Adhesive tape, articles and electronic devices
The adhesive tape with a specific acrylic copolymer and crosslinking agent on a foam base material addresses the challenges of oil and impact resistance, ensuring durable adhesion in electronic devices despite exposure to sweat and drops.
Patent Information
- Application Number
- JP2020107643
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-23
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-06-23
AI Technical Summary
Adhesive tapes used for fixing components in electronic devices face challenges in maintaining oil resistance and impact resistance, particularly in environments where they are exposed to sweat, sebum, and drops, as devices become larger and thinner, reducing the adhesive area.
An adhesive tape with a specific composition of an acrylic copolymer and crosslinking agent on a foam base material, having a foaming density of 0.25 to 0.75 g/cm³, which includes 2% to 30% carboxyl group-containing monomer, 10% to 70% alkoxyalkyl (meth)acrylate, and one or more alkyl (meth)acrylate monomers with an average carbon atom count less than 4, providing both oil resistance and impact resistance.
The adhesive tape maintains excellent adhesive strength over time, resisting swelling from sweat and sebum and offering impact resistance, ensuring components remain securely attached even under impact.
Smart Images

Figure 0007552096000004 
Figure 0007552096000005 
Figure 0007552096000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive tape that can be used to fasten members constituting an article, for example, to fasten parts constituting electronic devices such as portable electronic terminals, and to an electronic device. [Background technology]
[0002] Adhesive tapes are used to fix members constituting articles, and are widely used, for example, in situations where parts constituting electronic devices are to be fixed, etc. Specifically, the adhesive tapes are used to fix protective panels and housings of image display units constituting small electronic devices such as portable electronic terminals, cameras, and personal computers, and to fix rigid parts such as exterior parts and batteries to the small electronic devices.
[0003] The above-mentioned pressure-sensitive adhesive tape is required to have a level of impact resistance that does not cause parts to break off or peel off due to the impact even when an article such as a portable electronic terminal is dropped, etc. As such double-sided pressure-sensitive adhesive tape, for example, a double-sided pressure-sensitive adhesive tape having pressure-sensitive adhesive layers on both sides of a flexible foam substrate is known as a tape that is thin, has excellent conformability to an adherend, and absorbs impact (see, for example, Patent Document 1).
[0004] On the other hand, the adhesive tape used to fix the member is required to have weather resistance according to the environment in which the member is used. For example, electronic devices such as portable electronic terminals are used in a wide variety of situations, so the adhesive tape used to fix the components of the electronic devices is usually required to be able to maintain excellent adhesive strength for a long period of time regardless of the influence of water, heat, etc. In particular, the adhesive tape used in the manufacturing scene of portable electronic devices that are often touched by people and the fixing scene of automobile interior members is required to be able to maintain excellent adhesive strength even when, for example, sweat, sebum, etc. are attached, that is, to have excellent oil resistance.
[0005] As an example of the pressure-sensitive adhesive tape having excellent oil resistance, there is known a pressure-sensitive adhesive tape obtained using a pressure-sensitive adhesive composition containing, as components, 50 to 90 mass % of a (meth)acrylic acid alkyl ester (A1) having an alkyl group having 4 to 12 carbon atoms, 3 to 20 mass % of a carboxyl group-containing monomer (A2), 3 to 20 mass % of a hydroxyl group-containing monomer (A3), and 3 to 15 mass % of a (meth)acrylic acid alkyl ester (A4) having an alkyl group having 1 to 3 carbon atoms, and containing a hydroxyl group- and carboxyl group-containing acrylic copolymer (A) having a weight-average molecular weight of 700,000 to 2,000,000 and a theoretical Tg of -40°C or less, and a crosslinking agent (B) (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2010-260880 A [Patent Document 2] International Publication 2014 / 002203 Brochure Summary of the Invention [Problem to be solved by the invention]
[0007] As the environments and conditions under which articles are used become more diverse, there is a demand for adhesive tapes used to fix parts constituting articles with further improved oil resistance against sweat, sebum, etc., and impact resistance against dropping, etc. In particular, electronic devices such as portable electronic terminals are increasingly touched by people, and as the screens of portable electronic terminals and the like become larger and thinner, the application area of the adhesive tape becomes smaller and the width of the adhesive tape becomes narrower. In this situation, there is a demand for adhesive tapes with even better oil resistance and even better impact resistance.
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide an adhesive tape having even better oil resistance and impact resistance, as well as an article and an electronic device using the adhesive tape. [Means for solving the problem]
[0009] The present inventors have found that the above-mentioned problems can be solved by an adhesive tape comprising, as constituent components, a specific content of a carboxyl group-containing monomer, a specific content of an alkoxyalkyl (meth)acrylate, and one or more types of alkyl (meth)acrylate monomer, wherein the alkoxyalkyl (meth)acrylate and the alkyl (meth)acrylate monomer have an average number of carbon atoms within a predetermined range, and an acrylic adhesive composition containing a crosslinking agent, and the adhesive layer is provided on a foam substrate having a foam density within a specific range.
[0010] That is, the present invention is a pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer on at least one surface of a foam substrate directly or via another layer, wherein the foam substrate has a foam density of 0.25 g / cm. 3 ~0.75g / cm 3 the pressure-sensitive adhesive layer contains an acrylic pressure-sensitive adhesive composition containing an acrylic copolymer and a crosslinking agent, and the acrylic copolymer is (A) a carboxyl group-containing monomer in the range of 2% by mass to 30% by mass, (B) an alkoxyalkyl (meth)acrylate in the range of 10% by mass to 70% by mass, and (C) one or more selected from the group consisting of alkyl (meth)acrylate monomers other than the monomers (A) and (B), Contains as a constituent The present invention provides a pressure-sensitive adhesive tape, characterized in that the saturated hydrocarbon groups contained in the monomers (B) and (C) have an average number of carbon atoms of less than 4. Effect of the Invention
[0011] The pressure-sensitive adhesive tape of the present invention has good initial adhesive strength, is not easily swollen even when sweat, sebum, etc. are attached, has oil resistance that enables it to maintain excellent adhesive strength for a long period of time, and can have excellent impact resistance against being dropped, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (Adhesive tape) The pressure-sensitive adhesive tape of the present invention is a pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer on at least one surface of a foam substrate directly or via another layer, and the foam substrate has a foam density of 0.25 g / cm 3 ~0.75g / cm 3 the pressure-sensitive adhesive layer contains an acrylic pressure-sensitive adhesive composition containing an acrylic copolymer and a crosslinking agent, and the acrylic copolymer is (A) a carboxyl group-containing monomer in the range of 2% by mass to 30% by mass, (B) an alkoxyalkyl (meth)acrylate in the range of 10% by mass to 70% by mass, and (C) one or more selected from the group consisting of alkyl (meth)acrylate monomers other than the monomers (A) and (B) above Contains as a constituent The monomers (B) and (C) are characterized in that the average number of carbon atoms in the saturated hydrocarbon groups is less than 4.
[0013] According to the pressure-sensitive adhesive tape of the present invention, by providing a pressure-sensitive adhesive layer having a predetermined composition on a foam substrate having a predetermined foaming density, it is possible to achieve both excellent oil resistance and impact resistance. In detail, the pressure-sensitive adhesive tape of the present invention has a good initial adhesive strength, is not easily swollen even when sweat or sebum is attached, has oil resistance that can maintain excellent adhesive strength for a long period of time, and has excellent impact resistance that is not easily peeled off even when impacted when an article using the pressure-sensitive adhesive tape of the present invention is dropped, etc.
[0014] The embodiment of the pressure-sensitive adhesive tape of the present invention may have a pressure-sensitive adhesive layer on at least one side of the foam substrate directly or via another layer, and may have a pressure-sensitive adhesive layer on one side of the foam substrate, or may have a pressure-sensitive adhesive layer on each of both sides of the foam substrate (first and second main surfaces facing each other). Among these, a pressure-sensitive adhesive tape having the pressure-sensitive adhesive layer on both sides of the foam substrate directly or via another layer is preferred. In particular, when used to fix two or more adherends (components) constituting an article such as an electronic device, it is preferred to use a double-sided pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer on each of both sides of the foam substrate.
[0015] The pressure-sensitive adhesive tape of the present invention may be stored with a release film laminated on the surface of the pressure-sensitive adhesive layer. There are no particular limitations on the release film, and any general-purpose release film may be used.
[0016] The thickness (total thickness) of the pressure-sensitive adhesive tape of the present invention is preferably in the range of 80 μm to 500 μm, more preferably in the range of 100 μm to 500 μm, further preferably in the range of 150 μm to 400 μm, and particularly preferably in the range of 200 μm to 300 μm, in order to provide even more excellent durability against sweat, sebum, etc., and excellent impact resistance. Note that the thickness of the pressure-sensitive adhesive tape does not include the thickness of the release film.
[0017] (Adhesive layer) The adhesive layer constituting the adhesive tape of the present invention is preferably one having a thickness in the range of 5 μm to 100 μm, more preferably one having a thickness in the range of 10 μm to 90 μm, and even more preferably one having a thickness in the range of 30 μm to 80 μm, in order to be able to exert the desired adhesive strength, to have even better durability against sweat, sebum, and the like, and to contribute to the thinning of electronic devices and the like.
[0018] The acrylic pressure-sensitive adhesive composition used in the pressure-sensitive adhesive layer may be (A) a carboxyl group-containing monomer in the range of 2% by mass to 30% by mass, (B) an alkoxyalkyl (meth)acrylate in the range of 10% by mass to 70% by mass, and (C) one or more selected from the group consisting of alkyl (meth)acrylate monomers other than the monomers (A) and (B), As a base polymer, an acrylic copolymer containing the above as a constituent component may be used, and an acrylic adhesive composition may be used in which additives such as a tackifier resin and a crosslinking agent are blended with this as necessary.
[0019] <Acrylic copolymer> The acrylic copolymer contains, as essential components, a predetermined amount of a carboxyl group-containing monomer (A), a predetermined amount of an alkoxyalkyl (meth)acrylate (B), and an alkyl (meth)acrylate (C) other than the monomers (A) and (B). That is, the acrylic copolymer is a polymer containing these monomers as monomer units.
[0020] <<(A) Carboxy group-containing monomer>> Examples of the carboxyl group-containing monomer that can be used in the production of the acrylic copolymer include acrylic acid, methacrylic acid, itaconic acid, maleic acid, (meth)acrylic acid dimer, crotonic acid, and ethylene oxide modified succinic acid acrylate. The carboxyl group-containing monomer may be used alone or in combination of two or more. Among them, acrylic acid is preferred. In other words, the acrylic copolymer preferably contains acrylic acid as a constituent (monomer unit). The use of acrylic acid as a copolymerization component is preferred in terms of exhibiting even better durability against sweat, sebum, alcohol, and the like.
[0021] The content of the carboxyl group-containing monomer in the total amount of acrylic monomers used in producing the acrylic copolymer is within the range of 2% by mass to 30% by mass, more preferably within the range of 3% by mass to 20% by mass, even more preferably within the range of 5% by mass to 15% by mass, and most preferably within the range of 7% by mass to 12% by mass. By setting the content within this range, it is possible to exhibit even more excellent durability against sweat, sebum, alcohol, etc. When two or more kinds of carboxyl group-containing monomers are used in combination, it is preferable that the total content thereof is within the above range.
[0022] <<(B) Alkoxyalkyl (meth)acrylate>> The alkoxyalkyl (meth)acrylate is a (meth)acrylate monomer having an alkoxyalkyl group at the end. By containing the alkoxyalkyl (meth)acrylate in the acrylic adhesive composition used in the adhesive layer, the adhesive layer can exhibit the effect of preventing the penetration of oil into the adhesive layer while maintaining the flexibility required for impact resistance.
[0023] The number of carbon atoms of the alkoxyalkyl group of the alkoxyalkyl (meth)acrylate is preferably 2 to 16, more preferably 2 to 14, and most preferably 2 to 12. Examples of the alkoxyalkyl (meth)acrylate include methoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, and 4-ethoxybutyl (meth)acrylate. The alkoxyalkyl (meth)acrylate may be used alone or in combination of two or more.
[0024] Among them, it is preferable that the alkoxyalkyl(meth)acrylate contains 2-methoxyethyl(meth)acrylate, in other words, it is preferable that the acrylic copolymer contains 2-methoxyethyl(meth)acrylate as a constituent component (monomer unit).
[0025] The content of the alkoxyalkyl (meth)acrylate is within the range of 10% by mass to 70% by mass of the total amount of the acrylic monomer, and is preferably within the range of 10% by mass to 50% by mass, more preferably within the range of 15% by mass to 40% by mass, even more preferably within the range of 15% by mass to 30% by mass, and most preferably within the range of 20% by mass to 30% by mass. By adjusting the content within this range, it becomes easier to achieve both excellent durability against sweat, sebum, etc. and impact resistance. When two or more types of alkoxyalkyl (meth)acrylates are used in combination, it is preferable that the total content is within the above range.
[0026] <<(C) Alkyl (meth)acrylate monomers other than the above (A) and (B)>> The alkyl (meth)acrylate monomer is a (meth)acrylate monomer having an alkyl group at the ester terminal. The alkyl group of the alkyl (meth)acrylate monomer may be a straight chain or a branched chain.
[0027] Examples of the alkyl (meth)acrylate monomer include (meth)acrylates in which the alkyl group has 1 to 18 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isostearyl (meth)acrylate. One or more of these can be used, but it is preferable to use two or more.
[0028] Among them, it is preferable to use a (meth)acrylate monomer having an alkyl group with 1 to 12 carbon atoms, and it is more preferable to use a (meth)acrylate monomer having 1 to 10 carbon atoms. In particular, by using at least one (meth)acrylate monomer having 1 to 4 carbon atoms, it is easy to adjust the average number of carbon atoms in the alkyl group of the (meth)acrylate monomer to less than 4, which is preferable.
[0029] The content of one or more selected from the group consisting of the alkyl (meth)acrylate monomers (C) in the total amount of acrylic monomers usable in producing the acrylic copolymer is preferably within the range of 20% by mass to 80% by mass, more preferably within the range of 25% by mass to 75% by mass, even more preferably within the range of 30% by mass to 70% by mass, and most preferably within the range of 40% by mass to 70% by mass. When two or more alkyl (meth)acrylate monomers (C) are used in combination, the total content is preferably within the above range.
[0030] <<Monomers other than the above (A) to (C)>> The acrylic copolymer may contain one or more other monomers (D) other than the monomers (A) to (C) described above. Examples of the other monomers (D) include polar group-containing monomers. Specific examples include sulfonic acid group-containing monomers, cyano group-containing monomers, amide group-containing monomers, hydroxyl group-containing monomers, amino group-containing monomers, imide group-containing monomers, epoxy group-containing monomers, and isocyanate group-containing monomers. When the acrylic copolymer contains a polar group-containing monomer as a constituent, it is possible to introduce a crosslinking point into the acrylic polymer or to increase the cohesive strength of the acrylic polymer. In particular, it is preferable that the acrylic copolymer contains one or more hydroxyl group-containing monomers as a constituent, since the pressure-sensitive adhesive layer in the present invention is more likely to have the cohesive strength required to exhibit the desired functions such as oil resistance and impact resistance.
[0031] Examples of the hydroxyl group-containing monomer that can be used include hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate.
[0032] The content of the hydroxyl group-containing monomer in the total amount of the acrylic monomers is desirably 1.0% by mass or less, preferably 0.01% by mass to 0.85% by mass, preferably 0.02% by mass to 0.7% by mass, more preferably 0.03% by mass to 0.5% by mass, and even more preferably 0.04% by mass to 0.3% by mass, and is particularly preferably 0.05% by mass to 0.2% by mass in order to exhibit even better durability against sweat, sebum, and the like.
[0033] In addition to the polar group-containing monomer, the acrylic copolymer may contain, as the other monomer (D), aromatic vinyl compounds such as styrene and substituted styrene; olefins such as ethylene, propylene, and butadiene; vinyl esters such as vinyl acetate; and vinyl chloride.
[0034] <Acrylic copolymer> In the acrylic copolymer, the average number of carbon atoms in the saturated hydrocarbon group of one or more selected from the group consisting of the monomers (B) and (C), i.e., the group consisting of the alkoxyalkyl (meth)acrylate monomer (B) and the alkyl (meth)acrylate monomer (C) is less than 4. In particular, the average number of carbon atoms in the saturated hydrocarbon group of the monomer selected from the group consisting of the monomers (B) and (C) is more preferably 2.0 to 3.9, more preferably 2.9 to 3.7, more preferably 3.1 to 3.6, and more preferably 3.3 to 3.6. By setting it within the above range, it becomes easier to achieve both excellent durability against sweat, sebum, etc. and impact resistance.
[0035] The average number of carbon atoms in the saturated hydrocarbon group of one or more selected from the alkoxyalkyl (meth)acrylate (B) and the alkyl (meth)acrylate (C) can be calculated by adding up the product of the number of carbon atoms in each saturated hydrocarbon group and its molar concentration (mol%), and dividing the sum by the total molar concentration (mol%) of one or more selected from the group consisting of all the alkoxyacrylates (B) and alkyl (meth)acrylate monomers (C). For example, when the alkoxyalkyl (meth)acrylate monomer with carbon number A is a (mol%), the acrylate monomer with carbon number B is b (mol%), and the acrylate monomer with carbon number C is c (mol%), the average number of carbon atoms can be calculated by (A×a+B×b+C×c) / (a+b+c).
[0036] The acrylic copolymer can be obtained by copolymerization by known polymerization methods such as solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization, but from the viewpoint of water resistance of the adhesive layer, solution polymerization and bulk polymerization are preferred. The polymerization initiation method can be arbitrarily selected from thermal initiation methods using peroxide-based thermal polymerization initiators such as benzoyl peroxide and lauroyl peroxide, and azo-based thermal polymerization initiators such as azobisisobutylnitrile, ultraviolet irradiation initiation methods using acetophenone-based, benzoin ether-based, benzil ketal-based, acylphosphine oxide-based, benzoin-based, and benzophenone-based photopolymerization initiators, and electron beam irradiation methods.
[0037] The weight average molecular weight of the acrylic copolymer is preferably 500,000 or more, more preferably within the range of 700,000 to 1,200,000, and even more preferably within the range of 900,000 to 1,100,000, in terms of standard polystyrene measured by gel permeation chromatography (GPC), in order to exhibit even better durability against sweat, sebum, alcohol, etc.
[0038] Here, the weight average molecular weight by the GPC method is a value calculated as standard polystyrene, measured using a GPC apparatus (HLC-8329GPC) manufactured by Tosoh Corporation, and the measurement conditions are as follows.
[0039] Sample concentration: 0.5% by mass (THF solution) Sample injection volume: 100 μL Eluent:THF Flow rate: 1.0mL / min Measurement temperature: 40℃ Column: TSKgel GMHXL x 4 Guard column: TSKgel HXL-H Detector: Differential refractometer Standard polystyrene molecular weight: 10,000 to 20 million (Tosoh Corporation)
[0040] <Crosslinking agent> Examples of the crosslinking agent contained in the acrylic pressure-sensitive adhesive composition include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, a metal chelate-based crosslinking agent, an aziridine-based crosslinking agent, etc. Among them, it is preferable to use a crosslinking agent that is easy to use by mixing with the acrylic copolymer or a solution thereof and can rapidly proceed with the crosslinking reaction, and more specifically, it is more preferable to use an isocyanate-based crosslinking agent or an epoxy-based crosslinking agent, and it is more preferable to use an isocyanate-based crosslinking agent.
[0041] Examples of the isocyanate crosslinking agent that can be used include tolylene diisocyanate, naphthylene-1,5-diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, and trimethylolpropane-modified tolylene diisocyanate. It is preferable to use tolylene diisocyanate and trimethylolpropane-modified tolylene diisocyanate.
[0042] As the epoxy-based crosslinking agent, for example, Tetrad X or Tetrad C manufactured by Mitsubishi Gas Chemical Co., Ltd., or E-05X manufactured by Soken Chemical Co., Ltd. can be used.
[0043] The crosslinking agent is preferably contained in an amount such that the gel fraction of the adhesive layer with respect to toluene falls within the range described below. Specifically, the content of the crosslinking agent is preferably within the range of 0.2 to 2.5 parts by mass relative to 100 parts by mass of the resin solid content in the acrylic adhesive composition in order to exhibit durability against sweat, sebum, etc., and is preferably within the range of 0.4 to 2.3 parts by mass, more preferably within the range of 0.6 to 2.2 parts by mass, and even more preferably within the range of 0.9 to 1.8 parts by mass in order to exhibit even better durability against sweat, sebum, etc. The resin solid content in the acrylic adhesive composition refers to the solid content of the acrylic copolymer when the acrylic adhesive composition contains only the acrylic copolymer, and refers to the sum of the solid content of the acrylic copolymer and the solid content of the adhesive resin other than the acrylic copolymer, such as a tackifier resin, when the acrylic adhesive composition contains an adhesive resin other than the acrylic copolymer in addition to the acrylic copolymer.
[0044] <Other ingredients> In order to obtain a pressure-sensitive adhesive sheet having even more excellent adhesiveness, the acrylic pressure-sensitive adhesive composition of the present invention may contain a tackifier resin.
[0045] Examples of the tackifier resin that can be used include rosin-based tackifier resins, polymerized rosin-based tackifier resins, polymerized rosin ester-based tackifier resins, rosin phenol-based tackifier resins, stabilized rosin ester-based tackifier resins, disproportionated rosin ester-based tackifier resins, hydrogenated rosin ester-based tackifier resins, terpene-based tackifier resins, terpene phenol-based tackifier resins, petroleum resin-based tackifier resins, and (meth)acrylate resin-based tackifier resins.
[0046] When the acrylic pressure-sensitive adhesive composition contains a tackifier resin, the content of the tackifier resin is preferably in the range of 10 parts by mass to 50 parts by mass relative to 100 parts by mass of the acrylic copolymer, and more preferably in the range of 15 parts by mass to 30 parts by mass in order to obtain a pressure-sensitive adhesive tape with high adhesive strength.
[0047] The softening point of the tackifier resin is not particularly limited.
[0048] The acrylic pressure-sensitive adhesive composition may further contain additives such as a plasticizer, a softener, an antioxidant, a flame retardant, a filler such as glass or plastic fibers / balloons, beads, metals, metal oxides or metal nitrides, a colorant such as a pigment or dye, a leveling agent, a thickener, a water repellent or an antifoaming agent.
[0049] <Adhesive layer> The gel fraction of the adhesive layer in the adhesive tape of the present invention is preferably within the range of 40% by mass to 80% by mass, more preferably within the range of 40% by mass to 70% by mass, even more preferably within the range of 40% by mass to 65% by mass, and particularly preferably 40% by mass to 65% by mass. By having the gel fraction of the adhesive layer within the above range, it becomes easier to obtain an adhesive sheet that has both excellent adhesion to the adherend or foam substrate and excellent conformability. In addition, if the gel fraction is too low, it affects the oil resistance, and if it is too high, it affects the impact resistance, so it is preferable to set it within the above range in order for the adhesive tape to exhibit good oil resistance and impact resistance.
[0050] The gel fraction of the pressure-sensitive adhesive layer refers to the gel fraction relative to toluene, and is a value measured by the method described below. The above-mentioned acrylic adhesive composition was applied to the release-treated surface of the release liner so that the thickness after drying was 50 μm, and the coating was dried in an environment of 100 ° C for 3 minutes, and then aged in an environment of 40 ° C for 2 days to form an adhesive layer. The adhesive layer was cut into a square of 50 mm length and 50 mm width to prepare a test piece, and the mass (G1) of the test piece was measured. Then, the test piece was immersed in toluene for 24 hours in an environment of 23 ° C., and after immersion, the mixture of the test piece and toluene was filtered using a 300 mesh wire net to extract the insoluble components in toluene. The insoluble components were dried in an environment of 110 ° C. for 1 hour, and the mass (G2) of the insoluble components was measured, and the gel fraction was calculated based on the mass (G1) and mass (G2) and the following formula. Gel fraction (mass%) = (G2 / G1) x 100
[0051] The pressure-sensitive adhesive layer in the pressure-sensitive adhesive tape of the present invention preferably has a temperature within the range of -40°C to 10°C, which indicates a peak value of loss tangent (tan δ) at a frequency of 1 Hz. By setting the peak value of the loss tangent of the pressure-sensitive adhesive layer within this range, it becomes easier to impart good adhesion to an adherend at room temperature. Furthermore, from the viewpoint of improving drop impact resistance, it is more preferably within the range of -35°C to 0°C, even more preferably within the range of -35°C to -10°C, and most preferably within the range of -35 to -20°C.
[0052] The loss tangent (tan δ) of the adhesive layer at a frequency of 1 Hz is calculated from the storage modulus (G') and loss modulus (G") obtained by dynamic viscoelasticity measurement using temperature dispersion, using the formula tan δ = G" / G'. In measuring dynamic viscoelasticity, a viscoelasticity tester (manufactured by TA Instruments Japan, product name: ARES G2) is used to sandwich a test piece of an adhesive layer formed to a thickness of approximately 2 mm between parallel disks with a diameter of 8 mm, which is the measurement section of the tester, and the storage modulus (G') and loss modulus (G") are measured at a frequency of 1 Hz from -50°C to 150°C.
[0053] The pressure-sensitive adhesive layer can be formed from an acrylic pressure-sensitive adhesive composition containing at least the above-mentioned acrylic copolymer and a crosslinking agent. When forming the pressure-sensitive adhesive layer, it is preferable to use the pressure-sensitive adhesive composition in a solution (pressure-sensitive adhesive solution) containing a solvent in order to maintain good coating workability. Examples of the solvent that can be used include toluene, xylene, ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, and hexane. In addition, when the pressure-sensitive adhesive composition is a water-based pressure-sensitive adhesive, water or an aqueous solvent mainly composed of water can be used.
[0054] (Foam base material) The pressure-sensitive adhesive tape of the present invention has a foam substrate.
[0055] The density of the foam substrate is 0.25 g / cm in order to achieve both impact resistance and excellent adhesion to the adherend. 3 ~0.75g / cm 3 but preferably in the range of 0.3 g / cm 3 ~0.7g / cm 3 and more preferably within the range of 0.35 g / cm 3 ~0.65g / cm 3 in the range of 0.5 g / cm 3 ~0.65g / cm 3 is within the range.
[0056] The density of the foam base material was measured in accordance with JIS K6767. In detail, the foam base material was cut into a rectangle of 4 cm x 5 cm and cut into a rectangular shape of about 15 cm. 3 100 ml of the powder is prepared, its mass is measured, and the apparent density is calculated and this value is used.
[0057] The foam substrate preferably has a 25% compressive strength of 30 kPa or more, more preferably in the range of 50 kPa to 1000 kPa, more preferably in the range of 120 kPa to 800 kPa, and even more preferably in the range of 150 kPa to 700 kPa. By setting the 25% compressive strength within the above range, it is possible to exhibit suitable adhesive strength to an adherend having an uneven shape or a rough surface.
[0058] The 25% compression strength was measured in accordance with JIS K 6767. More specifically, foam base material cut into a 25-sided square (250 mm x 250 mm) was stacked to a thickness of about 10 mm to prepare a sample, which was then sandwiched between stainless steel plates with a larger area than the sample and compressed to about 2.5 mm (25% of the original thickness) at 23°C at a speed of 10 mm / min, at which point the strength was measured.
[0059] As the foam base material, a foam base material having an interlaminar strength of 4 N / cm or more, preferably in the range of 6 N / cm to 150 N / cm, more preferably in the range of 10 N / cm to 100 N / cm, more preferably in the range of 20 N / cm to 60 N / cm can be suitably used. By using a foam having an interlaminar strength in the above range, good conformability to the adherend and excellent impact resistance can be realized. Furthermore, even if interlaminar cracks occur in the foam base material when the adhesive tape or parts are peeled off from a work-in-progress (rework) to improve the yield during the manufacture of portable electronic devices, or when the housing or parts are separated, disassembled, or dismantled to repair, regenerate, or reuse a finished product, the adhesive tape can be easily peeled off.
[0060] The interlaminar strength is measured by the following method. A 50 μm thick adhesive layer with strong adhesion (not peeled off from the adherend and the foam substrate during the high-speed peel test described below) is attached to both sides of the foam substrate to be evaluated for interlaminar strength, and then aged at 40° C. for 48 hours to prepare a double-sided adhesive tape for measuring interlaminar strength. Next, a double-sided adhesive tape with a width of 1 cm and a length of 15 cm (in the flow direction and width direction of the foam substrate) with one adhesive side backed by a 25 μm thick polyester film is pressed and attached to a 50 μm thick, 3 cm wide, and 20 cm long polyester film at 23° C. and 50% RH with a 2 kg roller going back and forth once, and left to stand at 60° C. for 48 hours. After leaving it to stand for 24 hours at 23°C, the side that is attached to the 50 μmm thick polyester film at 23°C and 50% RH is fixed to the mounting jig of a high-speed peel tester, and the 25 μm thick polyester film is pulled in a 90 degree direction at a tensile speed of 15 m / min to measure the maximum strength when the foam is torn.
[0061] The tensile modulus of the foam base material in the machine direction and the width direction is not particularly limited, but is preferably 200 N / cm 2 It is preferably equal to or greater than 300 N / cm 2 ~1800N / cm 2 In addition, the tensile modulus in the direction with the lower tensile modulus, either the machine direction or the width direction, is within the range of 500 N / cm 2 ~800N / cm 2It is preferable that the range is 600N / cm 2 ~700N / cm 2 In this case, the tensile modulus in the higher direction is preferably within the range of 700 N / cm 2 ~1800N / cm 2 It is preferable that the range is 800N / cm 2 ~1600N / cm 2 It is more preferable that the tensile elongation is within the range of 200% to 1500%, more preferably 400% to 1000%, and even more preferably 450% to 800%. By using a foam base material having a tensile modulus or tensile elongation within the range, it is possible to suppress deterioration in the processability of the adhesive tape and deterioration in the application workability even in the case of a foamed, soft base material. In addition, when the adhesive tape is peeled off, interlayer destruction or tearing of the foam is unlikely to occur, and even if interlayer cracking occurs, it is possible to impart ease of peeling of the adhesive tape.
[0062] The tensile modulus of elasticity in the machine direction and width direction of the foam substrate was measured in accordance with JIS K 6767. More specifically, it is the maximum strength measured on a foam substrate sample with a gauge length of 2 cm and width of 1 cm using a Tensilon tensile tester at a tensile speed of 300 mm / min in an environment of 23°C and 50% RH.
[0063] The cell structure of the foam base material may be a closed cell structure or an open cell structure, but a closed cell structure is preferred because it can effectively prevent water or oil from penetrating through the cut surface of the foam base material. The shape of the cells forming the closed cell structure is preferably such that the average cell diameter in the flow direction or width direction, or both, is longer than the average cell diameter in the thickness direction of the foam, thereby providing appropriate conformability and cushioning properties.
[0064] The average bubble diameter in the machine direction and width direction of the foam base material is within a range of 1.2 μm to 700 μm, preferably 10 μm to 500 μm, more preferably 30 μm to 300 μm, and even more preferably 50 μm to 200 μm. By setting the average bubble diameter in the machine direction and width direction within this range, the number of closed bubbles present per unit width increases even when the width of the pressure-sensitive adhesive tape is narrowed, so that paths for water and oil penetration from the cross section of the foam base material can be suitably blocked.
[0065] The average cell diameter in the thickness direction of the foam base material is 1 μm to 150 μm, preferably 5 μm to 100 μm, and more preferably 10 μm to 60 μm, depending on the thickness of the foam base material.
[0066] The ratio of the average bubble diameter in the flow direction of the foam substrate to the average bubble diameter in the thickness direction of the foam substrate (average bubble diameter in the flow direction / average bubble diameter in the thickness direction) and the ratio of the average bubble diameter in the width direction of the foam substrate to the average bubble diameter in the thickness direction of the foam substrate (average bubble diameter in the width direction / average bubble diameter in the thickness direction) are both 1.2 to 15 or less, more preferably 1.2 to 10, and furthermore 2 to 8. When the ratio is 1.2 or more, flexibility in the thickness direction is easily ensured, so that the conformability is improved. Furthermore, when the ratio is 15 times or less, durability against foam interlayer breakage upon impact from a drop is dramatically improved. Furthermore, the flexibility and tensile strength of the foam substrate are less likely to vary between the flow direction and the width direction. An adhesive tape using a foam base material having this average cell diameter ratio has good conformability and cushioning properties in the thickness direction, so that the pressure during application is concentrated at the joint, making it easy to push out any air present at the adhesive interface, thereby achieving excellent adhesion that does not create gaps through which water or oil can enter, even when joining rigid bodies.
[0067] Furthermore, the ratio of the average cell diameter in the machine direction to the width direction is not particularly limited, but is preferably 0.25 to 4 times, more preferably 0.33 to 3 times, even more preferably 0.6 to 1.5 times, and particularly preferably 0.7 to 1.3 times, when the machine direction is taken as 1. When the ratio is within the above range, the flexibility and tensile strength of the foam base material are less likely to vary between the machine direction and the width direction.
[0068] The average bubble diameter in the width direction, flow direction, and thickness direction of the foam substrate is measured as follows. First, the foam substrate is cut into approximately 1 cm pieces in both the width direction and flow direction. Next, the cut surface of the foam substrate is magnified 200 times with a digital microscope (product name "KH-7700", manufactured by HiROX), and the cut surface of the foam substrate in the width direction or flow direction is photographed. In the obtained magnified image, the bubble diameters of all bubbles present on the cut surface with an actual length of 2 mm before enlargement in the flow direction or width direction are measured, and the average bubble diameter is calculated from the average value. The average bubble diameter was calculated from the results of measurements at 10 arbitrary points.
[0069] The interlaminar strength, compressive strength, and tensile modulus of the foam substrate can be appropriately adjusted depending on the material and foam structure of the foam substrate used. The material of the foam substrate used in the present invention is not particularly limited as long as it has the above interlaminar strength, 25% compressive strength, and tensile modulus of elasticity, and examples thereof include polyolefin resin, polyester resin, polyvinyl chloride resin, polyphenylene sulfide resin, amide resin, polyimide resin, polyether ether ketone (PEEK), styrene resin, polyurethane resin, and rubber resin. Among them, it is preferable to include at least one resin selected from the group consisting of polyolefin resin, polyurethane resin, and rubber resin. Specifically, the types of foam substrate that can be used include polyolefin foams made of polyolefin resins such as polyethylene, polypropylene, ethylene-propylene copolymer, and ethylene-vinyl acetate copolymer; polyurethane foams made of polyurethane resins; and rubber foams made of rubber resins such as acrylic rubber and other elastomers. Of these, polyolefin foams are preferably used because they are easy to produce into a foam substrate with a thin, closed-cell structure that has excellent conformability to the unevenness of the adherend surface and excellent shock-absorbing properties.
[0070] Among polyolefin foams using polyolefin resins, polyethylene resins are preferred because they can be easily produced with a uniform thickness and can easily impart suitable flexibility. In particular, the content of polyethylene resin in the polyolefin resin is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, and particularly preferably 100% by mass.
[0071] In addition, as the polyethylene resin used for the polyolefin foam, a polyethylene resin obtained by using a metallocene compound containing a tetravalent transition metal as a polymerization catalyst has a narrow molecular weight distribution, and in the case of a copolymer, the copolymer component is introduced into each molecular weight component at an almost equal ratio, so that the polyolefin foam can be crosslinked uniformly. Therefore, since the foam sheet is crosslinked uniformly, it is easy to uniformly stretch the foam sheet as necessary, and the thickness of the obtained polyolefin resin foam can be made uniform overall, which is preferable.
[0072] Furthermore, the polyolefin resin constituting the polyolefin foam may contain a polyolefin resin other than the polyethylene resin obtained by using a metallocene compound containing a tetravalent transition metal as a polymerization catalyst. Such polyolefin resins include polyethylene resins and polypropylene resins other than those mentioned above. The polyolefin resins may be used alone or in combination of two or more kinds.
[0073] Examples of such polyethylene resins include linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-α-olefin copolymers containing 50% or more by weight of ethylene, and ethylene-vinyl acetate copolymers containing 50% or more by weight of ethylene, and these may be used alone or in combination of two or more. Examples of α-olefins constituting the ethylene-α-olefin copolymers include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene.
[0074] The polypropylene resin is not particularly limited, and examples thereof include polypropylene and propylene-α-olefin copolymers containing 50% by weight or more of propylene, which may be used alone or in combination of two or more. Examples of the α-olefins constituting the propylene-α-olefin copolymer include ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, and 1-octene.
[0075] The polyolefin foam may be crosslinked, but in the case where the expandable polyolefin resin sheet is expanded by a thermally decomposable foaming agent, it is preferably crosslinked.
[0076] Next, a method for producing a polyolefin-based resin foam will be described. The method for producing a polyolefin-based resin foam is not particularly limited, and includes, for example, a method including a step of producing a foamable polyolefin-based resin sheet by feeding a polyolefin-based resin containing 40% by weight or more of a polyethylene-based resin obtained using a metallocene compound containing a tetravalent transition metal as a polymerization catalyst, a thermal decomposition type foaming agent, a foaming assistant, and a colorant for coloring the foam black or white, etc., to an extruder, melting and kneading the foamable polyolefin-based resin composition, and extruding the sheet from the extruder, a step of crosslinking the foamable polyolefin-based resin sheet, a step of foaming the foamable polyolefin-based resin sheet, and a step of melting or softening the foamed sheet obtained and stretching the foamed sheet in either one or both of the flow direction and the width direction. The step of stretching the foamed sheet may be performed as necessary, and may be performed multiple times.
[0077] Examples of methods for crosslinking the polyolefin-based resin foam substrate include a method of irradiating a foamable polyolefin-based resin sheet with ionizing radiation, a method of blending an organic peroxide in advance with a foamable polyolefin-based resin composition, and heating the resulting foamable polyolefin-based resin sheet to decompose the organic peroxide, and the like. These methods may be used in combination.
[0078] Examples of ionizing radiation include electron beams, α-rays, β-rays, and γ-rays. The dose of ionizing radiation is appropriately adjusted so that the gel fraction of the polyolefin resin foam substrate falls within the above-mentioned preferred range, and is preferably in the range of 5 kGy to 200 kGy. In addition, since it is easy to obtain a uniform foamed state, it is preferable to irradiate both sides of the expandable polyolefin resin sheet with ionizing radiation, and it is more preferable to irradiate both sides with the same dose.
[0079] Examples of organic peroxides include 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(t-butylperoxy)octane, n-butyl-4,4-bis(t-butylperoxy)valerate, di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, 2,5-di Examples of the peroxyalkylene oxide include methyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, benzoyl peroxide, cumyl peroxy neodecane, t-butyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxy isopropyl carbonate, and t-butylperoxy allyl carbonate. These may be used alone or in combination of two or more.
[0080] The amount of the organic peroxide added is preferably within a range of 0.01 to 5 parts by mass, and more preferably within a range of 0.1 to 3 parts by mass, relative to 100 parts by mass of the polyolefin resin.
[0081] The amount of the thermally decomposable foaming agent added to the foamable polyolefin resin composition may be appropriately determined depending on the expansion ratio of the polyolefin resin foam substrate, but is preferably in the range of 1 to 40 parts by mass, and more preferably 1 to 30 parts by mass, per 100 parts by mass of the polyolefin resin.
[0082] The method for foaming the foamable polyolefin resin sheet is not particularly limited, and examples thereof include a method of heating with hot air, a method of heating with infrared rays, a method using a salt bath, a method using an oil bath, etc., which may be used in combination. Among these, the method of heating with hot air and the method of heating with infrared rays are preferred because they produce little difference between the front and back of the appearance of the polyolefin resin foam substrate surface.
[0083] The stretching of the foam substrate may be performed after the foam substrate is obtained by foaming the foamable polyolefin resin sheet, or may be performed while the foamable polyolefin resin sheet is being foamed. When the foam substrate is stretched after the foam substrate is obtained by foaming the foamable polyolefin resin sheet, the foam substrate may be stretched while maintaining the molten state at the time of foaming without cooling the foam substrate, or the foam substrate may be stretched after cooling the foam substrate and then heating the foam sheet again to make it molten or softened.
[0084] Here, the molten state of the foam base material refers to a state in which the foam base material is heated to a temperature equal to or higher than the melting point of the polyolefin resin constituting the foam base material. In addition, the softening of the foam base material refers to a state in which the foam base material is heated to a temperature equal to or higher than the softening point and lower than the melting point of the polyolefin resin constituting the foam base material. By stretching the foam base material, the bubbles of the foam base material are stretched and deformed in a predetermined direction, and a polyolefin foam having an aspect ratio of the bubbles within a predetermined range can be produced.
[0085] Furthermore, the foam substrate is stretched in the machine direction or width direction of the long foamable polyolefin resin sheet, or in the machine direction and width direction. When the foam substrate is stretched in the machine direction and width direction, the foam substrate may be stretched in the machine direction and width direction simultaneously, or may be stretched in each direction separately.
[0086] Examples of the method for stretching the foam substrate in the machine direction include a method for stretching the foam substrate in the machine direction by making the speed at which the long foamable polyolefin resin sheet is wound up while being cooled after foaming (winding speed) faster than the speed at which the long foamable polyolefin resin sheet is supplied to the foaming process (supply speed), and a method for stretching the foam substrate in the machine direction by making the speed at which the foam substrate is wound up (winding speed) faster than the speed at which the obtained foam substrate is supplied to the stretching process (supply speed).
[0087] In the former method, since the expandable polyolefin resin sheet expands in the machine direction due to its own foaming, when stretching the foam substrate in the machine direction, it is necessary to take into account the expansion in the machine direction due to the foaming of the expandable polyolefin resin sheet, and adjust the supply speed and take-up speed of the foam substrate so that the foam substrate is stretched in the machine direction by more than the amount of expansion.
[0088] In addition, as a method for stretching the foam base material in the width direction, a method is preferred in which both ends in the width direction of the foam base material are gripped by a pair of gripping members, and the pair of gripping members are gradually moved in a direction away from each other to stretch the foam base material in the width direction. Since the foamable polyolefin resin sheet expands in the width direction due to its own foaming, when stretching the foam base material in the width direction, it is necessary to take into account the expansion in the width direction due to the foaming of the foamable polyolefin resin sheet, and adjust the stretching amount of the foam base material in the width direction to be more than the expansion amount.
[0089] Here, the stretching ratio in the machine direction of the polyolefin foam is preferably in the range of 1.1 to 2.0 times, more preferably in the range of 1.2 to 1.5 times. The stretch ratio in the width direction of the polyolefin foam substrate is preferably in the range of 1.2 to 4.5 times, more preferably in the range of 1.5 to 3.5 times.
[0090] The foam substrate may be colored in order to impart design, light-shielding or concealing properties, light reflectivity, and light resistance to the pressure-sensitive adhesive tape. The colorants may be used alone or in combination of two or more kinds.
[0091] In the case of imparting light-shielding properties, concealing properties, and light resistance to the pressure-sensitive adhesive tape of the present invention, the foam substrate is preferably colored black.As the black colorant contained in the black foam substrate, carbon black, graphite, copper oxide, manganese dioxide, aniline black, perylene black, titanium black, cyanine black, activated carbon, ferrite, magnetite, chromium oxide, iron oxide, molybdenum disulfide, chromium complex, composite oxide-based black pigment, anthraquinone-based organic black pigment, etc. can be used.Among them, carbon black is preferred from the viewpoints of cost, availability, insulation, and heat resistance that can withstand the temperature of the process of extruding the foamable polyolefin-based resin composition and the heat foaming process.
[0092] In the case of imparting design properties and light reflectivity to the pressure-sensitive adhesive tape of the present invention, the foam base is preferably colored white. Examples of the white colorant contained in the white foam base include inorganic white colorants such as titanium oxide, zinc oxide, aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, calcium oxide, tin oxide, barium oxide, cesium oxide, yttrium oxide, magnesium carbonate, calcium carbonate, barium carbonate, zinc carbonate, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, zinc hydroxide, aluminum silicate, calcium silicate, barium sulfate, calcium sulfate, barium stearate, zinc oxide, talc, silica, alumina, clay, kaolin, titanium phosphate, mica, gypsum, white carbon, diatomaceous earth, bentonite, lithopone, zeolite, and sericite, and organic white colorants such as silicone resin particles, acrylic resin particles, urethane resin particles, and melamine resin particles. Among these, aluminum oxide and zinc oxide are preferred from the viewpoints of cost, availability, color tone, and heat resistance capable of withstanding the temperatures in the step of extruding the expandable polyolefin resin composition and the step of heating and expanding the composition.
[0093] In addition, the expandable polyolefin resin composition may contain known substances such as plasticizers, antioxidants, foaming assistants such as zinc oxide, bubble nucleation regulators, heat stabilizers, flame retardants such as aluminum hydroxide and magnesium hydroxide, antistatic agents, glass or plastic hollow balloon beads, metal powders, metal compounds, conductive fillers, and thermally conductive fillers, as long as the physical properties of the polyolefin resin foam substrate are not impaired. The polyolefin resin foam substrate used in the pressure-sensitive adhesive sheet of the present invention is preferably in the range of 0.1% by mass to 10% by mass, and more preferably in the range of 1% by mass to 7% by mass, based on the polyolefin resin, in order to maintain appropriate conformability and cushioning properties.
[0094] When the above-mentioned colorant, thermally decomposable foaming agent, foaming assistant, etc. are blended with the foamable polyolefin-based resin composition, it is preferable to prepare a masterbatch with the foamable polyolefin-based resin composition or a thermoplastic resin that is highly compatible with the foamable polyolefin-based resin composition before supplying it to the extruder, from the viewpoint of preventing uneven coloring and partial excessive or insufficient foaming.
[0095] The foam substrate may be surface-treated by corona treatment, flame treatment, plasma treatment, hot air treatment, ozone / ultraviolet treatment, coating of an easy-adhesion treatment agent, etc., in order to improve adhesion to the adhesive layer and other layers. The surface treatment is performed to obtain a wetting index of 36 mN / m or more, preferably 40 mN / m or more, more preferably 48 mN / m or more, using a wetting reagent, so that good adhesion to the adhesive layer can be obtained. The foam substrate with improved adhesion may be attached to the adhesive layer in a continuous process, or may be once wound up. When the foam substrate is once wound up, it is preferable to wind up the foam substrate together with an insert such as paper, polyethylene, polypropylene, or polyester film, in order to prevent blocking between the foam substrates with improved adhesion, and a polypropylene film or polyester film having a thickness of 25 μm or less is preferable.
[0096] The thickness of the foam substrate is preferably within a range of 50 μm to 400 μm, more preferably within a range of 50 μm to 300 μm, even more preferably within a range of 100 μm to 300 μm, and most preferably within a range of 100 μm to 200 μm. By setting the thickness of the foam substrate within this range, it is possible to impart excellent tape processability and excellent conformability to an adherend.
[0097] (Method of manufacturing adhesive tape) Methods for producing the pressure-sensitive adhesive tape of the present invention include a method (direct method) in which the above-mentioned pressure-sensitive adhesive composition is applied to one or both sides of a foam substrate and dried or the like to produce the tape; or a method (transfer method) in which the above-mentioned pressure-sensitive adhesive composition is applied to the surface of a release liner and dried or the like to form a pressure-sensitive adhesive layer, and then the pressure-sensitive adhesive layer is transferred to one or both sides of the foam substrate to produce the tape.
[0098] The pressure-sensitive adhesive tape of the present invention can be produced by applying the above-mentioned pressure-sensitive adhesive composition to one or both sides of the foam substrate using a knife coater, roll coater, die coater, etc., and drying the composition. The pressure-sensitive adhesive tape can also be produced by a transfer method in which the above-mentioned pressure-sensitive adhesive composition is applied to the surface of a release liner using a knife coater, roll coater, die coater, etc., and dried to form a pressure-sensitive adhesive layer, and then the pressure-sensitive adhesive layer is bonded to one or both sides of the foam substrate.
[0099] The pressure-sensitive adhesive composition may be dried, for example, for 30 seconds to 10 minutes at 50° C. to 140° C. After drying, the composition may be further aged at a temperature in the range of 30° C. to 50° C. in order to promote the curing reaction.
[0100] (Application) The adhesive tape of the present invention has good initial adhesive strength, is not easily swollen even when, for example, sweat or sebum is attached, has oil resistance that enables it to maintain excellent adhesive strength for a long period of time, and has excellent impact resistance, so it can be suitably used in a variety of fields, such as double-sided tapes used for bonding the housings that constitute electronic devices such as portable electronic terminals and tablet computers, labels that impart design to the surface of the housings, waterproof tapes, and medical adhesive tapes.
[0101] (Goods) The article of the present invention has a configuration in which two or more adherends are adhered by the above-mentioned pressure-sensitive adhesive tape of the present invention. According to the article of the present invention, the initial adhesive strength of the pressure-sensitive adhesive tape is good, and the pressure-sensitive adhesive tape is not likely to swell even when, for example, sweat or sebum is attached, so that excellent adhesive strength can be maintained for a long period of time. Furthermore, according to the article of the present invention, the adherends are not likely to break or peel off even when dropped, and the article has excellent impact resistance.
[0102] In particular, electronic devices such as portable electronic terminals, which have become larger and thinner in recent years and therefore have limited application areas, are prone to being dropped during use and are often touched by people's hands, making them susceptible to sweat, sebum, and the like, and therefore are highly required to have oil resistance and impact resistance. For this reason, it is preferable that the article is an electronic device. That is, an example of the article of the present invention can be an electronic device having a configuration in which two or more components constituting the electronic device are bonded by the above-mentioned pressure-sensitive adhesive tape of the present invention.
[0103] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0104] The present invention will now be described in more detail with reference to examples.
[0105] (Gel fraction measurement) The gel fraction of the pressure-sensitive adhesive composition prepared in each Preparation Example was measured by the method described below. The gel fraction of the pressure-sensitive adhesive composition corresponds to the gel fraction of the pressure-sensitive adhesive layer in each of the Examples and Comparative Examples formed using the pressure-sensitive adhesive composition.
[0106] The adhesive composition was applied to the release-treated surface of the release liner so that the thickness after drying was 50 μm, and the adhesive composition was dried for 3 minutes in an environment at 100 ° C., and then aged for 2 days in an environment at 40 ° C. to form an adhesive layer. The adhesive layer was cut into a square of 50 mm length and 50 mm width to prepare a test piece, and the mass (G1) of the test piece was measured. Then, the test piece was immersed in toluene for 24 hours in an environment at 23 ° C., and after immersion, the mixture of the test piece and toluene was filtered using a 300 mesh wire net to extract the insoluble components in toluene. The insoluble components were dried for 1 hour in an environment at 110 ° C., and the mass (G2) of the insoluble components was measured, and the gel fraction was calculated based on the mass (G1) and mass (G2) and the following formula. Gel fraction (mass%) = (G2 / G1) x 100
[0107] (Average number of carbon atoms in the saturated hydrocarbon group of the alkoxyalkyl (meth)acrylate (B) and the carboxyl group-containing monomer (A) and the alkyl (meth)acrylate (C) other than the alkoxyalkyl (meth)acrylate (B)) The average number of carbon atoms in the saturated hydrocarbon group of one or more selected from alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate monomers in the acrylic copolymer prepared in the Preparation Example was calculated by adding up the product of the number of carbon atoms in each saturated hydrocarbon group and its molar concentration (mol%), and dividing the sum by the total molar concentration (mol%) of one or more selected from the group consisting of all (B) alkoxyacrylate and (C) alkyl (meth)acrylate monomers containing the total. For example, when the alkoxyalkyl (meth)acrylate monomer with the number of carbon atoms A in the saturated hydrocarbon group is a (mol%), the alkyl (meth)acrylate monomer with the number of carbon atoms B in the saturated hydrocarbon group is b (mol%), and the alkyl (meth)acrylate monomer with the number of carbon atoms C in the saturated hydrocarbon group is c (mol%), the average number of carbon atoms was calculated by (A×a+B×b+C×c) / (a+b+c).
[0108] [Preparation Example 1] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 75.94 parts by mass of n-butyl acrylate, 9 parts by mass of acrylic acid, 5 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 10 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0109] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0110] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-1) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.65.
[0111] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-1) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-1).
[0112] [Preparation Example 2] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 70.94 parts by mass of n-butyl acrylate, 9 parts by mass of acrylic acid, 5 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 15 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0113] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0114] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-2) solution having a weight average molecular weight of 1.1 million and an average carbon atom number of the saturated hydrocarbon group of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.60.
[0115] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-2) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-2).
[0116] [Preparation Example 3] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 65.94 parts by mass of n-butyl acrylate, 9 parts by mass of acrylic acid, 5 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 20 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0117] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0118] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-3) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.55.
[0119] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-3) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-3).
[0120] [Preparation Example 4] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 57.94 parts by mass of n-butyl acrylate, 5 parts by mass of acrylic acid, 7 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 30 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0121] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0122] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-4) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.38.
[0123] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-4) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of resin solids in the solution, thereby obtaining a solution containing an adhesive composition (P-4).
[0124] [Preparation Example 5] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 58.44 parts by mass of n-butyl acrylate, 3.5 parts by mass of acrylic acid, 8 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 30 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0125] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0126] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-5) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.35.
[0127] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-5) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-5).
[0128] [Preparation Example 6] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 48.44 parts by mass of n-butyl acrylate, 3.5 parts by mass of acrylic acid, 8 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 40 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0129] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0130] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-6) solution having a weight average molecular weight of 1.1 million and an average carbon atom number of the saturated hydrocarbon group of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.25.
[0131] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-6) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-6).
[0132] [Preparation Example 7] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 38.44 parts by mass of n-butyl acrylate, 3.5 parts by mass of acrylic acid, 8 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 50 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0133] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0134] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-7) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.15.
[0135] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-7) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-7).
[0136] [Preparation Example 8] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 32.94 parts by mass of n-butyl acrylate, 3.5 parts by mass of acrylic acid, 12 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 50 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0137] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0138] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-8) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 2.97.
[0139] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-8) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-8).
[0140] [Preparation Example 9] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 20.94 parts by mass of n-butyl acrylate, 3 parts by mass of acrylic acid, 6 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 70 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0141] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0142] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire net to obtain an acrylic copolymer (A-9) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.03.
[0143] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-9) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-9).
[0144] [Preparation Example 10] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 58.44 parts by mass of n-butyl acrylate, 3.5 parts by mass of acrylic acid, 8 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 30 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0145] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0146] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-10) solution having a weight average molecular weight of 900,000 and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.35.
[0147] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-10) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-10).
[0148] [Preparation Example 11] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-10) solution in an amount such that the gel fraction of the adhesive composition was 40% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-11).
[0149] [Preparation Example 12] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-10) solution in an amount such that the gel fraction of the adhesive composition was 63% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-12).
[0150] [Preparation Example 13] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-10) solution in an amount such that the gel fraction of the adhesive composition was 72% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-13).
[0151] [Preparation Example 14] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 80.94 parts by mass of n-butyl acrylate, 9 parts by mass of acrylic acid, 5 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 5 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0152] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0153] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-11) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.71.
[0154] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-11) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-14).
[0155] [Preparation Example 15] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 84.94 parts by mass of n-butyl acrylate, 7 parts by mass of acrylic acid, 8 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0156] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0157] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-12) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.63.
[0158] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-12) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-15).
[0159] [Preparation Example 16] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 85.94 parts by mass of n-butyl acrylate, 9 parts by mass of acrylic acid, 5 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0160] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0161] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-13) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.76.
[0162] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-13) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-16).
[0163] [Preparation Example 17] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 77.94 parts by mass of n-butyl acrylate, 7 parts by mass of acrylic acid, 15 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0164] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0165] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-14) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 3.33.
[0166] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-14) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-17).
[0167] [Preparation Example 18] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 66.94 parts by mass of n-butyl acrylate, 5 parts by mass of acrylic acid, 28 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0168] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0169] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-15) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 2.85.
[0170] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-15) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-18).
[0171] [Preparation Example 19] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 44.94 parts by mass of n-butyl acrylate, 40 parts by mass of 2-ethylhexyl acrylate, 7 parts by mass of acrylic acid, 8 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then held at 75°C for 5 hours.
[0172] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0173] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-16) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 4.89.
[0174] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-16) solution in an amount such that the gel fraction of the adhesive composition was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing an adhesive composition (P-19).
[0175] [Preparation Example 20] A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 1.94 parts by mass of n-butyl acrylate, 10 parts by mass of acrylic acid, 13 parts by mass of methyl acrylate, 0.06 parts by mass of 4-hydroxybutyl acrylate, 75 parts by mass of methoxyethyl acrylate, and 200 parts by mass of ethyl acetate, and the mixture was held at 72°C for 4 hours with stirring, and then at 75°C for 5 hours.
[0176] Next, 2 parts by mass of a solution of 2,2'-azobis(2-methylbutyronitrile) previously dissolved in ethyl acetate (solid content 0.1% by mass) was added to the mixture in the reaction vessel, and the mixture was held at 72°C for 4 hours under stirring, and then at 75°C for 5 hours.
[0177] Next, the mixture in the reaction vessel was diluted with 98 parts by mass of ethyl acetate and filtered through a 200 mesh wire screen to obtain an acrylic copolymer (A-18) solution having a weight average molecular weight of 1.1 million and an average number of carbon atoms of the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate and alkyl (meth)acrylate of 2.61.
[0178] An adduct of tolylene diisocyanate and trimethylolpropane ("Burnoc D-40" manufactured by DIC Corporation, hereinafter abbreviated as "D-40") was added to the above acrylic copolymer (A-18) solution in an amount such that the gel fraction was 55% per 100 parts by mass of the resin solid content in the solution, thereby obtaining a solution containing a pressure-sensitive adhesive composition (P-20).
[0179] [Example 1] A solution containing the adhesive composition (P-1) obtained in Preparation Example 1 was applied to the release-treated surface of a release liner (a 75 μm-thick polyethylene terephthalate film with one side treated for release) so that the adhesive layer would have a thickness of 75 μm after drying, and was dried at 100° C. for 3 minutes to produce two adhesive layers each 75 μm thick.
[0180] Next, in a 23°C environment, a polyolefin foam (F-1) (thickness 100 μm, density 0.5 g / cm 3 The above 75 μm thick pressure-sensitive adhesive layers were attached to both sides of a sheet of polyester (manufactured by Sekisui Chemical Co., Ltd., the surface of which had been corona-treated to give a wetting index of 54 mN / m) and then laminated from the top of the release liner using a roll at a linear pressure of 5 kg / cm. Thereafter, the mixture was aged in an environment of 40° C. for 48 hours to obtain a double-sided adhesive tape (T-1) having a thickness of 250 μm.
[0181] [Example 2] A double-sided adhesive tape (T-2) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-2) was used instead of the adhesive composition (P-1).
[0182] [Example 3] A double-sided adhesive tape (T-3) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-3) was used instead of the adhesive composition (P-1).
[0183] [Example 4] A double-sided pressure-sensitive adhesive tape (T-4) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the pressure-sensitive adhesive composition (P-4) was used instead of the pressure-sensitive adhesive composition (P-1).
[0184] [Example 5] A double-sided adhesive tape (T-5) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-5) was used instead of the adhesive composition (P-1).
[0185] [Example 6] A double-sided adhesive tape (T-6) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-6) was used instead of the adhesive composition (P-1).
[0186] [Example 7] A double-sided adhesive tape (T-7) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-7) was used instead of the adhesive composition (P-1).
[0187] [Example 8] A double-sided adhesive tape (T-8) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-8) was used instead of the adhesive composition (P-1).
[0188] [Example 9] A double-sided adhesive tape (T-9) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-9) was used instead of the adhesive composition (P-1).
[0189] [Example 10] A double-sided adhesive tape (T-10) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-10) was used instead of the adhesive composition (P-1).
[0190] [Example 11] A double-sided adhesive tape (T-11) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-11) was used instead of the adhesive composition (P-1).
[0191] [Example 12] A double-sided adhesive tape (T-12) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-12) was used instead of the adhesive composition (P-1).
[0192] [Example 13] A double-sided adhesive tape (T-13) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-13) was used instead of the adhesive composition (P-1).
[0193] [Example 14] A solution containing the adhesive composition (P-5) was used instead of the adhesive composition (P-1), and a polyolefin foam (F-2) (thickness 100 μm, density 0.25 g / cm) was used instead of the polyolefin foam (F-1). 3 A 250 μm-thick double-sided adhesive tape (T-14) was obtained in the same manner as in Example 1, except that the above-mentioned 75 μm-thick adhesive layer was attached to both sides of a 250 μm-thick double-sided adhesive tape (T-14) made by Sekisui Chemical Co., Ltd., the surface of which had been corona-treated to give a wettability index of 54 mN / m.
[0194] [Example 15] A solution containing the adhesive composition (P-5) was used instead of the adhesive composition (P-1), and a polyolefin foam (F-3) (thickness 100 μm, density 0.33 g / cm) was used instead of the polyolefin foam (F-1). 3 A 250 μm-thick double-sided adhesive tape (T-15) was obtained in the same manner as in Example 1, except that the above-mentioned 75 μm-thick adhesive layer was attached to both sides of a 250 μm-thick double-sided adhesive tape (T-15) made by Sekisui Chemical Co., Ltd., the surface of which had been corona-treated to give a wettability index of 54 mN / m.
[0195] [Example 16] A solution containing the adhesive composition (P-5) was used instead of the adhesive composition (P-1), and a polyolefin foam (F-4) (thickness 100 μm, density 0.63 g / cm) was used instead of the polyolefin foam (F-1). 3 A 250 μm-thick double-sided adhesive tape (T-16) was obtained in the same manner as in Example 1, except that the above-mentioned 75 μm-thick adhesive layer was attached to both sides of a 250 μm-thick double-sided adhesive tape (T-16) made by Sekisui Chemical Co., Ltd., the surface of which had been corona-treated to give a wettability index of 54 mN / m.
[0196] [Example 17] Two adhesive layers with a thickness of 25 μm were prepared by using a solution containing the adhesive composition (P-5) instead of the adhesive composition (P-1), and polyolefin foam (F-5) (thickness 200 μm, density 0.5 g / cm) was used instead of the polyolefin foam (F-1). 3 A 250 μm-thick double-sided adhesive tape (T-17) was obtained in the same manner as in Example 1, except that the above-mentioned 25 μm-thick adhesive layer was attached to both sides of a 250 μm-thick double-sided adhesive tape (T-17) made by Sekisui Chemical Co., Ltd., the surface of which had been corona-treated to give a wettability index of 54 mN / m.
[0197] [Example 18] Two 50 μm-thick adhesive layers were prepared using a solution containing the adhesive composition (P-5) instead of the adhesive composition (P-1), and the 50 μm-thick adhesive layers were attached to both sides of a polyolefin foam (F-1) in the same manner as in Example 1, to obtain a 200 μm-thick double-sided adhesive tape (T-18).
[0198] [Example 19] Two 100 μm-thick adhesive layers were prepared using a solution containing the adhesive composition (P-5) instead of the adhesive composition (P-1), and the 100 μm-thick adhesive layers were attached to both sides of a polyolefin foam (F-1) in the same manner as in Example 1, to obtain a 300 μm-thick double-sided adhesive tape (T-19).
[0199] [Comparative Example 1] A double-sided adhesive tape (T-20) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-14) was used instead of the adhesive composition (P-1).
[0200] [Comparative Example 2] A double-sided adhesive tape (T-21) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-15) was used instead of the adhesive composition (P-1).
[0201] [Comparative Example 3] A double-sided pressure-sensitive adhesive tape (T-22) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the pressure-sensitive adhesive composition (P-16) was used instead of the pressure-sensitive adhesive composition (P-1).
[0202] [Comparative Example 4] A double-sided adhesive tape (T-23) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-17) was used instead of the adhesive composition (P-1).
[0203] [Comparative Example 5] A double-sided adhesive tape (T-24) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-18) was used instead of the adhesive composition (P-1).
[0204] [Comparative Example 6] A double-sided adhesive tape (T-25) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-19) was used instead of the adhesive composition (P-1).
[0205] [Comparative Example 7] A double-sided adhesive tape (T-26) having a thickness of 250 μm was obtained in the same manner as in Example 1, except that a solution containing the adhesive composition (P-20) was used instead of the adhesive composition (P-1).
[0206] [Comparative Example 8] A solution containing the adhesive composition (P-3) was used instead of the adhesive composition (P-1), and a polyolefin foam (F-6) (thickness 100 μm, density 0.13 g / cm) was used instead of the polyolefin foam (F-1). 3 A 250 μm-thick double-sided adhesive tape (T-27) was obtained in the same manner as in Example 1, except that the above-mentioned 75 μm-thick adhesive layer was attached to both sides of a 250 μm-thick double-sided adhesive tape (T-27) made by Sekisui Chemical Co., Ltd., the surface of which had been corona-treated to give a wettability index of 54 mN / m.
[0207] [Comparative Example 9] A solution containing the adhesive composition (P-3) was used instead of the adhesive composition (P-1), and a polyolefin foam (F-7) (thickness 100 μm, density 0.17 g / cm) was used instead of the polyolefin foam (F-1). 3 A 250 μm-thick double-sided adhesive tape (T-28) was obtained in the same manner as in Example 1, except that the above-mentioned 75 μm-thick adhesive layer was attached to both sides of a 250 μm-thick double-sided adhesive tape (T-28) made by Sekisui Chemical Co., Ltd., the surface of which had been corona-treated to give a wettability index of 54 mN / m.
[0208] <Evaluation> [Method of measuring push strength] The double-sided adhesive tapes obtained in the Examples and Comparative Examples were cut to 18.5 mm square and 2 mm wide, and in an environment of 23°C temperature and 50% RH, the release liner on one side of the double-sided adhesive tape was peeled off, and one piece of the adhesive tape was attached to a 20 mm square soda glass plate (hue: colorless and transparent) with a thickness of 3 mm.
[0209] The release liner on the other side of the test piece was peeled off and attached to the surface of a 2 mm thick polycarbonate plate (Bayer, Makrolon, color: transparent) with a 12 mm diameter hole in the center (adhesive area: 1.32 cm). 2), and the upper surface is subjected to 50N / cm 2 The adhesive was applied for 10 seconds at 0.5° C. to obtain a patch.
[0210] The above-mentioned adhesive was left for 24 hours in an atmosphere of 23°C and 50% RH, and then left for 24 hours in an atmosphere of 60°C and 90% RH. Then, it was left for 24 hours at 23°C and 50% RH. Next, a 7 mm diameter probe was pressed against a glass plate at a speed of 5 mm / min from the back side of the polycarbonate plate of the above-mentioned adhesive, and the strength (G1) at which the glass plate peeled off was measured.
[0211] [Oil resistance evaluation method] The patch obtained by the above [Method for measuring push strength] was left in an atmosphere of 23°C and 50% RH for 24 hours, and then 10 mg of a solution of 99% by mass oleic acid solution: squalene acid = 1:1 was dropped through the hole in the polycarbonate plate, and the plate was left in an atmosphere of 60°C and 90% RH for 24 hours. Thereafter, the sample was left at 23° C. and 50% RH for 24 hours. Next, a probe having a diameter of 7 mm was pressed against the glass plate from the rear surface of the polycarbonate plate of the above-mentioned adhesive at a speed of 5 mm / min, and the strength (G2) at which the glass plate peeled off was measured.
[0212] The adhesive strength retention was calculated from the push strength obtained in the above-mentioned push strength measurement and the oil resistance evaluation. Adhesive strength retention rate (%)=(G2 / G1)×100
[0213] Based on the calculated adhesive strength retention, the adhesive strength was judged according to the following criteria A to D. Criteria A to C were rated as good. A: Adhesion retention was 70% or more. B: Adhesion retention was 60% or more and less than 70%. C: Adhesion retention was 50% or more and less than 60%. D: Adhesion retention was less than 50%.
[0214] [Impact resistance evaluation method] The adhesive obtained by the above [Method for measuring push strength] was left for 24 hours in an atmosphere of 23°C and 50% RH, and then the glass plate of the test piece was placed on the base of a DuPont impact tester (manufactured by Tester Sangyo Co., Ltd.) with the glass plate of the test piece facing downward.
[0215] Next, a stainless steel impact core with a diameter of 9.5 mm and a mass of 200 g was dropped from a height of 10 cm three times from the polycarbonate plate side, and the presence or absence of peeling of the adhesive sheet of the test piece or damage to the substrate was evaluated. If there was no peeling, the drop height was increased by 10 cm from the previous time, and the presence or absence of peeling of the adhesive sheet of the test piece or damage to the substrate after the three drops was confirmed. Thereafter, if there was no peeling or damage to the substrate, the drop height was increased by 10 cm each time and the test was repeated in the same manner, and the drop height (cm) at which peeling of the adhesive sheet of the test piece or damage to the substrate was finally observed was measured and judged according to the following criteria A to E. Criteria A to C were considered good.
[0216] A: The fall height was 80cm or more. B: The fall height was 70cm or more and less than 80cm. C: The fall height was 60cm or more and less than 70cm. D: The fall height was 50cm or more and less than 60cm. E: The fall height was less than 50 cm.
[0217] The details of the pressure-sensitive adhesive tapes of the Examples and Comparative Examples, as well as the evaluation results, are shown in the table below. The abbreviations of the adhesive compositions in the table represent the following monomers. The "average number of carbon atoms" in the table refers to the average number of carbon atoms in the saturated hydrocarbon groups of the alkoxyalkyl (meth)acrylate (B) and the carboxyl group-containing monomer (A) and the alkyl (meth)acrylate monomer (C) other than the alkoxyalkyl (meth)acrylate (B), and the calculation method is as described above.
[0218] (Monomer abbreviation) BA: n-butyl acrylate 2EHA: 2-ethylhexyl acrylate MA: Methyl acrylate MEA: Methoxyethyl acrylate AA: Acrylic acid 4HBA: 4-hydroxybutyl acrylate
[0219] [Table 1]
[0220] [Table 2]
[0221] [Table 3]
[0222] [Table 4]
[0223] [Table 5]
[0224] [Table 6]
[0225] In Examples 1 to 19, the oil resistance and impact resistance were both good, being rated A to C. In contrast, in Comparative Examples 1 to 9, the oil resistance was rated D and / or the impact resistance was rated D or E, meaning that both the oil resistance and the impact resistance could not be achieved.
Claims
1. A pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer on at least one surface of a foam substrate, either directly or via another layer, The foam density of the foam base material is within a range of 0.25 g / cm3 to 0.75 g / cm3, the pressure-sensitive adhesive layer contains an acrylic pressure-sensitive adhesive composition containing an acrylic copolymer and a crosslinking agent, The acrylic copolymer is (A) a carboxyl group-containing monomer in the range of 2% by mass to 30% by mass, (B) an alkoxyalkyl (meth)acrylate in the range of 10% by mass to 70% by mass; and (C) one or more alkyl (meth)acrylate monomers other than the monomers (A) and (B); (D) Hydroxyl group-containing monomer in the range of 0.01 to 1.0 mass % Contains as a constituent The average number of carbon atoms in the saturated hydrocarbon groups of the monomers (B) and (C) is less than 4.
2. The pressure-sensitive adhesive tape according to claim 1, wherein the foam substrate has a thickness in the range of 50 μm to 400 μm.
3. 3. The pressure-sensitive adhesive tape according to claim 1, wherein the thickness of the pressure-sensitive adhesive tape is within a range of 80 μm to 500 μm.
4. The pressure-sensitive adhesive tape according to any one of claims 1 to 3, wherein the pressure-sensitive adhesive layer has a gel fraction in the range of 40% to 80%.
5. The pressure-sensitive adhesive tape according to any one of claims 1 to 4, wherein the acrylic copolymer has a weight average molecular weight of 500,000 or more.
6. The pressure-sensitive adhesive tape according to any one of claims 1 to 5, wherein the foam substrate comprises at least one resin selected from the group consisting of polyolefin resins, polyurethane resins and rubber-based resins.
7. The pressure-sensitive adhesive tape according to any one of claims 1 to 6, wherein the alkoxyalkyl (meth)acrylate comprises 2-methoxyethyl (meth)acrylate.
8. The pressure-sensitive adhesive tape according to any one of claims 1 to 7, wherein the crosslinking agent is an isocyanate-based crosslinking agent.
9. An article having a configuration in which two or more adherends are adhered with the pressure-sensitive adhesive tape according to any one of claims 1 to 8.
10. An electronic device having two or more components that constitute the electronic device, which are adhered by the adhesive tape according to any one of claims 1 to 8.
Citation Information
Patent Citations
The medical adhesive tape or sheet tape - sheet -
JP1983120724U
Adhesive material for fixation to living body
JP1992005807U
Adhesive sheet for application on skin and first aid adhesive tape
JP1998014973A
Adhesive tape
JP2006036911A
Double-sided adhesive tape