Colored photosensitive resin composition, color filter and display device produced using the same

The optimized colored photosensitive resin composition with specific pigment ratios and additives addresses high light transmittance and crosstalk issues in small pixel sizes, enhancing performance in color image sensors.

JP7551799B2Active Publication Date: 2024-09-17DONGWOO FINE CHEM CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023018359
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-09
Publication Date
2024-09-17
Estimated Expiration
2043-02-09

AI Technical Summary

Technical Problem

Existing pigment combinations in colored photosensitive compositions fail to achieve high light transmittance and exacerbate crosstalk issues in small pixel sizes for color image sensors.

Method used

A colored photosensitive resin composition comprising specific ratios of blue and violet pigments, along with a violet dye, an alkali-soluble resin, a photopolymerizable compound, and a photoinitiator, optimized to enhance light transmittance and reduce crosstalk.

Benefits of technology

The composition achieves high light transmittance in the blue region while minimizing crosstalk, with improved developability and residue characteristics, meeting stringent pixel size requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551799000008
    Figure 0007551799000008
  • Figure 0007551799000003
    Figure 0007551799000003
  • Figure 0007551799000004
    Figure 0007551799000004
Patent Text Reader

Abstract

To provide a colored photosensitive composition, a color filter including a color pattern produced therewith, and a display device including the color filter.SOLUTION: A colored photosensitive resin composition includes a colorant, an alkali-soluble resin, a photopolymerizable compound, a photopolymerization initiator, and a solvent, wherein the colorant includes, based on the total weight of the colorant, 60-85 wt.% of a blue pigment (A-1), 5-20 wt.% of a blue pigment (A-2) other than the blue pigment (A-1), 5-20 wt.% of a violet pigment (B) and 0.5-5 wt.% of a violet dye (C). There are also provided a color filter including a color pattern produced therewith, and a display device including the color filter.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a colored photosensitive composition, a color filter including a colored pattern produced using the same, and a display device including the color filter. [Background technology]

[0002] Image sensors are image capturing device components that generate images in mobile phone cameras, DSCs (Digital Still Cameras), etc., and can be largely classified into charge coupled device (CCD) image sensors and complementary metal oxide semiconductor (CMOS) image sensors according to their manufacturing process and application. Among them, color image sensors used in solid-state image sensors generally separate colors by providing color filters with red, green, and blue filter segments on the light receiving element. Recently, the pattern size of color filters mounted on such color image sensors is usually 2 μm or less, which is 1 / 100 to 1 / 200 of the color filter pattern for existing LCDs. As a result, achieving high light transmittance and improving crosstalk of color filters mounted on color image sensors have become even more important factors that affect performance.

[0003] In this regard, Korean Patent Publication No. 10-2006-0047854 discloses the use of a purple colorant, CI Pigment Violet 23, in combination with CI Pigment Blue 15:6 as a colorant for a blue photosensitive composition forming a blue pixel, but the combination of these pigments makes it difficult to achieve the high light transmittance of 400 to 500 nm required for recent image sensors. Also, as the size of pixels becomes increasingly finer, crosstalk increases due to the influence on adjacent green and red pixels.

[0004] Therefore, there is a demand for the development of a colored photosensitive composition that can improve crosstalk, including high light transmittance, which has been difficult to achieve with existing pigment combinations. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Korean Patent Publication No. 10-2006-0047854 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made to improve the above-mentioned problems of the conventional technology, and has an object to provide a colored photosensitive resin composition that can improve crosstalk, including high light transmittance in the blue region, which has been difficult to achieve with existing pigment combinations.

[0007] Another object of the present invention is to provide a color filter including a color pattern produced by using the colored photosensitive resin composition of the present invention, and a display device including the color filter.

[0008] However, the problems to be solved by the present application are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]

[0009] In order to achieve the above object, the present invention provides a colored photosensitive resin composition comprising a colorant, an alkali-soluble resin, a photopolymerizable compound, a photopolymerization initiator, and a solvent, wherein the colorant contains, relative to the total weight of the colorant, 60 to 85 wt % of a blue pigment (A-1), 5 to 20 wt % of a blue pigment (A-2) other than the blue pigment (A-1), 5 to 20 wt % of a violet pigment (B), and 0.5 to 5 wt % of a violet dye (C).

[0010] The present invention also provides a color filter including a colored pattern produced from the colored photosensitive resin composition.

[0011] Furthermore, the present invention provides a display device including the color filter. Effect of the Invention

[0012] The colored photosensitive resin composition according to the present invention can exhibit high light transmittance in the blue region, which has been difficult to achieve with existing pigment combinations, while reducing the transmittance in the wavelength region of 600 nm or more, thereby improving the crosstalk phenomenon, and has good effects on residue characteristics due to improved developability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention relates to a colored photosensitive resin composition, and a color filter and a display device including a colored pattern produced using the same. The colored photosensitive resin composition according to the present invention comprises a colorant, an alkali-soluble resin, a photopolymerizable compound, a photopolymerization initiator, and a solvent, and the colorant comprises 60 to 85% by weight of a blue pigment (A-1), 5 to 20% by weight of a blue pigment (A-2) other than the blue pigment (A-1), 5 to 20% by weight of a violet pigment (B), and 0.5 to 5% by weight of a violet dye (C) based on the total weight of the colorant. The colored photosensitive resin composition of the present invention can exhibit high light transmittance in the blue region, which was difficult to achieve with existing pigment combinations, while reducing the transmittance in the wavelength region of 600 nm or more, thereby improving the crosstalk phenomenon, and it has been experimentally confirmed that the improved developability has a favorable effect on residue characteristics, thereby completing the present invention.

[0014] The colored photosensitive resin composition is characterized in that it is for forming a blue pixel, and the line width of the blue pixel is characterized in that it is 1 μm or less.

[0015] The colored photosensitive resin composition is also characterized in that a coating film produced from the colored photosensitive resin composition has a transmittance of 88.5% or more at a wavelength of 445 nm and a transmittance of 20% or less at a wavelength of 700 nm.

[0016] Each component constituting the colored photosensitive resin composition of the present invention will be described in detail below, but the present invention is not limited to these components.

[0017] <Colored photosensitive resin composition> Coloring agent Blue pigment (A) The colored photosensitive resin composition of the present invention contains a blue pigment as a colorant, specifically, a blue pigment (A-1) and a blue pigment (A-2) other than the blue pigment (A-1).

[0018] Blue pigment (A-1) The blue pigment (A-1) of the present invention can include one or more pigments selected from the group consisting of CI Pigment Blue 15:6, CI Pigment Blue 15, and CI Pigment Blue 16, and can preferably include CI Pigment Blue 15:6.

[0019] The blue pigment (A-1) is contained in an amount of 60 to 85% by weight, and more preferably 60 to 80% by weight, based on the total weight of the colorant.

[0020] When the blue pigment (A-1) satisfies the above range, there is an advantage in that the light transmittance in the blue region is improved.

[0021] Blue pigment (A-2) The blue pigment (A-2) of the present invention may include one or more selected from the group consisting of CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 60, CI Pigment Blue 21, CI Pigment Blue 28, CI Pigment Blue 64, and CI Pigment Blue 74, and preferably includes one or more selected from the group consisting of CI Pigment Blue 15:3, CI Pigment Blue 15:4, and CI Pigment Blue 60.

[0022] The blue pigment (A-2) is contained in an amount of 5 to 20% by weight, and more preferably 7 to 20% by weight, based on the total weight of the colorant.

[0023] When the blue pigment (A-2) satisfies the above range, the crosstalk transmittance is improved.

[0024] Violet pigment (B) The violet pigment (B) may be, for example, a compound classified as Pigment Violet in the color index. Specifically, it may include one or more selected from the group consisting of CI Pigment Violet 1, CI Pigment Violet 19, CI Pigment Violet 23, CI Pigment Violet 29, CI Pigment Violet 32, CI Pigment Violet 36, and CI Pigment Violet 38, and in particular, CI Pigment Violet 23 is preferred.

[0025] The violet pigment (B) is contained in an amount of 5 to 20% by weight, and more preferably 7 to 20% by weight, based on the total weight of the colorant.

[0026] When the violet pigment (B) satisfies the above range, there is an advantage in that the light transmittance in the blue region is improved.

[0027] Violet dye (C) The violet dye (C) is characterized by containing a compound represented by formula (1).

[0028] [ka]

[0029] (In formula (1), R 1 ~R 4 are each independently a hydrogen atom, -R 6or a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms. The hydrogen atoms contained in the aromatic hydrocarbon group having 6 to 10 carbon atoms are each independently selected from the group consisting of a halogen atom, -R 6 , -OH, -OR 6 , -SO 3 - , -SO 3 H, -SO 3 M, -CO 2 H, -CO 2 R 6 , -SO 3 R 6 OR -SO 2 N(R 8 )R 9 may be substituted with. R 5 -SO 3 - , -SO 3 H, -SO 3 M, -CO 2 H or -CO 2 R 6 Shows. m represents an integer of 0 to 5. When m is an integer of 2 or more, a plurality of R 5 may be the same or different. X represents a halogen atom. a represents an integer of 0 or 1. R 6 represents a monovalent saturated hydrocarbon group having 1 to 10 carbon atoms. A hydrogen atom contained in the saturated hydrocarbon group having 1 to 10 carbon atoms may be substituted with a halogen atom or an alkoxy group having 1 to 10 carbon atoms. R 8 and R 9 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, or -Q, and the hydrogen atom contained in the alkyl group and the cycloalkyl group is -OH, a halogen atom, -Q, -CH=CH 2 or -CH=CHR 6 The alkyl group and the cycloalkyl group may be substituted with -CH 2 - is -O-, -S-, -CO-, -NH- or -NR 6 -, R8 and R 9 may be bonded to each other to form a heterocycle having 1 to 10 carbon atoms, and a hydrogen atom contained in the heterocycle is -R 6 , -OH or -Q. Q represents a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms or a monovalent aromatic heterocyclic group having 5 to 10 carbon atoms, and the hydrogen atoms contained in the aromatic hydrocarbon group and the aromatic heterocyclic group are each independently selected from the group consisting of -OH, -R 6 , -OR 6 , -NO 2 , -CH=CH 2 , -CH=CHR 6 or may be substituted with a halogen atom.

[0030] The violet dye (C) is contained in an amount of 0.5 to 5% by weight based on the total weight of the colorant.

[0031] When the violet dye (C) satisfies the above range, there is an advantage in that the light transmittance in the blue region is improved.

[0032] The content of the colorant is not particularly limited, but is 3 to 60% by weight, preferably 5 to 50% by weight, based on the total weight of the solid content of the colored photosensitive resin composition. Within this range, the colorant does not flow out and the desired color reproducibility can be achieved.

[0033] Alkali-soluble resin In the present invention, the alkali-soluble resin is an acrylic copolymer that is soluble in the solvent of the present invention, has reactivity to the action of light or heat, functions as a binder resin for the colorant, and is soluble in an alkaline developer, and the type of the alkali-soluble resin can be used without any particular limitation.

[0034] Examples of the acrylic copolymer include copolymers of a carboxyl group-containing monomer and other monomers copolymerizable with the above monomer.

[0035] Specific examples of carboxyl group-containing monomers include unsaturated carboxylic acids such as unsaturated monocarboxylic acids, unsaturated dicarboxylic acids, unsaturated tricarboxylic acids, and other unsaturated polycarboxylic acids having one or more carboxyl groups in the molecule.

[0036] Examples of the unsaturated monocarboxylic acid include acrylic acid, methacrylic acid, crotonic acid, α-chloroacrylic acid, and cinnamic acid.

[0037] Examples of the unsaturated dicarboxylic acid include maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, etc. The unsaturated polycarboxylic acid may be an acid anhydride, and specific examples thereof include maleic anhydride, itaconic anhydride, citraconic anhydride, etc.

[0038] The unsaturated polycarboxylic acid may be a mono(2-methacryloyloxyalkyl)ester thereof, such as mono(2-acryloyloxyethyl) succinate, mono(2-methacryloyloxyethyl) succinate, mono(2-acryloyloxyethyl) phthalate, mono(2-methacryloyloxyethyl) phthalate, etc. The unsaturated polycarboxylic acid may be a mono(meth)acrylate of a polymer having dicarboxylates at both ends thereof, such as ω-carboxypolycaprolactone monoacrylate, ω-carboxypolycaprolactone monomethacrylate, etc.

[0039] These carboxyl group-containing monomers can be used alone or in combination of two or more.

[0040] Specific examples of other monomers copolymerizable with the carboxyl group-containing monomer include aromatic vinyl compounds such as styrene, α-methylstyrene, o-vinyltoluene, m-vinyltoluene, p-vinyltoluene, p-chlorostyrene, o-methoxystyrene, m-methoxystyrene, p-methoxystyrene, o-vinylbenzyl methyl ether, m-vinylbenzyl methyl ether, p-vinylbenzyl methyl ether, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, and indene; Methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-propyl acrylate, n-propyl methacrylate, i-propyl acrylate, i-propyl methacrylate, n-butyl acrylate, n-butyl methacrylate, i-butyl acrylate, i-butyl methacrylate, sec-butyl acrylate, sec-butyl methacrylate, t-butyl acrylate, t-butyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl acrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl acrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, allyl acrylate, allyl methacrylate, benzyl acrylate, benzyl methacrylate, silyl unsaturated carboxylic acid esters such as cyclohexyl acrylate, cyclohexyl methacrylate, phenyl acrylate, phenyl methacrylate, 2-methoxyethyl acrylate, 2-methoxyethyl methacrylate, 2-phenoxyethyl acrylate, 2-phenoxyethyl methacrylate, methoxydiethylene glycol acrylate, methoxydiethylene glycol methacrylate, methoxytriethylene glycol acrylate, methoxytriethylene glycol methacrylate, methoxypropylene glycol acrylate, methoxypropylene glycol methacrylate, methoxydipropylene glycol acrylate, methoxydipropylene glycol methacrylate, isobornyl acrylate, isobornyl methacrylate, dicyclopentadienyl acrylate, dicyclopentadienyl methacrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl methacrylate, glycerol monoacrylate, and glycerol monomethacrylate; unsaturated carboxylic acid aminoalkyl esters such as 2-aminoethyl acrylate, 2-aminoethyl methacrylate, 2-dimethylaminoethyl acrylate, 2-dimethylaminoethyl methacrylate, 2-aminopropyl acrylate, 2-aminopropyl methacrylate, 2-dimethylaminopropyl acrylate, 2-dimethylaminopropyl methacrylate, 3-aminopropyl acrylate, 3-aminopropyl methacrylate, 3-dimethylaminopropyl acrylate, and 3-dimethylaminopropyl methacrylate; Unsaturated carboxylic acid glycidyl esters such as glycidyl acrylate and glycidyl methacrylate; Vinyl esters of carboxylic acids, such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl benzoate; Unsaturated ethers such as vinyl methyl ether, vinyl ethyl ether, and allyl glycidyl ether; Vinyl cyanide compounds such as acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, and vinylidene cyanide; Unsaturated amides such as acrylamide, methacrylamide, α-chloroacrylamide, N-2-hydroxyethyl acrylamide, and N-2-hydroxyethyl methacrylamide; Unsaturated imides such as maleimide, N-phenylmaleimide, and N-cyclohexylmaleimide; Aliphatic conjugated dienes such as 1,3-butadiene, isoprene, and chloroprene; Examples of the monomer include macromonomers having a monoacryloyl group or monomethacryloyl group at the end of the polymer molecular chain of polystyrene, polymethyl acrylate, polymethyl methacrylate, poly-n-butyl acrylate, poly-n-butyl methacrylate, and polysiloxane.

[0041] These monomers can be used alone or in combination of two or more.

[0042] The content of the carboxyl group-containing monomer unit in the alkali-soluble resin is usually 10 to 50% by mass, preferably 15 to 40% by mass, and more preferably 25 to 40% by mass. When the content of the carboxyl group-containing monomer unit is 10 to 50% by mass, the solubility in the developer is good, and a pattern tends to be accurately formed during development, which is preferable.

[0043] Examples of the acrylic copolymer include (meth)acrylic acid / methyl (meth)acrylate copolymer, (meth)acrylic acid / benzyl (meth)acrylate copolymer, (meth)acrylic acid / 2-hydroxyethyl (meth)acrylate / benzyl (meth)acrylate copolymer, (meth)acrylic acid / methyl (meth)acrylate / polystyrene macromonomer copolymer, (meth)acrylic acid / methyl (meth)acrylate / polymethyl (meth)acrylate macromonomer copolymer, (meth)acrylic acid / benzyl (meth)acrylate / polystyrene macromonomer copolymer, (meth)acrylic acid / benzyl (meth)acrylate / polymethyl (meth)acrylate macromonomer copolymer, (meth)acrylic acid / 2-hydroxyethyl (meth)acrylate / benzyl (meth)acrylate ) acrylate / polystyrene macromonomer copolymer, (meth)acrylic acid / 2-hydroxyethyl (meth)acrylate / benzyl (meth)acrylate / polymethyl (meth)acrylate macromonomer copolymer, (meth)acrylic acid / styrene / benzyl (meth)acrylate / N-phenylmaleimide copolymer, (meth)acrylic acid / mono(2-acryloyloxy) succinate / styrene / benzyl (meth)acrylate / N-phenylmaleimide copolymer, (meth)acrylic acid / mono(2-acryloyloxyethyl) succinate / styrene / allyl (meth)acrylate / N-phenylmaleimide copolymer, (meth)acrylic acid / benzyl (meth)acrylate / N-phenylmaleimide / styrene / glycerol mono(meth)acrylate copolymer, etc. are mentioned. Here, (meth)acrylate means acrylate or methacrylate.

[0044] Of these, (meth)acrylic acid / benzyl (meth)acrylate copolymer, (meth)acrylic acid / benzyl (meth)acrylate / styrene copolymer, (meth)acrylic acid / methyl (meth)acrylate copolymer, and (meth)acrylic acid / methyl (meth)acrylate / styrene copolymer are preferably used.

[0045] The weight average molecular weight of the alkali-soluble resin in terms of polystyrene is usually 5,000 to 50,000, preferably 8,000 to 40,000, more preferably 10,000 to 35,000, and most preferably 10,000 to 30,000. When the molecular weight of the alkali-soluble resin is 5,000 to 50,000, the coating hardness is improved, the residual film rate is high, the solubility of the unexposed portion in the developer is good, and there is a tendency for the resolution to be improved, which is preferable.

[0046] The acid value of the alkali-soluble resin is usually 50 to 150 KOHmg / g, preferably 60 to 140 KOHmg / g, more preferably 80 to 135 KOHmg / g, and most preferably 80 to 130 KOHmg / g. When the acid value is 50 to 150 KOHmg / g, the solubility in the developer is improved, the unexposed area is easily dissolved, the sensitivity is increased, and the pattern of the exposed area remains during development, which tends to improve the residual film rate, which is preferable. Here, the acid value is a value measured as the amount (mg) of potassium hydroxide required to neutralize 1 g of an acrylic polymer, and is usually determined by titration using an aqueous potassium hydroxide solution.

[0047] The alkali-soluble resin is contained in an amount of 5 to 85% by weight, preferably 10 to 70% by weight, based on the total solid weight of the colored photosensitive resin composition of the present invention. When contained in such an amount, the resin has sufficient solubility in a developer, and development residues are unlikely to occur on the substrate in non-pixel areas, and the film reduction in pixel areas of exposed areas is unlikely to occur during development, which is preferable since there is a tendency for the non-pixel areas to be less likely to be chipped.

[0048] photopolymerizable compound The photopolymerizable compound is a compound that can be polymerized by the action of a photopolymerization initiator, and a monofunctional monomer or a multifunctional monomer having two or more functional groups can be used. Preferably, a multifunctional monomer having two or more functional groups can be used.

[0049] Specific examples of the monofunctional monomer include, but are not limited to, nonylphenylcarbitol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-ethylhexylcarbitol acrylate, 2-hydroxyethyl acrylate, and N-vinylpyrrolidone.Specific examples of the bifunctional monomer include, but are not limited to, 1,6-hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, bis(acryloyloxyethyl)ether of bisphenol A, and 3-methylpentanediol di(meth)acrylate. Specific examples of trifunctional or higher polyfunctional monomers include, but are not limited to, trimethylolpropane tri(meth)acrylate, ethoxylated trimethylol, propane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ethoxylated dipentaerythritol hexa(meth)acrylate, propoxylated dipentaerythritol hexa(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0050] The photopolymerizable compound is preferably contained in an amount of 5 to 45% by weight, more preferably 7 to 45% by weight, based on the total weight of the solid content in the colored photosensitive resin composition. When the photopolymerizable compound is contained in the above-mentioned range, the strength and smoothness of the pixel portion are improved, which is preferable.

[0051] Photoinitiator In one embodiment of the present invention, the photopolymerization initiator can be used without any particular limitation as long as it can polymerize the alkali-soluble resin and the photopolymerizable monomer. In particular, it is preferable to use one or more compounds selected from the group consisting of triazine-based compounds, acetophenone-based compounds, biimidazole-based compounds, and oxime compounds from the viewpoints of polymerization characteristics, initiation efficiency, absorption wavelength, availability, price, etc.

[0052] Specific examples of the triazine-based compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-piperonyl-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[ 2-(5-methylfuran-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine, and the like.

[0053] Specific examples of the acetophenone-based compound include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one, and 2-(4-methylbenzyl)-2-(dimethylamino)-1-(4-morpholinophenyl)butan-1-one.

[0054] Specific examples of the biimidazole-based compound include 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2,3-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(alkoxyphenyl)biimidazole, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetra(trialkoxyphenyl)biimidazole, 2,2-bis(2,6-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, and imidazole compounds in which the phenyl groups at the 4,4',5,5'-positions are substituted with carboalkoxy groups. Of these, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(2,3-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole or 2,2-bis(2,6-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole is preferably used.

[0055] Specific examples of the oxime compound include o-ethoxycarbonyl-α-oximino-1-phenylpropan-1-one and compounds represented by the following chemical formulas 1 to 3.

[0056] [Chemical formula 1] [ka]

[0057] [Chemical formula 2] [ka]

[0058] [Chemical formula 3] [ka]

[0059] In addition, other photopolymerization initiators that are commonly used in the technical field may be additionally used in combination to the extent that the effect of the present invention is not impaired.

[0060] The content of the photopolymerization initiator in the colored photosensitive composition of the present invention is preferably 0.05 to 30% by weight, more preferably 0.5 to 20% by weight, and even more preferably 0.5 to 10% by weight, based on the total weight of the solid content in the colored photosensitive resin composition. When the content of the photopolymerization initiator satisfies the above range, it is advantageous for realizing good pattern characteristics of the target size.

[0061] solvent As the solvent, any solvent used in a typical photosensitive resin composition can be used without any particular limitation as long as it is effective in dissolving other components contained in the colored photosensitive resin composition. In particular, ethers, aromatic hydrocarbons, ketones, alcohols, esters, amides, etc. can be preferably used.

[0062] Specific examples of the solvent include ethylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; diethylene glycol dialkyl ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; ethylene glycol alkyl ether acetates such as methyl cellosolve acetate and ethyl cellosolve acetate; propylene glycol monomethyl ether acetate, propylene glycol mono Examples of the alkylene glycol alkyl ether acetates include ethyl ether, propylene glycol monopropyl ether acetate, methoxybutyl acetate, and methoxypentyl acetate; aromatic hydrocarbons such as benzene, toluene, xylene, and mesitylene; ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, and glycerin; esters such as ethyl 3-ethoxypropionate and methyl 3-methoxypropionate, and cyclic esters such as γ-butyrolactone.

[0063] From the viewpoint of coatability and drying property, the solvent is preferably an organic solvent having a boiling point of 100° C. to 200° C., and more preferably, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, cyclohexanone, ethyl lactate, butyl lactate, ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, etc. The above-exemplified solvents can be used alone or in combination of two or more kinds.

[0064] The solvent is contained in an amount of 60 to 90% by weight, preferably 80 to 90% by weight, based on the total weight of the colored photosensitive resin composition of the present invention. When the solvent is contained in the above-mentioned range, the effect of improving the coatability can be obtained when the composition is coated with a coating device such as a roll coater, a spin coater, a slit and spin coater, a slit coater (sometimes called a die coater), or an inkjet.

[0065] Additives The additives can be selectively added as necessary, and examples thereof include other polymer compounds, curing agents, surfactants, adhesion promoters, antioxidants, ultraviolet absorbers, and anti-aggregation agents.

[0066] Specific examples of the other polymer compounds include photosensitive resins such as epoxy resins and maleimide resins, and thermoplastic resins such as polyvinyl alcohol, polyacrylic acid, polyethylene glycol monoalkyl ether, polyfluoroalkyl acrylate, polyester, and polyurethane.

[0067] The curing agent is used to cure deep portions and increase mechanical strength, and specific examples of the curing agent include epoxy compounds, polyfunctional isocyanate compounds, melamine compounds, and oxetane compounds.

[0068] Specific examples of the epoxy compound in the curing agent include bisphenol A epoxy resins, hydrogenated bisphenol A epoxy resins, bisphenol F epoxy resins, hydrogenated bisphenol F epoxy resins, novolac epoxy resins, other aromatic epoxy resins, alicyclic epoxy resins, glycidyl ester resins, glycidyl amine resins, or brominated derivatives of such epoxy resins, aliphatic, alicyclic or aromatic epoxy compounds other than epoxy resins and their brominated derivatives, epoxidized butadiene (co)polymers, epoxidized isoprene (co)polymers, glycidyl (meth)acrylate (co)polymers, triglycidyl isocyanurate, and the like.

[0069] Specific examples of the oxetane compound in the curing agent include carbonate bisoxetane, xylene bisoxetane, adipate bisoxetane, terephthalate bisoxetane, and cyclohexanedicarboxylate bisoxetane.

[0070] The curing agent may be used in combination with a curing auxiliary compound that enables ring-opening polymerization of the epoxy group of the epoxy compound and the oxetane skeleton of the oxetane compound. Examples of the curing auxiliary compound include polycarboxylic acids, polycarboxylic anhydrides, and acid generators. The polycarboxylic anhydrides may be commercially available epoxy resin curing agents. Specific examples of the epoxy resin curing agent include trade names (ADEKA HARDNER EH-700) (manufactured by ADEKA KOGYO CO., LTD.), (RIKACID HH) (manufactured by Shin-Nihon Rika Co., Ltd.), and (MH-700) (manufactured by Shin-Nihon Rika Co., Ltd.). The curing agents exemplified above may be used alone or in combination of two or more.

[0071] The surfactant can be used to further improve the film-forming properties of the photosensitive resin composition, and a fluorine-based surfactant or a silicone-based surfactant can be preferably used.

[0072] Examples of the silicone surfactants include DC3PA, DC7PA, SH11PA, SH21PA, and SH8400 from Dow Corning Toray Silicones, and TSF-4440, TSF-4300, TSF-4445, TSF-4446, TSF-4460, and TSF-4452 from GE Toshiba Silicones. Examples of the fluorine surfactants include Megapeace F-470, F-471, F-475, F-482, and F-489 from Dainippon Ink and Chemicals, Inc. The surfactants exemplified above can be used alone or in combination of two or more.

[0073] Specific examples of the adhesion promoter include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, etc. The adhesion promoters exemplified above can be used alone or in combination of two or more. The adhesion promoter is contained in an amount of usually 0.01 to 10% by weight, and preferably 0.05 to 2% by weight, based on the weight fraction of the solid content of the colored photosensitive resin composition.

[0074] Specific examples of the antioxidant include 2,2'-thiobis(4-methyl-6-t-butylphenol) and 2,6-di-t-butyl-4-methylphenol.

[0075] Specific examples of the ultraviolet absorber include 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole and alkoxybenzophenone.

[0076] Specific examples of the anti-aggregating agent include sodium polyacrylate.

[0077] <Color filters and display devices> The present invention also provides a color filter including a colored pattern produced from the colored photosensitive resin composition of the present invention, and a display device including the color filter. The color filter and display device of the present invention may not include a polarizing plate, and may also include a polarizing plate within the scope of the present invention.

[0078] Display devices that may be provided with such color filters include, but are not limited to, liquid crystal displays, OLEDs, flexible displays, etc., and may include any display device known in the art that is applicable.

[0079] A color filter can be produced by applying the above-mentioned colored photosensitive resin composition of the present invention onto a substrate, followed by photocuring and development to form a pattern.

[0080] First, a colored photosensitive resin composition is applied to a substrate, and then heated and dried to remove volatile components such as the solvent, thereby obtaining a smooth coating film.

[0081] The coating method can be, for example, spin coating, casting coating, roll coating, slit and spin coating, or slit coating. After coating, the coating is heated and dried (pre-baked), or dried under reduced pressure, and then heated to volatilize volatile components such as the solvent. The heating temperature is usually 70 to 200°C, preferably 80 to 130°C. The coating film thickness after drying is usually about 1 to 8 μm. The coating film thus obtained is irradiated with ultraviolet light through a mask for forming a desired pattern. At this time, it is preferable to use a device such as a mask aligner or a stepper so that the entire exposed area is uniformly irradiated with parallel light and the mask and the substrate are accurately aligned. When ultraviolet light is irradiated, the area irradiated with ultraviolet light is cured.

[0082] As the ultraviolet ray, g-ray (wavelength: 436 nm), h-ray, i-ray (wavelength: 365 nm), etc. can be used. The amount of ultraviolet ray can be appropriately selected as necessary, and is not limited thereto in the present invention. The coating film after curing is brought into contact with a developer to dissolve the non-exposed areas and develop the coating film, thereby forming the desired pattern shape.

[0083] The developing method may be any of a liquid addition method, a dipping method, a spray method, and the like. In addition, the substrate may be tilted at any angle during development. The developing solution is usually an aqueous solution containing an alkaline compound and a surfactant. The alkaline compound may be either an inorganic or organic alkaline compound. Specific examples of inorganic alkaline compounds include sodium hydroxide, potassium hydroxide, disodium hydrogen phosphate, sodium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, potassium dihydrogen phosphate, sodium silicate, potassium silicate, sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium borate, potassium borate, and ammonia. Specific examples of organic alkaline compounds include tetramethylammonium hydroxide, 2-hydroxyethyltrimethylammonium hydroxide, monomethylamine, dimethylamine, trimethylamine, monoethylamine, diethylamine, triethylamine, monoisopropylamine, diisopropylamine, and ethanolamine.

[0084] These inorganic and organic alkaline compounds can be used alone or in combination of two or more. The concentration of the alkaline compound in the alkaline developer is preferably 0.01 to 10% by mass, more preferably 0.03 to 5% by mass.

[0085] The surfactant in the alkaline developer can be at least one selected from the group consisting of nonionic surfactants, anionic surfactants, and cationic surfactants.

[0086] Specific examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene aryl ethers, polyoxyethylene alkylaryl ethers, other polyoxyethylene derivatives, oxyethylene / oxypropylene block copolymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, and polyoxyethylene alkylamines.

[0087] Specific examples of the anionic surfactant include higher alcohol sulfates such as sodium lauryl alcohol sulfate and sodium oleyl alcohol sulfate, alkyl sulfates such as sodium lauryl sulfate and ammonium lauryl sulfate, and alkylaryl sulfonates such as sodium dodecylbenzenesulfonate and sodium dodecylnaphthalenesulfonate.

[0088] Specific examples of the cationic surfactant include amine salts such as stearylamine hydrochloride and lauryltrimethylammonium chloride, and quaternary ammonium salts. These surfactants can be used alone or in combination of two or more.

[0089] The concentration of the surfactant in the developer is usually 0.01 to 10% by mass, preferably 0.05 to 8% by mass, and more preferably 0.1 to 5% by mass. After development, the film is washed with water, and may be post-baked at 80 to 230° C., preferably 80 to 120° C., for 10 to 60 minutes, as required. EXAMPLES

[0090] The present invention will be described in more detail below based on examples, but the embodiment of the present invention disclosed below is merely illustrative, and the scope of the present invention is not limited to these embodiments. The scope of the present invention is set forth in the claims, and includes all modifications within the scope and meaning equivalent to the claims. In the following examples and comparative examples, the "%" and "parts" indicating the content are based on mass unless otherwise specified.

[0091] <Example> Synthesis Example: Synthesis of Violet Dye C 20 parts of 3',6'-dichlorospiro[benzo[c][1,2]oxazole-3,9'-xanthene]1,1-dioxide compound and 200 parts of 2,6-dimethylaniline were mixed under light-shielded conditions, and the resulting solution was stirred at 110°C for 6 hours. The resulting reaction solution was cooled to room temperature, and then added to a mixture of 800 parts of water and 50 parts of 35% hydrochloric acid and stirred at room temperature for 1 hour, resulting in the precipitation of crystals. The precipitated crystals were obtained as a residue by suction filtration, and then dried to obtain 24 parts of a compound represented by formula C (dye C).

[0092] [ka]

[0093] Production Examples 1 to 5: Production of Pigment Dispersion Production Example 1: Production of Pigment Dispersion A-1 Pigment dispersion A-1 was prepared by mixing and dispersing 11 parts by weight of CI Pigment Blue 15:6 as a pigment, 5.0 parts by weight of DISPERBYK-2001 (manufactured by BYK) as a pigment dispersant, and 84.0 parts by weight of propylene glycol methyl ether acetate as a solvent using a bead mill for 12 hours.

[0094] Production Example 2: Production of Pigment Dispersion A-2-1 12 parts by weight of CI Pigment Blue 15:4 as a pigment, 8.4 parts by weight of DISPERBYK-2001 (manufactured by BYK) as a pigment dispersant, and 79.6 parts by weight of propylene glycol methyl ether acetate as a solvent were mixed and dispersed for 12 hours using a bead mill to produce pigment dispersion A-2-1.

[0095] Production Example 3: Production of pigment dispersion A-2-2 12 parts by weight of CI Pigment Blue 15:3 as a pigment, 8.4 parts by weight of DISPERBYK-2001 (manufactured by BYK) as a pigment dispersant, and 79.6 parts by weight of propylene glycol methyl ether acetate as a solvent were mixed and dispersed for 12 hours using a bead mill to produce pigment dispersion A-2-2.

[0096] Production Example 4: Production of Pigment Dispersion B Pigment dispersion B was prepared by mixing and dispersing 11 parts by weight of CI Pigment Violet 23 as a pigment, 5.0 parts by weight of DISPERBYK-2001 (manufactured by BYK) as a pigment dispersant, and 84.0 parts by weight of propylene glycol methyl ether acetate as a solvent using a bead mill for 12 hours.

[0097] Production Example 5: Production of Dye Dispersion C Dye dispersion C was prepared by mixing and dispersing 8 parts by weight of dye C according to the synthesis example, 6.4 parts by weight of DISPERBYK-2001 (manufactured by BYK) as a dispersant, and 85.6 parts by weight of propylene glycol methyl ether acetate as a solvent using a bead mill for 12 hours.

[0098] Examples 1 to 15 and Comparative Examples 1 to 7: Production of Colored Photosensitive Resin Compositions Colored photosensitive resin compositions of Examples 1 to 15 and Comparative Examples 1 to 7 were produced according to the compositions and contents in Table 1 below.

[0099] [Table 1]

[0100] The components used in the above examples and comparative examples are as follows. Colorant A-1: ​​Pigment dispersion A-1 of Production Example 1 Colorant A-2-1: Pigment dispersion A-2-1 of Production Example 2 Colorant A-2-2: Pigment dispersion A-2-2 of Production Example 3 Colorant B: Pigment dispersion B of Production Example 4 Colorant C: Dye dispersion C of Production Example 5 Resin D: A copolymer of methacrylic acid and benzyl methacrylate having a molar ratio of methacrylic acid units to benzyl methacrylate units of 31:69, a weight average molecular weight of 12,500, and an acid value of 95. Photopolymerizable compound E: Dipentaerythritol hexaacrylate (KAYARAD DPHA, product of Nippon Kayaku Co., Ltd.) Photopolymerization initiator F: OXE-01 (manufactured by BASF) Additive G: SH-8400 (Product of Dow Corning Korea Co., Ltd.) Solvent H: Propylene glycol monomethyl ether acetate

[0101] Experimental Example 1.Transmittance evaluation First, a color filter was manufactured using the colored photosensitive resin compositions manufactured in the examples and comparative examples. Specifically, each of the colored photosensitive resin compositions was applied onto a glass substrate by spin coating, and then maintained in a heating oven at 100°C for 1 minute and 30 seconds to form a thin film. Next, after cooling to 23°C, the formed colored photosensitive resin composition layer was exposed to light. At this time, a 1kW high pressure mercury lamp including all g, h, and i rays was used as the ultraviolet light source, and 150 mJ / cm was used. 2 No special optical filter was used. After that, the color filter was manufactured by heating for 5 minutes in a heating oven at 220°C for thermal curing. After making the color layer of the manufactured color filter to a thickness of 0.5 μm, the transmittance was measured and evaluated according to the following evaluation criteria, and the results are shown in Table 2 below. <Transmittance evaluation criteria> ×: Transmittance of 445 nm is less than 88.5% or transmittance of 700 nm is more than 20% ○: 445nm transmittance 88.5% or more but less than 89.5% and 700nm transmittance 19% or more but less than 20% ◎: Transmittance of 89.5% or more at 445 nm and 19% or less at 700 nm

[0102] 2.Residue evaluation The colored photosensitive resin compositions obtained in the examples and comparative examples were applied to the surface of a 6-inch Si-wafer by spin coating, and then dried at 100° C. for 90 seconds to volatilize the volatile components to form a photosensitive composition layer. After cooling to 23° C., the formed photosensitive composition layer was exposed using an i-line stepper. The wafer on which the exposed coating film was formed was developed with a 0.2 wt % tetramethylammonium hydroxide (TMAH) aqueous solution, and then post-heated at 220° C. for 180 seconds to form pixels. The thickness of the obtained pixels was 0.5 μm in each case. The minimum line width (resolution) of the formed pixels was 1.0 μm. The obtained patterns were observed using a CD-SEM, and the presence or absence of residue was evaluated according to the following evaluation criteria, and the results are shown in Table 2 below. <Residue evaluation criteria> 1: Severely bad, 2: Bad, 3: Average, 4: Good, 5: Excellent

[0103] [Table 2]

[0104] Referring to Table 2, it can be seen that in the case of Examples 1 to 15 according to the present invention, the standard transmittance at wavelengths of 445 nm and 700 nm is satisfied, and the residue also shows an average or higher result.

[0105] In contrast, in the case of Comparative Example 1, which contains only CI Pigment Blue 15:6 and CI Pigment Violet 23 as colorants, the standard transmittance was met at a wavelength of 445 nm, but the transmittance at a wavelength of 700 nm was high. In the cases of Comparative Examples 2 to 4, which further contain only Violet Dye C in the composition of the colorant according to Comparative Example 1, the transmittance at a wavelength of 445 nm was good, but the transmittance at a wavelength of 700 nm was still high. And in the cases of Comparative Examples 5 to 7, which further contain only CI Pigment Blue 15:4 in the composition of the colorant according to Comparative Example 1, the transmittance at a wavelength of 700 nm was good, but a decrease in the transmittance occurred at a wavelength of 445 nm, and the standard was not met.

[0106] To summarize the above results, it can be seen that the conventional colored photosensitive resin composition containing only CI Pigment Blue 15:6 and CI Pigment Violet 23 as colorants is highly unfavorable in terms of crosstalk transmittance.

Claims

1. The composition includes a colorant, an alkali-soluble resin, a photopolymerizable compound, a photopolymerization initiator, and a solvent, The colorant comprises, relative to the total weight of the colorant, 60 to 85% by weight of a blue pigment (A-1), 5 to 20% by weight of a blue pigment (A-2) other than the blue pigment (A-1), 5 to 20% by weight of a violet pigment (B), and 0.5 to 5% by weight of a violet dye (C).

2. The colored photosensitive resin composition according to claim 1, wherein the blue pigment (A-1) comprises C.I. Pigment Blue 15:

6.

3. The blue pigment (A-2) is selected from the group consisting of C.I. Pigment Blue 15:3, C.I. Pigment Blue 15:4 and C.I. Pigment Blue 60. The colored photosensitive resin composition according to claim 1, wherein the blue pigment (A-2) is selected from the group consisting of C.I. Pigment Blue 15:3, C.I. Pigment Blue 15:4 and C.I. Pigment Blue 60.

4. The colored photosensitive resin composition according to claim 1, wherein the violet pigment (B) comprises one or more selected from the group consisting of C.I. Pigment Violet 1, C.I. Pigment Violet 19, C.I. Pigment Violet 23, C.I. Pigment Violet 29, C.I. Pigment Violet 32, C.I. Pigment Violet 36 and C.I. Pigment Violet 38.

5. The colored photosensitive resin composition according to claim 1 , wherein the violet dye (C) comprises a compound represented by the following formula (1): [Formula 1] (In formula (1), R 1 ~R 4 are each independently a hydrogen atom, -R 6 or a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms. The hydrogen atoms contained in the aromatic hydrocarbon group having 6 to 10 carbon atoms are each independently selected from the group consisting of a halogen atom, -R 6 , -OH, -OR 6 , -SO 3 - , -SO 3 H, -SO 3 M, -CO 2 H, -CO 2 R 6 , -SO 3 R 6 or -SO 2 N (R 8 ) R 9 may be substituted with. R 5 is -SO 3 - , -SO 3 H, -SO 3 M, -CO 2 H or -CO 2 R 6 Shows. m represents an integer of 0 to 5. When m is an integer of 2 or more, multiple R5's may be the same or different. X represents a halogen atom. a represents an integer of 0 or 1. R 6 represents a monovalent saturated hydrocarbon group having 1 to 10 carbon atoms. A hydrogen atom contained in the saturated hydrocarbon group having 1 to 10 carbon atoms may be substituted with a halogen atom or an alkoxy group having 1 to 10 carbon atoms. R 8 and R 9 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, or -Q, and the hydrogen atom contained in the alkyl group and the cycloalkyl group is -OH, a halogen atom, -Q, -CH=CH 2 Or -CH=CHR 6 The alkyl group and the cycloalkyl group may be substituted with —CH 2 - is -O-, -S-, -CO-, -NH- or -NR 6 -, R 8 and R 9 may be bonded to each other to form a heterocycle having 1 to 10 carbon atoms, and a hydrogen atom contained in the heterocycle is -R 6 , -OH or -Q. Q represents a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms or a monovalent aromatic heterocyclic group having 5 to 10 carbon atoms, and the hydrogen atoms contained in the aromatic hydrocarbon group and the aromatic heterocyclic group are each independently selected from the group consisting of -OH, -R 6 , -OR 6 , -NO 2 , -CH=CH 2 , -CH=CHR 6 Or may be substituted with a halogen atom.)

6. 2. The colored photosensitive resin composition according to claim 1, wherein a coating film produced from the colored photosensitive resin composition has a transmittance of 88.5% or more at a wavelength of 445 nm and a transmittance of 20% or less at a wavelength of 700 nm.

7. The colored photosensitive resin composition according to claim 1 , which is for forming a blue pixel.

8. 8. The colored photosensitive resin composition according to claim 7, wherein the line width of the blue pixel is 1 μm or less.

9. Relative to the total weight of solids in the colored photosensitive resin composition, Colorant 5-60% by weight; 5 to 85% by weight of an alkali-soluble resin; Photopolymerizable compound 5-45% by weight; 0.05 to 30% by weight of a photoinitiator; and 2. The colored photosensitive resin composition according to claim 1, comprising 60 to 90% by weight of a solvent based on the total weight of the colored photosensitive resin composition.

10. A color filter comprising a colored pattern produced from the colored photosensitive resin composition according to any one of claims 1 to 9.

11. A display device comprising the color filter according to claim 10.

Citation Information

Patent Citations

  • Colored photosensitive resin composition

    JP2011118369A

  • Colored curable resin composition

    JP2013050693A

  • Color filter, organic el display element, and colored composition

    JP2016106270A

  • Colored composition, colored cured film and method for forming the same, and display element

    JP2018009132A

  • Photoinitiator and photosensitive composition thereof

    JP2018197343A