Silica-titania composite oxide powder
Silica-titania composite oxide particles with controlled refractive index distribution and reduced coarse particles address transparency issues in organic-inorganic composites, enhancing their optical and mechanical properties.
Patent Information
- Application Number
- JP2021509035
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-25
- Filing Date
- 2020-03-12
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2040-03-12
AI Technical Summary
Existing organic-inorganic composite materials face issues with reduced transparency due to mismatched refractive indices and the presence of coarse particles, which are unsuitable for high transparency applications.
The development of silica-titania composite oxide particles with controlled refractive index distribution and reduced coarse particle content, achieved by limiting nitrogen content before firing and optimizing particle size and refractive index matching, results in improved transparency and mechanical properties.
The silica-titania composite oxide particles enhance transparency and functionality by minimizing refractive index variation and coarse particle formation, making them suitable for high transparency applications.
Abstract
Description
[Technical field]
[0001] The present invention relates to a silica-titania composite oxide powder having a controlled refractive index and distribution and reduced coarse particles of 5 μm or more, which can be suitably used as a filler for highly transparent resins and transparent resin adhesives, an antiblocking agent for films, and a hard coat material. [Background technology]
[0002] Thermoplastic resins such as PET, polycarbonate, PMMA, and polystyrene are widely used industrially due to their excellent transparency, mechanical properties, moldability, etc. As a means of improving the physical properties of organic polymers, research is being conducted on composite materials of organic and inorganic compounds (hereinafter referred to as organic-inorganic composite materials) that retain the characteristics of organic polymers such as flexibility, low density, and moldability while possessing the characteristics of inorganic compounds such as high strength, high elasticity, and heat resistance.
[0003] One method for producing an organic-inorganic composite material is known to be a method of directly adding an inorganic filler to an organic polymer. For example, Patent Document 1 proposes a method of improving mechanical properties such as tensile strength and flame retardancy by adding surface-treated silica particles, which are an inorganic filler, to polycarbonate.
[0004] However, the addition of inorganic filler reduces the transparency of the organic-inorganic composite material. In order to improve this point, a method has been proposed in which an inorganic filler having a refractive index equivalent to that of the organic material (usually various resins) used is used to improve the function of the organic-inorganic composite material while suppressing the decrease in transparency. For example, Patent Document 2 proposes a method of maintaining the transparency of the organic-inorganic composite material while controlling the thermal expansion coefficient by using silica-titania particles having the same refractive index as the resin in an epoxy resin composition. However, even when an inorganic filler having substantially the same refractive index as the resin used is added, the transparency of the resin itself is not maintained, and no mechanism for the optical loss has been elucidated, nor has any countermeasure for the optical loss been proposed. For this reason, conventional organic-inorganic composite materials could not be used in applications requiring high transparency.
[0005] In addition, many studies have been conducted on the manufacturing method of such an inorganic filler with an adjusted refractive index, and among them, many manufacturing methods have been proposed using the so-called sol-gel method, which produces spherical particles by hydrolysis of metal alkoxide. For example, Patent Document 3 proposes spherical particles composed of silica and an oxide of a Group IV metal, and Patent Document 4 proposes a method of obtaining relatively large silica-titania particles with high monodispersity by simultaneously adding a basic catalyst and an alkoxide raw material and discharging a part of it out of the system. Patent Documents 5 and 6 propose the use of a chain-forming agent to produce particles with a high titania content. In addition to these, many other proposals have been made (Patent Documents 7, 8, etc.).
[0006] On the other hand, in recent years, with the progress of larger screens and higher definitions of flat panel displays, optical films are required to be substantially free of defects in addition to high transparency. However, when manufacturing optical films, if coarse particles or agglomerates are contained in the inorganic filler, it may cause defects or scratches. In addition, when used for applications such as semiconductor underfill, the organic-inorganic composite material needs to flow through a narrow flow path, but if coarse particles or agglomerates are contained, they will prevent the material from flowing uniformly through the narrow flow path, causing voids and poor adhesion. Therefore, it is very important that the content of coarse particles and agglomerates is extremely low in various optical adhesives, including those for optical semiconductors, in order to prevent defects. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2004-107470 A [Patent Document 2] Japanese Patent Application Publication No. 6-65475 [Patent Document 3] Japanese Patent Application Publication No. 03-33721 [Patent Document 4] Japanese Patent Application Publication No. 08-48505 [Patent Document 5] JP 2007-269612 A [Patent Document 6] JP 2008-37700 A [Patent Document 7] JP 2007-269594 A [Patent Document 8] JP 2003-252616 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present inventors have conducted extensive research to solve the above problems. As a result, they have noticed that even if the refractive index of the inorganic particles used in the organic-inorganic composite material is adjusted to match the refractive index of the organic polymer, high transparency cannot be obtained if the inorganic particles have a distribution in refractive index, that is, if the refractive index of each inorganic particle varies. In addition, although the refractive index distribution of the inorganic particles tends to improve by firing at a high temperature, the effect is insufficient, and there is also a problem that coarse particles are easily generated when firing at such a temperature.
[0009] As a result of further investigation, the inventors discovered that by controlling the amount of nitrogen contained in the powder during the production stage of the inorganic particles, specifically after drying and before firing, to a specific range or less, it is possible to prepare silica-titania composite oxide particle powder that has a suppressed refractive index distribution and produces little coarse particles when fired at a low temperature, and thus completed the present invention.
[0010] That is, the present invention relates to a silica-titania composite oxide powder having an average particle diameter D (μm) measured by a laser scattering method in the range of 0.1 μm or more and 3.0 μm or less, an average refractive index at a measurement wavelength of 589 nm of 1.47 or more, and a minimum absorbance S obtained by measuring a dispersion of 30 mass % of silica-titania composite oxide particles in a liquid having the same refractive index as the average refractive index, which satisfies the following relationship:
[0011] S<0.026-0.008×D Effect of the Invention
[0012] By using the silica-titania composite oxide particles with a suppressed refractive index distribution of the present invention, an organic-inorganic composite material with higher transparency can be obtained compared to the transparency obtained by using particles whose refractive index is simply matched to an organic polymer. In addition, since the generation of coarse particles can be suppressed, it has become possible to actively improve the function by adding inorganic fillers. BEST MODE FOR CARRYING OUT THEINVENTION
[0013] In the silica-titania composite oxide powder according to the embodiment, the particles constituting the powder are composed of silica (SiO2) and titania (TiO2), which are composited at the atomic level. Composited at the atomic level means that the particles contain a bond state (Si-O-Ti) in which one oxygen atom is bonded to both an Si atom and a Ti atom. Even if the particles partially contain Si-O-Si bonds and Ti-O-Ti bonds, the present embodiment can be said to be composited at the atomic level because the ratio of silica and titania in one particle is almost uniform at any point by the manufacturing method described below, and Si-O-Ti is contained.
[0014] The ratio of silica to titania is not particularly limited, but titania is preferably contained in an amount of 25 mol% or less of the total oxides, more preferably 20 mol% or less, and particularly preferably 17 mol% or less, because it is easy to produce spherical particles that are individually independent and the range of refractive index is close to that of many resins. The refractive index tends to increase as the titania content increases. In addition, the particles constituting the silica-titania composite oxide powder of this embodiment are preferably amorphous, but when the titania content of the particle constituents increases, that is, when the silica content decreases, it becomes difficult to obtain an amorphous structure due to the silica component, and titania microcrystals tend to occur in the particles.
[0015] On the other hand, in consideration of making the refractive index higher than that of silica, the lower limit of the titania content is preferably 1 mol % or more, and particularly preferably 3 mol % or more.
[0016] The silica-titania composite oxide powder of this embodiment has a cumulative 50% volume diameter (hereinafter referred to as "average particle diameter") measured by a laser scattering method in the range of 0.1 μm to 3.0 μm. If the average particle diameter is smaller than 0.1 μm, the individual particles are likely to aggregate, and such aggregates are likely to cause optical and physical defects after composite formation. On the other hand, if the particles are too large, the transparency changes significantly due to a slight difference in refractive index, making it difficult to obtain a transparent composite material. For this reason, the more preferable particle size is an average particle diameter in the range of 0.2 μm to 2 μm, and even more preferably, in the range of 0.4 μm to 1.5 μm.
[0017] In addition, there is no problem with the particle size distribution if the average particle size is within this range, but since a wide particle size distribution is likely to produce coarse particles, it is preferable that the monodispersity is high.
[0018] The silica-titania composite oxide powder of this embodiment has an average refractive index at a measurement wavelength of 589 nm (hereinafter, when the term "refractive index" is used, it refers to the average refractive index at a measurement wavelength of 589 nm) of 1.47 or more. While the refractive index of silica, which is a single element, is 1.46, titania is composited, and therefore exhibits a higher refractive index than silica alone. Therefore, when composited with various resins that often have a refractive index exceeding 1.5, it is easy to match the refractive index, and therefore it is possible to obtain a product with excellent optical properties such as transparency.
[0019] The average refractive index is a value measured by the liquid immersion method as follows. That is, a plurality of liquids having different refractive indices at a wavelength of 589 nm are prepared, and silica-titania composite oxide powder is dispersed in these liquids. The transparency (transmittance or absorbance) of the dispersion liquid at a wavelength of 589 nm is measured, and the refractive index of the liquid that gives the most transparent dispersion liquid is regarded as the refractive index of the silica-titania composite oxide powder at a wavelength of 589 nm.
[0020] Since moisture adsorbed to the silica-titania composite oxide powder may affect the refractive index, the refractive index is measured after drying the powder at 100° C. for 12 hours or more.
[0021] Here, as a method for adjusting the refractive index of the liquid, a method of mixing a plurality of substances with different refractive indices to obtain a desired refractive index, a method of changing the temperature during measurement, etc. can be adopted. Note that a liquid that is substantially transparent at a wavelength of 589 nm is adopted as the liquid used as the dispersion medium used in the measurement. For example, water, toluene, 1-bromonaphthalene, 1-chloronaphthalene, diiodomethane, diiodomethane containing sulfur, 2-methoxyethanol, benzyl alcohol, methyl salicylate, methyl benzoate, silicone oil, etc. can be used as the liquid, and these can be appropriately mixed, and further various salts and organic solids can be dissolved in order to adjust the refractive index. In addition, liquids with various refractive indices are commercially available as standard solutions for the refractive index, and these may be used.
[0022] In addition to the above method, the refractive index of the silica-titania composite oxide powder may be determined in accordance with JIS K 7142, Method B for Determining the Refractive Index of Plastics (a method for measuring the refractive index of a powder or granular transparent material by a liquid immersion method using a microscope).
[0023] The refractive index of the silica-titania composite oxide powder of this embodiment can be controlled by changing the ratio of silica to titania. That is, as described above, the refractive index of pure silica is 1.46, and the refractive index increases as the ratio of titania increases.
[0024] The greatest feature of the silica-titania composite oxide powder of this embodiment is that when 30 mass% of silica-titania composite oxide particles are dispersed in a liquid having the same refractive index (wavelength 589 nm) as the average refractive index calculated as described above, the minimum absorbance S is defined as the absorbance at a wavelength of 589 nm, and the average particle size D satisfies the following formula (1).
[0025] S<0.026-0.008×D (1)
[0026] In the above formula (1), the minimum absorbance S is an index of the variation (distribution) of the refractive index of the particles constituting the silica-titania composite oxide powder. As defined above, the minimum absorbance S is measured in a liquid having the same refractive index as that of the silica-titania composite oxide powder, so the refractive index difference is 0, and therefore the absorbance should also be 0. However, the particles constituting the silica-titania composite oxide powder do not all have the same refractive index, and each particle has a slightly different refractive index, and the average value is measured by the liquid immersion method.
[0027] Therefore, in the dispersion of silica-titania composite oxide, there will be a considerable number of particles having a refractive index different from that of the liquid, and such particles will reduce transparency and increase the minimum absorbance S. In other words, the smaller the minimum absorbance S, the smaller the proportion of particles having a refractive index that deviates from the average refractive index.
[0028] Here, particles having the same refractive index means that the difference in refractive index is within the range of ±0.001.
[0029] As is well known, the transparency (absorbance) of a particle dispersion is affected by the particle size, and if the particle size is small, the effect of the refractive index difference is relatively small. The above formula (1) takes into account the effect of the particle size (D) on the variation in the refractive index.
[0030] The silica-titania composite oxide powder of the present embodiment has an unprecedentedly small variation in refractive index between particles, and therefore can achieve unprecedentedly high transparency when dispersed in a resin or solvent.
[0031] In the silica-titania composite oxide powder of this embodiment, the ratio of the number of coarse particles having a particle diameter of 5 μm or more to the total number is preferably 500 ppm or less, particularly 200 ppm or less. Here, the coarse particles are a group of several independent particles or are composed of independent particles. If there are a large number of such coarse particles, defects are likely to occur after forming a composite material by, for example, compounding with a resin.
[0032] The above-mentioned coarse particles are determined by adding silica-titania composite oxide powder to water or methanol to make a concentration of 2.5% by mass, dispersing the powder in an ultrasonic disperser, and measuring the number of particles of 5 μm or more using a Coulter counter, repeating the measurement 5 times (for a total of 250,000 particles). The shape of each particle contained in the silica-titania composite oxide powder of this embodiment is not particularly limited, but is preferably spherical in consideration of the flowability and moldability of the organic-inorganic composite material.
[0033] Furthermore, the silica-titania composite oxide powder of this embodiment preferably has a low content of metals other than silicon and titanium, and in particular, the content of alkali metals such as sodium and potassium is preferably 10 ppm or less, and more preferably 1 ppm or less.
[0034] Depending on the use mode of the silica-titania composite oxide powder of this embodiment, the surface of the particles can be appropriately prepared by surface treatment or the like. When compounding with a resin, the surface can be modified by performing surface treatment by a known method as long as it does not affect the minimum absorbance, taking into consideration the compatibility with the resin used. For example, when compounding with a resin having a hydrophilic site, it is preferable that a large number of hydrophilic silanol groups are present on the surface of the particles. In this case, the silica-titania composite oxide powder can be used as it is, or the surface can be coated with an inorganic material to further improve the affinity. On the other hand, when it is desired to reduce the hydrophilicity of the surface, the surface can be modified by appropriately using a silane coupling agent having a methyl group.
[0035] The silica-titania composite oxide powder of the present embodiment does not contain coarse particles and has excellent transparency when filled into an organic polymer, so it can be suitably used as a filler for resin compositions for electronic materials that require such properties. Furthermore, when added to a resin, it provides excellent flowability of the resin composition when melted, and allows control of the transparency of the molded product and precise control of the surface irregularities, so it can be suitably used for various molded product applications, including film applications.
[0036] The type of resin to be mixed with the silica-titania composite oxide powder of the present embodiment is not particularly limited. The type of resin may be appropriately selected depending on the desired application, but taking into account the refractive index, examples of the resin include epoxy resin, acrylic resin, silicone resin, polyester resin, and olefin resin.
[0037] For example, for semiconductor encapsulation applications, epoxy resins, acrylic resins, silicone resins, etc. are preferred, while for film applications, olefin resins (polypropylene, polyethylene, polystyrene, etc.) and polyester resins are preferred.
[0038] Furthermore, when used as a structure, polycarbonate, acrylic resin, etc. are preferred.
[0039] In the composition in which the silica-titania composite oxide powder is added to the resin, the loading amount of the silica-titania composite oxide powder may be appropriately adjusted according to the application and purpose. Specifically, when used as a semiconductor encapsulant, the loading amount is preferably in the range of 30 to 900 parts by mass per 100 parts by mass of the resin component, and when used as a film, the loading amount is preferably in the range of 0.01 to 10 parts by mass per 100 parts by mass of the resin component. When used as a structural material, the loading amount is preferably in the range of 0.01 to 100 parts by mass per 100 parts by mass of the resin component.
[0040] When the silica-titania composite oxide powder of this embodiment is added to a resin to be used as a resin composition, it is of course possible to contain other components, such as a different filler, as necessary.
[0041] Furthermore, the silica-titania composite oxide powder of this embodiment can be used as a raw material for producing the above-mentioned films, paints, and the like in a state where it is dispersed in a solvent.
[0042] <<Method of manufacturing silica-titania composite oxide powder>> The silica-titania composite oxide powder of this embodiment can basically be produced by the so-called sol-gel method using the silicon alkoxide and titanium alkoxide shown below (hereinafter referred to as this production method). (1) A process for preparing a composite alkoxide raw material by mixing silicon alkoxide and titanium alkoxide to form a composite (hereinafter referred to as the composite process). (2) A process in which a nitrogen-containing base catalyst is placed in a dispersion medium containing water, the composite alkoxide raw material is added thereto, and composite oxide particles are generated by a reaction of hydrolysis and condensation, thereby obtaining a dispersion liquid in which the composite oxide particles are dispersed in the dispersion medium (hereinafter also referred to as a reaction process). (3) A step of subjecting the dispersion to solid-liquid separation (4) Drying the solids (5) The dried product is fired.
[0043] The sol-gel method is well known, but in order to obtain the silica-titania composite oxide powder of the present embodiment, the nitrogen content is adjusted to be within the following range after the drying step (4) and before the firing step (5). Nitrogen content (mass%)<0.19×Ti content+0.35 (Note that the Ti content is the percentage of Ti when the total amount of Ti and Si on a molar basis is 100%) By satisfying the above formula, that is, by making the nitrogen content smaller than the above numerical value, it is possible to reduce the number of fine voids remaining after the subsequent firing step, and to obtain composite oxide particles with small variations in refractive index.
[0044] If necessary, it is possible to carry out a process of filtering the raw material liquid or each process liquid to remove impurities, or a process of crushing and classifying the dried powder or the fired powder.
[0045] Each of the above steps will be described below, but steps (1) to (3) and (5) may be carried out in the same manner as steps widely known as a method for producing a composite oxide by a sol-gel method, and therefore, the steps not described below may be carried out by appropriately selecting such known techniques. In addition, the method described below may be carried out by modifying it as necessary.
[0046] (1) Composite process In this production method, first, a composite alkoxide is prepared by combining a silicon alkoxide and a titanium alkoxide.
[0047] Known methods can be used for the composite formation. For example, as described in Patent Document 4, a method in which water is added to a silicon alkoxide to prepare a partially hydrolyzed alkoxide, and this liquid is mixed with a titanium alkoxide can be preferably used.
[0048] As the alkoxide of silicon, alkoxides such as tetramethoxysilane, tetraethoxysilane, and tetrapropoxide can be used.
[0049] Examples of alkoxides of titanium that can be used include alkoxides such as titanium tetraisopropoxide, titanium tetra-n-butoxide, etc. Among these, titanium tetraisopropoxide is particularly preferred because it is easily available industrially and is easy to handle.
[0050] The titanium alkoxide and the silicon alkoxide may each be used alone, or two or more of each may be used in combination.
[0051] The alkoxide is preferably used in combination with an organic solvent such as alcohol, etc. In this case, the type of organic solvent may be changed depending on the alkoxide used.
[0052] The amount of the organic solvent used can be adjusted depending on the particle size and the desired particle size distribution.
[0053] The amount of water used in the partial hydrolysis may be an appropriate amount.
[0054] In addition, it is preferable to use a catalyst in order to rapidly promote the partial hydrolysis of silicon alkoxide and the composite formation of alkoxide. The catalyst is preferably an acid, and specific examples thereof include hydrochloric acid, sulfuric acid, nitric acid, and oxalic acid. It is preferable to use an acid after adjusting the pH of the aqueous solution to a range of 1 to 4.
[0055] Hereinafter, the alkoxide obtained by the above-mentioned composite is called a composite alkoxide.
[0056] In the above composite, the silicon alkoxide bonded to the titanium alkoxide may be a monomer or an oligomer. The composite alkoxide is an alkoxide having one Ti atom, at least 3 to 4 Si atoms, and at least 10 to 12 alkoxy groups in one molecule. In addition, the composite alkoxide may have some alkoxy groups hydrolyzed.
[0057] In this embodiment, the ratio of the alkoxide of silicon to the alkoxide of titanium used can be changed according to the desired refractive index.
[0058] A part of the silicon alkoxide is used for the composite with the titanium alkoxide, but it is not necessary that the entire amount of the silicon alkoxide is used for the composite.
[0059] (2) Reaction process In this manufacturing method, the composite alkoxide prepared as described above is used as a raw material, and a particulate product is obtained from the composite alkoxide raw material. Here, in the above-mentioned composite step, a mixture containing the composite alkoxide is usually obtained, and further containing the alkoxide of silicon and its hydrolyzate, water, and an organic solvent. However, it is not necessary to isolate the composite alkoxide from this mixture, and the mixture can be used as it is.
[0060] In this process, fine particles called nuclei are generated from the composite alkoxide raw material, and the hydroxyl groups present on the surface of the nuclei are condensed with the hydroxyl groups generated by hydrolysis of the composite alkoxide raw material, thereby bonding the alkoxide raw material in the solution to the particle surfaces. This process is repeated countless times to obtain particles of the desired size.
[0061] The particles obtained in this step are grown by repeated condensation as described above.
[0062] The particles have a network structure having continuously bonded Si-O-Si bonds, Si-O-Ti bonds, and partially Ti-O-Ti bonds.
[0063] The particles contain alkoxy groups which remain without being hydrolyzed, Si-OH groups and Ti-OH groups which are generated by hydrolysis of the alkoxy groups and remain without condensing, and basic catalysts, water and solvent components which are chemically bonded to these.
[0064] Thus, the particles obtained in this reaction process have an inorganic skeleton, but also contain various molecules and bonding groups inside, such as the solvent used in the reaction and alcohol generated by hydrolysis.
[0065] The reaction step in this production method can be carried out by a known method, such as a method in which the above-mentioned composite alkoxide raw material is added to an alkaline solvent to obtain a composite oxide as described in Patent Document 3, or a method in which an alkaline aqueous solution is added together with the addition of the composite alkoxide raw material to compensate for the water raw material due to hydrolysis as described in Patent Document 4.
[0066] In the sol-gel method, the reaction system is usually carried out under basic conditions for the above hydrolysis and condensation, but in the present production method, a nitrogen-containing basic catalyst is used. The nitrogen-containing basic catalyst does not contain components that are difficult to remove after the reaction, and in particular, the possibility that alkali metals and the like are contained in the produced composite oxide can be eliminated. Examples of such nitrogen-containing basic catalysts include ammonia, quaternary ammonium hydroxide, and various amine compounds. Examples of such amine compounds include methylamine, dimethylamine, trimethylamine, ethylamine, dimethylamine, and trimethylamine. Examples of quaternary ammonium hydroxide include hydroxides such as tetramethylammonium and tetraethylammonium. Among these, it is particularly preferable to use ammonia because it is highly volatile and easy to remove, and the reaction rate of the sol-gel method is fast.
[0067] The proportion of the nitrogen-containing basic catalyst used may be appropriately determined taking into consideration the reaction rates of the hydrolysis and polycondensation reactions of the metal alkoxide, etc. The proportion of the nitrogen-containing basic catalyst used is usually required to make the pH of the reaction solution 8 or higher.
[0068] The amount of each raw material used in the reaction step of the present production method may be appropriately selected from known ranges and determined so as to obtain a silica-titania powder having the desired refractive index and particle size, taking into consideration the configuration of the reaction apparatus and the reaction scale.
[0069] The reaction equipment used in the production method of this embodiment is preferably equipment having a reactor equipped with a stirring device, a supply device and a liquid supply pipe capable of controlling the amount of added liquid, and further a temperature control device for maintaining the temperature of the reaction liquid.
[0070] The reaction temperature is not particularly limited as long as it is a temperature at which the sol-gel reaction proceeds smoothly depending on the types of raw materials used, and may be appropriately selected from a known range depending on the particle size of the desired silica-titania composite oxide particles. In order to obtain silica-based composite oxide particles with an average particle size of 0.1 to 3.0 μm, the reaction temperature is preferably in the range of −10 to 60° C.
[0071] In order to ensure the progress of the reaction, after the addition of the liquid is completed, stirring may be continued at a temperature approximately equal to the reaction temperature, i.e., a so-called aging operation may be performed. The time for aging is preferably 0.25 to 5 hours.
[0072] In order to obtain particles of a desired size, a part of the liquid after the reaction may be used to continue the reaction using the same composite alkoxide raw material.
[0073] By the above-mentioned method, a dispersion liquid of silica-titania composite oxide particles having an average particle size of 0.1 to 3.0 μm as determined by the laser diffraction scattering method is obtained.
[0074] In the above dispersion, the silica-titania composite oxide particles are obtained in a well-dispersed state without forming substantially any adhered particles or agglomerates, but due to localized excessive reaction progress, there is a possibility that a small amount of coarse independent primary particles having a particle size of more than 5 μm are mixed in. Therefore, in order to remove such coarse particles, it is preferable to carry out filtering after the completion of the reaction process.
[0075] (3) Solid-liquid separation Next, the silica-titania composite oxide particles obtained by the reaction step are separated from the reaction solution. The liquid after the reaction contains miscellaneous substances such as unreacted alkoxide, nitrogen-containing basic catalyst, water, and solvent (hereinafter, the components contained in the reaction solution other than the silica-titania composite oxide particles are referred to as reaction solution components).
[0076] As a method for separation, a known method can be used, such as a method of removing the solvent by evaporation and separating the evaporation residue containing the silica-titania composite oxide particles, a method of settling the silica-titania composite oxide particles by centrifugal force and gravity, and then removing the supernatant to obtain a concentrate containing the silica-titania composite oxide particles, and a method of passing the reaction liquid through a filter medium to obtain a concentrate containing the silica-titania composite oxide particles captured on the filter medium.
[0077] In addition, a method that combines the above methods, for example, a method in which a filter medium is placed in a centrifuge container, the solution that passes through the filter medium is removed by centrifugal force, and a concentrate containing filter-like silica-titania composite oxide particles is obtained can be preferably used.
[0078] Among the above, the method involving filtration is particularly preferred because it is easy to reduce the nitrogen content, which will be described later.
[0079] Furthermore, in order to facilitate the solid-liquid separation operation, a method of adding a coagulant to the reaction liquid to form a loose aggregate, promote sedimentation, or improve filterability may be used in combination.
[0080] It is also preferable to further carry out washing after filtration, since this makes it easier to reduce the nitrogen content.
[0081] <Reduction of nitrogen content> The concentrate containing silica-titania composite oxide particles obtained by solid-liquid separation contains not only reaction solution components that simply remain in the gaps between the silica-titania composite oxide particles, but also unreacted alkoxy groups, uncondensed Si-OH groups, and Ti-OH groups present inside the silica-titania composite oxide particles, and reaction solution components chemically bonded to these.
[0082] The reaction solution components remaining between the silica-titania composite oxide particles easily flow out when used as an inorganic filler, and become a factor that hinders mixing with organic polymers. In addition, unreacted alkoxy groups and uncondensed Si-OH and Ti-OH groups usually exist in the form of fine voids, which are a factor that reduces the physical properties of the silica-titania composite oxide particles, such as their mechanical strength, and also have a negative effect on the refractive index. Furthermore, since such fine voids are not uniformly present, the refractive index of each silica-titania composite oxide particle is likely to differ, and therefore the variation in the refractive index becomes large.
[0083] Therefore, in order to obtain the silica-titania composite oxide powder of this embodiment, it is necessary to heat the concentrate obtained by solid-liquid separation as described below to remove the reaction liquid components and to convert the unreacted alkoxy groups and uncondensed Si-OH groups and Ti-OH groups to MOM (M is Si or Ti).
[0084] Here, what is more important in obtaining the silica-titania composite oxide powder of the present embodiment is to satisfy the following relational expression before the temperature is raised to 400° C. or higher in the above heating. Nitrogen content (mass%)<0.19×Ti content+0.35 (Note that the Ti content is the percentage of Ti when the total amount of Ti and Si on a molar basis is 100%) The reason why such a requirement must be met is unclear, but the following is considered.
[0085] That is, at temperatures generally above 400°C, mainly in the temperature range of 400°C to 600°C, many of the reaction solution components that are chemically bonded to unreacted alkoxy groups and uncondensed Si-OH groups or Ti-OH groups present in the particles are decomposed or detached, and most of the Si-OH groups or Ti-OH groups are condensed into MOM.
[0086] In the present production method, as described above, a nitrogen-containing basic catalyst is used, but the basic catalyst is not completely separated by solid-liquid separation, and a part of it is chemically bonded to the above-mentioned Si-OH groups and Ti-OH groups (hereinafter collectively referred to as "hydroxyl groups"), and therefore the area near the hydroxyl groups is spatially occupied by the nitrogen-containing basic catalyst.
[0087] If such a hydroxyl group does not have a nitrogen-containing basic catalyst nearby, it will condense with other nearby hydroxyl groups (becoming MOM) when heated, and the network structure will simply be strengthened. On the other hand, if the vicinity of a hydroxyl group is spatially occupied by a nitrogen-containing basic catalyst, the hydroxyl group cannot approach other hydroxyl groups and cannot condense. For this reason, it is thought that if there is a large amount of remaining nitrogen-containing basic catalyst, there will be many hydroxyl groups that cannot condense.
[0088] Of course, when the temperature is raised, the nitrogen-containing basic catalyst is decomposed and released, and the hydroxyl group becomes free to move, but on the other hand, when the temperature reaches the decomposition temperature, most of the other hydroxyl groups have already finished condensation, and there are no hydroxyl groups in the vicinity of this hydroxyl group that can react with it, and the network structure is considered to be stronger. Therefore, after the nitrogen-containing basic catalyst is released, the fine gaps as mentioned above are left behind.
[0089] Due to the above mechanism, when the nitrogen content in the concentrate is high (i.e., when the amount of nitrogen-containing basic catalyst is large), if the concentrate is fired at a high temperature as is, many fine voids will be generated in the silica-titania composite oxide particles, and the variation in the amount of voids in each silica-titania composite oxide particle will become relatively large, and therefore the variation in the refractive index of each silica-titania composite oxide particle will become large. In order to avoid the occurrence of such a phenomenon, in the present production method, the nitrogen content in the concentrate is highly reduced as shown in the above formula.
[0090] As shown in the formula, the higher the titanium content, the higher the allowable nitrogen content.
[0091] This is because when the titanium content is low, i.e., when the silica content is high, the network structure tends to become stronger, and therefore rearrangement of the network structure that reduces fine voids is less likely to occur even at the same temperature.
[0092] On the other hand, apart from the influence on the variation in the refractive index, if baking (heating at high temperature) is performed in a state where the solvent component, particularly the organic solvent component, among the reaction liquid components remains, various problems such as the risk of fire may occur in the workability. For this reason, drying is usually performed. Drying is often accompanied by heating, but the above-mentioned events involving the risk of fire, etc. do not usually occur when heating for drying. In addition, the nitrogen content may change (usually decrease) as a result of drying.
[0093] Therefore, in the present production method, drying is performed before firing, so that the nitrogen content in the dried product before firing satisfies the above formula.
[0094] In this production method, the term "calcination" refers to applying a temperature of 400°C or higher. Even when the drying is performed with heating, the upper limit of the temperature must be less than 400°C, preferably less than 300°C.
[0095] Below, several methods for making the nitrogen content satisfy the above formula when the dried material is obtained will be described.
[0096] For example, there can be mentioned a method of washing (preferably with water) multiple times after filtration, a method of drying for a long time or at a relatively high temperature, a method of drying under conditions that make it easy to remove volatile components such as air drying or reduced pressure drying, etc. The following two methods are particularly preferred.
[0097] (I) One of the preferred methods for reducing the nitrogen content of the dried powder after solid-liquid separation is to reduce the nitrogen-containing basic catalyst by acidifying the silica-titania composite oxide particle dispersion.
[0098] As described above, the reaction step is carried out under a basic condition to obtain the desired silica-titania composite oxide particles, and a silica-titania composite oxide particle dispersion is obtained upon completion of the reaction step. In order to reduce the nitrogen content of the powder after solid-liquid separation and drying, a method of adding an acid to the dispersion before solid-liquid separation to make it acidic and then carrying out solid-liquid separation can be mentioned. The nitrogen-containing basic catalyst reacts with the added acid to form a salt rather than with the hydroxyl group as described above, and therefore is easily removed by washing with water.
[0099] The acid used to neutralize and acidify the dispersion may be an inorganic acid such as hydrochloric acid, sulfuric acid, nitric acid, or phosphoric acid, or an organic acid such as citric acid or acetic acid.
[0100] The amount of acid to be added may be an amount that can adjust the pH of the reaction liquid or dispersion to 7 or less, but in order to efficiently reduce the basic catalyst contained inside the silica-titania composite oxide particles, it is preferable to add an amount of acid that can adjust the pH of the particle dispersion to 4 or less, more preferably 3 or less. The temperature at which the acid is added is preferably the same as or higher than the temperature used for the reaction in order to effectively reduce the basic components.
[0101] When this method is adopted, the solid-liquid separation should be carried out by a method involving filtration.
[0102] The above method is carried out on the dispersion before solid-liquid separation. However, instead of adding an acid to the dispersion before solid-liquid separation, a method may be used in which a concentrate containing particles obtained by solid-liquid separation is dispersed in a liquid not containing a basic catalyst, and then an acid is added thereto and then solid-liquid separation is carried out.
[0103] This method is preferable because the amount of acid required is less than that when the acid is added directly to the reaction solution. The method of dispersing the concentrate is preferably a method of stirring the collected concentrate while adding a washing liquid. A known stirring method can be used. The solution added when dispersing the concentrate is preferably water or an organic solvent. The amount of solution added when dispersing the concentrate is preferably in the range of 5 to 50 mass% of the silica-titania composite oxide particles. If it is less than 5%, the amount of solution used increases, which is not preferable. On the other hand, if the concentration of the silica-titania composite oxide particles is higher than 50%, strong stirring is required to disperse the concentrate, which is not preferable. The temperature of the liquid in which the silica-titania composite oxide particles are dispersed is preferably the temperature used in the reaction or higher, because the basic catalyst can be efficiently removed.
[0104] The solid matter is then collected again by filtration. Alternatively, after the solid-liquid separation is performed by adding an acid to the dispersion before the solid-liquid separation, the concentrate containing the particles obtained by the solid-liquid separation may be dispersed in a liquid not containing a basic catalyst, and then an acid may be added thereto, followed by the solid-liquid separation.
[0105] (II) Another method for reducing the nitrogen content of the dried powder after solid-liquid separation is to contact the silica-titania composite oxide particles with a gas containing water vapor in the drying step described below.
[0106] This method involves contacting the particles with water vapor to replace the nitrogen-containing basic catalyst remaining on the particle surface with hydroxyl groups, thereby reducing the nitrogen content in the dry powder that is attributable to the nitrogen-containing basic catalyst.
[0107] Gas containing water vapor is gas containing water vapor at a partial pressure of 0.05 to 0.5 relative to the total gas. If the partial pressure of water vapor is less than 0.05, it is not possible to effectively replace the nitrogen-containing basic catalyst, and the same amount of nitrogen remains as in normal drying. On the other hand, if a gas with a partial pressure of water vapor greater than 0.5 is used, drying does not proceed, and replacement with the nitrogen-containing basic catalyst cannot be performed efficiently.
[0108] The temperature of the gas containing water vapor is preferably 60°C or higher. This is because the nitrogen-containing basic catalyst is difficult to remove when the gas temperature is low. The gas temperature is also preferably 200°C or lower. When the temperature is high, the nitrogen-containing basic catalyst is easily removed, but the condensation reaction of the hydroxyl group is also likely to proceed, and the network structure becomes strong while the nitrogen-containing basic catalyst is still included, which is not preferable. The time for introducing the gas containing water vapor is not particularly limited, but is usually in the range of 30 minutes to 8 hours.
[0109] Silica-titania composite oxide particles that come into contact with a gas containing water vapor are likely to become water-incorporated, and therefore must be dried separately in a gas that does not contain water vapor.
[0110] The above-mentioned operations for reducing the amount of nitrogen may be carried out alone, or the operations may be combined to more efficiently reduce the nitrogen content.
[0111] (4) Drying process In the present production method, drying is a process for removing the reaction solution components present between the silica-titania composite oxide particles and a part of the reaction solution components remaining inside the particles. The removal of these components is accompanied by a significant change in mass.
[0112] The end of drying is when no significant mass loss occurs even if drying is continued under the same conditions, that is, when the reaction solution components remaining between the silica-titania composite oxide particles and some of the reaction solution components remaining in the silica-titania composite oxide particles and easily removed have been sufficiently removed. Furthermore, the mass loss is expected to be 3% or less in terms of mass change, but since the adverse effects of other components are significantly less than the nitrogen content, it is not necessary to stick to this value of 3%.
[0113] In the present production method, the drying method is not particularly limited, and in addition to static drying, air drying, drying under reduced pressure, etc. can be used.
[0114] The drying temperature depends on the solvent components used, but is preferably above the boiling point of the solvent. If the drying is carried out at atmospheric pressure, the drying temperature is preferably 70°C to 200°C. The drying time is not particularly limited, but is preferably about 2 to 48 hours. By carrying out such drying, the dried material can be obtained as a powder. Hereinafter, the dried material will be referred to as "dried powder".
[0115] The nitrogen content may decrease as a result of the drying, depending on the drying method, etc. Therefore, in the present production method, it is not necessarily necessary to know the nitrogen content at the time when the operation for decreasing the nitrogen content is carried out, and it is sufficient to know and manage the nitrogen content at the stage of the dried powder before firing.
[0116] The nitrogen content in the dried material can be calculated using a general CHN analyzer. When applying the formula above, the nitrogen content is calculated in percentage.
[0117] The Ti content can be determined from the charge amount of the raw materials, and can be confirmed after firing if necessary.
[0118] (5) Firing process Various components remain inside the silica-titania composite oxide particles after the drying process described above, and the skeletal structure is weak and does not provide the hardness and excellent thermal stability required for inorganic substances. Therefore, in this production method, firing is performed to remove the remaining components and obtain a strong skeletal structure.
[0119] As mentioned above, the unreacted alkoxy groups and uncondensed hydroxyl groups remaining in the silica-titania composite oxide particles, as well as many of the reaction solution components chemically bonded to these, are decomposed and eliminated by firing in the temperature range of 400°C to 600°C, and the mechanical strength is improved, but some of the hydroxyl groups remain, causing fine voids. The proportion of these fine voids is not uniform in each silica-titania composite oxide particle. For this reason, the refractive index difference between each silica-titania composite oxide particle is large, and the value of the minimum absorbance S cannot be made sufficiently small.
[0120] Therefore, in the present production method, the silica-titania composite oxide powder of the present embodiment is obtained by performing calcination at a higher temperature, specifically at a temperature of 800° C. or higher. That is, when the calcination temperature is increased, the formed network structure is easily rearranged, and generally, more Si—OH groups and Ti—OH groups are removed.
[0121] As a result, the proportion of microvoids in any given particle decreases, decreasing the minimum absorbance.
[0122] On the other hand, when the firing temperature is increased, the hydroxyl groups present in the vicinity of the contact points between particles undergo a condensation reaction with the hydroxyl groups of the adjacent silica-titania composite oxide particles.
[0123] As condensation between silica-titania composite oxide particles progresses, the particles tend to become one with each other, and when such a combination is formed of a plurality of silica-titania composite oxide particles, aggregate particles are formed.
[0124] The formation of such agglomerated particles varies depending on the circumstances and cannot be generalized, but it is likely to occur when firing is performed at a temperature exceeding 1100°C, and agglomerated particles can also occur when firing at 1000°C to 1100°C.
[0125] Therefore, the firing temperature should be 1100° C. or lower, and more preferably 1000° C. or lower.
[0126] The firing can be carried out by a known method, and generally, a method in which a container filled with dry powder is placed in a furnace at a desired temperature can be preferably used.
[0127] The calcination time is not particularly limited as long as the above-mentioned calcination objective can be achieved. However, if the calcination time is too long, the productivity decreases, so it is sufficient to calcinate the mixture by maintaining the temperature at the desired calcination temperature for 0.5 to 48 hours, more preferably 2 to 24 hours.
[0128] The atmosphere during firing is not particularly limited, and firing can be performed in an inert gas atmosphere such as argon or nitrogen, or in the air. EXAMPLES
[0129] The present embodiment will be described in detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0130] (Measuring the average refractive index and minimum absorbance) A number of mixed solvents with different refractive indices were prepared by mixing toluene, 1-bromonaphthalene, 1-chloronaphthalene, diiodomethane, sulfur-containing diiodomethane, 2-methoxyethanol and benzyl alcohol in various ratios.
[0131] 14.0 g of the above mixed solvent was placed in a 30 ml clean glass container, and 6.0 g of silica-titania composite oxide powder that had been dried at 100°C for 24 hours was weighed and added. After that, the mixture was dispersed using an ultrasonic homogenizer (BRANSON, Sonifier250) at 20 W for 1 minute, and then the dispersion was introduced into a quartz cell (optical path length 10 mm) for measuring absorbance.
[0132] As a blank, a mixed solvent containing no silica-titania composite oxide powder was introduced into the quartz cell.
[0133] The above quartz cell was attached to a spectrophotometer (JASCO Corporation, UV-Visible Spectrophotometer V-650) equipped with a temperature control folder, and the absorbance was measured to four decimal places under the following conditions.
[0134] Measurement wavelength: 589 nm Temperature range: 5℃~40℃ Measurement temperature interval: 1℃
[0135] For the condition showing the lowest absorbance, it was confirmed that the absorbance was a minimum value, and the absorbance value at this time was taken as the minimum absorbance S.
[0136] The refractive index of the mixed solvent that showed the minimum absorbance at a wavelength of 589 nm at the temperature at which the minimum absorbance was shown was taken as the average refractive index of the silica-titania composite oxide powder.
[0137] The average refractive index was determined by measuring the refractive index of each mixed solvent at a wavelength of 589 nm to four decimal places using an Abbe refractometer at temperatures ranging from 5°C to 40°C.
[0138] (Volume-based cumulative 50% diameter (average particle size)) Approximately 0.1 g of silica-titania composite oxide powder was weighed out on an electronic balance into a 50 mL glass bottle, and approximately 40 mL of distilled water was added. The powder was dispersed using an ultrasonic homogenizer (BRANSON, Sonifier250) at 40 W for 10 minutes. The volume-based cumulative 50% diameter (μm) and coefficient of variation of the silica-titania composite oxide powder were then measured using a laser diffraction / scattering particle size distribution analyzer (Beckman Coulter, LS-230).
[0139] (Amount of coarse particles of 5μm or more measured by Coulter counter method) Five 50mL glass bottles were prepared, and 1g of silica-titania composite oxide powder was weighed out into each vial using an electronic balance. 19g of distilled water or ethanol was added to each vial, and the powder was dispersed at 40W for 10 minutes using an ultrasonic homogenizer (BRANSON, Sonifier250) to prepare the measurement samples. The particle size of each silica-titania composite oxide particle in each sample was measured using a Coulter counter (Beckman Coulter, MultisizerIII). The number of particles measured per sample was approximately 50,000, and the total number of particles measured for the five samples was approximately 250,000. The number of particles with a particle size of 5μm or more was calculated, and the amount of coarse particles (ppm) relative to the total number measured was calculated.
[0140] (Nitrogen content) The nitrogen content in the dried powder was measured as follows: The dried powder was heated to 950°C in an oxygen atmosphere, and the nitrogen content was determined using a CHN analyzer (Yanagimoto Seisakusho: CHN Coder MT-5).
[0141] <Example 1> A 200 ml three-necked glass flask was charged with 54.6 g of tetramethoxysilane (manufactured by Tama Chemical Industry Co., Ltd., ortho-methyl silicate, hereinafter referred to as TMOS) as a metal alkoxide, 5.5 g of methanol as an organic solvent, and 2.2 g of 0.035 mass % hydrochloric acid as an acid catalyst, and the mixture was stirred with a stirrer at room temperature for 10 minutes to hydrolyze the TMOS.
[0142] Next, 8.9 g of titanium tetraisopropoxide (A-1 (hereinafter, TPT) manufactured by Nippon Soda Co., Ltd.) was charged as a metal alkoxide into a 30 ml glass container, and 8.9 g of isopropyl alcohol (hereinafter, IPA) was added while stirring with a stirrer.
[0143] The diluted TPT solution was added to the hydrolyzed TMOS solution being stirred with a stirrer to obtain 80.1 g of a transparent composite alkoxide solution.
[0144] The titania content calculated from the amount of alkoxide used was 8.0 mol%.
[0145] A 300 ml four-neck flask was equipped with a propeller-equipped stirrer, and 6.1 g of IPA, 43.0 g of methanol, and 9.4 g of 25% by mass ammonia water were charged and kept at 40° C. while stirring. The above composite alkoxide solution and 28.1 g of 25% by mass ammonia water were dropped into the liquid separately. After starting the addition of the raw materials, the solution turned white 30 minutes later. After that, the supply of the raw materials was completed in 4.3 hours while adjusting the addition rate, and silica-titania composite oxide particles were grown.
[0146] After the dropping was completed, the dispersion was dispensed into a centrifuge tube and centrifuged at 6000 rpm to obtain a concentrate containing particles.
[0147] Pure water was added to this concentrate, and the concentrate was dispersed using a stirrer and heated to 40° C. 1.0 N hydrogen chloride was added to this liquid to adjust the pH of the dispersion to 4.
[0148] This liquid was centrifuged to obtain a concentrate containing the particles.
[0149] The obtained concentrate was introduced into a vacuum dryer and kept at 100°C. The weight stabilized 4 hours after the start of drying. A portion of the powder was taken out after the drying was completed and the nitrogen content was measured, which was 1.71%. This value was smaller than the value of 1.87 calculated by 0.19 × Ti content + 0.35 from the Ti charge of 8.0%.
[0150] The dried powder was sintered under the conditions of a heating rate of 5°C / min, a sintering temperature of 900°C, and a sintering holding time of 12 hours.
[0151] The silica-titania composite oxide powder obtained by calcination was measured with a laser particle size distribution analyzer, and the average particle size was found to be 0.64 μm. As a result of the coarse particle measurement, the particles of 5 μm or more were 46 ppm. The average refractive index of the particles was 1.504. The minimum absorbance S was 0.0135, which was significantly smaller than the value calculated from the average particle size of 0.64 μm (0.026-0.008×D=0.0209).
[0152] <Comparative Example 1> Silica-titania composite oxide particles were obtained in the same manner as in Example 1, except that the reaction liquid was centrifuged and dried as it was.
[0153] The nitrogen content of the dry powder was 2.11%, which was greater than the value of 1.87 calculated by 0.19 × Ti content + 0.35 from the Ti content of 8.0%.
[0154] The silica-titania composite oxide powder obtained by firing was measured with a laser particle size distribution analyzer, and the average particle size was 0.64 μm. As a result of the coarse particle measurement, the particles of 5 μm or more were 42 ppm. The average refractive index of the particles was 1.504. The minimum absorbance S was 0.0310, which was greater than 0.0209.
[0155] <Example 2> Silica-titania composite oxide particles were obtained in the same manner as in Example 1, except that the supply of the raw materials was completed in 2.4 hours in Example 1. The nitrogen content of the dried powder was 1.73%.
[0156] The silica-titania composite oxide powder obtained by calcination was measured with a laser particle size distribution analyzer, and the average particle size was found to be 0.35 μm. Coarse particle measurements showed that particles of 5 μm or more constituted 84 ppm. The average refractive index of the particles was 1.504. The minimum absorbance S was 0.0148, which was significantly smaller than the value calculated from the average particle size of 0.35 μm (0.026-0.008×D=0.0232).
[0157] <Comparative Example 2> Silica-titania composite oxide particles were obtained in the same manner as in Example 2, except that the reaction liquid was centrifuged and directly used for drying in Example 2. The nitrogen content of the dried powder was 2.35%.
[0158] The silica-titania composite oxide powder obtained by firing was measured with a laser particle size distribution analyzer, and the average particle size was 0.35 μm. As a result of the coarse particle measurement, the particles of 5 μm or more were 88 ppm. The average refractive index of the particles was 1.504. The minimum absorbance S was 0.0271, which was greater than 0.0232.
[0159] <Example 3> Silica-titania composite oxide particles were obtained in the same manner as in Example 1, except that the dried powder obtained in Example 2 was calcined at a calcination temperature of 1000°C.
[0160] The silica-titania composite oxide powder obtained by calcination was measured with a laser particle size distribution analyzer, and the average particle size was found to be 0.34 μm. As a result of the coarse particle measurement, the number of particles 5 μm or larger was 284 ppm. The average refractive index of the particles was 1.504. The minimum absorbance was 0.0139, which was significantly smaller than the value calculated from the average particle size of 0.34 μm (0.026-0.008×D=0.0233).
[0161] <Example 4> A 200-mL three-necked glass flask was charged with 51.6 g of TMOS as a metal alkoxide, 5.5 g of methanol as an organic solvent, and 3.7 g of 0.035% by mass hydrochloric acid as an acid catalyst, and the mixture was stirred with a stirrer at room temperature for 10 minutes to hydrolyze the TMOS.
[0162] Next, 14.4 g of TPT was charged as a metal alkoxide in a 50 ml glass container, and 8.9 g of IPA was added thereto while stirring with a stirrer.
[0163] The diluted TPT solution was added to the hydrolyzed TMOS solution being stirred with a stirrer to obtain 84.1 g of a transparent composite alkoxide solution.
[0164] The titania content calculated from the amount of alkoxide used was 13.0 mol%.
[0165] A 300 ml four-neck flask was equipped with a propeller-equipped stirrer, and 6.1 g of IPA, 43.0 g of methanol, and 9.4 g of 25% by mass ammonia water were charged and kept at 40° C. while stirring. The above composite alkoxide solution and 28.1 g of 25% by mass ammonia water were dropped into the liquid separately. After starting the addition of the raw materials, the solution turned white 30 minutes later. After that, the supply of the raw materials was completed in 11.4 hours while adjusting the addition rate, and silica-titania composite oxide particles were grown.
[0166] After the dropping was completed, the dispersion was dispensed into a centrifuge tube and centrifuged at 6000 rpm to obtain a concentrate containing particles.
[0167] This liquid was centrifuged to obtain a concentrate containing the particles.
[0168] The obtained concentrate was introduced into a vacuum dryer and kept at 100°C. Eight hours after the start of drying, the pressure was returned to atmospheric pressure, and the mixture was introduced into a tubular dryer (inner volume 0.4 L) previously kept at 100°C, and air with a partial pressure of water vapor of 0.3 was circulated at 20 ml / min for four hours. After the introduction of water vapor was terminated, vacuum drying was carried out again. The weight stabilized 16 hours after the start of re-drying. A portion of the powder after this drying was taken out and the nitrogen content was measured, which was 2.68%. This value was smaller than the value of 2.82 calculated from the Ti charge value of 13.0% (0.19 × Ti content + 0.35).
[0169] The dried powder was sintered under the conditions of a heating rate of 5°C / min, a sintering temperature of 900°C, and a sintering holding time of 12 hours.
[0170] The silica-titania composite oxide powder obtained by calcination was measured with a laser particle size distribution analyzer, and the average particle size was found to be 1.35 μm. Coarse particle measurements showed that particles of 5 μm or more constituted 28 ppm. The average refractive index of the particles was 1.543. The minimum absorbance S was 0.0123, which was significantly smaller than the value calculated from the average particle size of 1.35 μm (0.026-0.008×D=0.0152).
[0171] <Comparative Example 3> Silica-titania composite oxide particles were obtained in the same manner as in Example 4, except that the vacuum drying was continued for 16 hours and the operation of contacting with a gas containing water vapor was not performed during the process.
[0172] The nitrogen content of the dry powder was 3.04%, which was greater than the value of 2.82 calculated by multiplying the Ti content by 13.0% by 0.19 × Ti content + 0.35.
[0173] The silica-titania composite oxide powder obtained by calcination was measured with a laser particle size distribution analyzer, and the average particle size was 1.35 μm. As a result of the coarse particle measurement, the particles of 5 μm or more were 24 ppm. The average refractive index of the particles was 1.543. The minimum absorbance S was 0.0168, which was greater than 0.0152.
Claims
1. A silica-titania composite oxide powder having an average particle diameter D (μm) in the range of 0.1 μm or more and 3.0 μm or less as measured by a laser scattering method, an average refractive index at a measurement wavelength of 589 nm as measured by a liquid immersion method of 1.47 or more, and a minimum absorbance S obtained by dispersing 30 mass % of silica-titania composite oxide particles in a liquid having the same refractive index as the average refractive index and measuring the same satisfies the following relationship: S<0.026-0.008×D
2. 2. The silica-titania composite oxide powder according to claim 1, wherein the proportion of particles having a size of 5 μm or more as measured by a Coulter counter method is 200 ppm or less on a number basis.
3. A method for producing silica-titania composite oxide particles using silicon alkoxide and titanium alkoxide as raw materials includes the steps of: mixing silicon alkoxide and titanium alkoxide to prepare a composite alkoxide raw material; reacting the composite alkoxide raw material in the presence of water and a nitrogen-containing base catalyst to produce particles; subjecting the produced particles to solid-liquid separation; drying the particles; and calcining the dried particles, wherein the nitrogen content of the particles after drying is within the following range compared to before calcination. Nitrogen content (mass%) < 0.19 x Ti content + 0.35 (Note that the Ti content is the Ti content expressed in % when the total amount of Ti and Si on a molar basis is 100%). The method for producing a silica-titania composite oxide powder is characterized in that
4. A resin composition comprising the silica-titania composite oxide powder according to claim 1 or 2.
5. 3. A dispersion in which the silica-titania composite oxide powder according to claim 1 or 2 is dispersed in a solvent.
Citation Information
Patent Citations
Color liquid crystal display device
JP1991033721A
Epoxy resin composition
JP1994065475A
Production of metal oxide particles
JP1996048505A
Silica composite oxide particle and its production method
JP2003252616A
Polycarbonate resin composition, its molded article, and its manufacturing process
JP2004107470A