Red mud iron extraction method based on electric arc furnace hydrogen plasma smelting reduction technology
Through electric arc furnace hydrogen plasma smelting reduction technology, the problems of complicated processes and environmental pollution in the process of iron extraction from red mud are solved, efficient, environmentally friendly and high-grade iron extraction is achieved, the process flow is simplified and the utilization rate of red mud is improved.
Patent Information
- Application Number
- CN202410899924.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-05
AI Technical Summary
The existing red mud iron extraction technology has problems such as complex processes, introduction of impurities, environmental pollution and inconvenient forms of iron products, resulting in low utilization rates and high costs.
Electric arc furnace hydrogen plasma smelting reduction technology is used to extract high-purity iron from red mud through the steps of pressing, roasting, molten hydrogen plasma reduction, crushing and screening. Plasma hydrogen is used as the reducing agent, avoiding the use of solid reducing agents and CO2 emissions.
It achieves efficient and environmentally friendly extraction of high-grade iron from red mud, simplifies the process, improves production efficiency, and has a purity of more than 98%. The product exists in the form of iron blocks, is easy to process and apply, and achieves the complete processing and application of red mud. Utilization and resource recycling.
Smart Images

Figure CN118726684A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of red mud recycling, and in particular to a red mud iron extraction method based on electric arc furnace hydrogen plasma melting reduction technology, which utilizes electric arc furnace and hydrogen plasma technology for melting reduction to extract industrial pure iron from Bayer process red mud. Background Art
[0002] Red mud, as a highly alkaline industrial solid waste produced after refining alumina from bauxite, contains a large number of valuable components, such as SiO2, Al2O3, CaO and Fe2O3, among which the iron content of Bayer red mud is particularly significant, usually between 30-60wt.%. However, despite the rich red mud resources in my country, its utilization rate is currently less than 10%, and a large amount of red mud is still treated by damming and stockpiling, which not only occupies precious land resources, but also poses serious environmental and safety risks.
[0003] In recent years, in order to improve the utilization rate of red mud and recover the valuable components, especially iron, a variety of technical methods have been proposed. For example, a patent proposes a method of melting red mud in an electric furnace, mixing and granulating by adding reducing agents, binders, etc., and then extracting molten iron through preheating, roasting and electric furnace reduction. There is also a patent that uses biomass pyrolysis gas as a reducing agent to reduce the iron oxide in red mud at low temperature. In addition, there are methods such as fluidized bed reduction magnetization treatment, suspended roasting and rotary hearth furnace direct reduction to prepare iron concentrate or recover iron.
[0004] However, these methods all have certain limitations in practical applications. First, most methods require the red mud to be dried and crushed in advance, and auxiliary materials such as reducing agents and binders need to be added, which not only increases the complexity of the process, but also may introduce new impurities. Secondly, in the traditional reduction roasting process, coal powder or coke powder is often used as a reducing agent, resulting in large carbon dioxide emissions, which does not meet current environmental protection requirements. Furthermore, the iron produced by reduction is mostly in the form of iron powder, which is difficult to extract and has a high cost. Summary of the invention
[0005] In view of the shortcomings of the existing technology, it is urgent to develop a new method for extracting iron from red mud that is efficient, energy-saving and environmentally friendly. The present invention is proposed based on this demand and aims to achieve efficient and clean extraction of iron resources from Bayer red mud through electric arc furnace hydrogen plasma melting reduction technology.
[0006] The technical solution adopted by the present invention is: a method for extracting iron from red mud based on electric arc furnace hydrogen plasma melting reduction technology, and the method for extracting iron from red mud comprises the following steps:
[0007] Pressing into blanks: First, the red mud raw materials are formed through a pressing process to form a blank with a certain shape and density, ensuring the initial shape and physical properties of the raw materials;
[0008] Calcination: Next, the pressed green body is calcined. The calcination process causes physical and chemical changes inside the green body through high temperature, further stabilizing its structure and preparing for the subsequent reduction process;
[0009] Molten hydrogen plasma reduction: After roasting, the green body is reduced using molten hydrogen plasma technology. This step uses the special properties of molten hydrogen plasma to deeply reduce the green body, making its composition more uniform and removing impurities;
[0010] Crushing: The reduced green body is sent to the crusher for crushing. Through crushing, the green body is broken into fine powder, which is convenient for subsequent screening and separation;
[0011] Screening: Finally, the crushed powder is screened, and the residue powder, iron ingots and iron beads of different particle sizes are separated through a sieve or other screening equipment, ensuring the purity and quality of the final product.
[0012] In the pressing process, the red mud raw material is pressed under 5-10 MPa to form a red mud blank.
[0013] In the roasting process, the pressed red mud blank is calcined at 800 to 1200 degrees Celsius for 30 to 120 minutes.
[0014] In the molten hydrogen plasma reduction process, the calcined red mud blank is placed in a vacuum arc melting furnace for hydrogen plasma reduction treatment, and the specific treatment method includes a first step of pre-melting and a second step of removing residual gas.
[0015] The first step of pre-melting is to introduce 0.06MPa high-purity Ar gas and a current of 100-200A into an electric arc furnace to melt the red mud billet into a melt.
[0016] The second step of removing residual gas is to remove the residual gas in the first step, introduce 80-90vol.% Ar gas and 10-20vol.% H2, the total pressure of the mixed gas is above 0.06MPa, the current is 80-200A, and hydrogen plasma reduction treatment is performed. Each treatment lasts 1-5min. This step is repeated more than 3 times to complete the reduction treatment.
[0017] After the reduced red mud ingots are crushed and screened, large pieces of pure iron with a purity higher than 98% can be obtained.
[0018] The vacuum arc melting furnace has a device for introducing a mixed gas of Ar gas and H2, and a device for controlling current and pressure.
[0019] The technical effect of the technical solution of the present invention is: the present invention provides a method for extracting iron from red mud based on electric arc furnace hydrogen plasma melting reduction technology, which achieves the goal of efficiently extracting iron from red mud. Through innovative process flow and optimized parameter setting, the goal of efficiently and environmentally friendly extraction of high-grade iron from red mud is achieved, while achieving complete utilization of waste, with significant economic and environmental benefits, which are specifically embodied as follows:
[0020] First, by using plasma hydrogen as a reducing agent, this method avoids the cumbersome processes of drying, crushing, mixing, etc. introduced by conventional solid reducing agents, thereby simplifying the process flow and improving production efficiency. At the same time, since the product after reduction is water, the emission of greenhouse gases such as carbon dioxide is effectively avoided, which has a significant environmental protection effect.
[0021] Secondly, by optimizing the process flow and parameter settings, this method allows the iron after extraction and reduction to exist in the form of iron blocks with a purity of more than 90% and above 98%. This high-grade, high-purity iron product is not only easy to extract and process later, but also has higher market value and application prospects.
[0022] In addition, this method also achieves full utilization of red mud. The low-alkalinity residue can be directly used for engineering applications such as paving and backfilling, which not only solves the problem of red mud waste disposal, but also achieves resource recycling and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION
[0024] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings:
[0025] like Figure 1 As shown, a method for extracting iron from red mud based on electric arc furnace hydrogen plasma melting reduction technology, the method for extracting iron from red mud comprises the following steps:
[0026] Pressing into blanks: First, the red mud raw materials are formed through a pressing process to form a blank with a certain shape and density, ensuring the initial shape and physical properties of the raw materials;
[0027] Calcination: Next, the pressed green body is calcined. The calcination process causes physical and chemical changes inside the green body through high temperature, further stabilizing its structure and preparing for the subsequent reduction process;
[0028] Molten hydrogen plasma reduction: After roasting, the green body is reduced using molten hydrogen plasma technology. This step uses the special properties of molten hydrogen plasma to deeply reduce the green body, making its composition more uniform and removing impurities;
[0029] Crushing: The reduced green body is sent to the crusher for crushing. Through crushing, the green body is broken into fine powder, which is convenient for subsequent screening and separation;
[0030] Screening: Finally, the crushed powder is screened, and the residue powder, iron ingots and iron beads of different particle sizes are separated through a sieve or other screening equipment, ensuring the purity and quality of the final product.
[0031] The implementation purpose and principle of the present invention are mainly controlled by the following contents:
[0032] 1. Raw material preparation: Red mud, a toxic waste produced during the refining process of bauxite, is used as the main raw material. This red mud usually contains a large amount of iron oxide and other metal oxides.
[0033] 2. Reducing agent and equipment
[0034] Reducing agent: Plasma hydrogen is used as a reducing agent. Compared with traditional solid reducing agents, plasma hydrogen has higher reactivity and is more environmentally friendly.
[0035] Equipment: A device similar to an electric arc furnace is used in which a hydrogen plasma is generated.
[0036] 3. Process steps
[0037] Melting: Red mud is placed in an electric arc furnace and melted by high temperatures to form a viscous melt.
[0038] Reduction: The molten red mud is exposed to hydrogen plasma for rapid liquid reduction. In this process, iron oxide is reduced to iron, and the main byproduct is water, avoiding the emission of greenhouse gases such as carbon dioxide.
[0039] Separation: After the reduction reaction, liquid iron and liquid oxide will naturally separate due to the difference in density and viscosity.
[0040] Extraction: Liquid iron can be easily extracted, and after it cools and solidifies, high-purity iron blocks can be obtained.
[0041] 4. Product Features
[0042] Purity: The extracted iron has high purity, usually reaching more than 95%, or even up to 98%, with extremely low content of harmful elements, and can be directly used for steelmaking or other high-end applications.
[0043] Environmental protection: The only by-product produced in the whole process is water, which fully meets environmental protection requirements.
[0044] 5. Optimization direction
[0045] Fume treatment: Fumes may be generated during the reduction and extraction process, and appropriate treatment equipment is required to ensure environmental safety.
[0046] Process optimization: Although the current reduction time is relatively short (e.g., 10-15 minutes), there is still room for further process optimization and improvement of reduction efficiency.
[0047] Large-scale application: At present, this technology may still be in the laboratory or small-scale test stage. To achieve industrial application, a large number of pilot and large-scale tests are needed to verify its economy and feasibility.
[0048] The following will provide additional explanations through specific examples. The Bayer red mud used in the following experiments comes from Zhongzhou Aluminum Co., Ltd., and the iron content of the red mud measured by IPC-MS is 53%.
[0049] Embodiment 1:
[0050] Pressing into blanks: The pH value of the red mud residual liquid is 10-11, and it is pressed into red mud blanks under 5-10MPa conditions.
[0051] Calcination: The pressed red mud blank was calcined at 800 degrees Celsius for 60 minutes.
[0052] Molten hydrogen plasma reduction: 30g of calcined red mud blanks are placed in a vacuum arc melting furnace for hydrogen plasma reduction treatment. The first step is pre-melting. 0.06MPa high-purity Ar gas is introduced into the arc furnace with a current of 80A to melt the red mud blank into a melt. The second step is to remove the residual gas from the first step, introduce 90vol.% Ar gas and 10vol.% H2, with a total pressure of 0.06MPa and a current of 80A, and perform hydrogen plasma reduction treatment. Each treatment lasts 2min, and this step is repeated twice to complete the reduction treatment.
[0053] Crushing and screening: After the reduced red mud ingots are crushed and screened, about 8g of iron beads with a diameter of about 5-10mm can be obtained. The scanning electron microscope energy spectrum test shows that the iron content is 99.6wt%, and the extraction rate is 50.3%. The pH of the residue is between 7.5-8.
[0054] Embodiment 2:
[0055] Pressing into blanks: The pH value of the red mud residual liquid is 10-11, and it is pressed into red mud blanks under 5-10MPa conditions.
[0056] Calcination: The pressed red mud blank was calcined at 800 degrees Celsius for 60 minutes.
[0057] Molten hydrogen plasma reduction: 30g of calcined red mud blanks were placed in a vacuum arc melting furnace for hydrogen plasma reduction treatment. The first step was pre-melting. 0.06MPa high-purity Ar gas was introduced into the arc furnace with a current of 130A to melt the red mud blank into a melt. The second step was to remove the residual gas from the first step, introduce 90vol.% Ar gas and 10vol.% H2, with a total pressure of 0.06MPa of the mixed gas and a current of 130A, and perform hydrogen plasma reduction treatment. Each treatment lasted 2min, and this step was repeated 4 times to complete the reduction treatment.
[0058] Crushing and screening: After the reduced red mud ingots are crushed and screened, about 8.8g of iron beads with a diameter of about 5-10mm can be obtained. The scanning electron microscope energy spectrum test shows that the iron content is 99.8wt%, and the extraction rate is 55%. The pH of the residue is between 7.5-8.
[0059] Embodiment three:
[0060] Pressing into blanks: The pH value of the red mud residual liquid is 10-11, and it is pressed into red mud blanks under 5-10MPa conditions.
[0061] Calcination: The pressed red mud blank was calcined at 1200 degrees Celsius for 60 minutes.
[0062] Molten hydrogen plasma reduction: 60g of calcined red mud blanks were placed in a vacuum arc melting furnace for hydrogen plasma reduction treatment. The first step was pre-melting. 0.06MPa high-purity Ar gas was introduced into the arc furnace with a current of 200A to melt the red mud blank into a melt. The second step was to remove the residual gas from the first step, introduce 90vol.% Ar gas and 10vol.% H2, with a total pressure of 0.06MPa and a current of 200A, and perform hydrogen plasma reduction treatment. Each treatment lasted 4min, and this step was repeated 5 times to complete the reduction treatment.
[0063] Crushing and screening: After the reduced red mud ingots are crushed and screened, about 18.8g of iron blocks with a diameter of about 10-20mm can be obtained. The scanning electron microscope energy spectrum test shows that the iron content is 99.6wt%, and the extraction rate is 59%. The pH of the residue is between 7.5-8.
[0064] Embodiment 4:
[0065] This embodiment provides an optimized method for extracting iron from red mud, which is further improved and optimized on the basis of the first embodiment to improve the extraction rate and purity of iron.
[0066] Pressing into green bodies: Select pre-treated red mud raw materials and form them through efficient pressing processes to form high-density green bodies. Pretreatment includes dehydration and removal of impurities to ensure the purity and uniformity of the raw materials. During the pressing process, advanced pressure control technology is used to ensure that the green bodies are evenly compressed under 5-10MPa to form green bodies with excellent physical properties.
[0067] Calcination: The pressed green body is calcined under a precisely controlled temperature curve at a temperature of 900-1100 degrees Celsius for 45-90 minutes. By optimizing the calcination temperature and time, the physical and chemical changes inside the green body are further promoted, creating more favorable conditions for the subsequent reduction process.
[0068] Molten hydrogen plasma reduction: Use advanced electric arc furnace equipment, equipped with high-precision gas control and current regulation systems. In the first pre-melting stage, 0.6MPa of high-purity Ar gas is introduced, and the current is precisely controlled within the range of 120-180A to ensure that the red mud billet is completely melted into a melt. In the second step of removing residual gas, the mixing ratio of the introduced Ar gas and H2, as well as the current and pressure parameters are optimized to improve the reduction efficiency. Specifically, 85-95vol.% Ar gas and 5-15vol.% H2 are introduced, the total pressure of the mixed gas is maintained at 0.6-0.8MPa, the current is controlled within the range of 100-180A, each processing time is 2-4 minutes, and this step is repeated more than 4 times to ensure sufficient reduction.
[0069] Crushing and screening: Use efficient crushing equipment to crush the reduced green body into fine powder. Through the multi-stage screening system, the residual powder, iron ingots and iron beads of different particle sizes are accurately separated to ensure the purity and quality of the final product.
[0070] Embodiment five:
[0071] This embodiment focuses on improving the environmental protection and resource utilization rate of the red mud iron extraction method.
[0072] Environmental protection measures: During the entire iron extraction process, the emission of waste gas, waste water and solid waste is strictly controlled. An advanced waste gas treatment system is used to ensure that the emitted gas meets national environmental protection standards. Waste water is deeply treated to achieve recycling or safe discharge of waste water. Solid waste generated is classified and processed, and the recyclable part is reused and the non-recyclable part is safely disposed of.
[0073] Resource utilization: The extracted high-purity iron blocks can be directly used in steel production or other industrial fields that require high-purity iron. The low-alkalinity residues produced during the reduction process can be used in building materials, roadbed materials and other fields after further treatment, thus realizing the recycling of resources.
[0074] The present invention innovatively uses plasma hydrogen as a reducing agent and industrial waste red mud as the only raw material, achieving efficient and environmentally friendly utilization of resources. This technical solution not only significantly simplifies the complex processes of drying, crushing, mixing, etc. in traditional processes, but also avoids the environmental and operational inconveniences that may be caused by conventional solid reducing agents due to its uniqueness of using plasma hydrogen. The only by-product produced by this method during the reduction process is water. This feature gives it a significant advantage in environmental protection, completely eliminates the emission of greenhouse gases such as carbon dioxide, and is of great significance for promoting the development of green environmental protection and low-carbon economy. After the iron is reduced by this method, more than 90% of it is pure in the form of iron blocks, and its purity is as high as more than 98%. This high-grade, high-purity iron is not only of superior quality, but also more convenient for later extraction and processing, greatly improving production efficiency and product quality. In addition, the process is simple and easy to understand, easy to operate, not only reduces production costs, but also improves production efficiency. At the same time, its environmental protection characteristics also meet the current society's urgent need for sustainable development, achieving the dual goals of economic benefits and environmental protection. The implementation of this invention has undoubtedly opened up a new way for the comprehensive utilization of red mud, which not only improves the utilization rate of resources, but is also expected to play a huge role in future industrial production. Its broad application prospects and market potential will surely lead the technological innovation and industrial upgrading of related industries.
Claims
1. A method for extracting iron from red mud based on arc furnace hydrogen plasma melting reduction technology, characterized in that: The method for extracting iron from red mud comprises the following steps: Pressing into blanks: First, the red mud raw materials are formed through a pressing process to form a blank with a certain shape and density, ensuring the initial shape and physical properties of the raw materials; Calcination: Next, the pressed green body is calcined. The calcination process causes physical and chemical changes inside the green body through high temperature, further stabilizing its structure and preparing for the subsequent reduction process; Molten hydrogen plasma reduction: After roasting, the green body is reduced using molten hydrogen plasma technology. This step uses the special properties of molten hydrogen plasma to deeply reduce the green body, making its composition more uniform and removing impurities; Crushing: The reduced green body is sent to the crusher for crushing. Through crushing, the green body is broken into fine powder, which is convenient for subsequent screening and separation; Screening: Finally, the crushed powder is screened, and the residue powder, iron ingots and iron beads of different particle sizes are separated through a sieve or other screening equipment, ensuring the purity and quality of the final product.
2. The method for extracting iron from red mud based on arc furnace hydrogen plasma melting reduction technology according to claim 1, characterized in that: In the pressing process, the red mud raw material is pressed under 5-10 MPa to form a red mud blank.
3. The method for extracting iron from red mud based on arc furnace hydrogen plasma melting reduction technology according to claim 1, characterized in that: In the roasting process, the pressed red mud blank is calcined at 800 to 1200 degrees Celsius for 30 to 120 minutes.
4. The method for extracting iron from red mud based on arc furnace hydrogen plasma melting reduction technology according to claim 1, characterized in that: In the molten hydrogen plasma reduction process, the calcined red mud blank is placed in a vacuum arc melting furnace for hydrogen plasma reduction treatment, and the specific treatment method includes a first step of pre-melting and a second step of removing residual gas.
5. The method for extracting iron from red mud based on arc furnace hydrogen plasma melting reduction technology according to claim 1, characterized in that: The first step of pre-melting is to introduce 0.06MPa high-purity Ar gas and a current of 100-200A into an electric arc furnace to melt the red mud billet into a melt.
6. The method for extracting iron from red mud based on arc furnace hydrogen plasma melting reduction technology according to claim 1, characterized in that: The second step of removing residual gas is to remove the residual gas in the first step, introduce 80-90vol.% Ar gas and 10-20vol.% H2, the total pressure of the mixed gas is above 0.06MPa, the current is 80-200A, and hydrogen plasma reduction treatment is performed. Each treatment lasts 1-5min. This step is repeated more than 3 times to complete the reduction treatment.
7. The method for extracting iron from red mud based on arc furnace hydrogen plasma melting reduction technology according to claim 1, characterized in that: After the reduced red mud ingots are crushed and screened, large pieces of pure iron with a purity higher than 98% can be obtained.
8. The method for extracting iron from red mud based on arc furnace hydrogen plasma melting reduction technology according to claim 4, characterized in that: The vacuum arc melting furnace has a device for introducing a mixed gas of Ar gas and H2, and a device for controlling current and pressure.
Citation Information
Patent Citations
Red mud comprehensive utilization method and system
CN106148684A
Method and system for treating red mud
CN106148718A
Method for red mud reduction by adopting gas-based shaft furnace
CN106755966A
Red mud comprehensive utilization technology
CN108754134A
Iron-containing red mud coal-based direct reduction process and system
CN111763791A
Cited By
Low-calcium clinker and preparation method thereof
CN119461908A
Low calcium clinker and preparation method thereof
CN119461908B