Method of melting raw materials in an electric furnace

By switching to submerged arc heating when the carbon concentration in molten steel reaches 0.80 mass% or less, the method addresses nitrogen absorption issues in steel production, enhancing steel quality and reducing defects.

JP7551261B2Active Publication Date: 2024-09-17KOBE STEEL LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2021208484
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-22
Publication Date
2024-09-17
Estimated Expiration
2041-12-22

AI Technical Summary

Technical Problem

Existing methods for producing steel in electric arc furnaces face challenges in suppressing nitrogen absorption into molten steel, leading to increased raw material costs, yield reduction, and defects due to nitrogen absorption, as they do not effectively control carbon concentration and slag formation during the melting process.

Method used

A method that involves using carbon-containing reduced iron as a raw material in an electric arc furnace, switching from open arc heating to submerged arc heating when the carbon concentration in molten steel reaches 0.80 mass% or less to generate slag and cover the molten steel, thereby preventing nitrogen absorption.

Benefits of technology

This approach effectively reduces nitrogen absorption in molten steel to less than 50 ppm, improving steel quality by preventing defects such as wrinkles and cracks during subsequent processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551261000018
    Figure 0007551261000018
  • Figure 0007551261000016
    Figure 0007551261000016
  • Figure 0007551261000015
    Figure 0007551261000015
Patent Text Reader

Abstract

To provide a raw material melting method in an electric furnace capable of preventing nitrogen absorption of a molten steel by covering by generating slug by performing submerged arc heating in a low concentration region of a carbon concentration in the molten steel, when manufacturing the molten steel by dissolving with an arc type electric furnace, with reduced iron containing carbon as a raw material.SOLUTION: A raw material melting method in an electric furnace 1 of the present invention, when producing a molten steel M with an arc type electric furnace 1, in a raw material melting method in the electric furnace 1 that melts by heating reduced iron R containing carbon as a raw material, in a state where a carbon concentration of the molten steel generated by heating is 0.80 mass% or less, the submerged arc heating is performed to melt the raw material R.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a technique relating to the operation of an electric furnace, and more particularly to a technique for preventing nitrogen absorption by molten steel when melting reduced iron. [Background technology]

[0002] Conventionally, when producing steel in an electric furnace, iron sources such as scrap and reduced iron are charged into the furnace together with flux, and the iron sources are heated and melted by an electric arc. After the iron sources are fully melted, dephosphorization is performed by blowing oxygen gas into the molten steel from a lance. In recent years, the importance of steelmaking using electric furnaces has been rediscovered from the perspective of energy conservation and recycling. However, electric furnace steel has a limited range of applications due to its high nitrogen content. For this reason, there is a technology to suppress the absorption of nitrogen into steel.

[0003] Patent Document 1 discloses a method for producing low-nitrogen steel in an electric arc furnace using iron sources such as scrap, reduced iron, and pig iron as raw materials. Specifically, after scrap or other raw materials are melted down, O2 and C are supplied to the molten iron. In addition, the purity of O2 is 99.5 vol.% or more, and the oxygen supply rate Q o2 and oxygen supply time t * is to be limited to the following: 0.55≦Q o2 ≦1.35(Nm 3 / min / ton), t * ≧-7.2Q o2 +15(min).

[0004] And the following formula: C add ≧(12 / 11.2)Q o2 t * W.C. MD If the value on the right side of (kg) is positive, the amount of C added that satisfies the above formula is C add is supplied to the molten iron. At that time, the N concentration in the C carrier gas is set to 3 vol.% or less. Here, W is the amount of molten iron at the end of raw material melting (tons), C isMD is the weight of carbon (kg) contained in the molten iron at the end of raw material melting. Patent Document 2 discloses a method for producing low-nitrogen molten steel in an electric furnace by determining the state of slag foaming by measuring the amount of NOx in the exhaust gas, and adjusting the slag foaming state to completely cut off contact between the molten steel and the atmosphere. Specifically, based on the idea that NOx is generated at the arc spot and that slag is foaming if NOx is not generated, the foaming state is determined from the NOx concentration in the exhaust gas. Based on the result of this determination, operations are performed to foam the slag during the refining period and the temperature rise period.

[0005] Patent Document 3 discloses a method for producing low-nitrogen steel in an electric arc furnace using iron sources such as scrap, reduced iron, and pig iron as raw materials. Specifically, after the raw materials are melted, pure oxygen with a purity of 99.0 vol.% or more is blown into the molten iron at an oxygen supply rate Q o2 The oxygen supply time t * It is recommended that the steel be blown for a period of 10 minutes. Here, Q o2 = in the range of 0.55 to 1.35 t * ≧-7.2Q o2 +15(min) During this blowing, formula: C add ≧(12 / 11.2)Q o2 t * W.C. MD Where W is the amount of molten iron at the end of raw material melting (tons), C MD : The amount of carbon added calculated from the weight (kg) of carbon contained in the molten iron at the end of raw material melting add is to be added.

[0006] Patent Document 4 discloses a method for producing high-purity molten steel with low concentrations of nitrogen and sulfur by melting iron ore, reduced iron, and scrap in an electric arc furnace. Specifically, the electrodes of the electric furnace are made hollow, and the iron is melted while a hydrocarbon gas of 20 Nm / sec or more is supplied from the electrodes, and then the molten iron is decarburized by blowing oxygen gas onto the molten iron. The carbon concentration in the molten iron at the time of melting down is set to 1 mass% or more. Patent Document 5 aims to utilize the exhaust gas from an electric furnace as reducing gas for an attached shaft furnace.

[0007] Specifically, reduced iron is reduced and melted by an electric arc while carbon material is added to an arc-type reduction melting furnace, and then, as necessary, oxygen gas is blown onto the molten iron to perform a decarburization process to produce molten steel. At the same time, exhaust gas generated in the arc-type reduction melting furnace is used as a reducing gas in the shaft furnace, so that the reduction rate of the reduced iron produced in the shaft furnace is set to 50% or more, and the carbon concentration in the molten iron when the reduced iron melts down by the electric arc is set to 1% by mass or more.

[0008] The aim of Patent Document 6 is to form slag by injecting carbon powder in order to improve the efficiency of temperature rise after meltdown. By blowing carbon powder into the slag using a carrier gas, bubbles made of the carbon powder are formed on the slag surface, which covers the molten steel and efficiently raises the temperature of the molten steel. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 11-012634 [Patent Document 2] Patent No. 3743095 [Patent Document 3] Japanese Patent Application Publication No. 10-121123 [Patent Document 4] Patent No. 6413710 [Patent Document 5] Patent No. 6476940 [Patent Document 6] Japanese Patent Application Publication No. 55-089414 Summary of the Invention [Problem to be solved by the invention]

[0010] However, although Patent Documents 1 to 6 disclose techniques for producing steel in an electric arc furnace, there are thought to be technical concerns regarding suppressing nitrogen absorption into molten steel when melting raw materials. Since Patent Document 1 does not describe or suggest an arc heating method according to the carbon concentration of molten steel, there is a risk that nitrogen absorption may occur, unnecessary oxygen or carbonaceous material may be used, resulting in high raw material costs, or a large amount of CO2 may be generated, depending on the situation. In addition, the document mentions that the yield may decrease due to scattering or oxidation of molten steel caused by irradiation of oxygen.

[0011] In Patent Document 2, when reduced iron is mixed with the melting raw material, the carbon concentration of the molten steel may become high, and since nitrogen is not absorbed when the carbon concentration is high, NOx is not generated regardless of the slag foaming state. Therefore, the slag foaming state cannot be determined by looking at NOx alone. In addition, this document cannot determine foaming due to CO gas. Therefore, even if excessive CO gas is generated, it cannot be detected, and there is a risk that the iron yield will decrease due to excessive foaming.

[0012] Patent Document 3 does not state or suggest an arc heating method according to the carbon concentration of molten steel, and therefore there is a risk that nitrogen absorption may occur, unnecessary oxygen or carbonaceous material may be used, resulting in high raw material costs, or a large amount of CO2 may be generated, depending on the situation. In addition, the document mentions that the yield may decrease due to scattering or oxidation of molten steel caused by irradiation of oxygen. In Patent Document 4, the electrode needs to be hollow, which makes it difficult to manufacture and manage the electrode. In addition, although the same document specifies the carbon concentration at the time of melting that is necessary for denitrification using CO gas, there is no description or suggestion regarding slag control after decarburization has progressed, so there is a risk of nitrogen absorption depending on the situation.

[0013] In Patent Document 5, the carbon concentration during reduced iron melting in an arc furnace is set to 1 mass% or more for denitrification by CO gas, but since there is no description or suggestion of a slag control method in the range of 1 mass% or less where nitrogen absorption occurs, there is a risk that the nitrogen concentration will increase depending on the situation. In addition, this document requires the shaft furnace and electric furnace to be installed nearby, which is technically very difficult.

[0014] Since Patent Document 6 does not contain any description regarding reduction in N, there is a risk that the N concentration may become high depending on the situation. In other words, it is not suitable for preventing nitrogen absorption by molten steel. In view of the above problems, an object of the present invention is to provide a method for melting raw materials in an electric furnace, in which reduced iron containing carbon is used as a raw material and melted in an arc-type electric furnace to produce molten steel, and in a region where the carbon concentration in the molten steel is low, submerged arc heating is performed to generate slag to cover the molten steel, thereby preventing nitrogen absorption by the molten steel. [Means for solving the problem]

[0015] In order to achieve the above object, the present invention provides the following technical solutions. The method for melting raw materials in an electric furnace according to the present invention is a method for melting raw materials in an electric furnace in which reduced iron containing carbon is used as a raw material to produce molten steel in an arc-type electric furnace, and the raw material is melted by heating, wherein the carbon concentration of the molten steel produced by heating is 0.80 mass% or less. When the carbon concentration of the molten steel is higher than 0.80 mass%, open arc heating is performed to melt the raw materials, and before the carbon concentration of the molten steel becomes 0.80 mass% or less, the open arc heating is switched to submerged arc heating, and The method is characterized in that the raw material is melted by submerged arc heating in a state where the content of the raw material is 0.80 mass% or less. Effect of the Invention

[0016] According to the present invention, when reduced iron containing carbon is used as a raw material and melted in an arc-type electric furnace to produce molten steel, in a region where the carbon concentration in the molten steel is low, submerged arc heating is performed to generate slag to cover the molten steel, thereby making it possible to prevent nitrogen absorption by the molten steel. [Brief description of the drawings]

[0017] [Figure 1] 1 is a diagram showing a schematic outline of a method for melting raw materials in an electric furnace according to the present invention. FIG. [Diagram 2] FIG. 1 is a graph showing the relationship between the [C] concentration (mass%) in molten steel at the end of nitrogen top blowing and the change (ppm) in the [N] concentration in molten steel from after converter blowing to the start of the next process. [Diagram 3] FIG. 1 is a graph showing the amount of nitrogen absorbed during ladle refining. [Figure 4] 1 is a graph showing the relationship between the [C] concentration (mass%) in molten steel when switching between submerged heating in an electric furnace and the [N] concentration (mass%) in molten steel when tapping from an electric furnace. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the method for melting raw materials in an electric furnace according to the present invention will be described with reference to the drawings. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example. First, an electric furnace 1 in which the raw material melting method according to the present invention is performed will be described. However, the raw material melting method according to the present invention may be performed in a type of electric furnace other than the electric furnace 1 exemplified below.

[0019] FIG. 1 shows a schematic diagram of a method for melting raw material (reduced iron R) in an electric furnace 1 of the present invention. As shown in Fig. 1, the electric furnace 1 can be divided into an upper part and an lower part. That is, the electric furnace 1 has a main body 2 which is open at the top and into which reduced iron R (cold iron source) or the like can be charged, and a lid 3 which covers the opening of the main body 2. The insides of the main body 2 and the lid 3 are lined with firebricks or the like. A slag outlet 4 is formed on a side surface of the electric furnace 1. In addition, a tapping port 5 for tapping molten steel M is formed on the side surface of the electric furnace 1 opposite to the slag outlet 4. The electric furnace 1 is capable of melting raw materials such as reduced iron R and flux, which are charged with the lid open, inside the main body 2 and storing them as molten metal M (molten steel M).

[0020] The electric furnace 1 is provided with a plurality of electrodes 6 that are inserted from above toward the inside. In this embodiment, three electrodes 6 are inserted. The electrodes 6 are graphite electrodes to which three-phase alternating current is supplied, and an arc is generated between the electrodes 6 and the reduced iron R charged inside, whereby the reduced iron R melts and molten metal M can be formed. An oxygen lance 7 can be inserted from the slag outlet 4 of the electric furnace 1. By blowing oxygen gas from the oxygen lance 7 into the molten metal M, it is possible to promote slag formation and perform dephosphorization and decarburization.

[0021] The electric furnace 1 is provided with a furnace tilting device (not shown) that tilts the position. By operating this furnace tilting device to tilt the electric furnace 1 so that the slag outlet 4 is lowered, slag S is discharged from the slag outlet 4. In addition, by operating the furnace tilting device to tilt the electric furnace 1 so that the tapping outlet 5 is lowered, molten steel M is tapped from the tapping outlet 5. FIG. 1 shows a schematic diagram of a method for melting raw materials in an electric furnace 1 according to the present invention. As shown in FIG. 1, the method of melting raw materials in an electric furnace 1 of the present invention is characterized in that, when producing molten steel M in an arc-type electric furnace 1, reduced iron R containing carbon is used as a raw material (melting raw material) and melted by heating, submerged arc heating is performed on the molten steel M to melt the reduced iron R in a state in which the carbon concentration of the molten steel M produced by heating is 0.80 mass% or less.

[0022] Next, a method for melting the raw material (reduced iron R) in the electric furnace 1 of the present invention will be specifically described. When molten steel M is produced using a melting raw material in an electric arc furnace 1, scrap is generally used as the melting raw material in the operation of the electric furnace 1. The electric furnace 1 may also be referred to as an electric furnace 1. The carbon concentration of scrap is basically 1 mass% or less (for example, see Reference (Tomi) (See Ura Azusa, Iron and Steel World 11 (1996) p. 25.) When only scrap is used as the melting raw material, the carbon concentration of the molten steel M will not exceed 1 mass%.

[0023] On the other hand, reduced iron R contains more than 1 mass% carbon. In some cases, reduced iron R containing this carbon is used as a melting raw material. The present invention is a technique that can be applied to the production of molten steel M in an arc-type electric furnace 1 using reduced iron R containing carbon as a melting raw material. Table 1 shows the composition of HBI (Hot Briquetted Iron) as an example of the composition of reduced iron R containing carbon. For more information on Table 1, please refer to references such as (Tanaka Hidetoshi, Kobe Steel R&D Vol. 64 (2014), No. 1, pp. 2-7.) and (Tanaka Hidetoshi et al., Tetsu to Hagane 92 (2006), pp. 1022-1028.). Table 1 is merely an example, and reduced iron R is not limited to HBI. The definition of HBI is "5 g / cm2 briquette at a temperature of 650 °C or higher. 3 This is based on "reduced iron with an apparent density of 1000 or more (based on JIS M 8700:2013)".

[0024] [Table 1]

[0025] As shown in Table 1, HBI (reduced iron) contains more than 1 mass% C. Table 1 also includes other unavoidable contaminant components. For example, scrap and reduced iron R containing carbon may be combined to form the raw material for melting, and the combination of the raw materials for melting is not particularly limited. For example, even if a material containing carbon, reduced iron R, and scrap are used in combination, the present invention is still within the scope of the present invention.

[0026] The operation of the electric furnace 1 is roughly divided into a process of melting the iron source by arc heating or the like, and a process of performing oxidative refining (dephosphorization and decarburization) by adding flux and supplying oxygen gas. In the oxidation refining process, a specified gas such as oxygen is blown into the molten metal M after melting from a gas pipe located at the bottom of the electric furnace 1 or from a lance 7 inserted into the electric furnace 1, and the molten steel M is stirred while decarburizing with the oxygen gas, and dephosphorization is performed by a reaction between the slag S formed by adding flux and the metal (molten steel M).

[0027] It should be noted that the above two steps are not clearly separated, and oxygen may be injected during the dissolution process. That is, the above-mentioned processes cannot be generally distinguished, and it is difficult to clearly distinguish the boundary between the melting process and the oxidation refining process, but as an example, the time required for the entire process of operating the electric furnace 1 is about 1 to 2 hours. In terms of the breakdown, the time required for the first half of the iron source melting process is about 60 to 80% of the total time, and the remaining time (40 to 20%) is the time for the oxidation refining process.

[0028] Now, the molten steel M containing carbon is decarburized by a reaction with oxygen injected into the molten steel M. The carbon concentration in the molten steel M can be controlled by the amount of oxygen injected. Conversely, the carbon concentration in the molten steel at any timing can be estimated (predicted) from the amount of oxygen injected. Alternatively, the carbon concentration in the molten steel can be determined by actually measuring and analyzing a sample of the molten steel M taken using a measuring jig or the like.

[0029] In an operation to obtain molten steel M in an electric arc furnace 1, it is known that submerged arc heating has a higher heat transfer efficiency. Submerged arc heating is a method in which, after all the raw material (reduced iron R) has melted down and the molten metal M has become a flat bath, slag is foamed to cover the surface of the molten steel M with slag S, and an electrode 6 is immersed in the slag S to heat it. Note that this method is sometimes referred to as submerged heating or submerged heating.

[0030] On the other hand, if slag foaming is started while some of the raw materials remain in a solid state, the slag S will cover the solid raw materials, and the slag S covering the raw materials will inhibit the raw materials from dissolving. Therefore, in order to melt the solid raw material (reduced iron R) and quickly turn the molten metal M into a flat bath, it is better to use open arc heating, in which an arc is directly applied to the solid raw material (reduced iron R) to melt it, without generating slag S.

[0031] In particular, when using reduced iron R as the raw material, it is effective to actively use open arc heating to efficiently melt it, since reduced iron R has more gangue components and voids than scrap and has a lower melting efficiency. It is also stated that if slag foaming is performed when unmelted raw material R is present, it becomes difficult to melt the raw material (Reference: Morii Suzue, Electric Furnace Steelmaking Method, 2000, p. 155).

[0032] However, when open arc heating is performed, the molten steel M comes into contact with the atmosphere, and there is a possibility that the molten steel M may absorb N from the atmosphere (nitrogen absorption). It is preferable that the [N] concentration in the steel be low. It is generally known that nitrogen dissolved in molten steel M causes defects such as wrinkles and cracks on the surface of the steel during the rolling or forging process in the subsequent processes. Therefore, in order to suppress defects (improve steel quality), it is necessary to suppress the nitrogen absorption of molten steel M during the operation of electric furnace 1 and to keep the nitrogen concentration after treatment in electric furnace 1 to less than 50 ppm.

[0033] Therefore, in order to efficiently melt the raw material (reduced iron R), it is important to aim for open arc heating as much as possible while preventing nitrogen absorption in the molten steel M. Incidentally, the carbon concentration in molten steel affects the nitrogen absorption behavior of molten steel M. The reason for this is as follows. First, the equilibrium nitrogen concentration [%N] of molten steel M ecan be calculated using the following formula (1) (see references such as Nabeshima et al., Tetsu-to-Hagane 101 (2015), p627-635.).

[0034]

number

[0035] However, [N] e : Equilibrium nitrogen concentration of molten steel (mass%) P N2 : Nitrogen partial pressure of the gas in contact with molten steel T: Absolute temperature (K) R: gas constant f in Eq. (1) N is the activity coefficient of nitrogen, and can be calculated using the following equation (2).

[0036]

number

[0037] Where, [%J]: solute components in molten steel (mass%) e in Equation (2) j N is the interaction coefficient for each component in the same metal with nitrogen, and e C N = 0.13 (see references such as "Recommended Values ​​for Steelmaking Reactions, edited by the 19th Committee of the Japan Society for the Promotion of Science, (1984)"). Also, e C N Since f is a value greater than zero (0), it increases with the increase in the [C] concentration in the molten steel. N becomes larger.

[0038] Therefore, the increase in the [C] concentration in the molten steel N As the equilibrium nitrogen concentration [N] increases, e becomes smaller, that is, the nitrogen concentration that can be dissolved in the molten steel M becomes lower. In addition, the denitrification and nitrogen absorption rates of molten steel M when the mass transfer on the molten steel M side is rate-limiting are expressed by the following equation (3 ) (References: see Nabeshima et al., Tetsu-to-Hagane 101 (2015), p627-635, etc.)

[0039]

number

[0040] Where, [N]: Nitrogen concentration in molten steel (mass%) [N] e : Equilibrium nitrogen concentration of molten steel (mass%) A: Area of ​​molten steel in contact with gas (m 2 ) V: Volume of molten steel (m 3 ) k Nm : Mass transfer coefficient (m / min)

[0041] As shown above, as the [C] concentration in molten steel increases, the equilibrium nitrogen concentration [N] e becomes smaller. Also, the equilibrium nitrogen concentration [N] e A lower temperature means that the N concentration in the molten steel is lower, and the nitrogen absorption rate of the molten steel M is also slower. The above is the reason why nitrogen absorption by molten steel M is difficult to occur when the [C] concentration in the molten steel is high. Therefore, when the [C] concentration in the molten steel is high, the molten steel M does not absorb nitrogen even when it comes into contact with the air, so open arc heating may be actively performed.

[0042] On the other hand, since nitrogen absorption by the molten steel M progresses in low carbon concentration regions, in regions below a certain carbon concentration, submerged heating must be performed to cover the molten steel M with slag S in order to suppress nitrogen absorption by the molten steel M. The threshold value of the [C] concentration in molten steel at which nitrogen absorption by molten steel M occurs was derived from tests conducted in a converter.

[0043] [Example 1] Examples and comparative examples of tests carried out in a converter are described below. Note that the contents described in the examples are merely illustrative of the present invention, and the present invention is not limited thereto. [Conditions (converter)] The operating conditions of the converter in this embodiment are as follows. Table 2 shows the operating conditions of the converter.

[0044] [Table 2]

[0045] Other conditions for carrying out the present invention were those commonly used by those skilled in the art. In this embodiment, a test was carried out in a 250 ton converter to study the effect of nitrogen absorption by molten steel M on the [C] concentration in molten steel. However, the operation of a 250 ton converter is a common practice for those skilled in the art, and the [C] concentration in the molten iron M (molten pig iron M or molten steel M) is gradually reduced by irradiating oxygen from the top. Furthermore, in this test, in addition to oxygen, nitrogen was also blown at 20 Nm 3 / min for top blowing.

[0046] In this test, multiple charges were conducted in which nitrogen top blowing was started from the beginning of blowing and the carbon concentration in the molten steel was changed when nitrogen top blowing was stopped. The nitrogen absorption behavior in the nitrogen top blowing test was evaluated as follows. First, the [N] concentration in molten steel after blowing in a normal operation ch (non-test ch) where nitrogen is not top-blown can be calculated using a prediction formula with operational condition factors as variables.

[0047] In addition, in the next process of the converter, a sample of the molten steel M is taken before the start of processing, and the [N] concentration in the molten steel is actually measured. From these, the change in the [N] concentration in molten steel after blowing in a normal operation channel and the change in the [N] concentration in molten steel before the start of the next process can be calculated. In addition, the average and standard deviation σ of the change in the [N] concentration in molten steel in a normal operation channel can also be calculated.

[0048] Incidentally, the prediction formula for the N concentration in molten steel after blowing does not include a term related to nitrogen top blowing. Therefore, even if the N concentration in molten steel increases with nitrogen top blowing, the predicted N concentration in molten steel after blowing is approximately the same as the N concentration in molten steel during normal operation. On the other hand, the actually measured N concentration in molten steel at the start of the next process increases depending on the amount of nitrogen absorbed by the molten steel M. For this reason, if the N concentration in molten steel is increased by nitrogen top blowing, the amount of change between the N concentration in molten steel after converter blowing and the N concentration in molten steel at the start of the next process will be large.

[0049] From the above, in the nitrogen top blowing test ch, a graph was drawn showing the relationship between the change in [C] concentration in the molten steel and the change in [N] concentration in the molten steel when the supply of nitrogen by top blowing was stopped, and if there was a ch in which the change in nitrogen was outside the normal range, it could be determined that nitrogen absorption by the molten steel M had progressed in that ch. In this embodiment, when the amount of change in nitrogen deviated from the average +3σ of the amount of change in the [N] concentration in the molten steel during normal operation ch, it was determined that nitrogen absorption (nitrogen absorption) in the molten steel M had progressed. Data from 10 nitrogen top blowing test channels were used, and data from 187 normal operation channels (non-test channels) were used. Table 3 shows the data of the nitrogen blowing test ch (charge).

[0050] [Table 3] Tables 4 to 7 show data for normal operation ch (charge).

[0051] [Table 4]

[0052] [Table 5]

[0053] [Table 6]

[0054] [Table 7]

[0055] The carbon concentration in the molten steel at the end of nitrogen blowing was calculated from the material balance taking into account the amount of carbon discharged outside the system as exhaust gas from the amount of carbon input to the converter. [Examples and Comparative Examples (Converter)] Figure 2 shows the relationship between the [C] concentration (mass%) in the molten steel at the end of nitrogen top blowing and the change (ppm) in the [N] concentration in the molten steel from after converter blowing to the start of the next process.

[0056] 2, it can be seen that when the [C] concentration in the molten steel is 0.80 mass% or less, the [N] concentration in the molten steel becomes high. In other words, when the change in the [N] concentration in the molten steel (ppm) becomes high, nitrogen absorption in the molten steel M occurs. As a result of considering the above, such as the relationship shown in Figure 2 and experiment number N-9 in Table 3, it was found that nitrogen absorption by M in molten steel is suppressed when the [C] concentration in molten steel is in the range of > 0.80 mass%, so the [C] concentration in molten steel is specified as > 0.80 mass%. In other words, a [C] concentration in molten steel > 0.80 mass% is necessary to suppress nitrogen absorption by M in molten steel.

[0057] Thus, when the [C] concentration in the molten steel is greater than 0.80 mass%, submerged arc heating must be performed. The [C] concentration in the molten steel (0.80 mass%) may be a predicted value or an actually measured value. In this embodiment, the predicted value is used for the [C] concentration in the molten steel (0.80 mass%). As a result of further intensive research, the intersection point between the average change in [N] concentration in molten steel during normal operation +3σ=18.1 ppm and the linear approximation of the four points with the lowest carbon concentration in molten steel at the end of nitrogen blowing is 0.83 mass%, as shown in Figure 2. From this, it was found that a [C] concentration in molten steel > 0.83 mass% is preferable. [Example 2] Next, an embodiment and a comparative example of the test carried out in the electric furnace 1 will be described. Note that the contents described in the embodiment are merely examples of the present invention, and the present invention is not limited thereto. [Conditions (electric furnace)] The operating conditions of the electric furnace 1 in this embodiment are as follows.

[0058] [Table 8]

[0059] Other conditions for carrying out the present invention were those commonly used by those skilled in the art. Table 9 shows an example of the composition of the scrap and pig iron used. Note that the main component in Table 9 is Fe. Also, all of the components contain other unavoidable contaminant components. Also, Table 9 is merely an example, and the compositions of the scrap and pig iron are not limited to this.

[0060] [Table 9]

[0061] An example of the composition of HBI is shown in Table 1. Table 1 also includes other unavoidable contaminating ingredients. Table 10 shows an example of the flux composition (mass%). Note that in Table 10, blanks indicate no analytical value, and all values ​​include other unavoidable contaminant components. Also, Table 10 is merely an example, and the composition of the flux is not limited to this example.

[0062] [Table 10]

[0063] In this embodiment and the comparative example, the electric furnaces 1 were 20 t and 100 t. In the electric furnace 1, in the operation of this embodiment and the comparative example, open arc heating was performed at the beginning, and then submerged arc heating in which the electrode 6 was immersed was performed halfway through the treatment. Before switching to the submerged heating, oxygen was injected. This injected oxygen reacts with C in the molten steel M.

[0064] That is, the carbon concentration in the molten steel before switching to submerged heating can be controlled by the amount of oxygen injected. The carbon concentration in the molten steel at this time can be calculated assuming that the injected oxygen reacts stoichiometrically with the C in the molten steel M. In this embodiment, the effect was confirmed by operation in the electric furnace 1 as described above, but the carbon concentration in the molten steel does not have to be controlled by oxygen injection, and open arc heating and submerged arc heating may be appropriately switched between while appropriately measuring the carbon concentration in the molten steel.

[0065] When the [C] concentration in the molten steel falls to 0.80 mass% or less, the amount of nitrogen absorption by the molten steel M increases, as shown in Fig. 2. In order to suppress the amount of nitrogen absorption, it is preferable to cover the molten steel M with slag S by submerged heating, thereby blocking contact between the molten steel M and the atmosphere. In the operation of the electric furnace 1, a good method for switching between open arc heating and submerged arc heating is, for example, changing the height of the electrode 6, and it is advisable to adopt the most suitable method taking into account the facilities of each factory.

[0066] The amount of nitrogen absorbed during ladle refining is shown in Figure 3. For more information on Figure 3, please refer to references such as Abe et al., Iron and Steel 68 (1982), 1955. As shown in Figure 3, it has been confirmed that slag S covers the surface of molten steel M, thereby suppressing nitrogen absorption into the molten steel M, as shown in reference literature. [Examples and Comparative Examples (Electric Furnace)] Table 11 shows examples and comparative examples of tests carried out in electric furnace 1.

[0067] [Table 11]

[0068] However, the [C] concentration in the molten steel when switching to submerged arc heating in Table 11 was calculated assuming that the [C] concentration in the molten steel and the injected oxygen react stoichiometrically. FIG. 4 shows the relationship between the [C] concentration (mass%) in the molten steel when electric furnace 1 is switched to submerged arc heating and the [N] concentration (mass%) in the molten steel when electric furnace 1 is tapping. As shown in FIG. 4, Table 11, etc., in experiment number E-1 of this embodiment, submerged arc heating was switched to when the [C] concentration in the molten steel was 1.59 mass%, and submerged arc heating was performed at a [C] concentration in the molten steel necessary for suppressing nitrogen absorption in the molten steel M of 0.80 mass% or less. As a result, the [N] concentration in the molten steel when it was tapped from the electric furnace 1 was 36 ppm, which was less than 50 ppm, and a good result was obtained.

[0069] In experiment number E-2 of this embodiment, submerged arc heating was switched to when the [C] concentration in the molten steel was 1.68 mass%, and submerged arc heating was performed at a [C] concentration in the molten steel of 0.80 mass% or less, which is necessary for suppressing nitrogen absorption in the molten steel M. As a result, the [N] concentration in the molten steel when it was tapped from the electric furnace 1 was 40 ppm, which was less than 50 ppm, and a good result was obtained. On the other hand, when submerged arc heating was used when the [C] concentration in the molten steel was below 0.80 mass% (0.61 mass%, 0.78 mass%), as in the comparative example experiment numbers E-3 and E-4, the [N] concentration in the molten steel when tapped from the electric furnace 1 exceeded 50 ppm (57 ppm, 50 ppm), which was not the desired result.

[0070] In other words, when the carbon concentration of molten steel M is 0.80 mass% or less, if the molten steel M is subjected to submerged arc heating to melt raw material R (reduced iron R), the [N] concentration in the molten steel at the time of tapping will be less than 50 ppm. The reason for setting the nitrogen concentration in the molten steel in the electric furnace 1 to less than 50 ppm is as follows.

[0071] It is generally known that nitrogen dissolved in the molten steel M causes defects such as wrinkles and cracks on the surface of the steel during the rolling or forging process in the subsequent processes. Therefore, in order to suppress defects caused by nitrogen absorption and improve the quality of the steel, it is necessary to make the nitrogen concentration in the molten steel after processing in the electric furnace 1 less than 50 ppm. If carried out as detailed above, by switching to submerged arc heating during operation in electric furnace 1 before the [C] concentration in the molten steel becomes ≦0.80 mass%, it is possible to reduce the nitrogen concentration in the molten steel after treatment in electric furnace 1 to less than 50 ppm.

[0072] That is, in the raw material melting process using reduced iron R as the raw material, open arc heating, which has excellent heat transfer efficiency, may be selected and performed in the C>0.80 mass% region, but in the low carbon concentration region (C≦0.80 mass%), submerged arc heating, which suppresses nitrogen absorption by the molten steel M, is performed, making it possible to keep the nitrogen concentration in the molten steel at a low level when it is tapped. As described above, according to the method of melting a raw material (reduced iron R) in an electric furnace 1 of the present invention, when reduced iron R containing carbon is used as a raw material and melted in an arc-type electric furnace 1 to produce molten steel M, in a region where the carbon concentration in the molten steel is low (C≦0.80 mass%), submerged arc heating is performed to generate slag S to cover the molten steel M, thereby making it possible to prevent nitrogen absorption by the molten steel M.

[0073] It should be noted that the embodiments disclosed herein should be considered as illustrative in all respects and not restrictive. In particular, matters not explicitly stated in the embodiments disclosed herein, such as operating conditions, operating conditions, various parameters, dimensions, weights, volumes of components, etc., are within the scope of ordinary practice of a person skilled in the art. The values ​​used are within the range and can be easily assumed by a person of ordinary skill in the art. [Explanation of symbols]

[0074] 1 Electric furnace (electric furnace) 2 Main unit 3 Lid 4. Slag outlet 5 Steel tapping port 6 electrodes 7 Oxygen Lance M Molten steel (molten metal, molten iron) S slug R Reduced iron

Claims

1. In the production of molten steel in an electric arc furnace, a method for melting reduced iron containing carbon as a raw material is used and melted by heating, comprising the steps of: When the carbon concentration of the molten steel produced by heating is higher than 0.80 mass%, open arc heating is performed to melt the raw materials; switching the open arc heating to submerged arc heating before the carbon concentration of the molten steel becomes 0.80 mass% or less; The raw material is melted by submerged arc heating in a state where the carbon concentration of the molten steel is 0.80 mass% or less.

2. A method for melting raw materials in an electric furnace.

Citation Information

Patent Citations

  • JP1975039209A

  • Refining method for molten low nitrogen high chromium steel in electic arc furnace

    JP1978106619A

  • Refining method of molten steel

    JP1980089414A

  • Manufacture of thin coil provided with core

    JP1989013710A

  • Formation of ceramic