Sacrificial cathode material with reduced gas generation and lithium secondary battery including same
The use of lithium cobalt zinc oxide with controlled zinc doping in the cathode material addresses gas generation and capacity loss in lithium secondary batteries, enhancing battery stability and performance.
Patent Information
- Application Number
- JP2022580998
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-23
- Filing Date
- 2022-02-21
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2042-02-21
AI Technical Summary
Existing lithium secondary batteries face issues with irreversible capacity loss and gas generation due to unstable sacrificial cathode materials, leading to reduced performance and lifespan.
A sacrificial cathode material composed of lithium cobalt zinc oxide (Li x Co (1-y) Zn y O 4) with specific doping of zinc and adjusted electrical conductivity is used to reduce gas generation and enhance charge/discharge capacity.
The material effectively reduces oxygen gas production and improves battery stability and lifespan by maintaining high charge/discharge capacity and low resistance changes during cycling.
Smart Images

Figure 0007551212000005 
Figure 0007551212000004 
Figure 0007551212000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a sacrificial cathode material that is doped with zinc ions and has controlled electrical properties, thereby reducing the amount of gas generated during charging, and a lithium secondary battery including the same.
[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0024264, filed on February 23, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. [Background technology]
[0003] Recently, the demand for secondary batteries as an energy source has been increasing rapidly. Among such secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Graphite is mainly used as the negative electrode material for lithium secondary batteries, but since graphite has a small capacity per unit mass of 372 mAh / g, it is difficult to increase the capacity of lithium secondary batteries. For this reason, in order to increase the capacity of lithium secondary batteries, negative electrode materials that form intermetallic compounds with lithium, such as silicon, tin, and their oxides, have been developed and used as non-carbon-based negative electrode materials that have a higher energy density than graphite. However, such non-carbon-based negative electrode materials have a problem that although they have a large capacity, their initial efficiency is low, resulting in a large amount of lithium consumption during initial charging and discharging, and a large irreversible capacity loss.
[0005] In this regard, a method has been proposed to overcome the irreversible capacity loss of the negative electrode by using a material that can provide a source or reservoir of lithium ions for the positive electrode material and that is electrochemically active after the first cycle so as not to degrade the performance of the entire battery. Specifically, a method is known in which an oxide containing an excess amount of lithium, such as Li6CoO4, is applied to the positive electrode as a sacrificial positive electrode material or an irreversible additive (or overdischarge inhibitor).
[0006] However, such sacrificial cathode materials or irreversible additives have an unstable structure and may generate oxygen gas inside the battery due to oxidation during the battery activation stage as well as the subsequent charge and discharge process. The generated oxygen gas may induce volume expansion, which may be one of the main causes of deterioration of battery performance.
[0007] Therefore, there is a demand for the development of a sacrificial cathode material that reduces the amount of oxygen gas generated during the charge and discharge process of a battery and exhibits high charge and discharge capacity. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent Publication No. 10-2019-0059115 Summary of the Invention [Problem to be solved by the invention]
[0009] Therefore, an object of the present invention is to provide a sacrificial cathode material that generates a small amount of oxygen gas during the charge and discharge process of a battery and has a higher charge and discharge capacity, and a cathode and a lithium secondary battery including the same. [Means for solving the problem]
[0010] In order to solve the above problems, the present invention provides, in one embodiment, The present invention includes a lithium cobalt zinc oxide represented by the following chemical formula 1: Powder electrical conductivity is 1×10 -4 S / cm~1×10 -2 Provide a sacrificial cathode material that is S / cm:
[0011] [Chemical formula 1] Li x Co (1-y) Zinc y O4
[0012] In the above Chemical Formula 1, x and y are within the range of 5≦x≦7 and 0.05≦y≦0.5.
[0013] Specifically, y in Chemical Formula 1 may be 0.2≦y≦0.4.
[0014] The powder electrical conductivity of the sacrificial positive electrode material is 1×10 -3 S / cm~9×10 -3 It may be S / cm.
[0015] The sacrificial cathode material may also have a tetragonal structure with a space group of P42 / nmc.
[0016] In one embodiment, the present invention provides a method for producing a composition comprising: A positive electrode current collector; a positive electrode mixture layer on the positive electrode current collector, the positive electrode mixture layer including a positive electrode active material, a conductive material, an organic binder polymer, and a sacrificial positive electrode material; The sacrificial cathode material contains lithium cobalt zinc oxide represented by the following chemical formula 1, and has a powder electrical conductivity of 1×10 -4 S / cm~1×10 -2 Provide a cathode that is S / cm:
[0017] [Chemical formula 1] Li x Co (1-y) Zinc y O4
[0018] In the above Chemical Formula 1, x and y are within the range of 5≦x≦7 and 0.05≦y≦0.5.
[0019] In this case, the content of the sacrificial positive electrode material may be 0.001 to 5.0 parts by weight with respect to 100 parts by weight of the positive electrode active material.
[0020] The content of the conductive material may be 0.5 to 10 parts by weight with respect to 100 parts by weight of the entire positive electrode mixture layer.
[0021] The conductive material may contain one or more carbonaceous materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber.
[0022] The positive electrode active material may be a lithium transition metal composite oxide containing two or more elements selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), aluminum (Al), zinc (Zn), titanium (Ti), magnesium (Mg), chromium (Cr), and zirconium (Zr).
[0023] In addition, the positive electrode mixture layer may have an average thickness of 100 μm to 200 μm.
[0024] The positive electrode may have a change rate of resistance after 30 charge / discharge cycles of 10% or less compared to the resistance at the initial charge / discharge.
[0025] In one embodiment, the present invention provides an electrode assembly including the positive electrode described above.
[0026] In one embodiment, the present invention provides a lithium secondary battery including the electrode assembly. Effect of the Invention
[0027] The sacrificial cathode material according to the present invention includes a lithium cobalt metal oxide represented by Chemical Formula 1, which is doped with zinc at a specific range of fraction, and has a powder electrical conductivity controlled within a specific range, thereby reducing the generation of gas, particularly oxygen (O2) gas, generated during charging and discharging of a battery after an activation step, and realizing a high charge and discharge capacity, and thus has the advantage of being excellent in the effect of improving the stability and lifespan of a battery including the same. [Brief description of the drawings]
[0028] [Figure 1] 1 is a graph showing the amount of gas generated depending on the number of charge / discharge cycles (temperature condition: 45° C.) for sacrificial positive electrode materials with and without zinc (Zn) doping. [Diagram 2] 1 is a graph showing the amount of gas generated depending on the storage period (temperature condition: 60° C.) of sacrificial positive electrode materials with and without zinc (Zn) doping. [Diagram 3] 1 is a graph showing the gas components and amounts generated depending on the charge / discharge and storage period of a sacrificial positive electrode material with or without zinc (Zn) doping. [Figure 4] 1 is a graph showing the initial charge / discharge capacity of a sacrificial cathode material with or without zinc (Zn) doping. BEST MODE FOR CARRYING OUT THEINVENTION
[0029] Although the present invention can be modified in various ways and can have various embodiments, a specific embodiment will be described in detail in the detailed description.
[0030] However, it should be understood that this is not intended to limit the invention to the particular embodiment, but rather to include all modifications, equivalents, or alternatives falling within the spirit and scope of the invention.
[0031] In the present invention, the terms "comprise" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0032] In addition, in the present invention, when a part such as a layer, film, region, or plate is described as being "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part in between. Conversely, when a part such as a layer, film, region, or plate is described as being "under" the other part, this includes not only the case where it is "directly under" the other part, but also the case where there is another part in between. In addition, in the present application, being "located on" can include not only the case where it is located at the top, but also the case where it is located at the bottom.
[0033] The present invention will now be described in more detail.
[0034] Sacrificial cathode material In one embodiment, the present invention comprises: The present invention includes a lithium cobalt zinc oxide represented by the following chemical formula 1: Powder electrical conductivity is 1×10 -4 S / cm~1×10 -2 Provide a sacrificial cathode material that is S / cm:
[0035] [Chemical formula 1] Li x Co (1-y) Zinc y O4
[0036] In the above Chemical Formula 1, x and y are within the range of 5≦x≦7 and 0.05≦y≦0.5.
[0037] The sacrificial cathode material according to the present invention includes, as a main component, lithium cobalt metal oxide represented by Chemical Formula 1. Here, the term "main component" means that the sacrificial cathode material includes 80 wt% or more, 90 wt% or more, 95 wt% or more, or 97.5 wt% or more of the lithium cobalt metal oxide represented by Chemical Formula 1 based on the total weight of the sacrificial cathode material, and in some cases, it may mean that the entire sacrificial cathode material is made of the lithium cobalt metal oxide represented by Chemical Formula 1, i.e., 100 wt%.
[0038] The lithium cobalt metal oxide represented by the formula 1 has a structure in which zinc is doped at the cobalt site of the lithium cobalt oxide that releases a large amount of lithium ions, and the amount of zinc doped may be 5 to 50 mole fraction (i.e., 0.05≦y≦0.5), specifically, 10 to 50 mole fraction (0.1≦y≦0.5); 15 to 50 mole fraction (0.15≦y≦0.5); 15 to 45 mole fraction (0.15≦y≦0.45); 20 to 40 mole fraction (0.2≦y≦0.4); or 25 to 35 mole fraction (0.25≦y≦0.35). The present invention can reduce the structural twist of the lithium cobalt oxide by adjusting the amount of zinc doped to the above mole fraction range, thereby further improving the structural stability.
[0039] In addition, the lithium cobalt metal oxide represented by the formula 1 may have a tetragonal crystal structure, and may have a space group of P42 / nmc. Generally, lithium metal oxides having a tetragonal crystal structure have a twisted rhombohedral structure formed by cobalt and oxygen elements, and have a structurally unstable structure. Due to this structural instability, gases including oxygen gas are generated during charging after activation of the battery. However, the sacrificial cathode material of the present invention can exhibit an effect of reducing the amount of gas generated even if it contains the lithium metal oxide represented by the formula 1 having a tetragonal crystal structure.
[0040] The sacrificial positive electrode material is a lithium cobalt metal oxide represented by the chemical formula 1, and the lithium cobalt metal oxide is 1×10 -4 S / cm~1×10 -2 The powder may have a powder electrical conductivity of 1×10 S / cm. -4 S / cm~5×10 -3 S / cm; 5×10 -4 S / cm~1×10 -2 S / cm; 5×10 -4 S / cm~5×10 -3 S / cm; 8×10 -4 S / cm~9×10 -3 S / cm; 1×10 -3 S / cm~9×10-3 S / cm; 1×10 -3 S / cm~8×10 -3 S / cm; or 2.5×10 -3 S / cm~5.5×10 -3 The powder electrical conductivity of the sacrificial positive electrode material may be adjusted by the manufacturing conditions of the sacrificial positive electrode material, and by adjusting the powder electrical conductivity to the above range, the amount of gas generated during charging of the battery can be reduced and the charge / discharge capacity can be improved.
[0041] The sacrificial cathode material according to the present invention includes a lithium cobalt metal oxide represented by Chemical Formula 1, which is doped with zinc at a specific range of fraction, and has a powder electrical conductivity adjusted to a specific range, thereby reducing the generation of gas, particularly oxygen (O2) gas, generated in the electrode assembly during charging and discharging of the battery after the activation step, and realizing a high charge and discharge capacity, which is advantageous in that it has an excellent effect of improving the stability and lifespan of the battery including the same.
[0042] positive electrode In one embodiment, the present invention provides a method for producing a composition comprising: A positive electrode current collector; a positive electrode mixture layer on the positive electrode current collector, the positive electrode mixture layer including a positive electrode active material, a conductive material, an organic binder polymer, and a sacrificial positive electrode material; The sacrificial cathode material contains lithium cobalt zinc oxide represented by the following chemical formula 1, and has a powder electrical conductivity of 1×10 -4 S / cm~1×10 -2 Positive electrode in S / cm:
[0043] [Chemical formula 1] Li x Co (1-y) Zinc y O4
[0044] In the above Chemical Formula 1, x and y are within the range of 5≦x≦7 and 0.05≦y≦0.5.
[0045] The positive electrode according to the present invention has a structure in which a positive electrode composite layer is formed on a positive electrode current collector, and the positive electrode composite layer includes a sacrificial positive electrode material containing lithium cobalt metal oxide represented by Chemical Formula 1, which is produced by the production method of the present invention together with a positive electrode active material; a conductive material; and an organic binder polymer, and has a high charge / discharge capacity and is excellent in reducing gas, particularly oxygen (O2) gas, generated during charging and discharging of a battery.
[0046] Here, the positive electrode active material may be a lithium composite transition metal oxide containing two or more elements selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), aluminum (Al), zinc (Zn), titanium (Ti), magnesium (Mg), chromium (Cr) and zirconium (Zr). For example, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2) or a layered compound substituted with one or more transition metals; 1+x Mn 2-x Lithium manganese oxides such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxides such as Li2CuO2; vanadium oxides such as LiV3O8, LiFe3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi 1-x M x Lithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (where M=Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x=0.01 to 0.3); 2-x M x Lithium manganese composite oxide represented by Li2Mn3MO8 (wherein M=Co, Ni, Fe, Cr, Zn or Ta, and x=0.01 to 0.1) or Li2Mn3MO8 (wherein M=Fe, Co, Ni, Cu or Zn); LiNi x Mn 2-x Examples include lithium manganese oxides with a spinel structure represented by O4; LiMn2O4, in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion; disulfide compounds; and Fe2(MoO4)3.
[0047] The sacrificial positive electrode material may be included in an amount of 0.001 to 5.0 parts by weight relative to 100 parts by weight of the positive electrode active material. More specifically, the sacrificial positive electrode material may be included in an amount of 0.001 to 4.0 parts by weight, 0.001 to 3.0 parts by weight, 0.001 to 2.0 parts by weight, 0.001 to 1.0 parts by weight, 0.01 to 2.0 parts by weight, 0.05 to 2.0 parts by weight, 0.1 to 2.0 parts by weight, or 0.1 to 1.5 parts by weight relative to 100 parts by weight of the positive electrode active material.
[0048] The conductive material may be added in an amount of 1 to 20 parts by weight relative to 100 parts by weight of the positive electrode active material, and specifically, the conductive material may be added in an amount of 1 to 10 parts by weight, 1 to 5 parts by weight, 3 to 8 parts by weight, or 2 to 5 parts by weight relative to 100 parts by weight of the positive electrode active material.
[0049] Furthermore, such a conductive material is not particularly limited as long as it is conductive without inducing a chemical change in the battery, and examples of such conductive materials that can be used include graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0050] The organic binder polymer is a component that assists in binding between the active material and the conductive material and between the active material and the current collector, and may be added in an amount of 1 to 20% by weight relative to 100 parts by weight of the positive electrode active material. Specifically, the organic binder polymer may be added in an amount of 1 to 10 parts by weight, 1 to 5 parts by weight, 3 to 8 parts by weight, or 2 to 5 parts by weight relative to 100 parts by weight of the positive electrode active material.
[0051] Examples of such organic binder polymers include polyvinylidene fluoride (PVdF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diether polymer (EPDM), sulfonated EPDM, styrene-butylene rubber, fluororubber, and various copolymers.
[0052] In addition, the positive electrode may further include a filler for suppressing the expansion of the positive electrode in the positive electrode mixture layer in addition to the positive electrode active material, the conductive material, and the organic binder polymer, and such a filler is not particularly limited as long as it is a fibrous material that does not induce chemical changes in the battery. Specifically, the filler may be an olefin polymer such as polyethylene or polypropylene; or a fibrous material such as glass fiber or carbon fiber.
[0053] As an example, the positive electrode mixture layer is made of lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2) 100 parts by weight of sacrificial cathode material (Li6Co 0.7 Zinc 0.3 O4) 1 part by weight; acetylene black, which is a conductive material, 5 parts by weight; and binder (PVdF) 10 parts by weight.
[0054] The positive electrode mixture layer may have an average thickness of 100 μm to 200 μm, specifically, 120 μm to 180 μm; 140 μm to 170 μm; or 150 μm to 200 μm.
[0055] In addition, the positive electrode mixture layer may be a single layer or may have a multi-layer structure of two or more layers. When the positive electrode mixture layer has a multi-layer structure of two or more layers, the sacrificial positive electrode material contained in the positive electrode mixture layer may have different contents; the positive electrode active material, conductive material, and binder may be the same or different in type and / or content.
[0056] As an example, the positive electrode mixture layer may have a two-layer structure in which a first mixture layer and a second mixture layer are located on a positive electrode current collector, and the first mixture layer is made of lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2) 100 parts by weight of sacrificial cathode material (Li6Co 0.7 Zinc 0.3 O4) 1 part by weight; acetylene black as a conductive material 5 parts by weight; and binder (PVdF) 10 parts by weight. The second composite layer is made of lithium nickel cobalt manganese oxide (LiNi 0.6 Co 0.2 Mn 0.2 O2) 100 parts by weight of sacrificial cathode material (Li6Co 0.7 Zinc 0.3 O4) 2 parts by weight; acetylene black, which is a conductive material, 5 parts by weight; and binder (PVdF), 9 parts by weight.
[0057] In addition, the positive electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. can be used, and in the case of aluminum or stainless steel, it may be surface-treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode current collector can be formed with fine irregularities on the surface to increase the adhesive force of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the positive electrode current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the positive electrode to be manufactured.
[0058] In addition, the positive electrode according to the present invention has excellent electrical performance due to the above-mentioned composition. Specifically, the positive electrode has low electrode resistance at room temperature (23±2° C.), and even after repeated charging and discharging of the battery, the amount of change in electrode resistance is small, thereby improving the battery life.
[0059] For example, the positive electrode has a low resistance change rate of 10% or less after 30 charge / discharge cycles compared to the electrode resistance value at the initial charge / discharge (e.g., activation stage). For example, the positive electrode may have an electrode resistance change rate of 8% or less, 6% or less, 4% or less, or 3% or less after the initial charge / discharge and 30 charge / discharge cycles.
[0060] electrode assembly In one embodiment, the present invention provides an electrode assembly including the positive electrode described above.
[0061] The electrode assembly according to the present invention may have a structure including the above-mentioned positive electrode, negative electrode, and a separator interposed between the positive electrode and the negative electrode, and in some cases, the separator may be omitted.
[0062] Here, the negative electrode is prepared by applying a negative electrode active material onto a negative electrode current collector, drying and pressing the same, and may further selectively include the same conductive material, organic binder polymer, filler, etc. as described above, as necessary.
[0063] In addition, the negative electrode active material may be, for example, graphite having a perfect layered crystal structure such as natural graphite, soft carbon having a low crystalline layered crystal structure (graphene structure; a structure in which hexagonal honeycomb-shaped carbon planes are arranged in layers), hard carbon in which such a structure is mixed with a non-crystalline portion, carbon and graphite materials such as artificial graphite, expanded graphite, carbon fiber, non-graphitizable carbon, carbon black, carbon nanotubes, fullerene, and activated carbon; Li x Fe2O3(0≦x≦1), Li x WO2(0≦x≦1), Sn x Me 1-x Me' y O z(Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogens; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8), etc. metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; titanium oxides; lithium titanium oxides, etc. can be used.
[0064] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery. For example, copper, stainless steel, nickel, titanium, fired carbon, etc. can be used. In the case of copper or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. may be used. Also, similar to the positive electrode current collector, the negative electrode current collector can also form fine irregularities on its surface to strengthen the bonding force with the negative electrode active material, and various forms such as films, sheets, foils, nets, porous bodies, foams, non-woven bodies, etc. are possible. Further, the average thickness of the negative electrode current collector can be appropriately applied at 3 to 500 μm in consideration of the conductivity and total thickness of the manufactured negative electrode.
[0065] In addition, the separator is interposed between the positive electrode and the negative electrode, and an insulating thin film having high ion permeability and mechanical strength is used. The separator is not particularly limited as long as it is commonly used in the industry. Specifically, sheets or non-woven fabrics made of chemical-resistant and hydrophobic polypropylene; glass fibers; or polyethylene, etc. can be used. In some cases, a composite separator in which inorganic particles / organic particles are coated on a porous polymer substrate such as the sheet or non-woven fabric with an organic binder polymer may also be used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separator. Also, the pore diameter of the separator is on average 0.01 to 10 μm, and the thickness may be on average 5 to 300 μm.
[0066] Meanwhile, the electrode assembly may be wound in a jelly roll form and housed in a cylindrical battery, a prismatic battery, or a pouch-type battery, or may be housed in a pouch-type battery in a folded or stack-and-folded form, but is not limited thereto.
[0067] Lithium secondary battery In one embodiment, the present invention provides a lithium secondary battery including the above-mentioned electrode assembly.
[0068] The lithium secondary battery according to the present invention may have a structure in which the electrode assembly is impregnated with an electrolyte solution containing a lithium salt.
[0069] In this case, the lithium salt-containing electrolyte may be composed of an electrolyte and a lithium salt, and the electrolyte may be a non-aqueous organic solvent, an organic solid electrolyte, an inorganic solid electrolyte, or the like.
[0070] Examples of non-aqueous organic solvents that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran (franc), 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0071] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymeric materials containing ionic dissociation groups.
[0072] Examples of inorganic solid electrolytes that can be used include nitrides, halides, and sulfates of Li, such as Li3N, LiI, Li5Ni2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.
[0073] Lithium salts are substances that are easily dissolved in non-aqueous electrolytes, such as LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium 4-phenylboronate, imides, etc. can be used.
[0074] In addition, for the purpose of improving charge / discharge characteristics, flame retardancy, etc., the electrolyte may contain, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. In some cases, in order to impart non-flammability, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further contained, and in order to improve high-temperature storage characteristics, carbon dioxide gas may be further contained, or FEC (Fluoro-Ethylene Carbonate), PRS (Propene Sultone), etc. may be further contained.
[0075] Meanwhile, in one embodiment, the present invention provides a battery module including the above-mentioned secondary battery as a unit cell, and provides a battery pack including the battery module.
[0076] The battery pack can be used as a power source for medium- to large-sized devices that require high temperature stability, long cycle characteristics, and high rate characteristics. Specific examples of such medium- to large-sized devices include power tools that are driven by electric motors; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheeled vehicles, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts; and power storage systems, and more specifically, a hybrid electric vehicle (HEV) can be mentioned, but is not limited thereto.
[0077] The present invention will now be described in more detail with reference to examples and experimental examples.
[0078] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.
[0079] Examples 1 to 3 and Comparative Examples 1 to 5. Production of sacrificial cathode materials Lithium oxide (Li2O), cobalt oxide (CoO) and zinc oxide (ZnO) were put into a reactor and uniformly dry-mixed for about 30 minutes using a mixer. The raw material mixture was then placed in an electric furnace and fired at about 700±10°C for 10 hours under argon gas (Ar) conditions to obtain lithium cobalt oxide (Li6Co 1-x Zinc x O4).
[0080] At this time, the molar ratio of lithium oxide and cobalt oxide charged into the reactor was 1:3.0 to 3.03, and the molar ratio of cobalt oxide and zinc oxide was as shown in Table 1 below.
[0081] In addition, the surface resistance of each sacrificial cathode material due to the volume and pressure change was measured using a powder resistance characteristic measuring device using a 4-point probe method, and the powder electrical conductivity of the sacrificial cathode material was calculated using the measured volume and input mass. The results are shown in Table 1 below.
[0082] [Table 1]
[0083] Experimental example. In order to evaluate the performance of the sacrificial cathode material prepared according to the present invention, the following experiment was carried out.
[0084] a) Measurement of gas emission amount N-methylpyrrolidone solvent was poured into a homomixer, and the sacrificial cathode materials prepared in Examples 1 to 3 and Comparative Examples 1 to 5 and the cathode active material (LiNi 0.6 Co 0.2 Mn 0.2 O2), the modified silanol binder and the dispersant were added in a weight ratio of 70:28:1.7:0.3, and then mixed at 3,000 rpm for 60 minutes to prepare a pre-dispersion.
[0085] The content of the sacrificial cathode material is the cathode active material (LiNi 0.6 Co 0.2 Mn 0.2A pre-dispersion liquid prepared in an amount of 2 parts by weight per 100 parts by weight of O2) was mixed with the positive electrode active material, and the positive electrode active material mixed in N-methylpyrrolidone solvent, PVdF as a binder, and carbon black as a conductive material were added to a homomixer in a weight ratio of 96:1:3, and dispersed at 3,000 rpm for 80 minutes to prepare a positive electrode slurry. The prepared positive electrode slurry was applied to one side of an aluminum current collector, dried at 100°C, and rolled to prepare a positive electrode. At this time, the positive electrode was prepared so that the average thickness of the positive electrode composite layer was about 170 μm, and the total thickness of the positive electrode composite layer and the positive electrode current collector was about 200 μm.
[0086] A 2032-type coin cell was manufactured using the positive electrode and lithium metal counter electrode. A separator (thickness: about 16 μm) made of a porous polyethylene (PE) film was placed between the positive electrode and the lithium metal counter electrode, and an electrolyte was injected to manufacture a coin cell in the form of a half cell.
[0087] In this case, the electrolyte used was a mixed solution of ethylene carbonate (EC):ethyl methyl carbonate (EMC) = 3:7 (volume ratio), lithium hexafluorophosphate (LiPF6, 0.7M), lithium bis(fluorosulfonyl)imide (LiFSI, 0.5M), lithium tetrafluoroborate (LiBF4, 0.2 wt%), vinyl carbonate (VC, 2 wt%), 1,3-propane sultone (PS, 0.5 wt%), and ethylene sulfate (Esa, 1 wt%).
[0088] The manufactured coin cells were charged and discharged once at 25°C and 4.5C / 1.5C to perform formation, and then charged and discharged 50 times at 45°C and 1.5C / 1.5C to analyze the amount of gas generated during each charge and discharge, and the amount and composition of gas generated during storage at 60°C for 4 weeks. The results are shown in Table 2 and Figures 1 to 3 below.
[0089] [Table 2]
[0090] As shown in Table 2 and Figures 1 to 3, the sacrificial cathode material prepared according to the present invention is a lithium cobalt oxide doped with zinc (Zn) at a specific molar fraction, and the powder electrical conductivity is adjusted to a specific range, so that the amount of gas generated during the activation stage as well as subsequent charging and discharging of the battery is reduced. Specifically, the battery of Example 2 showed a 16% reduction in gas generation during the activation stage and a 75% reduction in gas generation after 50 charge and discharge cycles compared to the battery of Comparative Example 1, which used a sacrificial cathode material not doped with zinc. In addition, the battery of Example 2 was confirmed to show an 85% reduction in gas generation during storage for 4 weeks compared to the battery of Comparative Example 1.
[0091] From these results, it can be seen that the sacrificial cathode material according to the present invention is doped with zinc at a specific molar fraction, and the powder electrical conductivity is controlled, thereby reducing the amount of gas generation.
[0092] b) Evaluation of electrical performance A coin cell in the form of a half-cell was fabricated using the same method as that used for measuring the amount of gas released, and E2DVC was used as the electrolyte. Here, "E2DVC" refers to a type of carbonate-based electrolyte, a solution in which lithium hexafluorophosphate (LiPF6, 1.0M) and vinyl carbonate (VC, 2% by weight) are mixed with a mixture of ethylene carbonate (EC): dimethyl carbonate (DMC): diethyl carbonate (DEC) = 1:1:1 (volume ratio).
[0093] The fabricated coin cells were formed by charging and discharging once at 400mAh / 144mAh at 25°C, and then charged and discharged 30 times at 200mAh / 200mAh at 25°C to measure the electrode resistance and initial charge capacity of each coin cell at the initial stage and after 30 charge / discharge cycles. The electrode resistance change rate was calculated from the measured electrode resistance values before and after charge / discharge, and the calculated results and the measured initial charge capacity are shown in Table 3 and Figure 4 below.
[0094] [Table 3]
[0095] As shown in Table 3, the sacrificial cathode material prepared according to the present invention has the effect of improving the performance of the battery.
[0096] Specifically, it was confirmed that the electrode resistance of the battery including the sacrificial cathode material of the embodiment changed to 10% or less even after 30 charge / discharge cycles. This means that the degree to which the battery life is reduced as the number of charge / discharge cycles of the battery increases is improved. In addition, it was confirmed that the battery including the sacrificial cathode material of the embodiment had a high initial charge capacity of 690mAh or more, whereas the battery including the sacrificial cathode material of the comparative example had a low initial charge capacity of less than 680mAh. In addition, the batteries including the sacrificial cathode materials of Comparative Examples 1 and 2 showed a high initial charge capacity of more than 700mAh, but the electrode resistance increased as charge / discharge cycles were repeated, and it was confirmed that the electrode resistance increased by more than 15% after 30 charge / discharge cycles.
[0097] From these results, it can be seen that the sacrificial cathode material according to the present invention is excellent in improving the stability and lifespan of a battery containing the same because the sacrificial cathode material according to the present invention is doped with zinc at a specific molar fraction and the powder electrical conductivity is controlled to improve the electrical performance of the battery.
[0098] Although the present invention has been described above with reference to preferred embodiments, it will be understood that a person skilled in the art or having ordinary knowledge in the art can make various modifications and variations to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.
[0099] Therefore, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
Claims
1. The present invention includes a lithium cobalt zinc oxide represented by the following chemical formula 1: Powder electrical conductivity is 1 x 10 -4 S / cm to 1×10 -2 S / cm, [Chemical formula 1] Li x Co (1-y) Zhn y O 4 In the above formula 1, x and y are 5≦x≦7 and 0.05≦y≦0.
5.
2. The sacrificial cathode material of claim 1 , wherein y in Formula 1 satisfies 0.2≦y≦0.
4.
3. The powder electrical conductivity of the sacrificial positive electrode material is 1×10 -3 S / cm to 9 x 10 -3 2. The sacrificial cathode material of claim 1, wherein the sacrificial cathode material has a conductivity of 1.5 S / cm.
4. The sacrificial cathode material has a space group of P4 2 2. The sacrificial cathode material of claim 1 having a tetragonal structure where Mn is 0.1-0.
25.
5. A positive electrode current collector; a positive electrode mixture layer on the positive electrode current collector, the positive electrode mixture layer including a positive electrode active material, a conductive material, an organic binder polymer, and a sacrificial positive electrode material; The sacrificial cathode material contains lithium cobalt zinc oxide represented by the following chemical formula 1, and has a powder electrical conductivity of 1×10 -4 S / cm to 1×10 -2 S / cm, [Chemical formula 1] Li x Co (1-y) Zhn y O 4 In the above Chemical Formula 1, x and y are 5≦x≦7 and 0.05≦y≦0.
5.
6. The positive electrode according to claim 5, wherein the content of the sacrificial positive electrode material is 0.001 to 5.0 parts by weight per 100 parts by weight of the positive electrode active material.
7. The positive electrode according to claim 5, wherein the content of the conductive material is 0.5 to 10 parts by weight per 100 parts by weight of the entire positive electrode mixture layer.
8. 6. The positive electrode according to claim 5, wherein the conductive material comprises one or more carbonaceous materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber.
9. 6. The positive electrode according to claim 5, wherein the positive electrode active material is a lithium transition metal oxide containing two or more elements selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), aluminum (Al), zinc (Zn), titanium (Ti), magnesium (Mg), chromium (Cr), and zirconium (Zr).
10. The positive electrode according to claim 5, wherein the positive electrode mixture layer has an average thickness of 100 μm to 200 μm.
11. The positive electrode according to claim 5 , wherein a rate of change in resistance value after 30 charge / discharge cycles compared to a resistance value at an initial charge / discharge cycle is 10% or less.
12. An electrode assembly comprising the positive electrode according to claim 5 .
13. A lithium secondary battery comprising the electrode assembly according to claim 12.
Citation Information
Patent Citations
High-power lithium secondary battery with improved power density characteristics
JP2014513409A
Lithium metal oxide particles coated with a mixture of core material elements and one or more metal oxides.
JP2014523840A
Positive active material for rechargeable lithium battery and rechargeable lithium battery including same
KR1020130079109A
Irreversible Additive Comprised in Cathode Material for Lithium Secondary Battery, Preparing Method thereof, and Cathode Material Comprising the Same
KR1020190059115A
Nonaqueous-electrolyte secondary battery and method for manufacturing nonaqueous-electrolyte secondary battery