becomes difficult to process the groove 2 by injection molding. Of course, if the groove 2 is formed by laser processing, the groove depth D can be made deeper than this.

[0021] The distance L between the grooves 2, i.e., the width L of the protrusions 3 formed between the grooves 2, is preferably 0.05 mm to 1.0 mm, and more preferably 0.1 mm to 0.5 mm. The narrower the distance between the grooves 2, the larger the relative area of ​​the grooves 2 that are formed can be, and the higher the water retention can be.

[0022] The protrusions 3 that define the grooves 2 can be disposed at equal intervals so that the grooves 2 are formed in a lattice pattern as shown in Fig. 2. In the figure, the protrusions 3 are square in plan view, but they may be rectangular such as a rectangular parallelepiped, rhombus, or parallelogram, circular such as a perfect circle or ellipse, triangular, houndstooth, etc. Furthermore, the protrusions 3 can be parallel ridges, so that the grooves 2 have the form of parallel grooves.

[0023] For example, in the case of a protrusion 3 having a substantially square shape in plan view, the upper part of the protrusion 3 may be a quadrangular prism as shown in Fig. 1, or a quadrangular pyramid as shown in Figs. 3 and 4. In this case, the width W of the groove 2 and the width L of the protrusion 3 refer to the width at the intermediate depth D / 2 of the depth D of the groove 2. Of course, the protrusion 3 may have a shape in which the corners of the upper surface are chamfered as shown in Fig. 5.

[0024] The resin product 1 of the present invention can be manufactured by injection molding or blow molding. In the case of injection molding or blow molding, molding can be performed by forming irregularities in the molding die corresponding to the grooves 2 and the protrusions 3. The irregularities in the die can be formed by etching or laser processing.

[0025] Moreover, the grooves 2 may be formed on the surface of the molded resin article 1 by laser processing.

[0026] The resin product 1 having the above-mentioned configuration has hydrophilicity and water retention properties in that when the resin product 1 is immersed in water for 10 seconds and then pulled up so that the surface on which the grooves 2 are formed is perpendicular to the water, water 4 is pooled in the grooves 2 as shown in Fig. 6. The depth d of pooled water 4 in the grooves 2 is preferably 1 / 2 or more of the depth D of the grooves 2. The water 4 does not adhere to the surface of the resin product 1 in the form of droplets, but spreads within the grooves 2 and adheres as shown in Fig. 6.

[0027] The resin product 1 of the present invention has the above-mentioned hydrophilic and water-retentive properties because it uses an amorphous resin as the resin material and has the above-mentioned grooves 2 formed on its surface. As a result, the water 4 pooled in the grooves 2 is retained even when the surface of the resin product 1 is turned vertically or downward.

[0028] The resin product 1 of the present invention has excellent hydrophilicity and water retention properties, and is therefore suitable for components that require water droplets to be prevented, such as the exterior parts of automobiles, the exterior walls of buildings, the interior parts of bathrooms, home appliances, etc. Specific application examples include automobile side mirror covers, bathroom ceilings, and the inner walls of dishwashers. The resin product 1 of the present invention has the advantage that water droplets are unlikely to form on its surface due to its excellent hydrophilicity and water retention properties, so the resin product 1 dries quickly and leaves no water droplet marks when it dries. EXAMPLES

[0029] As shown in Table 1, 6 types of test samples were produced with different resin types and surface conditions, 20 pieces each, and tests were conducted to compare hydrophilicity, water retention, and water repellency. All test samples were injection molded plates with a length of 150 mm, width of 100 mm, and thickness of 3 mm. The resins used for the test samples were ABS, an amorphous resin, polystyrene (PS), an amorphous resin, and polypropylene (PP), a crystalline resin, and the surface was embossed with and without grooves.

[0030] [Table 1]

[0031] Both Invention Examples 1 and 2 have grooves made of amorphous resin, Comparative Example 1 has grooves made of crystalline resin, Comparative Examples 2 and 3 have matte finish made of amorphous resin, and Comparative Example 4 has matte finish made of crystalline resin.

[0032] Inventive Examples 1 and 2 and Comparative Example 1, grooves 2 with a groove width W of 0.1 mm and a spacing L of 0.4 mm (the width L of the protrusions 3 is 0.4 mm) are formed in a lattice pattern on one surface. In order to confirm the hydrophilicity, water retention, and water repellency resulting from differences in groove depth D, the surface of each test example was divided into three regions as shown in Figure 8, and grooves 20-22 with different groove depths D were formed. Groove 20 has a groove depth D of 0.05 mm, groove 21 has a groove depth D of 0.075 mm, and groove 22 has a groove depth D of 0.1 mm.

[0033] The surfaces of the prepared test specimens were subjected to etching and blasting (#150, working pressure 5).

[0034] The hydrophilicity, water retention and water repellency tests were carried out by preparing a cylindrical container 50 filled with water 4 as shown in Figure 7, immersing each test sample in the water 4 for 10 seconds, and then pulling it up so that the surface on which the grooves 2 were formed was vertical. The hydrophilicity, water retention and water repellency were evaluated by observing the amount of air bubbles adhering to the resin surface underwater, the way the water flowed when pulling it up, and the state of the water 4 remaining on the surface after pulling it up, and the hydrophilicity, water retention and water repellency were evaluated on a three-level scale of "○ (good), △ (average) and × (poor)". The results are shown in Table 1.

[0035] Considering the hydrophilicity, water retention, and water repellency tests, Invention Examples 1 and 2 had no air bubbles attached to the surface when immersed in water 4, and when pulled out, the water gently flowed down from the convex parts 3 on the surface towards the grooves 2, and accumulated in the grooves 2. Figure 9 is a photograph of the surface of Invention Example 1 immediately after it was pulled out of the water 4. It was confirmed that water had accumulated to more than half the depth of the grooves 2 when the groove depths D were 0.075 mm (reference number 21) and 0.1 mm (reference number 22). Therefore, for Invention Example 1 with groove depths D of 0.075 mm (reference number 21) and 0.1 mm (reference number 22), the hydrophilicity and water retention were evaluated as ○, and the water repellency was evaluated as ×.

[0036] On the other hand, even in Example 1, water flowed easily when the groove depth D was 0.05 mm (symbol 20), and the hydrophilicity and water retention were inferior to those of grooves 2 having depths D of 0.075 mm and 0.1 mm, with the hydrophilicity and water retention being △ and the water repellency being ×.

[0037] When Comparative Example 1 was immersed in water 4, air bubbles adhered to the resin surface. Furthermore, when it was pulled up, almost no water remained in the grooves 2, but instead ran down in the form of droplets, regardless of the depth of the grooves 2. The water remaining on the resin surface remained on the protrusions 3, straddling the grooves 2 in multiple places, as shown in Fig. 10. Therefore, for Comparative Example 1, regardless of the depth of the grooves 2, the hydrophilicity and water retention were evaluated as △, and the water repellency was also evaluated as △.

[0038] On the other hand, in the case of the matte finish Comparative Example 2-4, regardless of the type of resin, i.e., amorphous or crystalline, many air bubbles adhered to the surface when the sample was immersed in water 4. In addition, when the sample was pulled out, some of the water turned into droplets and ran down. The water remaining on the resin surface remained on the protrusions 3, straddling the grooves 2. Therefore, the hydrophilicity and water retention were evaluated as ×, and the water repellency was evaluated as △.

[0039] From the above, it can be seen that the present invention is able to improve hydrophilicity and water retention by forming grooves 2 on the surface of the amorphous resin.

[0040] The above description is for the purpose of explaining the present invention, and should not be interpreted as limiting the invention described in the utility model claims or restricting the scope. In addition, the configuration of each part of the present invention is not limited to the above embodiment, and various modifications are possible within the technical scope described in the utility model claims. [Explanation of symbols]

[0041] 1. Resin products 2 grooves 3 Convex

Claims

1. Made of amorphous resin, A plurality of grooves having a width of 1.0 mm or less and a depth of 0.06 mm or more are formed on the surface. A resin product with excellent hydrophilicity and water retention properties.

2. When the surface is immersed in water for 10 seconds and then vertically removed from the water, water is retained to a depth of at least half the depth of the groove.

2. The resin product having excellent hydrophilicity and water retention properties according to claim 1.

3. The groove has a width of 0.05 mm or more and a depth of 1.0 mm or less.

3. A resin product having excellent hydrophilicity and water retention properties according to claim 2.

4. The grooves have a distance between adjacent grooves of 0.05 mm to 1.0 mm.

4. A resin product having excellent hydrophilicity and water retention properties according to claim 3.

5. A pyramidal convex portion is formed between adjacent grooves.

5. A resin product having excellent hydrophilicity and water retention properties according to claim 4.

6. The convex portions formed between adjacent grooves have chamfered corners.

5. A resin product having excellent hydrophilicity and water retention properties according to claim 4.

Citation Information

Patent Citations

  • Method for imparting hydrophilicity to resin surface, resin product and glass product

    JP2004307548A