Multi-layer composite non-woven material and preparation method and preparation system thereof

By using multi-layer composite structures and hot-rolled spunlace technology in nonwoven materials, the problems of reduced strength and poor water absorption caused by short fiber lengths are solved, and multi-layer composite non-woven materials with high strength, high water absorption and low fluff are realized. Woven materials.

CN118721944AActive Publication Date: 2024-10-01SHANDONG XIRUI NEW MATERIAL CO LTD

Patent Information

Application Number
CN202410788987.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-01
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

When existing nonwoven materials use short fiber lengths, it is difficult to achieve good reinforcement effects and water absorption properties, resulting in reduced strength and excessive fluff on the surface of the fabric.

Method used

Using the preparation method of multi-layer composite nonwoven materials, the first and second fiber web layers are prepared by melt blowing or spun bonding, and an intermediate fiber web layer is formed on the surface, and the combined structure of carded and mixed fiber webs is used, combined with hot rolling and spunlace technology to form materials with high strength and high water absorption properties.

Benefits of technology

The tight entanglement and mixing of fibers is achieved, which improves the strength and water-absorbing properties of the material, while reducing the fluff on the surface of the fabric and improving the surface density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721944A_ABST
    Figure CN118721944A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of non-woven composite materials, and particularly relates to a multi-layer composite non-woven material and a preparation method and a preparation system thereof. The first fiber web layer and the second fiber web layer of the composite material are prepared through melt-blowing or spunbonding and serve as the two outermost surface layers of the composite material; meanwhile, carded fiber webs are obtained from carded short fibers through a carding web forming method, the carded fiber webs obtained from the short fibers through carding web forming are mixed with filaments obtained through melt-blowing to form mixed fiber webs, and the carded fiber webs and / or the mixed fiber webs are / is used as middle water absorption layer fiber webs of the composite material; and carrying out hot rolling, pre-spunlacing, spunlacing and drying to obtain the composite non-woven material. The multi-layer composite non-woven material prepared by the method provided by the invention is high in strength, good in water absorption performance, less in fluff on the surface of the fabric, high in surface compactness and clear in pattern appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of non-woven composite materials, and in particular relates to a multi-layer composite non-woven material and a preparation method and a preparation system thereof. Background Art

[0002] At present, the demand for disposable sanitary materials in my country has greatly increased, which has also brought about the vigorous development of the nonwoven industry. The fibers produced by the spunmelt process have smaller fiber fineness and stronger wiping and cleaning capabilities than cellulose fibers, but their water absorption performance is relatively poor. At present, the carding and hydroentanglement methods are generally used to prepare nonwoven materials with good water absorption performance. In the reinforcement process, the reinforcement effect is mainly achieved by the entanglement of the carded fibers.

[0003] However, the conventional carding and spunlace reinforcement methods currently have high requirements for fiber length, otherwise they cannot achieve good carding and reinforcement effects. The shorter the fiber, the worse the entanglement effect during the reinforcement process, and thus the worse the reinforcement effect, and the lower the product strength. Especially when some recycled fibers or noil fibers with shorter fiber lengths are used as raw materials for non-woven materials, the non-woven material strength will be low and there will be more fluff on the surface of the fabric. Summary of the invention

[0004] The object of the present invention is to provide a multi-layer composite nonwoven material and a preparation method and a preparation system thereof. The multi-layer composite nonwoven material prepared by the method provided by the present invention has high strength and less fluff on the surface of the fabric.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a multi-layer composite nonwoven material, comprising the following steps:

[0007] Performing a first melt-blowing or a first spun-bonding process on a first raw material to obtain a first web layer, wherein the first raw material includes a first thermoplastic polymer;

[0008] An intermediate fiber web layer is prepared on the surface of the first fiber web layer, and the intermediate fiber web layer includes a plurality of stacked mixed fiber webs and / or a plurality of carded fiber webs; the preparation method of the mixed fiber web comprises the following steps: a first water-absorbent staple fiber is subjected to a first carding process to form a web, to obtain a first carded fiber web, a second raw material is subjected to a second melt-blowing process, and the obtained melt-blown filaments are mixed with the first carded fiber web to obtain a mixed fiber web; the second raw material includes a second thermoplastic polymer; the preparation method of the carded fiber web comprises the following steps: a second water-absorbent staple fiber is subjected to a second carding process to form a web;

[0009] On the surface of the intermediate fiber web layer, a third raw material is subjected to a third melt-blowing or a second spun-bonding to form a second fiber web layer, thereby obtaining a multi-layer fiber web; the third raw material comprises a third thermoplastic polymer;

[0010] The multi-layer web is hot-rolled by a hot-rolling roller to obtain a hot-rolled web, wherein the first web layer of the multi-layer web forms the lower surface of the hot-rolled web, and the second web layer of the multi-layer web forms the upper surface of the hot-rolled web; the hot-rolling is performed by a hot-rolling roller, and a pattern is arranged on the roller surface of the hot-rolling roller;

[0011] The hot rolled web is pre-spunlaced and then spunlaced to obtain a spunlaced web; the spunlaced web includes sequentially performing first rotary drum reverse spunlacing, rotary drum forward spunlacing, second rotary drum reverse spunlacing and flat net forward spunlacing; the first rotary drum reverse spunlacing is to perform first spunlacing on the lower surface of the hot rolled web on the rotating circumference of the drum, the rotary drum forward spunlacing is to perform second spunlacing on the upper surface of the hot rolled web on the rotating circumference of the drum, the second rotary drum reverse spunlacing is to perform third spunlacing on the lower surface of the hot rolled web on the rotating circumference of the drum, and the flat net forward spunlacing is to perform fourth spunlacing on the upper surface of the hot rolled web on a suction net curtain, and vacuum is simultaneously drawn on the lower surface of the hot rolled web;

[0012] The spunlace web is dried to obtain the multi-layer composite nonwoven material.

[0013] Preferably, the diameters of the meltblown filaments obtained by the first meltblown, the second meltblown and the third meltblown and the spunbonded filaments obtained by the first spunbond and the second spunbond are independently 2 to 20 μm; the gram weights of the first web layer and the second web layer are independently 1 to 25 gsm; the total mass of the first web layer and the second web layer accounts for 5 to 60% of the mass of the multi-layer composite nonwoven material, more preferably 10 to 60%;

[0014] The gram weight of the intermediate fiber web layer is 10 to 80 gsm; the mass of the intermediate fiber web layer accounts for 40 to 95% of the mass of the multi-layer composite nonwoven material, and more preferably 40 to 90%.

[0015] Preferably, the first thermoplastic polymer, the second thermoplastic polymer and the third thermoplastic polymer independently include one or more of polypropylene, polyethylene, polyester, nylon, polyurethane, polylactic acid and thermoplastic biodegradable plastics. The thermoplastic biodegradable plastic preferably includes polybutylene terephthalate-adipate and / or polybutylene succinate; the first thermoplastic polymer, the second thermoplastic polymer and the third thermoplastic polymer independently are monocomponent fibers or multicomponent fibers.

[0016] Preferably, the first raw material further includes a first functional masterbatch, the mass ratio of the first thermoplastic polymer to the first functional masterbatch is (80-100): (0-20), and the first functional masterbatch is not 0;

[0017] The second raw material further includes a second functional masterbatch, the mass ratio of the second thermoplastic polymer to the second functional masterbatch is (80-100): (0-20), and the second functional masterbatch is not 0;

[0018] The third raw material further includes a third functional masterbatch, the mass ratio of the third thermoplastic polymer to the third functional masterbatch is (80-100): (0-20), and the third functional masterbatch is not 0;

[0019] The first functional masterbatch, the second functional masterbatch and the third functional masterbatch independently include one or more of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch.

[0020] Preferably, the first water-absorbent short fibers and the second water-absorbent short fibers independently include one or more of cotton fibers, cashmere fibers, hemp fibers, viscose fibers and lyocell fibers;

[0021] The first water-absorbent short fibers and the second water-absorbent short fibers are independently monocomponent short fibers or bicomponent short fibers, and the bicomponent short fibers include one or more of a sheath-core type, a side-by-side type, a trilobal type, and a segmented orange type;

[0022] The lengths of the first water-absorbent short fibers and the second water-absorbent short fibers are greater than 10 mm.

[0023] Preferably, the hot rolling roller comprises an upper heating roller and a lower heating roller, the hot rolling temperature is 80-120° C., and the inter-roller pressure between the upper heating roller and the lower heating roller is 25-100 bar;

[0024] The pattern includes a dot pattern, a line pattern or a combined pattern.

[0025] Preferably, the water pressure of the pre-hydraulic needle jet is 0.5-60 Bar; the water pressure of the first rotary drum reverse needle jet, rotary drum forward needle jet, second rotary drum reverse needle jet and flat net forward needle jet is independently 20-120 Bar;

[0026] The drying is oven drying, and the oven drying temperature is 90-130°C.

[0027] The present invention provides a composite multi-layer nonwoven material prepared by the preparation method described in the above technical scheme, comprising a first layer structure, an intermediate layer structure and a second layer structure stacked in sequence; the first layer structure is formed by a first meltblown fiber web or a second spunbond fiber web; the intermediate layer structure is formed by a plurality of mixed-spray fiber webs and / or a plurality of carded fiber webs, and the second layer structure is formed by a second meltblown fiber web or a second spunbond fiber web.

[0028] The present invention provides a preparation system used in the preparation method described in the above technical solution, comprising a web-forming curtain, a web-forming system arranged above the web-forming curtain, the web-forming system comprising a first polymer melt-blown forming system and / or a polymer spunbond forming system, and also comprising a plurality of mixed-spray systems and / or a plurality of second combing systems; the mixed-spray system comprises at least one second polymer melt-blown forming system, one first combing system and one forming box;

[0029] A hot rolling device disposed downstream of the web-forming curtain, a first rotary drum disposed downstream of the hot rolling device, the first rotary drum rotating counterclockwise, a pre-wetting water jet disposed below the first rotary drum, and a first water jet disposed on the right side of the first rotary drum;

[0030] A second drum is arranged above the first drum; the second drum rotates clockwise, and a second water jet head is arranged on the left side and / or above the second drum;

[0031] a third drum disposed downstream of the first drum; the third drum rotates counterclockwise, and a third water jet head is disposed on the left side and / or below the third drum;

[0032] A suction net curtain disposed downstream of the third drum; a fourth water jet head disposed above the suction net curtain, and a suction device disposed below the suction net curtain;

[0033] A drying device is arranged downstream of the suction curtain, and a winding device is arranged downstream of the drying device.

[0034] Preferably, the spinnerets of the first polymer melt-blown forming system and the second polymer melt-blown forming system include a first spinneret, a second spinneret or a third spinneret;

[0035] The first spinneret is provided with a single row of first spinneret holes, the first spinneret holes are inverted conical holes, the outer cone surface of the first spinneret holes is sleeved with first airflow drafting holes, the first airflow drafting holes are inverted conical holes and are coaxial with the first spinneret holes, the long fibers ejected from the first spinneret holes and the drafting gas ejected from the first airflow drafting holes converge at the apex, and the angle between the drafting gas and the long fibers is 30-70°;

[0036] The second spinneret is provided with a single row or multiple rows of second spinneret holes, the second spinneret holes are cylindrical holes, the outer circumference of the second spinneret holes is sleeved with second airflow drafting holes, the second airflow drafting holes are annular holes and are coaxial with the second spinneret holes;

[0037] The third spinneret is provided with a single row or multiple rows of third airflow drafting holes, the third airflow drafting holes are cylindrical holes, the outer peripheral surface of the third airflow drafting holes is sleeved with third spinneret holes, the third spinneret holes are annular holes and are coaxial with the third airflow drafting holes.

[0038] The present invention provides a method for preparing a multi-layer composite nonwoven material. The preparation method provided by the present invention prepares a first fiber web layer and a second fiber web layer of a composite material by melt-blowing or spun-bonding as the two outermost surface layers of the composite material; at the same time, the short fibers with combability are combed into a web to obtain a combed fiber web, and the combed fiber web obtained by combing the short fibers into a web is mixed with the filaments obtained by melt-blowing to form a mixed fiber web, and the combed fiber web is used alone as an intermediate fiber web of the composite material as an intermediate water-absorbing layer in the composite material, or the combed fiber web and the mixed fiber web are used together as the intermediate fiber web of the composite material as the water-absorbing layer of the composite material; a multi-layer fiber web with a "sandwich" structure is obtained. After that, the composite nonwoven material is obtained after hot rolling, pre-spunlace, spunlace and drying. In the process of hot rolling for compounding the three-layer fiber mesh layer, the hot rolling roller embossing method is used to apply the pattern, and the hot rolling roller is used to give the product a pattern. Since the filaments obtained from the thermoplastic polymer in the hot rolling process are melted, the clarity of the pattern effect given in the hot rolling composite molding process will be better; then the spunlace method is used to make the filaments and the water-absorbent staple fibers in the product more tightly entangled and mixed, and the obtained multi-layer composite nonwoven material has high strength, good water absorption performance, less fluff on the surface of the fabric, and high surface density.

[0039] At the same time, the preparation method provided by the present invention is completed directly from raw materials to finished cloth in one step, which can reduce a large number of intermediate processes, save a lot of electricity, manpower, and equipment, and can greatly reduce processing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a schematic diagram of the structure of the device used in Example 1 of the present invention;

[0041] Figure 2 This is a schematic diagram of the structure of a multi-layer composite nonwoven material prepared in Example 1 of the present invention;

[0042] Figure 3 This is a schematic diagram of the structure of the device used in Example 2 of the present invention;

[0043] Figure 4 A schematic diagram of the structure of a multi-layer composite nonwoven material prepared in Example 2 of the present invention;

[0044] Figure 5 This is a schematic diagram of the structure of the device used in Example 3 of the present invention;

[0045] Figure 6 This is a schematic diagram of the structure of a multi-layer composite nonwoven material prepared in Example 3 of the present invention;

[0046] Figure 7 This is a schematic diagram of the structure of the device used in Example 4 of the present invention;

[0047] Figure 8 A schematic diagram of the structure of a multi-layer composite nonwoven material prepared in Example 4 of the present invention;

[0048] Fig. 9 This is a schematic diagram of the structure of the device used in Example 5 of the present invention;

[0049] Fig.10 This is a schematic diagram of the structure of a multi-layer composite nonwoven material prepared in Example 5 of the present invention;

[0050] Fig.11 This is a schematic diagram of the structure of the device used in Example 6 of the present invention;

[0051] Fig.12 A schematic diagram of the structure of a multi-layer composite nonwoven material prepared in Example 6 of the present invention;

[0052] Fig.13 This is a schematic diagram of the structure of the device used in Example 7 of the present invention;

[0053] Fig.14 This is a schematic diagram of the structure of a multi-layer composite nonwoven material prepared in Example 7 of the present invention;

[0054] Fig.15 This is a schematic diagram of the structure of the device used in Example 8 of the present invention;

[0055] Fig.16 This is a schematic diagram of the structure of a multi-layer composite nonwoven material prepared in Example 8 of the present invention;

[0056] Fig.17 This is a schematic diagram of the structure of the device used in Example 9 of the present invention;

[0057] Fig.18 This is a schematic structural diagram of a multi-layer composite nonwoven material prepared in Example 9 of the present invention;

[0058] Fig.19 This is a pattern effect diagram of the multi-layer composite nonwoven material prepared in Example 1 of the present invention;

[0059] Fig. 20 This is a pattern effect diagram of the multi-layer composite nonwoven material prepared in Comparative Example 1 of the present invention;

[0060] Fig.21 This is a pattern effect diagram of the commercially available nonwoven material of the present invention;

[0061] In the figure: 1 is the first structural layer, 2 is the middle structural layer, 3 is the second structural layer, 4 is the first polymer melt-blown molding system, 5 is the second polymer melt-blown molding system, 6 is the first combing system, 7 is the first transmission mesh curtain, 8 is the mesh curtain, 9 is the hot rolling system, 10 is the pre-wetting spurt head, 11 is the first spurt head, 12 is the first drum, 13 is the second spurt head, 14 is the second drum, 15 is the third spurt head, 16 is the third drum, 17 is the fourth spurt head, 18 is the suction mesh curtain, 19 is the drying device, 20 is the winding device, 21 is the third polymer melt-blown molding system, 22 is the fourth polymer melt-blown molding system, 23 is the second combing system, 24 is the first polymer spunbond molding system, 25 is the second polymer spunbond molding system, 26 is the first molding box, 27 is the second molding box, and 28 is the second transmission mesh curtain. DETAILED DESCRIPTION

[0062] The present invention provides a method for preparing a multi-layer composite nonwoven material, comprising the following steps:

[0063] Performing a first melt-blowing or a first spun-bonding process on a first raw material to obtain a first web layer, wherein the first raw material includes a first thermoplastic polymer;

[0064] An intermediate fiber web layer is prepared on the surface of the first fiber web layer, and the intermediate fiber web layer includes a plurality of stacked mixed fiber webs and / or a plurality of carded fiber webs; the preparation method of the mixed fiber web comprises the following steps: a first water-absorbent staple fiber is subjected to a first carding process to form a web, to obtain a first carded fiber web, a second raw material is subjected to a second melt-blowing process, and the obtained melt-blown filaments are mixed with the first carded fiber web to obtain a mixed fiber web; the second raw material includes a second thermoplastic polymer; the preparation method of the carded fiber web comprises the following steps: a second water-absorbent staple fiber is subjected to a second carding process to form a web;

[0065] On the surface of the intermediate fiber web layer, a third raw material is subjected to a third melt-blowing or a second spun-bonding to form a second fiber web layer, thereby obtaining a multi-layer fiber web; the third raw material comprises a third thermoplastic polymer;

[0066] The multi-layer web is hot-rolled by a hot-rolling roller to obtain a hot-rolled web, wherein the first web layer of the multi-layer web forms the lower surface of the hot-rolled web, and the second web layer of the multi-layer web forms the upper surface of the hot-rolled web; the hot-rolling is performed by a hot-rolling roller, and a pattern is arranged on the roller surface of the hot-rolling roller;

[0067] The hot rolled web is pre-spunlaced and then spunlaced to obtain a spunlaced web; the spunlaced web includes sequentially performing first rotary drum reverse spunlacing, rotary drum forward spunlacing, second rotary drum reverse spunlacing and flat net forward spunlacing; the first rotary drum reverse spunlacing is to perform first spunlacing on the lower surface of the hot rolled web on the rotating circumference of the drum, the rotary drum forward spunlacing is to perform second spunlacing on the upper surface of the hot rolled web on the rotating circumference of the drum, the second rotary drum reverse spunlacing is to perform third spunlacing on the lower surface of the hot rolled web on the rotating circumference of the drum, and the flat net forward spunlacing is to perform fourth spunlacing on the upper surface of the hot rolled web on a suction net curtain, and vacuum is simultaneously drawn on the lower surface of the hot rolled web;

[0068] The spunlace web is dried to obtain the multi-layer composite nonwoven material.

[0069] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0070] The present invention performs a first melt-blowing or a first spun-bonding on a first raw material to obtain a first web layer, wherein the first raw material includes a first thermoplastic polymer. In the present invention, the first thermoplastic polymer preferably includes one or more of polypropylene, polyethylene, polyester, nylon, polyurethane, polylactic acid and thermoplastic biodegradable plastics. The thermoplastic biodegradable plastic preferably includes polybutylene terephthalate-adipate (PBAT) and / or polybutylene succinate (PBS). The first thermoplastic polymer is preferably a monocomponent fiber or a multicomponent fiber, more preferably a monocomponent fiber, a bicomponent fiber or a multicomponent fiber. The first raw material preferably also includes a first functional masterbatch. The first functional masterbatch preferably includes one or more of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch, more preferably includes one, two or three of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch. When the first functional masterbatch preferably includes any two of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch, the mass ratio of any two first functional masterbatches is preferably (5-6): (1-5), and is specifically preferably 6:1 or 5:5. In the present invention, when the first raw material preferably also includes a first functional masterbatch, the mass ratio of the first thermoplastic polymer and the first functional masterbatch is preferably (80-100): (0-20), and the first functional masterbatch is not 0, and is more preferably (85-95): (5-15), and is specifically preferably 95:5, 93:7, 90:10, 92:8. The present invention has no special requirements for the specific implementation process of the first meltblowing or the first spunbonding. The diameter of the meltblown filaments obtained by the first meltblowing is preferably 2-20 μm, and more preferably 5-15 μm. The diameter of the spunbonded filaments obtained by the first spunbonding is preferably 2-20 μm, and more preferably 5-15 μm. The gram weight of the first web layer is preferably 1-25 gsm, more preferably 2-20 gsm, and more preferably 17.5 gsm, 2 gsm, 2.5 gsm or 10 gsm. The mass of the first web layer accounts for 2.5-30% of the mass of the multi-layer composite nonwoven material, and more preferably 25%, 3.335%, 4.4%, 13.9%, 13.15%, 16.65%, 14.3%, 11.1%, 12.5%.

[0071] After obtaining the first fiber web layer, the present invention prepares an intermediate fiber web layer on the surface of the first fiber web layer, and the intermediate fiber web layer includes a plurality of stacked mixed fiber webs and / or a plurality of combed fiber webs; the preparation method of the mixed fiber web includes the following steps: subjecting a second raw material to a second melt-blowing, the second raw material includes a second thermoplastic polymer; subjecting the first water-absorbent staple fibers to a first combing web to obtain a first combed fiber web, and mixing the melt-blown filaments obtained by the second melt-blowing on the first combed fiber web to obtain a mixed fiber web; the preparation method of the combed fiber web includes the following steps: subjecting the second water-absorbent staple fibers to a second combing web.

[0072] In the present invention, the number of layers of the mixed fiber web is preferably 1 or 2. The preparation method of the mixed fiber web comprises the following steps: subjecting the second raw material to a second melt-blowing, wherein the second raw material comprises a second thermoplastic polymer; subjecting the first water-absorbent staple fibers to a first carding web to a first carding web, and mixing the melt-blown filaments obtained by the second melt-blowing on the first carding web to obtain a mixed fiber web. The second thermoplastic polymer preferably comprises one or more of polypropylene, polyethylene, polyester, nylon, polyurethane, polylactic acid and thermoplastic biodegradable plastics. The thermoplastic biodegradable plastic preferably comprises polybutylene terephthalate-adipate (PBAT) and / or polybutylene succinate (PBS). The second thermoplastic polymer is preferably a monocomponent fiber or a multi-component fiber, more preferably a monocomponent fiber, a bicomponent fiber or a multi-component fiber. The second raw material preferably also comprises a second functional masterbatch. The second functional masterbatch preferably includes one or more of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch, and more preferably includes one, two or three of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch. When the second functional masterbatch preferably includes any two of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch, the mass ratio of any two first functional masterbatches is preferably (5-6): (1-5), and more preferably 6:1 or 5:5. In the present invention, when the first raw material preferably also includes the first functional masterbatch, the mass ratio of the first thermoplastic polymer and the first functional masterbatch is preferably (80-100): (0-20), and the first functional masterbatch is not 0, more preferably (85-95): (5-15), and more preferably 98:2, 93:7 or 95:5. The present invention has no special requirements for the specific implementation process of the second meltblown or the first spunbond. The diameter of the meltblown filaments obtained by the second meltblowing is preferably 2 to 20 μm, more preferably 5 to 15 μm. The diameter of the spunbond filaments obtained by the first spunbonding is preferably 2 to 20 μm, more preferably 5 to 15 μm. The first absorbent staple fiber preferably includes one or more of cotton fiber, cashmere fiber, hemp fiber, viscose fiber and lyocell fiber, more preferably includes one or two of cotton fiber, cashmere fiber, hemp fiber, viscose fiber and lyocell fiber. The first absorbent staple fiber is preferably a new fiber used for the first time or a recycled fiber, such as cotton wool, recycled cotton, or recycled fibers of other synthetic fibers in textile processing. The first absorbent staple fiber is preferably a single-component staple fiber or a two-component staple fiber, and the two-component staple fiber preferably includes one or more of a skin-core type, a parallel type, a trilobal type and a pie type. The length of the first absorbent staple fiber is preferably 10 to 65 mm, and is not 10 mm. The present invention has no special requirements for the specific implementation process of the first carding web.In the present invention, the melt-blown filaments obtained by the second melt-blown are mixed with the first carded web, preferably in a forming box, and the mixed web is obtained on a web curtain after mixing in the forming box. In the present invention, the melt-blown filaments obtained by the second melt-blown are mixed on any one surface of the first carded web, or the melt-blown filaments obtained by the second melt-blown are mixed on both surfaces of the first carded web. When the melt-blown filaments obtained by the second melt-blown are mixed on both surfaces of the first carded web, the compositions of the two melt-blown surface layers formed on the two surfaces of the first carded web are preferably the same or different; the gram weights of the two melt-blown surface layers formed on the two surfaces of the first carded web are preferably equal or unequal. In the present invention, the gram weight of the web layer formed by the melt-blown filaments obtained by the second melt-blown in the mixed web is preferably 16gsm, 7.5gsm, 8gsm, 15gsm, 30gsm. The first carded web formed by the first carding is 40gsm, 18.5gsm, 20gsm, 45gsm or 65gsm.

[0073] In the present invention, the number of layers of the second carded web obtained by the second carding is preferably 1 layer. The preparation method of the carded web comprises the following steps: the second absorbent staple fibers are carded into a web for the second time. In the present invention, the second absorbent staple fibers preferably include one or more of cotton fibers, cashmere fibers, hemp fibers, viscose fibers and lyocell fibers, and more preferably include one or two of cotton fibers, cashmere fibers, hemp fibers, viscose fibers and lyocell fibers. The second absorbent staple fibers are preferably new fibers used for the first time or recycled fibers, such as cotton wool, regenerated cotton, or recycled fibers of other synthetic fibers in textile processing. The second absorbent staple fibers are preferably single-component staple fibers or bi-component staple fibers, and the bi-component staple fibers preferably include one or more of skin-core type, parallel type, trilobal type and orange segment type. The length of the second absorbent staple fibers is preferably 10 to 65 mm, and is not 10 mm. The present invention has no special requirements for the specific implementation process of the second carding web. The second carded web formed by the second carded web has a weight of 35 gsm, 40 gsm or 45 gsm.

[0074] As one or more embodiments of the present invention, the intermediate web layer is composed of a second carded web obtained by a second carding process. The carded web obtained by the second carding process preferably has a grammage of 35 gsm, and the mass of the carded web obtained by the second carding process preferably accounts for 50% of the mass of the multi-layer composite nonwoven material.

[0075] As one or more embodiments of the present invention, the intermediate web layer is composed of a layer of mixed web. The meltblown filaments obtained by the second meltblowing in the layer of mixed web are mixed on both surfaces of the first carded web. The weight of the web formed by the meltblown filaments on both surfaces of the layer of mixed web is preferably 8gsm, 7.5gsm or 15gsm, respectively, the weight of the first carded web obtained by the first carding is preferably 40gsm, 45gsm or 65gsm, and the mass of the mixed web accounts for 93.3% of the mass of the multi-layer composite nonwoven material.

[0076] As one or more embodiments of the present invention, the intermediate web layer is composed of two layers of mixed webs. The meltblown filaments obtained by the second meltblowing in each layer of the mixed web are mixed on one surface of the first carded web, and the surface layers formed by the meltblown filaments obtained by the second meltblowing in the two layers of the mixed web are in contact with each other. The gram weight of the web formed by the meltblown filaments obtained by the second meltblowing in the two layers of the mixed web is preferably 7.5gsm or 8gsm, respectively, and the gram weight of the first carded web formed by the first carded web in the two layers of the mixed web is preferably 18.5gsm or 20gsm, respectively.

[0077] In the present invention, the grammage of the intermediate fiber web layer is 10 to 80 gsm, more preferably 20 to 70 gsm, further preferably 25 to 65 gsm, and specifically preferably 56 gsm, 26 gsm, 28 gsm, 60 gsm or 65 gsm.

[0078] In the present invention, the mass of the intermediate fiber web layer preferably accounts for 40-95% of the mass of the multi-layer composite nonwoven material, more preferably 40-90%, specifically preferably 50%, 93.33%, 91.2%, 72.2%, 73.7%, 66.7%, 75% or 64.3%.

[0079] After obtaining the intermediate web layer, the present invention performs a third melt-blowing or a second spun-bonding on the surface of the intermediate web layer to obtain a second web layer, thereby obtaining a multilayer web; the third raw material includes a third thermoplastic polymer. In the present invention, the third thermoplastic polymer preferably includes one or more of polypropylene, polyethylene, polyester, nylon, polyurethane, polylactic acid and thermoplastic biodegradable plastics. The thermoplastic biodegradable plastic preferably includes polybutylene terephthalate-adipate (PBAT) and / or polybutylene succinate (PBS). The third thermoplastic polymer is preferably a monocomponent fiber or a multicomponent fiber, more preferably a monocomponent fiber, a bicomponent fiber or a multicomponent fiber. The first raw material preferably also includes a third functional masterbatch. The third functional masterbatch preferably includes one or more of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch, and more preferably includes one, two or three of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch. When the third functional masterbatch preferably includes any two of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch, the mass ratio of any two third functional masterbatches is preferably (5-6): (1-5), and is preferably 6:1 or 5:5. In the present invention, when the third raw material preferably also includes a third functional masterbatch, the mass ratio of the third thermoplastic polymer and the third functional masterbatch is preferably (80-100): (0-20), and the third functional masterbatch is not 0, and is more preferably (85-95): (5-15), and is preferably 95:5, 93:7, 90:10, 92:8. The present invention has no special requirements for the specific implementation process of the third meltblowing or the second spunbonding. The diameter of the meltblown filaments obtained by the third meltblowing is preferably 2-20 μm, and more preferably 5-15 μm. The diameter of the spunbonded filaments obtained by the second spunbonding is preferably 2-20 μm, and more preferably 5-15 μm. The gram weight of the second web layer is preferably 1-25gsm, more preferably 2-20gsm, and specifically preferably 17.5gsm, 2gsm, 2.5gsm, 15gsm or 10gsm. The mass of the third web layer accounts for 2.5-30% of the mass of the multi-layer composite nonwoven material, and specifically preferably 25%, 3.335%, 4.4%, 13.9%, 13.15%, 16.65%, 21.4%, 16.7%, 12.5%.

[0080] In the present invention, the first fiber web layer and the third fiber web layer have the same gram weight and account for the same mass percentage of the multi-layer composite nonwoven material.

[0081] After obtaining the multi-layer web, the present invention performs hot rolling on the multi-layer web to obtain a hot rolled web, wherein the first web layer of the multi-layer web forms the lower surface of the hot rolled web, and the second web layer of the multi-layer web forms the upper surface of the hot rolled web; the hot rolling is performed using a hot rolling roller, and a pattern is provided on the roller surface of the hot rolling roller. In the present invention, the hot rolling roller preferably includes an upper heating roller and a lower heating roller, and the temperature of the hot rolling is preferably 80 to 120°C, more preferably 90 to 110°C. In a specific embodiment of the present invention, the temperature of the upper heating roller is preferably 115°C, 110°C or 120°C, and the temperature of the lower heating roller is preferably 110°C, 105°C or 115°C. The inter-roll pressure between the upper heating roller and the lower heating roller is preferably 25 to 100 bar, more preferably 50 bar, 58 bar or 48 bar. The pattern includes a dot pattern, a line pattern or a combined pattern. In a specific embodiment of the present invention, the pattern preferably includes a regular hexagonal geometric pattern, a leaf line pattern, a cartoon character line pattern, a dot pattern or a "sesame dot" pattern.

[0082] After obtaining the hot-rolled web, the present invention performs hydroentanglement after pre-hydroentanglement on the hot-rolled web to obtain the hydroentangled web; the hydroentanglement includes sequentially performing first rotary drum reverse entanglement, rotary drum forward entanglement, second rotary drum reverse entanglement and flat net forward entanglement; the first rotary drum reverse entanglement is to perform first hydroentanglement on the lower surface of the hot-rolled web on the rotating circumference of the drum, the rotary drum forward entanglement is to perform second hydroentanglement on the upper surface of the hot-rolled web on the rotating circumference of the drum, the second rotary drum reverse entanglement is to perform third hydroentanglement on the lower surface of the hot-rolled web on the rotating circumference of the drum, and the flat net forward entanglement is to perform fourth hydroentanglement on the upper surface of the hot-rolled web on the suction net curtain, and vacuum is simultaneously drawn on the lower surface of the hot-rolled web. In the present invention, the water pressure of the hydroentanglement head of the pre-hydroentanglement is preferably 0.5 to 60 Bar, and specifically preferably 10 Bar or 5 Bar. The water pressure of the first rotary drum reverse puncture water jet head is preferably 20-120 Bar, and is preferably 90 Bar, 80 Bar, 85 Bar, and 60 Bar. The water pressure of the rotary drum forward puncture water jet head is preferably 20-120 Bar, and is preferably 90 Bar, 80 Bar, 85 Bar, and 60 Bar. The water pressure of the second rotary drum reverse puncture water jet head is preferably 20-120 Bar, and is preferably 90 Bar, 80 Bar, 85 Bar, and 60 Bar. The water pressure of the flat net forward puncture water jet head is preferably 20-120 Bar, and is preferably 90 Bar, 80 Bar, 85 Bar, and 60 Bar.

[0083] The present invention performs pre-hydroentanglement treatment on the initially formed composite material; the first hydroentanglement head and the third hydroentanglement head cooperate with the first drum and the third drum respectively to hydroentangle the back side of the composite material; the second hydroentanglement head cooperates with the second drum, and the fourth hydroentanglement head cooperates with the suction net curtain to hydroentangle the front side of the composite material; the fourth hydroentanglement head cooperates with the suction net curtain to perform perforation treatment on the product, so as to further allow water molecules to more easily contact the cellulose fibers inside the composite material, thereby further improving the water absorption performance of the product.

[0084] After obtaining the spunlace web, the present invention dries the spunlace web and then rolls it up to obtain the multi-layer composite nonwoven material. In the present invention, the drying is oven drying, and the oven drying temperature is preferably 90 to 130°C, and more preferably 120°C, 110°C, 105°C, or 125°C.

[0085] The present invention provides a composite multi-layer nonwoven material prepared by the preparation method described in the above technical scheme, comprising a first layer structure, an intermediate layer structure and a second layer structure stacked in sequence; the first layer structure is formed by a first meltblown fiber web or a second spunbond fiber web; the intermediate layer structure is formed by a plurality of mixed-spray fiber webs and / or a plurality of carded fiber webs, and the second layer structure is formed by a second meltblown fiber web or a second spunbond fiber web.

[0086] The present invention provides a preparation system used in the preparation method described in the above technical solution, comprising a web-forming curtain, a web-forming system arranged above the web-forming curtain, the web-forming system comprising a first polymer melt-blown forming system and / or a polymer spunbond forming system, and also comprising a plurality of mixed-spray systems and / or a plurality of second combing systems; the mixed-spray system comprises at least one second polymer melt-blown forming system, one first combing system and one forming box;

[0087] A hot rolling device disposed downstream of the web-forming curtain, a first rotary drum disposed downstream of the hot rolling device, the first rotary drum rotating counterclockwise, a pre-wetting water jet disposed below the first rotary drum, and a first water jet disposed on the right side of the first rotary drum;

[0088] A second drum is arranged above the first drum; the second drum rotates clockwise, and a second water jet head is arranged on the left side and / or above the second drum;

[0089] a third drum disposed downstream of the first drum; the third drum rotates counterclockwise, and a third water jet head is disposed on the left side and / or below the third drum;

[0090] A suction net curtain disposed downstream of the third drum; a fourth water jet head disposed above the suction net curtain, and a suction device disposed below the suction net curtain;

[0091] A drying device is arranged downstream of the suction curtain, and a winding device is arranged downstream of the drying device.

[0092] In the present invention, the web forming system above the web forming curtain is provided with the number and arrangement order of the first polymer melt-blown forming system, the polymer spun-bonded forming system, the mixed-spraying system and the second combing system according to the layer structure of the composite multi-layer nonwoven material. The web forming system above the web forming curtain is preferably selectively operated or closed, so as to change the structure of the composite material.

[0093] As one or more embodiments of the present invention, the web-forming system above the web-forming curtain is provided with one or two first polymer melt-blowing forming systems according to the layer structure of the composite multi-layer nonwoven material.

[0094] As one or more embodiments of the present invention, the web-forming system above the web-forming curtain is provided with one or two polymer spunbond forming systems according to the layer structure of the composite multi-layer nonwoven material.

[0095] As one or more embodiments of the present invention, the web-forming system above the web-forming curtain is provided with one or two mixing spray systems according to the layer structure of the composite multi-layer nonwoven material.

[0096] As one or more embodiments of the present invention, the web-forming system above the web-forming curtain is provided with a second combing system according to the layer structure of the composite multi-layer nonwoven material.

[0097] In the present invention, the spinnerets of the first polymer melt-blown forming system and the second polymer melt-blown forming system preferably include a first spinneret, a second spinneret or a third spinneret;

[0098] A single row of first spinneret holes is arranged on the first spinneret plate, the first spinneret holes are inverted conical holes, the outer cone surface of the first spinneret holes is sleeved with first airflow stretching holes, the first airflow stretching holes are inverted conical holes and are coaxial with the first spinneret holes, the long fibers ejected from the first spinneret holes and the stretching gas ejected from the first airflow stretching holes converge at the apex, and the angle between the stretching gas and the long fibers is 30 to 70°.

[0099] The second spinneret is provided with a single row or multiple rows of second spinneret holes, the second spinneret holes are cylindrical holes, the outer circumference of the second spinneret holes is sleeved with second airflow drafting holes, the second airflow drafting holes are annular holes and are coaxial with the second spinneret holes. The angle between the second airflow ejected from the second airflow drafting holes and the filament stream ejected from the first spinneret holes is preferably less than 10°.

[0100] The third spinneret is provided with a single row or multiple rows of third airflow drafting holes, the third airflow drafting holes are cylindrical holes, the outer circumference of the third airflow drafting holes is sleeved with third spinneret holes, the third spinneret holes are annular holes and are coaxial with the third airflow drafting holes. The angle between the third airflow ejected from the third airflow drafting holes and the filament stream ejected from the first spinneret holes is preferably less than 10°.

[0101] In the present invention, the configuration form of the spinneret of the first polymer melt-blown forming system and the second polymer melt-blown forming system can be a "slit air knife" melt-blown type or a "coaxial" melt-blown type. The "slit air knife" melt-blown type is that two drafting gas flows converge to form a single airflow, and the drafting gas forms an angle of about 30-70° with the direction of the filament flow. When the polymer filaments leave the spinneret holes in the melt-blown mold, they are cooled and stretched by the air knife, and finally bonded to the mesh curtain. Each spinneret hole of the "coaxial" melt-blown type has an annular fluid release hole around it, and the drafting gas can form an angle of less than 10° with the direction of the filament flow, so that the substantially parallel airflows perform coaxial stretching on the polymer melt. When the configuration form of the melt-blown device is a "slit air knife" melt-blown type, the spinneret is a single row of holes; when the configuration form of the melt-blown device is a "coaxial" melt-blown type, the spinneret can be a single row of holes or multiple rows of holes, and the multiple rows of holes spinneret include 2 rows, 3 rows, 4 rows or more rows.

[0102] In the present invention, the drying device is preferably an oven, and the types of the oven include tunnel type, round screen type, infrared heating type, and finally the finishing device is used for finishing to give the wiping material a certain functionality.

[0103] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0104] Example 1

[0105] This embodiment follows Figure 1 The structure diagram of the device shown in FIG. 1 is used to prepare a multi-layer composite nonwoven material. The structure diagram of the prepared multi-layer composite nonwoven material is shown in FIG. Figure 2 As shown, the multi-layer composite nonwoven material prepared in this embodiment comprises, from top to bottom, a first meltblown layer, a middle water-absorbing layer, and a second meltblown layer.

[0106] The first and second melt-blown layers are thermoplastic materials polypropylene and hydrophilic masterbatch (purchased from Argus, model: HYL1047), which are respectively passed through a first polymer melt-blown molding system and a second polymer melt-blown molding system, and are melted, extruded, stretched, and cooled to form a polypropylene melt-blown fiber web; the first polymer melt-blown molding system and the second polymer melt-blown molding system adopt a "coaxial melt-blown" form, and the number of rows of spinnerets used is eight, wherein the raw materials used in the first polymer melt-blown molding system and the second polymer melt-blown molding system: the mass ratio of polypropylene to hydrophilic masterbatch is 95%:5%.

[0107] The middle water-absorbing layer is a bicomponent fiber of recycled cotton and orange peel (Lu Thai Textile Co., Ltd., a bicomponent chemical fiber), wherein the mass of the recycled cotton fiber accounts for 70% of the total mass of the middle water-absorbing layer, and the mass of the bicomponent fiber of orange peel accounts for 30% of the total mass of the middle water-absorbing layer; after the first combing system, the mixed fibers are combed into a relatively parallel fiber web, flatly laid between the first and second melt-blown layers, adsorbed by the mesh curtain, and transported to the hot rolling process with the first and second melt-blown layers for hot rolling.

[0108] The first and second meltblown fiber webs have a gram weight of 17.5 gsm respectively. Calculated by mass percentage, the total mass of the first and second meltblown fiber webs accounts for 50% of the entire composite fiber material; the middle water-absorbing layer fiber web has a gram weight of 35 gsm, which accounts for 50% of the entire composite fiber material according to mass percentage.

[0109] In the hot rolling process, the upper roller temperature is 115° C., the lower roller temperature is 110° C., and the pressure between the rollers is set to 50 bar; the pattern of the hot rolling roller is composed of a regular hexagonal geometric pattern.

[0110] The formed composite fiber web material is hydroentangled by the subsequent hydroentanglement reinforcement system and dried by the drying device. At the same time, during the hydroentanglement reinforcement process, the orange segment bicomponent fiber is opened by the impact of high-pressure water flow and decomposed into ultrafine fibers with a diameter of about 2 microns, which are entangled with the cotton fibers, thereby greatly enhancing the strength of the product.

[0111] The water pressure of the pre-water jet head is 10 Bar; the water pressure of the first to fourth water jet heads is 90 Bar; the drying device is a tunnel-type (flat mesh) hot air penetration drying device; the drying temperature is 120°C; the final product is wound and formed by a winding device to form a multi-layer composite non-woven material. Fig.19 This is a pattern effect diagram of the multi-layer composite nonwoven material prepared in Example 1 of the present invention.

[0112] Example 2

[0113] This embodiment follows Figure 3The structure diagram of the device shown in FIG. 1 is used to prepare a multi-layer composite nonwoven material. The structure diagram of the prepared multi-layer composite nonwoven material is shown in FIG. Figure 4 As shown, the multi-layer composite nonwoven material prepared in this embodiment is composed of a first melt-blown layer, a mixed-spray water-absorbing layer, and a second melt-blown layer from top to bottom;

[0114] The first and second melt-blown layers are thermoplastic materials polypropylene and hydrophilic masterbatch (purchased from Argus, model: HYL1047), which are respectively passed through the first polymer melt-blown molding system and the second polymer melt-blown molding system, and are melted, extruded, stretched, and cooled to form a polypropylene melt-blown fiber web; the first polymer melt-blown molding system and the second polymer melt-blown molding system adopt the form of "coaxial melt-blowing", and the number of rows of spinnerets used is eight, wherein the mass ratio of raw material polypropylene to hydrophilic masterbatch used in the first polymer melt-blown molding system and the second polymer melt-blown molding system is 95%:5%.

[0115] The mixed spray water-absorbing layer is composed of a third melt-blown layer, a fourth melt-blown layer and a cotton fiber web combed by a first combing system, and mixed spraying is performed in a forming box; the third melt-blown layer and the fourth melt-blown layer are thermoplastic materials polypropylene and hydrophilic masterbatch, which are melted, extruded, stretched and cooled through a third polymer melt-blown molding system and a fourth polymer melt-blown molding system to form polypropylene melt-blown fibers; the third polymer melt-blown molding system and the fourth polymer melt-blown molding system adopt the form of "coaxial melt-blowing", and the number of rows of spinnerets used is fourteen rows, wherein the mass ratio of polypropylene and hydrophilic masterbatch (purchased by Argus, model: HYL1047) used in the third polymer melt-blown molding system and the fourth polymer melt-blown molding system is 98%:2%, and the cotton fiber web combed by the combing system is combined with each other in the forming box.

[0116] The mixed spray absorbent layer is formed in the forming box, laid flat on the mesh curtain between the first and second meltblown layers, and sent to the hot rolling process by the mesh curtain for hot rolling; the first and second meltblown fiber webs have a gram weight of 2gsm respectively; the fiber web formed by the third and fourth meltblown fibers in the mixed spray absorbent has a gram weight of 8gsm respectively, and the weight of the cotton fiber web after combing by the first combing system is 40gsm; the outer fiber web of the composite material (the total mass of the first and second meltblown layers) accounts for 6.67% of the entire composite fiber material according to mass percentage, and the middle mixed spray absorbent layer accounts for 93.33% of the entire composite material.

[0117] In the hot rolling process, the temperature of the upper hot rolling roll is 110° C., the temperature of the lower hot rolling roll is 105° C., and the pressure between the rolls is set to 58 bar; the pattern of the hot rolling roll is composed of a leaf line pattern.

[0118] The formed composite fiber web material is hydroentangled by the subsequent hydroentanglement reinforcement system and dried by the drying device; wherein the water pressure of the pre-hydroentanglement hydroentanglement head is 5 Bar; the water pressure of the first to fourth hydroentanglement heads is 80 Bar; the drying device is a round mesh hot air penetration drying equipment, the temperature is set to 110°C, and the drying treatment is performed; the final product is wound and formed by a winding device to form a multi-layer composite non-woven material.

[0119] Example 3

[0120] This embodiment follows Figure 5 The structure diagram of the device shown in FIG. 1 is used to prepare a multi-layer composite nonwoven material. The structure diagram of the prepared multi-layer composite nonwoven material is shown in FIG. Figure 6 As shown, the multi-layer composite nonwoven material prepared in this embodiment is composed of a first melt-blown layer, a first mixed-blown water-absorbing layer, a second mixed-blown water-absorbing layer, and a second melt-blown layer from top to bottom.

[0121] The first and second melt-blown layers are thermoplastic materials polypropylene, hydrophilic masterbatch (purchased from Argus, model: HYL1047) and biodegradable masterbatch (Hubei Jinlong Nonwoven Fabric Co., Ltd., PLM v3.2.14a), which are respectively passed through a first polymer melt-blown molding system and a second polymer melt-blown molding system, and are melted, extruded, stretched and cooled to form a polypropylene melt-blown fiber web; the first polymer melt-blown molding system and the second polymer melt-blown molding system adopt the form of "coaxial melt-blowing", and the number of rows of spinnerets used is eight rows, wherein the mass ratio of raw materials polypropylene: hydrophilic masterbatch (purchased from Argus, model: HYL1047): biodegradable masterbatch (Hubei Jinlong Nonwoven Fabric Co., Ltd., PLM v3.2.14a) used in the first polymer melt-blown molding system and the second polymer melt-blown molding system is 93%:6%:1%.

[0122] The first mixed spray water-absorbing layer is formed by mixed spraying the third melt-blown layer and the cotton fiber web combed by the first combing system in the first forming box, and the second mixed spray water-absorbing layer is formed by mixed spraying the fourth melt-blown layer and the cotton fiber web combed by the second combing system in the second forming box; the third melt-blown layer and the fourth melt-blown layer are thermoplastic materials polypropylene, hydrophilic masterbatch (purchased by: Argus, model: HYL1047) and biodegradable masterbatch (Hubei Jinlong Nonwoven Fabric Co., Ltd., PLM v3.2.14a) through the third polymer melt-blown molding system and the fourth polymer melt-blown molding system, through melting, extrusion, drawing, cooling to form polypropylene melt-blown fibers, the third polymer melt-blown molding system and the fourth polymer melt-blown molding system adopt the form of "coaxial melt-blowing", and the number of rows of the spinneret used is fourteen rows, wherein the polypropylene used in the third polymer melt-blown molding system and the fourth polymer melt-blown molding system: hydrophilic masterbatch (purchased by: Argus, model: HYL1047): biodegradable masterbatch (Hubei Jinlong Nonwoven Fabric Co., Ltd., PLM v3.2.14a) v3.2.14a) has a mass ratio of 93%:6%:1%, and the first cotton fiber web and the second cotton fiber web combed by the first combing web system and the second combing web system in the first forming box and the second forming box are combined with each other; the first mixed spray absorbent layer and the second mixed spray absorbent layer come out of the first forming box and the second forming box, are laid on the web curtain between the first and the second meltblown layers, and are sent to the hot rolling process by the web curtain for hot rolling; the first and the second meltblown fiber webs have a gram weight of 2.5gsm respectively; the third and the fourth meltblown fiber webs have a gram weight of 7.5gsm respectively, and the intermediate short fiber webs (the first cotton fiber web and the second cotton fiber web) have a gram weight of 18.5gsm respectively; wherein the outer fiber web of the composite material (the first and the second meltblown fiber webs) accounts for 8.8% of the entire composite fiber material according to the mass percentage, and the intermediate mixed spray absorbent layer (the first mixed spray absorbent layer and the second mixed spray absorbent layer) accounts for 91.2% of the entire composite material.

[0123] In the hot rolling process, the upper roller temperature is 120° C., the lower roller temperature is 115° C., and the pressure between the rollers is set to 48 bar; the pattern of the hot rolling roller is composed of cartoon character line patterns.

[0124] The formed composite fiber web material is subjected to hydroentanglement reinforcement by a subsequent hydroentanglement reinforcement system and is dried by a drying device; wherein the water pressure of the pre-hydroentanglement hydroentanglement head is 10 Bar; the water pressure of the first to fourth hydroentanglement heads is 85 Bar; the drying device is a round mesh hot air penetration drying device, the temperature of which is set to 105°C for drying; the final product is wound and formed by a winding device to form a multi-layer composite non-woven material.

[0125] Example 4

[0126] This embodiment follows Figure 7 The structure diagram of the device shown in FIG. 1 is used to prepare a multi-layer composite nonwoven material. The structure diagram of the prepared multi-layer composite nonwoven material is shown in FIG. Figure 8 As shown, the multi-layer composite nonwoven material prepared in this embodiment comprises, from top to bottom, a first spunbond layer, a first mixed spray absorbent layer, a second mixed spray absorbent layer, and a second spunbond layer.

[0127] The first and second spunbond layers are thermoplastic materials polypropylene, hydrophilic masterbatch (purchased from Argus, model: HYL1047) and biodegradable masterbatch (Hubei Jinlong Nonwoven Fabric Co., Ltd., PLM v3.2.14a), which are formed into a first polypropylene spunbond fiber web and a second polypropylene spunbond fiber web through a first polymer spunbond molding system and a second polymer spunbond molding system through melting, extrusion, cooling and drawing; wherein the mass ratio of polypropylene: hydrophilic masterbatch (purchased from Argus, model: HYL1047): biodegradable masterbatch (Hubei Jinlong Nonwoven Fabric Co., Ltd., PLM v3.2.14a) in the first polymer spunbond molding system and the second polymer spunbond molding system is 93%:6%:1%.

[0128] The first mixed spray water-absorbing layer is formed by mixed spraying of the third melt-blown layer and the cotton fiber web combed by the first combing system in the first forming box, and the second mixed spray water-absorbing layer is formed by mixed spraying of the fourth melt-blown layer and the cotton fiber web combed by the second combing system in the second forming box; the third melt-blown layer and the fourth melt-blown layer are thermoplastic materials polypropylene, hydrophilic masterbatch (purchased by: Argus, model: HYL1047) and biodegradable masterbatch (Hubei Jinlong Nonwoven Fabric Co., Ltd., PLM v3.2.14a) through the third polymer melt-blown molding system and the fourth polymer melt-blown molding system, through melting, extrusion, drawing, cooling to form polypropylene melt-blown fibers, the third polymer melt-blown molding system and the fourth polymer melt-blown molding system adopt the form of "coaxial melt-blowing", and the number of rows of the spinnerets used is fourteen rows, wherein the third polymer melt-blown molding system and the third polymer melt-blown molding system polypropylene: hydrophilic masterbatch (purchased by: Argus, model: HYL1047): biodegradable masterbatch (Hubei Jinlong Nonwoven Fabric Co., Ltd., PLM v3.2.14a) v3.2.14a) has a mass ratio of 93%:6%:1%, and the first cotton fiber web combed by the first carding web system and the second cotton fiber web combed by the second carding web system in the first forming box and the second forming box are combined with each other; the first mixed spray absorbent layer and the second mixed spray absorbent layer come out of the first forming box and the second forming box, are laid flat between the bottom spunbond layer and the top spunbond layer, and are transmitted to the hot rolling process by the transmission mesh curtain for hot rolling treatment; the gram weight of the bottom spunbond layer fiber web is 10gsm, and the gram weight of the top spunbond fiber web is 10gsm, and the first and second melts are The gram weight of the sprayed fiber web is 7.5gsm, and the gram weight of the two layers of intermediate short fiber web (the first cotton fiber web and the second cotton fiber web) is 18.5gsm. The outer fiber web of the composite material (the first spunbond layer and the second spunbond layer) accounts for 27.8% of the entire composite fiber material according to the mass percentage, and the intermediate mixed spray absorbent layer (the first mixed spray absorbent layer and the second mixed spray absorbent layer) accounts for 72.2% of the entire composite material; the hot rolling process has a hot rolling upper roller temperature of 120°C, a lower roller temperature of 115°C, and a roller pressure of 48 bar; the pattern of the hot rolling roller is a dot pattern.

[0129] The formed composite fiber web material is subjected to hydroentanglement reinforcement by a subsequent hydroentanglement reinforcement system and is dried by a drying device; wherein the water pressure of the pre-hydroentanglement hydroentanglement head is 10 Bar; the water pressure of the first to fourth hydroentanglement heads is 85 Bar; the drying device is a round mesh hot air penetration drying device, the temperature of which is set to 105°C for drying; the final product is wound and formed by a winding device to form a multi-layer composite non-woven material.

[0130] Example 5

[0131] This embodiment follows Fig. 9 The structure diagram of the device shown in FIG. 1 is used to prepare a multi-layer composite nonwoven material. The structure diagram of the prepared multi-layer composite nonwoven material is shown in FIG. Fig.10 As shown, the multi-layer composite nonwoven material prepared in this embodiment comprises, from top to bottom, a first spunbond layer, a first mixed spray absorbent layer, a second mixed spray absorbent layer, and a second meltblown layer.

[0132] The first spunbond layer is a thermoplastic material polypropylene, a hydrophilic masterbatch (purchased from Argus, model: HYL1047), and a soft masterbatch (Zhejiang Jinchun Polymer Materials Co., Ltd., 5068M), which are respectively passed through a first polymer spunbond molding system, and are melted, extruded, cooled, and stretched to form a polypropylene spunbond fiber web; wherein the mass ratio of polypropylene, hydrophilic masterbatch, and soft masterbatch in the first polymer spunbond molding system is 90%:5%:5%.

[0133] The second melt-blown layer is a thermoplastic material polypropylene and a hydrophilic masterbatch (purchased from Argus, model: HYL1047), which are melted, extruded, stretched and cooled through a second polymer melt-blown molding system to form a polypropylene melt-blown fiber web; wherein the mass ratio of polypropylene to hydrophilic masterbatch is 95%:5%; the second polymer melt-blown molding system adopts a "coaxial melt-blown" form, and the number of rows of the spinneret used is eight.

[0134] The first mixed spray water-absorbing layer is formed by the third melt-blown layer and the cotton fiber web combed by the first combing system, which are mixed and sprayed in the first forming box, and the second mixed spray water-absorbing layer is formed by the fourth melt-blown layer and the cotton fiber web combed by the second combing system, which are mixed and sprayed in the second forming box; the third melt-blown layer and the fourth melt-blown layer are thermoplastic materials polypropylene, hydrophilic masterbatch (purchased from Argus, model: HYL1047) and biodegradable masterbatch (Hubei Jinlong Nonwoven Fabric Co., Ltd., PLM v3.2.14a) The third polymer melt-blown forming system and the fourth polymer melt-blown forming system are used to form polypropylene melt-blown fibers through melting, extrusion, drawing and cooling. The third polymer melt-blown forming system and the fourth polymer melt-blown forming system adopt the form of "coaxial melt-blowing". The number of rows of spinnerets used is fourteen. The mass ratio of polypropylene to hydrophilic masterbatch (purchased by: Argus, model: HYL1047) in the third polymer melt-blown forming system and the fourth polymer melt-blown forming system is 95%:5%. The first cotton fiber web combed by the first carding web system and the second cotton fiber web combed by the second carding web system are combined with each other in the first molding box and the second molding box; the first mixed spray water-absorbing layer and the second mixed spray water-absorbing layer are formed by the first molding box and the second molding box. The fiber web of the bottom spunbond layer has a gram weight of 10 gsm, the gram weight of the top meltblown fiber web is 10 gsm, the gram weight of the third and fourth meltblown fiber webs are 8 gsm respectively, and the gram weight of the intermediate short fiber webs are 20 gsm respectively, wherein the outer fiber web of the composite material (the first spunbond layer and the second meltblown layer) accounts for 26.3% of the entire composite fiber material according to the mass percentage, and the intermediate mixed spray water-absorbing layer (the first mixed spray water-absorbing layer and the second mixed spray water-absorbing layer) accounts for 73.7% of the entire composite material; the upper roller temperature of the hot rolling process is 120°C, the lower roller temperature is 115°C, and the pressure between the rollers is set to 48 bar; the pattern of the hot rolling roller is composed of a dot pattern.

[0135] The formed composite fiber web material is subjected to hydroentanglement reinforcement by a subsequent hydroentanglement reinforcement system and is dried by a drying device; wherein the water pressure of the pre-hydroentanglement hydroentanglement head is 10 Bar; the water pressure of the first to fourth hydroentanglement heads is 85 Bar; the drying device is a round mesh hot air penetration drying device, the temperature of which is set to 105°C for drying; the final product is wound and formed by a winding device to form a multi-layer composite non-woven material.

[0136] Example 6

[0137] This embodiment follows Fig.11 The structure diagram of the device shown in FIG. 1 is used to prepare a multi-layer composite nonwoven material. The structure diagram of the prepared multi-layer composite nonwoven material is shown in FIG. Fig.12 As shown, the multi-layer composite nonwoven material prepared in this embodiment comprises, from top to bottom, a first spunbond layer, a middle water-absorbing layer, and a second spunbond layer.

[0138] The first and second spunbond layers are thermoplastic materials polypropylene and hydrophilic masterbatch (purchased from Argus, model: HYL1047), which are respectively passed through a first polymer spunbond molding system and a second polymer spunbond molding system, and are melted, extruded, cooled, and stretched to form a first polypropylene spunbond fiber web and a second polypropylene spunbond fiber web; wherein the mass ratio of polypropylene to hydrophilic masterbatch (purchased from Argus, model: HYL1047) in the first polymer spunbond molding system and the second polymer spunbond molding system is 95%:5%.

[0139] The middle absorbent layer is a mixture of recycled cotton and ES fibers. After the combing system, the mixed fibers are combed into a relatively parallel fiber web, laid flat between the first spunbond layer and the second spunbond layer, adsorbed by the mesh curtain, and transported to the hot rolling processing step together with the first and second spunbond layers.

[0140] The first and second spunbond fiber webs weigh 10 gsm respectively, accounting for 33.3% of the entire composite fiber material by mass percentage; the middle water-absorbing layer fiber web weighs 40 gsm, accounting for 66.7% of the entire composite fiber material by mass percentage.

[0141] In the hot rolling process, the upper roller temperature is 115° C., the lower roller temperature is 110° C., and the pressure between the rollers is set to 50 bar; the pattern of the hot rolling roller is composed of a regular hexagonal geometric pattern.

[0142] The formed composite fiber web material is hydroentangled by the subsequent hydroentanglement reinforcement system, punched by the fourth hydroentanglement head, and dried by the drying device; at the same time, the ES fiber passes through the hot air drying system, and is bonded with the surrounding short fibers to form a curled spatial shape; wherein the water pressure of the pre-hydroentanglement hydroentanglement head is 10Bar; the water pressure of the first to third hydroentanglement heads is 70Bar; the fourth hydroentanglement head is 85Bar; the drying device is a tunnel-type (flat mesh) hot air penetration drying equipment; the drying temperature is 120°C; the final product is wound and formed by a winding device to form a multi-layer composite non-woven material.

[0143] Example 7

[0144] This embodiment follows Fig.13 The structure diagram of the device shown in FIG. 1 is used to prepare a multi-layer composite nonwoven material. The structure diagram of the prepared multi-layer composite nonwoven material is shown in FIG. Fig.14 As shown, the multi-layer composite nonwoven material prepared in this embodiment comprises, from top to bottom, a first spunbond layer, a mixed spray absorbent layer, and a second spunbond layer.

[0145] The first and second spunbond layers are thermoplastic materials polypropylene, hydrophilic masterbatch (purchased from Argus, model: HYL1047), and elastomer masterbatch (Zhejiang Jinchun Polymer Materials Co., Ltd., high molecular weight EVA wax), which are respectively passed through a first polymer spunbond molding system and a second polymer spunbond molding system, and are melted, extruded, cooled, and stretched to form a polypropylene spunbond fiber web; wherein the mass ratio of polypropylene: hydrophilic masterbatch: elastomer masterbatch in the first polymer spunbond molding system and the second polymer spunbond molding system is 90%:5%:5%.

[0146] The mixed spray water-absorbing layer is composed of a third melt-blown layer, a fourth melt-blown layer and a combed cotton fiber web, which are mixed and sprayed in a forming box; the third melt-blown layer and the fourth melt-blown layer are thermoplastic materials polypropylene and hydrophilic masterbatch (purchased by: Argus, model: HYL1047) through a third polymer melt-blown molding system and a fourth polymer melt-blown molding system, through melting, extrusion, drawing, and cooling to form polypropylene melt-blown fibers, the third polymer melt-blown molding system and the fourth polymer melt-blown molding system adopt the form of "coaxial melt-blowing", and the number of rows of the spinneret used is eight rows, wherein the mass ratio of polypropylene to hydrophilic masterbatch (purchased by: Argus, model: HYL1047) in the third polymer melt-blown molding system and the fourth polymer melt-blown molding system is 98%:2%, and is combined with the cotton fiber web combed by the carding and web-forming system in the first molding box.

[0147] The mixed spray absorbent layer comes out of the first forming box, is spread on the mesh curtain between the first and second spunbond layers, and is sent to the hot rolling process by the mesh curtain for hot rolling; the first spunbond layer and the second spunbond layer have a gram weight of 10gsm respectively; the third meltblown layer and the fourth meltblown layer have a gram weight of 7.5gsm respectively, the intermediate short fiber web has a gram weight of 45gsm, and the total weight of the composite material is 80gsm.

[0148] In the hot rolling process, the temperature of the upper hot rolling roll is 110° C., the temperature of the lower hot rolling roll is 105° C., and the pressure between the rolls is set to 58 bar; the pattern of the hot rolling roll is composed of a leaf line pattern.

[0149] The formed composite fiber web material is hydroentangled by the subsequent hydroentanglement reinforcement system and dried by the drying device; wherein the water pressure of the pre-hydroentanglement hydroentanglement head is 10 Bar; the water pressure of the first to fourth hydroentanglement heads is 85 Bar; the drying device is a round mesh hot air penetration drying equipment, the temperature is set to 110°C, and the drying treatment is performed; the final product is wound and formed by a winding device to form a multi-layer composite non-woven material.

[0150] Example 8

[0151] This embodiment follows Fig.15 The structure diagram of the device shown in FIG. 1 is used to prepare a multi-layer composite nonwoven material. The structure diagram of the prepared multi-layer composite nonwoven material is shown in FIG. Fig.16 As shown, the multi-layer composite nonwoven material prepared in this embodiment comprises, from top to bottom, a first spunbond layer, a middle water-absorbing layer, and a second meltblown layer.

[0152] The spunbond layer is a thermoplastic material polypropylene and a hydrophilic masterbatch (purchased from Argus, model: HYL1047) which pass through a first polymer spunbond forming system, undergo melting, extrusion, cooling, and stretching to form a polypropylene spunbond fiber web; wherein the mass ratio of polypropylene to the hydrophilic masterbatch in the first polymer spunbond forming system is 92%:8%.

[0153] The meltblown layer is a thermoplastic material polypropylene and a hydrophilic masterbatch (purchased from Argus, model: HYL1047) which pass through a second polymer meltblown molding system, undergo melting, extrusion, drawing, and cooling to form a polypropylene meltblown fiber web; wherein the mass ratio of polypropylene to the hydrophilic masterbatch in the second polymer meltblown molding system is 95%:5%.

[0154] The middle water-absorbing layer is a mixture of recycled cotton and ES fibers. After the first combing system, the mixed fibers are combed into a relatively parallel fiber web, laid flat between the spunbond layer and the meltblown layer, adsorbed by the mesh curtain, and sent to the hot rolling processing step together with the spunbond layer and the meltblown layer.

[0155] The first spunbond layer has a grammage of 10 gsm, which accounts for 14.3% of the entire composite fiber material by mass percentage; the second meltblown layer has a grammage of 15 gsm, which accounts for 21.4% of the entire composite material by mass percentage; the intermediate water-absorbing layer fiber web has a grammage of 45 gsm, which accounts for 64.3% of the entire composite fiber material by mass percentage.

[0156] In the hot rolling process, the upper roller temperature is 120° C., the lower roller temperature is 110° C., and the pressure between the rollers is set to 48 bar; the pattern of the hot rolling roller is a “sesame dot” pattern.

[0157] The formed composite fiber web material is hydroentangled by the subsequent hydroentanglement reinforcement system and dried by the drying device; at the same time, the ES fiber passes through the hot air drying system, and is bonded with the surrounding short fibers to form a curled spatial shape; wherein the water pressure of the pre-hydroentanglement hydroentanglement head is 10 Bar; the water pressure of the first to fourth hydroentanglement heads is 60 Bar; the drying device is a tunnel-type (flat mesh) hot air penetration drying equipment; the drying temperature is 125°C; the final product is wound and formed by a winding device to form a multi-layer composite non-woven material.

[0158] Example 9

[0159] This embodiment follows Fig.17 The structure diagram of the device shown in FIG. 1 is used to prepare a multi-layer composite nonwoven material. The structure diagram of the prepared multi-layer composite nonwoven material is shown in FIG. Fig.18 As shown, the multi-layer composite nonwoven material prepared in this embodiment comprises, from top to bottom, a first spunbond layer, a mixed spray water-absorbing layer, and a second melt-blown layer.

[0160] The first spunbond layer is a thermoplastic material polypropylene, a hydrophilic masterbatch (purchased from Argus, model: HYL1047), and an elastomer masterbatch (Zhejiang Jinchun Polymer Materials Co., Ltd., high molecular weight EVA wax), which are respectively passed through a first polymer spunbond molding system, and are melted, extruded, cooled, and stretched to form a polypropylene spunbond fiber web; wherein the mass ratio of polypropylene: hydrophilic masterbatch: elastomer masterbatch in the first polymer spunbond molding system is 90%:5%:5%.

[0161] The second melt-blown layer is a thermoplastic material polypropylene and a hydrophilic masterbatch (purchased from Argus, model: HYL1047), which are respectively passed through a second polymer melt-blown molding system, melted, extruded, stretched, and cooled to form a polypropylene melt-blown fiber web; wherein the mass ratio of polypropylene to hydrophilic masterbatch (purchased from Argus, model: HYL1047) in the second polymer melt-blown molding system is 95%:5%.

[0162] The mixed spray water-absorbing layer is composed of a third melt-blown layer, a fourth melt-blown layer and a combed cotton fiber web, which are mixed and sprayed in a first molding box; the third melt-blown layer and the fourth melt-blown layer are thermoplastic materials polypropylene and hydrophilic masterbatch, which are melted, extruded, stretched and cooled through a third polymer melt-blown molding system and a fourth polymer melt-blown molding system to form polypropylene melt-blown fibers; the third polymer melt-blown molding system and the fourth polymer melt-blown molding system adopt the form of "coaxial melt-blown", and the number of rows of spinnerets used is eight, wherein the mass ratio of polypropylene to hydrophilic masterbatch (purchased by Argus, model: HYL1047) in the third polymer melt-blown molding system and the fourth polymer melt-blown molding system is 98%:2%, and the cotton fiber web combed by the carding web forming system is combined with each other in the first molding box; the mixed spray water-absorbing layer comes out of the first molding box, is laid on the web curtain between the first spunbond layer and the second melt-blown layer, and is sent to the hot rolling process by the web curtain for hot rolling.

[0163] The first spunbond layer has a gram weight of 10 gsm, which accounts for 11.1% of the entire composite fiber material by mass percentage; the second meltblown layer has a gram weight of 15 gsm, which accounts for 16.7% of the entire composite material by mass percentage; the middle water-absorbing layer fiber web has a gram weight of 65 gsm, which accounts for 72.2% of the entire composite fiber material by mass percentage; the total gram weight of the composite material is 90 gsm.

[0164] In the hot rolling process, the upper roller temperature is 115° C., the lower roller temperature is 105° C., and the pressure between the rollers is set to 58 bar; the pattern of the hot rolling roller is composed of a leaf line pattern.

[0165] The formed composite fiber web material is hydroentangled by the subsequent hydroentanglement reinforcement system and dried by the drying device; wherein the water pressure of the hydroentanglement head for pre-hydroentanglement is 8 Bar; the water pressure of the first to fourth hydroentanglement heads is 80 Bar; the drying device is a round mesh hot air penetration drying equipment, the temperature is set to 115°C, and the drying treatment is performed; the final product is wound and formed by a winding device to form a multi-layer composite non-woven material.

[0166] Comparative Example 1

[0167] The regenerated cotton fibers are processed into a web by a carding device, the carded fiber web is subjected to hydroentanglement reinforcement by a subsequent hydroentanglement reinforcement system, and is dried by a drying device; wherein the water pressure of the pre-hydroentanglement hydroentanglement head is 10 Bar; the water pressure of the first to fourth hydroentanglement heads is 85 Bar; the drying device is a round mesh hot air penetration drying device, the temperature is set to 115°C, and the drying process is performed; the final product is wound and formed by a winding device to form a pure cotton non-woven material.

[0168] Test Case

[0169] The nonwoven materials prepared in Examples 1 to 9 and Comparative Example 1 and a commercially available nonwoven material (Quanmianshidai - baby cotton wipes) were subjected to performance tests. The test results are shown in Table 1.

[0170] Table 1 Performance test results of Examples 1 to 9 comparing commercially available pure cotton spunlace fabrics and nonwoven materials made by combing and spunlace of recycled cotton fibers

[0171]

[0172] From the above embodiments, it can be known that the method provided by the present invention prepares the first fiber web layer and the second fiber web layer of the composite material by meltblowing or spunbonding as the two outermost surface layers of the composite material; at the same time, the short fibers with combability are carded into a web to obtain a carded fiber web, and the carded fiber web obtained by carding the short fibers is mixed with the filaments obtained by meltblowing to form a mixed fiber web, and the carded fiber web is used alone as the intermediate fiber web of the composite material as the intermediate water-absorbing layer in the composite material, or the carded fiber web and the mixed fiber web are used together as the intermediate fiber web of the composite material as the water-absorbing layer of the composite material; After the multi-layer fiber web of the "sandwich" structure is formed, the composite non-woven material is obtained after hot rolling, pre-spunlace, spunlace and drying. In the process of hot rolling for compounding the three-layer fiber web layer, the hot rolling roller is used to give the product a pattern. Since the filaments obtained from the thermoplastic polymer in the hot rolling process are melted, the clarity of the pattern effect given in the hot rolling composite molding process will be better; then the spunlace method is used to make the filaments and the water-absorbent staple fibers in the product more tightly entangled and mixed, and the obtained multi-layer composite non-woven material has high strength, good water absorption performance, less fluff on the surface of the fabric, and high surface density.

[0173] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a multi-layer composite nonwoven material, characterized in that: The following steps are involved: Performing a first melt-blowing or a first spun-bonding process on a first raw material to obtain a first web layer, wherein the first raw material includes a first thermoplastic polymer; An intermediate fiber web layer is prepared on the surface of the first fiber web layer, and the intermediate fiber web layer includes a plurality of stacked mixed fiber webs and / or a plurality of carded fiber webs; the preparation method of the mixed fiber web comprises the following steps: a first water-absorbent staple fiber is subjected to a first carding process to form a web, to obtain a first carded fiber web, a second raw material is subjected to a second melt-blowing process, and the obtained melt-blown filaments are mixed with the first carded fiber web to obtain a mixed fiber web; the second raw material includes a second thermoplastic polymer; the preparation method of the carded fiber web comprises the following steps: a second water-absorbent staple fiber is subjected to a second carding process to form a web; On the surface of the intermediate fiber web layer, a third raw material is subjected to a third melt-blowing or a second spun-bonding to form a second fiber web layer, thereby obtaining a multi-layer fiber web; the third raw material comprises a third thermoplastic polymer; The multi-layer web is hot-rolled by a hot-rolling roller to obtain a hot-rolled web, wherein the first web layer of the multi-layer web forms the lower surface of the hot-rolled web, and the second web layer of the multi-layer web forms the upper surface of the hot-rolled web; the hot-rolling is performed by a hot-rolling roller, and a pattern is arranged on the roller surface of the hot-rolling roller; The hot rolled web is pre-spunlaced and then spunlaced to obtain a spunlaced web; the spunlaced web includes sequentially performing first rotary drum reverse spunlacing, rotary drum forward spunlacing, second rotary drum reverse spunlacing and flat net forward spunlacing; the first rotary drum reverse spunlacing is to perform first spunlacing on the lower surface of the hot rolled web on the rotating circumference of the drum, the rotary drum forward spunlacing is to perform second spunlacing on the upper surface of the hot rolled web on the rotating circumference of the drum, the second rotary drum reverse spunlacing is to perform third spunlacing on the lower surface of the hot rolled web on the rotating circumference of the drum, and the flat net forward spunlacing is to perform fourth spunlacing on the upper surface of the hot rolled web on a suction net curtain, and vacuum is simultaneously drawn on the lower surface of the hot rolled web; The spunlace web is dried to obtain the multi-layer composite nonwoven material.

2. The preparation method according to claim 1, characterized in that: The diameters of the meltblown filaments obtained by the first meltblown, the second meltblown and the third meltblown and the spunbonded filaments obtained by the first spunbond and the second spunbond are independently 2 to 20 μm; the gram weights of the first web layer and the second web layer are independently 1 to 25 gsm; the total mass of the first web layer and the second web layer accounts for 5 to 60% of the mass of the multi-layer composite nonwoven material; The gram weight of the intermediate fiber web layer is 10 to 80 gsm; the mass of the intermediate fiber web layer accounts for 40 to 95% of the mass of the multi-layer composite nonwoven material.

3. The preparation method according to claim 1 or 2, characterized in that: The first thermoplastic polymer, the second thermoplastic polymer and the third thermoplastic polymer independently include one or more of polypropylene, polyethylene, polyester, nylon, polyurethane, polylactic acid and thermoplastic biodegradable plastics.

4. The preparation method according to claim 1 or 2, characterized in that: The first raw material further includes a first functional masterbatch, the mass ratio of the first thermoplastic polymer to the first functional masterbatch is (80-100): (0-20), and the first functional masterbatch is not 0; The second raw material further includes a second functional masterbatch, the mass ratio of the second thermoplastic polymer to the second functional masterbatch is (80-100): (0-20), and the second functional masterbatch is not 0; The third raw material further includes a third functional masterbatch, the mass ratio of the third thermoplastic polymer to the third functional masterbatch is (80-100): (0-20), and the third functional masterbatch is not 0; The first functional masterbatch, the second functional masterbatch and the third functional masterbatch independently include one or more of an elastomer masterbatch, a hydrophilic masterbatch, a soft masterbatch and a biodegradable masterbatch.

5. The preparation method according to claim 1 or 2, characterized in that: The first absorbent short fibers and the second absorbent short fibers independently include one or more of cotton fibers, cashmere fibers, hemp fibers, viscose fibers, and lyocell fibers; The first water-absorbent short fibers and the second water-absorbent short fibers are independently monocomponent short fibers or bicomponent short fibers, and the bicomponent short fibers include one or more of a sheath-core type, a side-by-side type, a trilobal type, and a segmented orange type; The length of the first water-absorbent short fibers and the second water-absorbent short fibers is 10 to 65 mm, and is not 10 mm.

6. The preparation method according to claim 1, characterized in that: The hot rolling rollers include an upper heating roller and a lower heating roller, the hot rolling temperature is 80-120° C., and the inter-roller pressure between the upper heating roller and the lower heating roller is 25-100 bar; The pattern includes a dot pattern, a line pattern or a combined pattern.

7. The preparation method according to claim 1, characterized in that: The water pressure of the pre-hydraulic needle jet is 0.5-60 Bar; the water pressure of the first rotary drum reverse needle jet, rotary drum forward needle jet, second rotary drum reverse needle jet and flat net forward needle jet are independently 20-120 Bar; The drying is oven drying, and the oven drying temperature is 90-130°C.

8. The composite multi-layer nonwoven material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: It includes a first layer structure, an intermediate layer structure and a second layer structure which are stacked in sequence; the first layer structure is formed by a first meltblown fiber web or a second spunbond fiber web; the intermediate layer structure is formed by a plurality of mixed-spray fiber webs and / or a plurality of carded fiber webs, and the second layer structure is formed by a second meltblown fiber web or a second spunbond fiber web.

9. The preparation system used in the preparation method according to any one of claims 1 to 7, characterized in that: It comprises a web-forming curtain, a web-forming system arranged above the web-forming curtain, the web-forming system comprises a first polymer melt-blowing forming system and / or a first polymer spunbond forming system, and also comprises a plurality of mixed-spraying systems and / or a plurality of second combing systems; each mixed-spraying system comprises at least one second polymer melt-blowing forming system, one first combing system and one forming box; A hot rolling device disposed downstream of the web-forming curtain, a first rotary drum disposed downstream of the hot rolling device, the first rotary drum being rotatable counterclockwise, a pre-wetting water jet head disposed below the first rotary drum, and a first water jet head disposed on the right side of the first rotary drum; A second rotating drum is arranged above the first rotating drum; the second rotating drum can rotate clockwise, and a second water jet head is arranged on the left side and / or above the second rotating drum; a third drum disposed downstream of the first drum; the third drum rotates counterclockwise, and a third water jet head is disposed on the left side and / or below the third drum; A suction net curtain disposed downstream of the third drum; a fourth water jet head disposed above the suction net curtain, and a suction device disposed below the suction net curtain; A drying device is arranged downstream of the suction curtain, and a winding device is arranged downstream of the drying device.

10. The preparation system according to claim 9, characterized in that: The spinnerets of the first polymer melt-blown forming system and the second polymer melt-blown forming system include a first spinneret, a second spinneret or a third spinneret; The first spinneret is provided with a single row of first spinneret holes, the first spinneret holes are inverted conical holes, the outer cone surface of the first spinneret holes is sleeved with first airflow drafting holes, the first airflow drafting holes are inverted conical holes and are coaxial with the first spinneret holes, the long fibers ejected from the first spinneret holes and the drafting gas ejected from the first airflow drafting holes converge at the apex, and the angle between the drafting gas and the long fibers is 30-70°; The second spinneret is provided with a single row or multiple rows of second spinneret holes, the second spinneret holes are cylindrical holes, the outer circumference of the second spinneret holes is sleeved with second airflow drafting holes, the second airflow drafting holes are annular holes and are coaxial with the second spinneret holes; The third spinneret is provided with a single row or multiple rows of third airflow drafting holes, the third airflow drafting holes are cylindrical holes, the outer peripheral surface of the third airflow drafting holes is sleeved with third spinneret holes, the third spinneret holes are annular holes and are coaxial with the third airflow drafting holes.

Citation Information

Patent Citations

  • Method and device for preparing multi-layer composite non-woven fabric

    CN116837536A

  • Multi-layer composite non-woven material and preparation method thereof

    CN117283965A

Cited By

  • Non-woven composite material, preparation method and application thereof, and production device of non-woven composite material

    CN119189471A

  • A nonwoven composite material, a method for producing and using the same, and an apparatus for producing a nonwoven composite material

    CN119189471B

  • Diversion layer and preparation process and system thereof

    CN119567667A

  • Polylactic acid melt-blown fiber production and treatment process and device

    CN120138818A

  • Slightly-fragrant environment-friendly non-woven material as well as preparation method and application thereof

    CN120311402A