Composite materials
A composite material combining metal foam and a polymeric component addresses the issues of thermal conductivity, impact resistance, and workability by using a metal foam with high porosity and metal content, achieving effective thermal management with improved mechanical properties.
Patent Information
- Application Number
- JP2020515222
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-09-15
- Filing Date
- 2018-09-17
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2038-09-17
AI Technical Summary
Existing composite materials with high thermal conductivity suffer from poor workability and impact resistance due to the addition of large amounts of filler components.
A composite material comprising a metal foam with a porosity of at least 10% and a metal content of 55% by weight or more, combined with a polymeric component, which ensures high thermal conductivity while maintaining impact resistance and workability.
The composite material achieves excellent thermal conductivity, impact resistance, and workability, with thermal conductivity ranging from 0.4 W/mK to 5.5 W/mK, depending on the composition and manufacturing method.
Smart Images

Figure 0007551086000002 
Figure 0007551086000001
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2017-0118735, filed on September 15, 2017, the entire contents of which are incorporated herein by reference.
[0002] This application relates to composite materials. [Background technology]
[0003] Heat dissipation materials are used in a variety of applications. For example, batteries and various electronic devices generate heat during their operation, and materials that can effectively manage this heat are required.
[0004] Ceramic materials with good thermal conductivity are known as materials with good heat dissipation properties, but such materials are poor in processability, so a composite material manufactured by blending the above-mentioned ceramic filler, which has high thermal conductivity, into a polymer matrix can be used.
[0005] However, in this method, a large amount of filler must be used to ensure high thermal conductivity, which can cause various problems. For example, when a material contains a large amount of filler, the material itself tends to become hard, resulting in poor impact resistance. Summary of the Invention [Problem to be solved by the invention]
[0006] The present application relates to a composite material, and an object of the present application is to provide, as an example, a composite material or a manufacturing method thereof that has excellent thermal conductivity characteristics while also ensuring other physical properties such as impact resistance and processability. [Means for solving the problem]
[0007] This application relates to composites. In this application, the term "composite" refers to a material that includes a metal foam and a polymeric component.
[0008] As used herein, the term "metal foam or metal skeleton" refers to a porous structure containing metal as a main component. The term "containing metal as a main component" refers to a case where the ratio of metal is 55 wt% or more, 60 wt% or more, 65 wt% or more, 70 wt% or more, 75 wt% or more, 80 wt% or more, 85 wt% or more, 90 wt% or more, or 95 wt% or more based on the total weight of the metal foam or metal skeleton. The upper limit of the ratio of metal contained as the main component is not particularly limited, and may be, for example, about 100 wt%, 99 wt%, or 98 wt%.
[0009] As used herein, the term "porosity" refers to a porosity of at least 10%, 20%, 30%, 40%, 50%, 60%, 70%, 75%, or 80%. The upper limit of the porosity is not particularly limited, and may be, for example, less than about 100%, about 99% or less, or about 98% or less. The porosity can be calculated by a known method by calculating the density of the metal foam or the like.
[0010] The composite material has a high thermal conductivity, which makes it suitable for use in materials for heat management, such as heat dissipation materials.
[0011] For example, the composite may have a thermal conductivity of about 0.4 W / mK or more, 0.45 W / mK or more, 0.5 W / mK or more, 0.55 W / mK or more, 0.6 W / mK or more, 0.65 W / mK or more, 0.7 W / mK or more, 0.75 W / mK or more, 0.8 W / mK or more, 0.85 W / mK or more, 0.9 W / mK or more, 0.95 W / mK or more, 1 W / mK or more, 1.5 W / mK or more, 2 W / mK or more, 2.5 W / mK or more, 3 W / mK or more, 3.5 W / mK or more, 4 W / mK or more, 4.5 W / mK or more, or 5 W / mK or more. The higher the thermal conductivity of the composite material, the better the thermal control function of the composite material, and is not particularly limited, and may be, for example, about 100 W / mK or less, 90 W / mK or less, 80 W / mK or less, 70 W / mK or less, 60 W / mK or less, 50 W / mK or less, 40 W / mK or less, 30 W / mK or less, 20 W / mK or less, or 10 W / mK or less. The method for measuring the thermal conductivity is not particularly limited, and may be, for example, the method described in the examples below.
[0012] The thermal conductivity of the composite material is measured by the method described in the Examples section below.
[0013] In the present specification, when the measurement temperature affects a physical property, the physical property is measured at room temperature unless otherwise specified. The term "room temperature" refers to a natural temperature that is not heated or cooled, and means, for example, any one of temperatures within a range of about 10°C to 30°C, about 23°C or about 25°C.
[0014] The composite material of the present application has excellent thermal conductivity properties as described above, while at the same time other physical properties such as processability and impact resistance can be stably ensured, and such effects can be achieved by the contents described in this specification.
[0015] The shape of the metal foam contained in the composite material is not particularly limited, but may be, for example, a film shape. In the composite material of the present application, a polymer component present on the surface or inside of the film-shaped metal foam is added.
[0016] Such a polymer component may form a surface layer on at least one surface of the metal foam, or may be present by filling pores inside the metal foam, and in some cases, may form the surface layer and also fill the interior of the metal foam. When forming a surface layer, the polymer component may form a surface layer on at least one surface, some surfaces, or all surfaces of the metal foam. As an example, the polymer component may form a surface layer on at least the upper and / or lower surfaces, which are the main surfaces of the metal foam. The surface layer may be formed so as to cover the entire surface of the metal foam, or may be formed so as to cover only a part of the surface.
[0017] In the composite, the metal foam may have a porosity in the range of about 10% to 99%. The metal foam with such a porosity has a porous metal skeleton that forms a suitable heat transfer network, and therefore can ensure good thermal conductivity even when the metal foam is applied in a small amount. In other examples, the porosity may be 15% or more, 20% or more, 25% or more, 30% or more, 35% or more, 40% or more, 45% or more, or 50% or more, or 98% or less.
[0018] As described above, the metal foam may be in the form of a film. In this case, the thickness of the film may be adjusted in consideration of the desired thermal conductivity, thickness ratio, etc., when producing a composite material by the method described below. The thickness of the film may be, for example, about 10 μm or more, about 20 μm or more, about 30 μm or more, about 40 μm or more, about 45 μm or more, about 50 μm or more, about 55 μm or more, about 60 μm or more, about 65 μm or more, or about 70 μm or more in order to ensure the desired thermal conductivity. The upper limit of the thickness of the film is controlled according to the purpose and is not particularly limited, but may be, for example, about 1,000 μm or less, about 900 μm or less, about 800 μm or less, about 700 μm or less, about 600 μm or less, about 500 μm or less, about 400 μm or less, about 300 μm or less, about 200 μm or less, or about 150 μm or less.
[0019] As used herein, thickness may be the minimum thickness, maximum thickness or average thickness of an object if the thickness of the object is not constant.
[0020] The metal foam may be a material having high thermal conductivity. For example, the metal foam may include or consist of a metal or metal alloy having a thermal conductivity of about 8 W / mK or more, about 10 W / mK or more, about 15 W / mK or more, about 20 W / mK or more, about 25 W / mK or more, about 30 W / mK or more, about 35 W / mK or more, about 40 W / mK or more, about 45 W / mK or more, about 50 W / mK or more, about 55 W / mK or more, about 60 W / mK or more, about 65 W / mK or more, about 70 W / mK or more, about 75 W / mK or more, about 80 W / mK or more, about 85 W / mK or more, or about 90 W / mK or more. The thermal conductivity is not particularly limited because a smaller amount of metal foam can be used while ensuring the desired thermal control properties as the thermal conductivity is higher, and may be, for example, about 1,000 W / mK or less.
[0021] The skeleton of the metal foam may be made of various kinds of metals or metal alloys, and a material that can exhibit the thermal conductivity in the above-mentioned range may be selected from the metals and metal alloys. Examples of such materials include, but are not limited to, any one metal selected from the group consisting of copper, gold, silver, aluminum, nickel, iron, cobalt, magnesium, molybdenum, tungsten, and zinc, and an alloy of two or more of the above.
[0022] Various metal foams are known in the art, and various methods for manufacturing such metal foams are also known in the art. In the present application, such known metal foams or metal foams manufactured by the known methods may be applied.
[0023] Known methods for producing metal foam include a method of sintering a composite material of a metal and a pore-forming agent such as a salt, a method of coating a metal on a support such as a polymer foam and sintering it in that state, a slurry method, etc. The metal foam may also be produced by the methods disclosed in the applicant's prior applications, Korean Application Nos. 2017-0086014, 2017-0040971, 2017-0040972, 2016-0162154, 2016-0162153, and 2016-0162152.
[0024] The metal foam may also be manufactured by an induction heating method among the methods disclosed in the prior application, and in this case, the metal foam may contain at least a conductive magnetic metal. In this case, the metal foam may contain the conductive magnetic metal in an amount of 30% by weight or more, 35% by weight or more, 40% by weight or more, 45% by weight or more, or 50% by weight or more based on weight. As another example, the ratio of the conductive magnetic metal in the metal foam may be about 55% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, or 90% by weight or more. The upper limit of the ratio of the conductive magnetic metal is not particularly limited, and may be, for example, less than about 100% by weight or less than 95% by weight.
[0025] As used herein, the term "conductive magnetic metal" refers to a metal having a given relative magnetic permeability and electrical conductivity, and capable of generating heat by induction heating to a degree sufficient to permit sintering of the metal.
[0026] As an example, the conductive metal may have a relative magnetic permeability of 90 or more. ris the ratio μ / μ0 of the magnetic permeability μ of the substance to the magnetic permeability μ0 in a vacuum. The metal has a relative magnetic permeability of 95 or more, 100 or more, 110 or more, 120 or more, 130 or more, 140 or more, 150 or more, 160 or more, 170 or more, 180 or more, 190 or more, 200 or more, 210 or more, 220 or more, 230 or more, 240 or more, 250 or more, 260 or more, 270 or more, 280 or more, 290 or more, 300 or more, 310 or more, 320 or more, 330 or more, 340 or more, 350 or more, 360 or more, 370 or more, 380 or more, 390 or more, 400 or more, 410 or more, 420 or more, 430 or more, 440 or more, 450 or more, 460 or more, 470 or more, 480 or more, 490 or more, 500 or more, 510 or more, 520 or more, 530 or more, 540 or more, 550 or more, 560 or more, 570 or more, 580 or more, 590 or more, 600 or more, 610 or more, 620 or more, 630 or more, 640 or more, 650 or more, 660 or more, 670 or more, 680 or more, 690 or more, 700 or more, 710 or more, 720 or more, 730 or more, 740 or more, 750 or more, 760 The relative permeability may be 0 or more, 350 or more, 360 or more, 370 or more, 380 or more, 390 or more, 400 or more, 410 or more, 420 or more, 430 or more, 440 or more, 450 or more, 460 or more, 470 or more, 480 or more, 490 or more, 500 or more, 510 or more, 520 or more, 530 or more, 540 or more, 550 or more, 560 or more, 570 or more, 580 or more, or 590 or more. The higher the relative permeability, the higher the heat generated when an electromagnetic field for induction heating described later is applied, so the upper limit is not particularly limited. As an example, the upper limit of the relative permeability may be, for example, about 300,000 or less.
[0027] The conductive magnetic metal may have an electrical conductivity of about 8 MS / m or more, 9 MS / m or more, 10 MS / m or more, 11 MS / m or more, 12 MS / m or more, 13 MS / m or more, or 14.5 MS / m or more at 20° C. The upper limit of the electrical conductivity is not particularly limited, and for example, the electrical conductivity may be about 30 MS / m or less, 25 MS / m or less, or 20 MS / m or less.
[0028] Specific examples of such conductive magnetic metals include, but are not limited to, nickel, iron, or cobalt.
[0029] As described above, the composite further includes a polymer component present on the surface of the metal foam or inside the metal foam, and the ratio T / MT of the thickness MT of the metal foam to the total thickness T of the composite may be 2.5 or less. The thickness ratio may be about 2 or less, 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, 1.15 or less, or 1.1 or less, as another example. The lower limit of the thickness ratio is not particularly limited, but may be about 1 or more, about 1.01 or more, about 1.02 or more, about 1.03 or more, about 1.04 or more, or about 1.05 or more, as an example. Under such a thickness ratio, a composite having excellent processability, impact resistance, etc., while ensuring a desired thermal conductivity, may be provided.
[0030] The type of polymer component contained in the composite material of the present application is not particularly limited, and may be selected in consideration of, for example, the processability, impact resistance, insulating properties, etc. Examples of polymer components applicable to the present application include, but are not limited to, one or more selected from the group consisting of known acrylic resins, silicone resins, epoxy resins, urethane resins, amino resins, and phenolic resins.
[0031] In the case of the composite material, by applying the above-mentioned metal foam, it is possible to ensure excellent thermal conductivity while minimizing the ratio of components that mainly ensure thermal conductivity, and therefore it is possible to ensure the desired physical properties without compromising processability, impact resistance, etc.
[0032] As one example, the ratio MV / PV of the volume PV of the polymer component contained in the composite material to the volume MV of the metal foam may be 10 or less. As another example, the ratio MW / PV may be about 9 or less, 8 or less, 7 or less, 6 or less, 5 or less, 4 or less, 3 or less, 2 or less, 1 or less, or about 0.5 or less. The lower limit of the volume ratio is not particularly limited, and may be, for example, about 0.1. The volume ratio can be calculated using the weights of the polymer component and the metal foam contained in the composite material and the densities of the components.
[0033] The present application also relates to a method for producing the composite material in the above form, which may include curing a curable polymer composition on or in the metal foam, for example, a film-shaped metal foam containing a metal or metal alloy having a thermal conductivity of 8 W / mK or more.
[0034] The details of the metal foam applied in the method are as described above, and the details of the composite material produced may also follow the above description.
[0035] Meanwhile, the polymer composition used in the above is not particularly limited as long as it can form the above-mentioned polymer component through curing or the like, and such polymer components are variously known in the art.
[0036] That is, for example, the composite material can be produced by using a material having an appropriate viscosity among known components and curing it using a known method. Effect of the Invention
[0037] The present application provides a composite material that includes a metal foam and a polymer component and has excellent thermal conductivity as well as other physical properties such as impact resistance, processability, and insulation properties. [Brief description of the drawings]
[0038] [Figure 1] 1 is a photograph of a composite material produced in an example. [Diagram 2] 1 is a photograph of a composite material produced in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] The present application will be described in detail below through examples and comparative examples, but the scope of the present application is not limited to the following examples.
[0040] Example 1 The metal foam used was a copper metal foam in the form of a film having a thickness of about 70 μm and a porosity of about 70%. The copper metal foam was impregnated with a thermosetting epoxy resin composition containing a thermosetting epoxy compound (KUKDO CHEMICAL, YD128) and a hardener (KUKDO CHEMICAL, G640), and an applicator was used to remove excess composition so that the final composite had a thickness of about 120 μm. The material was then cured in an oven at about 80° C. for about 1 hour to produce a composite. The ratio MV / PV of the volume PV of the polymer component to the volume MV of the metal foam was about 0.2, calculated based on the density and weight of the applied polymer component (epoxy resin) and metal foam (copper metal foam). FIG. 1 is a photograph of the composite produced, and the thermal conductivity of the composite was about 0.411 W / mK.
[0041] The thermal conductivity was calculated by determining the thermal diffusivity A, specific heat B, and density C of the composite material, and then using the formula thermal conductivity=ABC, where the thermal diffusivity A was measured using a laser flash method (LFA device, model name: LFA467), the specific heat was measured using a differential scanning calorimeter (DSC) device, and the density was measured using the Archimedes method. The thermal conductivity is a value in the thickness direction (Z axis) of the composite material.
[0042] Example 2 A composite was prepared in the same manner as in Example 1, except that a thermosetting silicone composition (PDMS, Sylgard 183 kit) was used as the polymer composition and the curing process was carried out in an oven at 230°C for about 10 minutes (final composite thickness: about 120μm). The ratio MV / PV of the volume PV of the polymer component to the volume MV of the metal foam was about 0.2, calculated based on the density and applied weight of the applied polymer component (silicone resin) and metal foam (copper metal foam). Figure 2 is a photograph of the prepared composite, and the thermal conductivity of this composite was measured by the method mentioned above, and was about 0.673W / mK.
[0043] Example 3 The composite was manufactured in the same manner as in Example 2, but the thickness of the final composite was adjusted to about 100 μm, and the curing process was carried out at about 120° C. for about 10 minutes. The ratio MV / PV of the volume PV of the polymer component to the volume MV of the metal foam was calculated based on the density and applied weight of the applied polymer component (silicone resin) and metal foam (copper metal foam), and was about 0.25. The thermal conductivity of this composite was measured by the method mentioned above and was about 2.633 W / mK.
[0044] Example 4 The composite was manufactured in the same manner as in Example 2, but the thickness of the final composite was about 80 μm, and the curing process was carried out at about 120° C. for about 10 minutes. The ratio MV / PV of the volume PV of the polymer component to the volume MV of the metal foam was about 0.34, as calculated based on the density and applied weight of each of the applied polymer component (silicone resin) and metal foam (copper metal foam). The thermal conductivity of this composite was measured by the above-mentioned method and was about 3.065 W / mK.
[0045] Example 5 A composite was manufactured in the same manner as in Example 2, except that the polymer composition was changed to a thermosetting silicone composition (PDMS, Sylgard 527 kit), and the curing process was carried out at about 120°C for about 90 minutes. The ratio MV / PV of the volume PV of the polymer component to the volume MV of the metal foam was about 0.25, as calculated based on the density and applied weight of the applied polymer component (silicone resin) and metal foam (copper metal foam). The thermal conductivity of this composite was measured by the method mentioned above, and was about 3.403 W / mK.
[0046] Example 6 The composite was manufactured in the same manner as in Example 5, but the thickness of the final composite was about 80 μm. The ratio MV / PV of the volume PV of the polymer component to the volume MV of the metal foam was about 0.34, as calculated based on the density and weight of the applied polymer component (silicone resin) and metal foam (copper metal foam). The thermal conductivity of this composite was measured by the method mentioned above, and was about 5.474 W / mK.
[0047] Comparative Example 1 Only the polymer composition applied in Example 1 was cured to form a film having a thickness of about 120 μm. The thermal conductivity of the formed film was about 0.199 W / mK.
[0048] Comparative Example 2 Only the polymer composition applied in Example 2 was cured to form a film having a thickness of about 120 μm. The thermal conductivity of the formed film was about 0.270 W / mK.
[0049] Comparative Example 3 A composite was formed in the same manner as in Example 1, except that the final thickness of the composite was about 200 μm. The thermal conductivity of the formed composite was about 0.367 W / mK.
Claims
1. The present invention includes a metal foam in the form of a film, and a polymer component present on the surface of the metal foam and inside the metal foam, the polymer component forms a surface layer on the surface of the metal foam; The metal foam has a thickness of 10 μm or more and 300 μm or less, The ratio T / MT of the thickness MT of the metal foam to the total thickness T is 2 or less; the metal foam has a porosity in the range of 10-70%; A ratio MV / PV of a volume PV of the polymer component to a volume MV of the metal foam is 0.25 or more and 10 or less, A composite material having a thermal conductivity (T) of 1 W / mK or more according to Formula 1: [Formula 1] T = A x B x C where A is the thermal diffusivity of the composite, B is the specific heat of the composite, and C is the density of the composite.
2. 2. The composite of claim 1, wherein the ratio T / MT of the thickness of the metal foam MT to the total thickness T is 1.01 or greater.
3. 3. The composite material according to claim 1 or 2, wherein the ratio T / MT of the thickness MT of the metal foam to the total thickness T is less than or equal to 1.
5.
4. 4. The composite of claim 1 , wherein the metal foam comprises a metal or metal alloy having a thermal conductivity (T) of 8 W / mK or greater.
5. 5. The composite material according to claim 1, wherein the metal foam has a skeleton containing any one metal selected from the group consisting of copper, gold, silver, aluminum, nickel, iron, cobalt, magnesium, molybdenum, tungsten and zinc, or two or more of the above.
6. 6. The composite material according to claim 1, wherein the polymer component comprises one or more resins selected from the group consisting of acrylic resins, silicone resins, epoxy resins, urethane resins, amino resins and phenolic resins.
7. 2. The method of claim 1, comprising: curing a curable polymer composition on or within a film-shaped metal foam, the metal foam comprising a metal or metal alloy having a thermal conductivity of 8 W / mK or more.
Citation Information
Patent Citations
Heat dissipating sheet
JP2004289063A
Thermal pad, method for manufacturing a thermal pad, heat dissipation device, and electronic device
JP2014534645A
Foamed metal component for a wireless communication tower
JP2016503575A